Phenolic resin foam, thermal decomposition method for phenolic resin foam, thermal decomposition product of phenolic resin foam, and method for producing phenolic resin foam
The thermal decomposition of phenolic resin foam under controlled conditions allows for the reuse of the decomposed product as a raw material, overcoming recycling challenges and achieving high-performance phenolic resin foam production, thus addressing environmental concerns and improving material reuse.
Patent Information
- Application Number
- PCT/JP2024/015325
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-31
AI Technical Summary
The recycling of phenolic resin foam is challenging due to its crosslinked structure, which makes it difficult to dissolve in solvents and reuse as a raw material for producing high-performance phenolic resin foam, leading to environmental concerns from disposal methods like incineration or landfill.
A method involving the thermal decomposition of phenolic resin foam under specific conditions of temperature, pressure, and the use of a mononuclear phenolic compound or water solution to achieve a high decomposition rate, allowing the reuse of the decomposed product as a raw material for producing phenolic resin foam with improved properties.
This method enables the production of phenolic resin foam with excellent thermal conductivity, closed cell ratio, and mechanical strength, while reducing environmental impact by allowing the reuse of recycled materials, resulting in a product comparable to conventional phenolic resin foams.
Smart Images

Figure JP2024015325_31102024_PF_FP_ABST
Abstract
Description
Phenolic resin foam, method for thermal decomposition of phenolic resin foam, product of thermal decomposition of phenolic resin foam, and method for manufacturing phenolic resin foam CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to Japanese Patent Application No. 2023-075264, filed on April 28, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a phenolic resin foam, a method for thermally decomposing a phenolic resin foam, a product of the thermally decomposed phenolic resin foam, and a method for producing a phenolic resin foam.
[0003] Phenolic resin foam has high thermal insulation, flame retardancy, and heat resistance among foam plastic insulation materials, and is therefore widely used as a building material and general industrial material. However, unlike thermoplastic resins, phenolic resin forms a cross-linked structure once cured, so it does not soften or melt due to heat and is difficult to dissolve in solvents. For this reason, it has been technically difficult to recycle cured phenolic resin as a plastic raw material.
[0004] Therefore, phenolic resin foam contained in industrial waste and general waste has been disposed of by incineration or landfill, but due to concerns about the environmental impact, there has been a strong demand for technology that would allow it to be reused rather than treated as waste.
[0005] A technique for dissolving thermosetting resins for the purpose of recycling them is reported in Patent Document 1. Patent Document 1 discloses a technique for obtaining low molecular weight components by heating a thermosetting resin that has been cured in a non-foamed state in a solvent in a subcritical state.
[0006] Patent Document 2 discloses a technology in which a phenolic resin foam is pulverized into particles (powder), extruded in the presence of phenols, and the recovered extrudate is used as a raw material for the phenolic resin foam.
[0007] JP 2001-151933 A JP 2003-183475 A
[0008] However, in Patent Document 1, the thermosetting resin cured in a non-foamed state is crushed in advance and then decomposed. However, due to the presence of by-products and solid residues after the decomposition treatment, if the decomposition product is used as a raw material for a resin foam as is, a good foam cannot be obtained. In addition, there are problems such as a large load on the manufacturing equipment, making it impossible to produce a foam.
[0009] In Patent Document 2, the phenolic resin foam is decomposed in an extruder for a short period of time, which may result in insufficient decomposition or the production of carbonized products, thereby potentially reducing the performance of the phenolic resin foam.
[0010] That is, there has been a need for a so-called chemical recycling technology that can completely decompose phenolic resin foam and then make it usable as a raw material for phenolic resin foam without any particularly complicated treatment.
[0011] The object of the present invention is to provide a phenolic resin foam having excellent performance by chemically decomposing a phenolic resin foam and reusing the recovered material as part of a resin raw material.
[0012] That is, the present invention is as follows: [1] A phenolic resin foam, in which, when the phenolic resin foam is subjected to pyrolysis gas chromatography mass spectrometry under heating conditions of 600°C, the ratio [A] / [B] is 2.0 or more and 15 or less, where [A] is the area value of the signal of structural formula (A) and [B] is the area value of the signal of structural formula (B). [2] The phenolic resin foam according to [1], having a thermal conductivity of 0.016 W / (m K) or more and 0.026 W / (m K) or less. [3] The phenolic resin foam according to [1] or [2], having a closed cell ratio of 85% or more. [4] A density of 20 kg / m 3 More than 70kg / m 3The phenolic resin foam according to any one of [1] to [3] below. [5] A method for thermal decomposition of phenolic resin foam, comprising heating and pressurizing the phenolic resin foam in a mononuclear phenolic compound or a water / mononuclear phenolic compound solution at 260°C to 370°C, 1.5 MPa to 20 MPa, and for 60 minutes to 240 minutes, to obtain a decomposition product with a decomposition rate of 95% or more. [6] A decomposition product obtained by thermal decomposition of phenolic resin foam, containing 0.01% to 4.0% xanthene. [7] A method for producing the phenolic resin foam according to any one of [1] to [4], comprising adding the decomposition product according to [6] in an amount of 0.1 parts by mass to 20.0 parts by mass per 100 parts by mass of phenolic resin, followed by foaming and curing.
[0013] According to the method of the present invention, it is possible to obtain a good phenolic resin foam containing xanthene. Furthermore, the decomposition product containing xanthene, which is a by-product of the decomposition of the raw phenolic resin foam, can be reused as part of the raw material for a new phenolic resin foam.
[0014] The present invention relates to a phenolic resin foam containing a predetermined amount of xanthene. It has also been discovered that by solubilizing the phenolic resin foam by chemical decomposition under specific conditions and reusing the solubilized component as part of the raw material for newly produced phenolic resin foam, a phenolic resin foam with excellent performance comparable to that of conventional products can be obtained.
[0015] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and various modifications can be made within the scope of the gist thereof.
[0016] The pyrolysis gas chromatography mass spectrometry, density, thermal conductivity, and closed cell ratio of the phenolic resin foam obtained according to this embodiment can be determined by the methods described in the examples.
