Method for producing colloidal dispersion

The method of neutralizing carboxyl groups and using phase inversion emulsification in solution polymerization addresses the limitations of existing water-based paint production, achieving stable and high-solid content coatings with reduced organic solvent use and improved water resistance.

WO2024225157A1PCT designated stage expired Publication Date: 2024-10-31NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015384
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for producing water-based paints, such as emulsion polymerization, face limitations in reducing organic solvent use and can result in decreased water resistance and limited resin design freedom, while solution polymerization still requires organic solvents, posing environmental concerns.

Method used

A method involving solution polymerization where a basic compound is added to neutralize carboxyl groups in the resin at controlled temperatures, followed by deionized water addition for phase inversion emulsification, achieving a colloidal dispersion with high solid content concentration and excellent dispersion stability without removing organic solvents.

Benefits of technology

This approach reduces organic solvent use, enhances dispersion stability, and improves the water resistance of the coating film, allowing for high-solid content aqueous coatings with reduced environmental impact and odor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-I000002
    Figure JPOXMLDOC01-APPB-I000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This method for producing a colloidal dispersion comprises: a step in which a monomer mixture including a carboxylated, ethylenically unsaturated monomer (a) is dropped into a reactive solvent (x) having one glycidyl group, at a temperature of 50-180°C to obtain a varnish including a first resin (A); and a step in which a basic compound is added to the varnish at a temperature of 70-98°C to neutralize the carboxyl groups remaining in the first resin (A) and then deionized water is further introduced to cause phase-inversion emulsification and obtain a colloidal dispersion containing particles of the neutralized first resin (A). The varnish has a solid concentration of 85 mass % or higher, the first resin (A) contained in the varnish has a weight-average molecular weight of 13,000-80,000, and the particles of the neutralized first resin (A) have an average particle diameter of 20-200 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing colloidal dispersions

[0001] The present invention relates to a method for producing a colloidal dispersion.

[0002] In recent years, environmental pollution has become a serious problem, leading to stricter international regulations on organic solvent emissions. In the paint industry, too, there has been a shift from traditional organic solvent-based paints to water-based paints. In particular, the conversion of automotive paints to water-based paints is considered to be highly effective in reducing organic solvents. Water-based resins are blended into water-based paints. One method for converting resins to water-based paints is emulsion polymerization using an emulsifier. Emulsion polymerization is simple and does not require organic solvents, making it extremely effective in reducing the use of organic solvents. However, because this method uses water as a solvent, the raw material monomers that can be used are limited, limiting the flexibility of resin design. Furthermore, because emulsion polymerization requires an emulsifier, paint films using the resulting resins tend to have reduced water resistance.

[0003] Therefore, a method has been proposed in which a resin is polymerized in an organic solvent and then the resin is made aqueous (indirect emulsification method).For example, in Patent Documents 1 and 2, a resin is polymerized in an organic solvent (solution polymerization), the organic solvent is removed by distillation under reduced pressure, and then the resin is neutralized to obtain an emulsion.

[0004] JP 8-199114 A JP 2018-2900 A

[0005] However, since an organic solvent is used during solution polymerization, there remains a problem in terms of reducing the use of organic solvents.

[0006] An object of the present invention is to provide a method for producing a colloidal dispersion that has excellent dispersion stability while reducing the use of organic solvents.

