Biodegradable resin composition, molded article, and methods for producing same
Incorporating polyarylene sulfide with a specific molecular weight into biodegradable resin compositions addresses the stability and biodegradability challenges of conventional resins by maintaining stability in dark conditions and promoting decomposition under UV exposure, achieving balanced storage and degradation performance.
Patent Information
- Application Number
- PCT/JP2024/014627
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional biodegradable resins face issues with stability in the dark and limited decomposition promotion, leading to premature deterioration and inadequate biodegradability, especially when not exposed to ultraviolet irradiation.
Incorporating polyarylene sulfide (PAS) with a weight average molecular weight of 120,000 or less into biodegradable resin compositions, which acts as a biodegradation accelerator, enhancing stability in dark conditions and promoting decomposition under ultraviolet irradiation.
The biodegradable resin compositions exhibit high stability in dark environments and excellent decomposition properties when exposed to ultraviolet rays, effectively balancing storage stability and degradation efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Biodegradable resin composition, molded article, and method for producing the same
[0001] The present invention relates to a biodegradable resin composition, a molded article, and a method for producing the same.
[0002] In recent years, from the viewpoint of preventing environmental pollution, the use of biodegradable resins has been actively studied in a wide range of fields. Conventionally, biodegradable resins such as polylactic acid, polyester resins, and polyamide resins have been known, but the speed and rate of biodegradation of these resins vary depending on their structure. In addition, depending on the soil and climate in which they are used, their biodegradability may not be fully realized, resulting in poor decomposition.
[0003] To solve these problems, a technique for controlling decomposition by blending various degradation accelerators with biodegradable resins is known. For example, Patent Document 1 discloses a resin composition in which polylactic acid and polybutylene succinate are blended with polysaccharides such as starch, cellulose, and chitin. Patent Document 2 discloses a biodegradable resin composition blended with a biodegradation accelerator containing polysaccharides and / or monosaccharides with a xylose content of 15% by mass or more. Patent Document 3 discloses a biodegradable resin composition to which 0.1 to 50 parts by weight of a polymer (oligomer) of a 3-hydroxyalkanoic acid (e.g., 3-hydroxybutyric acid) has been added.
[0004] JP 11-241009 A JP 2022-21326 A JP 2018-16720 A
[0005] However, conventional biodegradation accelerators accelerate the degradation of biodegradable resins even in environments other than those exposed to ultraviolet light, and therefore exert their function during transportation and storage of the final product made of the biodegradable resin composition before use. This has been problematic because the final product deteriorates even before use, shortening the quality assurance period. Furthermore, the degree of improvement in degradation acceleration has been limited.
[0006] Therefore, the problem to be solved by the present invention is to provide a biodegradable resin composition and molded article that are highly stable when not irradiated with ultraviolet light and exhibit excellent decomposition effects when irradiated with ultraviolet light, as well as methods for producing the same.
[0007] As a result of intensive research to solve the above-mentioned problems, the inventors have found that by incorporating polyarylene sulfide (hereinafter referred to as PAS) having a specific weight-average molecular weight as a biodegradation promoter into a biodegradable resin, it is possible to achieve both excellent stability in dark places and excellent decomposition promotion properties under ultraviolet irradiation, and have thus completed the present invention.
[0008] That is, the present disclosure relates to a biodegradable resin composition comprising a biodegradable resin (A) having at least an ester bond or an amide bond in the main chain and a biodegradation promoter (B) as essential components, wherein the biodegradation promoter (B) contains a PAS having a weight-average molecular weight of 120,000 or less.
[0009] The present disclosure also relates to a molded article obtained by melt molding the biodegradable resin composition described above.
[0010] The present disclosure also relates to a method for producing a biodegradable resin composition, comprising a step of blending, as essential components, a biodegradable resin (A) having at least an ester bond or an amide bond in its main chain and a biodegradation accelerator (B), and melt-kneading the mixture at a temperature equal to or higher than the melting point of the biodegradable resin (A), wherein the biodegradation accelerator (B) contains a PAS having a weight-average molecular weight of 120,000 or less.
[0011] The present disclosure also relates to a method for producing a molded article, which comprises a step of melt-molding the biodegradable resin composition produced by the method described above.
[0012] In this disclosure, a dark place refers to an environment where ultraviolet rays are blocked, i.e., an environment where ultraviolet rays are not irradiated, such as the inside of a transport vehicle or a storage warehouse, or a state where the product is packaged in a material that does not transmit ultraviolet rays.
[0013] According to the present invention, it is possible to provide a biodegradable resin composition and molded article that are highly stable when stored in a dark place and exhibit an excellent decomposition-accelerating effect when irradiated with ultraviolet light, as well as methods for producing the same.
[0014] Hereinafter, an embodiment of the present disclosure will be described in detail, but the scope of the present disclosure is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present disclosure. Furthermore, when multiple upper and lower limit values are described for a specific parameter, any upper and lower limit values can be combined to form a suitable numerical range.
[0015] <Biodegradable Resin Composition> The biodegradable resin composition according to this embodiment comprises a biodegradable resin (A) having at least an ester bond or an amide bond in the main chain and a biodegradation promoter (B) blended as essential components.
[0016] Biodegradable Resin (A) The biodegradable resin composition according to this embodiment contains, as an essential component, a biodegradable resin (A) having at least an ester bond or an amide bond in the main chain (hereinafter, sometimes simply referred to as biodegradable resin (A)). There are no particular limitations on the biodegradable resin (A) as long as it does not impair the effects of the present invention, and known resins can be used. For example, poly(α-hydroxycarboxylic acids) such as polyglycolic acid and polylactic acid or copolymers thereof; poly(ω-hydroxyalkanoates) such as poly(ε-caprolactone); aliphatic polyesters such as polyethylene succinate, polybutylene succinate, polybutylene adipate, and polybutylene succinate lactate obtained by polycondensation of a glycol having 2 to 12 carbon atoms with an aliphatic dicarboxylic acid having 2 to 12 carbon atoms; and poly(butylene adipate / terephthalate) copolymers and poly(butylene adipate / isophthalate) copolymers obtained by polycondensation of a glycol having 2 to 12 carbon atoms, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, and terephthalic acid or isophthalic acid. Examples of suitable polyamide resins include aliphatic polyester resins such as polymers, or polyester resins such as aliphatic-aromatic polyester copolymers; aliphatic polyamide resins (polyamide 6, polyamide 66, polyamide 610, polyamide 11, polyamide 12, polyamide 612, etc.), alicyclic polyamide resins (polymers of bis(aminomethyl)cyclohexane and adipic acid, etc.), aromatic polyamides (polyamide MXD (polymers of xylylenediamine and adipic acid), polymers of trimethylhexamethylenediamine and terephthalic acid, etc.), and copolyamides thereof (copolyamides copolymerized with homopolyamide components, for example, copolyamide 6 / 66, copolyamide 6 / 11, copolyamide 66 / 12, etc.). Other suitable polyamide resins include polyesteramide resins, polyestercarbonate resins, polycarbonate resins, and polyaspartic acid, which are derived from bio-derived raw materials. Furthermore, the raw materials for the biodegradable resin (A) may include biomass raw materials or biosynthesized raw materials. The above resins may be used alone or in combination of two or more. From the viewpoint of mechanical properties and processability, polyamide resins and polyester resins are preferred.
