Composite resin and method for producing same

By integrating a silane compound with epoxy and hydrolyzable silyl groups into the polysiloxane and bonding it with phenolic resin, the composite resin achieves superior heat resistance, flexibility, and scratch resistance, addressing the limitations of conventional composite resins and enhancing their performance in coating applications.

WO2024224984A1PCT designated stage expired Publication Date: 2024-10-31DIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013973
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-04
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional composite resins formed by combining phenolic resins and polysiloxane lack sufficient heat resistance, flexibility, and scratch resistance, limiting their performance in coating applications.

Method used

Incorporating a silane compound with an epoxy group and a hydrolyzable silyl group into the polysiloxane, which is then bonded with phenolic resin through a specific polycondensation process, to create a composite resin with enhanced structural units that improve heat resistance, flexibility, and scratch resistance.

Benefits of technology

The resulting composite resin exhibits excellent heat resistance, flexibility, and scratch resistance, along with improved compatibility, storage stability, and coating appearance, making it suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013973_31102024_PF_FP_ABST
    Figure JP2024013973_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a composite resin comprising a polysiloxane and a phenolic resin combined with each other, wherein the polysiloxane has a structural unit represented by formula (1A) or (1B) and a structural unit represented by formula (2) and the phenolic resin is combined with the polysiloxane via a hydroxyl group. R11 represents a monovalent group having an epoxy group; R12 represents an alkyl group; R14 represents a linking group and R15 represents a hydrogen atom or a hydrocarbon group, R14 and R15 may be bonded to each other to form a ring; p1 and p2 are such that (p1, p2)=(0, 1) or (1, 0); and * indicates a bond. R21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group, q1 and q2 are such that (q1, q2)=(1,1) or (2, 0), and * indicates a bond.
Need to check novelty before this filing date? Find Prior Art

Description

Composite resin and its manufacturing method

[0001] The present invention relates to a composite resin and a method for producing the same.

[0002] Due to their excellent heat resistance, durability, mechanical properties, and surface properties such as hardness, phenolic resins have been widely used in various industrial fields, including electrical, electronic, automotive, construction, and civil engineering, as molding materials, coating materials, binder materials, etc. In recent years, as performance requirements have become more sophisticated, extensive research has been conducted to improve resin properties such as heat resistance and coating strength by combining phenolic resins with inorganic materials as reinforcing materials.

[0003] For example, Patent Document 1 discloses a method for producing an electrode material, which includes a step of heating a polymer in which a specific polysiloxane is bonded to a polymer having repeating units derived from an organic monomer that does not contain a silicon atom.

[0004] Patent No. 6274032

[0005] According to the investigations of the present inventors, it has been found that there is room for improvement in the heat resistance, flexibility, and scratch resistance of a composite resin in which a phenolic resin and a polysiloxane are bonded together when a coating film is formed.

[0006] Therefore, an object of one aspect of the present invention is to provide a composite resin of a phenolic resin and a polysiloxane that can form a coating film that is excellent in heat resistance, flexibility, and scratch resistance.

[0007] As a result of investigations aimed at solving the above problems, the present inventors have found that by using a silane compound having an epoxy group and a hydrolyzable silyl group as the silane compound, which is a raw material for polysiloxane, a composite resin of a phenolic resin and a polysiloxane can be obtained that is capable of forming a coating film that is excellent in heat resistance, flexibility, and scratch resistance. The present invention includes the following aspects.

[0008] [1] A composite resin in which a polysiloxane and a phenolic resin are bonded to each other, wherein the polysiloxane has a structural unit represented by the following formula (1A) or (1B) and a structural unit represented by the following formula (2), and the phenolic resin is bonded to the polysiloxane via a hydroxyl group possessed by the phenolic resin. In the formula, R 11 represents a monovalent group having an epoxy group, R 12 represents an alkyl group, and R 14 represents a linking group, R 15 represents a hydrogen atom or a hydrocarbon group, R 14 and R 15 may be bonded to each other to form a ring, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

[0009] [2] The composite resin according to [1], wherein the amount of the structural unit represented by formula (1A) or (1B) is 10 to 60 mol% based on the total amount of the structural unit represented by formula (1A) or (1B) and the structural unit represented by formula (2).

[0010] [3] The composite resin according to [1] or [2], wherein the phenol resin is bonded to a structural unit represented by formula (1A) or (1B).

[0011] [4] A method for producing a composite resin, comprising: a step of reacting a phenolic resin with a silane compound represented by the following formula (11) to obtain an intermediate; and a step of polycondensing the intermediate with a silane compound represented by the following formula (12). In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 represent either (m1, m2)=(0, 3) or (1, 2). In the formula, R 21represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).

[0012] [5] A method for producing a composite resin, comprising a step of polycondensing a phenol and an aldehyde in the presence of a polysiloxane having a structural unit represented by the following formula (21) and a structural unit represented by the following formula (22): In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

[0013] [6] A method for producing a composite resin, comprising a step of simultaneously polycondensing a phenol, an aldehyde, a silane compound represented by the following formula (11), and a silane compound represented by the following formula (12): In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 represent either (m1, m2)=(0, 3) or (1, 2). In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).

[0014] [7] The production method according to [4] or [6], wherein the amount of the silane compound represented by formula (11) is 10 to 60 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12).

[0015] [8] The method according to [5], wherein the amount of the structural unit represented by formula (21) is 10 to 60 mol% based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22).

[0016] According to one aspect of the present invention, there is provided a composite resin of a phenolic resin and a polysiloxane that can form a coating film that is excellent in heat resistance, flexibility, and scratch resistance. According to another aspect of the present invention, the composite resin can also be excellent in terms of compatibility, storage stability, and coating film appearance.

[0017] According to another aspect of the present invention, by utilizing a bottom-up process, the composition, solids ratio, etc. of the phenolic resin-polysiloxane can be freely designed, and a composite resin with a controlled structure can be obtained.

[0018] [Method for Producing a Composite Resin] One embodiment of the present invention is a method for producing a composite resin in which a polysiloxane and a phenolic resin are bonded to each other. This method, as described in detail below, is characterized by using a silane compound having an epoxy group and a hydrolyzable silyl group (hereinafter also referred to as an "epoxysilane compound") as a raw material for the polysiloxane. Examples of such a production method include a production method in which a silane compound containing an epoxysilane compound is polycondensed in the presence of a phenolic resin to produce a polysiloxane and thereby obtain a composite resin (hereinafter also referred to as "Production Method A"); a production method in which a phenolic resin is polycondensed in the presence of a silane compound containing an epoxysilane compound to produce a phenolic resin and thereby obtain a composite resin (hereinafter also referred to as "Production Method B"); and a production method in which a phenolic resin, an aldehyde, and a silane compound containing an epoxysilane compound are polycondensed all at once to obtain a composite resin in which a polysiloxane and a phenolic resin are bonded to each other (hereinafter also referred to as "Production Method C"). In either production method, it is essential to use an epoxysilane compound as a raw material for polysiloxane.

[0019] (Production Method A) A method for producing a composite resin according to one embodiment of the present invention (production method A) includes a step (step (A-1)) of reacting a phenolic resin with a silane compound represented by the following formula (11) to obtain an intermediate. In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 represent either (m1, m2)=(0, 3) or (1, 2).

[0020] The phenolic resin used in step (A-1) is not particularly limited. The phenolic resin can be obtained by reacting a phenol with an aldehyde by a known method. Alternatively, a commercially available phenolic resin may be used as the phenolic resin. In this specification, the term "phenol" refers to a phenolic compound as a monomer constituting a phenolic resin, and does not include phenolic resins.

