Cellulose fiber-containing resin molded body
The cellulose fiber-containing resin molded article, produced via dry papermaking and injection molding, achieves excellent bending rigidity and recyclability by controlling stiffness loss, overcoming the biodegradability and recyclability issues of traditional fiber-reinforced plastics.
Patent Information
- Application Number
- PCT/JP2024/014681
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-21
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-31
AI Technical Summary
Fiber-reinforced plastic molded products using traditional reinforcing fibers like carbon and glass fibers have low biodegradability, leading to disposal challenges and reduced recyclability, resulting in decreased bending stiffness and impact resistance when recycled.
A cellulose fiber-containing resin molded article is developed with a controlled rate of decrease in stiffness during recycling, achieved through a process involving dry papermaking to produce fiber aggregates, which are then compressed into sheets and melt-kneaded into pellets for injection molding, maintaining high bending rigidity and impact resistance.
The cellulose fiber-containing resin molded article exhibits excellent bending rigidity and recyclability, with a reduced rate of stiffness loss and improved impact resistance, addressing the limitations of traditional fiber-reinforced plastics.
Smart Images

Figure JP2024014681_31102024_PF_FP_ABST
Abstract
Description
Cellulose fiber-containing resin molding
[0001] The present invention relates to a cellulose fiber-containing resin molded article.
[0002] Fiber-reinforced plastic molded products made from nonwoven fabrics containing reinforcing fibers such as carbon fiber and glass fiber (also called sheets for fiber-reinforced plastic molded products) are already used in a variety of fields, including sports and leisure goods, aircraft materials, electronic device components, etc. Thermosetting resins and thermoplastic resins are used as the matrix resins in fiber-reinforced plastic molded products, but in recent years, development of fiber-reinforced plastic molded products using thermoplastic resins has been progressing.
[0003] Carbon fiber, glass fiber, aramid fiber, etc. are used as reinforcing fibers. Such reinforcing fibers serve to increase the strength of fiber-reinforced plastic molded bodies. When such molded products are to be disposed of, they are usually disposed of in landfills or incinerated. However, molded products using such reinforcing fibers have low biodegradability after being landfilled, and there are problems with the load on incinerators and other equipment when they are incinerated.
[0004] For this reason, in recent years, the use of pulp fibers as reinforcing fibers has been proposed (for example, Patent Documents 1 to 3). In Patent Documents 1 and 2, a molded article is obtained by making a slurry containing pulp fibers and a thermoplastic resin into a paper, and then molding the molded intermediate product under heat and pressure. Patent Document 3 proposes forming pellets from a slurry containing pulp fibers and a thermoplastic resin, and then injection molding the pellets to produce a molded article.
[0005] JP-A-6-322699 JP-A-6-346399 JP-A-6-345944
[0006] In recent years, the recycling of fiber-reinforced plastic molded articles has also been studied. It has been found that when a fiber-reinforced plastic molded article is pulverized and then used as a raw material for reuse, the recycled molded article has a problem of reduced bending rigidity compared to the molded article before recycling. The present invention aims to provide a cellulose fiber-containing resin molded article that has excellent bending rigidity and excellent recyclability.
[0007] The present inventors have found that the above-mentioned problems can be solved by limiting the rate of decrease in bending rigidity to a certain value or less when a cellulose fiber-containing resin molded body is recycled. The present invention relates to the following items <1> to <12>. <1> A cellulose fiber-containing resin molded body having a flexural modulus of 2.5 GPa or more as measured in accordance with JIS K 7171:2016, and a recycled cellulose fiber-containing resin molded body obtained by melt-kneading and remolding the cellulose fiber-containing resin molded body, in which the rate of decrease in flexural modulus is 10% or less compared to the cellulose fiber-containing resin molded body. <2> The cellulose fiber-containing resin molded body according to <1>, in which the rate of decrease in bending strength is 10% or less compared to the cellulose fiber-containing resin molded body. <3> The cellulose fiber-containing resin molded body according to <1> or <2>, in which the rate of decrease in Charpy impact strength is 30% or less compared to the cellulose fiber-containing resin molded body. <4> The cellulose fiber-containing resin molded body according to any one of <1> to <3>, wherein the cellulose fiber content is 10% by mass or more and 90% by mass or less. <5> A density of 0.8 g / cm 3 1.5g / cm or more 3 <6> The cellulose fiber-containing resin molded article according to any one of <1> to <4>, having a thickness of 2 mm or more. <7> The cellulose fiber-containing resin molded article according to any one of <1> to <5>, having a Charpy impact strength of 2.0 kJ / m at a thickness of 4 mm, measured in accordance with JIS K 7111-1:2012. 2The cellulose fiber-containing resin molded body according to any one of <1> to <6>, wherein the initial cellulose fiber-containing resin molded body before the first recycling is a molded body obtained by a method comprising the following steps 1, 2, 3, and 4 in this order: Step 1: a fiber assembly production step of producing a fiber assembly containing cellulose fibers and resin A by dry papermaking; Step 2: a cellulose fiber-containing resin sheet production step of compressing the fiber assembly to produce a cellulose fiber-containing resin sheet; Step 3: a cellulose fiber-containing resin pellet production step of melt-kneading the cellulose fiber-containing resin sheet to produce pellets; and Step 4: a step of molding the cellulose fiber-containing resin pellets. <9> The cellulose fiber-containing resin molded body according to <8>, wherein the resin A contains resin fibers. <10> The cellulose fiber-containing resin molded body according to <8> or <9>, wherein T / Y is 0.5 or more and 1.5 or less, where T is the tensile strength of the cellulose fiber-containing resin sheet in a first direction and Y is the tensile strength in a second direction perpendicular to the first direction. <11> The cellulose fiber-containing resin molded body according to any one of <8> to <10>, wherein in step 2, the cellulose fiber-containing resin sheet to be subjected to step 3 has a bulk specific gravity of 0.10 g / mL or more and 0.60 g / mL or less. <12> The cellulose fiber-containing resin molded body according to any one of <8> to <11>, wherein step 4 is a step of injection molding cellulose fiber-containing resin pellets.
[0008] According to the present invention, a cellulose fiber-containing resin molded article having excellent bending rigidity and excellent recyclability is provided.
[0009] FIG. 1 shows the web forming apparatus used in the examples.
[0010] [Cellulose fiber-containing resin molded body] The cellulose fiber-containing resin molded body of this embodiment (hereinafter simply referred to as the "molded body") has a flexural modulus of 2.5 GPa or more measured in accordance with JIS K 7171:2016, and a recycled cellulose fiber-containing resin molded body (hereinafter simply referred to as the "recycled molded body") obtained by melt-kneading and remolding the cellulose fiber-containing resin molded body has a flexural modulus reduction of 10% or less compared to the cellulose fiber-containing resin molded body. According to the present invention, a cellulose fiber-containing resin molded body having excellent bending rigidity and excellent recyclability is provided. Until now, the reduction in bending rigidity upon recycling has not been studied. In the present invention, the reduction in bending rigidity due to recycling was studied, and it was found that by setting this within a specific range, a cellulose fiber-containing resin molded body having extremely excellent recyclability can be provided, in which not only bending rigidity and strength but also reduction in impact resistance and the like are suppressed. In the following description, the initially molded molded body will be referred to as the "molded body (initial)", a recycled cellulose fiber-containing resin molded body obtained by melt-kneading and remolding the molded body (initial) will be referred to as the "molded body (first recycled)", a recycled cellulose fiber-containing resin molded body obtained by melt-kneading and remolding the molded body (first recycled) will be referred to as the "molded body (second recycled)", and similarly hereinafter, all of these will be referred to as the "molded body (nth recycled)". In this embodiment, the flexural modulus of the molded body (initial) and the molded body (nth recycled) measured in accordance with JIS K 7171:2016 is 2.5 GPa or more. Furthermore, the reduction in the flexural modulus of the molded body (first recycled) compared to the molded body (initial) is 10% or less. Furthermore, the reduction in the flexural modulus of the molded body (n+1th recycled) compared to the molded body (nth recycled) is 10% or less. The present invention will be described in further detail below.