[0017] Biodegradation Accelerator (B) The biodegradation accelerator (B) according to this embodiment contains, as an essential component, PAS having a molecular weight of 120,000 or less.
[0018] Polyarylene sulfide PAS has a resin structure having a repeating unit in which an aromatic ring and a sulfur atom are bonded, and specifically, a polyarylene sulfide PAS represented by the following general formula (1):
[0019] (In the formula, R 1 and R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a nitro group, an amino group, a phenyl group, a methoxy group, or an ethoxy group, and, if necessary, a structural portion represented by the following general formula (2):
[0020] The trifunctional structural moiety represented by formula (2) is preferably present in an amount of 0.001 to 3 mol %, particularly preferably 0.01 to 1 mol %, based on the total number of moles of the trifunctional structural moiety and other structural moieties.
[0021] Here, the structural moiety represented by the general formula (1) is particularly R 1 and R 2 is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS resin, and in that case, examples include those bonded at the para position represented by the following formula (3) and those bonded at the meta position represented by the following formula (4).
[0022] Among these, a structure in which the bond between the sulfur atom and the aromatic ring in the repeating unit is at the para position represented by the general formula (3) is particularly preferred in terms of the heat resistance of the PAS.
[0023] In addition, the PAS may contain not only the structural moieties represented by the general formulas (1) and (2) but also the structural moieties represented by the following structural formulas (5) to (8):
[0024] The structural moieties represented by the general formula (1) and the general formula (2) may be contained in an amount of 30 mol % or less of the total of the structural moieties represented by the general formula (1) and the general formula (2). In particular, in the present disclosure, it is preferable that the structural moieties represented by the general formulas (5) to (8) be 10 mol % or less from the viewpoint of the heat resistance and mechanical strength of the PAS. When the structural moieties represented by the general formulas (5) to (8) are contained in the PAS resin, the bonding mode thereof may be either a random copolymer or a block copolymer.
[0025] The PAS may have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, relative to the total number of moles including other structural moieties.
[0026] (Molecular Weight) The weight average molecular weight (Mw) of the PAS applicable to this embodiment is 120,000 or less. Within this range, excellent compatibility with the biodegradable resin can be exhibited. From the viewpoint of even better compatibility and the decomposition rate of the biodegradable resin, it is preferably 100,000 or less, more preferably 50,000 or less, even more preferably 30,000 or less, and particularly preferably 10,000 or less. The weight average molecular weight (Mw) in the present disclosure can be determined by gel permeation chromatography using the method described in the Examples.
[0027] The PAS applicable to this embodiment may have a weight-average molecular weight of 120,000 or less, and may therefore contain oligoarylene sulfide (hereinafter referred to as PAS oligomer). PAS oligomers include linear and cyclic PAS oligomers, but the blending ratio of linear and cyclic PAS oligomers in the PAS oligomer used in this embodiment is not particularly limited. The repeat number of the PAS oligomer is not particularly limited as long as it does not impair the effects of the present invention. From the viewpoint of excellent melt stability, however, it is preferably a tetramer or more, more preferably a pentamer or more, and even more preferably a hexamer or more. Furthermore, the PAS oligomer may be a PAS oligomer having a single repeat number, or a mixture of PAS oligomers having different repeat numbers. In this disclosure, PAS oligomer refers to a PAS having 2 to 40 repeat units (dimer to 40-mer).
[0028] (Thermal properties) The thermal properties of the PAS applicable to this embodiment are not particularly limited, but from the viewpoints of processability and stability, it is preferable that the PAS include one having a melting point of 285°C or less. Furthermore, from the viewpoint of suppressing thermal decomposition of the biodegradable resin, it is more preferable that the PAS include one having a melting point of 270°C or less, and even more preferable that the PAS include one having a melting point of 260°C or less. Furthermore, from the viewpoint of processability, it is preferable that the PAS include one having a glass transition point of 100°C or less. The melting point and glass transition point can be measured using a differential scanning calorimeter according to the method described in the examples.
[0029] (Melt Viscosity) The melt viscosity (V6) of the PAS applicable to this embodiment is not particularly limited, but from the viewpoint of better compatibility with biodegradable resins, it is preferably 600 Pa s or less, more preferably 300 Pa s or less, even more preferably 50 Pa s or less, and particularly preferably 2 Pa s or less. However, the melt viscosity (V6) of the PAS resin is measured using a flow tester, CFT-500D, manufactured by Shimadzu Corporation, at 300°C and a load of 1.96 × 10 6 The melt viscosity is measured after holding the sample at a temperature of 10 (mm) / 1 (mm) for 6 minutes.
[0030] (Production Method) The method for producing the PAS is not particularly limited, but examples thereof include (Production Method 1) a method in which a dihalogenoaromatic compound is polymerized in the presence of sulfur and sodium carbonate, and if necessary, a polyhalogenoaromatic compound or other copolymerization component is added; (Production Method 2) a method in which a dihalogenoaromatic compound is polymerized in a polar solvent in the presence of a sulfidizing agent or the like, and if necessary, a polyhalogenoaromatic compound or other copolymerization component is added; (Production Method 3) a method in which p-chlorothiophenol is added, and if necessary, other copolymerization components are added, and then self-condensed; and (Production Method 4) a method in which a diiodoaromatic compound and elemental sulfur are melt-polymerized under reduced pressure in the presence of a polymerization inhibitor that may have a functional group such as a carboxyl group or an amino group. Of these methods, (Production Method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above-mentioned (Production Method 2) methods, there is a method for producing PAS by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno aromatic compound at a rate at which water can be removed from the reaction mixture, and then adding the dihalogeno aromatic compound and the sulfidizing agent, and optionally a polyhalogeno aromatic compound, in the organic polar solvent to react with each other, and controlling the amount of water in the reaction system to be in the range of 0.02 to 0.5 moles per mole of the organic polar solvent (see JP-A-07-228699). Particularly preferred is a compound obtained by a method in which a dihalogenoaromatic compound and, if necessary, a polyhalogenoaromatic compound or other copolymerization component are added in the presence of potassium metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the organic acid alkali metal salt in the range of 0.01 to 0.9 mol per mol of the sulfur source and the amount of water in the reaction system to 0.02 mol or less per mol of the aprotic polar organic solvent (see WO2010 / 058713 pamphlet).Specific examples of dihalogeno aromatic compounds and polyhalogeno structure compounds include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, and 4,4'-dihalobenzophenone. , 4,4'-dihalodiphenyl sulfone, 4,4'-dihalodiphenyl sulfoxide, 4,4'-dihalodiphenyl sulfide, and compounds having an alkyl group having 1 to 18 carbon atoms on the aromatic ring of each of the above compounds, and examples of polyhalogeno aromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. Furthermore, the halogen atoms contained in each of the above compounds are preferably chlorine atoms or bromine atoms.