[0007] In order to solve the above problems, the present invention provides the following aspects: [1] A method for producing a colloidal dispersion, comprising: a step of dropping a monomer mixture containing a carboxyl group-containing ethylenically unsaturated monomer (a) into a reactive solvent (x) having one glycidyl group at a temperature of 50°C to 180°C to obtain a varnish containing a first resin (A); and a step of adding a basic compound to the varnish at a temperature of 70°C to 98°C to neutralize any remaining carboxyl groups in the first resin (A), and then adding deionized water to perform phase inversion emulsification to obtain a colloidal dispersion containing particles of the neutralized first resin (A), wherein the solids concentration of the varnish is 85% by mass or more, the weight-average molecular weight of the first resin (A) contained in the varnish is 13,000 to 80,000, and the average particle size of the particles of the neutralized first resin (A) is 20 to 200 nm. [2] A method for producing the colloidal dispersion of the above [1], which does not include a step of removing the organic solvent. [3] A method for producing the colloidal dispersion of the above [1] or [2], wherein the average particle size of the particles of the neutralized first resin (A) is 20 nm or more and 150 nm or less. [4] A method for producing the colloidal dispersion of any of the above [1] to [3], wherein the mass of the reactive solvent (x) used in the step of obtaining a varnish is 20 parts by mass or more and 60 parts by mass or less relative to 100 parts by mass of the varnish. [5] The method for producing a colloidal dispersion according to any one of [1] to [4] above, wherein the reactive solvent (x) further has a hydrophobic group, and the step of obtaining the varnish comprises: a first step of adding dropwise a first monomer mixture containing a first carboxy group-containing ethylenically unsaturated monomer (a1) into the reactive solvent (x) at a temperature of 130°C or higher and 180°C or lower to synthesize a hydrophobic resin (A1) and obtain a liquid material containing the hydrophobic resin (A1); and a second step of adding dropwise a second monomer mixture containing a second carboxy group-containing ethylenically unsaturated monomer (a2) into the liquid material at a temperature of 70°C or higher and 180°C or lower to synthesize a carboxy group-containing resin (A2) and obtain the varnish containing the first resin (A) having the hydrophobic resin (A1) and the carboxy group-containing resin (A2).[6] The method for producing a colloidal dispersion according to [5] above, wherein the reactive solvent (x) has a linear or branched alkyl group having 5 to 24 carbon atoms as the hydrophobic group. [7] The method for producing a colloidal dispersion according to any of [1] to [4] above, wherein the step of obtaining a varnish comprises: adding dropwise the monomer mixture containing the carboxy group-containing ethylenically unsaturated monomer (a) into the reactive solvent (x) at a temperature of 50°C or higher and lower than 130°C to polymerize the monomer mixture to obtain a precursor of the first resin (A); and raising the temperature to 130°C or higher and 180°C or lower to react the reactive solvent (x) with the precursor to obtain a varnish containing the first resin (A). [8] The method for producing a colloidal dispersion according to [1] to [7] above, wherein the solubility parameter of particles of the first resin (A) is 10.0 or higher and 11.3 or lower.

[0008] According to the present invention, there is provided a method for producing a colloidal dispersion that has excellent dispersion stability while reducing the amount of organic solvent used.

[0009] The method for producing a colloidal dispersion according to the present disclosure includes the steps of: adding dropwise, at a temperature of 50°C or higher and 180°C or lower, a monomer mixture containing a carboxy group-containing ethylenically unsaturated monomer (a) into a reactive solvent (x) having one glycidyl group, to obtain a varnish containing a first resin (A); and adding, at a temperature of 70°C or higher and 98°C or lower, a basic compound to the varnish to neutralize any remaining carboxy groups in the first resin (A), and then adding deionized water to perform phase inversion emulsification to obtain a colloidal dispersion containing particles of the neutralized first resin (A).

[0010] In solution polymerization, raw monomers are usually added dropwise to a large amount of organic solvent to control (remove) the heat generated by the polymerization reaction of the raw monomers. The organic solvent is also an important component for ensuring the polymerization reaction proceeds uniformly. On the other hand, organic solvent is not an essential component for colloidal dispersions and water-based paints. A process to remove most of the organic solvent is usually carried out before preparing water-based paints.

[0011] By using the reactive solvent (x), it is possible to control the reaction heat and carry out a uniform reaction while reducing the amount of organic solvent used, and as a result, it is possible to increase the solids concentration of the varnish.

[0012] Since the solids concentration of the varnish is 85% by mass or more, i.e., the organic solvent content is less than 15% by mass, the colloidal dispersion can be produced without removing the organic solvent. That is, the step of removing the organic solvent can be omitted in the production of the colloidal dispersion, thereby reducing the environmental load. Furthermore, since the amount of organic solvent used is small, the odor of the colloidal dispersion can also be reduced.

[0013] The solid content of the varnish is calculated from the residue when the varnish is heated at 150°C.

[0014] The weight-average molecular weight of the first resin (A) contained in the varnish is 13,000 or more and 80,000 or less. If the weight-average molecular weight of the first resin (A) is less than 13,000, the dispersion stability of the particles of the first resin (A) in the colloidal dispersion decreases, and the coating strength decreases. If the weight-average molecular weight of the first resin (A) exceeds 80,000, the viscosity of the varnish increases.

[0015] The neutralized particles of the first resin (A) (hereinafter sometimes simply referred to as "resin particles") have an average particle size of 20 nm or more and 200 nm or less. If the average particle size of the neutralized resin particles exceeds 200 nm, they tend to settle and have poor dispersion stability. Although a smaller average particle size of the neutralized resin particles is desirable, the lower limit may be 20 nm.

