Polycarbonate resin and optical member using said resin

The polycarbonate resin, tailored with specific molecular structures and properties, addresses the limitations of existing polycarbonate resins by achieving low orientational birefringence and high refractive index, enabling effective use in thin optical components like imaging lenses through improved fluidity and mechanical strength.

WO2024225099A1PCT designated stage expired Publication Date: 2024-10-31TEIJIN LTD

Patent Information

Application Number
PCT/JP2024/014996
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Polycarbonate resins used for optical members face challenges with high orientational birefringence, photoelastic coefficient, and refractive index, making them unsuitable for thin optical components like imaging lenses, and they have limitations in molecular weight for injection molding applications.

Method used

A polycarbonate resin with a specific molecular structure, incorporating units represented by formulas (1) and (3), optimized for weight average molecular weight, molar ratios, and specific properties to achieve low orientational birefringence, high Abbe number, and high refractive index, suitable for thin optical members.

Benefits of technology

The optimized polycarbonate resin exhibits excellent fluidity, reduced birefringence, and improved mechanical strength, enabling successful injection molding of thin optical components with enhanced optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014996_31102024_PF_FP_ABST
    Figure JP2024014996_31102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] The first purpose of the present invention is to provide a polycarbonate resin that has excellent fluidity and has a small orientation birefringence. The second purpose of the present invention is, in addition to the first purpose, to further provide a polycarbonate resin that has a high Abbe number and has a small orientation birefringence and a small photoelastic coefficient. The third purpose of the present invention is, in addition to the first purpose, to further provide a polycarbonate resin that has a small orientation birefringence and has a high refractive index and a high glass transition temperature. [Solution] This polycarbonate resin includes a unit that is represented by formula (1) and / or formula (2), and a unit that is represented by formula (3), wherein the weight average molecular weight Mw is 10,000 to 55,000. (In formula (3), R1-R4 each independently represent a hydrogen atom or a C1-10 hydrocarbon group.)
Need to check novelty before this filing date? Find Prior Art

Description

Polycarbonate resin and optical member using said resin

[0001] The present invention relates to a polycarbonate resin and an optical member using the resin.

[0002] Glass, which has traditionally been used as a material for optical systems, is capable of achieving various required optical properties and has excellent environmental resistance, but has the problem of poor processability. In response to this problem, resins, which are cheaper than glass materials and have excellent processability, have come to be used for optical components.

[0003] Patent Document 1 describes an optical lens having a high refractive index and low orientation birefringence, which is made of a polycarbonate resin having a structure of pentacyclopentadecanedimethanol (hereinafter sometimes abbreviated as PCPDM) and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as BPEF).

[0004] Furthermore, in the optical design of optical units, it is known to correct chromatic aberration by combining multiple lenses with different Abbe numbers. For example, chromatic aberration has been corrected by combining a lens made of an alicyclic polyolefin resin, which has a low refractive index and a high Abbe number, with a lens made of a polycarbonate resin (nd = 1.59, vd = 31) derived from bisphenol A, which has a high refractive index and a low Abbe number. In recent years, the development of resins with high refractive indexes and low Abbe numbers has been actively pursued, and this has led to an increase in demand for resins with high Abbe numbers. Furthermore, polycarbonate resins derived from bisphenol A, obtained by reacting 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A) with phosgene or carbonate esters, have excellent heat resistance and transparency, as well as excellent mechanical properties such as impact resistance. Therefore, they are widely used not only as structural materials but also as optical materials, such as optical disk substrates, various lenses, prisms, and optical fibers. However, polycarbonate resins derived from bisphenol A have the problem of high birefringence due to molecular orientation and residual stress during molding. Therefore, with the recent expansion of optical material applications, there is a strong demand for the development of materials with even lower birefringence. For example, Patent Document 2 describes a polycarbonate resin that has a high Abbe number but a low photoelastic coefficient, which is produced by copolymerizing bisphenol A and PCPDM. Furthermore, Patent Document 3 proposes a method for producing a carbonate derivative without using a base, by subjecting a halogenated methane and a specific amount of a hydroxyl group-containing compound to a photoreaction in the presence of oxygen, and cites as an example a copolymerized polycarbonate of BPEF and PCPDM.

[0005] JP 2005-241962 A, JP 2000-302860 A, WO 2020 / 100977 A

[0006] However, polycarbonate resins having the above-mentioned PCPDM and BPEF structure are difficult to mold when applied to thin-walled optical components such as imaging lenses, and further improvement in orientation birefringence is required. Furthermore, the above-mentioned polycarbonate resins composed of bisphenol A and PCPDM have room for improvement in their photoelastic coefficient, large orientation birefringence, and low refractive index and glass transition temperature. Furthermore, the resulting resins have high molecular weights, making them unsuitable for injection molding applications and unable to be used for thin-walled optical components such as imaging lenses. Furthermore, the above-mentioned BPEF and PCPDM copolymer polycarbonate has an extremely low weight-average molecular weight of 3,360, making it insufficient for use as a structural or optical material.

[0007] Therefore, a first object of the present invention is to provide a polycarbonate resin which has excellent flowability and small orientation birefringence.

[0008] A second object of the present invention is to provide a polycarbonate resin which, in addition to the first object, has a high Abbe number, and small orientation birefringence and photoelastic coefficient.

[0009] A third object of the present invention is to provide a polycarbonate resin which, in addition to the first object, has a small orientation birefringence, a high refractive index and a high glass transition temperature.

[0010] The present inventors have found that the above problems can be solved by the present invention having the following aspects.

[0011] That is, the present invention is as follows: <<Aspect 1>> A polycarbonate resin containing units represented by formula (1) and / or formula (2) and units represented by formula (3), and having a weight average molecular weight Mw of 10,000 to 55,000.

[0012]

[0013] (In the formula, R 1 ~R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. 1 ~R 4is a hydrogen atom. Aspect 3: The polycarbonate resin according to aspect 1 or 2, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is 99:1 to 1:99. Aspect 4: The polycarbonate resin according to aspect 3, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is 65:35 to 35:65. Aspect 5: The polycarbonate resin having an absolute value of orientation birefringence of 7.0 x 10 -3 The polycarbonate resin according to aspect 1 or 2, having a photoelastic coefficient of 35×10 or less. -12 The polycarbonate resin according to aspect 1 or 2, having a modulus of elasticity of less than 1 Pa. Aspect 7 The polycarbonate resin according to aspect 1, comprising units represented by formula (1) and / or formula (2) in an amount of 50 mol % or more of all repeating units, and having a weight average molecular weight Mw of 10,000 to 50,000. Aspect 8 The polycarbonate resin according to aspect 7, comprising units represented by formula (3) in an amount of more than 0 mol % but not more than 50 mol % of all repeating units. Aspect 9 The polycarbonate resin according to aspect 7 or 8, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is 99:1 to 50:50. Aspect 10 The polycarbonate resin according to aspect 1, having a modulus of elasticity of less than 1 Pa. -12 The polycarbonate resin according to aspect 7 or 8, having an Abbe number of less than 25.0. Aspect 11 The polycarbonate resin according to aspect 7 or 8, having an Abbe number of 25.0 or more. Aspect 12 The polycarbonate resin according to aspect 1, comprising more than 0% and less than 50 mol% of units represented by formula (1) and / or formula (2) in all repeating units, and having a weight average molecular weight Mw of 10,000 to 50,000. Aspect 13 The polycarbonate resin according to aspect 12, comprising more than 50 mol% of units represented by formula (3) in all repeating units. Aspect 14 The polycarbonate resin according to aspect 12 or 13, having a molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) of 1:99 to 49:51. Aspect 15 The polycarbonate resin having an absolute value of orientation birefringence of 3.0 x 10 -3The polycarbonate resin according to aspect 12 or 13, wherein the refractive index nd is 1.600 or higher. Aspect 16: The polycarbonate resin according to aspect 12 or 13, wherein the refractive index nd is 1.600 or higher. Aspect 17: The polycarbonate resin according to aspect 12 or 13, wherein the glass transition temperature is 140°C or higher. Aspect 18: An optical member made of the polycarbonate resin according to any one of aspects 1, 2, 7, or 12. Aspect 19: The optical member according to aspect 18, wherein the optical member is an imaging lens or a sensing camera lens. Aspect 20: The imaging lens or sensing camera lens according to aspect 19, wherein the thickness of the center portion is 0.05 to 3.0 mm.