[0031] The method for post-treating the reaction mixture containing PAS obtained by the polymerization step is not particularly limited, and examples thereof include: (post-treatment 1) after the completion of the polymerization reaction, first, distilling off the solvent under reduced pressure or normal pressure from the reaction mixture as is or after adding an acid or base, and then washing the solid remaining after the solvent distillation once or twice or more times with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low-molecular-weight polymer), acetone, methyl ethyl ketone, or alcohols, followed by neutralization, washing with water, filtration, and drying; or (post-treatment 2) after the completion of the polymerization reaction, adding a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, or aliphatic hydrocarbons (a solvent that is soluble in the polymerization solvent used and is a poor solvent for at least PAS) to the reaction mixture. or (post-treatment 3) a method in which, after the polymerization reaction is completed, a reaction solvent (or an organic solvent having a solubility equivalent to that of the low-molecular-weight polymer) is added to the reaction mixture, the mixture is stirred, and the mixture is filtered to remove the low-molecular-weight polymer, followed by washing once or twice or more times with a solvent such as water, acetone, methyl ethyl ketone, or an alcohol, followed by neutralization, washing with water, filtration, and drying; (post-treatment 4) a method in which, after the polymerization reaction is completed, water is added to the reaction mixture, the mixture is washed with water, filtered, and if necessary, an acid is added during the water washing to perform an acid treatment, and then the mixture is dried; or (post-treatment 5) a method in which, after the polymerization reaction is completed, the reaction mixture is filtered, and if necessary, the mixture is washed once or twice or more times with the reaction solvent, followed by further washing with water, filtration, and drying. Among these methods, (post-treatment 4) is preferred because it can produce a PAS resin having carboxyl groups at the PAS molecular terminals.
[0032] In the post-treatment methods exemplified above as (Post-treatment 1) to (Post-treatment 5), the PAS may be dried in a vacuum, in air, or in an inert gas atmosphere such as nitrogen.
[0033] The PAS used in this embodiment may be a PAS newly polymerized by the above method, or a recycled PAS. For example, PAS recovered from a PAS resin composition or a PAS resin molded product may be used. Specifically, PAS may be obtained by heating a PAS resin composition or a PAS resin molded product in an organic polar solvent to dissolve the PAS contained therein, and then performing the above-mentioned post-treatment on the resulting solution.
[0034] When a PAS oligomer is used as the PAS, the PAS can be produced by a method including, for example, a step (1) of reacting a polyhaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least an oligoarylene sulfide, an alkali metal halide, and an organic polar solvent; a step (2) of removing a solid phase component from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component (A) containing at least an oligoarylene sulfide and an organic polar solvent; and a step (3) of removing the organic polar solvent from the liquid phase component (A) to obtain a reaction mixture (B).
[0035] -Step (1)- Step (1) is a step of reacting a polyhaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent to obtain a crude reaction mixture containing at least an oligoarylene sulfide, an alkali metal halide, and an organic polar solvent.
[0036] The polyhalogenated aromatic compound may be the same as the dihalogenated aromatic compound and polyhalogenated structural compound described above. The production method uses an alkali metal sulfide or an alkali metal hydrosulfide and an alkali metal hydroxide (hereinafter sometimes referred to as a sulfidizing agent) as raw materials.
[0037] The alkali metal sulfides include lithium sulfide, sodium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. The alkali metal sulfides can be used as hydrates, aqueous mixtures, or anhydrides. The alkali metal sulfides can also be derived by reacting an alkali metal hydrosulfide with an alkali metal hydroxide. A small amount of alkali metal hydroxide may be added to react with the alkali metal hydrosulfide and alkali metal thiosulfate, which are usually present in trace amounts in the alkali metal sulfide.
[0038] The alkali metal hydrosulfides include lithium hydrogen sulfide, sodium hydrogen sulfide, rubidium hydrogen sulfide, cesium hydrogen sulfide, and mixtures thereof. Such alkali metal hydrosulfides can be used as hydrates, aqueous mixtures, or anhydrous forms.
[0039] The alkali metal hydrosulfide is used together with the alkali metal hydroxide. Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide. These may be used alone or in combination of two or more. Among these, lithium hydroxide, sodium hydroxide, and potassium hydroxide are preferred because of their easy availability, and sodium hydroxide is particularly preferred.
[0040] In the production method, a hydrous sulfidizing agent can also be used as a raw material, and in that case, it is preferable to subject the hydrous sulfidizing agent to a polymerization reaction of a PAS resin after a step of dehydrating the agent in the presence of at least an aprotic polar solvent. Furthermore, when the amount of the aprotic polar solvent charged is small, for example, when it is less than 1 mole per mole of sulfur atoms in the sulfidizing agent, it is preferable to dehydrate the hydrous sulfidizing agent and the aprotic polar solvent in the presence of a polyhaloaromatic compound.
[0041] The dehydration step of the hydrous sulfidizing agent is carried out by charging at least an aprotic polar solvent and a hydrous alkali metal sulfide or a hydrous alkali hydrosulfide and an alkali metal hydroxide as the hydrous sulfidizing agent into a reaction vessel equipped with a distillation apparatus, heating to a temperature at which water is removed azeotropically, specifically, in the range of 300° C. or less, preferably in the range of 80 to 220° C., more preferably in the range of 100 to 200° C., and discharging water by distillation to the outside of the system. In the dehydration step, dehydration is preferably carried out until the amount of water in the polymerization system is 5 moles or less, more preferably in the range of 0.01 to 2.0 moles, per mole of sulfur atoms in the sulfidizing agent.
[0042] Examples of the organic polar solvent include amides, ureas, and lactams such as formamide, acetamide, N-methylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methyl phenyl ketone, and mixtures thereof. Among these, amides having an aliphatic cyclic structure, such as N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid, are preferred, and N-methyl-2-pyrrolidone is more preferred.