[0016] The average particle size of the neutralized resin particles is the 50% average particle size (D50) in the volume-based particle size distribution measured using a laser diffraction / scattering particle size distribution measuring device.

[0017] In the present disclosure, the term "colloidal dispersion" refers to an aqueous dispersion containing dispersed neutralized resin particles, and includes the neutralized resin particles as the dispersoid and deionized water as the dispersion medium.

[0018] The step of removing the organic solvent refers to intentionally removing the organic solvent from the reaction system. The ability to omit the step of removing the organic solvent means that the operation of intentionally removing the organic solvent from the reaction system can be omitted. Examples of methods for intentionally removing the solvent include atmospheric distillation and reduced-pressure distillation. Reduced-pressure distillation is generally used in terms of solvent removability. In reduced-pressure distillation, for example, distillation is carried out under a reduced pressure of 0.05 Pa or more but less than 0.1 Pa, at a temperature of 30°C or more and 200°C or less, for 10 minutes to 200 minutes. In the present disclosure, a colloidal dispersion can be obtained without, for example, performing such reduced-pressure distillation during the period from the start of varnish production to the preparation of the colloidal dispersion.

[0019] Because the resin particles have excellent dispersion stability, a colloidal dispersion can be obtained with a small amount of deionized water. In other words, the resulting colloidal dispersion has a high solids concentration. When preparing an aqueous coating composition using the colloidal dispersion, there is no need to add additional solvent (water) (or the amount of solvent added can be reduced), and an aqueous coating composition with a high solids concentration can be obtained. As a result, a coating film without sagging can be obtained.

[0020] Resin particles have relatively high hydrophobicity. Therefore, colloidal dispersions can disperse hydrophobic resins well. A hydrophobic resin is, for example, a resin whose solubility parameter (SP value) measured by the method described below is 9.5 or more (typically 10.0 or more) and 12.0 or less. The type of hydrophobic resin is not particularly limited. Examples of hydrophobic resins include melamine resins, polyester resins, urethane resins, epoxy resins, and acrylic resins, each having an SP value of 9.5 or more and 12.0 or less. Hereinafter, the ability to disperse other resins will be referred to as dispersibility.

[0021] Colloidal dispersions have the ability to maintain a dispersed state over a long period of time in addition to their initial dispersion performance (hereinafter referred to as dispersion stability performance).

[0022] The smaller the average particle size of the neutralized resin particles contained in the colloidal dispersion, the higher the dispersibility and dispersion stability of the colloidal dispersion. From the viewpoint of dispersibility and dispersion stability, the average particle size of the neutralized resin particles may be 20 nm or more and 150 nm or less.

[0023] The SP value of the resin particles may be 10.0 or more and 11.3 or less. A colloidal dispersion containing resin particles with an SP value of 10.0 or more and 11.3 or less exhibits higher dispersion performance and dispersion stability performance. The SP value of the resin particles may be 10.2 or more, 10.4 or more, or 10.6 or more. The SP value of the resin particles may be 11.2 or less, or 11.0 or less.

[0024] A colloidal dispersion containing resin particles having an SP value of 10.0 to 11.3 and an average particle size of 20 to 150 nm exhibits particularly high dispersion performance and dispersion stability. The SP value corresponds to the resin particles before neutralization.

[0025] Colloidal dispersions contain neutralized resin particles. In neutralized resin particles, many of the neutralized carboxyl groups are present near the surface of the resin particles due to their high hydrophilicity, while unneutralized carboxyl groups may exist inside the resin particles. Therefore, the interior of the resin particles is hydrophobic. Colloidal dispersions can disperse hydrophobic resins by incorporating them into the resin particles. In other words, the dispersion performance and dispersion stability of hydrophobic resins are affected by the resin components inside the resin particles that do not contain neutralized carboxyl groups. Colloidal dispersions exhibit dispersion performance and dispersion stability of hydrophobic resins because they contain resin particles with hydrophobic portions that do not contain neutralized carboxyl groups.

[0026] The SP value is an abbreviation for solubility parameter, and is a measure of solubility. The larger the SP value, the higher the polarity, and conversely, the smaller the SP value, the lower the polarity.

