Method for producing pellets of cellulose-fiber-containing resin and method for producing molded object

The method of melt-kneading cellulose fiber-containing resin sheets to produce pellets enhances the mechanical properties and productivity of cellulose fiber-containing resin pellets, offering a sustainable alternative to traditional fiber-reinforced plastics with improved biodegradability and disposal outcomes.

WO2024225060A1PCT designated stage expired Publication Date: 2024-10-31OJI HLDG CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014680
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Fiber-reinforced plastic molded bodies using traditional reinforcing fibers like carbon and glass have low biodegradability, leading to disposal challenges and increased load on incinerators, prompting the need for more sustainable alternatives with improved mechanical properties.

Method used

A method for producing cellulose fiber-containing resin pellets through melt-kneading cellulose fiber-containing resin sheets using a screw-type kneader, optimizing the cross-sectional area ratio and processing conditions to enhance productivity and mechanical properties such as bending rigidity and impact resistance.

Benefits of technology

The method results in cellulose fiber-containing resin pellets with higher productivity and molded articles exhibiting excellent bending rigidity and impact resistance, addressing the biodegradability and disposal issues of traditional fiber-reinforced plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014680_31102024_PF_FP_ABST
    Figure JP2024014680_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a method for producing pellets of a cellulose-fiber-containing resin with better production efficiency, the pellets yielding a molded object having excellent bending rigidity and impact resistance; and a method for producing a molded object by molding the pellets. This method for producing pellets of a cellulose-fiber-containing resin comprises melt-kneading a sheet of the cellulose-fiber-containing resin with a screw kneader to produce the pellets of the cellulose-fiber-containing resin, wherein the ratio of the cross-sectional area of the sheet of the cellulose-fiber-containing resin to the area of an introduction opening of the screw kneader, (cross-sectional area of sheet of cellulose-fiber-containing resin) / (area of introduction opening of screw kneader), is 0.065 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing cellulose fiber-containing resin pellets and method for producing molded articles

[0001] The present invention relates to a method for producing cellulose fiber-containing resin pellets and a method for producing a molded article using the pellets.

[0002] Fiber-reinforced plastic molded products made from nonwoven fabrics containing reinforcing fibers such as carbon fiber and glass fiber (also called sheets for fiber-reinforced plastic molded products) are already used in a variety of fields, including sports and leisure goods, aircraft materials, electronic device components, etc. Thermosetting resins and thermoplastic resins are used as the matrix resins in fiber-reinforced plastic molded products, but in recent years, development of fiber-reinforced plastic molded products using thermoplastic resins has been progressing.

[0003] Carbon fiber, glass fiber, aramid fiber, etc. are used as reinforcing fibers. Such reinforcing fibers serve to increase the strength of fiber-reinforced plastic molded bodies. When such molded products are to be disposed of, they are usually disposed of in landfills or incinerated. However, molded products using such reinforcing fibers have low biodegradability after being landfilled, and there are problems with the load on incinerators and other equipment when they are incinerated.

[0004] For this reason, in recent years, the use of pulp fibers as reinforcing fibers has been proposed (for example, Patent Documents 1 to 3). In Patent Documents 1 and 2, a molded article is obtained by making a slurry containing pulp fibers and a thermoplastic resin into a paper, and then molding the molded intermediate product under heat and pressure. Patent Document 3 proposes forming pellets from a slurry containing pulp fibers and a thermoplastic resin, and then injection molding the pellets to produce a molded article.

[0005] JP-A-6-322699 JP-A-6-346399 JP-A-6-345944

[0006] The present invention aims to provide a method for producing cellulose fiber-containing resin pellets with improved productivity, which allows for the production of molded articles having excellent bending rigidity and impact resistance from the pellets, and a method for producing molded articles obtained by molding the pellets.

[0007] The present inventors have discovered that in a method for producing cellulose fiber-containing resin pellets, which includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw kneader to produce cellulose fiber-containing resin pellets, by setting the ratio of the cross-sectional area of ​​the cellulose fiber-containing sheet to the inlet area of ​​the screw kneader to a specific value or less, excellent productivity can be achieved and a molded article having excellent bending rigidity and impact resistance can be obtained from the resulting cellulose fiber-containing resin pellets, and have completed the present invention. The present invention relates to the following <1> to <14>. <1> A method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet in a screw kneader, wherein the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw kneader (cross-sectional area of ​​cellulose fiber-containing resin sheet / inlet area of ​​screw kneader) is 0.065 or less. <2> A method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet in a screw kneader, wherein the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw kneader (cross-sectional area of ​​cellulose fiber-containing resin sheet / inlet area of ​​screw kneader) is 0.065 or less. 2 ) (cross-sectional area (cm ) of the cellulose fiber-containing resin sheet 2<3> The method for producing cellulose fiber-containing resin pellets according to <1>, wherein the ratio (discharge rate / circumferential speed) of the discharge rate (kg / h) to the peripheral speed (m / min) of the screw of the screw-type kneader is 0.50 or more. <4> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <3>, wherein the cellulose fiber content in the cellulose fiber-containing resin pellets is 10% by mass or more and 90% by mass or less. <5> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <4>, wherein a cellulose fiber-containing resin sheet is produced by a production method including the following steps 1 and 2: Step 1: a fiber aggregate production step of producing a fiber aggregate containing cellulose fibers and resin A by dry papermaking; and Step 2: a cellulose fiber-containing resin sheet production step of compressing the fiber aggregate to produce a cellulose fiber-containing resin sheet. <6> The method for producing cellulose fiber-containing resin pellets according to <5>, wherein the resin A contains resin fibers. <7> A method for producing cellulose fiber-containing resin pellets according to any one of <1> to <6>, wherein T / Y is 0.5 or more and 1.5 or less, where T is the tensile strength of the cellulose fiber-containing resin sheet in a first direction and Y is the tensile strength in a second direction perpendicular to the first direction. <8> A method for producing cellulose fiber-containing resin pellets according to any one of <1> to <7>, wherein the cellulose fiber-containing resin sheet has a bulk specific gravity of 0.10 g / mL or more and 0.60 g / mL or less. <9> A method for producing a molded body, comprising a step of producing cellulose fiber-containing resin pellets by the method according to any one of <1> to <8>, and a step of molding the cellulose fiber-containing resin pellets. <10> A method for producing a molded body according to <9>, wherein the molding step is a step of injection molding the cellulose fiber-containing resin pellets. <11> A method for producing a molded body according to any one of <1> to <7>, wherein the density of the obtained molded body is 0.8 g / cm 3 1.5g / cm or more 3<12> The method for producing a molded article according to any one of <9> to <11>, wherein the thickness of the obtained molded article is 2 mm or more. <13> The method for producing a molded article according to any one of <9> to <12>, wherein the flexural modulus of the obtained molded article measured in accordance with JIS K 7171:2016 is 1.5 GPa or more. <14> The method for producing a molded article according to <9> or <12>, wherein the Charpy impact strength of the obtained molded article measured in accordance with JIS K 7111-1:2012 is 2.0 kJ / m or more. 2 The method for producing a molded body according to any one of <9> to <13> above.

[0008] According to the present invention, there are provided a method for producing cellulose fiber-containing resin pellets with improved productivity, which allows for the production of molded articles having excellent bending rigidity and impact resistance from the pellets, and a method for producing molded articles obtained by molding the pellets.

[0009] FIG. 1 shows the web forming apparatus used in the examples.

[0010] [Method for producing cellulose fiber-containing resin pellets] The method for producing cellulose fiber-containing resin pellets (hereinafter simply referred to as "pellets") of this embodiment involves melt-kneading a cellulose fiber-containing resin sheet (hereinafter simply referred to as "sheet") in a screw kneader to produce cellulose fiber-containing resin pellets, in which the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw kneader (cross-sectional area of ​​cellulose fiber-containing resin sheet / inlet area of ​​screw kneader) is 0.065 or less. The production method of the present invention is more productive than conventional methods. Furthermore, the molded article obtained from the pellets has excellent bending rigidity and impact resistance.