[0011] <Characteristics of Molded Body> (Flexural Modulus) The molded body of this embodiment has a flexural modulus of 2.5 GPa or more measured in accordance with JIS K 7171:2016. The flexural modulus of the molded body is preferably 3.0 GPa or more, more preferably 3.3 GPa or more, and even more preferably 3.5 GPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of manufacture, it is preferably 10 GPa or less. Note that this does not mean that only the flexural modulus of the molded body (initial) is 2.5 GPa or more, but that the flexural modulus of the molded body before recycling is 2.5 GPa or more. Therefore, for example, when recycling is performed a total of two times, the flexural modulus of the molded body (initial) and the molded body (recycled once) is 2.5 GPa or more.
[0012] (Bending strength) The molded article of this embodiment preferably has high bending strength, and having high bending strength of the molded article results in a molded article with excellent rigidity, which is preferable. The bending strength of the molded article is preferably 20 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 150 MPa or less. The bending strength of the molded article is measured in accordance with JIS K 7171:2016.
[0013] (Charpy impact strength) The molded article of the present embodiment preferably has high Charpy impact strength, and the Charpy impact strength of a molded article having a thickness of 4 mm is preferably 1.5 kJ / m 2 More preferably, 2.0 kJ / m 2 More preferably, 3.0 kJ / m 2 More preferably, 4.0 kJ / m 2 The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 kJ / m 2 Less than or equal to 30 kJ / m, more preferably 30 kJ / m 2 More preferably, 20 kJ / m or less 2 The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and more specifically, by the method described in the examples.
[0014] (Density) In this embodiment, the density of the molded body is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.85 g / cm 3 More preferably, 0.90 g / cm 3 The density of the molded body is preferably 2.0 g / cm 3 or less, more preferably 1.5 g / cm 3 More preferably, 1.2 g / cm or less 3 The following is the result.
[0015] (Thickness) The thickness of the molded article is not particularly limited, but is 0.5 mm or more and 200 mm or less, more preferably 1 mm or more, even more preferably 2 mm or more, and more preferably 100 mm or less, even more preferably 50 mm or less, still more preferably 20 mm or less, and particularly preferably 10 mm or less. Note that, by making the thickness of the molded article 2 mm or more, it can be suitably used in applications requiring impact resistance, so it is particularly preferable that the thickness of the molded article be 2 mm or more.
[0016] (Composition of Molded Body) The molded body contains at least cellulose fibers and a resin component. From the viewpoint of obtaining a molded body that is excellent in recyclability, has a high degree of biomass conversion, excellent bending rigidity and strength, and excellent impact resistance, the cellulose fiber content in the molded body is preferably 10% by mass or more and 90% by mass or less, more preferably 15% by mass or more, even more preferably 20% by mass or more, still more preferably 25% by mass or more, and more preferably 80% by mass or less, even more preferably 70% by mass or less, and still more preferably 60% by mass or less. Other components contained in the molded body will be described later.
[0017] <Recycling Properties> (Decrease in Flexural Modulus) In the molded article of this embodiment, the molded article is melt-kneaded and re-molded into a recycled molded article, and the decrease in flexural modulus from the flexural modulus of the molded article before recycling is 10% or less. The decrease in flexural modulus after the first recycling is expressed by the following formula: Decrease in flexural modulus after the first recycling = (flexural modulus of molded article (initial) - flexural modulus of molded article (first recycling)) ÷ flexural modulus of molded article (initial) × 100 Similarly, the decrease in flexural modulus after the second recycling is expressed by the following formula: Decrease in flexural modulus after the second recycling = (flexural modulus of molded article (first recycling) - flexural modulus of molded article (second recycling)) ÷ flexural modulus of molded article (first recycling) × 100 The decrease in flexural modulus is preferably 7% or less, more preferably 5% or less, and even more preferably 3% or less, with no particular lower limit. The flexural modulus is measured in accordance with JIS K 7171:2016.
[0018] (Decrease in bending strength) The molded body of this embodiment is preferably such that the decrease in bending strength of a recycled molded body obtained by melt-kneading the molded body and re-molding the molded body is 10% or less compared to the bending strength of the molded body before recycling. The decrease in bending strength after the first recycling is expressed by the following formula: Decrease in bending strength after the first recycling = (Bending strength of molded body (initial) - Bending strength of molded body (first recycling)) ÷ Bending strength of molded body (initial) × 100 Similarly, the decrease in bending strength after the second recycling is expressed by the following formula: Decrease in bending strength after the second recycling = (Bending strength of molded body (first recycling) - Bending strength of molded body (second recycling)) ÷ Bending strength of molded body (first recycling) × 100 The decrease in bending strength is preferably 8% or less, more preferably 7% or less, and even more preferably 5% or less, with no particular lower limit. The bending strength of the molded body is measured in accordance with JIS K 7171:2016.
[0019] (Reduction rate of Charpy impact strength) In the molded body of this embodiment, it is preferable that the reduction rate of the Charpy impact strength of a recycled molded body obtained by melt-kneading the molded body and re-molding the molded body is 30% or less compared to the Charpy impact strength of the molded body before recycling. Note that the Charpy impact strength is the Charpy impact strength of a molded body having a thickness of 4 mm. The reduction rate of the Charpy impact strength after the first recycling is expressed by the following formula: Reduction rate of Charpy impact strength after the first recycling = (Charpy impact strength of molded body (initial) - Charpy impact strength of molded body (first recycling)) ÷ Charpy impact strength of molded body (initial) × 100 Similarly, the reduction rate of Charpy impact strength after the second recycling is expressed by the following formula. Reduction rate of Charpy impact strength after second recycling = (Charpy impact strength of molded body (recycled for the first time) - Charpy impact strength of molded body (recycled for the second time)) ÷ Charpy impact strength of molded body (recycled for the first time) × 100 The reduction rate of Charpy impact strength is preferably 25% or less, more preferably 20% or less, even more preferably 17% or less, and even more preferably 15% or less, with no particular lower limit. The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and in detail, is measured by the method described in the examples.
[0020] [Method for Manufacturing Molded Body (Initial)] In this embodiment, the initial cellulose fiber-containing resin molded body before the first recycling, i.e., the molded body (initial), may be a molded body obtained by any method, but is preferably a molded body obtained by a method including the following steps 1 to 4 in this order. It is difficult to directly identify the molded body (initial) based on its structure or properties. Compared to conventional methods of simply melt-kneading cellulose fibers and resin to produce pellets, a fiber aggregate is produced by dry papermaking, and then compressed into a cellulose fiber-containing resin sheet to produce pellets. Since the cellulose fibers are uniformly dispersed in the cellulose fiber-containing resin sheet, aggregation and poor dispersion of the cellulose fibers during melt-kneading are suppressed. The cellulose fibers are highly dispersible in the cellulose fiber-containing resin pellets, and the high dispersibility of the cellulose fibers is maintained in the molded body. As a result, a molded body with excellent bending rigidity and strength, as well as excellent impact resistance, is obtained. Step 1: A fiber assembly manufacturing process in which a fiber assembly containing cellulose fibers and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing process in which the fiber assembly is compressed to manufacture a cellulose fiber-containing resin sheet. Step 3: A cellulose fiber-containing resin pellet manufacturing process in which the cellulose fiber-containing resin sheet is melt-kneaded to manufacture pellets. Step 4: A process in which the cellulose fiber-containing resin pellets are molded. Each step is explained below.
[0021] <Step 1> Step 1 is a fiber assembly production step in which a fiber assembly containing cellulose fibers and resin A is produced by dry papermaking. (Cellulose Fibers) The cellulose fibers are not particularly limited in terms of their production method or type. Pulp fibers are preferred as cellulose fibers, and may be, for example, chemical pulps such as hardwood and / or softwood kraft pulp, mechanical pulps such as SGP, RGP, BCTMP, and CTMP, waste paper pulp such as deinked pulp, or non-wood pulps such as kenaf, jute, bagasse, bamboo, straw, and hemp. Chlorine-free pulps such as ECF pulp and TCF pulp can also be used. Pulp fibers are preferred as cellulose fibers, but are not limited thereto. For example, paper flour, wood flour, etc. may also be used.
[0022] Among the above pulp fibers, kraft pulp fibers, particularly long-fiber softwood bleached kraft pulp fibers (NBKP), are preferably used as cellulose fibers because the resulting molded articles have superior flexural modulus and impact resistance.
[0023] From the viewpoint of improving the flexural modulus and impact resistance of the resulting molded article and from the viewpoint of ease of production of the fiber assembly, the average fiber length of the cellulose fibers is preferably 0.1 mm or more, more preferably 0.5 mm or more, even more preferably 1 mm or more, and is preferably 50 mm or less, more preferably 10 mm or less, even more preferably 5 mm or less, and still more preferably 2.5 mm or less. The average fiber length of the cellulose fibers is measured by the method described in the Examples.