[0027] For example, the SP value can be measured by the following method [Reference: SUH, CLARKE, J. P. S. A-1, 5, 1671-1681 (1967)]. Specifically, a colloidal dispersion (solid mass 0.5 g) is weighed into a 100 ml glass beaker and heated at 150°C for 1 hour to remove the organic solvent and water. Then, 10 ml of acetone is added using a volumetric pipette, and the resin particles are completely dissolved using a magnetic stirrer to obtain a sample. A poor solvent is added dropwise to this sample using a 50 ml burette at a measurement temperature of 20°C, and the point at which turbidity occurs is defined as the amount added. Ion-exchanged water is used as a high SP poor solvent, and n-hexane is used as a low SP poor solvent, and the turbidity point is measured for each poor solvent. The SP value δ of an organic solvent is given by the following formula:

[0028] δ=(V ml 1/2 δ ml +V mh 1/2 δ mh ) / (V ml 1/2 +V mh 1/2 ) V m =V 1 V 2 / (φ 1 V 2 +φ 2 V 1 ) δ m =φ 1 δ 1 +φ 2 δ 2 V i : Molar volume of solvent (ml / mol) φ i : Volume fraction of each solvent at the clouding point δ i : SP value of solvent ml: low SP poor solvent mixed system mh: high SP poor solvent mixed system

[0029] The sample used to calculate the SP value is a colloidal dispersion heated at 150°C for 1 hour. This heating removes the basic compound that neutralized the carboxyl groups on the resin particle surface, leaving the resin particles in an unneutralized state. That is, according to the above method, an SP value corresponding to the SP value of the resin particles before neutralization is calculated. The SP value may also be measured directly using the resin particles before neutralization by other methods.

[0030] Dispersion performance is affected by the amount of resin to be dispersed. A colloidal dispersion having a solids concentration of 10% by mass or more and 20% by mass or less can disperse, for example, a hydrophobic resin having a solids concentration of 40% by mass or less.

[0031] (1) Step of Obtaining Varnish A monomer mixture containing a carboxyl group-containing ethylenically unsaturated monomer (a) is added dropwise to a reactive solvent (x) having one glycidyl group at a temperature of 50°C or higher and 180°C or lower.

[0032] In this step, so-called solution polymerization is carried out. Since the reactive solvent (x) also functions as a solvent for the polymerization reaction, the solids concentration of the resulting varnish can be 85% by mass or more, in other words, the amount of organic solvent can be kept below 15% by mass of the varnish. The solids concentration of the varnish can be 87% by mass or more, or even 90% by mass or more.

[0033] In this process, radical polymerization of the monomer mixture and a ring-opening addition reaction between the glycidyl group of the reactive solvent (x) and the carboxy group of the carboxy group-containing monomer (a) proceed. This results in the synthesis of the first resin (A). Because this synthesis is carried out under heating, a varnish containing the first resin (A) in a molten state is obtained. The monomer mixture contains the carboxy group-containing ethylenically unsaturated monomer (a) and other ethylenically unsaturated monomers. The first resin (A) is typically an acrylic resin.

[0034] The process for obtaining the varnish (which can also be referred to as the synthesis process for the first resin (A)) may be carried out in two or more stages. Two embodiments for obtaining the varnish in two or more stages are described below. However, the process for obtaining the varnish in the present disclosure is not limited to these embodiments.

[0035] (1-1) First embodiment of the process for obtaining a varnish This embodiment is suitable for the case where the reactive solvent (x) has a hydrophobic group. In this embodiment, the process for obtaining a varnish includes: a first step of adding a first monomer mixture containing a first carboxyl group-containing ethylenically unsaturated monomer (a1) dropwise into a reactive solvent (x) having one glycidyl group and a hydrophobic group at a temperature of 130°C to 180°C to synthesize a hydrophobic resin (A1) and obtain a liquid product containing the hydrophobic resin (A1); and a second step of adding a second monomer mixture containing a second carboxyl group-containing ethylenically unsaturated monomer (a2) dropwise into the liquid product at a temperature of 70°C to 180°C to synthesize a carboxyl group-containing resin (A2) and obtain a varnish containing the first resin (A) having the hydrophobic resin (A1) and the carboxyl group-containing resin (A2).

[0036] In this embodiment, different raw material monomers can be used for polymerization in each step, which increases the degree of freedom in resin design.

[0037] After the second step, the carboxyl group-containing resin (A2) is hydrophilized by neutralization, and then phase inversion emulsification is carried out to obtain core-shell structured resin particles having a hydrophobic resin (A1) as a core portion and a hydrophilic resin (A2′) as a shell portion.