[0014] The polycarbonate resin of the present invention has excellent flowability and small orientation birefringence, and therefore can be suitably used for thin optical components such as imaging lenses, and the industrial effects thereof are exceptional.

[0015] Furthermore, a more preferable polycarbonate resin of the present invention has a high Abbe number, and further has a small orientation birefringence and photoelastic coefficient.

[0016] Furthermore, other more preferable polycarbonate resins of the present invention have small orientation birefringence, and high refractive index and glass transition temperature. Thus, the industrial effects of the polycarbonate resins of the present invention are exceptional.

[0017] The present invention will be described in further detail. <Embodiment 1> <Polycarbonate Resin> A polycarbonate resin containing a unit represented by formula (1) and / or formula (2) and a unit represented by formula (3), and having a weight average molecular weight Mw of 10,000 or more and 55,000 or less.

[0018] The polycarbonate resin of the present invention contains units represented by formula (1) and / or formula (2) and units represented by formula (3). The units represented by formula (1) and / or formula (2) are contained in an amount of more than 0 mol% but less than 100 mol% of all repeating units, and the units represented by formula (3) are contained in an amount of more than 0 mol% but less than 100 mol% of all repeating units. The units represented by formula (1) and / or formula (2) are preferably contained in an amount of 10 mol% or more of all repeating units, more preferably 20 mol% or more, and even more preferably 35 mol% or more. Furthermore, the units represented by formula (1) and / or formula (2) are preferably contained in an amount of 90 mol% or less of all repeating units, more preferably 80 mol% or less, and even more preferably 65 mol% or less. Within the above ranges, orientation birefringence is small, and the balance of refractive index, Abbe number, and photoelastic coefficient is excellent. The molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is preferably 99:1 to 1:99, more preferably 80:20 to 20:80, and even more preferably 65:35 to 35:65. When the ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is within the above range, the orientation birefringence is small, and the balance of the refractive index, Abbe number, and photoelastic coefficient is excellent.

[0019] In the definitions of mol % and molar ratios described above, the units represented by formula (1) and / or formula (2) refer to the total units of formula (1) and formula (2) when the polycarbonate resin contains units represented by formula (1) and formula (2), and refer to either one of the units represented by formula (1) or formula (2) when the polycarbonate resin contains either one of the units contained.

[0020]

[0021] (In the formula, R 1 ~R 4each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.) The polycarbonate resin of the present invention has a weight-average molecular weight Mw of 10,000 or more, preferably 15,000 or more, and more preferably 20,000 or more. A weight-average molecular weight Mw of 10,000 or more is preferable because it has sufficient mechanical strength for use as a structural material or optical material. Furthermore, the weight-average molecular weight Mw is 55,000 or less, more preferably 50,000 or less, even more preferably 40,000 or less, particularly preferably less than 35,000, and most preferably 30,000 or less. A weight-average molecular weight Mw of 55,000 or less is preferable because it provides excellent fluidity during injection molding. In particular, the polycarbonate resin of the present invention is preferable because it provides excellent fluidity when used in thin-walled optical components such as imaging lenses. The weight-average molecular weight Mw can be measured by GPC using polystyrene of known molecular weight as a standard sample and chloroform as a developing solvent.

[0022] The polycarbonate resin of the present invention has an absolute value of orientation birefringence of 7.0 × 10 -3 It is preferable that the absolute value of orientation birefringence is not more than the above range, since birefringence due to molecular orientation is less likely to occur. Orientation birefringence is measured at a wavelength of 589 nm after cutting a test piece 70 mm long (45 mm between chucks) and 15 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin and stretching it twice at Tg+10°C.

[0023] The polycarbonate resin of the present invention has a photoelastic coefficient of 35×10 -12 It is preferable that the photoelastic coefficient is less than Pa. When the photoelastic coefficient is in the above range, birefringence due to stress is less likely to occur. The photoelastic coefficient is measured by cutting a test piece 50 mm long and 10 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin using a Spectroellipsometer M-220 manufactured by JASCO Corporation.

[0024] The polycarbonate resin of the present invention preferably has a refractive index nd of 1.540 or more, measured at a temperature of 20°C and a wavelength of 587.56 nm. A refractive index of 1.540 or more is preferred because it allows for the thinning of optical components. The refractive index nd may also be 1.650 or less. A refractive index nd within the above range is preferred because it increases the degree of freedom in optical design when combining and using multiple lenses.

[0025] The polycarbonate resin of the present invention preferably has an Abbe number of 25.0 or more. An Abbe number of 25.0 or more is preferable because chromatic aberration of the optical member is reduced. The Abbe number may be 57.0 or less. An Abbe number within the above range is preferable because it increases the degree of freedom in optical design when multiple lenses are used in combination.

[0026] Here, the Abbe number (νd) is calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0027] νd=(nd−1) / (nF−nC) where nd is the refractive index at a wavelength of 587.56 nm, nF is the refractive index at a wavelength of 486.13 nm, and nC is the refractive index at a wavelength of 656.27 nm.

[0028] The polycarbonate resin of the present invention preferably has a glass transition temperature of 130°C or higher. A glass transition temperature in this range is preferred because the temperature range in which optical components can be used is widened. The glass transition temperature may also be 160°C or lower. A glass transition temperature in this range is preferred because an excellent balance between heat resistance and moldability is achieved.

[0029] The polycarbonate resin of the present invention preferably has a thermal decomposition temperature of 370°C or higher. A thermal decomposition temperature of 370°C or higher is preferable because the polycarbonate resin of the present invention has excellent processing stability when molded and is less likely to be discolored. The thermal decomposition temperature may also be 420°C or lower. The thermal decomposition temperature can be measured by TGA (thermogravimetric analysis) and is the temperature at which the weight decreases by 5%.

[0030] The polycarbonate resin of the present invention preferably has a melt viscosity (Pa s) of 30 or more at 260°C and a shear rate of 1,216 / sec. Furthermore, the melt viscosity (Pa s) at 260°C and a shear rate of 1,216 / sec is preferably 500 or less. A melt viscosity within the above range is preferred because it provides excellent moldability during injection molding. The melt viscosity during molding is particularly important when injection molding thin-walled molded articles such as lenses, and a melt viscosity within the above range is preferred because it allows the desired lens shape to be obtained. The melt viscosity is measured using a Capilograph 1D (manufactured by Toyo Seiki Seisaku-sho, Ltd.) after drying the polycarbonate resin at 120°C for 4 hours.

[0031] The specific viscosity of the polycarbonate resin of the present invention is preferably 0.12 to 0.32. When the specific viscosity is 0.12 to 0.32, an excellent balance between moldability and strength is achieved.

[0032] The specific viscosity is measured by measuring the specific viscosity (ηSP) at 20° C. of a solution prepared by dissolving 0.7 g of polycarbonate resin in 100 ml of methylene chloride using an Ostwald viscometer, and calculating the specific viscosity from the following formula:

[0033] ηSP=(t−t0) / t0 (t0 is the number of seconds it takes for methylene chloride to fall, and t is the number of seconds it takes for the sample solution to fall). 1 ~R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, and an aryl group.

[0034] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, and a t-butyl group, with a methyl group and an ethyl group being preferred.

[0035] Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a bicyclo[1.1.1]pentanyl group.

[0036] Examples of the aryl group include a phenyl group, a tolyl group, a naphthyl group, and a xylyl group, with a phenyl group being preferred.