[0024] From the viewpoint of improving the bending rigidity and impact resistance of the resulting molded article and from the viewpoint of ease of production of the fiber assembly, the average fiber width of the cellulose fibers is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, still more preferably 15 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and still more preferably 50 μm or less. The average fiber width of the cellulose fibers is measured by the method described in the Examples.
[0025] In this embodiment, when the fiber aggregate is formed by an air-laid method, the cellulose fibers may be in the form of, for example, defibrated dry pulp.
[0026] The cellulose fibers are preferably unbeaten cellulose fibers from the viewpoint of improving the impact resistance of the resulting molded body. For the molded body to exhibit impact resistance, the cellulose fibers must be properly pulled out of the resin when an impact is applied. For this purpose, unbeaten cellulose fibers with a low fine fiber ratio are preferred, and unbeaten pulp fibers are even more preferred. From the above viewpoints, the fine fiber ratio of the cellulose fibers is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less, with no particular lower limit. The fine fiber ratio of the cellulose fibers is measured by the method described in the Examples.
[0027] From the viewpoint of obtaining a molded product having excellent flexural modulus and impact resistance, and from the viewpoint of the productivity and ease of manufacturing of the cellulose fiber-containing resin sheet, the content of cellulose fibers in the cellulose fiber-containing resin sheet is preferably 10% by mass or more and 90% by mass or less, more preferably 15% by mass or more, even more preferably 20% by mass or more, still more preferably 25% by mass or more, and more preferably 85% by mass or less, even more preferably 80% by mass or less, and still more preferably 75% by mass or less.
[0028] (Resin A) Examples of resin A components include polyolefin, polyvinyl chloride, polystyrene, ABS (acrylonitrile-butadiene-styrene), acrylonitrile-styrene, polyester, acrylic resin, polyamide, polyacetal, polycarbonate, polybutylene succinate, and polylactic acid. Furthermore, resins or elastomers exemplified as lubricants, plasticizers, nucleating agents, flame retardants, antistatic agents, fillers, and papermaking chemicals listed in the section "Other Components" below may also be used. In other words, resin A refers to the resin component contained in the molded body. As described in the molded body manufacturing method described below, the molded body of this embodiment is preferably manufactured by dry-laid papermaking of a cellulose fiber aggregate containing cellulose fibers and resin A, followed by compressing the cellulose fiber-containing resin sheet. In other words, at least resin A is preferably blended with the cellulose fiber aggregate. In the manufacturing of the molded body, further resins or elastomers may be added.
[0029] In the present invention, the resin A contained in the fiber assembly can be in the form of any of fibers, powder, granules, and pellets. Among these, from the viewpoint of ease of papermaking in Step 1 described below and the dispersibility of cellulose fibers in pellets and molded bodies, the resin A contained in the fiber assembly is preferably in the form of fibers or powder, and more preferably fibers. That is, the resin A contained in the fiber assembly preferably contains resin fibers or resin powder, more preferably contains resin fibers, and even more preferably contains resin fibers. Preferred examples of the fibers of the resin A contained in the fiber assembly include polyolefin fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, polyamide fibers, polycarbonate fibers, and polylactic acid fibers. Preferred examples of the components of the powder, granules, and pellets of the resin A contained in the fiber assembly include polyolefins, polyvinyl chloride, polyesters, acrylics, polyamides, polycarbonates, polylactic acid, polystyrene, ABS, acrylonitrile-styrene, polyacetal, and polybutylene succinate. In particular, preferred examples of resin A powder include polyolefin powder, polystyrene powder, ABS powder, acrylonitrile-styrene powder, polyacetal powder, and polybutylene succinate powder. Examples of the polyolefin include those specific examples of polyolefin in the polyolefin fiber shown below. Among these, polyolefin fiber is preferred as the resin A to be contained in the fiber assembly. Resin A to be contained in the fiber assembly can be used alone or in combination of two or more. For example, a combination of two types of resin A, polylactic acid fiber and polybutylene succinate powder, can be used.
[0030] [Polyolefin Fiber] In this embodiment, when polyolefin fiber is used as the resin A contained in the fiber assembly, the polyolefin constituting the polyolefin fiber is not particularly limited, and examples thereof include polyolefin (unmodified polyolefin) and modified polyolefin. From the viewpoint of ease of molding and suppression of deterioration of cellulose fiber, the melting point of the polyolefin constituting the polyolefin fiber is preferably 80°C or higher and 200°C or lower, more preferably 195°C or lower, even more preferably 180°C or lower, more preferably 90°C or higher, even more preferably 100°C or higher.
[0031] Examples of polyolefins include polyethylene, polypropylene, and ethylene-propylene copolymers (also referred to as propylene-ethylene copolymers), with polyethylene and polypropylene being preferred. Regarding modified polyolefins, examples of methods for modifying polyolefins include acid modification and chlorination. Among these, acid modification is preferred from the viewpoint of improving affinity with cellulose fibers. The acid-modifying component used for the acid modification of acid-modified polyolefins is preferably an unsaturated carboxylic acid component. Examples of unsaturated carboxylic acid components include components derived from unsaturated carboxylic acids and their acid anhydrides. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, and crotonic acid. Among these, the unsaturated carboxylic acid component is preferably at least one selected from acrylic acid, methacrylic acid, maleic acid, and maleic anhydride, and particularly preferably at least one selected from maleic acid and maleic anhydride. Polyolefins modified with at least one of maleic acid and maleic anhydride are also referred to as maleic acid-modified polyolefins. The acid-modified polyolefin is preferably a maleic acid-modified polyolefin, more preferably a maleic acid-modified polyethylene or a maleic acid-modified polypropylene. The acid-modified polyolefin may be at least partially acid-modified.
[0032] The polyolefin is particularly preferably at least one selected from the group consisting of polyethylene, polypropylene, polyethylene at least partially modified with maleic acid, polypropylene at least partially modified with maleic acid, and ethylene-propylene copolymer. From the viewpoint of improving the flexural modulus of the resulting molded article, it is preferable that the polyolefin contains an acid-modified polyolefin, more preferably the polyolefin contains at least one of polyethylene at least partially modified with maleic acid and polypropylene at least partially modified with maleic acid, and even more preferably the polyolefin contains polyethylene at least partially modified with maleic acid. Furthermore, from the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that the polyolefin does not contain an acid-modified polyolefin, and it is more preferable that the polyolefin contains only polyethylene, polypropylene, and ethylene-propylene copolymer. The polyolefin fibers may be used alone or in combination of two or more types.
[0033] The polyolefin fiber may be a composite fiber made of two or more polyolefins, and examples thereof include split fibers, sea-island fibers, sheath-core fibers, and laminated fibers. Among these, sheath-core fibers are preferred from the viewpoint of obtaining a molded article having excellent bending rigidity and impact resistance. When using sheath-core fibers, fibers with a concentric cross-sectional structure or an eccentric cross-sectional structure are used, but fibers with a concentric cross-sectional structure are preferred. Fibers with a concentric cross-sectional structure are preferred because they can obtain a more uniform fiber assembly.
[0034] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fiber length of the polyolefin fiber is preferably 0.1 mm or more, more preferably 1.0 mm or more, even more preferably 2.0 mm or more, and even more preferably 3.0 mm or more, and is preferably 50 mm or less, more preferably 20 mm or less, and even more preferably 10 mm or less. The fiber length of the polyolefin fiber is measured by the method described in the Examples.
[0035] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fiber diameter of the polyolefin fiber is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 10 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. The fiber diameter of the polyolefin fiber is measured by the method described in the Examples.
[0036] From the viewpoint of obtaining a uniform fiber assembly and facilitating the production of the fiber assembly, the fineness of the polyolefin fiber is preferably 0.01 dtex or more, more preferably 0.1 dtex or more, even more preferably 1 dtex or more, and preferably 100 dtex or less, more preferably 50 dtex or less, even more preferably 10 dtex or less. The fineness of the polyolefin fiber is measured by the method described in the examples.
[0037] When the resin A contained in the fiber aggregate is a polyolefin fiber, the content of the polyolefin fiber in the fiber aggregate is preferably 90% by mass or less from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, more preferably 80% by mass or less, even more preferably 65% by mass or less from the viewpoint of productivity and ease of production, and even more preferably 50% by mass or less, particularly preferably 45% by mass or less from the viewpoint of the degree of biomass conversion and productivity. Also, from the same viewpoint, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. Note that when two or more types of polyolefin fiber are used, the above content refers to the total content of the polyolefin fibers.