[0021] Examples of phenolic resins include novolac-type phenolic resins (e.g., obtained by reacting phenols with aldehydes in the presence of an acid catalyst) and resol-type phenolic resins (e.g., obtained by reacting phenols with aldehydes in the presence of an alkali catalyst).

[0022] Examples of phenols include monohydric phenols such as phenol, cresols such as o-cresol, m-cresol, and p-cresol; xylenols such as 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol; ethylphenols such as o-ethylphenol, m-ethylphenol, and p-ethylphenol; butylphenols such as isopropylphenol, butylphenol, and p-tert-butylphenol; alkylphenols such as p-tert-amylphenol, p-octylphenol, p-nonylphenol, and p-cumylphenol; halogenated phenols such as fluorophenol, chlorophenol, bromophenol, and iodophenol; substituted monohydric phenols such as p-phenylphenol, aminophenol, nitrophenol, dinitrophenol, and trinitrophenol; and naphthols such as 1-naphthol and 2-naphthol. Further, examples of phenols include divalent or higher phenols such as resorcinol, alkylresorcinol, pyrogallol, catechol, alkylcatechol, hydroquinone, alkylhydroquinone, phloroglucinol, and dihydroxynaphthalene. Further, examples of phenols include bisphenols such as bisphenol F and bisphenol A, and phenol derivatives derived from natural products such as cashew oil. These phenols may be used alone or in combination of two or more.

[0023] Examples of effective aldehydes include formaldehydes such as formaldehyde, paraformaldehyde, and trioxane; acetaldehyde, furfural, and urotropine (hexamethylenetetramine). These aldehydes may be used alone or in combination of two or more.

[0024] The amount of aldehydes may be 10 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of phenols. The molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.

[0025] The phenolic resin may be modified with a modifying agent such as a compound containing a triazine ring, such as melamine, acetoguanamine, benzoguanamine, cyanuric acid, methyl cyanurate, ethyl cyanurate, acetyl cyanurate, or cyanuric chloride; a urea-based compound, such as urea, ethylene urea, or thiourea; dicyandiamide; or guanidine.

[0026] The polysiloxane, phenols, and aldehydes can be reacted by adding a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst as a reaction catalyst. Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, malic acid, paratoluenesulfonic acid, and phenolsulfonic acid. Examples of inorganic acid catalysts include boric acid, phosphoric acid, hydrochloric acid, and sulfuric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.

[0027] R in formula (11) 11In one embodiment, may be a monovalent group having a glycidyl group, is preferably a monovalent group having a glycidoxy group, and is more preferably a group represented by the following formula (11a): In the formula, R a represents an alkylene group, and * represents a bond bonded to the Si atom in formula (11).

[0028] R a The alkylene group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, or 3 or more, and may be 10 or less, 9 or less, or 8 or less.

[0029] R in formula (11) 11 In one embodiment, may be a monovalent group having an alicyclic epoxy group, and is preferably a group represented by the following formula (11b): In the formula, R b represents a single bond or an alkylene group, and * represents a bond bonded to the Si atom in formula (11).

[0030] R b The alkylene group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, or 3 or more, and may be 10 or less, 9 or less, or 8 or less.

[0031] R 12 and R 13 The alkyl groups represented by the formula (I) may each independently be linear or branched. The number of carbon atoms in the alkyl groups may each independently be 1 or more, 5 or less, 4 or less, 3 or less, or 2 or less, or may be 1 or 2. 13 may be the same as each other or may be different from each other.

[0032] Specific examples of the silane compound represented by formula (11) include glycidoxypropyltrimethoxysilane, epoxycyclohexyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 8-glycidoxyoctyltrimethoxysilane.

[0033] The amount of the silane compound represented by formula (11) may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.

[0034] The amount of the silane compound represented by formula (11) may be 7 mol% or more and 62 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. From the viewpoint of obtaining even better compatibility, the amount of the silane compound represented by formula (11) is preferably 10 to 60 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The lower limit of the amount of the silane compound represented by formula (11) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the silane compound represented by formula (11) may be 58 mol%, 56 mol%, or 54 mol%.

[0035] In step (A-1), a catalyst may be used when reacting the phenolic resin with the silane compound represented by formula (11). Specific examples of the catalyst include imidazoles, organic phosphines, and tertiary amines. Examples of imidazoles include 2-methylimidazole, 2-phenylimidazole, 2-phenyl-2-methylimidazole, and 2-heptadecylimidazole. Examples of organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine. Examples of tertiary amines include triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethyl, and tris(dimethylaminomethyl)phenol.

[0036] In step (A-1), in addition to the phenolic resin and the silane compound represented by formula (11), a silane compound other than the silane compound represented by formula (11) may be further reacted. As such a silane compound, a silane compound represented by formula (12) described in step (A-2) below can be used.

[0037] When a silane compound other than the silane compound represented by formula (11) is used, the amount of the silane compound may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.

[0038] The reaction temperature and reaction time in step (A-1) can be appropriately set. The reaction temperature may be, for example, 70° C. or higher and 160° C. or lower. The reaction time may be, for example, 1 hour or higher and 5 hours or lower.

[0039] By the above step (A-1), an intermediate is obtained, which is a reaction product of the phenolic resin and the silane compound represented by formula (11) (and further, a silane compound other than the silane compound represented by formula (11) that is used as needed). More specifically, a hydroxyl group in the phenolic resin and an epoxy group or an alkoxysilyl group in the silane compound represented by formula (11) (Si—OR 13 The hydroxyl group in the phenolic resin may be a phenolic hydroxyl group (a hydroxyl group bonded to an aromatic ring in the phenolic resin), or, when the phenolic resin has a methylol group, may be a hydroxyl group constituting the methylol group.

[0040] Following the step (A-1), the production method A includes a step (A-2) of polycondensing the intermediate obtained in the step (A-1) with a silane compound represented by the following formula (12): In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).

[0041] R 21 The alkyl group represented by the formula (I) may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group may be 1 or more, 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less, or may be 1.

[0042] R 21 The aromatic hydrocarbon group represented by the formula (I) is a monovalent hydrocarbon group having an aromatic ring. Examples of the aromatic hydrocarbon group include an aryl group and an aralkyl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group. Examples of the aralkyl group include a benzyl group and a phenethyl group. When n1 is 2, two R groups present in one molecule are 21 may be the same as each other or may be different from each other.

[0043] R 21 The alkyl portion of the (meth)acryloyloxyalkyl group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkyl portion may be 1 or more, and may be 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, or 3 or less.

[0044] R 22 The alkyl group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkyl group may be 1 or more, 4 or less, 3 or less, or 2 or less, or may be 1. 22 may be the same as each other or may be different from each other.

[0045] In step (A-2), one or more, preferably two or more, silane compounds represented by formula (12) are used. When two or more silane compounds represented by formula (12) are used, R 21 is an alkyl group, or a silane compound 21 is an aryl group, and 21 It is more preferable to combine two or more silane compounds each having an aryl group as an essential component.

[0046] Specific examples of the silane compound represented by formula (12) include silane compounds having an aromatic hydrocarbon group (R 21wherein R is an aromatic hydrocarbon group), silane compounds such as methyltrimethoxysilane, methyltriethoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldi-n-butoxysilane, diethyldimethoxysilane, and methylcyclohexyldimethoxysilane. 21 silane compounds in which all of R 21 a silane compound having a (meth)acryloyloxyalkyl group (R 21 and silane compounds in which the alkyl group is a (meth)acryloyloxyalkyl group.

[0047] The amount of the silane compound represented by formula (12) may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.