[0037] R 1 ~R 4 are each independently preferably a hydrogen atom, a methyl group, or a phenyl group, more preferably a hydrogen atom or a phenyl group, and R 1 and R 2 are each independently a hydrogen atom or a phenyl group, and R 3 and R 4 is more preferably a hydrogen atom.

[0038] The repeating units represented by the above formula (1) and / or formula (2) are repeating units derived from pentacyclopentadecanedimethanol, and the repeating units represented by the above formula (1) and / or formula (2) may be pure substances or mixtures of isomers in any ratio. Pentacyclopentadecanedimethanol includes the following structural formulas:

[0039]

[0040]

[0041] The repeating unit represented by the above formula (3) is preferably a repeating unit derived from 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene or 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene, and more preferably a repeating unit derived from 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene.

[0042] The polycarbonate resin of the present invention may contain repeating units other than those represented by the above formulas (1) to (3) as long as the advantageous effects of the present invention are obtained. Examples of dihydroxy compounds that provide such repeating units include ethylene glycol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, tricyclo[5.2.1.0]diol, and the like. 2,6] decanedimethanol, cyclohexane-1,4-dimethanol, decalin-2,6-dimethanol, norbornane dimethanol, cyclopentane-1,3-dimethanol, isosorbide, isomannide, isoidide, hydroquinone, resorcinol, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,3-bis(2-(4-hydroxyphenyl) Examples of such repeating units include 4,4'-(4-hydroxyphenyl)-2-propyl)benzene, 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol, 4,4'-cyclohexylidenebisphenol, 4,4'-(3-methylcyclohexylidene)bisphenol, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfide, biphenol, bisphenolfluorene, biscresolfluorene, 1,1'-bi-2-naphthol, and 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene. Such repeating units may account for 30 mol % or less of all repeating units.

[0043] In the polycarbonate resin of the present invention, the total amount of repeating units represented by the above formulas (1) to (3) is preferably 70 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol % or more, of all repeating units.

[0044] The terminals of the polycarbonate resin of the present invention are composed of hydroxyl groups or phenyl groups, and the proportion of terminal phenyl groups in all terminals is preferably 70 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, and even more preferably 95 mol % or more.

[0045] The polycarbonate resin of the present invention has a total light transmittance of preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more when molded into a 1 mm thick article, which can be obtained by subjecting the polycarbonate resin of the present invention to injection molding, hot press molding, melt extrusion molding, or the like.

[0046] The saturated water absorption of the polycarbonate resin of the present invention may be 0.10% to 0.70%, 0.20% to 0.70%, or 0.30% to 0.65%.

[0047] <Method for producing polycarbonate resin> The polycarbonate resin of the present invention is produced by a reaction means known per se for producing ordinary polycarbonate resins, for example, a method of reacting a dihydroxy compound with a carbonate precursor such as a carbonate diester. Next, the basic means for these production methods will be briefly described.

[0048] The transesterification reaction using a carbonate diester as a carbonate precursor is carried out by stirring a predetermined ratio of dihydroxy component with a carbonate diester under heating in an inert gas atmosphere, and distilling off the resulting alcohol or phenol. The reaction temperature varies depending on the boiling point of the resulting alcohol or phenol, but is usually in the range of 120 to 300°C. The reaction is completed by reducing the pressure from the beginning of the reaction to distill off the resulting alcohol or phenol. If necessary, a terminal capping agent, antioxidant, etc. may also be added.

[0049] Examples of the carbonate diester used in the transesterification reaction include esters of an aryl group or aralkyl group having 6 to 12 carbon atoms, which may be substituted. Specific examples include diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl)carbonate, and m-cresyl carbonate. Of these, diphenyl carbonate is particularly preferred. The amount of diphenyl carbonate used is preferably 0.95 to 1.10 mol, more preferably 0.98 to 1.04 mol, per mol of the total amount of dihydroxy compounds.

[0050] In the melt polymerization method, a polymerization catalyst can be used to increase the polymerization rate. Examples of such a polymerization catalyst include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds.

[0051] As such compounds, organic acid salts, inorganic salts, oxides, hydroxides, hydrides, alkoxides, quaternary ammonium hydroxides, etc. of alkali metals or alkaline earth metals are preferably used, and these compounds can be used alone or in combination.

[0052] Examples of alkali metal compounds include sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenylphosphate, disodium salt, dipotassium salt, dicesium salt, dilithium salt of bisphenol A, sodium salt, potassium salt, cesium salt, and lithium salt of phenol.

[0053] Examples of alkaline earth metal compounds include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium diacetate, calcium diacetate, strontium diacetate, and barium diacetate.

[0054] Examples of the nitrogen-containing compound include quaternary ammonium hydroxides having an alkyl or aryl group, such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and trimethylbenzylammonium hydroxide. Examples include bases or basic salts such as tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, and tetraphenylammonium tetraphenylborate.

[0055] Other transesterification catalysts include salts of zinc, tin, zirconium, lead, titanium, germanium, antimony, and osmium, such as zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin (II) chloride, tin (IV) chloride, tin (II) acetate, tin (IV) acetate, dibutyltin dilaurate, dibutyltin oxide, dibutyltin dimethoxide, zirconium acetylacetonate, zirconium oxyacetate, zirconium tetrabutoxide, lead (II) acetate, lead (IV) acetate, titanium tetrabutoxide (IV), etc. The catalysts used in WO 2011 / 010741 and JP 2017-179323 A may also be used.

[0056] Furthermore, a catalyst comprising aluminum or a compound thereof and a phosphorus compound may be used, and in this case, the amount is preferably 80 μmol to 1000 μmol, more preferably 90 μmol to 800 μmol, and even more preferably 100 μmol to 600 μmol per 1 mol of the dihydroxy component.

[0057] Examples of aluminum salts include organic and inorganic aluminum salts. Examples of organic aluminum salts include aluminum carboxylates, specifically aluminum formate, aluminum acetate, aluminum propionate, aluminum oxalate, aluminum acrylate, aluminum laurate, aluminum stearate, aluminum benzoate, aluminum trichloroacetate, aluminum lactate, aluminum citrate, and aluminum salicylate. Examples of inorganic aluminum salts include aluminum chloride, aluminum hydroxide, aluminum hydroxide chloride, aluminum carbonate, aluminum phosphate, and aluminum phosphonate. Examples of aluminum chelate compounds include aluminum acetylacetonate, aluminum acetylacetate, aluminum ethylacetoacetate, and aluminum ethylacetoacetate diisopropoxide.

[0058] Examples of phosphorus compounds include phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phosphonous acid compounds, phosphinous acid compounds, and phosphine compounds. Among these, phosphonic acid compounds, phosphinic acid compounds, and phosphine oxide compounds are particularly preferred, and phosphonic acid compounds are particularly preferred.

[0059] The amount of these polymerization catalysts used is preferably 0.1 μmol to 500 μmol, more preferably 0.5 μmol to 300 μmol, and even more preferably 1 μmol to 100 μmol, per mol of the dihydroxy component.

[0060] A catalyst deactivator can also be added in the latter stage of the reaction. Known catalyst deactivators are effectively used as the catalyst deactivator, but among these, ammonium salts and phosphonium salts of sulfonic acid are preferred. Salts of dodecylbenzenesulfonic acid, such as tetrabutylphosphonium dodecylbenzenesulfonate, and salts of paratoluenesulfonic acid, such as tetrabutylammonium paratoluenesulfonate, are more preferred.

[0061] Preferred examples of sulfonic acid esters include methyl benzenesulfonate, ethyl benzenesulfonate, butyl benzenesulfonate, octyl benzenesulfonate, phenyl benzenesulfonate, methyl paratoluenesulfonate, ethyl paratoluenesulfonate, butyl paratoluenesulfonate, octyl paratoluenesulfonate, and phenyl paratoluenesulfonate. Of these, tetrabutylphosphonium dodecylbenzenesulfonate is most preferably used.