[0011] The detailed mechanism by which the above-mentioned effects are obtained is partially believed to be as follows. When cellulose fibers and a resin component are supplied and melt-kneaded in the melt-kneading process, the cellulose fibers are hydrophilic, while the resin component is generally hydrophobic, resulting in aggregation of the cellulose fibers and poor dispersibility of the cellulose fibers in the resin component. Furthermore, the need for high shear force can lead to breakage of the cellulose fibers or the formation of fine fibers. It is believed that a molded body obtained from the pellets thus obtained has poor bending rigidity and impact resistance. The present inventors have conducted studies to solve the above-mentioned problems, and International Publication No. 2023 / 074842 describes a method in which a fiber aggregate containing cellulose fibers such as pulp fibers and a resin component (resin A) is first produced by dry papermaking, and the fiber aggregate sheet is compressed into a sheet-like shape, and the resulting fiber aggregate sheet is melt-kneaded to produce pellets, which are then molded to produce a molded body. In the examples of WO 2023 / 074842, when the material is fed to a melt kneader, it is cut into a size that can be fed to the melt kneader and then fed to the melt kneader. However, when feeding the cut raw material, the raw material is bulky and difficult to penetrate into the screw in the melt kneader, resulting in low productivity. The inventors of the present invention have considered that by feeding the sheet-like raw material directly into the melt kneader, once it penetrates into the screw of the melt kneader, the sheet is continuously fed, thereby significantly improving pellet productivity. As a result of extensive research, it has been found that by setting the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw kneader to 0.065 or less, it is possible for the sheet to penetrate into the screw and be continuously fed to the screw kneader. Furthermore, as described above, the molded body produced using pellets obtained by continuously supplying sheet-like raw material has excellent bending rigidity and impact resistance, similar to pellets obtained by supplying cut raw material, and further, it was found that supplying sheet-like raw material results in even better bending rigidity and impact resistance than when cut raw material is supplied.This is thought to be because smooth supply to the kneader reduces the residence time inside the kneader and the time the cellulose fibers are exposed to heat, thereby suppressing breakage and thermal degradation of the cellulose fibers. Note that the mechanism by which the effects of the present invention are obtained is not limited to the above. The present invention will be described in further detail below.

[0012] <Step of Producing Pellets> The method for producing cellulose fiber-containing resin pellets of this embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets.

[0013] (Cross-sectional area of ​​cellulose fiber-containing resin sheet / inlet area of ​​screw-type kneader) In this embodiment, the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet (cm 2 ) / Inlet area of ​​screw type kneader (cm 2 )) is 0.065 or less. By setting the above ratio to 0.065 or less, the cellulose fiber-containing resin sheet can be easily bitten into the screw of the kneader, and the cellulose fiber-containing resin sheet can be continuously supplied to the kneader. The above ratio is preferably 0.063 or less, more preferably 0.061 or less, and even more preferably 0.060 or less. The lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 0.010 or more, more preferably 0.020 or more, and even more preferably 0.030 or more. The cross-sectional area of ​​the cellulose fiber-containing resin sheet is calculated from the width and thickness of the sheet. The width and thickness of the sheet are measured by the method described in the Examples. The inlet area of ​​the screw-type kneader may be measured using a vernier caliper or the like.

[0014] The cross-sectional area (cm 2 ) and the inlet area of ​​the screw mixer (cm 2 ) can vary greatly depending on the scale of the kneader used, but for example, the cross-sectional area (cm 2 ) is preferably 0.5 cm 2 More preferably, 1.0 cm2 and preferably 100 cm 2 Less than 50 cm, more preferably 2 The area of ​​the inlet of the screw-type kneader (cm 2 ) is, for example, preferably 5 cm 2 More than 10cm, preferably 2 and preferably 30,000 cm 2 or less, more preferably 10,000 cm 2 More preferably, 5000 cm 2 The following is the result.

[0015] In this embodiment, the cross-sectional area (cm ) of the cellulose fiber-containing resin sheet relative to the screw diameter (mm) of the screw-type kneader is 2 ) (cross-sectional area (cm ) of the cellulose fiber-containing resin sheet 2 ) / screw diameter (mm)) is preferably 0.100 or less. When the ratio is 0.100 or less, the cellulose fiber-containing resin sheet is easily bitten into the screw of the kneader, and the cellulose fiber-containing resin sheet can be continuously supplied to the kneader, which is preferable. The ratio is more preferably 0.090 or less, even more preferably 0.085 or less, and even more preferably 0.080 or less. The lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 0.010 or more, more preferably 0.020 or more, and even more preferably 0.030 or more.

[0016] The screw diameter (mm) of the screw-type kneader described above can vary greatly depending on the scale of the kneader used, but is, for example, preferably 10 mm or more and 500 mm or less, more preferably 20 mm or more, even more preferably 30 mm or more, and more preferably 300 mm or less, even more preferably 150 mm or less. The screw diameter (mm) is often disclosed by the kneader manufacturer, and the manufacturer's value may be used. Alternatively, it may be measured using a vernier caliper or the like.

[0017] In this embodiment, the ratio of the discharge speed (kg / h) to the peripheral speed (m / min) of the screw of the screw-type kneader (discharge speed / peripheral speed) is preferably 0.50 or more. A discharge speed to peripheral speed of 0.50 or more is preferable because it increases productivity and suppresses breakage and pulverization of cellulose fibers due to excessive shear. The ratio of the discharge speed to peripheral speed is more preferably 0.60 or more, even more preferably 0.70 or more, still more preferably 0.80 or more, and even more preferably 0.90 or more. There is no particular upper limit, but from the viewpoint of ease of production, it is preferably 3.00 or less, more preferably 2.50 or less, and even more preferably 2.00 or less.

[0018] The peripheral speed (m / min) of the screw of the screw-type kneader is, for example, preferably 0.3 m / min or more and 500 m / min or less, more preferably 1.0 m / min or more, even more preferably 3 m / min or more, and more preferably 300 m / min or less, and even more preferably 100 m / min or less, from the viewpoints of productivity and suppression of shear heating. The peripheral speed (m / min) of the screw may be appropriately set during operation of the kneader. Furthermore, the discharge rate (kg / h) may vary greatly depending on the scale of the kneader used, but from the viewpoints of productivity and ease of production, it is preferably 1 kg / h or more and 1000 kg / h or less, more preferably 3 kg / h or more, and even more preferably 5 kg / h or more.

[0019] <Cellulose fiber-containing resin sheet> The pellet manufacturing method of this embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw kneader to manufacture pellets. In this embodiment, the cellulose fiber-containing resin sheet is fed in sheet form through a raw material inlet of the screw kneader. The cellulose fiber-containing resin sheet contains a resin component (resin A) in addition to cellulose fibers. Resin A is preferably a thermoplastic resin and preferably contains a fibrous resin (resin fiber). The cellulose fiber-containing resin sheet may be obtained by any method, but is preferably manufactured by the following steps 1 and 2. Step 1: A fiber aggregate manufacturing step in which a fiber aggregate containing cellulose fibers and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step in which the fiber aggregate is compressed to manufacture a cellulose fiber-containing resin sheet. A preferred method for manufacturing a cellulose fiber-containing resin sheet in this embodiment, which includes steps 1 and 2, will now be described in detail.

[0020] (Step 1) Step 1 is a fiber assembly manufacturing step in which a fiber assembly containing cellulose fibers and resin A is manufactured by dry papermaking.

[0021] [Cellulose Fibers] There are no particular limitations on the production method or type of cellulose fibers. Pulp fibers are preferred as cellulose fibers, and examples thereof include chemical pulps such as kraft pulp from hardwoods and / or softwoods, mechanical pulps such as SGP, RGP, BCTMP, and CTMP, waste paper pulp such as deinked pulp, and non-wood pulps such as kenaf, jute, bagasse, bamboo, straw, and hemp. Chlorine-free pulps such as ECF pulp and TCF pulp can also be used. Pulp fibers are preferred as cellulose fibers, but are not limited thereto. For example, paper flour, wood flour, etc. may also be used.

[0022] Among the above pulp fibers, kraft pulp fibers, particularly long-fiber softwood bleached kraft pulp fibers (NBKP), are preferably used as cellulose fibers because the resulting molded articles have superior flexural modulus and impact resistance.

[0023] From the viewpoint of improving the flexural modulus and impact resistance of the resulting molded article and from the viewpoint of ease of production of the fiber assembly, the average fiber length of the cellulose fibers is preferably 0.1 mm or more and 50 mm or less, more preferably 0.5 mm or more, even more preferably 1 mm or more, and more preferably 10 mm or less, even more preferably 5 mm or less, and still more preferably 2.5 mm or less. The average fiber length of the cellulose fibers is measured by the method described in the Examples.

[0024] From the viewpoint of improving the bending rigidity and impact resistance of the resulting molded article and from the viewpoint of ease of production of the fiber assembly, the average fiber width of the cellulose fibers is preferably 1 μm or more and 150 μm or less, more preferably 5 μm or more, even more preferably 10 μm or more, still more preferably 15 μm or more, and more preferably 100 μm or less, even more preferably 80 μm or less, and still more preferably 50 μm or less. The average fiber width of the cellulose fibers is measured by the method described in the Examples.

[0025] In this embodiment, when the fiber aggregate is formed by an air-laid method, the cellulose fibers may be in the form of, for example, defibrated dry pulp.