[0017] In this specification, a phenolic resin foam that has been subjected to a decomposition treatment as described below is referred to as a "decomposition-treated product." Furthermore, a "phenolic resin" to which a surfactant and a decomposition-treated product have been added is referred to as a "phenolic resin composition." A "phenolic resin composition" to which a foaming agent, a foam nucleating agent, an acidic curing agent, etc. have been added to impart foamability or both foamability and curability is referred to as a "foamable phenolic resin composition." A foam obtained by foaming and curing a phenolic resin composition is referred to as a "phenolic resin foam."
[0018] It is known that even if a known phenolic resin foam does not contain xanthene, xanthene is generally produced by the heating operation during pyrolysis gas chromatography-mass spectrometry, which will be described later. In the present invention, a phenolic resin foam is subjected to a heating and pressurizing treatment under high-temperature and high-pressure conditions in a predetermined solution, and the decomposition product is reused as part of the raw material for the phenolic resin foam. It has been found that the decomposition product contains xanthene, resulting in a phenolic resin foam containing more xanthene than known phenolic resin foams. Pyrolysis gas chromatography-mass spectrometry is used as a means for measuring xanthene in the phenolic resin foam.
[0019] In a chromatogram of pyrolysis gas chromatography-mass spectrometry of the phenolic resin foam obtained by the present invention under heating conditions of 600°C, the ratio [[A] / [B]] of the area value [A] of the signal of xanthene (A) to the area value [B] of the signal of a diphenylmethane derivative-derived component (B) decomposed and detected from the phenolic resin foam is 2.0 or more and 15 or less, preferably 2.2 or more and 13 or less, and more preferably 2.4 or more and 10 or less. If [[A] / [B]] is less than 2.0, the amount of raw material to be subjected to the thermal decomposition treatment is small, making the reuse of the phenolic resin foam less meaningful. If it is greater than 15, the closed cell content of the resulting phenolic resin foam is reduced.
[0020]
[0021]
[0022] The density of the phenolic resin foam obtained by the present invention is 20 kg / m 3 More than 70kg / m 3 or less, preferably 25 kg / m 3 More than 60kg / m 3 The density of the phenolic resin foam is 20 kg / m or less. 3 When the density of the phenolic resin foam is 70 kg / m or more, mechanical strength such as compressive strength and bending strength can be ensured, and breakage of the plate-shaped phenolic resin foam during handling can be reduced. 3
[0033] When the density is less than 100%, the heat transfer in the phenolic resin portion of the phenolic resin foam is less likely to increase, thereby maintaining the heat insulating performance. The density of the phenolic resin foam can be adjusted to a desired value mainly by changing the proportion of the blowing agent, the temperature of the foamable phenolic resin composition, the timing of preforming in the step of discharging the mixed foamable phenolic resin composition onto the lower surface material, the ratio of the amount of blowing agent added to the amount of organic acid added as an acidic curing agent, and curing conditions such as temperature and residence time.
[0023] The thickness of the phenolic resin foam obtained by the present invention is not particularly limited and can be set appropriately. The thickness of the phenolic resin foam is preferably 30 mm or more and 200 mm or less, more preferably 35 mm or more and 200 mm or less, and even more preferably 40 mm or more and 200 mm or less.
[0024] The closed cell ratio of the phenolic resin foam obtained by the present invention is preferably 85% or more, more preferably 90% or more. The closed cell ratio is, for example, 99% or less, 98% or less, or 97% or less. Since the closed cell ratio is an index of heat insulating performance, a closed cell ratio of 85% or more is preferable because the heat insulating performance is good.
[0025] The closed cell ratio can be adjusted to a desired value mainly by adjusting the ratio of component (A) in the foam, the reactivity and temperature of the phenolic resin, and also by changing the curing temperature conditions.
[0026] The thermal conductivity of the phenolic resin foam obtained by the present invention is 0.026 W / (m·K) or less, preferably 0.016 W / (m·K) or more and 0.025 W / (m·K) or less, more preferably 0.016 W / (m·K) or more and 0.024 W / (m·K) or less, and even more preferably 0.016 W / (m·K) or more and 0.023 W / (m·K) or less.
[0027] The shape of the phenolic resin foam obtained by the present invention is not particularly limited and can be any shape. Examples of the shape of the phenolic resin foam include a rectangular parallelepiped (e.g., a plate, layer, sheet, etc.), a polyhedron other than a rectangular parallelepiped (e.g., a regular polyhedron such as a regular tetrahedron, a regular octahedron, a regular dodecahedron, and a regular icosahedron), a sphere, a pyramid, a cone, a torus, a hollow cylinder, a solid cylinder (cylinder), and an irregular shape. In one embodiment, the phenolic resin foam is a rectangular parallelepiped.
[0028] As the phenolic resin, a resol type phenolic resin synthesized from an alkali metal hydroxide or an alkaline earth metal hydroxide is used.
[0029] The starting molar ratio of phenols to aldehydes in the synthesis of the phenolic resin is preferably in the range of 1:1 to 1:4.5, more preferably in the range of 1:1.5 to 1:2.5.
[0030] Here, in this embodiment, phenols preferably used in synthesizing the phenolic resin include phenol itself and other phenols, and examples of other phenols include resorcinol, catechol, o-, m-, and p-cresol, xylenols, ethylphenols, p-tert-butylphenol, etc. Dinuclear phenols can also be used.
[0031] The aldehyde may be any compound that can serve as an aldehyde source, and the aldehyde may preferably be formaldehyde itself, or other aldehydes or derivatives thereof, such as glyoxal, acetaldehyde, chloral, furfural, and benzaldehyde.
[0032] Resole phenolic resins are synthesized by heating phenols and aldehydes as raw materials in the presence of an alkali catalyst at a temperature range of 40 to 100°C. Furthermore, additives such as urea, dicyandiamide, and melamine may be added as needed during or after the synthesis of the resol phenolic resin. When adding these additives, it is more preferable to mix urea that has been methylolated with an alkali catalyst in advance with the resol phenolic resin. Since resol phenolic resins after synthesis usually contain excess moisture, the moisture content is adjusted to an appropriate level for foaming before foaming.