[0062] When at least one polymerization catalyst selected from alkali metal compounds and / or alkaline earth metal compounds is used, the amount of these catalyst deactivators used is preferably 0.5 to 50 mol, more preferably 0.5 to 10 mol, and even more preferably 0.8 to 5 mol per mol of the catalyst. <Optional Additives> The polycarbonate resin of the present invention can be used as a resin composition by appropriately adding additives such as a mold release agent, a heat stabilizer (sometimes referred to as an antioxidant), an ultraviolet absorber, a bluing agent, an antistatic agent, a flame retardant, a plasticizer, a filler, an antioxidant, a light stabilizer, a polymerization metal deactivator, a lubricant, a surfactant, and an antibacterial agent, as needed. Specific preferred examples of mold release agents and heat stabilizers include those described in International Publication No. 2011 / 010741.

[0063] Particularly preferred release agents include stearic acid monoglyceride, stearic acid triglyceride, pentaerythritol tetrastearate, and a mixture of stearic acid triglyceride and stearyl stearate. The amount of the ester in the release agent is preferably 90% by weight or more, and more preferably 95% by weight or more, based on 100% by weight of the release agent. The content of the release agent is preferably in the range of 0.005 to 2.0 parts by weight, more preferably 0.01 to 0.6 parts by weight, and even more preferably 0.02 to 0.5 parts by weight, relative to 100 parts by weight of the polycarbonate resin.

[0064] Examples of the heat stabilizer include phosphorus-based heat stabilizers, sulfur-based heat stabilizers, and hindered phenol-based heat stabilizers.

[0065] Particularly preferred phosphorus-based heat stabilizers include tris(2,4-di-tert-butylphenyl)phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, distearylpentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, cyclic neopentanetetraylbis(2,6-di-tert-butyl-4-methylphenyl phosphite), and bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite. The content of the phosphorus-based heat stabilizer is preferably 0.001 to 0.2 parts by weight per 100 parts by weight of the polycarbonate resin.

[0066] A particularly preferred sulfur-based heat stabilizer is pentaerythritol-tetrakis(3-laurylthiopropionate). The content of the sulfur-based heat stabilizer is preferably 0.001 to 0.2 parts by weight per 100 parts by weight of the polycarbonate resin.

[0067] Preferred hindered phenol-based heat stabilizers include octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-trimethyl-2,4,6-tris(3 ,5-di-tert-butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane.

[0068] The content of the hindered phenol-based heat stabilizer is preferably 0.001 to 0.3 parts by weight per 100 parts by weight of the polycarbonate resin.

[0069] The phosphorus-based heat stabilizer and the hindered phenol-based heat stabilizer can also be used in combination.

[0070] The ultraviolet absorber is preferably at least one ultraviolet absorber selected from the group consisting of benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, triazine-based ultraviolet absorbers, cyclic iminoester-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers.

[0071] Of the benzotriazole-based ultraviolet absorbers, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] are more preferred.

[0072] Benzophenone-based ultraviolet absorbers include 2-hydroxy-4-n-dodecyloxybenzophenone and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0073] Examples of triazine-based ultraviolet absorbers include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-[(octyl)oxy]-phenol.

[0074] As the cyclic iminoester-based ultraviolet absorber, 2,2'-p-phenylenebis(3,1-benzoxazin-4-one) is particularly suitable.

[0075] Examples of cyanoacrylate ultraviolet absorbers include 1,3-bis-[(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0076] The blending amount of the ultraviolet absorber is preferably 0.01 to 3.0 parts by weight per 100 parts by weight of the polycarbonate resin, and within this blending amount range, it is possible to impart sufficient weather resistance to molded articles of the polycarbonate resin depending on the application.

[0077] <Optical Member> The optical member of the present invention contains the above-mentioned polycarbonate resin. Such optical members are not particularly limited as long as they are used for optical applications in which the above-mentioned polycarbonate resin is useful, and examples thereof include optical disks, transparent conductive substrates, optical cards, sheets, films, optical fibers, lenses, prisms, optical films, substrates, optical filters, and hard coat films.

[0078] The optical member of the present invention may be composed of a resin composition containing the above-mentioned polycarbonate resin, and the resin composition may contain additives such as heat stabilizers, plasticizers, light stabilizers, polymerized metal deactivators, flame retardants, lubricants, antistatic agents, surfactants, antibacterial agents, UV absorbers, mold release agents, bluing agents, fillers, and antioxidants, as necessary. <Optical Lenses> The optical member of the present invention may particularly include optical lenses. Examples of such optical lenses include imaging lenses for mobile phones, smartphones, tablet devices, personal computers, digital cameras, video cameras, vehicle-mounted cameras, surveillance cameras, etc., and sensing camera lenses such as TOF cameras.

[0079] When the optical lens of the present invention is produced by injection molding, molding is preferably carried out under conditions of a cylinder temperature of 220 to 350°C and a mold temperature of 70 to 180°C. Molding is more preferably carried out under conditions of a cylinder temperature of 240 to 300°C and a mold temperature of 80 to 170°C. If the cylinder temperature is higher than 350°C, the polycarbonate resin will decompose and discolor, and if it is lower than 230°C, the melt viscosity will be high, making molding difficult. Furthermore, if the mold temperature is higher than 180°C, it will be difficult to remove a molded piece made of polycarbonate resin from the mold. On the other hand, if the mold temperature is lower than 70°C, the resin will harden too quickly in the mold during molding, making it difficult to control the shape of the molded piece and making it difficult to sufficiently transfer the shape imprinted on the mold.

[0080] The optical lens of the present invention is preferably implemented as an aspherical lens, if necessary. Since a single aspherical lens can substantially eliminate spherical aberration, it is not necessary to eliminate spherical aberration by combining multiple spherical lenses, which allows for weight reduction and reduced molding costs. Therefore, aspherical lenses are particularly useful as camera lenses, among other optical lenses.

[0081] Furthermore, because the polycarbonate resin of the present invention has high molding fluidity, it is useful as a material for thin, small, and complex-shaped optical lenses, and is particularly useful for imaging lenses and sensing camera lenses. Specific lens sizes include a central thickness of 0.05 to 3.0 mm, more preferably 0.05 to 2.0 mm, even more preferably 0.1 to 2.0 mm, and particularly preferably 0.1 to 1.0 mm. Furthermore, the diameter is 1.0 mm to 20.0 mm, more preferably 1.0 to 10.0 mm, and even more preferably 3.0 to 10.0 mm. Furthermore, the shape is preferably a meniscus lens, with one convex surface and one concave surface.

[0082] Lenses made from the polycarbonate resin of the present invention can be formed by any method, such as mold molding, cutting, polishing, laser processing, electrical discharge machining, or etching. Among these, mold molding is more preferred in terms of production costs. <Embodiment 2> Regarding the polycarbonate resin of the present invention, the details described in Embodiment 1 above also apply to Embodiment 2, unless otherwise specified below. <Polycarbonate Resin> The polycarbonate resin of the present invention contains units represented by formula (1) and / or formula (2) and units represented by formula (3), and preferably contains 50 mol% or more of the units represented by formula (1) and / or formula (2) in all repeating units. The units represented by formula (1) and / or formula (2) are preferably contained in 90 mol% or less, more preferably 80 mol% or less, and even more preferably 65 mol% or less of the units represented by formula (1) and / or formula (2) in all repeating units. Furthermore, the units represented by formula (3) are preferably contained in more than 0% but not more than 50 mol% in all repeating units. It is more preferable that the unit represented by formula (3) is contained in 10 mol% or more of all repeating units, even more preferably 20 mol% or more, and particularly preferably 35 mol% or more. This range is preferable because it results in a high Abbe number and excellent orientation birefringence and photoelastic coefficient. Furthermore, the molar ratio of the unit represented by formula (1) and / or formula (2) to the unit represented by formula (3) is preferably 99:1 to 50:50, more preferably 95:5 to 50:50, even more preferably 90:10 to 50:50, even more preferably 85:15 to 50:50, particularly preferably 80:20 to 50:50, and most preferably 65:35 to 50:50. When the ratio of the unit represented by formula (1) and / or formula (2) to the unit represented by formula (3) is within the above range, it is preferable because it results in a high Abbe number and excellent orientation birefringence and photoelastic coefficient.