[0048] The amount of the silane compound represented by formula (12) may be 38 mol% or more and 93 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). From the viewpoint of obtaining even better compatibility, the amount of the silane compound represented by formula (12) is preferably 40 to 90 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The lower limit of the amount of the silane compound represented by formula (12) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the silane compound represented by formula (12) may be 88 mol%, 86 mol%, or 84 mol%.

[0049] In step (A-2), a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst may be used to promote the reaction (hydrolysis condensation reaction) between the intermediate and the silane compound represented by formula (12). Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, and malic acid. Examples of inorganic acid catalysts include boric acid and phosphoric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.

[0050] In step (A-2), the intermediate and the silane compound represented by formula (12) may be reacted in one step or in multiple steps (for example, two steps). For example, in the case of a two-step reaction, first, the intermediate and the silane compound represented by formula (12) R 21 is an aryl group, and then reacting with a silane compound represented by the formula (12) 21 can be further reacted with a silane compound in which is an alkyl group.

[0051] The reaction temperature and reaction time in step (A-2) can be appropriately set. The reaction temperature may be, for example, 70° C. or higher and 120° C. or lower. The reaction time may be, for example, 1 hour or higher and 5 hours or lower.

[0052] Production method A may further include, after step (A-2), a step (A-3) of distilling the reaction product obtained in step (A-2) under reduced pressure. By step (A-3), for example, methanol and water produced in step (A-2) can be removed.

[0053] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described manufacturing method A. The composite resin will be described in detail later.

[0054] (Production Method B) A method for producing a composite resin according to another embodiment of the present invention (Production Method B) includes a step (step (B-1)) of polycondensing a phenol and an aldehyde in the presence of a polysiloxane having a structural unit represented by the following formula (21) and a structural unit represented by the following formula (22). In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

[0055] R in formula (21) 11 , R 12 and R 13 The details of R in formula (11) explained in the above-mentioned production method A are 11 , R 12 and R 13 are the same as the above. R in formula (22) 21 and R 22 The details of R in formula (21) explained in the above-mentioned production method A are 21 and R 22 are the same as

[0056] A polysiloxane having a structural unit represented by formula (21) and a structural unit represented by formula (22) can be obtained by polycondensing a silane compound represented by formula (11) and a silane compound represented by formula (12), which are described in the above-mentioned production method A, by a known method.

[0057] The polysiloxane has one or more, preferably two or more, structural units represented by formula (22). When the polysiloxane has two or more structural units represented by formula (22), the polysiloxane preferably has one or more structural units represented by formula (22) in which R 21is an alkyl group or a structural unit in which R 21 is an aryl group, and more preferably R 21 is an aryl group.

[0058] The amount of the structural unit represented by formula (21) may be 7 mol% or more and 62 mol% or less, based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). From the viewpoint of obtaining even better compatibility, the amount of the structural unit represented by formula (21) is preferably 10 to 60 mol% based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The lower limit of the amount of the structural unit represented by formula (21) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the structural unit represented by formula (21) may be 58 mol%, 56 mol%, or 54 mol%.

[0059] The amount of the structural unit represented by formula (22) may be 38 mol% or more and 93 mol% or less, based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). From the viewpoint of obtaining even better compatibility, the amount of the structural unit represented by formula (22) is preferably 60 to 90 mol% based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The lower limit of the amount of the structural unit represented by formula (22) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the structural unit represented by formula (22) may be 88 mol%, 86 mol%, or 84 mol%.

[0060] In step (B-1), the polysiloxane is reacted with a phenol and an aldehyde to polycondense the phenol and the aldehyde. As the phenol and the aldehyde, one or more of the phenols and the aldehydes described in the above-mentioned production method A can be used.

[0061] The amount of polysiloxane may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 4,500 parts by mass or less, 4,000 parts by mass or less, or 3,500 parts by mass or less, per 100 parts by mass of the phenols.

[0062] The amount of aldehydes may be 10 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of phenols. When the phenolic resin is a resol-type phenolic resin, the molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.

[0063] In the step (B-1), the following may be used as the modifying agent: a compound containing a triazine ring, such as melamine, acetoguanamine, benzoguanamine, cyanuric acid, methyl cyanurate, ethyl cyanurate, acetyl cyanurate, or cyanuric chloride; a urea-based compound, such as urea, ethylene urea, or thiourea; dicyandiamide; or guanidine.

[0064] In step (B-1), the polysiloxane, phenols, and aldehydes can be reacted by adding a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst as a reaction catalyst. Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, malic acid, paratoluenesulfonic acid, and phenolsulfonic acid. Examples of inorganic acid catalysts include boric acid, phosphoric acid, hydrochloric acid, and sulfuric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.

[0065] The reaction temperature and reaction time in step (B-1) can be appropriately set. The reaction temperature may be, for example, 60° C. or higher and 180° C. or lower. The reaction time may be, for example, 1 hour or higher and 24 hours or lower.

[0066] Production method B may further include, after step (B-1), a step (B-2) of dehydrating the reaction product obtained in step (B-1) under reduced pressure. By step (B-2), for example, water generated in step (B-1) can be removed.

[0067] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described manufacturing method B. The composite resin will be described in detail later.

[0068] (Production Method C) A method for producing a composite resin according to another embodiment of the present invention (production method C) includes a step (step (C-1)) of simultaneously polycondensing a phenol, an aldehyde, a silane compound represented by the above formula (11), and a silane compound represented by the above formula (12).

[0069] Details of the phenols, the silane compound represented by formula (11), and the silane compound represented by formula (12) used in step (C-1) are the same as the details of the phenols, the silane compound represented by formula (11), and the silane compound represented by formula (12) described in production method A.

[0070] Details of the aldehydes are the same as those of the aldehydes described in Production Method A. In this step (C-1), the phenols and the aldehydes are polycondensed to form a phenolic resin, the silane compound represented by Formula (11) and the silane compound represented by Formula (12) are polycondensed to form a polysiloxane, and further, the phenolic resin and the polysiloxane are bonded to each other to form a composite resin.

[0071] The amount of the silane compound represented by formula (11) may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 3,500 parts by mass or less, 3,300 parts by mass or less, or 3,100 parts by mass or less, relative to 100 parts by mass of the phenols.

[0072] The amount of the silane compound represented by formula (12) may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 4,500 parts by mass or less, 4,000 parts by mass or less, or 3,500 parts by mass or less, relative to 100 parts by mass of the phenols.

[0073] The molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.

[0074] The amount of the silane compound represented by formula (11) may be 7 mol% or more and 62 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. From the viewpoint of obtaining even better compatibility, the amount of the silane compound represented by formula (11) is preferably 10 to 60 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The lower limit of the amount of the silane compound represented by formula (11) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the silane compound represented by formula (11) may be 58 mol%, 56 mol%, or 54 mol%.

[0075] The amount of the silane compound represented by formula (12) may be 38 mol% or more and 93 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). From the viewpoint of obtaining even better compatibility, the amount of the silane compound represented by formula (12) is preferably 40 to 90 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The lower limit of the amount of the silane compound represented by formula (12) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the silane compound represented by formula (12) may be 88 mol%, 86 mol%, or 84 mol%.

[0076] In the step (C-1), a catalyst (organic acid catalyst, inorganic acid catalyst, alkali catalyst, etc.) described in the production method A may be used to promote the reaction (hydrolysis condensation reaction).

[0077] The reaction temperature and reaction time in step (C-1) can be appropriately set. The reaction temperature may be, for example, 60° C. or higher and 180° C. or lower. The reaction time may be, for example, 1 hour or higher and 24 hours or lower.

[0078] Production method C may further include, after step (C-1), a step (C-2) of distilling the reaction product obtained in step (C-1) under reduced pressure. By step (C-2), for example, methanol and water produced in step (C-1) can be removed.