[0038] When resin A is a fiber other than polyolefin fiber, the preferred fiber length, fiber diameter, fineness, and content of the fiber are the same as the preferred fiber length, fiber diameter, fineness, and content of polyolefin fiber, respectively. When resin A is a powder, granules, or pellets, the preferred content of the powder, granules, or pellets is the same as the preferred content of the polyolefin fiber. When resin A is a powder, granules, or pellets, the particle size of the powder, granules, or pellets is not particularly limited.
[0039] [Other Components] When the resin A in the fiber assembly of this embodiment is a polyolefin fiber, the fiber assembly may contain other components in addition to the cellulose fiber and polyolefin fiber described above. Examples of other components include an elastomer and a binder component, which will be described later. When a binder component is contained, the content of the binder component is preferably 0.1% by mass or more and 40% by mass or less, more preferably 0.3% by mass or more and 30% by mass or less, even more preferably 0.4% by mass or more and 20% by mass or less, and even more preferably 0.5% by mass or more and 10% by mass or less, relative to the total mass of the fiber assembly. By keeping the content of the binder component within the above range, handleability and the like can be improved when producing a molded product. Examples of binder components that can be used include various starches, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose, acrylic resins, styrene-(meth)acrylic acid ester copolymer resins, urethane resins, polyvinyl alcohol (PVA) resins, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymers, styrene-maleic anhydride copolymer alkali salts, isobutylene-maleic anhydride copolymer alkali salts, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, and ethylene-vinyl acetate copolymers.
[0040] The fiber assembly may further contain fillers, papermaking chemicals, and fatty acid metal salts. Examples of fillers include mineral pigments such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, as well as organic pigments such as polystyrene resins, urea resins, melamine resins, acrylic resins, and vinylidene chloride resins. Examples of papermaking chemicals include paper strength agents, retention aids, drainage aids, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, and slime control agents. Examples of paper strength agents include polyacrylamides. Wet strength agents can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.
[0041] The fatty acid metal salt is preferably a metal salt of an aliphatic carboxylic acid, and the aliphatic carboxylic acid is preferably a saturated or unsaturated aliphatic carboxylic acid having from 12 to 24 carbon atoms. Specific examples include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, heneicosylic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid. Metal elements that form the metal salt include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium, and barium; and Group 3 elements such as zinc and aluminum, with calcium, magnesium, zinc, and aluminum being preferred. Examples of fatty acid metal salts include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, lithium stearate, zinc laurate, and barium laurate. Among these, from the viewpoint of excellent bending rigidity and impact resistance, calcium stearate, magnesium stearate, zinc stearate, aluminum stearate, calcium oleate, magnesium oleate, zinc oleate, aluminum oleate, zinc laurate, or calcium laurate is preferred, and calcium stearate is more preferred. From the viewpoint of bending rigidity and impact resistance, the content of the fatty acid metal salt in the molded product is 0.1% by mass or more and 10% by mass or less, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.8% by mass or more, and preferably 9% by mass or less, more preferably 8% by mass or less, even more preferably 7% by mass or less, and still more preferably 6% by mass or less.
[0042] When other components are contained, the content of the other components excluding cellulose fibers and polyolefin fibers is preferably 0.1 mass% or more and 40 mass% or less, more preferably 0.3 mass% or more and 30 mass% or less, even more preferably 0.4 mass% or more and 20 mass% or less, and still more preferably 0.5 mass% or more and 10 mass% or less, relative to the total mass of the fiber assembly.
[0043] [Fiber aggregate manufacturing process] Next, the fiber aggregate manufacturing process will be described. In the following explanation of the fiber aggregate manufacturing process, it will be explained that a preferred polyolefin fiber is used as the resin A. When a resin other than polyolefin fiber is used as the resin A, the resin used will be read as the resin A instead of polyolefin fiber, and the other explanations will be the same. Note that the resin A can be used alone or in combination of two or more types, as described below.
[0044] In the process for producing a fiber assembly (Step 1) of this embodiment, cellulose fibers and resin A are produced by dry papermaking. The process for producing a fiber assembly preferably includes a step of mixing cellulose fibers and polyolefin fibers in air and depositing the mixture. That is, the fiber assembly of this embodiment is preferably a dry nonwoven fabric.
[0045] When producing a fiber assembly using a dry papermaking method, it is preferable to use an airlaid method. The airlaid method is a method in which an airflow containing raw fibers, such as polyolefin fibers and cellulose fibers defibrated in the air and uniformly mixed in the airflow, is discharged onto a mesh-like endless belt equipped with a suction box below to form an airlaid web. That is, the airlaid method includes a step of mixing cellulose fibers and polyolefin fibers in the air and depositing them. In the airlaid method, the above operation may be repeated multiple times as necessary.
[0046] The web formed by the above method is made into a sheet by the fiber bonding process described below. Examples of the fiber bonding process include a needle punching method, in which polyolefin fibers or cellulose fibers are entangled by passing needles perpendicular to the web surface to form a sheet. This bonding process is preferably used in combination with a carding web formation method. The fiber bonding process can also be performed using a thermal bonding process, in which a heat-fusible adhesive incorporated into a dry-laid web is heated to fuse the raw fibers together; a chemical bonding process, in which an adhesive is applied to the resulting dry-laid web to bond the raw fibers; or a multi-bond process, which combines the thermal and chemical bonding processes.
[0047] In the thermal bonding method, it is preferable to heat at a temperature at least 20° C. higher than the melting point of the heat-fusible adhesive. Examples of the heat treatment include hot air treatment and hot-air treatment followed by low-pressure heat and pressure treatment.
[0048] When the thermal bond method or multi-bond method is employed, it is preferable to use a particulate or fibrous heat-fusible adhesive. The heat-fusible adhesive may be the polyolefin fiber or binder component described above. As the particulate heat-fusible adhesive, heat-fusible resin particles such as polyethylene, polypropylene, polyester low-melting point polyethylene terephthalate, low-melting point polyamide, low-melting point polylactic acid, and polybutylene succinate are used. As the fibrous heat-fusible adhesive, resins such as low-melting point polyethylene terephthalate, low-melting point polylactic acid, polybutylene succinate (PBS), and polyethylene terephthalate (PET), low-melting point polyamide, acrylic resin, and polyvinyl acetate (PVAc) are used. Furthermore, as the heat-fusible synthetic fiber, a core-sheath type heat-fusible composite synthetic fiber obtained by combining two types of resins with different melting points and in which only the surface of the fiber melts, can also be preferably used. A sheath-core heat-fusible composite synthetic fiber has a core made of a resin with a high melting point and a sheath made of a resin with a low melting point formed on the outer periphery thereof. Specific examples include a combination of two resins with different melting points (PET / PET composite fiber, PE / PET composite fiber, MAPE / PP composite fiber, PP / PET composite fiber, PE / PP composite fiber, PVAc / PET composite resin).
[0049] Furthermore, when a chemical bonding method is used to bond the fibers, it is preferable to add a binder component to bond the fibers together. The binder component can be appropriately selected as needed, and examples include solution-type binders such as starch, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose sodium salt, polyvinyl alcohol (PVA), and sodium polyacrylate, as well as emulsion-type binders such as polyacrylic acid esters, acrylic-styrene copolymers, polyvinyl acetate, ethylene-vinyl acetate copolymers, acrylonitrile-butadiene copolymers, methyl methacrylate-butadiene copolymers, urea-melamine resins, and styrene-butadiene copolymer resins. It is also preferable to use the binder components described above. The binders can be in various forms, such as fibers, powders, granules, solutions, or emulsions, and two or more types can be used in combination.
[0050] In a fiber aggregate produced by the above-described dry papermaking method, the fibers constituting the fiber aggregate are three-dimensionally oriented randomly in the longitudinal, width, and thickness directions. Therefore, in this embodiment, the tensile strength of the fiber aggregate in the first direction and the tensile strength in the second direction are approximately the same. That is, in this embodiment, a fiber aggregate with excellent isotropy in the planar direction is obtained.