[0083]

[0084] (In the formula, R 1 ~R 4each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.) The polycarbonate resin of the present invention has a weight-average molecular weight Mw of 10,000 or more, preferably 15,000 or more, and more preferably 20,000 or more. A weight-average molecular weight Mw of 10,000 or more is preferable because it has sufficient mechanical strength for use as a structural material or optical material. Furthermore, the weight-average molecular weight Mw is 55,000 or less, more preferably 50,000 or less, even more preferably 40,000 or less, particularly preferably less than 35,000, and most preferably 30,000 or less. A weight-average molecular weight Mw of 50,000 or less is preferable because it provides excellent fluidity during injection molding. This is particularly preferable because it provides excellent fluidity when the polycarbonate resin of the present invention is used for thin-walled optical components such as imaging lenses. The weight-average molecular weight Mw can be measured by GPC using polystyrene of known molecular weight as a standard sample and chloroform as a developing solvent.

[0085] The polycarbonate resin of the present invention has an absolute value of orientation birefringence of 7.0 × 10 -3 It is preferable that the value is 5.0 × 10 or less. -3 More preferably, it is 3.0 × 10 or less. -3 It is more preferable that the value is equal to or less than 2.5×10 -3 More preferably, it is 2.0 × 10 or less. -3 It is particularly preferable that the value is 1.5×10 or less. -3 It is most preferable that the absolute value of orientation birefringence is not more than the above range, since it is less likely that birefringence due to molecular orientation will occur. Orientation birefringence is measured at a wavelength of 589 nm after cutting a test piece 70 mm long (45 mm between chucks) and 15 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin and stretching it twice at Tg+10°C.

[0086] The polycarbonate resin of the present invention has a photoelastic coefficient of 25×10 -12 Pa, and preferably less than 20 × 10 -12It is more preferable that the photoelastic coefficient is in the above range because birefringence due to stress is unlikely to occur. The photoelastic coefficient is measured by cutting a test piece 50 mm long and 10 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin using a Spectroellipsometer M-220 manufactured by JASCO Corporation.

[0087] The polycarbonate resin of the present invention preferably has a refractive index nd measured at a temperature of 20°C and a wavelength of 587.56 nm of 1.540 or more, more preferably 1.550 or more, even more preferably 1.560 or more, even more preferably 1.570 or more, and particularly preferably 1.575 or more. A refractive index of at least the above range is preferred because it allows optical components to be made thinner. Furthermore, the refractive index nd may be 1.610 or less, 1.600 or less, 1.590 or less, or 1.580 or less. A refractive index nd within the above range is preferred because it increases the degree of freedom in optical design when combining and using multiple lenses.

[0088] The polycarbonate resin of the present invention preferably has an Abbe number of 25.0 or more, more preferably 28.0 or more, even more preferably 31.0 or more, even more preferably 34.0 or more, and particularly preferably 36.0 or more. An Abbe number of 25.0 or more is preferable because it reduces chromatic aberration of optical components. The Abbe number may also be 57.0 or less, 55.0 or less, 50.0 or less, or 45.0 or less. An Abbe number within the above range is preferable because it increases the degree of freedom in optical design when combining and using multiple lenses.

[0089] Here, the Abbe number (νd) is calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0090] νd=(nd−1) / (nF−nC) where nd is the refractive index at a wavelength of 587.56 nm, nF is the refractive index at a wavelength of 486.13 nm, and nC is the refractive index at a wavelength of 656.27 nm.

[0091] The polycarbonate resin of the present invention preferably has a glass transition temperature of 130°C or higher, more preferably 133°C or higher, and even more preferably 136°C or higher. A glass transition temperature within the above range is preferred because it broadens the temperature range in which optical components can be used. Furthermore, the glass transition temperature may be 155°C or lower, 150°C or lower, 145°C or lower, or 140°C or lower. A glass transition temperature within the above range is preferred because it provides an excellent balance between heat resistance and moldability.

[0092] The polycarbonate resin of the present invention preferably has a thermal decomposition temperature of 370°C or higher, more preferably 375°C or higher. A thermal decomposition temperature of 370°C or higher is preferable because the polycarbonate resin of the present invention exhibits excellent processing stability during molding and exhibits little discoloration. The thermal decomposition temperature may be 420°C or lower, or may be 400°C or lower. The thermal decomposition temperature can be measured by TGA (thermogravimetric analysis) and is the temperature at which the weight decreases by 5%. The polycarbonate resin of the present invention preferably has a melt viscosity (Pa s) of 30 or higher, more preferably 50 or higher, and even more preferably 70 or higher, at 260°C and a shear rate of 1,216 / sec. The melt viscosity (Pa s) at 260°C and a shear rate of 1,216 / sec is preferably 500 or lower, more preferably 400 or lower, even more preferably 300 or lower, and particularly preferably 200 or lower. A melt viscosity within the above range is preferable because the resin exhibits excellent moldability during injection molding. The melt viscosity during molding is particularly important when injection molding thin-walled molded articles such as lenses, and a melt viscosity within the above range is preferred because it allows the desired lens shape to be obtained. The melt viscosity is measured using a Capilograph 1D manufactured by Toyo Seiki Seisakusho, Ltd., after drying the polycarbonate resin at 120°C for 4 hours.

[0093] The specific viscosity of the polycarbonate resin of the present invention is preferably 0.12 to 0.32, and more preferably 0.18 to 0.30. When the specific viscosity is 0.12 to 0.32, an excellent balance between moldability and strength is achieved.

[0094] The specific viscosity is measured by measuring the specific viscosity (ηSP) at 20° C. of a solution prepared by dissolving 0.7 g of polycarbonate resin in 100 ml of methylene chloride using an Ostwald viscometer, and calculating the specific viscosity from the following formula:

[0095] ηSP=(t−t0) / t0 (t0 is the number of seconds it takes for methylene chloride to fall, and t is the number of seconds it takes for the sample solution to fall). Third Embodiment With regard to the polycarbonate resin of the present invention, the matters described in the first embodiment above are also applicable to the third embodiment unless otherwise specified below.

[0096] <Polycarbonate Resin> The polycarbonate resin of the present invention contains units represented by formula (1) and / or formula (2) and units represented by formula (3), and preferably contains more than 0% and less than 50 mol% of the units represented by formula (1) and / or formula (2) in all repeating units. The units represented by formula (1) and / or formula (2) are preferably contained in 10 mol% or more of all repeating units, more preferably 20 mol% or more, and even more preferably 35 mol% or more and less than 50 mol%. Furthermore, the units represented by formula (3) are preferably contained in more than 50 mol% of all repeating units. The units represented by formula (3) are preferably contained in 90 mol% or less of all repeating units, more preferably 80 mol% or less, and even more preferably 65 mol% or less. The above ranges are preferred because they result in low orientation birefringence and high refractive index and glass transition temperature. Furthermore, the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is preferably 1:99 to 49:51, more preferably 5:95 to 49:51, even more preferably 10:90 to 49:51, still more preferably 15:85 to 49:51, particularly preferably 20:80 to 49:51, and most preferably 35:65 to 49:51. When the ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is within the above range, orientation birefringence is small and the refractive index and glass transition temperature are high, which is preferable.

[0097]

[0098] (In the formula, R 1 ~R 4each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.) The polycarbonate resin of the present invention has a weight-average molecular weight Mw of 10,000 or more, preferably 15,000 or more, and more preferably 20,000 or more. A weight-average molecular weight Mw of 10,000 or more is preferable because it has sufficient mechanical strength for use as a structural material or optical material. Furthermore, the weight-average molecular weight Mw is 55,000 or less, more preferably 50,000 or less, even more preferably 40,000 or less, particularly preferably less than 35,000, and most preferably 30,000 or less. A weight-average molecular weight Mw of 50,000 or less is preferable because it provides excellent fluidity during injection molding. This is particularly preferable because it provides excellent fluidity when the polycarbonate resin of the present invention is used for thin-walled optical components such as imaging lenses. The weight-average molecular weight Mw can be measured by GPC using polystyrene of known molecular weight as a standard sample and chloroform as a developing solvent.