[0079] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described production method C. The composite resin will be described in detail later.

[0080] [Composite Resin] One embodiment of the present invention is a composite resin in which a polysiloxane and a phenolic resin are bonded to each other. The polysiloxane has a structural unit represented by the following formula (1A) or (1B) and a structural unit represented by the following formula (2). In the formula, R 11 represents a monovalent group having an epoxy group, R 12 represents an alkyl group, and R 14 represents a linking group, R 15 represents a hydrogen atom or a hydrocarbon group, R 14 and R 15 may be bonded to each other to form a ring, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

[0081] R in formula (1A) 11 and R 12 The details of R in formula (11) explained in the above-mentioned production method A are 11 and R 12 R in formula (1B) is the same as12 The details of R in formula (11) explained in the above-mentioned production method A are 12 R in formula (2) is the same as 21 The details of R in formula (12) explained in the above-mentioned production method A are 21 is the same as

[0082] The phenolic resin is bonded to the polysiloxane via a hydroxyl group contained in the phenolic resin. The hydroxyl group in the phenolic resin may be a phenolic hydroxyl group (a hydroxyl group bonded to an aromatic ring in the phenolic resin), or, if the phenolic resin has a methylol group, may be a hydroxyl group constituting the methylol group.

[0083] In one embodiment, the phenolic resin may be bonded to the structural unit represented by formula (1A) or (1B) via a hydroxyl group, and -(O-*) in the structural unit represented by formula (1A) p2 and -(O-*) in the structural unit represented by formula (1B) may be bonded to a bond of a group represented by formula (1B). p2 and in the structural unit represented by formula (1B), 14 -CH(OH)-CH(R 15 In another embodiment, the phenol resin may be bonded to the structural unit represented by formula (2) via a hydroxyl group, and the —(O-*) in the structural unit represented by formula (2) may be bonded to the bond of the group represented by formula (2). q2 It may be bonded to a bond of a group represented by the following formula:

[0084] The structural unit represented by formula (1B) is a structural unit produced by the reaction of an epoxy group in the silane compound represented by formula (11) or the structural unit represented by formula (21) with a hydroxyl group in the phenol resin. 14 and R 15 is R in formula (11) and formula (21). 11 is a group having a structure corresponding to the structure of

[0085] For example, R in formula (11) and formula (21) 11is a group represented by the above formula (11a), the structural unit represented by formula (1B) becomes a structural unit represented by the following formula (1C) (R 15 is a hydrogen atom). In the formula, R 12 , p1 and p2 are R in formula (1B) 12 , p1 and p2, and R a is R in formula (11a) a and * represents a bond.

[0086] For example, R in formula (11) and formula (21) 11 is a group represented by the above formula (11b), the structural unit represented by formula (1B) becomes a structural unit represented by the following formula (1D) (R 14 and R 15 are bonded to each other to form a ring). In the formula, R 12 , p1 and p2 are R in formula (1B) 12 , p1 and p2, and R b is R in formula (11b). b and * represents a bond.

[0087] In another embodiment, when the phenolic resin has an amino group, the phenolic resin may be bonded to the structural unit represented by formula (1B) via the amino group, and -R 14 -CH(OH)-CH(R 15 )-- may be bonded to a bond of the group represented by *.

[0088] In another embodiment, the polysiloxane has a vinyl group or a (meth)acryloyloxyalkyl group (R 21 is a vinyl group or a (meth)acryloyloxyalkyl group), the phenolic resin may be bonded to the polysiloxane via the vinyl group or the (meth)acryloyloxyalkyl group.

[0089] The polysiloxane has one or more, preferably two or more, structural units represented by formula (2). When the polysiloxane has two or more structural units represented by formula (2), the polysiloxane preferably has one or more structural units represented by formula (2) in which R 21 is an alkyl group or a structural unit in formula (22) 21 is an aryl group, and more preferably R 21 is an aryl group.

[0090] The amount of the structural units represented by formula (1A) or (1B) may be 7 mol% or more and 62 mol% or less, based on the total amount of the structural units represented by formula (1A) or (1B) and the structural units represented by formula (2). From the viewpoint of obtaining even better compatibility, the amount of the structural units represented by formula (1A) or (1B) is preferably 10 to 60 mol% based on the total amount of the structural units represented by formula (1A) or (1B) and the structural units represented by formula (2). The lower limit of the amount of the structural units represented by formula (1A) or (1B) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the structural units represented by formula (1A) or (1B) may be 58 mol%, 56 mol%, or 54 mol%.

[0091] The amount of the structural unit represented by formula (2) may be 38 mol% or more and 93 mol% or less, based on the total amount of the structural unit represented by formula (1A) or (1B) and the structural unit represented by formula (2). From the viewpoint of obtaining even better compatibility, the amount of the structural unit represented by formula (2) is preferably 40 to 90 mol% based on the total amount of the structural unit represented by formula (1A) or (1B) and the structural unit represented by formula (2). The lower limit of the amount of the structural unit represented by formula (2) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the structural unit represented by formula (2) may be 88 mol%, 86 mol%, or 84 mol%.

[0092] In the composite resin, the mass ratio (polysiloxane segment / phenolic resin segment) of the content of the structure derived from the polysiloxane (polysiloxane segment) to the content of the structure derived from the phenolic resin (phenolic resin segment) may be 5 / 95 or more or 10 / 90 or more, and may be 95 / 5 or less, 90 / 10 or less, 80 / 20 or less, or 70 / 30 or less.

[0093] The composite resin described above may be dissolved in a solvent. That is, another embodiment of the present invention is a resin composition containing the composite resin described above and a solvent. The solvent is not particularly limited, and examples thereof include alcohols, ketones, ethers, esters, cellosolves, and aromatic compounds.

[0094] Specific examples of the solvent include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, t-butyl alcohol, benzyl alcohol, 2-methoxyethanol, 2-ethoxyethanol, 2-(methoxymethoxy)ethanol, 2-butoxyethanol, furfuryl alcohol, tetrahydrofurfuryl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, diacetone alcohol, acetone, methyl ethyl ketone, 2-pentanone, 3-pentanone, 2-hexanone, methyl isobutyl ketone, 2-heptanone, 4-heptanone, diisobutyl ketone, cyclohexanone, methylcyclohexanone, acetophenone, and diethyl ether. ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, anisole, tetrahydrofuran, tetrahydropyran, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, glycerin ether, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate Examples of the solvent include butyl, pentyl acetate, isopentyl acetate, 3-methoxybutyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, methyl propionate, ethyl propionate, butyl propionate, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-phenoxyethyl acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, benzene, toluene, and xylene.

[0095] The composite resin can be suitably used in electric and electronic materials such as IC sealing materials and laminates, adhesives, coating agents, inks, and the like.

[0096] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these examples.

[0097] Example A1 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 525 parts by mass of xylenol acid R-2 (a mixture of xylenol isomers, cresol, and ethylphenol, manufactured by Nippon Steel Chemical & Material Co., Ltd.), 386 parts by mass of 50% formalin, and 10.6 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80°C with stirring and reacted at 80°C for 2 hours. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of methyl ethyl ketone (MEK) was added to obtain 1,000 parts by mass of a phenolic resin a1 solution having a nonvolatile content of 60.0% by mass.

[0098] Subsequently, 500 parts by mass of the phenolic resin a1, 189 parts by mass of glycidoxypropyltrimethoxysilane (GPTMS), and 1.0 part by mass of 1,2-dimethylimidazole were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, and the mixture was stirred for 3 hours to obtain an intermediate.