[0026] The cellulose fibers are preferably unbeaten cellulose fibers from the viewpoint of improving the impact resistance of the resulting molded body. For the molded body to exhibit impact resistance, the cellulose fibers must be properly pulled out of the resin when an impact is applied. For this purpose, unbeaten cellulose fibers with a low fine fiber ratio are preferred, and unbeaten pulp fibers are even more preferred. From the above viewpoints, the fine fiber ratio of the cellulose fibers is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less, with no particular lower limit. The fine fiber ratio of the cellulose fibers is measured by the method described in the Examples.

[0027] The content of cellulose fibers in the cellulose fiber-containing resin sheet is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, even more preferably 25% by mass or more, and more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 75% by mass or less, from the viewpoint of obtaining a molded product having excellent flexural modulus and impact resistance, and from the viewpoint of the productivity and ease of manufacturing of the cellulose fiber-containing resin sheet.

[0028] [Resin A] Examples of resin A components include polyolefin, polyvinyl chloride, polystyrene, ABS (acrylonitrile-butadiene-styrene), acrylonitrile-styrene, polyester, acrylic resin, polyamide, polyacetal, polycarbonate, polybutylene succinate, and polylactic acid. Furthermore, resins or elastomers exemplified as lubricants, plasticizers, nucleating agents, flame retardants, antistatic agents, fillers, and papermaking chemicals listed in the section [Other Components] below may also be used. In other words, resin A refers to the resin component contained in the molded body. As described in the molded body manufacturing method described below, the molded body of this embodiment is preferably manufactured by producing a cellulose fiber aggregate containing cellulose fibers and resin A by dry papermaking, followed by compressing the cellulose fiber-containing resin sheet. In other words, at least resin A is preferably blended with the cellulose fiber aggregate. In the manufacturing of the molded body, further resins or elastomers may be added.

[0029] In the present invention, the resin A contained in the fiber assembly can be any of fibers, powder, granules, and pellets. Among these, from the viewpoint of ease of papermaking in step 1 described below, the resin A contained in the fiber assembly is preferably fiber or powder, and more preferably fiber. That is, the resin A contained in the fiber assembly preferably contains resin fiber or resin powder, more preferably resin fiber, and even more preferably resin fiber. Preferred examples of the resin A fiber contained in the fiber assembly include polyolefin fiber, polyvinyl chloride fiber, polyester fiber, acrylic fiber, polyamide fiber, polycarbonate fiber, and polylactic acid fiber. Preferred examples of the resin A powder, granule, and pellet components contained in the fiber assembly include polyolefin, polyvinyl chloride, polyester, acrylic, polyamide, polycarbonate, polylactic acid, polystyrene, ABS, acrylonitrile-styrene, polyacetal, and polybutylene succinate. In particular, preferred examples of resin A powder include polyolefin powder, polystyrene powder, ABS powder, acrylonitrile-styrene powder, polyacetal powder, and polybutylene succinate powder. Examples of the polyolefin include those specific examples of polyolefin in the polyolefin fiber shown below. Among these, polyolefin fiber is preferred as the resin A to be contained in the fiber assembly. Resin A to be contained in the fiber assembly can be used alone or in combination of two or more. For example, a combination of two types of resin A, polylactic acid fiber and polybutylene succinate powder, can be used.

[0030] -Polyolefin Fiber-In this embodiment, when polyolefin fiber is used as resin A to be contained in the fiber assembly, the polyolefin constituting the polyolefin fiber is not particularly limited, and examples thereof include polyolefin (unmodified polyolefin) and modified polyolefin. From the viewpoint of ease of molding and suppression of deterioration of cellulose fiber, the melting point of the polyolefin constituting the polyolefin fiber is preferably 80°C or higher and 200°C or lower, more preferably 195°C or lower, even more preferably 180°C or lower, more preferably 90°C or higher, even more preferably 100°C or higher.

[0031] Examples of polyolefins include polyethylene, polypropylene, and ethylene-propylene copolymers (also referred to as propylene-ethylene copolymers), with polyethylene and polypropylene being preferred. Regarding modified polyolefins, examples of methods for modifying polyolefins include acid modification and chlorination. Among these, acid modification is preferred from the viewpoint of improving affinity with cellulose fibers. The acid-modifying component used for the acid modification of acid-modified polyolefins is preferably an unsaturated carboxylic acid component. Examples of unsaturated carboxylic acid components include components derived from unsaturated carboxylic acids and their acid anhydrides. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, and crotonic acid. Among these, the unsaturated carboxylic acid component is preferably at least one selected from acrylic acid, methacrylic acid, maleic acid, and maleic anhydride, and particularly preferably at least one selected from maleic acid and maleic anhydride. Polyolefins modified with at least one of maleic acid and maleic anhydride are also referred to as maleic acid-modified polyolefins. The acid-modified polyolefin is preferably a maleic acid-modified polyolefin, more preferably a maleic acid-modified polyethylene or a maleic acid-modified polypropylene. The acid-modified polyolefin may be at least partially acid-modified.

[0032] The polyolefin is particularly preferably at least one selected from the group consisting of polyethylene, polypropylene, polyethylene at least partially modified with maleic acid, polypropylene at least partially modified with maleic acid, and ethylene-propylene copolymer. From the viewpoint of improving the flexural modulus of the resulting molded article, it is preferable that the polyolefin contains an acid-modified polyolefin, more preferably the polyolefin contains at least one of polyethylene at least partially modified with maleic acid and polypropylene at least partially modified with maleic acid, and even more preferably the polyolefin contains polyethylene at least partially modified with maleic acid. Furthermore, from the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that the polyolefin does not contain an acid-modified polyolefin, and it is more preferable that the polyolefin contains only polyethylene, polypropylene, and ethylene-propylene copolymer. The polyolefin fibers may be used alone or in combination of two or more types.

[0033] The polyolefin fiber may be a composite fiber made of two or more polyolefins, and examples thereof include split fibers, sea-island fibers, sheath-core fibers, and laminated fibers. Among these, sheath-core fibers are preferred from the viewpoint of obtaining a molded article having excellent bending rigidity and impact resistance. When using sheath-core fibers, fibers with a concentric cross-sectional structure or an eccentric cross-sectional structure are used, but fibers with a concentric cross-sectional structure are preferred. Fibers with a concentric cross-sectional structure are preferred because they can obtain a more uniform fiber assembly.

[0034] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fiber length of the polyolefin fiber is preferably 0.1 mm or more and 50 mm or less, more preferably 1.0 mm or more, even more preferably 2.0 mm or more, even more preferably 3.0 mm or more, and more preferably 20 mm or less, even more preferably 10 mm or less. The fiber length of the polyolefin fiber is measured by the method described in the Examples.

[0035] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fiber diameter of the polyolefin fiber is preferably 0.1 μm or more and 100 μm or less, more preferably 1 μm or more, even more preferably 10 μm or more, and more preferably 80 μm or less, even more preferably 50 μm or less. The fiber diameter of the polyolefin fiber is measured by the method described in the Examples.

[0036] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fineness of the polyolefin fiber is preferably 0.01 dtex or more and 100 dtex or less, more preferably 0.1 dtex or more, even more preferably 1 dtex or more, and more preferably 50 dtex or less, even more preferably 10 dtex or less. The fineness of the polyolefin fiber is measured by the method described in the examples.

[0037] When the resin A contained in the fiber aggregate is a polyolefin fiber, the content of the polyolefin fiber in the fiber aggregate is preferably 90% by mass or less from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, more preferably 80% by mass or less, even more preferably 75% by mass or less, and even more preferably 65% ​​by mass or less from the viewpoint of productivity and ease of production, and even more preferably 50% by mass or less, particularly preferably 45% by mass or less from the viewpoint of biomass conversion degree and productivity. Also, from the same viewpoint, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. Note that when two or more types of polyolefin fiber are used, the above content refers to the total content of the polyolefin fibers.

[0038] When resin A is a fiber other than polyolefin fiber, the preferred fiber length, fiber diameter, fineness, and content of the fiber are the same as the preferred fiber length, fiber diameter, fineness, and content of polyolefin fiber, respectively. When resin A is a powder, granules, or pellets, the preferred content of the powder, granules, or pellets is the same as the preferred content of the polyolefin fiber. When resin A is a powder, granules, or pellets, the particle size of the powder, granules, or pellets is not particularly limited.