[0099] The polycarbonate resin of the present invention has an absolute value of orientation birefringence of 3.0 × 10 -3 It is preferable that the value is 2.0 × 10 or less. -3 More preferably, it is 1.0 × 10 or less. -3 It is more preferable that the value is 0.5×10 or less. -3 It is more preferable that the absolute value of orientation birefringence is not more than the above range, since it is less likely that birefringence due to molecular orientation will occur. Orientation birefringence is measured at a wavelength of 589 nm after cutting a test piece 70 mm long (45 mm between chucks) and 15 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin and stretching it twice at Tg+10°C.

[0100] The polycarbonate resin of the present invention has a photoelastic coefficient of 35×10 -12 Pa, and preferably less than 30 × 10 -12 Pa or less is more preferable, and 25×10 -12It is even more preferable that the photoelastic coefficient is not more than 100 Pa. When the photoelastic coefficient is in the above range, birefringence due to stress is less likely to occur, which is preferable. The photoelastic coefficient is measured by cutting a test piece 50 mm long and 10 mm wide from a 100 μm thick cast film obtained from a polycarbonate resin using a Spectroellipsometer M-220 manufactured by JASCO Corporation.

[0101] The polycarbonate resin of the present invention preferably has a refractive index nd measured at a temperature of 20°C and a wavelength of 587.56 nm of 1.600 or more, more preferably 1.605 or more, even more preferably 1.610 or more, even more preferably 1.615 or more, and particularly preferably 1.620 or more. A refractive index of at least the above range is preferred because it allows optical components to be made thinner. Furthermore, the refractive index nd may be 1.650 or less, 1.645 or less, 1.640 or less, or 1.635 or less. A refractive index nd within the above range is preferred because it increases the degree of freedom in optical design when combining and using multiple lenses.

[0102] The polycarbonate resin of the present invention preferably has an Abbe number of 25.0 or more, more preferably 30.0 or more. An Abbe number of 25.0 or more is preferable because chromatic aberration of the optical member is reduced. The Abbe number may be 33.0 or less, or 32.0 or less. An Abbe number within the above range is preferable because it increases the degree of freedom in optical design when multiple lenses are used in combination.

[0103] Here, the Abbe number (νd) is calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0104] νd=(nd−1) / (nF−nC) where nd is the refractive index at a wavelength of 587.56 nm, nF is the refractive index at a wavelength of 486.13 nm, and nC is the refractive index at a wavelength of 656.27 nm.

[0105] The polycarbonate resin of the present invention preferably has a glass transition temperature of 138°C or higher, more preferably 140°C or higher, even more preferably 142°C or higher, and even more preferably 144°C or higher. A glass transition temperature in the above range is preferred because it broadens the temperature range in which optical components can be used. The glass transition temperature may also be 160°C or lower, 155°C or lower, or 150°C or lower. A glass transition temperature in the above range is preferred because it provides an excellent balance between heat resistance and moldability.

[0106] The polycarbonate resin of the present invention preferably has a thermal decomposition temperature of 370°C or higher, more preferably 375°C or higher, and even more preferably 380°C or higher. A thermal decomposition temperature of 370°C or higher is preferable because the polycarbonate resin of the present invention has excellent processing stability when molded and is less likely to be discolored. The thermal decomposition temperature may be 420°C or lower, or may be 400°C or lower. The thermal decomposition temperature can be measured by TGA (thermogravimetric analysis) and is the temperature at which the weight decreases by 5%.

[0107] The polycarbonate resin of the present invention preferably has a melt viscosity (Pa s) of 30 or more, more preferably 50 or more, and even more preferably 70 or more, at 260°C and a shear rate of 1,216 / sec. The melt viscosity (Pa s) at 260°C and a shear rate of 1,216 / sec is preferably 500 or less, more preferably 400 or less, even more preferably 300 or less, and particularly preferably 200 or less. A melt viscosity within the above range is preferred because it provides excellent moldability during injection molding. In particular, when injection molding thin-walled molded products such as lenses, the melt viscosity during molding is important, and a melt viscosity within the above range is preferred because it allows the desired lens shape to be obtained. The melt viscosity is measured using a Capilograph 1D manufactured by Toyo Seiki Seisaku-sho, Ltd., after drying the polycarbonate resin at 120°C for 4 hours.

[0108] The specific viscosity of the polycarbonate resin of the present invention is preferably 0.12 to 0.32, and more preferably 0.18 to 0.30. When the specific viscosity is 0.12 to 0.32, an excellent balance between moldability and strength is achieved.

[0109] The specific viscosity is measured by measuring the specific viscosity (ηSP) at 20° C. of a solution prepared by dissolving 0.7 g of polycarbonate resin in 100 ml of methylene chloride using an Ostwald viscometer, and calculating the specific viscosity from the following formula:

[0110] ηSP=(t−t0) / t0 (t0: number of seconds it takes for methylene chloride to fall, t: number of seconds it takes for the sample solution to fall) The present invention will be described in more detail in the following examples, but the present invention is not limited thereto.

[0111] The evaluation was carried out by the following method. <Copolymerization ratio of polycarbonate resin> JNM-ECZ400S manufactured by JEOL 1 The copolymerization ratio of each polycarbonate resin was calculated by measuring 1 H NMR. <Weight average molecular weight (Mw) The weight average molecular weight Mw was measured using EcoSEC HLC-8320GPC manufactured by TOSOH under the conditions described below.

[0112] Detector: UV-8420, Solvent: Chloroform, Column: TSKgel SupermultiporeHZM-M × 3 + TSKgel guard column (4.6 × 200 nm) manufactured by TOSOH, Measurement temperature: 40°C, Flow rate: 0.35 ml / min, Injection amount: 5 μl, Sample concentration: 1 mg / 5 ml, Standard sample: TSKstandard Polystyrene <Refractive Index> A 3 mm thick test piece of each polycarbonate resin was prepared and polished, and then the refractive index nd (587.56 nm) was measured using a Kalnew Precision Refractometer KPR-2000 manufactured by Shimadzu Corporation. <Abbe Number> The Abbe number (νd) was calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0113] νd = (nd-1) / (nF-nC) nd: refractive index at a wavelength of 587.56 nm, nF: refractive index at a wavelength of 486.13 nm, nC: refractive index at a wavelength of 656.27 nm. <Absolute Value of Orientation Birefringence (|Δn|)> Polycarbonate resin was dissolved in methylene chloride, then cast onto a glass Petri dish and thoroughly dried to produce a cast film with a thickness of 100 μm. A test piece with a length of 70 mm (45 mm between chucks) and a width of 15 mm was cut out from the film and stretched twice at Tg + 10 ° C. The phase difference (Re) at 589 nm was measured using an Ellipsometer M-220 manufactured by JASCO Corporation, and the absolute value of orientation birefringence (|Δn|) was calculated using the following formula.