[0043] In the PAS polymerization step, the PAS resin is polymerized by reacting the alkali metal sulfide as a sulfidizing agent with a polyhaloaromatic compound in the presence of these organic polar solvents. Alternatively, the PAS resin is polymerized by reacting the alkali metal hydrosulfide and alkali metal hydroxide as sulfidizing agents with a polyhaloaromatic compound in the presence of these organic polar solvents. Polymerization conditions generally involve a temperature in the range of 200 to 330°C, and a pressure in a range that maintains the polymerization solvent and the polyhaloaromatic compound (polymerizable monomer) substantially in a liquid phase, generally selected from the range of 0.1 to 20 MPa, preferably 0.1 to 2 MPa. The amount of polyhaloaromatic compound charged is adjusted to 0.2 to 5.0 moles, preferably 0.8 to 1.3 moles, and more preferably 0.9 to 1.1 moles per mole of sulfur atoms in the sulfidizing agent. The amount of aprotic polar solvent charged is adjusted to be in the range of 1.0 to 6.0 mol, preferably 2.5 to 4.5 mol, per mol of sulfur atoms in the sulfidizing agent. The polymerization reaction is preferably carried out in the presence of a small amount of water, and the proportion is preferably adjusted appropriately taking into account the polymerization method, the molecular weight of the resulting polymer, and productivity. Specifically, the dehydration operation is carried out so that the amount of water is 2.0 mol or less, preferably 1.6 mol or less, per mol of sulfur atoms in the sulfidizing agent. Furthermore, when the dehydration operation is carried out in the presence of a polyhaloaromatic compound (for example, the method described in "5)" in the specific embodiment below), the dehydration operation may be carried out so that the amount of water is 0.9 mol or less, preferably 0.05 to 0.3 mol, more preferably 0.01 to 0.02 mol.
[0044] Specific embodiments of polymerizing a sulfidizing agent and a polyhaloaromatic compound in the presence of the aprotic polar solvent include, for example: 1) a method using a polymerization aid such as an alkali metal carboxylate or a lithium halide; 2) a method using a branching agent such as an aromatic polyhalogen compound; 3) a method of carrying out a polymerization reaction in the presence of a small amount of water and then adding water to carry out further polymerization; 4) a method of cooling the gas phase in a reaction vessel during the reaction of an alkali metal sulfide and an aromatic dihalogen compound, condensing part of the gas phase in the reaction vessel, and refluxing it into a liquid phase; 5) A method for producing a PAS resin, the essential steps of which include a step of reacting an alkali metal sulfide or a hydrous alkali metal hydrosulfide and an alkali metal hydroxide with an amide, urea, or lactam having an aliphatic cyclic structure in the presence of a polyhalo-aromatic compound while dehydrating the mixture to produce a slurry containing a solid alkali metal sulfide; a step of adding a polar organic solvent such as NMP after producing the slurry and distilling off water to dehydrate the slurry; and a step of reacting the polyhalo-aromatic compound, the alkali metal hydrosulfide, and the alkali metal salt of a hydrolyzate of the amide, urea, or lactam having an aliphatic cyclic structure in the slurry obtained through the dehydration step, at a concentration of 0.02 mol or less of water present in the reaction system per 1 mol of the polar organic solvent such as NMP, to polymerize the slurry.
[0045] In this way, by polymerizing a dihaloaromatic compound with (i) an alkali metal sulfide or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent, a mixture of PAS resin, PAS oligomer, etc. can be obtained as a product. Other substances contained after the reaction may include by-products such as an alkali metal-containing inorganic salt, a carboxyalkylamino group-containing compound, and a terminal SH group-containing compound, as well as unreacted raw materials and water.
[0046] -Step (2)- Step (2) is a step of removing a solid phase component from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component (A) containing at least a PAS oligomer and an organic polar solvent.
[0047] The solid-liquid separation is broadly divided into two types: a flash method and a quench method, which will be described later. In this step, the quench method is preferred from the viewpoint of yield.
[0048] The quenching method is a method of separating particulate PAS resin by slowly cooling a crude reaction mixture. Generally, the crude reaction mixture is gradually cooled from a high-temperature, high-pressure state to crystallize the PAS resin in the reaction system, followed by solid-liquid separation by filtration or other methods to separate the solids containing the PAS resin as granules. Generally, as the molecular weight of a polymer increases, the interactions between the polymers become stronger, resulting in poorer solubility in the solvent. Therefore, in this process, the PAS resin precipitates and becomes a solid, while the cyclic PAS and oligomers remain dissolved in the solvent. The cooling time in the quenching process is not particularly limited, but is typically preferably in the range of 0.1°C / min to 3°C / min. Furthermore, it is not necessary to slowly cool at the same rate throughout the entire slow cooling process. A method in which the cooling rate is in the range of 0.1°C / min to 1°C / min until the PAS resin granules crystallize, and then at a rate of 1°C / min or faster, is also preferred. It is preferable to finally cool the mixture to 70°C or higher, preferably 100°C or higher and 200°C or lower, and then remove the solids containing the PAS resin by solid-liquid separation. Examples of solid-liquid separation in the quench method include a method in which separation is performed using filtration or a centrifuge such as a screw decanter, and then water is directly added to the obtained filtration residue to form a slurry, followed by repeated solid-liquid separation, and a method in which the obtained filtration residue is heated in a non-oxidizing atmosphere to remove the remaining solvent.
[0049] In this case, if necessary, a step of removing a part or most of the organic polar solvent in the crude reaction mixture by distillation may be included, and after performing this step, the crude reaction mixture may be subjected to solid-liquid separation by filtration to remove solid phase components. Also, a step of washing the crude reaction mixture, or preferably the solid fraction (slurry) obtained after solid-liquid separation, by contacting it with water or an organic polar solvent may be included.
[0050] -Step (3)- Step (3) is a step of removing the organic polar solvent from the liquid phase component (A) to obtain a reaction mixture (B).
[0051] Examples of methods for removing the organic polar solvent in step (3) include a flash method in which the solvent is distilled off by flashing from a high-temperature, high-pressure state into an atmosphere of normal or reduced pressure, a method in which the solvent is distilled off by heating, and solvent removal using a membrane. When removing the organic polar solvent, it is desirable to remove the solvent so that the proportion of solids (non-volatile content) is in the range of 20 to 100 parts by mass, preferably 20 to 99.99 parts by mass, and more preferably 30 to 90 parts by mass. The temperature at which the solvent is removed by heating depends on the properties of the solvent used and cannot be uniquely limited, but can usually be selected from the range of 20 to 150°C, preferably 40 to 120°C. In addition, the pressure at which the solvent is removed is preferably normal pressure or less, which allows the solvent to be removed at a lower temperature.
[0052] In this embodiment, for the purpose of further removing impurities or adjusting the content of oligoarylene sulfide, a step of contacting the reaction mixture (B) with water at above 100 ° C. and a pH of 6 or higher (see JP 2020-007490 A) may be included as step (4). If necessary, as a pretreatment, the reaction mixture (B) may be contacted with water at above 100 ° C. and a pH of 6 or higher after being subjected to a treatment (water washing treatment) in which the reaction mixture (B) is contacted with water under conditions of 100 ° C. or less, preferably in the range of 20 to 100 ° C., and then the reaction mixture (B) may be contacted with water at above 100 ° C. and a pH of 6 or higher.
[0053] The reaction mixture (B) obtained through the above steps (1) to (3) and, if necessary, step (4) can be used as a biodegradation promoter as is, so long as the PAS oligomer content is 90 parts by mass or more. If the PAS oligomer content is 90 parts by mass or less, the reaction mixture (B) can be further washed or dried, or the PAS oligomer can be extracted and purified before use. In such cases, known extraction and purification procedures or drying can be performed.