[0039] [Other Components] When the resin A in the fiber assembly of this embodiment is a polyolefin fiber, the fiber assembly may contain other components in addition to the cellulose fiber and polyolefin fiber described above. Examples of other components include an elastomer and a binder component, which will be described later. When a binder component is contained, the content of the binder component is preferably 0.1% by mass or more and 40% by mass or less, more preferably 0.3% by mass or more and 30% by mass or less, even more preferably 0.4% by mass or more and 20% by mass or less, and even more preferably 0.5% by mass or more and 10% by mass or less, relative to the total mass of the fiber assembly. By keeping the content of the binder component within the above range, handleability and the like can be improved when producing a molded product. Examples of binder components that can be used include various starches, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose, acrylic resins, styrene-(meth)acrylic acid ester copolymer resins, urethane resins, polyvinyl alcohol (PVA) resins, various starches, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymers, alkali salts of styrene-maleic anhydride copolymers, alkali salts of isobutylene-maleic anhydride copolymers, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, and ethylene-vinyl acetate copolymers.

[0040] The fiber assembly may further contain fillers and papermaking chemicals. Examples of fillers include mineral pigments such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, as well as organic pigments such as polystyrene resins, urea resins, melamine resins, acrylic resins, and vinylidene chloride resins. Examples of papermaking chemicals include paper strength agents, retention aids, drainage aids, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, and slime control agents. Examples of paper strength agents include polyacrylamide. Wet strength agents can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.

[0041] The fiber assembly may further contain a fatty acid metal salt. The fatty acid metal salt is preferably a metal salt of an aliphatic carboxylic acid, and the aliphatic carboxylic acid is preferably a saturated or unsaturated aliphatic carboxylic acid having from 12 to 24 carbon atoms. Specific examples include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, heneicosylic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid. Examples of metal elements that form the metal salt include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium, and barium; and Group 3 elements such as zinc and aluminum, with calcium, magnesium, zinc, and aluminum being preferred. Examples of fatty acid metal salts include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, lithium stearate, zinc laurate, and barium laurate. Among these, calcium stearate, magnesium stearate, zinc stearate, aluminum stearate, calcium oleate, magnesium oleate, zinc oleate, aluminum oleate, zinc laurate, or calcium laurate is preferred, with calcium stearate being more preferred. From the viewpoint of bending rigidity and impact resistance, the content of fatty acid metal salt in the molded product is 0.1% by mass or more and 10% by mass or less, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.8% by mass or more, and preferably 9% by mass or less, more preferably 8% by mass or less, even more preferably 7% by mass or less, and even more preferably 6% by mass or less.

[0042] When other components are contained, the content of the other components excluding cellulose fibers and polyolefin fibers is preferably 0.1 mass% or more and 40 mass% or less, more preferably 0.3 mass% or more and 30 mass% or less, even more preferably 0.4 mass% or more and 20 mass% or less, and still more preferably 0.5 mass% or more and 10 mass% or less, relative to the total mass of the fiber assembly.

[0043] [Fiber aggregate manufacturing process] Next, the fiber aggregate manufacturing process will be described. In the following explanation of the fiber aggregate manufacturing process, it will be explained that a preferred polyolefin fiber is used as the resin A. When a resin other than polyolefin fiber is used as the resin A, the resin used will be read as the resin A instead of polyolefin fiber, and the other explanations will be the same. Note that the resin A can be used alone or in combination of two or more types, as described below.

[0044] In the process for producing a fiber assembly (Step 1) of this embodiment, cellulose fibers and resin A are produced by dry papermaking. The process for producing a fiber assembly preferably includes a step of mixing cellulose fibers and polyolefin fibers in air and depositing the mixture. That is, the fiber assembly of this embodiment is preferably a dry nonwoven fabric.

[0045] When producing a fiber assembly using a dry papermaking method, it is preferable to use an airlaid method. The airlaid method is a method in which an airflow containing raw fibers, such as polyolefin fibers and cellulose fibers defibrated in the air and uniformly mixed in the airflow, is discharged onto a mesh-like endless belt equipped with a suction box below to form an airlaid web. That is, the airlaid method includes a step of mixing cellulose fibers and polyolefin fibers in the air and depositing them. In the airlaid method, the above operation may be repeated multiple times as necessary.

[0046] The web formed by the above method is made into a sheet by the fiber bonding process described below. Examples of the fiber bonding process include a needle punching method, in which polyolefin fibers or cellulose fibers are entangled by passing needles perpendicular to the web surface to form a sheet. This bonding process is preferably used in combination with a carding web formation method. The fiber bonding process can also be performed using a thermal bonding process, in which a heat-fusible adhesive incorporated into a dry-laid web is heated to fuse the raw fibers together; a chemical bonding process, in which an adhesive is applied to the resulting dry-laid web to bond the raw fibers; or a multi-bond process, which combines the thermal and chemical bonding processes.

[0047] In the thermal bonding method, it is preferable to heat at a temperature at least 20° C. higher than the melting point of the heat-fusible adhesive. Examples of the heat treatment include hot air treatment and hot-air treatment followed by low-pressure heat and pressure treatment.

[0048] When the thermal bond method or multi-bond method is employed, it is preferable to use a particulate or fibrous heat-fusible adhesive. The heat-fusible adhesive may be the polyolefin fiber or binder component described above. As the particulate heat-fusible adhesive, heat-fusible resin particles such as polyethylene, polypropylene, polyester low-melting point polyethylene terephthalate, low-melting point polyamide, low-melting point polylactic acid, and polybutylene succinate are used. As the fibrous heat-fusible adhesive, resins such as low-melting point polyethylene terephthalate, low-melting point polylactic acid, polybutylene succinate (PBS), and polyethylene terephthalate (PET), low-melting point polyamide, acrylic resin, and polyvinyl acetate (PVAc) are used. Furthermore, as the heat-fusible synthetic fiber, a core-sheath type heat-fusible composite synthetic fiber obtained by combining two types of resins with different melting points and in which only the surface of the fiber melts, can also be preferably used. A sheath-core heat-fusible composite synthetic fiber has a core made of a resin with a high melting point and a sheath made of a resin with a low melting point formed on the outer periphery thereof. Specific examples include a combination of two resins with different melting points (PET / PET composite fiber, PE / PET composite fiber, MAPE / PP composite fiber, PP / PET composite fiber, PE / PP composite fiber, PVAc / PET composite resin).

[0049] Furthermore, when a chemical bonding method is used to bond the fibers, it is preferable to add a binder component to bond the fibers together. The binder component can be appropriately selected as needed, and examples include solution-type binders such as starch, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose sodium salt, polyvinyl alcohol (PVA), and sodium polyacrylate, as well as emulsion-type binders such as polyacrylic acid esters, acrylic-styrene copolymers, polyvinyl acetate, ethylene-vinyl acetate copolymers, acrylonitrile-butadiene copolymers, methyl methacrylate-butadiene copolymers, urea-melamine resins, and styrene-butadiene copolymer resins. It is also preferable to use the binder components described above. The binders can be in various forms, such as fibers, powders, granules, solutions, or emulsions, and two or more types can be used in combination.

[0050] In a fiber aggregate produced by the above-described dry papermaking method, the fibers constituting the fiber aggregate are three-dimensionally oriented randomly in the longitudinal, width, and thickness directions. Therefore, in this embodiment, the tensile strength of the fiber aggregate in the first direction and the tensile strength in the second direction are approximately the same. That is, in this embodiment, a fiber aggregate with excellent isotropy in the planar direction is obtained.

[0051] In the manufacturing process of the fiber assembly, any sheet that does not impair moldability may be laminated on the fiber assembly to manufacture a laminated sheet. For example, the optional sheet can be laminated on the surface of the fiber assembly or between sheets when laminating the fiber assembly. Sheets such as tissue and nonwoven fabric can be used as the optional sheet to be laminated. These optional sheets are laminated for the purpose of improving the surface properties of the fiber assembly or cellulose fiber-containing resin sheet during the manufacturing process, improving productivity, and imparting other functions.

[0052] (Step 2) Step 2 is a cellulose fiber-containing resin sheet production step in which the fiber aggregate obtained in Step 1 is compressed to produce a cellulose fiber-containing resin sheet. A sheet-like cellulose fiber-containing resin sheet is obtained by compressing the fiber aggregate obtained in Step 1. The compression may be performed simultaneously with the heat treatment or after the heat treatment.

[0053] Compression of the fiber aggregate can be achieved by applying pressure to the fiber aggregate using a roll press. Heating may be performed simultaneously during the roll press treatment, resulting in a heat-press treatment. The roll press treatment uses metal rolls or resin rolls to apply pressure, allowing the density of the resulting cellulose fiber-containing resin sheet to be controlled as desired. Specifically, a cellulose fiber-containing resin sheet with any density can be obtained by setting any number of rolls, any temperature, and any clearance for the roll press treatment, and heating and pressurizing the sheet. The sheet may be compressed to the desired density by passing through multiple rolls.