[0038] The "core portion" and the "shell portion" may or may not be chemically crosslinked. In the present disclosure, the resin particles having a core-shell structure have a hydrophobic resin (A1) inside and a hydrophilic resin (A2') on the outside, and at least a part of the hydrophobic resin (A1) is covered with the hydrophilic resin (A2').

[0039] (1-1-1) First Step In the first step, a first monomer mixture containing a first carboxy group-containing ethylenically unsaturated monomer (a1) is added dropwise to a reactive solvent (x) having one glycidyl group and a hydrophobic group at a temperature of 130° C. to 180° C. The first monomer mixture contains the first carboxy group-containing ethylenically unsaturated monomer (a1) and other ethylenically unsaturated monomers.

[0040] In the first step, a ring-opening addition reaction between the glycidyl group of the reactive solvent (x) and the carboxy group of the first carboxy group-containing monomer (a1) occurs, and a polymerization reaction of the first monomer mixture also occurs. This results in the synthesis of a hydrophobic resin (A1), and a liquid material containing the hydrophobic resin (A1) is obtained. The hydrophobic resin (A1) serves as the base resin for forming the coating film in the aqueous paint.

[0041] (1-1-2) Second Step In the second step, a second monomer mixture containing a second carboxyl group-containing ethylenically unsaturated monomer (a2) is added dropwise to the liquid material at a temperature of 70°C or higher and 180°C or lower. The second monomer mixture contains the second carboxyl group-containing ethylenically unsaturated monomer (a2) and another ethylenically unsaturated monomer. The second step may be carried out at a temperature of 100°C or higher and 180°C or lower.

[0042] In the second step, polymerization of the second monomer mixture mainly proceeds to synthesize a carboxyl group-containing resin (A2). When a basic compound is added in a subsequent step, the carboxyl groups are neutralized, and the carboxyl group-containing resin (A2) is hydrophilized to form a hydrophilic resin (A2'). The hydrophilic resin (A2') acts as a dispersing component for dispersing the first resin (A) in water, reducing the particle size of the resin particles and improving their dispersion stability.

[0043] Following the second step, a polymerization initiator may be added, and aging may be performed by stirring and heating. The aging may be performed, for example, at the same temperature as in the second step for 0.5 hours to 3 hours.

[0044] The weight average molecular weight of the resulting first resin (A) is 13,000 or more and 80,000 or less. The weight average molecular weight of the first resin (A) may be 15,000 or more, or 16,000 or more. The weight average molecular weight of the first resin (A) may be 60,000 or less, or 45,000 or less.

[0045] The weight-average molecular weight of the first resin (A) can be adjusted, for example, by the polymerization conditions in the first and second steps, the type of raw material monomer, the amount and type of polymerization initiator, and the aging conditions. For example, if the time of the second step and / or aging is extended, the weight-average molecular weight of the first resin (A) tends to increase, whereas if the aging time is shortened, the weight-average molecular weight of the first resin (A) tends to decrease.

[0046] The glass transition temperature (Tg) of the obtained first resin (A) (in this case, containing a hydrophobic resin (A1) and a hydrophilic resin (A2')) may be, for example, 0°C or higher and 50°C or lower. When the Tg of the first resin (A) is 50°C or lower, an increase in the viscosity of the system during neutralization and phase inversion emulsification is suppressed, and a decrease in productivity is suppressed. When the Tg of the first resin (A) is 0°C or higher, dispersion stability can be further improved. The Tg of the first resin (A) may be 5°C or higher, or 10°C or higher. The Tg of the first resin (A) may be 40°C or lower, or 30°C or lower.

[0047] The Tg may be calculated from the type and amount of raw material monomers, or may be measured by a differential scanning calorimeter (DSC). Since the Tg of the first resin (A) is approximately the same as the Tg of the resin particles, the Tg of the resin particles may be regarded as the Tg of the first resin (A). The Tg of the resin particles is calculated or measured by the above-mentioned method using the residue when the colloidal dispersion is heated at 150°C.

[0048] (First and Second Monomer Mixtures) The hydrophobic resin (A1) and the carboxyl group-containing resin (A2) are synthesized using a combination of one or more raw material monomers, each of which has an ethylenically unsaturated group.