[0054] The biodegradation accelerator (B) applicable to this embodiment preferably has a PAS content of 90 parts by mass or more, more preferably 92 parts by mass or more, and even more preferably 95 parts by mass or more. Within this range, an excellent degradation-promoting effect on biodegradable resins is exhibited. In the present disclosure, the PAS content in the biodegradation accelerator can be measured by the method described in the Examples. Furthermore, the volatile content of the biodegradation accelerator (B) is not particularly limited, but from the viewpoint of processability, it is preferably 10% or less, more preferably 5% or less.
[0055] The components contained in the biodegradation accelerator (B) other than PAS are not particularly limited as long as they do not impair the effects of the present invention. For example, the components may include by-products produced during PAS polymerization, such as alkali metal-containing inorganic salts, carboxyalkylamino group-containing compounds, and terminal SH group-containing compounds, as well as unreacted raw materials, organic solvents, and water.
[0056] In addition to the above components, the biodegradation accelerator (B) applicable to this embodiment may optionally contain known and commonly used additives such as plasticizers, fillers, silane coupling agents, dispersants, colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, release agents, antibacterial agents, nucleating agents, hydrolysis inhibitors, and rust inhibitors. These additives are not essential components and may be appropriately adjusted depending on the purpose and application so as not to impair the effects of the present invention. When the biodegradation accelerator (B) contains these optional components, they may be dry-blended with the PAS in advance, or may be further melt-kneaded in an extruder or the like after mixing.
[0057] In the biodegradable resin composition according to this embodiment, the amount of the biodegradation promoter (B) is preferably 0.001 to 50 parts by mass, more preferably 0.01 to 40 parts by mass, and even more preferably 0.1 to 30 parts by mass, per 100 parts by mass of the biodegradable resin (A). Within this range, the resin composition has an excellent balance between biodegradability control and processability while maintaining the mechanical properties of the biodegradable resin.
[0058] The biodegradation accelerator (B) incorporated into the biodegradable resin composition according to this embodiment is resistant to decomposition in environments without UV light, such as during product distribution or storage prior to use. Therefore, the presence or absence of the biodegradation accelerator (B) does not affect the shelf life of the resin composition or molded product. Furthermore, because it exhibits an excellent effect of promoting the degradation of biodegradable resins when irradiated with UV light, UV irradiation during outdoor use, after use, compost disposal, etc. can rapidly promote the decomposition of the biodegradable resin. While the reason for this effect is not entirely clear, it is presumed to be due to the following mechanism. First, unless exposed to UV light, the PAS added to the biodegradable resin remains stable in the composition and is thought to have no effect on the biodegradable resin. On the other hand, under UV light, molecular cleavage occurs at the S-benzene bond constituting the PAS, followed by oxidation reactions, hydrogen adsorption, and the like, to produce sulfonic acid. This sulfonic acid acts as a hydrolysis catalyst for the ester and amide bonds constituting the biodegradable resin, and, acting together with moisture in the usage environment, rapidly degrades the resin to a molecular weight that can be metabolized by microorganisms, thereby promoting biodegradability. This mechanism is not limited to the atmosphere, and it is believed that similar decomposition behavior occurs when ultraviolet light is irradiated in an aqueous solution (e.g., seawater), etc. Note that the above mechanism is merely speculation, and cases where the effects of the present invention are achieved for other reasons are also included in the technical scope of the present invention.
[0059] Optional Components The biodegradable resin composition according to this embodiment may contain, as necessary, known and commonly used additives as optional components, such as plasticizers, fillers, silane coupling agents, dispersants, colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, mold release agents, antibacterial agents, nucleating agents, hydrolysis inhibitors, and rust inhibitors. These additives are not essential components, and may be used by adjusting them appropriately depending on the purpose and application so as not to impair the effects of the present invention.
[0060] <Method for producing biodegradable resin composition> The method for producing a biodegradable resin composition according to this embodiment includes a step of blending the above-mentioned essential components and melt-kneading them at a temperature range equal to or higher than the melting point of the biodegradable resin (A). The method for producing the resin composition used in the present invention is not particularly limited, but examples thereof include a method of blending the essential components and, if necessary, optional components, and melt-kneading them, more specifically, a method of uniformly dry-mixing them, if necessary, using a tumbler or a Henschel mixer, and then feeding them into a twin-screw extruder and melt-kneading them.
[0061] The melt-kneading can be carried out by heating to a temperature range in which the resin temperature is equal to or higher than the melting point of the biodegradable resin (A), preferably equal to or higher than the melting point + 10°C, more preferably equal to or higher than the melting point + 10°C, even more preferably equal to or higher than the melting point + 20°C, to a temperature range in which the resin temperature is equal to or lower than the melting point + 150°C, more preferably equal to or lower than the melting point + 80°C.
[0062] From the viewpoints of dispersibility and productivity, the melt kneader is preferably a twin-screw kneading extruder. For example, it is preferable to melt knead while appropriately adjusting the resin component discharge rate in the range of 5 to 500 (kg / hr) and the screw rotation speed in the range of 50 to 500 (rpm). It is even more preferable to melt knead under conditions where the ratio (discharge rate / screw rotation speed) is in the range of 0.02 to 5 (kg / hr / rpm). Furthermore, the addition and mixing of the components to the melt kneader may be carried out simultaneously or in portions. For example, when a fibrous filler is added as needed, it is preferable from the viewpoint of dispersibility to feed the filler into the twin-screw kneading extruder through a side feeder. The position of the side feeder is preferably such that the ratio of the distance from the extruder's resin input section (top feeder) to the side feeder to the total screw length of the twin-screw kneading extruder is 0.1 or more, more preferably 0.3 or more. Furthermore, this ratio is preferably 0.9 or less, more preferably 0.7 or less.
[0063] The biodegradable resin composition according to the present disclosure obtained by melt-kneading in this manner is a molten mixture containing the essential components, optional components added as needed, and components derived therefrom. Therefore, the biodegradable resin composition according to the present disclosure has a morphology in which the biodegradable resin (A) forms a continuous phase and the biodegradation accelerator (B) and other optional components are dispersed.
[0064] After the melt-kneading, the biodegradable resin composition according to the present embodiment is preferably processed by a known method, for example, by extruding the molten resin composition into a strand shape, and then processing it into a form such as pellets, chips, granules, or powder, and then pre-drying it at a temperature in the range of 60 to 150°C as needed.