[0099] Next, the mixture was cooled to 70°C, and 114 parts by mass of phenyltrimethoxysilane (PTMS), 93 parts by mass of dimethyldimethoxysilane (DMDMS), and 49 parts by mass of methyltrimethoxysilane (MTMS) were added to the reaction vessel. 21 The proportion of silane compounds in which the aryl group was 22 mol%. A mixture of 0.9 parts by mass of butyl acid phosphate and 40 parts by mass of deionized water was then added dropwise over 30 minutes, followed by stirring at the same temperature for 5 hours to allow a hydrolysis-condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 6 hours to remove the produced methanol and water. Then, 90 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A1 with a nonvolatile content of 60.1% by mass.

[0100] Example A2 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 521 parts by mass of phenol, 16 parts by mass of melamine, 466 parts by mass of 50% formalin, and 20.8 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80° C. with stirring and reacted for 2 hours at 80° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 384 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of phenolic resin a2 having a nonvolatile content of 60.0% by mass.

[0101] Subsequently, 500 parts by mass of the phenolic resin a2, 174 parts by mass of GPTMS, and 0.5 parts by mass of triphenylphosphine (TPP) were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 85°C with stirring, and the mixture was stirred for 2 hours to obtain an intermediate.

[0102] Next, the mixture was cooled to 75° C., and 182 parts by mass of PTMS and 94 parts by mass of DMDMS were added to the reaction vessel. 21 The proportion of silane compounds in which the aryl group was 38 mol%. A mixture of 0.8 parts by mass of butyl acid phosphate and 60 parts by mass of deionized water was then added dropwise over one hour, followed by stirring at the same temperature for four hours to allow a hydrolysis-condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for eight hours to remove the produced methanol and water. Then, 80 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A2 with a nonvolatile content of 60.0% by mass.

[0103] (Example A3) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 702 parts by mass of phenol, 113 parts by mass of benzoguanamine, 324 parts by mass of 50% formalin, and 1.4 parts by mass of triethylamine. The mixture was heated to 100 ° C. with stirring, reacted at 100 ° C. for 5 hours, and then heated to 120 ° C. while removing water under normal pressure. Next, the mixture was reacted under reflux for 2 hours, and then heated to 160 ° C. while removing water under normal pressure. After further reacting under reflux for 3 hours, the mixture was heated to 180 ° C. while removing water under normal pressure. Next, under a reduced pressure of 10 to 300 kPa, dephenolization was performed under reduced pressure, and 430 parts by mass of MEK was added to obtain 1,000 parts by mass of a phenolic resin a3 solution having a nonvolatile content of 60.0% by mass.

[0104] Next, 500 parts by mass of the phenolic resin a3, 209 parts by mass of GPTMS, and 1.0 part by mass of TPP were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, and the mixture was stirred for 3 hours to obtain an intermediate.

[0105] Next, the mixture was cooled to 70°C, and 21 parts by mass of PTMS and 134 parts by mass of DMDMS were added to the reaction vessel. Then, a mixture of 0.8 parts by mass of butyl acid phosphate and 60 parts by mass of deionized water was added dropwise over 2 hours. Then, 80 parts by mass of MTMS was added, and the mixture was stirred at the same temperature for 4 hours to carry out a hydrolysis and condensation reaction, thereby obtaining a reaction product. The amount of the silane compound represented by the formula (12) and R 21 The proportion of silane compounds in which the aryl group is 8 mol % was then 8. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 7 hours to remove the produced methanol and water, and then 90 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A3 having a nonvolatile content of 60.1% by mass.

[0106] Example A4 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 292 parts by mass of phenol, 292 parts by mass of 2-naphthol, 430 parts by mass of 50% formalin, and 19.3 parts by mass of 25% aqueous ammonia, and the temperature was raised to 80°C with stirring, and the reaction was carried out at 80°C for 2 hours. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of phenolic resin a4 having a nonvolatile content of 60.0% by mass.

[0107] Subsequently, 500 parts by mass of the phenolic resin a4, 194 parts by mass of GPTMS, and 1.2 parts by mass of triethylamine (TEA) were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, and the mixture was stirred for 3 hours to obtain an intermediate.

[0108] Next, the mixture was cooled to 70°C, and 120 parts by mass of PTMS was added to the reaction vessel. Thereafter, a mixture of 1.0 part by mass of butyl acid phosphate and 60 parts by mass of deionized water was added dropwise over 2 hours. Thereafter, 121 parts by mass of MTMS was added, and the mixture was stirred at the same temperature for 4 hours to carry out a hydrolysis condensation reaction, thereby obtaining a reaction product. Note that, based on the total amount of the silane compound, the amount of the silane compound represented by the above formula (12), R 21 The proportion of silane compounds in which the aryl group is present was 22 mol %. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 6 hours to remove the produced methanol and water, and then 60 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A4 with a nonvolatile content of 60.0% by mass.

[0109] Example A5 500 parts by mass of each of phenol resin a1 and phenol resin a2 were mixed to obtain 1,000 parts by mass of a solution of phenol resin a5 having a nonvolatile content of 60.0% by mass.

[0110] Subsequently, 500 parts by mass of the phenolic resin a5, 226 parts by mass of GPTMS, and 0.9 parts by mass of TPP were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, followed by stirring for 3 hours to obtain an intermediate.

[0111] The mixture was then cooled to 75°C, and 152 parts by weight of DMDMS was added to the reaction vessel. A mixture of 0.7 parts by weight of butyl acid phosphate and 55 parts by weight of deionized water was then added dropwise over 2 hours. 66 parts by weight of MTMS was then added, and the mixture was stirred at the same temperature for 3 hours to carry out a hydrolysis-condensation reaction, yielding a reaction product. The reaction product was then distilled under a reduced pressure of 10 to 300 kPa at 60 to 80°C for 7 hours to remove the produced methanol and water. 55 parts by weight of MEK was then added, yielding 1,000 parts by weight of a solution of composite resin A5 with a nonvolatile content of 60.0% by weight.

[0112] Example A6 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 480 parts by mass of 3,5-xylenol, 274 parts by mass of 50% formalin, and 9.3 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80° C. with stirring and reacted at 80° C. for 2 hours. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 384 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of phenolic resin a6 having a nonvolatile content of 60.0% by mass.

[0113] Subsequently, 500 parts by mass of the phenolic resin a6, 224 parts by mass of GPTMS, 135 parts by mass of DMDMS, and 1.0 part by mass of 1,2-dimethylimidazole were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 90°C with stirring, and the mixture was stirred for 3 hours to obtain an intermediate.

[0114] Next, the mixture was cooled to 70° C., and 89 parts by mass of PTMS was added to the reaction vessel. 21The proportion of silane compounds in which the aryl group was 18 mol% was obtained. A mixture of 0.7 parts by mass of butyl acid phosphate and 55 parts by mass of deionized water was then added dropwise over two hours. The mixture was then stirred at the same temperature for an additional five hours to allow a hydrolysis-condensation reaction, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for seven hours to remove the produced methanol and water. Then, 63 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A6 with a nonvolatile content of 60.1% by mass.

[0115] Example A7 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 513 parts by mass of m-cresol, 393 parts by mass of 50% formalin, and 12.7 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80° C. with stirring and reacted at 80° C. for 2 hours. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 375 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of phenolic resin a7 having a nonvolatile content of 60.0% by mass.

[0116] Subsequently, 500 parts by mass of the phenolic resin a7, 218 parts by mass of GPTMS, 122 parts by mass of DMDMS, and 1.0 part by mass of TPP were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 85°C with stirring, followed by stirring for 2 hours to obtain an intermediate.