[0033] In addition to the surfactant added to the phenolic resin, other additives may be added, such as aliphatic hydrocarbons or high-boiling alicyclic hydrocarbons, or mixtures thereof, viscosity-adjusting diluents such as ethylene glycol and diethylene glycol, and other additives as needed. In this specification, when these additives are added, the term "phenolic resin" refers to the resin before the addition of additives such as surfactants, and the resin after the addition of additives is referred to as the "phenolic resin composition."
[0034] The viscosity of the phenolic resin at 40° C. is preferably 5,000 mPa·s or more and 100,000 mPa·s or less, more preferably 7,000 mPa·s or more and 50,000 mPa·s or less, and even more preferably 9,000 mPa·s or more and 30,000 mPa·s or less. The water content of the phenolic resin is preferably 1.5% by mass or more and 30% by mass or less.
[0035] Surfactants commonly used in the production of phenolic resin foams can be used as surfactants, but nonionic surfactants are particularly effective. Examples include alkylene oxides (copolymers of ethylene oxide and propylene oxide), condensates of alkylene oxides and castor oil, condensation products of alkylene oxides and alkylphenols such as nonylphenol and dodecylphenol, polyoxyethylene alkyl ethers having 14 to 22 carbon atoms in the alkyl ether moiety, fatty acid esters such as polyoxyethylene fatty acid esters, silicone compounds such as polydimethylsiloxane, and polyalcohols. These surfactants may be used alone or in combination of two or more. There are no particular restrictions on the amount used, but a range of 0.3 to 10 parts by weight per 100 parts by weight of phenolic resin is preferred.
[0036] The present invention is characterized in that, when producing a phenolic resin foam, the raw material phenolic resin or phenolic resin composition contains, as part of the raw materials, a decomposition product obtained by thermally decomposing a phenolic resin foam.
[0037] The phenolic resin foam used as a recycled raw material is preferably pulverized before thermal decomposition to increase the surface area of particles or powder. This is because the larger the surface area, the more efficiently the decomposition reaction proceeds. In this regard, in the present invention, the recycled raw material is obtained by pulverizing a phenolic resin foam rather than a phenolic resin cured in an unfoamed state. Therefore, due to the presence of the bubbles and bubble membranes that formed the foam, the surface area of the particles or powder obtained by pulverization is larger than that of particles or powder obtained by pulverizing a phenolic resin cured in an unfoamed state, thereby allowing the decomposition process to proceed more efficiently. The particle size of the phenolic resin foam powder used as a recycled raw material is preferably 5 μm or more and 1000 μm or less, more preferably 20 μm or more and 800 μm or less, and even more preferably 40 μm or more and 600 μm or less, as an average particle size. Furthermore, the bulk density of the phenolic resin foam powder is 10 kg / m or less. 3 More than 50kg / m 3 Preferably less than 15 kg / m3 45kg / m or more 3 More preferably, it is 20 kg / m or less. 3 More than 40kg / m 3 The following is the result.
[0038] The phenolic resin foam to be subjected to thermal decomposition treatment as a recycled material, particularly its pulverized powder, may contain components other than the phenolic resin foam. The proportion of the phenolic resin foam in the entire pulverized powder is preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more. Note that, as components other than the phenolic resin foam, the phenolic resin foam powder may contain surface material components such as polyester nonwoven fabric, paper, and glass fiber mixed paper laminated on the phenolic resin foam as a recycled raw material.
[0039] The phenolic compound used as a solvent during the thermal decomposition of the phenolic resin foam as a recycled raw material is not particularly limited, as long as it has at least one hydrogen atom bonded to a carbon atom in the aromatic ring substituted with a hydroxyl group, functions as a solvent in a supercritical or subcritical state, either alone or as a mixture with other solvents, and can decompose and / or solubilize the phenolic resin foam. Preferred phenolic compounds used as solvents are typically monocyclic phenolic compounds such as phenol, cresol, xylenol, resorcinol, and alkyl-substituted phenols, as well as polycyclic phenolic compounds such as 1-naphthol and 2-naphthol, and one or more of these compounds are used. Of these, phenol is preferred in terms of cost and its effect on thermal decomposition.
[0040] The solvent used for thermal decomposition of phenolic resin foam as a recycled raw material can be a phenolic compound alone or a mixture of a phenolic compound and another solvent. When using a mixture of a phenolic compound and another solvent, the other solvent may be any solvent commonly used in chemical reactions, including water, monoalcohols such as methanol and ethanol, glycols such as ethylene glycol and propylene glycol, ketones, ethers, esters, organic acids, and acid anhydrides. Multiple solvents may also be used in combination. Among these solvents, water is preferred as the other solvent due to its effect on decomposition and ease of availability. The mixing ratio of the other solvent to the phenolic compound is preferably 1 to 500 parts by weight of the other solvent per 100 parts by weight of the phenolic compound, and more preferably 5 to 50 parts by weight of the other solvent per 100 parts by weight of the phenolic compound. Adding more than 500 parts by weight of the other solvent may result in a decrease in the decomposition rate.
[0041] In the thermal decomposition of the phenolic resin foam as a recycled raw material, the ratio of the solvent to the phenolic resin foam is 50 to 2000 parts by mass, more preferably 100 to 1500 parts by mass, and even more preferably 150 to 1000 parts by mass, per 100 parts by mass of the phenolic resin foam.
[0042] If the amount of the solvent is less than 50 parts by mass, it may be difficult to smoothly decompose the phenolic resin foam, whereas if the amount of the solvent is more than 2,000 parts by mass, the energy required for heating may increase, resulting in an increase in processing costs, and further, the recycling rate when the phenolic resin foam is used as a raw material may decrease.
[0043] The decomposition temperature of the phenolic resin foam as a recycled raw material is 260° C. or higher and 370° C. or lower, preferably 280° C. or higher and 360° C. or lower, and more preferably 300° C. or higher and 350° C. or lower. If the decomposition temperature is lower than 260° C., the phenolic resin foam is not sufficiently decomposed and is unsuitable as a raw material. If the decomposition temperature is higher than 370° C., the amount of component (A) produced increases, making the foam unsuitable as a raw material for phenolic resin foam.