[0065] Furthermore, the method for producing a biodegradable resin composition according to this embodiment includes a method for producing a PAS resin composition, in which the biodegradable resin composition obtained by the above-described production method is used as a masterbatch and further diluted with a biodegradable resin. That is, another embodiment of the present disclosure is a method for producing a biodegradable resin composition, which includes a step of using the biodegradable resin composition obtained by the above-described production method as a masterbatch and further diluting with a biodegradable resin. The method for diluting the biodegradable resin composition may be dry blending, or it may be melt-kneaded again under the same conditions as in the above-described production method for the resin composition. The biodegradable resin used for dilution is not particularly limited as long as it does not impair the effects of the present invention. It may be the same as the resin blended in the masterbatch or a different type of biodegradable resin, and various types may be selected depending on the processing conditions and application. The amount of the biodegradation accelerator (B) blended per 100 parts by mass of the resin composition obtained after dilution is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.1 parts by mass, from the viewpoint of efficient resin decomposition.
[0066] <Molded article, method for manufacturing molded article> The molded article according to this embodiment is produced by melt-molding a biodegradable resin composition. The method for manufacturing a molded article according to this embodiment includes a step of melt-molding the biodegradable resin composition manufactured by the method described above. Therefore, the molded article according to this embodiment has a morphology in which the biodegradable resin (A) forms a continuous phase and the biodegradation promoter (B) and optional components are dispersed.
[0067] The biodegradable resin composition according to this embodiment can be subjected to various molding processes, such as injection molding, compression molding, extrusion molding of composites, sheets, pipes, etc., coextrusion molding, pultrusion molding, blow molding, transfer molding, and nonwoven fabric molding. When producing plate- or sheet-shaped molded articles, examples of suitable methods include melt molding using extrusion molding, flat press molding, profile extrusion molding, blow molding, compression molding, vacuum molding, and injection molding. When producing film-shaped molded articles, examples of suitable methods include melt extrusion, solution casting, inflation film molding, cast molding, extrusion lamination molding, calendar molding, sheet molding, fiber molding, blow molding, injection molding, rotational molding, and coating molding. These films may also be stretch-molded.
[0068] The molded article according to this embodiment may also be subjected to various known and commonly used secondary processes for the purpose of imparting surface functionality such as chemical functionality, electrical functionality, magnetic functionality, mechanical functionality, abrasion resistance, etc. Examples of secondary processes include painting, bonding, plating, various surface treatments (hydrophilic treatment, antistatic treatment, corona discharge treatment, plasma treatment, photochromism treatment, physical vapor deposition, chemical vapor deposition, coating, etc.), printing, machining, embossing, etc.
[0069] The molded article according to this embodiment includes a remolded article obtained by reusing a molded article obtained by melt-molding the biodegradable resin composition. Specifically, for example, it includes a molded article obtained by recycling a sprue or runner generated during the production of a molded article, a non-standard molded article recovered, or a molded article that has been used as a product, cleaning it as necessary, pulverizing it, and melt-molding it again at a temperature equal to or higher than the melting point of the biodegradable resin (A). When reusing, it is preferable to mix the pulverized molded article with the biodegradable resin composition from the viewpoint of mechanical properties. The size of the molded article to be pulverized is not particularly limited, but from the viewpoint of mixability and processability, it is preferable that the size be approximately the same as that of the biodegradable resin composition to be mixed. Furthermore, the mixing ratio is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 20 parts by mass or less, of the pulverized molded article per 100 parts by mass of the biodegradable resin composition. Within this range, recyclability can be improved without impairing the effects of the biodegradable resin composition of the present disclosure.
[0070] <Applications> The resin composition and molded article according to this embodiment are characterized by undergoing minimal change over time when stored in a dark place and exhibiting an excellent decomposition-promoting effect when irradiated with ultraviolet light, and therefore can be suitably used for applications such as agricultural materials such as greenhouse films, mulch films, coating materials, fertilizer coating materials, seedling pots, vegetation nets, and water-retaining sheets; fishing materials such as fishing nets, seaweed nets, aquaculture nets, fishing lines, and fishing bait bags; packaging materials and food applications such as trays, cutlery, stretch film, shrink film, bottles, and bags; and building materials such as curing sheets, construction formwork, and stakes. Furthermore, they can also be used for other general applications.
[0071] The present invention will be described below using examples and comparative examples, but is not limited to these examples. Unless otherwise specified, "%" and "parts" are based on mass.
[0072] <Reference Examples 1-2, Examples 1-8, and Comparative Examples 1-6> Each material was blended according to the compositional components and blending amounts shown in Tables 1-3. Thereafter, these blended materials were fed into a vented twin-screw extruder "TEX-30α (product name)" manufactured by The Japan Steel Works, Ltd., and melt-kneaded at a resin component discharge rate of 30 kg / hr, a screw rotation speed of 200 rpm, and a set resin temperature of 260°C to obtain pellets of a resin composition. The obtained pellets were pressed after 1 minute of preheating using an NF-37HH press manufactured by Shinto Metal Industries, Ltd., with a mold temperature set to 190°C, to obtain a pressed sheet with a thickness of approximately 1 mm. The obtained pressed sheet was used as a test piece and measured in the dark or under ultraviolet irradiation (60 W / m 2 ) at 55°C and 50% RH for 200 hours, and then the following tests were carried out.
[0073] <Evaluation>
[0074] (1) Evaluation of Intrinsic Viscosity (IV) Retention Rate For each test piece, initially, after dark storage, and after UV irradiation in the atmosphere, a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) was used as the viscosity measurement solvent, and the temperature was 30°C, the sample concentration was 1.00 × 10 -2 The intrinsic viscosity (IV) was measured using a fully automatic solution viscometer (Sentec Corporation, "2CH Type DJ504") with a 10000 vol / L solution. The retention rate was calculated using the following formula, which is the post-test value relative to the initial value. The results are shown in Tables 1 to 3. Retention rate (%) = post-test value (dL / g) / initial value (dL / g) × 100
[0075] (2) Evaluation of Melt Viscosity (MFR) Retention Rate For each sample of each test piece, initially, after storage in a dark place, and after exposure to ultraviolet light in the atmosphere, the melt viscosity (MFR) after 6 minutes of retention was measured using a Shimadzu flow tester "CFT-500D." Note that test pieces using A-1 as the biodegradable resin were measured at a temperature of 190°C and a load of 2 kg, and test pieces using A-2 were measured at a temperature of 320°C and a load of 20 kg. An orifice with L / D = 10 (mm) / 1 (mm) was used in both cases. The retention rate was calculated from the obtained values using the following formula. The retention rate was calculated using the following formula from the value after the test relative to the initial value. The results are shown in Tables 1 to 3. Retention rate (%) = value after test (Pa s) / initial value (Pa s) × 100
[0076] (3) Evaluation of soil biodegradability Each test specimen was frozen and crushed into powder after initial storage, dark storage, and UV irradiation in the atmosphere. Using 120 mg of each resulting powder, the biodegradability (%) after 60 days was measured based on the amount of carbon dioxide generated by microbial metabolism using a test method in accordance with ISO 14855-1. The results are shown in Tables 1 to 3.