[0114] |Δn|=|Re / d| Δn: orientation birefringence Re: phase difference (nm) d: thickness (nm) <Photoelastic coefficient> Polycarbonate resin was dissolved in methylene chloride, then cast onto a glass petri dish and thoroughly dried to produce a cast film with a thickness of 100 μm. Test pieces 50 mm long and 10 mm wide were cut out from the film, and the photoelastic coefficient was measured using an Ellipsometer M-220 manufactured by JASCO Corporation. <Glass transition temperature (Tg)> The obtained polycarbonate resin was measured using a Discovery DSC 25Auto model manufactured by TA Instruments Japan Co., Ltd. at a heating rate of 20°C / min. 5 to 10 mg of sample was used for the measurement. <Thermal decomposition temperature (Td-5)> The obtained polycarbonate resin was measured at a heating rate of 20°C / min using an SDT650 manufactured by TA Instruments Japan Co., Ltd., and the temperature at which the weight decreased by 5% was determined based on the weight at 50°C. The sample was 3 to 4 mg for measurement. <Melt viscosity (Pa s)> The polycarbonate resin was dried at 120°C for 4 hours, and then the melt viscosity was measured at 260°C and a shear rate of 1,216 / sec using a Capilograph 1D manufactured by Toyo Seiki Co., Ltd. Example 1 87.70 g (0.20 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as BPEF), 52.48 g (0.20 mol) of pentacyclopentadecanedimethanol (hereinafter sometimes abbreviated as PCPDM), 89.12 g (0.42 mol) of diphenyl carbonate, and 17 μL of a 60 mmol / L aqueous solution of sodium bicarbonate (sodium bicarbonate 2.5 μmol) and 227 μL of a 274 mmol / L aqueous solution of tetramethylammonium hydroxide (tetramethylammonium hydroxide 15 μmol) were heated to 180° C. under a nitrogen atmosphere and melted. Thereafter, the pressure inside the reactor was reduced to 20 kPa over 40 minutes, while the temperature was raised to 250° C. at a rate of 60° C. / hr. After 70% of the theoretical amount of phenol was distilled off, the pressure inside the reactor was reduced to 133 Pa or less over 1 hour. Thereafter, the reaction was terminated by stirring at 260° C. for 40 minutes while the pressure inside the reactor was kept at 133 Pa or less, and the resin was taken out.The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the resulting polycarbonate resin were evaluated. The resulting resin was then dried at 120°C for 4 hours, and 0.05% by mass of bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite and 0.10% by mass of glycerin monostearate were added based on the mass of the resin. The mixture was pelletized using a vented φ15 mm twin-screw extruder. The pellets were dried at 120°C for 4 hours, and then injection molded to obtain lenses with a thickness of 0.3 mm, a convex radius of curvature of 5 mm, a concave radius of curvature of 4 mm, and a φ5 mm diameter, at a cylinder temperature of 260°C and a mold temperature of Tg-5°C of the polycarbonate resin. Example 2 A polycarbonate resin was produced in the same manner as in Example 1, except that the amount of BPEF charged was 52.62 g (0.12 mol) and the amount of PCPDM charged was 73.47 g (0.28 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Lenses having a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm were then obtained by injection molding in the same manner as in Example 1. Example 3 A polycarbonate resin was produced in the same manner as in Example 1, except that the amount of BPEF charged was 43.85 g (0.10 mol) and the amount of PCPDM charged was 78.72 g (0.30 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the resulting polycarbonate resin were evaluated. Subsequently, lenses having a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm were obtained by injection molding in the same manner as in Example 1.Example 4 A polycarbonate resin was produced in the same manner as in Example 1, except that the amount of BPEF charged was 8.78 g (0.02 mol) and the amount of PCPDM charged was 99.71 g (0.38 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Thereafter, a lens having a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm was obtained by injection molding in the same manner as in Example 1. Comparative Example 1: 45.66 g (0.20 mol) of bisphenol A (hereinafter sometimes abbreviated as BPA), 52.48 g (0.20 mol) of PCPDM, 86.97 g (0.406 mol) of diphenyl carbonate, and 1.09 mg (12 μmol) of sodium bicarbonate as a catalyst were heated to 180 ° C. under a nitrogen atmosphere and melted. Thereafter, the reactor internal pressure was set to 20 kPa (150 mmHg), and the temperature was raised to 200 ° C. at a rate of 60 ° C. / hr, and the reaction was carried out while maintaining that temperature for 40 minutes. The temperature was then further raised to 225 ° C. at a rate of 75 ° C. / hr, and 40 minutes after the temperature increase was completed, the reactor internal pressure was reduced to 133 Pa (1 mmHg) or less over 1 hour while maintaining that temperature. The temperature was then raised to 235°C at a rate of 105°C / hr, and the reaction was carried out under stirring for a total of 6 hours. After the reaction was completed, nitrogen was blown into the reactor to return to normal pressure, and the resulting resin was removed. The copolymerization ratio of BPA and PCPDM in the resulting polycarbonate resin was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Subsequently, injection molding of a lens with a thickness of 0.3 mm, a convex radius of curvature of 5 mm, a concave radius of curvature of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 2> A polycarbonate resin was produced in the same manner as in Comparative Example 1, except that the amount of BPA charged was 63.92 g (0.28 mol) and the amount of PCPDM charged was 31.49 g (0.12 mol).The copolymerization ratio of BPA and PCPDM in the obtained polycarbonate resin was measured by 1H NMR. The weight average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Subsequently, injection molding of a lens with a thickness of 0.3 mm, a convex curvature radius of 5 mm, a concave curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 3> A polycarbonate resin was produced in the same manner as in Comparative Example 1, except that the amount of BPA charged was 27.40 g (0.12 mol) and the amount of PCPDM charged was 73.47 g (0.28 mol). The copolymerization ratio of BPA and PCPDM in the obtained polycarbonate resin was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Subsequently, injection molding of a lens with a thickness of 0.3 mm, a convex curvature radius of 5 mm, a concave curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 4> 87.70 g (0.20 mol) of BPEF, 52.48 g (0.20 mol) of PCPDM, 87.40 g (0.41 mol) of diphenyl carbonate, and 17 μL of a 60 mmol / L aqueous sodium bicarbonate solution (2.5 μmol of sodium bicarbonate) and 227 μL of a 274 mmol / L aqueous tetramethylammonium hydroxide solution (15 μmol of tetramethylammonium hydroxide) were heated to 180° C. under a nitrogen atmosphere and melted. The reactor internal pressure was then reduced to 20 kPa over 40 minutes, while the temperature was raised to 250°C at a rate of 60°C / hr. After 70% of the theoretical amount of phenol had been distilled off, the reactor internal pressure was reduced to 133 Pa or less over 1 hour. The reaction was then terminated by stirring at 260°C for 40 minutes at a reactor internal pressure of 133 Pa or less, and the resin was removed. The copolymerization ratio of BPEF and PCPDM in the resulting polycarbonate resin was measured by 1H NMR.The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Subsequently, injection molding of a lens with a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 5> A polycarbonate resin was produced in the same manner as in Comparative Example 4, except that the amount of BPEF charged was 70.16 g (0.16 mol) and the amount of PCPDM charged was 62.97 g (0.24 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Subsequently, injection molding of a lens with a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 6> A polycarbonate resin was produced in the same manner as in Comparative Example 4, except that the amount of BPEF charged was 52.62 g (0.12 mol) and the amount of PCPDM charged was 73.47 g (0.28 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Thereafter, an attempt was made to injection mold a lens having a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm, using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape.

[0115]