[0117] The mixture was then cooled to 75°C, and 102 parts by weight of MTMS was added to the reaction vessel. A mixture of 1.0 part by weight of butyl acid phosphate and 50 parts by weight of deionized water was then added, and the mixture was stirred at the same temperature for 5 hours to carry out a hydrolysis-condensation reaction, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 10 hours to remove the produced methanol and water. Then, 70 parts by weight of MEK was added, yielding 1,000 parts by weight of a solution of composite resin A7 with a nonvolatile content of 60.0% by weight.

[0118] Example A8 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 536 parts by mass of phenol, 32 parts by mass of urea, 477 parts by mass of 50% formalin, and 21.4 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80° C. with stirring and reacted for 2 hours at 80° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 384 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of phenolic resin a8 having a nonvolatile content of 60.0% by mass.

[0119] Subsequently, 500 parts by mass of the phenolic resin a8, 199 parts by mass of GPTMS, 101 parts by mass of DMDMS, and 1.0 part by mass of TPP were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, followed by stirring for 3 hours to obtain an intermediate.

[0120] Next, the mixture was cooled to 70°C, and 83 parts by mass of PTMS was added to the reaction vessel. Thereafter, a mixture of 0.8 parts by mass of butyl acid phosphate and 40 parts by mass of deionized water was added, and the mixture was stirred for 2 hours. Thereafter, 61 parts by mass of MTMS was added, and the mixture was further stirred at the same temperature for 3 hours to carry out a hydrolysis condensation reaction, thereby obtaining a reaction product. Note that, based on the total amount of the silane compound, the amount of the silane compound represented by the above formula (12), R 21 The proportion of silane compounds in which the aryl group is present was 15 mol %. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 9 hours to remove the produced methanol and water, and then 100 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin A8 with a nonvolatile content of 60.0% by mass.

[0121] Example A9 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 950 parts by mass of the phenolic resin a6, 21 parts by mass of GPTMS, 17 parts by mass of DMDMS, and 1.0 part by mass of 1,2-dimethylimidazole, and the temperature in the system was raised to 90°C with stirring. The mixture was then stirred for 3 hours to obtain an intermediate.

[0122] The mixture was then cooled to 70°C, and 7 parts by weight of MTMS was added to the reaction vessel. A mixture of 0.3 parts by weight of butyl acid phosphate and 10 parts by weight of deionized water was then added dropwise over 2 hours. The mixture was then stirred at the same temperature for an additional 5 hours to allow a hydrolysis-condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under a reduced pressure of 10 to 300 kPa at 60 to 80°C for 7 hours to remove the produced methanol and water. Then, 10 parts by weight of MEK was added, yielding 1,000 parts by weight of a solution of composite resin A9 with a nonvolatile content of 60.0% by weight.

[0123] Example A10 50 parts by mass of the phenolic resin a6, 396 parts by mass of GPTMS, 330 parts by mass of DMDMS, and 0.2 parts by mass of 1,2-dimethylimidazole were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature in the system was raised to 90°C with stirring, and the mixture was stirred for 3 hours to obtain an intermediate.

[0124] The mixture was then cooled to 70°C, and 136 parts by weight of MTMS was added to the reaction vessel. A mixture of 2.3 parts by weight of butyl acid phosphate and 240 parts by weight of deionized water was then added dropwise over 2 hours. The mixture was then stirred at the same temperature for an additional 5 hours to allow a hydrolysis-condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under a reduced pressure of 10 to 300 kPa at 60 to 80°C for 7 hours to remove the produced methanol and water. Then, 250 parts by weight of MEK was added, yielding 1,000 parts by weight of a solution of composite resin A10 with a nonvolatile content of 60.0% by weight.

[0125] Example B1 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 100 parts by mass of n-butyl acetate, 108 parts by mass of GPTMS, 372 parts by mass of PTMS, 198 parts by mass of DMDMS, and 226 parts by mass of MTMS. Thereafter, the temperature in the system was raised to 80° C. with stirring, and a mixture of 3 parts by mass of acetic acid and 60 parts by mass of deionized water was added. Note that, based on the total amount of the silane compounds, the amount of n-butyl acetate represented by the above formula (22), R 21The proportion of silane compounds in which the aryl group was present was 30 mol %. The mixture was then stirred at the same temperature for 10 hours to allow a hydrolysis and condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 8 hours to remove the produced methanol and water, and then 420 parts by mass of n-butyl acetate was added to obtain 1,000 parts by mass of a solution of polysiloxane b1 with a nonvolatile content of 60.0% by mass.

[0126] Subsequently, 496 parts by mass of xylenol acid R-2, 292 parts by mass of 50% formalin, 200 parts by mass of the polysiloxane b1, and 9.9 parts by mass of 25% aqueous ammonia were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature was raised to 80° C. with stirring, and the reaction was carried out at 80° C. for 2 hours. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B1 having a nonvolatile content of 60.0% by mass.

[0127] (Example B2) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube and a nitrogen gas inlet was charged with 120 parts by mass of isopropyl alcohol (IPA), 213 parts by mass of GPTMS, 338 parts by mass of PTMS, 186 parts by mass of DMDMS, and 163 parts by mass of MTMS. Then, the temperature in the system was raised to 80 ° C. with stirring, and a mixture of 4 parts by mass of acetic acid and 120 parts by mass of deionized water was added. Note that, based on the total amount of the silane compound, the amount of the silane compound represented by the formula (22) and R 21 The proportion of silane compounds in which the aryl group was present was 30 mol %. The mixture was then stirred at the same temperature for 10 hours to allow a hydrolysis and condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 8 hours to remove the produced methanol and water, and 430 parts by mass of IPA was then added to obtain 1,000 parts by mass of a solution of polysiloxane b2 with a nonvolatile content of 60.1% by mass.

[0128] Next, the same operation as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b2, to obtain a solution of composite resin B2.

[0129] (Example B3) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 100 parts by mass of MEK, 425 parts by mass of GPTMS, and 330 parts by mass of DMDMS. Then, the temperature in the system was raised to 75 ° C. with stirring, and a mixture of 1 part by mass of butyl acid phosphate and 160 parts by mass of deionized water was added dropwise over 1 hour. Thereafter, 194 parts by mass of MTMS was added, and the mixture was stirred at the same temperature for 4 hours to cause a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of polysiloxane b3 having a nonvolatile content of 60.0% by mass.

[0130] Next, the same procedure as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b3, to obtain a solution of composite resin B3.

[0131] (Example B4) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 100 parts by mass of n-butyl acetate, 524 parts by mass of GPTMS, 200 parts by mass of DMDMS, and 214 parts by mass of MTMS. Then, the temperature in the system was raised to 85 ° C. with stirring, and a mixture of 3 parts by mass of butyl acid phosphate and 200 parts by mass of deionized water was added dropwise over 2 hours. Then, the mixture was stirred at the same temperature for 6 hours to cause a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 400 parts by mass of n-butyl acetate was added. 1,000 parts by mass of a solution of polysiloxane b4 having a non-volatile content of 60.2% by mass was obtained.

[0132] Next, the same operation as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b4, to obtain a solution of composite resin B4.

[0133] (Example B5) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 180 parts by mass of MEK, 524 parts by mass of GPTMS, 200 parts by mass of DMDMS, and 214 parts by mass of MTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 5 parts by mass of TEA and 200 parts by mass of deionized water was added dropwise over 2 hours. The mixture was then stirred at the same temperature for 6 hours to allow a hydrolysis-condensation reaction to occur, resulting in a reaction product. The reaction product was then distilled under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. for 10 hours to remove the produced methanol and water. Then, 350 parts by mass of MEK was added, and 1,000 parts by mass of a solution of polysiloxane b5 having a nonvolatile content of 60.0% by mass was obtained.