[0077] (4) Evaluation of biodegradability in seawater Each test piece was initially frozen and crushed into powder after UV irradiation in the atmosphere. 100 mg of each resulting powder was used to measure the biodegradability (%) after 60 days based on the amount of carbon dioxide generated by microbial metabolism using a test method in accordance with ISO 23977-2. The results are shown in Tables 1 to 3.
[0078] (5) Evaluation of PAS Content of Biodegradation Accelerator Approximately 8.0 mg of the biodegradation accelerator obtained in each production example was placed in a Pt pan for TG-DTA measurement, and the mass was accurately measured. The Pt pan was heated in a TG-DTA (TG-DTA6200, manufactured by SII NanoTechnology Inc.) from room temperature (23°C) to 350°C at a heating rate of 50°C / min under a nitrogen stream, and held at 350°C for 30 minutes to thermally decompose and volatilize components other than PAS. The PAS content of the biodegradation accelerator was calculated from the difference between the weight after holding and the weight at room temperature (23°C).
[0079] (6) Evaluation of thermal properties of PAS in biodegradation accelerator The biodegradation accelerator obtained in each production example was melted at 350°C and then rapidly cooled to produce an amorphous film. Approximately 4 mg of this film was taken, and the melting point of the PAS was measured using a differential scanning calorimeter (Perkin Elmer "DSC8500"). When multiple melting points were measured, they were recorded in the format of "lowest melting point to highest melting point."
[0080] (7) Evaluation of molecular weight of PAS in biodegradation accelerator The weight-average molecular weight of PAS contained in the biodegradation accelerator was measured using gel permeation chromatography under the following measurement conditions. Calibration was performed using six types of monodisperse polystyrene. Apparatus: Ultra-high temperature polymer molecular weight distribution measurement apparatus ("SSC-7000" manufactured by Senshu Scientific Co., Ltd.) Column: UT-805L (manufactured by Showa Denko K.K.) Column temperature: 210°C Solvent: 1-chloronaphthalene Measurement method: UV detector (360 nm)
[0081]
[0082]
[0083]
[0084] The blending ratios of the blending components in Tables 1 to 3 were as follows. Biodegradable resins (A) A-1: Polyester resin "(product number) BioPBS FZ-71PB" manufactured by Mitsubishi Chemical Corporation A-2: Polyamide resin "(product number) ULTRAMID A3W" manufactured by BASF Japan Ltd. Biodegradation accelerators (B) B-1: PAS content 99 parts by mass, PAS weight average molecular weight 20,000, melting point 282°C, melt viscosity 10 Pa s B-2: PAS content 99 parts by mass, PAS weight average molecular weight 2,000, melting point approximately 140 to 250°C, melt viscosity 3 Pa s B-3: PBS masterbatch containing 50 parts by mass of PAS content 99 parts by mass, PAS weight average molecular weight 2,000, melting point approximately 140 to 250°C, and melt viscosity 3 Pa s B-4: PAS content 99 parts by mass, PAS weight average molecular weight 60,000, melting point 282°C, melt viscosity 400 Pa s b-5: PAS content 99 parts by mass, PAS weight average molecular weight 150,000, melting point approximately 282°C, melt viscosity 1,500 Pa s b-6: Poly[(R)-3-hydroxybutyric acid] (PHB) manufactured by Sigma-Aldrich Japan
[0085] (Production Example 1) Production method of B-1 A 150 L autoclave equipped with a stirring blade and bottom valve, connected to a force gauge, thermometer, and condenser, was charged with 14.148 kg of 45% sodium hydrosulfide (47.55 wt% NaSH), 9.541 kg of 48% caustic soda (48.8 wt% NaOH), and 38.0 kg of N-methyl-2-pyrrolidone (NMP). The temperature was raised to 209 ° C while stirring under a nitrogen stream, and 12.150 kg of water was distilled off (the remaining water content was 1.13 mol per mol of NaSH). The autoclave was then sealed and cooled to 180 ° C, and 17.874 kg of paradichlorobenzene (p-DCB) and 16.0 kg of NMP were charged. At a liquid temperature of 150 ° C, the pressure was increased to 0.1 MPa using nitrogen gas, and the temperature was raised. After the temperature rose to 260 ° C, the autoclave was cooled by spraying water over the top, and the reaction was carried out at 260 ° C for 2 hours. While cooling the top of the autoclave, the liquid temperature was kept constant so as not to drop. Next, the temperature was lowered and cooling of the top of the autoclave was stopped. The maximum pressure during the reaction was 0.87 MPa. After the reaction, the mixture was cooled, the bottom valve was opened at 100 ° C, and the reaction slurry was transferred to a 150 L flat plate filter and pressure filtered at 120 ° C. 50 kg of 70 ° C. hot water was added to the obtained cake, stirred, filtered, and then 25 kg of hot water was added and filtered. Next, 25 kg of hot water was added, stirred for 1 hour, filtered, and then 25 kg of hot water was added and filtered. This operation was repeated twice. The obtained cake was dried at 120 ° C. for 15 hours using a hot air circulation dryer to obtain a biodegradation accelerator (B-1).
[0086] (Production Example 2) Production method of B-2 A 150 L autoclave equipped with a stirring blade and a bottom valve, to which a pressure gauge, a thermometer, and a condenser were connected, was charged with flake sodium sulfide (60.3 wt % Na 219.413 kg (150 mol) of sodium sulfide (S) and 45.0 kg (454 mol) of NMP were charged. The temperature was raised to 209°C while stirring under a nitrogen stream, and 4.644 kg of water was distilled off (the remaining water content was 1.13 mol per mol of sodium sulfide). The autoclave was then sealed and cooled to 180°C, and 21.631 kg (147 mol) of p-DCB and 18.0 kg (182 mol) of NMP were charged. At a liquid temperature of 150°C, the pressure was increased to 0.1 MPa using nitrogen gas, and the temperature increase began. The liquid temperature was raised to 240°C over 135 minutes and maintained at that temperature for 30 minutes. The liquid temperature was then raised to 250°C over 40 minutes and maintained at that temperature for 73 minutes to complete the reaction. The autoclave was then cooled. The bottom valve of the autoclave was opened at 100°C, and the reaction slurry was transferred to a 150L plate filter and pressure filtered at 120°C. 48.0 kg of NMP was added, and the cake was again pressure washed and filtered. The weight of the recovered NMP filtrate was 80.0 kg. Water was added to the obtained NMP filtrate to form a water slurry, and then solid-liquid separation and water washing were repeated twice, and the mixture was then dried in a hot air dryer at 120°C for 4 hours to obtain a powdered biodegradation accelerator (B-2).
[0087] (Production Example 3) Production method for B-3
[0049] 100 parts by mass of the biodegradable resin (A-1) were blended with 100 parts by mass of the biodegradation accelerator (B-2) obtained in Production Example 2, and melt-kneaded using a vented twin-screw extruder in the same manner as in the production method for the resin composition described above to obtain a resin composition (masterbatch). This masterbatch was used in Example 6 as the biodegradation accelerator (B-3).