[0054] Compression of the fiber aggregate can also be achieved by pressure treatment using a hot press. The density of the resulting cellulose fiber-containing resin sheet can be controlled as desired by subjecting a fiber aggregate cut to an appropriate size, or a cellulose fiber-containing resin sheet that has been subjected to the roll press treatment, to pressure treatment using an autoclave method or a mold press method. Heating to a temperature of 100°C or higher and applying pressure to 2 MPa or higher can produce a cellulose fiber-containing resin sheet with a higher density than that obtained by pressure treatment using a roll press. A pre-pressing step may be included before achieving the above heating and pressure conditions. It is also preferable to perform pre-pressing at a lower pressure under the desired heating conditions, and then increase the pressure and perform pressure treatment using a hot press.

[0055] The pressure treatment step by hot pressing may be a stamping molding method. In the stamping molding method, a fiber assembly is heated in advance, the polyolefin is melted and softened, and the assembly is placed in a mold, the mold is then closed to clamp the assembly, and the assembly is then cooled under pressure. For heating, a heating device such as a far-infrared heater, a heating plate, a high-temperature oven, or a dielectric heater may be used.

[0056] The pressure treatment step by hot pressing may be a vacuum molding method. Vacuum molding can improve the adhesion between the fiber aggregate and the mold by creating a vacuum between the fiber aggregate and the mold, thereby improving moldability. Vacuum molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, vacuum molding is performed in the step of heating the fiber aggregate, melting and softening the polyolefin, placing it inside the mold, and then closing the mold to clamp it. In vacuum molding, vacuum suction is performed from the mold side. The molding pressure in vacuum molding is usually 1.0 kg / cm. 2 The molding is carried out for about 0.1 seconds to 60 seconds.

[0057] The pressure treatment step by heat pressing may be a pressure molding method. In the pressure molding method, compressed air is blown onto the fiber assembly to make it adhere to the mold, thereby increasing the adhesion between the fiber assembly and the mold. The pressure molding is preferably carried out in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, and the polyolefin is placed in a melted and softened state in a mold, and then compressed air is blown onto the fiber assembly side to perform molding. The pressure molding is carried out at a pressure of 3 kg / cm. 2 More than 8kg / cm 2 The molding is often carried out at a compressed air pressure of the following value, and molding is preferably carried out for 0.1 to 60 seconds.

[0058] Compression of the fiber assembly can also be achieved by supercalendering. In the supercalendering, the fiber assembly is molded by passing it between heated rollers while applying nip pressure. The heating temperature of the rollers used is preferably at least 10°C higher, more preferably at least 20°C higher, and even more preferably at least 30°C higher than the melting point of the polyolefin fiber, and is preferably not higher than 100°C, more preferably not higher than 90°C, and even more preferably not higher than 80°C than the melting point of the polyolefin fiber. The nip pressure is preferably at least 100 kg / cm, more preferably at least 150 kg / cm, and even more preferably at least 200 kg / cm, and is preferably not higher than 450 kg / cm, more preferably not higher than 400 kg / cm, and even more preferably not higher than 350 kg / cm. The number of nip stages is preferably at least 1, more preferably at least 3, and even more preferably at least 5, and preferably not higher than 20, more preferably not higher than 18, and even more preferably not higher than 16. When compressing a fiber aggregate to produce a cellulose fiber-containing resin sheet, a plurality of cellulose fiber-containing resin sheets may be stacked and compressed as appropriate depending on the desired thickness of the cellulose fiber-containing resin sheet, etc.

[0059] In the cellulose fiber-containing resin sheet of this embodiment, the tensile strength in a first direction is T, and the tensile strength in a second direction perpendicular to the first direction is Y. A T / Y ratio of 0.5 to 1.5 is preferred. By setting the T / Y ratio to 0.5 to 1.5, the fibers constituting the cellulose fiber-containing resin sheet are extremely uniformly mixed, resulting in a molded product that has excellent impact resistance as well as rigidity and strength against bending. T / Y is preferably 0.60 or more, more preferably 0.70 or more, even more preferably 0.80 or more, even more preferably 0.85 or more, and is preferably 1.40 or less, more preferably 1.30 or less, even more preferably 1.20 or less, and even more preferably 1.15 or less. The first direction of the cellulose fiber-containing resin sheet is any one direction in the planar direction of the cellulose fiber-containing resin sheet. However, if the fibers contained in the cellulose fiber-containing resin sheet are oriented in any direction in the planar direction, the orientation direction is defined as the first direction. Furthermore, when the flow direction in the manufacturing process of the fiber aggregate by dry papermaking is known, the flow direction is referred to as the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the flow direction in the manufacturing process is referred to as the first direction (MD direction), and the flow direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes referred to as the T-mesh. The second direction of the fiber aggregate is one direction in the planar direction of the fiber aggregate and is a direction perpendicular to the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the direction perpendicular to the flow direction in the manufacturing process is referred to as the second direction (CD direction), and the second direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes referred to as the Y-mesh. The tensile strength in the first and second directions of the cellulose fiber-containing resin sheet is measured in accordance with JIS P 8113:2006. The tensile strength in each direction was measured using a tensile tester, Tensilon manufactured by A&D Co., Ltd., at a speed of 20±5 mm / min on a strip of 15±0.1 mm×180±1 mm.

[0060] In this embodiment, the cellulose fiber-containing resin sheet is a sheet-like product obtained by mixing at least cellulose fibers and resin A (preferably polyolefin fibers) and then dry-pressing the mixture. The sheet is obtained by pressing a cotton-like fiber aggregate (hereinafter also referred to as a cotton-like fiber aggregate) after dry-pressing, and may have various bulk specific gravities (densities). The bulk specific gravity of the cellulose fiber-containing resin sheet to be fed to the screw-type kneader is preferably 0.10 g / mL or more, more preferably 0.15 g / mL or more, and preferably 0.60 g / mL or less, more preferably 0.50 g / mL or less, and even more preferably 0.40 g / mL or less, from the viewpoints of ease of compression in step 2, ease of subsequent melt-kneading, and ease of cutting when cutting for feeding to the melt-kneader. The bulk specific gravity of the cellulose fiber-containing resin sheet is measured by the method described in the examples.

[0061] (Pellet manufacturing process) The method for manufacturing cellulose fiber-containing resin pellets of this embodiment includes a process of melt-kneading a cellulose fiber-containing resin sheet in a screw kneader to manufacture pellets. Here, the cellulose fiber-containing resin sheet is supplied to the melt kneader while still in sheet form. At this time, the cellulose fiber-containing sheet may be cut to a width within a desired range, as necessary, from the viewpoint of setting the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw kneader within a desired range. Furthermore, if the kneader has multiple inlets, the cellulose fiber-containing sheet may be supplied from multiple inlets.

[0062] The method for producing the pellets is not particularly limited, and is not particularly limited as long as the cellulose fiber-containing resin sheet is supplied and melt-kneaded in a screw-type kneader. Examples of the screw-type kneader include a single-screw kneader and a twin-screw kneader, and from the viewpoint of kneading efficiency, a twin-screw kneader is preferred. Examples of methods include feeding a cellulose fiber-containing resin sheet into a screw-type kneader and melt-kneading it, followed by: (1) extruding it into a strand shape and cooling and solidifying it to obtain cellulose-containing resin pellets; (2) cooling and solidifying the molten mixture either directly or after being stretched into a sheet shape, and crushing it in a crusher to obtain cellulose fiber-containing resin pellets; (3) extruding it into a rod or cylindrical shape and cooling it to obtain cellulose fiber-containing resin pellets; (4) extruding it through a T-die to obtain a sheet or film-like cellulose fiber-containing resin, which is then cut or crushed to obtain cellulose fiber-containing resin pellets; or (5) cutting the molten kneaded product immediately after extrusion with a rotary blade in air or water to obtain cellulose fiber-containing resin pellets. The size of the resulting pellets is not particularly limited, but is preferably 1 to 10 mm from the viewpoint of ease of feeding into an injection molding machine.

[0063] The melt-kneading temperature (barrel set temperature) is not particularly limited, but is preferably adjusted so that the temperature of the melt-kneaded product (the temperature of the actually obtained kneaded product, the resin temperature) is at least 5°C higher than the melting point of the polyolefin, more preferably at least 10°C higher, and even more preferably at least 15°C higher. From the viewpoint of deterioration of the cellulose fiber, the barrel set temperature is preferably at most 100°C higher than the melting point of the polyolefin, more preferably at most 90°C higher, and even more preferably at most 80°C higher. The temperature of the melt-kneaded product becomes higher than the melt-kneading temperature (barrel set temperature) due to shear heat generated during melt-kneading. In other words, it varies depending on various conditions during melt-kneading, such as the melt-kneading temperature (barrel set temperature), discharge rate, rotation speed, and screw design of the melt-kneader. In the case of the method described in the examples, the temperature of the melt-kneaded product is about 20 to 40°C higher than the melt-kneading temperature (barrel set temperature), and therefore the melt-kneading temperature (barrel set temperature) is about 20 to 40°C lower than the preferred temperature of the melt-kneaded product.