[0051] In the manufacturing process of the fiber assembly, any sheet that does not impair moldability may be laminated on the fiber assembly to manufacture a laminated sheet. For example, the optional sheet can be laminated on the surface of the fiber assembly or between sheets when laminating the fiber assembly. Sheets such as tissue and nonwoven fabric can be used as the optional sheet to be laminated. These optional sheets are laminated for the purpose of improving the surface properties of the fiber assembly or cellulose fiber-containing resin sheet during the manufacturing process, improving productivity, and imparting other functions.
[0052] <Step 2> Step 2 is a cellulose fiber-containing resin sheet production step in which the fiber aggregate obtained in step 1 is compressed to produce a cellulose fiber-containing resin sheet. A sheet-like cellulose fiber-containing resin sheet is obtained by compressing the fiber aggregate obtained in step 1. The compression may be performed simultaneously with the heat treatment or after the heat treatment.
[0053] Compression of the fiber aggregate can be achieved by applying pressure to the fiber aggregate using a roll press. Heating may be performed simultaneously during the roll press treatment, resulting in a heat-press treatment. The roll press treatment uses metal rolls or resin rolls to apply pressure, allowing the density of the resulting cellulose fiber-containing resin sheet to be controlled as desired. Specifically, a cellulose fiber-containing resin sheet with any density can be obtained by setting any number of rolls, any temperature, and any clearance for the roll press treatment, and heating and pressurizing the sheet. The sheet may be compressed to the desired density by passing through multiple rolls.
[0054] Compression of the fiber aggregate can also be achieved by pressure treatment using a hot press. The density of the resulting cellulose fiber-containing resin sheet can be controlled as desired by subjecting a fiber aggregate cut to an appropriate size, or a cellulose fiber-containing resin sheet that has been subjected to the roll press treatment, to pressure treatment using an autoclave method or a mold press method. Heating to a temperature of 100°C or higher and applying pressure to 2 MPa or higher can produce a cellulose fiber-containing resin sheet with a higher density than that obtained by pressure treatment using a roll press. A pre-pressing step may be included before achieving the above heating and pressure conditions. It is also preferable to perform pre-pressing at a lower pressure under the desired heating conditions, and then increase the pressure and perform pressure treatment using a hot press.
[0055] The pressure treatment step by hot pressing may be a stamping molding method. In the stamping molding method, a fiber assembly is heated in advance, the polyolefin is melted and softened, and the assembly is placed in a mold, the mold is then closed to clamp the assembly, and the assembly is then cooled under pressure. For heating, a heating device such as a far-infrared heater, a heating plate, a high-temperature oven, or a dielectric heater may be used.
[0056] The pressure treatment step by hot pressing may be a vacuum molding method. Vacuum molding can improve the adhesion between the fiber aggregate and the mold by creating a vacuum between the fiber aggregate and the mold, thereby improving moldability. Vacuum molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, vacuum molding is performed in the step of heating the fiber aggregate, melting and softening the polyolefin, placing it inside the mold, and then closing the mold to clamp it. In vacuum molding, vacuum suction is performed from the mold side. The molding pressure in vacuum molding is usually 1.0 kg / cm. 2 The molding is carried out for about 0.1 seconds to 60 seconds.
[0057] The pressure treatment step by heat pressing may be a pressure molding method. In the pressure molding method, compressed air is blown onto the fiber assembly to make it adhere to the mold, thereby increasing the adhesion between the fiber assembly and the mold. The pressure molding is preferably carried out in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, and the polyolefin is placed in a melted and softened state in a mold, and then compressed air is blown onto the fiber assembly side to perform molding. The pressure molding is carried out at a pressure of 3 kg / cm. 2 More than 8kg / cm 2 The molding is often carried out at a compressed air pressure of the following value, and molding is preferably carried out for 0.1 to 60 seconds.
[0058] Compression of the fiber assembly can also be achieved by supercalendering. In the supercalendering, the fiber assembly is molded by passing it between heated rollers while applying nip pressure. The heating temperature of the rollers used is preferably at least 10°C higher, more preferably at least 20°C higher, and even more preferably at least 30°C higher than the melting point of the polyolefin fiber, and is preferably not higher than 100°C, more preferably not higher than 90°C, and even more preferably not higher than 80°C than the melting point of the polyolefin fiber. The nip pressure is preferably at least 100 kg / cm, more preferably at least 150 kg / cm, and even more preferably at least 200 kg / cm, and is preferably not higher than 450 kg / cm, more preferably not higher than 400 kg / cm, and even more preferably not higher than 350 kg / cm. The number of nip stages is preferably at least 1, more preferably at least 3, and even more preferably at least 5, and preferably not higher than 20, more preferably not higher than 18, and even more preferably not higher than 16. When compressing the fiber assembly to produce a cellulose fiber-containing sheet, a plurality of cellulose fiber-containing sheets may be stacked and compressed as appropriate depending on the desired thickness of the cellulose fiber-containing sheet.
[0059] In this embodiment, the cellulose fiber-containing resin sheet preferably has a T / Y ratio of 0.5 to 1.5, where T is the tensile strength in a first direction and Y is the tensile strength in a second direction perpendicular to the first direction. By setting the T / Y ratio to 0.5 to 1.5, the fibers constituting the cellulose fiber-containing resin sheet are extremely uniformly mixed, resulting in a molded product that has excellent impact resistance as well as rigidity and strength against bending. T / Y is preferably 0.60 or more, more preferably 0.70 or more, even more preferably 0.80 or more, even more preferably 0.85 or more, and is preferably 1.40 or less, more preferably 1.30 or less, even more preferably 1.20 or less, and even more preferably 1.15 or less. The first direction of the cellulose fiber-containing resin sheet is any one direction in the planar direction of the cellulose fiber-containing resin sheet. However, if the fibers contained in the cellulose fiber-containing resin sheet are oriented in any direction in the planar direction, the orientation direction is defined as the first direction. Furthermore, when the flow direction in the manufacturing process of the fiber aggregate by dry papermaking is known, the flow direction is referred to as the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the flow direction in the manufacturing process is referred to as the first direction (MD direction), and the flow direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes referred to as the T-mesh. The second direction of the fiber aggregate is one direction in the planar direction of the fiber aggregate and is a direction perpendicular to the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the direction perpendicular to the flow direction in the manufacturing process is referred to as the second direction (CD direction), and the second direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes referred to as the Y-mesh. The tensile strength in the first and second directions of the cellulose fiber-containing resin sheet is measured in accordance with JIS P 8113:2006. The tensile strength in each direction was measured using a tensile tester, Tensilon manufactured by A&D Co., Ltd., at a speed of 20±5 mm / min on a strip of 15±0.1 mm×180±1 mm.
[0060] In this embodiment, the cellulose fiber-containing resin sheet is a sheet-like product obtained by mixing at least cellulose fibers and resin A (preferably polyolefin fibers) and then dry-pressing the mixture. The sheet is obtained by pressing a cotton-like fiber aggregate (hereinafter also referred to as a cotton-like fiber aggregate) after dry-pressing, and may have various bulk specific gravities (densities). The bulk specific gravity of the cellulose fiber-containing resin sheet to be fed to the screw-type kneader is preferably 0.10 g / mL or more and 0.60 g / mL or less, more preferably 0.15 g / mL or more, and more preferably 0.50 g / mL or less, and even more preferably 0.40 g / mL or less, from the viewpoints of ease of compression in step 2, ease of subsequent melt-kneading, and ease of cutting when cutting for feeding to the melt-kneader. The bulk specific gravity of the cellulose fiber-containing resin sheet is measured by the method described in the examples.
[0061] <Step 3> Step 3 is a cellulose fiber-containing resin pellet production step in which the cellulose fiber-containing resin sheet is melt-kneaded to produce cellulose fiber-containing resin pellets (hereinafter also simply referred to as "pellets"). From the viewpoint of facilitating supply to a melt kneader before melt-kneading, it is preferable to cut, crush, etc. the cellulose fiber-containing resin sheet before feeding it into the melt kneader. The cutter is not particularly limited, and examples thereof include a shredder. The size after cutting, crushing, etc. is not particularly limited, and it is sufficient as long as it is a size that can be supplied to a kneader.