[0134] Next, the same operation as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b5, to obtain a solution of composite resin B5.

[0135] (Example B6) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 425 parts by mass of GPTMS and 330 parts by mass of DMDMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 0.8 parts by mass of butyl acid phosphate and 250 parts by mass of deionized water was added dropwise over 2 hours. Thereafter, 136 parts by mass of MTMS was added, and the mixture was stirred at the same temperature for 3 hours to cause a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 9 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 550 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of polysiloxane b6 having a nonvolatile content of 60.0% by mass.

[0136] Subsequently, 583 parts by mass of 3,5-xylenol, 343 parts by mass of 50% formalin, 50 parts by mass of the polysiloxane b6, and 11.6 parts by mass of 25% aqueous ammonia were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the temperature was raised to 80° C. with stirring, and the reaction was carried out at 80° C. for 2 hours. Next, dehydration was carried out under a reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B6 having a nonvolatile content of 60.0% by mass.

[0137] Example B7 The same synthesis operation as in Example B6 (Composite Resin B6) was performed, except that the charges after obtaining the polysiloxane b6 were changed to 434 parts by mass of 3,5-xylenol, 256 parts by mass of 50% formalin, 300 parts by mass of the polysiloxane b6, and 8.7 parts by mass of 25% aqueous ammonia, to obtain 1,000 parts by mass of a solution of Composite Resin B7.

[0138] Example B8 The same synthesis operation as in Example B6 (Composite Resin B6) was performed, except that the charges after obtaining the polysiloxane b6 were changed to 186 parts by mass of 3,5-xylenol, 110 parts by mass of 50% formalin, 700 parts by mass of the polysiloxane b6, and 3.7 parts by mass of 25% aqueous ammonia, to obtain 1,000 parts by mass of a solution of Composite Resin B8.

[0139] Example B9 The same synthesis operation as in Example B6 (Composite Resin B6) was performed, except that the charges after obtaining the polysiloxane b6 were changed to 31 parts by mass of 3,5-xylenol, 18 parts by mass of 50% formalin, 950 parts by mass of the polysiloxane b6, and 0.6 parts by mass of 25% aqueous ammonia, to obtain 1,000 parts by mass of a solution of Composite Resin B9.

[0140] Example B10 100 parts by mass of n-butyl acetate, 158 parts by mass of GPTMS, 662 parts by mass of PTMS, and 92 parts by mass of DMDMS were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, and the temperature in the system was then raised to 75° C. with stirring, and a mixture of 3 parts by mass of acetic acid and 60 parts by mass of deionized water was added. 21The proportion of silane compounds in which the aryl group was present was 70 mol %. The mixture was then stirred at the same temperature for 10 hours to allow a hydrolysis and condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 5 hours to remove the produced methanol and water, and then 410 parts by mass of n-butyl acetate was added to obtain 1,000 parts by mass of a solution of polysiloxane b10 with a nonvolatile content of 60.0% by mass.

[0141] Next, the same operation as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b10, to obtain a solution of composite resin B10.

[0142] (Example B11) Into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, 140 parts by mass of IPA, 152 parts by mass of GPTMS, 620 parts by mass of PTMS, and 144 parts by mass of DMDMS were charged, and then the temperature in the system was raised to 70°C with stirring, and a mixture of 5 parts by mass of acetic acid and 130 parts by mass of deionized water was added. Note that, based on the total amount of the silane compound, the amount of the silane compound represented by the formula (22) and R 21 The proportion of silane compounds in which the aryl group was present was 60 mol %. The mixture was then stirred at the same temperature for 10 hours to allow a hydrolysis and condensation reaction to occur, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 7 hours to remove the produced methanol and water, and then 420 parts by mass of IPA was added to obtain 1,000 parts by mass of a solution of polysiloxane b11 with a nonvolatile content of 60.1% by mass.

[0143] Next, the same operation as in Example B1 (composite resin B1) was carried out except that the polysiloxane b1 was changed to polysiloxane b11, to obtain a solution of composite resin B11.

[0144] (Example C1) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 142 parts by mass of GPTMS, 111 parts by mass of DMDMS, 65 parts by mass of MTMS, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80 ° C. with stirring and reacted for 2 hours at 80 ° C. Next, dehydration was performed under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin C1 having a non-volatile content of 60.0% by mass.

[0145] Example C2 A solution of composite resin C2 was obtained by the same operation as in Example C1 (composite resin C1), except that 143 parts by mass of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 107 parts by mass of DMDMS, and 44 parts by mass of MTMS were charged instead of 142 parts by mass of GPTMS, 111 parts by mass of DMDMS, and 65 parts by mass of MTMS.

[0146] Example C3 The same operation as in Example C1 (composite resin C1) was performed except that 142 parts by mass of GPTMS, 111 parts by mass of DMDMS, and 65 parts by mass of MTMS were replaced with 100 parts by mass of MEK, 139 parts by mass of 3-glycidoxypropylmethyldimethoxysilane, 116 parts by mass of DMDMS, and 48 parts by mass of MTMS, to obtain a solution of composite resin C2.

[0147] Example C4 A solution of composite resin C4 was obtained by the same operation as in Example C1 (composite resin C1), except that 120 parts by mass of IPA, 152 parts by mass of 8-glycidoxyoctyltrimethoxysilane, 90 parts by mass of DMDMS, and 38 parts by mass of MTMS were added instead of 142 parts by mass of GPTMS, 111 parts by mass of DMDMS, and 65 parts by mass of MTMS.

[0148] (Example C5) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 25 parts by mass of GPTMS, 15 parts by mass of DMDMS, 10 parts by mass of MTMS, 583 parts by mass of 3,5-xylenol, 343 parts by mass of 50% formalin, and 11.6 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80 ° C. with stirring and reacted for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin C5 having a nonvolatile content of 60.0% by mass.

[0149] Example C6 A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 468 parts by mass of GPTMS, 285 parts by mass of DMDMS, 197 parts by mass of MTMS, 31 parts by mass of 3,5-xylenol, and 18 parts by mass of 50% formalin, and the mixture was heated to 80° C. with stirring and reacted for 2 hours at 80° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin C6 having a nonvolatile content of 60.0% by mass.

[0150] (Comparative Example D1) 500 parts by mass of the phenolic resin a2, 47 parts by mass of PTMS, 298 parts by mass of DMDMS, and 1.0 part by mass of TPP were charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, and the temperature in the system was raised to 80°C with stirring, and stirred for 3 hours. Then, the system was cooled to 70°C, and 119 parts by mass of MTMS was added to the reaction vessel. Note that, based on the total amount of the silane compound, the amount of the phenolic resin a2 represented by the formula (12) and R 21 The proportion of silane compounds in which the aryl group was 6 mol% was obtained. A mixture of 0.8 parts by mass of butyl acid phosphate and 60 parts by mass of deionized water was then added and stirred for 6 hours to carry out a hydrolysis-condensation reaction, yielding a reaction product. The reaction product was then distilled under reduced pressure of 10 to 300 kPa at 60 to 80°C for 6 hours to remove the produced methanol and water. 50 parts by mass of MEK was then added to obtain 1,000 parts by mass of a solution of composite resin D1 with a nonvolatile content of 60.1% by mass.

[0151] Comparative Example D2 The phenol resin a2 obtained in Example A2 was used alone.