[0116] Compared to the comparative examples, Examples 1 to 4 of the present invention have lower melt viscosities and therefore superior moldability during injection molding. Furthermore, because they have excellent orientation birefringence, birefringence due to molecular orientation is unlikely to occur when obtaining optical components by injection molding or the like. Furthermore, because the photoelastic coefficient is small, birefringence due to stress is unlikely to occur when obtaining optical components by injection molding or the like. Therefore, these are preferred because they reduce the birefringence of the optical components. Example 5 166.64 g (0.38 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as BPEF), 5.25 g (0.02 mol) of pentacyclopentadecanedimethanol (hereinafter sometimes abbreviated as PCPDM), 89.12 g (0.42 mol) of diphenyl carbonate, and 17 μL of a 60 mmol / L aqueous sodium bicarbonate solution (sodium bicarbonate 2.5 μmol) and 227 μL of a 274 mmol / L aqueous tetramethylammonium hydroxide solution (tetramethylammonium hydroxide 15 μmol) were heated to 180° C. under a nitrogen atmosphere and melted. Thereafter, the pressure inside the reactor was reduced to 20 kPa over 40 minutes, while the temperature was raised to 250° C. at a rate of 60° C. / hr. After 70% of the theoretical amount of phenol was distilled out, the reactor internal pressure was reduced to 133 Pa or less over 1 hour. The reaction was then terminated by stirring at 260°C for 40 minutes at a reactor internal pressure of 133 Pa or less, and the resin was removed. The copolymerization ratio of BPEF and PCPDM in the resulting polycarbonate resin was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Lenses with a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm were then obtained by injection molding in the same manner as in Example 1. Example 6 A polycarbonate resin was produced in the same manner as in Example 1, except that the amount of BPEF charged was 131.56 g (0.30 mol) and the amount of PCPDM charged was 26.24 g (0.10 mol). The copolymerization ratio of BPEF and PCPDM in the obtained polycarbonate resin was measured by 1H NMR.The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Lenses with a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm were then obtained by injection molding in the same manner as in Example 1. Example 7 A polycarbonate resin was produced in the same manner as in Example 1, except that the amount of BPEF charged was 96.47 g (0.22 mol) and the amount of PCPDM charged was 47.23 g (0.18 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Thereafter, lenses having a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm were obtained by injection molding in the same manner as in Example 1. <Comparative Example 7> 45.66 g (0.20 mol) of bisphenol A (hereinafter sometimes abbreviated as BPA), 52.48 g (0.20 mol) of PCPDM, 86.97 g (0.406 mol) of diphenyl carbonate, and 1.09 mg (12 μmol) of sodium bicarbonate as a catalyst were heated to 180°C under a nitrogen atmosphere and melted. Thereafter, the internal pressure of the reactor was increased to 20 kPa (150 mmHg), and the temperature was raised to 200°C at a rate of 60°C / hr, and the reaction was carried out by maintaining that temperature for 40 minutes. The temperature was then increased to 225°C at a rate of 75°C / hr. After 40 minutes, the temperature was maintained and the reactor pressure was reduced to 133 Pa (1 mmHg) or less over 1 hour. The temperature was then increased to 235°C at a rate of 105°C / hr, and the reaction was continued for a total of 6 hours with stirring. After the reaction was completed, nitrogen was blown into the reactor to return the pressure to normal, and the resulting resin was removed. The copolymerization ratio of BPA and PCPDM in the resulting polycarbonate resin was measured by 1H NMR. The weight-average molecular weight (Mw), refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientational birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated.Thereafter, injection molding of a lens with a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 8> A polycarbonate resin was produced in the same manner as in Comparative Example 1, except that the amount of BPA charged was 63.92 g (0.28 mol) and the amount of PCPDM charged was 31.49 g (0.12 mol). The copolymerization ratio of BPA and PCPDM in the resulting polycarbonate resin was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Thereafter, injection molding of a lens with a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 9> A polycarbonate resin was produced in the same manner as in Comparative Example 1, except that the amount of BPA charged was 27.40 g (0.12 mol) and the amount of PCPDM charged was 73.47 g (0.28 mol). The copolymerization ratio of BPA and PCPDM in the resulting polycarbonate resin was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated. Thereafter, injection molding of a lens with a thickness of 0.3 mm, a convex surface curvature radius of 5 mm, a concave surface curvature radius of 4 mm, and a diameter of 5 mm was attempted using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape. <Comparative Example 10> A polycarbonate resin was produced in the same manner as in Comparative Example 4, except that the amount of BPEF charged was 122.79 g (0.28 mol) and the amount of PCPDM charged was 31.49 g (0.12 mol). The copolymerization ratio of the resulting polycarbonate resin derived from BPEF and PCPDM was measured by 1H NMR. The weight-average molecular weight Mw, refractive index, Abbe number, glass transition temperature, thermal decomposition temperature, absolute value of orientation birefringence, photoelastic coefficient, and melt viscosity of the polycarbonate resin were evaluated.Thereafter, an attempt was made to injection mold a lens having a thickness of 0.3 mm, a convex surface radius of curvature of 5 mm, a concave surface radius of curvature of 4 mm, and a diameter of 5 mm, using the same method as in Example 1, but due to the high melt viscosity of the resin, it was not possible to mold a thin lens of that shape.

[0117]

[0118] The melt viscosity of Examples 5 to 7 of the present invention is lower than that of the comparative examples, and therefore the moldability during injection molding is excellent. Furthermore, because the orientation birefringence is excellent, birefringence due to molecular orientation is unlikely to occur when obtaining optical components by injection molding or the like. Furthermore, the refractive index and glass transition temperature are high, making them suitable for optical components.

[0119] The polycarbonate resin of the present invention is used in optical materials, and can be used for optical members such as lenses, prisms, optical disks, transparent conductive substrates, optical cards, sheets, films, optical fibers, optical films, optical filters, and hard coat films. It is particularly useful for imaging lenses or sensing camera lenses, and is extremely useful for imaging lenses.

Claims

1. A polycarbonate resin containing a unit represented by formula (1) and / or formula (2) and a unit represented by formula (3) and having a weight average molecular weight Mw of 10,000 to 55,000. (In the formula, R 1 ~R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.

2. R in the above formula (3) 1 ~R 4 The polycarbonate resin according to claim 1, wherein is a hydrogen atom.

3. The polycarbonate resin according to claim 1 or 2, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is 99:1 to 1:

99.

4. The polycarbonate resin according to claim 3, wherein the molar ratio of the units represented by the formula (1) and / or the formula (2) to the units represented by the formula (3) is 65:35 to 35:

65.

5. The absolute value of orientation birefringence is 7.0 x 10 -3 3. The polycarbonate resin according to claim 1 or 2, wherein:

6. Photoelastic coefficient is 35 x 10 -12 The polycarbonate resin according to claim 1 or 2, having a modulus of less than Pa.

7. The polycarbonate resin according to claim 1, which contains units represented by formula (1) and / or formula (2) in an amount of 50 mol % or more in all repeating units and has a weight average molecular weight Mw of 10,000 to 50,000.

8. The polycarbonate resin according to claim 7, which contains more than 0% and not more than 50 mol % of the unit represented by formula (3) in all repeating units.

9. The polycarbonate resin according to claim 7 or 8, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is from 99:1 to 50:

50.

10. The photoelastic coefficient is 25 x 10 -12 The polycarbonate resin according to claim 7 or 8, having a modulus of less than Pa.

11. The polycarbonate resin according to claim 7 or 8, which has an Abbe number of 25.0 or more.

12. A polycarbonate resin according to claim 1, which contains more than 0% and less than 50 mol % of units represented by formula (1) and / or formula (2) in all repeating units and has a weight average molecular weight Mw of 10,000 to 50,000.

13. The polycarbonate resin according to claim 12, wherein the unit represented by formula (3) is contained in more than 50 mol % of all repeating units.

14. The polycarbonate resin according to claim 12 or 13, wherein the molar ratio of the units represented by formula (1) and / or formula (2) to the units represented by formula (3) is from 1:99 to 49:

51.

15. The absolute value of orientation birefringence is 3.0 x 10 -3 The polycarbonate resin according to claim 12 or 13, wherein:

16. The polycarbonate resin according to claim 12 or 13, which has a refractive index nd of 1.600 or more.

17. The polycarbonate resin according to claim 12 or 13, which has a glass transition temperature of 140°C or higher.

18. An optical member made of the polycarbonate resin according to any one of claims 1, 2, 7 and 12.

19. The optical member according to claim 18, wherein the optical member is an imaging lens or a sensing camera lens.

20. The imaging lens or sensing camera lens according to claim 19, wherein the thickness at the center is 0.05 to 3.0 mm.

Citation Information

Patent Citations

  • Imaging lens

    WO2017010318A1

  • Polycarbonate copolymer, optical lens and film in which said polycarbonate copolymer is used, and method for producing said copolymer

    WO2017175693A1

  • Polycarbonate resin composition and optical lens using same

    WO2018181157A1

  • Thermoplastic resin and optical member

    WO2019044214A1

  • Polycarbonate resin and optical member containing same

    WO2019188702A1

Cited By

  • Polycarbonate resin and optical member using same

    WO2025164207A1