[0062] The method for producing pellets is not particularly limited, and is not particularly limited as long as a cellulose fiber-containing resin sheet is supplied and melt-kneaded. Examples of devices used for melt-kneading include a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, a mixing roll mill, an open roll mill, and a glass mixer. After supplying and melt-kneading a cellulose fiber-containing resin sheet, (1) the cellulose fiber-containing resin is extruded into a strand shape and cooled and solidified to obtain cellulose fiber-containing resin pellets, (2) the cellulose fiber-kneaded product is cooled and solidified either directly or after being stretched into a sheet shape, and then crushed in a crusher to obtain cellulose fiber-containing resin pellets, (3) the cellulose fiber-containing resin is extruded into a rod or cylinder shape and cooled to obtain cellulose fiber-containing resin pellets, (4) the cellulose fiber-containing resin is extruded through a T-die to obtain a sheet or film-like cellulose fiber-containing resin, which is then cut or crushed to obtain cellulose fiber-containing resin pellets, or (5) the cellulose fiber-containing resin immediately after extrusion is cut with a rotary blade in air or water to obtain cellulose fiber-containing resin pellets.
[0063] The size of the pellets obtained in step 3 is not particularly limited, but is preferably 1 to 10 mm from the viewpoint of ease of feeding into an injection molding machine.
[0064] The melt-kneading temperature (barrel set temperature) is not particularly limited, but is preferably adjusted so that the temperature of the melt-kneaded product (the temperature of the actually obtained kneaded product, the resin temperature) is at least 5°C higher than the melting point of the polyolefin, more preferably at least 10°C higher, and even more preferably at least 15°C higher. From the viewpoint of deterioration of the cellulose fiber, the barrel set temperature is preferably at most 100°C higher than the melting point of the polyolefin, more preferably at most 90°C higher, and even more preferably at most 80°C higher. The temperature of the melt-kneaded product becomes higher than the melt-kneading temperature (barrel set temperature) due to shear heat generated during melt-kneading. In other words, it varies depending on various conditions during melt-kneading, such as the melt-kneading temperature (barrel set temperature), discharge rate, rotation speed, and screw design of the melt-kneader. In the case of the method described in the examples, the temperature of the melt-kneaded product is about 20 to 40°C higher than the melt-kneading temperature (barrel set temperature), and therefore the melt-kneading temperature (barrel set temperature) is about 20 to 40°C lower than the preferred temperature of the melt-kneaded product.
[0065] Various conditions during melt-kneading, such as discharge speed and rotation speed, may be adjusted according to known techniques. When the melt-kneading device is a twin-screw extruder, it is desirable to design the screw so that the kneading force is as weak as possible. In the present invention, the cellulose fibers and resin A are uniformly dispersed in the cellulose fiber-containing resin sheet in advance, and even when melt-kneading is performed without applying high shear force, the dispersion state of the cellulose fibers in the cellulose fiber-containing resin sheet is maintained as is, resulting in pellets with excellent cellulose fiber dispersion. Therefore, weak kneading force can prevent cellulose fiber breakage. Specifically, R-type kneading parts are mainly used as kneading parts, and the number of L-type and N-type kneading parts is preferably the same as or less than the number of R-type kneading parts, and more preferably less than the number of R-type kneading parts. The number of kneading parts is preferably 5 or less, and more preferably 3 or less, of the 10 parts divided into the entire screw.
[0066] In step 3, a resin component may be further blended and melt-kneaded together with the cellulose fiber-containing resin sheet, and the resin component is preferably a polyolefin resin or the above-mentioned elastomer. Blending at least one selected from a polyolefin resin and an elastomer in step 3 is preferred because it results in a molded product with superior impact resistance. That is, the obtained cellulose fiber-containing resin pellets contain the components blended in step 3 in addition to the components derived from the cellulose fiber-containing resin sheet.
[0067] Elastomers, which may be blended during melt kneading, are polymeric compounds that exhibit elastic deformation. They soften and become fluid when heated and return to a rubbery state when cooled. Specifically, elastomers have a structure consisting of two polymers: hard and soft segments. The hard segments act as crosslinks, while the soft segments exhibit rubber-like elasticity, resulting in elasticity. Therefore, at room temperature, the hard segments aggregate to form a pseudo-crosslinked state, exhibiting rubber-like properties. However, at high temperatures, they melt, losing their crosslinking function and allowing plastic deformation. Depending on the combination of hard and soft segment polymers, elastomers are classified as polystyrene-based, olefin / alkene-based, polyester-based, polyvinyl chloride-based, polyurethane-based, polyamide-based, polyacrylic elastomers, silicone-based, and polyimide-based. Furthermore, even within the same system, properties vary depending on the ratio of hard and soft segments and molecular weight. For example, polystyrene-based elastomers may use styrene for the hard segment and butadiene for the soft segment. In this case, a high styrene content results in high hardness and improved compatibility with polystyrene and polyphenylene ether, while a low styrene content results in low hardness, high flexibility, and improved compatibility with polyolefins. Furthermore, a high molecular weight improves temperature characteristics and mechanical properties, while a low molecular weight improves processability and transparency. Examples of polystyrene-based elastomers include the Tuftec series manufactured by Asahi Kasei Corporation. For example, there are olefin / alkene-based elastomers that combine ethylene, propylene, and 1-butene. The density, elastic modulus, and melting point can be varied depending on the combination and ratio. Furthermore, the structure when mixed with resins varies, resulting in islands-like dispersion or compatibility. Examples of olefin / alkene-based elastomers include the Tafmer series manufactured by Mitsui Chemicals, Inc. Among these, polystyrene-based elastomers and olefin / alkene-based elastomers are preferred from the perspective of impact resistance, etc. Examples of elastomers include the various elastomers described in paragraphs 0043 to 0065 of Published Japanese Patent Application No. 2020 / 080328.The method for adding the elastomer is not particularly limited, and it is preferable to supply the elastomer together with the cellulose fiber-containing resin sheet during melt-kneading of the cellulose fiber-containing resin sheet, and then melt-knead the elastomer.
[0068] When the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is, from the viewpoint of improving the flexural modulus, preferably 55% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, still more preferably 40% by mass or less, and particularly preferably 35% by mass or less, relative to the total mass of resin A and the elastomer. Furthermore, when the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is, from the viewpoint of improving the impact resistance, preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, still more preferably 12% by mass or more, and particularly preferably 15% by mass or more, relative to the total mass of resin A and the elastomer.
[0069] <Step 4> Step 4 is a step of molding the cellulose fiber-containing resin pellets obtained in Step 3. Various molding methods can be used for the molding step, including, for example, injection molding (e.g., injection compression molding (press injection, hot flow stamping molding, gas injection compression molding), gas injection molding, and ultra-high speed injection molding), various extrusion moldings (cold runner method or hot runner method), compression (press) molding, insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, and various profile extrusion moldings (e.g., two-color molding and sandwich molding). For example, various extrusion moldings are suitable for molding sheets, films, fibers, etc. Inflation, calendaring, casting, and other methods can also be used to mold sheets or films. Furthermore, a specific stretching operation may be performed. Hollow molded articles can also be formed by rotational molding, blow molding, or the like. Multiple molding steps may be combined, or multiple steps may be performed simultaneously to form a single process. For example, the cellulose fiber-containing resin pellets may be formed into a sheet and then subjected to heat press molding to obtain a molded article, or the cellulose fiber-containing resin pellets may be formed into a sheet and then subjected to supercalendering to obtain a molded article. After forming into a sheet, the cellulose fiber-containing resin pellets may be molded by vacuum forming, pressure forming, etc. Among these, injection molding is a preferred example.
[0070] When the molding step is an injection molding step, the injection molding step involves, for example, using a known injection molding machine to melt and knead the above-mentioned cellulose fiber-containing resin pellets and injecting the molten mixture into a mold to form the product. When melt-kneading, any known kneading machine can be used, such as a single-screw kneader or a twin-screw kneader. Examples of known injection molding machines include screw-type injection molding machines, screw pre-plasticizing injection molding machines, plunger pre-plasticizing injection molding machines, and plunger injection molding machines. Examples of drive systems include hydraulic, electric, and hydraulic-electric hybrid systems.
[0071] The temperature conditions for injection molding are determined appropriately depending on the type of resin contained in the pellets, and it is preferable to set the cylinder temperature of the injection molding machine to a temperature 0 to 100°C higher than the flow initiation temperature of the resin used. The temperature of the mold may be selected appropriately in view of the cooling rate and productivity of the resin used, and in the case of polyolefin, for example, it is preferable to set it in the range of room temperature (e.g., 23°C) to 120°C. Other injection conditions such as the screw rotation speed, back pressure, injection speed, dwell pressure, and dwell time may be adjusted appropriately.