[0044] The pressure during thermal decomposition of the phenolic resin foam as a recycled raw material is 1.5 MPa or more and 20 MPa or less, preferably 2.0 MPa or more and 15 MPa or less, and more preferably 2.5 MPa or more and 10 MPa or less. If the pressure is less than 1.5 MPa, the phenolic resin foam may not be sufficiently decomposed and is unsuitable as a raw material. Even if the pressure is increased above 20 MPa, the energy required for pressurization increases, resulting in increased processing costs. The pressure can be adjusted by the temperature and the amount of phenolic resin foam and solvent relative to the volume of the reaction vessel.
[0045] The treatment time for thermal decomposition of the phenolic resin foam as a recycled raw material can be adjusted within a range of 60 to 240 minutes, preferably 80 to 220 minutes, and more preferably 100 to 200 minutes. If the treatment time is shorter than 60 minutes, the decomposition of the phenolic resin foam does not proceed sufficiently. If the reaction time is longer than 240 minutes, the amount of by-products produced will simply increase.
[0046] The decomposition reaction of the phenolic resin foam as a recycled raw material is carried out in an inert gas atmosphere at high temperature and pressure, and is therefore preferably carried out in a closed reaction vessel such as an autoclave. As the inert gas, nitrogen is preferably used.
[0047] The decomposition rate of the phenolic resin foam as a recycled raw material is 95% or more, preferably 97% or more, and more preferably 99% or more. If the decomposition rate is 95% or more, there is no need to remove the undecomposed residue by filtration or the like, and when added to the phenolic resin, there is no increase in viscosity or a decrease in the closed cell rate of the phenolic resin foam. The decomposition rate can be calculated using formula (1). Decomposition rate (%) = [weight of phenolic resin foam before decomposition (g) - weight of solid residue (g)] / weight of phenolic foam before decomposition (g) - (1)
[0048] When a phenolic resin foam as a recycled raw material is thermally decomposed at high temperatures, xanthene is produced as a by-product. By decomposing the phenolic resin foam within the above-mentioned temperature range and time, it is possible to decompose the phenolic resin foam at a high decomposition rate while suppressing the production of xanthene.
[0049] The mass proportion of xanthene contained in the decomposition product after thermal decomposition of phenolic resin foam as a recycled raw material is 0.01% to 4.0%, preferably 0.05% to 3.5%, and more preferably 0.1% to 3.0%. The lower the xanthene content, the more suitable it is for a recycled raw material. However, to suppress the generation to 0.01% or less, the decomposition treatment must be performed at a temperature lower than the above range, making it difficult to decompose the phenolic resin foam. If the xanthene content is more than 4.0%, the closed cell rate decreases when the phenolic resin foam is produced, and the recycling rate cannot be increased.
[0050] The ratio of xanthene contained in the decomposition product can be measured by gas chromatography mass spectrometry.
[0051] The amount of decomposition product added as a recycled raw material may vary depending on foaming and curing conditions such as temperature and residence time, but is generally 0.1 to 20.0 parts by mass, preferably 0.5 to 15.0 parts by mass, and more preferably 1.0 to 10 parts by mass, per 100 parts by mass of phenolic resin. If the amount is less than 0.1 part by mass, the recycling rate will be low, and if it exceeds 20.0 parts by mass, the closed cell rate will decrease when the foam is produced.
[0052] In order to further reduce the thermal conductivity of the phenolic resin foam obtained by the present invention, the phenolic resin foam preferably contains a hydrocarbon, a hydrofluorocarbon, a chlorinated hydrofluoroolefin, a non-chlorinated hydrofluoroolefin, or a chlorinated hydrocarbon as a blowing agent.
[0053] The hydrocarbon is preferably a cyclic or chain alkane, alkene, or alkyne having 3 to 7 carbon atoms, and specific examples include normal butane, isobutane, cyclobutane, normal pentane, isopentane, cyclopentane, neopentane, normal hexane, isohexane, 2,2-dimethylbutane, 2,3-dimethylbutane, cyclohexane, etc. Among these, pentanes such as normal pentane, isopentane, cyclopentane, and neopentane, and butanes such as normal butane, isobutane, and cyclobutane are preferably used.
[0054] Examples of hydrofluorocarbons include hydrofluoropropene, hydrochlorofluoropropene, hydrobromofluoropropene, hydrofluorobutene, hydrochlorofluorobutene, hydrobromofluorobutene, hydrofluoroethane, hydrochlorofluoroethane, and hydrobromofluoroethane.
[0055] Examples of chlorinated hydrofluoroolefins that can be used as blowing agents include HCFO-1224yd(Z) (chemical name: (Z)-1-chloro-2,3,3,3-tetrafluoropropene), which has a particularly low thermal conductivity, 1-chloro-3,3,3-trifluoropropene (HCFO-1233zd, for example, E-isomer (HCFO-1233zd(E)), manufactured by Honeywell Japan, Ltd., product name: Solstice (trademark) LBA), and 1,1,2-trichloropropene (HCFO-1233zd(E)). 1,2-dichloro-3,3,3-trifluoropropene (HCFO-1223xa), 1,2-dichloro-3,3,3-trifluoropropene (HCFO-1223xd), 1,1-dichloro-3,3,3-trifluoropropene (HCFO-1223za), 1-chloro-1,3,3,3-tetrafluoropropene (HCFO-1224zb), 2,3,3-trichloro-3-fluoropropene (HCFO-1231xf), 2,3-dichloro-3,3-difluoropropene (HC 2-chloro-1,1,3-trifluoropropene (HCFO-1232xf), 2-chloro-1,1,3-trifluoropropene (HCFO-1233xc), 2-chloro-1,3,3-trifluoropropene (HCFO-1233xe), 2-chloro-3,3,3-trifluoropropene (HCFO-1233xf), 1-chloro-1,2,3-trifluoropropene (HCFO-1233yb), 3-chloro-1,1,3-trifluoropropene (HCFO-1233yc), 1-chloro-2,3,3-trifluoropropene These configurational isomers, i.e., E- and Z-isomers, may be used singly or in combination. Further examples include (E)-1-chloro-2,3,3,3-tetrafluoropropene (HCFO-1224yd(E)).