[0064] Various conditions during melt-kneading, such as the discharge rate and rotation speed, may be adjusted according to known techniques. It is preferable to appropriately adjust the discharge rate (discharge rate) relative to the screw peripheral speed described above so that it is within the desired range. When the melt-kneading device is a twin-screw extruder, it is desirable to design the screw so that the kneading force is as weak as possible. In the present invention, the cellulose fibers and resin A are uniformly dispersed in the fiber assembly sheet in advance, and even when melt-kneading is performed without applying high shear force, the dispersion state of the cellulose fibers in the fiber assembly sheet is maintained as is, resulting in pellets with excellent cellulose fiber dispersion. Therefore, weak kneading force can prevent cellulose fiber breakage. Specifically, R-type kneading parts are mainly used, and the number of L-type and N-type kneading parts is preferably the same or less than the number of R-type kneading parts, and more preferably less than the number of R-type kneading parts. When melt-kneading is performed using only cut chips of a fiber assembly sheet, the kneading mix may be composed of only R-type kneading parts, without using L-type or N-type kneading parts. The kneading parts are preferably 5 or less parts, more preferably 3 or less parts, out of the total 10 parts divided into the screw. When melt-kneading is performed using only cut chips of a fiber assembly sheet, the kneading parts may be only 1 part.

[0065] In addition, during melt kneading, a resin component may be blended with the cellulose fiber-containing resin sheet and melt kneaded. Examples of the resin component include the resin components listed above for resin A and the elastomers described below, with polyolefin resins and the elastomers described below being preferred. Blending at least one selected from resin A and an elastomer during melt kneading is preferred because it results in a molded product with superior impact resistance. That is, the resulting cellulose fiber-containing resin pellets may contain components blended during melt kneading in addition to the components derived from the cellulose fiber-containing resin sheet. The elastomer that may be blended during melt kneading refers to a polymer compound that exhibits elastic deformation, i.e., a substance that softens and becomes fluid when heated and returns to a rubbery state when cooled. Specifically, elastomers have a structure consisting of two polymers: hard segments and soft segments. The hard segments act as crosslinking points, while the soft segments exhibit rubbery elasticity, resulting in elasticity. Therefore, at room temperature, the hard segments aggregate to form a pseudo-crosslinked state, exhibiting rubber-like physical properties, but at high temperatures, they melt, losing their crosslinking function and allowing plastic deformation. Depending on the combination of hard segment polymers and soft segment polymers, elastomers are classified into polystyrene-based, olefin / alkene-based, polyester-based, polyvinyl chloride-based, polyurethane-based, polyamide-based, polyacrylic elastomers, silicone-based, polyimide-based, and other types. Furthermore, even within the same type, properties vary depending on the ratio of hard and soft segments and molecular weight. For example, polystyrene-based elastomers may use styrene for the hard segment and butadiene for the soft segment. In this case, a high styrene content results in high hardness and improved compatibility with polystyrene and polyphenylene ether, while a low styrene content results in low hardness, high flexibility, and improved compatibility with polyolefins. Furthermore, a high molecular weight results in improved temperature and mechanical properties, while a low molecular weight results in improved processability and transparency. An example of a polystyrene-based elastomer is the Tuftec series manufactured by Asahi Kasei Corporation. For example, an olefin / alkene-based elastomer may be a combination of ethylene, propylene, and 1-butene.The density, modulus of elasticity, and melting point can be changed by varying the combination and ratio. Furthermore, the structure when mixed with the resin also varies, with some being dispersed in an island-like manner and others being compatible. Examples of olefin / alkene-based elastomers include the Toughmer series manufactured by Mitsui Chemicals, Inc. Among these, polystyrene-based elastomers and olefin / alkene-based elastomers are preferred from the viewpoint of impact resistance, etc. Examples of elastomers include the various elastomers described in paragraphs 0043 to 0065 of Publication No. 2020 / 080328. The method of adding the elastomer is not particularly limited, and it is preferable to supply the elastomer together with the cellulose fiber-containing resin sheet during melt-kneading of the cellulose fiber-containing resin sheet and melt-knead it.

[0066] When the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is, from the viewpoint of improving the flexural modulus, preferably 55% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, still more preferably 40% by mass or less, and particularly preferably 35% by mass or less, relative to the total mass of resin A and the elastomer. Furthermore, when the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is, from the viewpoint of improving the impact resistance, preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, still more preferably 12% by mass or more, and particularly preferably 15% by mass or more, relative to the total mass of resin A and the elastomer.

[0067] In this embodiment, the content of cellulose fibers in the cellulose fiber-containing resin pellets is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, even more preferably 25% by mass or more, and more preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, from the viewpoint of obtaining a molded product having excellent flexural modulus and impact resistance.

[0068] <Uses> The cellulose fiber-containing resin pellets of the present embodiment are suitably used as resin pellets for various moldings.

[0069] [Method for Producing Molded Article] The method for producing a molded article according to this embodiment includes the steps of producing the cellulose fiber-containing resin pellets described above and molding the cellulose fiber-containing resin pellets. Various molding methods can be used in the molding step, including injection molding (e.g., injection compression molding (press injection, hot flow stamping molding, gas injection compression molding), gas injection molding, and ultra-high speed injection molding), various extrusion moldings (cold runner or hot runner), compression (press) molding, insert molding, in-mold coating molding, insulating mold molding, rapid heating and cooling mold molding, and various profile extrusion moldings (e.g., two-color molding and sandwich molding). For example, various extrusion molding methods are suitable for forming sheets, films, fibers, and the like. Inflation, calendaring, casting, and the like can also be used to form sheets or films. Furthermore, specific stretching operations can be performed. Hollow molded articles can also be formed by rotational molding, blow molding, or the like. Multiple molding steps can be combined, or multiple steps can be performed simultaneously to form a single process. For example, the cellulose fiber-containing resin pellets may be formed into a sheet and then subjected to heat press molding to obtain a molded article, or the cellulose fiber-containing resin pellets may be formed into a sheet and then subjected to supercalendering to obtain a molded article. After forming into a sheet, the cellulose fiber-containing resin pellets may be molded by vacuum forming, pressure forming, etc. Among these, injection molding is a preferred example.

[0070] When the molding step is an injection molding step, the injection molding step involves, for example, using a known injection molding machine to melt and knead the above-mentioned cellulose fiber-containing resin pellets and injecting the molten mixture into a mold to form the product. When melt-kneading, any known kneading machine can be used, such as a single-screw kneader or a twin-screw kneader. Examples of known injection molding machines include screw-type injection molding machines, screw pre-plasticizing injection molding machines, plunger pre-plasticizing injection molding machines, and plunger injection molding machines. Examples of drive systems include hydraulic, electric, and hydraulic-electric hybrid systems.

[0071] The temperature conditions for injection molding are determined appropriately depending on the type of resin contained in the pellets, and it is preferable to set the cylinder temperature of the injection molding machine to a temperature 0 to 100°C higher than the flow initiation temperature of the resin used. The temperature of the mold may be selected appropriately in view of the cooling rate and productivity of the resin used, and in the case of polyolefin, for example, it is preferable to set it in the range of room temperature (e.g., 23°C) to 120°C. Other injection conditions such as the screw rotation speed, back pressure, injection speed, dwell pressure, and dwell time may be adjusted appropriately.

[0072] The cellulose fiber-containing resin pellets of this embodiment may contain other resins, such as elastomers, by adding and melt-kneading other resins, such as elastomers, during molding. Furthermore, in the process of producing a molded article, other resins, various additives, masterbatches containing various additives, etc. may be added in addition to the cellulose fiber-containing resin pellets during injection molding. Examples of additives include those typically used in resin compositions. Examples of such additives include stabilizers, UV absorbers, plasticizers, flame retardants, flame retardant assistants, antistatic agents, surfactants, colorants, lubricants, and mold release agents. Examples of stabilizers include hindered phenols, hydroquinones, phosphites, and their substituted derivatives. Examples of UV absorbers include resorcinol, salicylate, benzotriazole, and benzophenone. Examples of colorants include dyes such as nitrosine, and pigments such as cadmium sulfide, phthalocyanine, and carbon black. Examples of lubricants include fatty acids such as stearic acid and montanic acid, their amides, their esters, their half esters with polyhydric alcohols, stearyl alcohol, stearamide, polyethylene wax, and paraffin wax.

[0073] <Characteristics of Molded Article> In this embodiment, the density of the obtained molded article is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.95 g / cm 3 More preferably, 1.0 g / cm 3The density of the molded body is preferably 2.0 g / cm 3 or less, more preferably 1.5 g / cm 3 More preferably, 1.2 g / cm or less 3 The following is the result.