[0152] (Comparative Example D3) A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 523 parts by mass of GPTMS and 182 parts by mass of DMDMS. Thereafter, a mixture of 0.9 parts by mass of butyl acid phosphate and 40 parts by mass of deionized water was added dropwise over 2 hours, and 168 parts by mass of MTMS was added. The mixture was stirred at the same temperature for 5 hours to carry out a hydrolysis-condensation reaction, yielding a reaction product. The reaction product was then distilled under a reduced pressure of 10 to 300 kPa at 60 to 80°C for 6 hours to remove the produced methanol and water. Then, 450 parts by mass of MEK was added to obtain 1,000 parts by mass of a polysiloxane solution with a nonvolatile content of 60.1% by mass.

[0153] (Comparative Example D4) 500 parts by mass of the phenolic resin a2 and 500 parts by mass of the polysiloxane obtained in Comparative Example D3 were added to a reaction vessel equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet, and the mixture was mixed and stirred at room temperature to obtain 1,000 parts by mass of a mixed resin solution having a non-volatile content of 60.0% by mass.

[0154] [Heat Resistance] Each of the obtained resin solutions was applied to a glass substrate (JIS R3202) so that the dry film thickness was 20 μm, and dried at 150°C for 30 minutes. The dried coating film was subjected to TG-DTA measurement, and the weight loss percentage at 300°C was calculated. Heat resistance was evaluated according to the following criteria. A lower weight loss value indicates better heat resistance. E: Weight loss of 0% or more but less than 10% S: Weight loss of 10% or more but less than 12% A: Weight loss of 12% or more but less than 15% B: Weight loss of 15% or more but less than 30% C: Weight loss of 30% or more

[0155] [Flexibility] Each of the obtained resin solutions was applied to a tinplate substrate (JIS G3303) so that the dry film thickness was 10 μm, and a cupping resistance test was performed in accordance with JIS K5600-5-2. The indentation depth (mm) at which cracks or peeling occurred in the coating film was recorded. The greater this depth, the greater the flexibility, and to achieve sufficient flexibility, a depth of 15 mm or more is preferred.

[0156] [Scratch Resistance] Each of the obtained resin solutions was applied to a glass substrate (JIS R3202) so that the dry film thickness was 10 μm, and dried at 150° C. for 30 minutes. The surface of the dried coating film was rubbed with #0000 steel wool under a load of 500 g. The haze values ​​before and after rubbing with the steel wool were measured, and the difference ΔH (%) between these haze values ​​was calculated. The scratch resistance was evaluated according to the following criteria. The smaller the difference ΔH (%) in haze values, the more excellent the scratch resistance (less susceptible to scratches). A: ΔH (%) is 0% or more and less than 10% B: ΔH (%) is 10% or more and less than 30% C: ΔH (%) is 30% or more

[0157] [Evaluation of Compatibility] Immediately after each resin solution was obtained, the appearance of the solution was observed and the compatibility was evaluated using the following criteria: A: The solution had a uniform appearance and no turbidity was observed. B: The solution had a uniform appearance, but turbidity was observed. C: Phase separation and significant turbidity were observed in the appearance of the solution.

[0158] [Evaluation of storage stability] The obtained resin solution was placed in a glass bottle and allowed to stand in an environment of 15°C for 30 days, after which the appearance of the solution was visually observed and the storage stability was evaluated using the following index. The absence of turbidity, sediment formation, or phase separation indicates excellent storage stability. A: No change in the appearance of the resin solution. B: Slight turbidity and sediment formation were observed. C: Significant turbidity, sediment formation, and phase separation were observed.

[0159] [Evaluation of coating film appearance] The obtained resin solution was applied to a glass substrate (JIS R3202) so that the dry film thickness was 20 μm, and dried at 150° C. for 30 minutes. The appearance of the coating film after drying was observed visually, and the coating film appearance was evaluated according to the following criteria: A: No abnormalities or whitening were observed. B: Slight abnormalities or whitening were observed. C: Significant abnormalities or whitening were observed.

[0160] The results of the above evaluations are shown in Tables 1 to 6. Tables 1 to 6 also show the mass ratio of the polysiloxane segment content to the phenol resin segment content in the composite resin (denoted as "PSi / Ph"), and the content (mol %) of the epoxy silane compound in the total amount of silane compounds.

[0161]

[0162]

[0163]

[0164]

[0165]

[0166]

[0167] As described above, in Examples A1 to A10 in which composite resins were produced by Production Method A, Examples B1 to B11 in which composite resins were produced by Production Method B, and Examples C1 to C6 in which composite resins were produced by Production Method C, by using a silane compound having an epoxy group and a hydrolyzable silyl group as a polysiloxane raw material, a composite resin excellent in heat resistance, flexibility, and scratch resistance could be obtained. In contrast, Comparative Example D1, which does not use a silane compound having an epoxy group and a hydrolyzable silyl group as a polysiloxane raw material, Comparative Example D2, which uses a phenolic resin a2 to which no polysiloxane is bonded, Comparative Example D3, which uses a polysiloxane to which no phenolic resin is bonded, and Comparative Example D4, which uses a mixture of phenolic resin and polysiloxane (a simple mixture, not a composite resin), were inferior in at least one of heat resistance, flexibility, and scratch resistance. Furthermore, the composite resins of each example were also excellent in terms of compatibility, storage stability, and coating appearance.

Claims

1. A composite resin in which a polysiloxane and a phenolic resin are bonded to each other, wherein the polysiloxane has a structural unit represented by the following formula (1A) or (1B) and a structural unit represented by the following formula (2), and the phenolic resin is bonded to the polysiloxane via a hydroxyl group possessed by the phenolic resin. [In the formula, R 11 represents a monovalent group having an epoxy group, R 12 represents an alkyl group, R 14 represents a linking group, R 15 represents a hydrogen atom or a hydrocarbon group; R 14 and R 15 may be bonded to each other to form a ring, p1 and p2 represent either (p1, p2) = (0, 1) or (1, 0), and * represents a bond. [In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

2. The composite resin according to claim 1, wherein the amount of the structural unit represented by the formula (1A) or (1B) is 10 to 60 mol % based on the total amount of the structural unit represented by the formula (1A) or (1B) and the structural unit represented by the formula (2).

3. The composite resin according to claim 1 or 2, wherein the phenolic resin is bonded to the structural unit represented by formula (1A) or (1B).

4. A method for producing a composite resin, comprising: a step of reacting a phenolic resin with a silane compound represented by the following formula (11) to obtain an intermediate; and a step of polycondensing the intermediate with a silane compound represented by the following formula (12). [In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 each represent (m1, m2)=(0, 3) or (1, 2). [In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).

5. A method for producing a composite resin, comprising a step of polycondensing a phenol and an aldehyde in the presence of a polysiloxane having a structural unit represented by the following formula (21) and a structural unit represented by the following formula (22): [In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. [In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.

6. A method for producing a composite resin, comprising a step of polycondensing a phenol, an aldehyde, a silane compound represented by the following formula (11), and a silane compound represented by the following formula (12) all at once. [In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 each represent (m1, m2)=(0, 3) or (1, 2). [In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).

7. The method according to claim 4 or 6, wherein the amount of the silane compound represented by the formula (11) is 10 to 60 mol % based on the total amount of the silane compound represented by the formula (11) and the silane compound represented by the formula (12).

8. The method according to claim 5, wherein the amount of the structural unit represented by the formula (21) is 10 to 60 mol % based on the total amount of the structural unit represented by the formula (21) and the structural unit represented by the formula (22).

Citation Information

Patent Citations

  • Organosilicon epoxy monomer modified phenolic resin and preparation method thereof

    CN111087564A

  • Preparation of phenol resin

    JP1989004612A

  • Hybrid compound, resist material and method of forming pattern

    JP2003119344A

  • Silicone-modified novolak phenolic resin for being compounded into rubber

    JP2003268062A

  • Epoxy-functional polysiloxane modified phenolic resin compositions and composites

    WO2001062829A1