[0088] (Production Example 4) Production method for B-4 [Step 1] 22.05 kg (150.0 mol) of p-DCB, 59.49 kg (600 mol) of NMP, and 1.08 kg (60.0 mol) of water were charged into a 150 L autoclave equipped with a stirring blade and a bottom valve, which was connected to a temperature sensor, a condenser, a dropping tank, a dropping pump, and a distillate separation tank, at room temperature, and the temperature was raised to 100°C over 20 minutes under a nitrogen atmosphere while stirring. The system was closed, and the temperature was further raised to 220°C over 40 minutes, and the internal pressure was controlled at that temperature to 0.22 MPa (gauge pressure). To the autoclave, flaky sodium hydrosulfide (Na 218.00 kg of hydrous flaky sodium hydrosulfide (NaSH: 71.2 wt%, Na 2 A mixture containing 2.7 kg of 2.7 wt% S, 2.90 kg (68.3 mol) of lithium chloride, and 5.1 kg of water was added dropwise over 3 hours. During the dropwise addition, a dehydration operation was simultaneously performed, and water was removed from the system. The p-DCB distilled together with the water was continuously returned to the autoclave. The dehydration operation and the p-DCB return operation were performed until the temperature was raised to 240°C, at which point the system was sealed. [Step 2] After that, the temperature and pressure were maintained for 1 hour, and then the internal temperature was raised to 240°C while the internal pressure was reduced to 0.17 MPa over 1 hour. This temperature was maintained for 1 hour to terminate the reaction, and the system was cooled to room temperature. [Step 3] 30 L of water was added to 6.0 kg of the resulting reaction slurry, and the mixture was stirred at 80°C for 1 hour and then filtered. The cake was again stirred with 15 L of warm water for 1 hour and filtered. After filtration, acetic acid was added to adjust the pH to 4.0, and the mixture was stirred for 30 minutes and then filtered. Furthermore, 15 L of warm water was added to the filter cake, and the mixture was stirred for 30 minutes and filtered. This operation was repeated three times, and after filtration, the mixture was dried in a hot air dryer at 120°C for 10 hours to obtain a powdered biodegradation accelerator (B-4).
[0089] (Production Example 5) Production Method of b-5 A powdery biodegradation accelerator (b-5) was obtained in the same manner as in Production Example 4, except that 6.96 kg (163.8 mol) of lithium chloride was used.
[0090] Comparing Examples 1 to 8 with Comparative Examples 1, 3, and 5 in Tables 1 to 3 shows that the use of a biodegradation accelerator containing a PAS having a specific weight-average molecular weight significantly reduces the melt viscosity and intrinsic viscosity under UV irradiation, thereby accelerating decomposition, and also improving biodegradability in soil and seawater. Comparing Examples 1 to 8 with Comparative Examples 2 and 4 shows that the biodegradation accelerator of the present disclosure can improve biodegradability under UV irradiation with a smaller amount added. Comparing Examples 1 to 8 with Comparative Example 6 shows that the resin composition of the present disclosure suppresses accelerated decomposition in the dark and improves biodegradability only under UV irradiation. Example 9 shows that the biodegradation accelerator of the present disclosure can improve the biodegradation of polyamide resins, without limiting the type of resin.
Claims
1. A biodegradable resin composition comprising as essential components a biodegradable resin (A) having at least an ester bond or an amide bond in its main chain and a biodegradability promoter (B), wherein the biodegradability promoter (B) contains a polyarylene sulfide having a weight average molecular weight of 120,000 or less.
2. The biodegradable resin composition according to claim 1, wherein the content of the polyarylene sulfide in the biodegradability promoter (B) is 90 parts by mass or more.
3. The biodegradable resin composition according to claim 1 or 2, wherein the polyarylene sulfide contained in the biodegradation promoter (B) includes an oligoarylene sulfide.
4. The biodegradable resin composition according to claim 3, wherein the oligoarylene sulfide contained in the biodegradability promoter (B) is obtained by the steps of: (1) reacting a polyhalo aromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least the oligoarylene sulfide, the alkali metal halide and the organic polar solvent; (2) removing a solid phase component from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component containing at least the oligoarylene sulfide and the organic polar solvent; and (3) removing the organic polar solvent from the liquid phase component to obtain a reaction mixture.
5. The biodegradable resin composition according to claim 1 or 2, wherein the biodegradable resin (A) is a polyamide resin or a polyester resin.
6. A biodegradable resin composition according to claim 1 or 2, wherein the amount of the biodegradability promoter (B) is 0.001 to 50 parts by mass per 100 parts by mass of the biodegradable resin (A).
7. A molded article obtained by melt molding the biodegradable resin composition according to claim 1 or 2.
8. A method for producing a biodegradable resin composition, comprising a step of blending a biodegradable resin (A) having at least an ester bond or an amide bond in its main chain and a biodegradability promoter (B) as essential components, and melt-kneading the mixture at a temperature equal to or higher than the melting point of the biodegradable resin (A), wherein the biodegradability promoter (B) contains a polyarylene sulfide having a weight-average molecular weight of 120,000 or less.
9. A method for producing a biodegradable resin composition according to claim 8, wherein the content of polyarylene sulfide in the biodegradability promoter (B) is 90 parts by mass or more.
10. A method for producing a biodegradable resin composition according to claim 8 or 9, wherein the polyarylene sulfide contained in the biodegradation promoter (B) includes an oligoarylene sulfide.
11. A method for producing a biodegradable resin composition according to claim 10, wherein the oligoarylene sulfide contained in the biodegradability promoter (B) is obtained by the steps of: (1) reacting a polyhalo aromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least the oligoarylene sulfide, the alkali metal halide and the organic polar solvent; (2) removing a solid phase component from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component containing at least the oligoarylene sulfide and the organic polar solvent; and (3) removing the organic polar solvent from the liquid phase component to obtain a reaction mixture.
12. A method for producing a biodegradable resin composition according to claim 8 or 9, wherein the amount of the biodegradability promoter (B) is 0.001 to 50 parts by mass per 100 parts by mass of the biodegradable resin (A).
13. A method for producing a molded article, comprising a step of melt-molding the biodegradable resin composition produced by the method according to claim 8 or 9.
14. A method for promoting hydrolysis in which a biodegradable resin having at least an ester bond or an amide bond in the main chain is blended with a polyarylene sulfide having a weight-average molecular weight of 120,000 or less to promote hydrolysis in an ultraviolet ray irradiation environment.
15. A method of using a polyarylene sulfide having a weight average molecular weight of 120,000 or less as a hydrolysis promoter.
Citation Information
Patent Citations
Plastic composition product
CN104356624A
Heat-resistant high-strength 3D printing material and preparation method thereof
CN111500036A
Thermoplastic resin composition and thermoplastic resin molded article
JP2006143884A
Crystalline resin composition
JP2008189900A