[0074] The thickness of the molded article is not particularly limited, but is 0.5 mm or more, more preferably 1 mm or more, even more preferably 2 mm or more, and is preferably 200 mm or less, more preferably 100 mm or less, even more preferably 50 mm or less, still more preferably 20 mm or less, and particularly preferably 10 mm or less. Note that, by making the thickness of the molded article 2 mm or more, it can be suitably used in applications requiring impact resistance, so it is particularly suitable that the thickness of the molded article is 2 mm or more.

[0075] The molded article of this embodiment preferably has a high flexural modulus, and a high flexural modulus of the molded article results in a molded article with excellent rigidity against bending. The flexural modulus of the molded article is preferably 1.5 GPa or more, more preferably 2.0 GPa or more, even more preferably 2.5 GPa or more, even more preferably 3.0 GPa or more, and even more preferably 3.0 GPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 10 GPa or less. The flexural modulus of the molded article is measured in accordance with JIS K 7171:2016.

[0076] The molded article of this embodiment preferably has high bending strength, and having high bending strength of the molded article results in a molded article with excellent rigidity. The bending strength of the molded article is preferably 20 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 MPa or less. The bending strength of the molded article is measured in accordance with JIS K 7171:2016.

[0077] The molded article of this embodiment preferably has high Charpy impact strength, and the Charpy impact strength of a molded article having a thickness of 4 mm is preferably 1.5 kJ / m 2 More preferably, 2.0 kJ / m 2More preferably, 3.0 kJ / m 2 More preferably, 4.0 kJ / m 2 The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 kJ / m 2 The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and more specifically, by the method described in the examples.

[0078] (Applications) The molded article obtained by the method for producing a molded article of the present embodiment is preferably used for electrical and electronic equipment, office automation equipment, home appliances, civil engineering and construction, automobile and aircraft parts, structural parts and housings, containers (e.g., food containers, drug packaging containers, cosmetic packaging containers, medical device packaging containers), furniture, daily necessities, medical tools, etc. Among these, it is suitable for applications requiring impact resistance, such as civil engineering and construction, automobile or aircraft parts, structural parts, and housings.

[0079] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.

[0080] (Example 1) <Preparation of fiber aggregate> NBKP was defibrated using a swirling jet airflow defibrator to obtain defibrated dry pulp. The processing air speed in the defibrator was 45 m / min, and turbulence was achieved using a baffle installed in the device. The obtained defibrated dry pulp had an average fiber length of 2.38 mm, an average fiber width of 34.3 μm, and a fine fiber ratio of 11.4%. Next, the obtained defibrated dry pulp, polypropylene fiber (melting point 160°C, fineness 6.6 dtex, fiber length 5 mm, fiber diameter 30 μm, also referred to as "PP fiber"), and polyethylene / polypropylene composite core-sheath fiber (core melting point 160°C, sheath melting point 110°C, fineness 1.7 dtex, fiber length 5 mm, fiber diameter 15 μm, core diameter 10.6 μm, core mass / sheath mass = 1 / 1, also referred to as "PE / PP composite fiber") were uniformly mixed using an air flow in a ratio (mass ratio) of 30 / 55 / 15 to obtain a fiber mixture.

[0081] Next, an air-laid web was formed from the fiber mixture using the web forming apparatus 1 shown in FIG. 1. Specifically, a first carrier sheet 41 was fed by a first carrier sheet supplying means 40 onto a permeable endless belt 20 that was attached to a conveyor 10 and running. In Example 1, tissue (basis weight 14 g / m) was used as the first carrier sheet 41. 2 The width was 1200 mm. The "basis weight" was measured in accordance with "Paper and paperboard - Method for measuring basis weight" described in JIS P8124:2011.

[0082] While the permeable endless belt 20 was being sucked by the suction box 60, the fiber mixture was dropped and deposited on the first carrier sheet 41 together with the air flow from the fiber mixture supply means 30, to obtain a cotton-like fiber aggregate. At this time, the set basis weight of the air-laid web portion was 400 g / m. 2 The fiber mixture was supplied so that the fiber mixture was in a state of being 100% of the original weight. Next, a second carrier sheet 51 was laminated on the cotton-like fiber aggregate on the first carrier sheet 41 by a second carrier sheet supplying means 50, thereby obtaining a fiber aggregate containing an air-laid web. In Example 1, tissue (basis weight 14 g / m) was used as the second carrier sheet 51. 2That is, in Example 1, the same sheet was used for the first carrier sheet 41 and the second carrier sheet 51.

[0083] <Preparation of cellulose fiber-containing resin sheet> The obtained fiber assembly containing the air-laid web was passed through a box-type dryer with a hot air circulation conveyor oven system and subjected to hot air treatment at a temperature of 140°C. Thereafter, the density was adjusted by roll press treatment so that the bulk specific gravity was 0.3 g / mL, and the sheet was then pressed into a resin sheet with a basis weight of 416 g / m without peeling off the first carrier sheet and the second carrier sheet. 2 The cellulose fiber-containing resin sheet had a T / Y ratio of 0.88, a bulk specific gravity of 0.32 g / mL, and a thickness of 1.3 mm. The cellulose fiber-containing resin sheet was slit using a slitter to a width of 150 mm.

[0084] <Preparation of Cellulose Fiber-Containing Resin Pellets> The cellulose fiber-containing resin sheet was mixed with a cellulose fiber pellet-forming machine (manufactured by Shibaura Machine Co., Ltd., TEM-37SX, screw diameter 37 mm) at the base of the extruder. The extruder had a cross-sectional area of ​​57 cm 2 The mixture was poured into the opening of the die. The kneading temperature was 165°C, the rotation speed was 70 rpm (circumferential speed 8.1 m / min), and the mixture was melted, kneaded, and dispersed. The screw used for kneading was an R-type kneading part, and all other parts were weakly kneaded and composed of feed screws. The strand extruded from the 4 mmφ die was cooled by air cooling and then cut with a pelletizer to obtain cellulose fiber-containing resin pellets with a length of 3 mm. The extrusion rate of the kneaded product measured by the method described below was 9.7 kg / h.

[0085] (Example 2) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the rotation speed was changed to 300 rpm (circumferential speed 34.9 m / min) in <Preparation of cellulose fiber-containing resin pellets> of Example 1. The discharge rate of the kneaded product was 47.3 kg / h.

[0086] (Example 3) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the rotation speed was changed to 500 rpm (circumferential speed 58.1 m / min) in <Preparation of cellulose fiber-containing resin pellets> of Example 1. The discharge rate of the kneaded product was 78.6 kg / h.

[0087] Example 4 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the width was changed to 200 mm in <Preparation of cellulose fiber-containing resin sheet> of Example 1. The discharge rate of the kneaded product was 11.7 kg / h.

[0088] (Example 5) In the <Production of cellulose fiber-containing resin sheet> of Example 1, the width was changed to 100 mm, and in the <Production of cellulose fiber-containing resin pellets>, the sheet feeding section was changed to a 22 cm cross-sectional area extruder provided in the middle of the extruder. 2 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the vent port was changed to 1. The discharge rate of the kneaded product was 7.5 kg / h.

[0089] (Example 6) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 4, except that in the <Preparation of fiber assembly> of Example 1, the fiber mixture was changed to a ratio (mass ratio) of 50 / 35 / 15. The basis weight of the cellulose fiber-containing resin sheet was 411 g / m 2 The T / Y ratio was 0.88, the bulk density was 0.29 g / mL, and the thickness was 1.44 mm. The discharge rate of the kneaded product was 13.8 kg / h.

[0090] Comparative Example 1 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that in <Preparation of cellulose fiber-containing resin sheet> of Example 1, the cellulose fiber-containing resin sheet was shredded with a shredder (AFS100M, manufactured by Iris Ohyama Co., Ltd.) to obtain press-shredded chips of approximately 4 mm x 13 mm, and the press-shredded chips were fed into a twin-screw extruder. The discharge rate of the kneaded product was 3.8 kg / h.

[0091] Comparative Example 2 Cellulose fiber-containing resin pellets were obtained in the same manner as in Comparative Example 1, except that the rotation speed was changed to 300 rpm (circumferential speed: 34.9 m / min). The discharge rate of the kneaded product was 12.5 kg / h.

[0092] Comparative Example 3 Cellulose fiber-containing resin pellets were obtained in the same manner as in Comparative Example 1, except that the rotation speed was changed to 500 rpm (circumferential speed: 58.1 m / min). The discharge rate of the kneaded product was 24.8 kg / h.