[0056] Examples of non-chlorinated hydrofluoroolefins include 1,3,3,3-tetrafluoroprop-1-ene (HFO-1234ze, for example, the E-form (HFO-1234ze(E)), manufactured by Honeywell Japan Co., Ltd., product name: Solstice™ ze), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz, for example, the Z-form (HFO-1336mzz(Z)), manufactured by Chemours Inc., Opteon™ 1100), and 2,3,3,3- Examples include tetrafluoro-1-propene (HFO-1234yf), 1,1,3,3,3-pentafluoropropene (HFO-1225zc), 1,3,3,3-tetrafluoropropene (HFO-1234ze), 3,3,3-trifluoropropene (HFO-1243zf), and 1,1,1,4,4,5,5,5-octafluoro-2-pentene (HFO-1438mzz), and these configurational isomers, i.e., E-isomers and Z-isomers, may be used alone or in combination.
[0057] When a chlorinated hydrofluoroolefin or a non-chlorinated hydrofluoroolefin is used, the content of the blowing agent in the total amount of blowing agents is preferably 30% by mass or more.
[0058] As the chlorinated hydrocarbon, linear or branched chlorinated aliphatic hydrocarbons having 2 to 5 carbon atoms can be preferably used. The number of bonded chlorine atoms is preferably 1 to 4, and examples thereof include dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, and isopentyl chloride. Of these, propyl chloride and isopropyl chloride, which are chloropropanes, are more preferably used.
[0059] The above-mentioned foaming agents may be used alone or in combination of two or more kinds, and can be selected arbitrarily.
[0060] When producing the phenolic resin foam obtained by the present invention, the amount of the foaming agent in the foamable phenolic resin composition is preferably 10.0 parts by mass or less, more preferably 4.5 parts by mass or more and 10.0 parts by mass or less, and even more preferably 5.0 parts by mass or more and 9.0 parts by mass or less, per 100 parts by mass of the phenolic resin or phenolic resin composition.
[0061] In this embodiment, a foam nucleating agent may be further used during the production of the phenolic resin foam obtained by the present invention. Examples of the foam nucleating agent include gaseous foam nucleating agents, such as nitrogen, helium, argon, and air, which have a boiling point 50° C. or more lower than that of the foaming agent. Solid foam nucleating agents may also be added, such as inorganic powders such as aluminum hydroxide powder, aluminum oxide powder, calcium carbonate powder, talc, kaolin, silica stone powder, silica sand, mica, calcium silicate powder, wollastonite, glass powder, glass beads, fly ash, silica fume, gypsum powder, borax, slag powder, alumina cement, and Portland cement, and organic powders such as crushed powder of phenolic resin foam. These may be used alone or in combination of two or more, regardless of whether they are gaseous or solid. The timing of adding the foam nucleating agent can be determined arbitrarily, as long as it is supplied to the mixer used to mix the foamable phenolic resin composition.
[0062] The amount of the gaseous foam nucleating agent added relative to the amount of the foaming agent is preferably 0.2 to 1.0% by mass, and more preferably 0.3 to 0.5% by mass, based on 100 parts by mass of the foaming agent. The amount of the solid foam nucleating agent added relative to 100 parts by mass of the phenolic resin or phenolic resin composition is preferably 3.0 to 10.0 parts by mass, and more preferably 4.0 to 8.0 parts by mass.
[0063] When producing the phenolic resin foam obtained by the present invention, the acidic curing agent added to the foamable phenolic resin composition must contain an organic acid as the acid component. The organic acid is preferably an arylsulfonic acid or an anhydride thereof. Examples of arylsulfonic acids and their anhydrides include toluenesulfonic acid, xylenesulfonic acid, phenolsulfonic acid, substituted phenolsulfonic acid, xylenolsulfonic acid, substituted xylenolsulfonic acid, dodecylbenzenesulfonic acid, benzenesulfonic acid, naphthalenesulfonic acid, and the like, as well as their anhydrides. These may be used alone or in combination. In this embodiment, resorcinol, cresol, saligenin (o-methylolphenol), p-methylolphenol, or the like may be added as a curing aid. These curing agents may also be diluted with solvents such as ethylene glycol and diethylene glycol.
[0064] The amount of acidic curing agent used varies depending on the type thereof. When a mixture of 80 mass % xylene sulfonic acid and 20 mass % diethylene glycol is used, the amount used is preferably 6 parts by mass or more and 16 parts by mass or less, more preferably 8 parts by mass or more and 13 parts by mass or less, per 100 parts by mass of the phenolic resin or phenolic resin composition.
[0065] Flexible face materials (flexible face materials) are used as the face materials disposed on at least the upper and lower surfaces of the phenolic resin foam obtained by the present invention. Preferred flexible face materials include nonwoven and woven fabrics primarily composed of polyester, polypropylene, nylon, etc.; papers such as kraft paper, glass fiber-blended paper, calcium hydroxide paper, aluminum hydroxide paper, and magnesium silicate paper; and inorganic fiber nonwoven fabrics such as glass fiber nonwoven fabrics. These may be mixed (or laminated) and used. In particular, when peeling the face material from the resulting phenolic resin foam laminate and using only the base material, inexpensive paper that can be disposed of after peeling is preferred. These face materials are usually provided in roll form. Furthermore, flexible face materials may be mixed with additives such as flame retardants. The method of bonding the face material to the phenolic resin foam is not particularly limited, and may include the adhesion force generated when the phenolic resin foam is thermally cured on the face material surface or the use of an adhesive such as an epoxy resin.
[0066] Next, a method for producing the phenolic resin foam obtained by the present invention will be described.
[0067] The method for producing the phenolic resin foam obtained by the present invention can preferably employ a continuous production method including the following steps: a mixing step in which a phenolic resin, a decomposition product as a recycled raw material, a foaming agent, and an acidic curing agent containing an organic acid are mixed in a mixer to obtain a foamable phenolic resin composition; a discharging step in which the foamable phenolic resin composition is discharged onto a lower surface material; a pre-molding step in which the foamable phenolic resin composition discharged onto the lower surface material is foamed and cured; a main molding step in which the foaming and curing reactions are carried out; and a post-curing step in which moisture in the foamable phenolic resin composition is dissipated.
[0068] In the continuous manufacturing method, it is preferable that the foamable phenolic resin composition ejected onto the lower surface material is covered with the upper surface material, and then the composition is pre-molded to be uniform from the top and bottom while foaming and curing, and then molded into a plate shape while foaming and curing are continued in the main molding process.