[0072] The cellulose fiber-containing resin pellets of this embodiment may contain other resins, such as elastomers, by adding and melt-kneading other resins, such as elastomers, during molding. Furthermore, in the process of producing a molded article, other resins, various additives, masterbatches containing various additives, etc. may be added in addition to the cellulose fiber-containing resin pellets during injection molding. Examples of additives include those typically used in resin compositions. Examples of such additives include stabilizers, UV absorbers, plasticizers, flame retardants, flame retardant assistants, antistatic agents, surfactants, colorants, lubricants, and mold release agents. Examples of stabilizers include hindered phenols, hydroquinones, phosphites, and their substituted derivatives. Examples of UV absorbers include resorcinol, salicylate, benzotriazole, and benzophenone. Examples of colorants include dyes such as nitrosine, and pigments such as cadmium sulfide, phthalocyanine, and carbon black. Examples of lubricants include fatty acids such as stearic acid and montanic acid, their amides, their esters, their half esters with polyhydric alcohols, stearyl alcohol, stearamide, polyethylene wax, and paraffin wax.
[0073] [Method for producing recycled cellulose fiber-containing resin molded body] A method for producing a recycled cellulose fiber-containing resin molded body (molded body (n+1th recycling)) by recycling a molded body (nth recycling) will be described as an example, but the same applies to the production of a molded body (first recycling) from a molded body (initial). When recycling a molded body (nth recycling), it is preferable to pulverize the molded body (nth recycling). The pulverization method is not particularly limited as long as it can be pulverized to a size that can be fed to an injection molding machine or a kneading machine, and various pulverizers can be selected appropriately. Note that, if necessary, a cleaning process or removal of unnecessary parts may be performed before pulverizing the molded body (nth recycling). It is preferable to mold the pulverized product as is, and it is more preferable to injection mold the pulverized product as is. The recycled cellulose fiber-containing resin molded body (n+1th recycling) of this embodiment is obtained by molding the pulverized product of a cellulose fiber-containing resin molded body (nth recycling) as is in the same manner as for the molded body (nth recycling).
[0074] In actual recycling, various embodiments as shown below may be adopted. 1. In addition to the pulverized material of the molded body (recycled nth time), one or more of cellulose fiber-containing resin pellets newly obtained from a cellulose fiber-containing resin sheet, or, when n is 2 or more, the pulverized material of the molded body (recycled n-mth time), are supplied to a molding machine and molded. Here, m is a natural number smaller than n. 2. The pulverized material of the molded body (recycled nth time) is supplied to a kneader to produce pellets, which are then molded. 3. In addition to the pulverized material of the molded body (recycled nth time), one or more of cut material of a cellulose fiber-containing resin sheet, cellulose fiber-containing resin pellets newly obtained from a cellulose fiber-containing resin sheet, or, when n is 2 or more, the pulverized material of the molded body (recycled n-mth time), are added to produce pellets, which are then molded. Here, m is a natural number smaller than n. 4. Various components are further added to the molding machine or kneader to satisfy the physical properties required of the molded body (recycled n+1th time). In actual recycling, a combination of the above-described modes may be employed. For example, a method can be exemplified in which 3. and 4. are combined to add cut pieces of a cellulose fiber-containing resin sheet and the above-described elastomer to the pulverized molded body (recycled n-th time), produce pellets, and then mold the pellets.
[0075] (Uses) The molded article of the present embodiment is preferably used for electrical and electronic equipment, office automation equipment, home appliances, civil engineering and construction, automobile and aircraft parts, structural parts and housings, containers (for example, food containers, drug packaging containers, cosmetic packaging containers, medical device packaging containers), furniture, daily necessities, medical tools, etc. Among these, it is suitable for uses requiring impact resistance, such as civil engineering and construction, automobile or aircraft parts, structural parts, and housings.
[0076] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.
[0077] (Example 1) <Preparation of fiber aggregate> NBKP was defibrated using a swirling jet airflow defibrator to obtain defibrated dry pulp. The processing air speed in the defibrator was 45 m / min, and turbulence was achieved using a baffle installed in the device. The obtained defibrated dry pulp had an average fiber length of 2.38 mm, an average fiber width of 34.3 μm, and a fine fiber ratio of 11.4%.
[0078] Next, the obtained defibrated dry pulp, polypropylene fiber (melting point 160°C, fineness 6.6 dtex, fiber length 5 mm, fiber diameter 30 μm, also referred to as PP fiber), and polyethylene / polypropylene composite core-sheath fiber (core melting point 160°C, sheath melting point 110°C, fineness 1.7 dtex, fiber length 5 mm, fiber diameter 15 μm, also referred to as PE / PP composite fiber) were uniformly mixed by air flow in a ratio (mass ratio) of 30 / 55 / 15 to obtain a fiber mixture.
[0079] Next, an air-laid web was formed from the fiber mixture using the web forming apparatus 1 shown in FIG. 1. Specifically, a first carrier sheet 41 was fed by a first carrier sheet supplying means 40 onto a permeable endless belt 20 that was attached to a conveyor 10 and running. In Example 1, tissue (basis weight 14 g / m) was used as the first carrier sheet 41. 2 The "basis weight" was measured in accordance with "Paper and paperboard - Method for measuring basis weight" described in JIS P8124:2011.
[0080] While the air-permeable endless belt 20 was being sucked by the suction box 60, the fiber mixture was dropped and deposited on the first carrier sheet 41 together with the air flow from the fiber mixture supply means 30, to obtain a cotton-like fiber aggregate. At this time, the basis weight (set basis weight) of the air-laid web portion was 400 g / m 2 The fiber mixture was supplied so that
[0081] Next, a second carrier sheet 51 was laminated on the cotton-like fiber aggregate on the first carrier sheet 41 by a second carrier sheet supplying means 50, to obtain a fiber aggregate containing an air-laid web. In Example 1, tissue (basis weight 14 g / m) was used as the second carrier sheet 51. 2That is, in Example 1, the same sheet was used for the first carrier sheet 41 and the second carrier sheet 51.
[0082] <Preparation of Cellulose Fiber-Containing Resin Sheet> The obtained fiber assembly containing the air-laid web was passed through a box-type dryer with a hot air circulation conveyor oven system and subjected to hot air treatment at a temperature of 140°C. Thereafter, the density was adjusted by roll press treatment so that the bulk specific gravity was 0.3 g / mL, and the basis weight was 449.5 g / m 2 A cellulose fiber-containing resin sheet was obtained. The cellulose fiber-containing resin sheet had a T / Y ratio of 0.88, a bulk specific gravity of 0.29 g / mL, and a thickness of 1.55 mm. The cellulose fiber-containing resin sheet was shredded using a shredder (AFS100M, manufactured by Iris Ohyama Co., Ltd.) to obtain cut chips of approximately 4 mm x 13 mm.
[0083] <Preparation of Molded Article of the Present Embodiment> The cut chips were fed into a twin-screw kneading extruder (HK-25D (41D) manufactured by Parker Corporation) and melt-kneaded and dispersed at a kneading temperature of 180°C and an output rate of 2.5 kg / hour. The screw used for kneading was divided into seven parts, with only the fifth part counting from the raw material inlet side using a kneading part consisting of six parts, and all the remaining parts having a weak kneading configuration consisting of feed screws. All kneading parts were R-type. After melt-kneading and dispersion, the mixture was air-cooled to produce pellets. Using the pellets, a Type A1 multipurpose test piece specified in JIS K 7139:2009 was injection-molded at a molding temperature of 170°C and an injection speed of 30 mm / sec to obtain a cellulose fiber-containing resin molded article (initial form) having a thickness of 4 mm.
[0084] (Example 2) A 4 mm thick cellulose fiber-containing resin molded body (initial) was obtained in the same manner as in Example 1, except that in <Preparation of fiber aggregate> in Example 1, the fiber mixture was changed to a ratio (mass ratio) of 50 / 35 / 15, the discharge rate was set to 3.0 kg / hour, and in <Preparation of molded body of this embodiment>, the molding temperature was changed to 180°C. The basis weight of the cellulose fiber-containing resin sheet before obtaining the cut chips was 438.9 g / m 2, T / Y was 0.88, bulk density was 0.33 g / mL, and thickness was 1.33 mm.