[0093] (Comparative Example 4) In the <Preparation of cellulose fiber-containing resin sheet> of Example 1, an attempt was made to obtain cellulose fiber-containing resin pellets in the same manner as in Example 1, except that the width was set to 300 mm. However, the cellulose fiber-containing resin sheet was not caught in the screw of the kneader, and cellulose fiber-containing resin pellets could not be obtained.

[0094] [Measurement and Evaluation Methods] (Method for Measuring Fiber Length and Fiber Diameter of Polyolefin Fiber) Twenty randomly selected polyolefin fibers were observed under an optical microscope, and the fiber length and fiber diameter were measured.

[0095] (Method for measuring average fiber length, average fiber diameter, and fine fiber ratio of pulp fibers (cellulose fibers)) In accordance with ISO 16065-2, the average fiber length and average fiber diameter of pulp fibers were measured using a fiber image analyzer (Valmet FS5, manufactured by Valmet Co., Ltd.) The proportion of fine fibers of 0.1 mm or less in the measured length-weighted average fiber length distribution was defined as the fine fiber ratio.

[0096] (Method for measuring the fineness of polyolefin fibers) When a catalog value or the like is available for the fineness of polyolefin fibers, the catalog value may be used. In this example, the catalog value was used. When no catalog value is available, the fineness is measured by Method B of JIS L 1013:2010 (Testing methods for chemical fiber filament yarns).

[0097] (Method for measuring the melting point of polyolefin fiber) When a catalog value for the polyolefin fiber is available, the catalog value may be used for the melting point of the polyolefin fiber. In this example, the catalog value was used. If a catalog value is not available, the melting point can be measured by the following method. 5 mg of polyolefin fiber is cut out, and the melting point of the polyolefin fiber is measured using a differential scanning calorimeter (DSC). The melting point is measured using a Diamond DSC manufactured by Perkin-Elmer, by increasing the temperature from 30°C to 280°C at a rate of 20°C / min under a nitrogen atmosphere.

[0098] (Method for measuring bulk density of cellulose fiber-containing resin sheet) The bulk density of the cellulose fiber-containing resin sheet was calculated by measuring the thickness and mass of a 50 mm square sheet after conditioning it for 24 hours under conditions of 23°C and 50% RH. The thickness of the sheet was measured with a digital thickness gauge (DG-127, manufactured by Ozaki Seisakusho Co., Ltd.).

[0099] (Method for measuring T / Y) The flow direction (running direction of the conveyor 10) of the obtained cellulose fiber-containing resin sheet in the fiber aggregate manufacturing process was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction. The tensile strength (unit: N / m) was measured in accordance with JIS P 8113:2006. The tensile strength in each direction was calculated by dividing the tensile strength by the thickness of the test piece. A Tensilon manufactured by A&D Co., Ltd. was used as a tensile tester, and a 15 mm x 180 mm strip was measured at a speed of 20 mm / min.

[0100] (Measurement of Discharge Rate of Kneaded Product) The discharge rate of the kneaded product was determined by measuring the mass of the kneaded product discharged from the die of the twin-screw extruder for 3 minutes to determine the discharge amount per hour. The average value of two measurements was taken as the discharge rate.

[0101] <Evaluation> Molded articles were obtained from the obtained cellulose fiber-containing resin pellets by the following method, and the density, flexural modulus, flexural strength, and impact resistance were measured. The results are shown in Table 2. (Molding of pellets) The pellets were used to injection-molde Type A1 multipurpose test pieces specified in JIS K 7139:2009 under conditions of a molding temperature of 170°C, a mold temperature of 40°C, and an injection speed of 10 mm / sec, to obtain molded articles with a thickness of 4 mm.

[0102] (Method for measuring density of molded article) The obtained molded article (molded body) was cut into a strip-shaped test piece of 80 mm length x 10 mm width. The thickness of the strip-shaped test piece was measured with a constant pressure thickness measuring device (manufactured by Teclock Corporation, model number PG-02J), and the volume of the strip-shaped test piece was calculated. Furthermore, the density was calculated by measuring the mass of the strip-shaped test piece.

[0103] (Method for measuring flexural modulus and flexural strength of molded article) The obtained molded article (molded body) was cut into a strip-shaped test piece of 80 mm length x 10 mm width, and a three-point bending test was performed in accordance with JIS K 7171: 2016. The obtained flexural modulus and flexural strength were evaluated such that the larger the numerical value, the better the rigidity and strength against bending, respectively.

[0104] (Method for measuring impact resistance of molded article) The obtained molded article (molded body) was cut into a strip-shaped test piece of 80 mm length x 10 mm width, and a notched Charpy impact test (impact direction: edgewise) was performed in accordance with JIS K 7111-1: 2012. The larger the obtained Charpy impact strength value, the better the impact resistance and the stronger it was evaluated to be against impact.

[0105]

[0106]

[0107] As shown in Table 1, increasing the rotation speed increases the extrusion amount. Productivity can be evaluated by the extrusion amount at the same rotation speed, but by considering the extrusion amount per rotation speed (the ratio of the extrusion speed (kg / h) to the peripheral speed of the screw (m / min) (extrusion speed / peripheral speed)), it is possible to compare productivity even between different rotation speeds. As shown in Examples 1 to 6, the cellulose fiber-containing pellets of the present invention have a high extrusion speed / peripheral speed and are highly productive. Furthermore, as shown in Table 2, the molded articles produced using the cellulose fiber-containing pellets of the present invention were excellent in bending rigidity and strength, as well as impact resistance.

[0108] According to the method for producing cellulose fiber-containing resin pellets of this embodiment, productivity is high, and furthermore, molded articles having excellent flexural modulus (rigidity against bending), flexural strength (strength against bending) and impact resistance can be obtained from the pellets.

[0109] REFERENCE SIGNS LIST 1 Web forming device 10 Conveyor 20 Permeable endless belt 30 Fiber mixture supply means 40 First carrier sheet supply means 41 First carrier sheet 50 Second carrier sheet supply means 51 Second carrier sheet 60 Suction box

Claims

1. A method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader, wherein the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet / inlet area of ​​the screw-type kneader) is 0.065 or less.

2. Cross-sectional area (cm) of cellulose fiber-containing resin sheet relative to screw diameter (mm) of screw-type kneader 2 ) (cross-sectional area (cm 2 2. The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the ratio of the screw diameter (mm) to the screw diameter (mm) is 0.100 or less.

3. A method for producing cellulose fiber-containing resin pellets according to claim 1 or 2, wherein the ratio of the discharge speed (kg / h) to the peripheral speed (m / min) of the screw of the screw-type kneader (discharge speed / peripheral speed) is 0.50 or more.

4. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 3, wherein the cellulose fiber content in the cellulose fiber-containing resin pellets is 10% by mass or more and 90% by mass or less.

5. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 4, wherein the cellulose fiber-containing resin sheet is produced by a production method including the following steps 1 and 2. Step 1: A fiber assembly production step of producing a fiber assembly containing cellulose fibers and resin A by dry papermaking. Step 2: A cellulose fiber-containing resin sheet production step of compressing the fiber assembly to produce a cellulose fiber-containing resin sheet.

6. The method for producing cellulose fiber-containing resin pellets according to claim 5, wherein the resin A contains resin fibers.

7. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 6, wherein when the tensile strength of the cellulose fiber-containing resin sheet in a first direction is T and the tensile strength in a second direction perpendicular to the first direction is Y, T / Y is 0.5 or more and 1.5 or less.

8. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 7, wherein the bulk density of the cellulose fiber-containing resin sheet is 0.10 g / mL or more and 0.60 g / mL or less.

9. A method for producing a molded product, comprising the steps of: producing cellulose fiber-containing resin pellets by the method according to any one of claims 1 to 8; and molding the cellulose fiber-containing resin pellets.

10. The method for producing a molded article according to claim 9, wherein the molding step is a step of injection molding cellulose fiber-containing resin pellets.

11. The density of the obtained molded body is 0.8 g / cm 3 1.5g / cm or more 3 The method for producing a molded body according to claim 9 or 10, wherein:

12. The method for producing a molded article according to any one of claims 9 to 11, wherein the thickness of the obtained molded article is 2 mm or more.

13. A method for producing a molded article according to any one of claims 9 to 12, wherein the resulting molded article has a flexural modulus of 1.5 GPa or more as measured in accordance with JIS K 7171:2016.

14. The Charpy impact strength of the obtained molded product measured in accordance with JIS K 7111-1:2012 is 2.0 kJ / m 2 The method for producing a molded article according to any one of claims 9 to 13, wherein the molded article is a molded product.

Citation Information

Patent Citations

  • Method of treating waste plastic film or sheet

    JP1987231709A

  • Thermoplastic resin composition, process for producing the same, and process for producing molding

    WO2008133214A1

  • Method for production of molded thermoplastic composition article

    WO2009072499A1