[0069] The method for adding the decomposition product to the phenolic resin or phenolic resin composition and kneading them is not particularly limited, and mixing may be performed using a hand mixer, a pin mixer, or the like, or a twin-screw extruder, a kneader, or the like.
[0070] The mixer used to obtain the foamable phenolic resin composition is not particularly limited, but the one disclosed in JP-A-10-225993 can be used. That is, the mixing section and the distribution section are each equipped with a temperature control jacket to enable temperature control, and a thermometer is installed at the outlet (mixing end section) of the mixing section before entering the distribution section to control the temperature of the foamable phenolic resin composition.
[0071] In the continuous production method, the preforming and main forming steps can be carried out by various methods depending on the production purpose, such as a method using a slat-type double conveyor, a method using a metal roll or a steel plate, or a method using a combination of these. Among these, when forming is carried out using a slat-type double conveyor, for example, a foamable phenolic resin composition coated with upper and lower face materials is continuously guided into the slat-type double conveyor, and then pressure is applied from above and below while heating, so that the composition is foamed and cured while being adjusted to a predetermined thickness, and formed into a plate.
[0072] The heating temperature control conditions in the preforming step are preferably a space temperature of 45°C or higher and 70°C or lower.
[0073] The heating temperature control conditions for the main molding step following the pre-molding step are preferably 70°C or higher and 100°C or lower. In this section, main molding can be performed using an endless steel belt type double conveyor, a slat type double conveyor, or rolls. If the temperature is 70°C or higher, curing tends to be accelerated. On the other hand, if the temperature exceeds 100°C, although the curing reactivity increases and high-speed molding becomes possible, the closed cell content of the plate-shaped phenolic resin foam tends to decrease, i.e., the heat of reaction inside the foam tends to be too strong during foaming and curing, which tends to deteriorate the heat insulating performance.
[0074] The post-curing step is carried out after the pre-molding step and the main molding step. The temperature in the post-curing step is preferably 90°C or higher and 120°C or lower.
[0075] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0076] <Synthesis of Phenolic Resin> A reactor was charged with 3,500 kg of a 52% by weight aqueous formaldehyde solution (52% by weight formalin) and 2,510 kg of 99% by weight phenol (containing water as an impurity). The mixture was stirred using a propeller-rotating stirrer, and the temperature of the liquid inside the reactor was adjusted to 40°C using a temperature controller. Next, a 48% by weight aqueous sodium hydroxide solution was added until the pH reached 8.7, and the temperature was then raised to 85°C to carry out the reaction. When the Ostwald viscosity of the reaction liquid reached 120 square millimeters per second (= 120 mm2 / s, measured at 25°C), urea was added while cooling the reaction liquid so that the urea content in the phenolic resin was 4.6% by weight. The reaction liquid was then cooled to 30°C, and a 50% by weight aqueous solution of paratoluenesulfonic acid monohydrate was added until the pH reached 6.3. The resulting reaction liquid was concentrated using a thin-film evaporator, and the weight-average molecular weight and viscosity were measured using the following methods. As a result, a phenolic resin having a weight average molecular weight of 1,800 and a viscosity at 40° C. of 12,000 mPa·s was obtained.
[0077] <Weight-Average Molecular Weight> Measurements were performed by gel permeation chromatography (GPC) under the following conditions, and the weight-average molecular weight Mw of the phenolic resin was determined from a calibration curve obtained using standard substances (standard polystyrene, 2-hydroxybenzyl alcohol, and phenol) shown below. Pretreatment: Approximately 10 mg of phenolic resin was dissolved in 1 ml of N,N-dimethylformamide (Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography), and the solution was filtered through a 0.2 μm membrane filter. The resulting solution was used as the measurement solution. Measurement Conditions: Measurement Apparatus: Shodex System 21 (Showa Denko K.K.) Column: Shodex Asahipak GF-310HQ (7.5 mm I.D. × 30 cm) Eluent: 0.1% by mass of lithium bromide dissolved in N,N-dimethylformamide (Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography). Flow rate: 0.6 ml / min Detector: RI detector Column temperature: 40°C Standard substances: standard polystyrene (Shodex standard SL-105 manufactured by Showa Denko K.K.), 2-hydroxybenzyl alcohol (Sigma-Aldrich, 99% product), phenol (Kanto Chemical Co., Ltd., special grade)
[0078] <Viscosity> A rotational viscometer (manufactured by Toki Sangyo Co., Ltd., R-100 model, rotor part 3°×R-14) was used, and the measured value after stabilizing at 40° C. for 3 minutes was taken as the viscosity of the phenolic resin.
[0079] <Water content of phenolic resin> A solution was prepared by dissolving phenolic resin in anhydrous methanol (manufactured by Kanto Chemical Co., Ltd.) in a range of 3% to 7% by mass. The water content of the phenolic resin was determined by subtracting the water content of the anhydrous methanol from the water content of the solution. A Karl Fischer moisture meter (MKC-510, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) was used for the measurement.
[0080] <Proportion of phenolic resin foam in the entire pulverized powder> 10 g of pulverized powder was weighed, and the weight proportion of the powder that passed through a 1 mm mesh sieve was taken as the proportion of phenolic resin foam, and the average value of three measurements was calculated. In this case, the face material in particular was not finely divided even after the pulverization process, and therefore could not pass through the mesh sieve and was removed.
[0081] <Average particle size of phenolic resin foam powder> The particle size distribution of the phenolic resin foam powder dispersed in water was measured, and the cumulative 50% particle size was taken as the average particle size. The measurement was performed using a particle size distribution analyzer (Microtrac MT3300EXII-SDC) with a particle refractive index of 1.81 and a measurement time of 30 seconds, and the average value of two measurements was calculated.