[0085] Comparative Example 1 Using pellets of glass fiber reinforced polypropylene (Prime Polypro R-200G, manufactured by Prime Polymer Co., Ltd.) containing 20% by mass of glass fiber, a Type A1 multipurpose test piece as specified in JIS K 7139:2009 was injection molded at a molding temperature of 220°C and an injection speed of 100 mm / sec to obtain a glass fiber-containing resin molded body (initial state) having a thickness of 4 mm.
[0086] <Preparation of Molded Articles for Evaluating Recyclability> A portion of the initial molded articles obtained by the methods of the above Examples and Comparative Examples was pulverized using a uniaxial low-speed crusher (SCUTTER SX-250-T, manufactured by STORZ Co., Ltd.) and then injection molded under the conditions of each Example and Comparative Example to obtain a first recycled cellulose fiber-containing resin molded article and a glass fiber-containing resin molded article. A portion of this first recycled molded article was pulverized using a uniaxial low-speed crusher (SCUTTER SX-250-T, manufactured by STORZ Co., Ltd.) and then injection molded under the conditions of each Example and Comparative Example to obtain a second recycled cellulose fiber-containing resin molded article and a glass fiber-containing resin molded article.
[0087] <Measurement and Evaluation> (Method for Measuring Fiber Length and Fiber Diameter of Polyolefin Fiber) Twenty randomly selected polyolefin fibers were observed under an optical microscope, and the fiber length and fiber diameter were measured.
[0088] (Method for measuring average fiber length, average fiber diameter, and fine fiber ratio of cellulose fibers) In accordance with ISO 16065-2, the average fiber length and average fiber diameter of cellulose fibers were measured using a fiber image analyzer (Valmet FS5, manufactured by Valmet Co., Ltd.) The proportion of fine fibers of 0.1 mm or less in the measured length-weighted average fiber length distribution was defined as the fine fiber ratio.
[0089] (Method for measuring the fineness of polyolefin fibers) When a catalog value or the like is available for the fineness of polyolefin fibers, the catalog value may be used. In this example, the catalog value was used. When no catalog value is available, the fineness is measured by Method B of JIS L 1013:2010 (Testing methods for chemical fiber filament yarns).
[0090] (Method for measuring the melting point of polyolefin fiber) When a catalog value for the polyolefin fiber is available, the catalog value may be used for the melting point of the polyolefin fiber. In this example, the catalog value was used. If a catalog value is not available, the melting point can be measured by the following method. 5 mg of polyolefin fiber is cut out, and the melting point of the polyolefin fiber is measured using a differential scanning calorimeter (DSC). The melting point is measured using a Diamond DSC manufactured by Perkin-Elmer, by increasing the temperature from 30°C to 280°C at a rate of 20°C / min under a nitrogen atmosphere.
[0091] (Method for measuring bulk density of cellulose fiber-containing resin sheet) The bulk density of the cellulose fiber-containing resin sheet was calculated by measuring the thickness and mass of a 50 mm square sheet after conditioning it for 24 hours under conditions of 23°C and 50% RH. The thickness of the sheet was measured with a digital thickness gauge (DG-127, manufactured by Ozaki Seisakusho Co., Ltd.).
[0092] (Method for measuring T / Y) The flow direction (running direction of the conveyor 10) in the manufacturing process of the obtained fiber aggregate was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction. The tensile strength (unit: N / m) of the cellulose fiber-containing resin sheet was measured in accordance with JIS P 8113:2006. The tensile strength in each direction was calculated by dividing the tensile strength by the thickness of the test piece (unit: MPa). A Tensilon manufactured by A&D Co., Ltd. was used as a tensile tester, and a 15 mm x 180 mm strip was measured at a speed of 20 mm / min.
[0093] (Method for measuring density of molded article) The obtained molded article (molded body) was cut into a strip-shaped test piece of 80 mm length x 10 mm width. The thickness of the strip-shaped test piece was measured with a constant pressure thickness measuring device (manufactured by Teclock Corporation, model number PG-02J), and the volume of the strip-shaped test piece was calculated. Furthermore, the density was calculated by measuring the mass of the strip-shaped test piece.
[0094] (Method for measuring flexural modulus and flexural strength of molded article) The obtained molded article was cut into a strip-shaped test piece of 80 mm length x 10 mm width, and a three-point bending test was performed in accordance with JIS K 7171: 2016. The obtained flexural modulus and flexural strength were evaluated such that the larger the numerical value, the better the rigidity and strength against bending, respectively.
[0095] (Method for measuring impact resistance of molded article) The obtained molded article was cut into a strip-shaped test piece of 80 mm length x 10 mm width, and a notched Charpy impact test (impact direction: edgewise) was performed in accordance with JIS K 7111-1: 2012. The larger the obtained Charpy impact strength value, the better the impact resistance and the stronger it was evaluated to be against impact.
[0096]
[0097] As shown in the examples, the cellulose fiber-containing resin molded article of the present invention had excellent bending rigidity and also excellent recyclability, while the molded article of Comparative Example 1 had poor recyclability.
[0098] REFERENCE SIGNS LIST 1 Web forming device 10 Conveyor 20 Permeable endless belt 30 Fiber mixture supply means 40 First carrier sheet supply means 41 First carrier sheet 50 Second carrier sheet supply means 51 Second carrier sheet 60 Suction box
Claims
1. A cellulose fiber-containing resin molded body having a flexural modulus of 2.5 GPa or more measured in accordance with JIS K 7171:2016, and a recycled cellulose fiber-containing resin molded body obtained by melt-kneading the cellulose fiber-containing resin molded body and re-molding the same, in which the flexural modulus is reduced by 10% or less compared to the cellulose fiber-containing resin molded body.
2. A cellulose fiber-containing resin molding according to claim 1, in which the rate of decrease in bending strength in the recycled cellulose fiber-containing resin molding is 10% or less compared to the cellulose fiber-containing resin molding.
3. A cellulose fiber-containing resin molding as described in claim 1 or 2, in which the reduction in Charpy impact strength at a thickness of 4 mm in the recycled cellulose fiber-containing resin molding is 30% or less compared to the cellulose fiber-containing resin molding.
4. A cellulose fiber-containing resin molding according to any one of claims 1 to 3, having a cellulose fiber content of 10% by mass or more and 90% by mass or less.
5. Density is 0.8 g / cm 3 1.5g / cm or more 3 The cellulose fiber-containing resin molded body according to any one of claims 1 to 4, wherein:
6. The cellulose fiber-containing resin molded article according to any one of claims 1 to 5, having a thickness of 2 mm or more.
7. Charpy impact strength at a thickness of 4 mm measured in accordance with JIS K 7111-1:2012 is 2.0 kJ / m 2 The cellulose fiber-containing resin molded article according to any one of claims 1 to 6.
8. The cellulose fiber-containing resin molded body according to any one of claims 1 to 7, wherein the initial cellulose fiber-containing resin molded body before the first recycling is a molded body obtained by a method including the following steps 1, 2, 3, and 4 in this order: Step 1: A fiber assembly production step of producing a fiber assembly containing cellulose fibers and resin A by dry papermaking; Step 2: A cellulose fiber-containing resin sheet production step of compressing the fiber assembly to produce a cellulose fiber-containing resin sheet; Step 3: A cellulose fiber-containing resin pellet production step of melt-kneading the cellulose fiber-containing resin sheet to produce pellets; Step 4: A step of molding the cellulose fiber-containing resin pellets.
9. The cellulose fiber-containing resin molded body according to claim 8, wherein the resin A contains resin fibers.
10. A cellulose fiber-containing resin molding as described in claim 8 or 9, in which when the tensile strength of the cellulose fiber-containing resin sheet in a first direction is T and the tensile strength in a second direction perpendicular to the first direction is Y, T / Y is 0.5 or more and 1.5 or less.
11. A cellulose fiber-containing resin molding according to any one of claims 8 to 10, wherein in step 2, the cellulose fiber-containing resin sheet subjected to step 3 has a bulk density of 0.10 g / mL or more and 0.60 g / mL or less.
12. The cellulose fiber-containing resin molded body according to any one of claims 8 to 11, wherein step 4 is a step of injection molding cellulose fiber-containing resin pellets.
Citation Information
Patent Citations
Pellet structure of fiber reinforced thermoplastic resin
JP1991007307A
Thermoplastic resin composition, process for producing the same, and process for producing molding
WO2008133214A1
Method for production of molded thermoplastic composition article
WO2009072499A1
Method for manufacturing pulp-fiber-containing resin pellet and method for manufacturing molded body
WO2023074842A1