[0082] Example 1 Decomposition of Phenolic Resin Foam as a Recycled Raw Material (1) After removing the surface material from phenolic foam (NEOMA FOAM, manufactured by Asahi Kasei Construction Materials Co., Ltd.), the foam was cut into pieces approximately 10 cm in size and pulverized for 10 minutes in a Henschel mixer (Mitsui Miike Machinery Works, Ltd.; Model FM20B) to produce a cross-linked, cured phenolic resin foam powder. The average particle size of the resulting phenolic resin foam powder was 174 μm. 100 g of this phenolic resin foam powder, 620 g of phenol, and 100 g of water were charged into an autoclave (internal volume 2 L) and heated to an internal temperature of 350°C, thereby increasing the internal pressure of the reactor to 5.6 MPa, creating a high-temperature, high-pressure state. The reaction system was maintained at 350°C and 5.6 MPa for 3 hours, then cooled to room temperature and pressure, and the recovered material was filtered to obtain a decomposition product. The decomposition rate of the phenolic resin foam was 99.5%. The proportion of phenolic resin foam in the crushed powder of phenolic resin foam after removing the face material, which was to be subjected to thermal decomposition treatment as a reusable material, was 100.0 wt %.
[0083] <Preparation of Phenolic Resin Foam Obtained According to the Present Invention> 100 parts by mass of phenolic resin was mixed with 2.8% by mass of a composition containing 50% by mass of an ethylene oxide-propylene oxide block copolymer and 50% by mass of polyoxyethylene dodecyl phenyl ether as surfactants. This mixture was then mixed with 5.0 parts by mass of the decomposition product relative to 100 parts by mass of the phenolic resin, and kneaded using a twin-screw extruder (manufactured by Technovel Corporation) to obtain a phenolic resin composition. To 100 parts by mass of this phenolic resin composition, 6.0 parts by mass of a mixture of 75% by mass of cyclopentane and 25% by mass of isobutane as a blowing agent, 0.4% by mass of nitrogen as a gas foam nucleating agent relative to the blowing agent, and 10 parts by mass of a composition consisting of a mixture of 80% by mass of xylene sulfonic acid and 20% by mass of diethylene glycol as an acidic curing agent were added, and the mixture was fed into a variable-speed mixing head. The resulting foamable phenolic resin composition was distributed using a multi-port distribution pipe and fed onto a moving underside material. The mixer used was the one disclosed in Japanese Patent Laid-Open Publication No. 10-225993. Specifically, the mixer had inlets for the phenolic resin composition and the foaming agent, including the foam nucleating agent, on the upper side of the mixer, and an inlet for the acidic curing agent on the side near the center of the agitation section where the rotor mixes. The agitation section was connected to a nozzle for discharging the foamable phenolic resin composition. The mixer was configured as follows: the section up to the acidic curing agent inlet (pre-stage); the section from the acidic curing agent inlet to the agitation end point (post-stage); and the section from the agitation end point to the nozzle (distribution section). A pressure gauge was installed on the upper side of the mixer, and a thermometer was installed at the agitation end point. The distribution section had multiple nozzles at its tip, designed to ensure uniform distribution of the resulting foamable phenolic resin composition. The mixer and nozzles were each temperature-adjustable using temperature-adjusted water, which was set to 25°C. The mixing head rotation speed was set to 500 rpm. The foamable phenolic resin composition supplied onto the lower surface material was introduced into the preforming step, and the space temperature in the preforming step was set to 65° C. The preforming was carried out from above the upper surface material using a free roller.The foam was then sandwiched between two face sheets and introduced into a slat-type double conveyor heated to a space temperature of 85°C (main molding process). In the main molding process, the foam was cured for 10 minutes and then cut perpendicular to the running direction to obtain a plate-shaped phenolic resin foam intermediate with a length of 1820 mm, which was easy to handle. This was then further cured for 3 hours in an oven at 110°C (post-curing process), to obtain a plate-shaped phenolic resin foam with a thickness of 50 mm. The face sheets for both the top and bottom surfaces were polyester nonwoven fabric (Eltas E05060, Asahi Kasei Corporation, basis weight 60 g / m). 2 ) was used.
[0084] <Gas Chromatography Mass Spectrometry> Solid residue was removed from the decomposition product by filtration, diluted with distilled water, and then measured. Gas chromatograph: Agilent Technologies 7890B Column: DB-5 (30 m x 0.25 mm Φ, film thickness 1 μm) Column temperature: 40°C (5 min) → temperature increase at 10°C / min → 300°C (29 min) Flow rate: 1 mL / min Injection port temperature: 320°C Split ratio: 1 / 50 Injection volume: 1 μL Mass spectrometer: Agilent Technologies, 5977 Interface temperature: 300°C Ionization: EI 70 eV Scan range: m / z 10-800 Ion source temperature: 240°C
[0085] <Pyrolysis Gas Chromatography Mass Spectrometry> The face material was peeled off from the phenolic resin foam, and 0.15 mg of the foam was scraped off and measured. Measurement conditions: Pyrolyzer device Frontier-lab, EGA / PY-3030D Heating condition 600°C Gas chromatograph device Agilent Technologies 7890A Column DB-1 (30m x 0.25mmΦ, film thickness 0.25µm) Column temperature 50°C (5min) → 20°C / min → 320°C (11.5min) Flow rate 1mL / min Injection port temperature 320°C Split ratio 1 / 50 Injection amount Approximately 0.15mg Mass spectrometer JEOL RESONANCE, JMS-Q1500GC Interface temperature 320°C Ionization EI 70eV Scan range m / Z 10 to 800 Ion source temperature 240°C
[0086] <Measurement of Density of Phenolic Resin Foam> A 200 mm square phenolic resin foam sample was used, and after removing the surface material from the sample, the mass and apparent volume were measured in accordance with JIS K7222 to determine the density.
[0087] <Thermal Conductivity> The thermal conductivity of the phenolic resin foam in the thickness direction was measured in an environment of 23° C. by the following method in accordance with JIS A 1412-2:1999. The specific procedure is as follows.
[0088] The phenolic resin foam was cut into 300 mm square pieces and placed in an atmosphere at 23±1°C and 50±2% humidity. The weight change over time was then measured every 24 hours, and the condition was checked and adjusted until the weight change after 24 hours was 0.2% by mass or less. The conditioned composite specimen was then placed in a thermal conductivity apparatus also placed in an atmosphere at 23±1°C and 50±2% humidity. If the thermal conductivity measuring apparatus was not placed in the same room controlled at 23±1% and 50±2% humidity as the composite specimen, the specimen whose condition had been checked and adjusted in the aforementioned atmosphere was quickly placed in a polyethylene bag, the bag was closed, and the specimen was removed from the bag within one hour and its thermal conductivity was immediately measured. Thermal conductivity measurements were performed using a single-test-piece, symmetrical configuration measuring apparatus (Eiko Seiki Co., Ltd., product name "HC-074 / FOX304") with a thermal conductivity at 23°C of 13°C for the low-temperature plate and 33°C for the high-temperature plate.
[0089] <Closed Cell Ratio of Phenolic Resin Foam> The closed cell ratio of phenolic resin foam was measured in accordance with ASTM-D-2856 (Method C). Specifically, after removing the surface material from the phenolic resin foam, cylindrical samples with diameters of 35 mm to 36 mm were bored using a cork borer, and the sample volume was measured using an air-comparison hydrometer (Tokyo Science, Model 1000). The volume of the wall (the portion excluding bubbles and voids) was calculated from the sample mass and the density of the cured phenolic resin. The apparent volume was calculated from the outer dimensions of the sample. The value obtained by subtracting the wall volume from the sample volume and dividing this value by the apparent volume was used to determine the closed cell ratio. The density of the phenolic resin was 1.3 kg / L.
[0090] Example 2 A phenolic resin foam was obtained in the same manner as in Example 1, except that the amount of the decomposition product added was 10.0 parts by mass relative to 100 parts by mass of the phenolic resin.
[0091] Example 3 A phenolic resin foam was obtained in the same manner as in Example 1, except that the decomposition temperature of the phenolic resin foam as the recycled raw material was set to 300° C. and the pressure was set to 2.6 MPa.
[0092] Example 4 A phenolic resin foam was obtained in the same manner as in Example 1, except that the amount of phenolic resin foam powder obtained by thermal decomposition of the phenolic resin foam as the recycled raw material was 50 g.
[0093] (Example 5) A phenolic resin foam was obtained in the same manner as in Example 1, except that the thermal decomposition of the phenolic resin foam as a recycled raw material was carried out by the method described below in <Decomposition of phenolic resin foam as a recycled raw material (2)>.
[0094] <Decomposition of phenolic resin foam as recycled raw material (2)> A decomposition treatment product was obtained in the same manner as in <Decomposition of phenolic resin foam (1)>, except that phenolic foam (Neoma Foam, manufactured by Asahi Kasei Construction Materials Co., Ltd.) was pulverized with the face material still laminated to produce phenolic resin foam powder. In this case, the decomposition rate of the phenolic resin foam was 99.4%. The proportion of phenolic resin foam in the pulverized powder of phenolic resin foam with face material to be thermally decomposed as recycled material was 97.1% by weight.
[0095] Example 6 A phenolic resin foam was obtained in the same manner as in Example 1, except that the pulverization time for producing the phenolic resin foam powder was 30 minutes, the average particle size was 62 μm, and the decomposition time was 60 minutes.
[0096] Comparative Example 1 A phenolic resin foam was obtained in the same manner as in Example 1, except that the amount of the decomposition product added was 22.0 parts by mass relative to 100 parts by mass of the phenolic resin.
[0097] Comparative Example 2 A phenolic resin foam was thermally decomposed in the same manner as in Example 1, except that the decomposition temperature of the decomposition product was 250°C and the pressure was 2.3 MPa. Since the decomposition of the phenolic resin foam as a recycled raw material did not progress, the viscosity of the phenolic resin to which the decomposition product was added increased, and a good phenolic resin foam could not be obtained.
[0098] (Comparative Example 3) A phenolic resin foam was obtained in the same manner as in Example 1, except that the amount of phenol used in the thermal decomposition of the phenolic resin foam as the recycled raw material was 1,240 g, the decomposition temperature was 380°C, the pressure was 0.6 MPa, and the decomposition time was 10 minutes.
[0099] (Comparative Example 4) The phenolic resin foam as the recycled raw material was subjected to decomposition treatment by extruding it using a co-rotating twin-screw extruder (40φ, L / D=50, manufactured by Technovel Co., Ltd.) set at 300° C. The solvent volatilized during extrusion, and a decomposed product could not be obtained.
[0100] Comparative Example 5 A phenolic resin foam was obtained in the same manner as in Example 1, except that the decomposition product was not added.
[0101] The decomposition rates and gas chromatography-mass spectrometry were performed on the decomposition products of Examples 1 to 6 and Comparative Examples 1 to 5, and the thermal conductivity, density, closed cell ratio, and pyrolysis gas chromatography-mass spectrometry were measured on the phenolic resin foams. The results are shown in Table 1. Table 1 also shows a summary of the decomposition treatment conditions and decomposition rates of the phenolic resin foam powders.
[0102]
Claims
1. A phenolic resin foam, in which, when the phenolic resin foam is subjected to pyrolysis gas chromatography mass spectrometry under heating conditions of 600°C, the ratio [A] / [B] is 2.0 or more and 15 or less, where [A] is the area value of the signal of structural formula (A) and [B] is the area value of the signal of structural formula (B).
2. The phenolic resin foam according to claim 1, having a thermal conductivity of 0.016 W / (m·K) or more and 0.026 W / (m·K) or less.
3. The phenolic resin foam according to claim 1 or 2, having a closed cell rate of 85% or more.
4. Density is 20 kg / m 3 More than 70kg / m 3 The phenolic resin foam according to claim 1 or 2, wherein:
5. A method for thermal decomposition of phenolic resin foam, comprising heating and pressurizing the phenolic resin foam in a solution of a mononuclear phenolic compound or a water / mononuclear phenolic compound under conditions of 260°C to 370°C, 1.5 MPa to 20 MPa, and for 60 minutes to 240 minutes, to obtain a decomposition product with a decomposition rate of 95% or more.
6. A product obtained by thermal decomposition of phenolic resin foam containing 0.01% or more and 4.0% or less of xanthene.
7. A method for producing a phenolic resin foam according to claim 1 or 2, comprising adding the decomposition product according to claim 6 in an amount of 0.1 parts by mass or more and 20.0 parts by mass or less per 100 parts by mass of phenolic resin, followed by foaming and curing.
Citation Information
Patent Citations
Phenolic resin molding material and its production
JP1996269227A
Recycled phenol resin composition
JP2003183475A
Molded item and vacuum heat insulator
JP2005023327A
Phenolic resin foam
WO1999011697A1