[0049] The raw material monomers used in the synthesis of the hydrophobic resin (A1) and the carboxyl group-containing resin (A2) may be the same or different. The combinations of raw material monomers used in the synthesis of the hydrophobic resin (A1) and the carboxyl group-containing resin (A2) may be the same or different. The blending ratios of the multiple raw material monomers used in the synthesis of the hydrophobic resin (A1) and the carboxyl group-containing resin (A2) may be the same or different.

[0050] <<First and Second Carboxy Group-Containing Monomers (a1) and (a2)>> Examples of the first and second carboxy group-containing monomers (a1) and (a2) include (meth)acrylic acid, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, and β-carboxyethyl acrylate. These may be used alone or in combination of two or more. (Meth)acrylic acid refers to acrylic acid and methacrylic acid.

[0051] The first carboxy group-containing monomer (a1) and the second carboxy group-containing monomer (a2) may be the same or different.

[0052] <<Other Ethylenically Unsaturated Monomers>> Each monomer mixture may contain other ethylenically unsaturated monomers in addition to the carboxy group-containing monomer.

[0053] Examples of other ethylenically unsaturated monomers include hydroxyl group-containing ethylenically unsaturated monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methallyl alcohol, and adducts of these with ε-caprolactone; esters of the above carboxyl group-containing monomers; styrenes such as styrene and α-methylstyrene; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-, i-, and t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ... methyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, methyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, methyl (meth)acrylate, methyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, methyl (meth)acrylate, methyl (meth)acrylate, methyl (meth)acrylate, ) Linear aliphatic acrylates such as allyl acrylate and lauryl (meth)acrylate; alicyclic acrylates such as cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate and dihydrodicyclopentadienyl (meth)acrylate; polymerizable amide compounds such as acrylamide and methacrylamide; polymerizable aromatic compounds, polymerizable nitriles, polymerizable alkylene oxide compounds, polyfunctional vinyl compounds, polymerizable amine compounds, α-olefins, dienes, polymerizable carbonyl compounds and polymerizable alkoxysilyl compounds. These may be used alone or in combination of two or more.

[0054] In particular, each monomer mixture may contain a (meth)acrylic acid alicyclic ester together with a carboxy group-containing monomer. This increases the hydrophobicity of the first resin (A), thereby improving the water resistance of the resulting coating film. Each monomer mixture may contain a hydroxyl group-containing ethylenically unsaturated monomer (hereinafter sometimes referred to as a hydroxyl group-containing monomer) together with the carboxy group-containing monomer. Because the hydroxyl group can serve as the starting point for the curing reaction, the use of a hydroxyl group-containing monomer tends to increase the hardness of the resulting coating film. Each monomer mixture may contain both a (meth)acrylic acid alicyclic ester and a hydroxyl group-containing monomer together with the carboxy group-containing monomer.

[0055] In order to improve the physical properties of the resulting coating film, the mass of the carboxyl group-containing monomer in the first monomer mixture may be 5 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the first monomer mixture. The mass of the carboxyl group-containing monomer may be 10 parts by mass or more. The mass of the carboxyl group-containing monomer may be 25 parts by mass or less.

[0056] In the first monomer mixture, the mass of the (meth)acrylic acid alicyclic ester may be 5 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the first monomer mixture. The mass of the (meth)acrylic acid alicyclic ester may be 10 parts by mass or more. The mass of the (meth)acrylic acid alicyclic ester may be 35 parts by mass or less.

[0057] In the first monomer mixture, the mass of the hydroxyl group-containing monomer may be 5 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the first monomer mixture. The mass of the hydroxyl group-containing monomer may be 7 parts by mass or more. The mass of the (meth)acrylic acid alicyclic ester may be 25 parts by mass or less.

[0058] In order to improve the dispersibility of the resulting hydrophilic resin (A2'), the mass of the carboxyl group-containing monomer in the second monomer mixture may be 5 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the second monomer mixture. The mass of the carboxyl group-containing monomer may be 10 parts by mass or more. The mass of the carboxyl group-containing monomer may be 25 parts by mass or less.

[0059] In the second monomer mixture, the mass of the (meth)acrylic acid alicyclic ester may be 5 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the second monomer mixture. The mass of the (meth)acrylic acid alicyclic ester may be 7 parts by mass or more. The mass of the (meth)acrylic acid alicyclic ester may be 35 parts by mass or less.

[0060] In the second monomer mixture, the mass of the hydroxyl group-containing monomer may be 5 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the second monomer mixture. The mass of the hydroxyl group-containing monomer may be 10 parts by mass or more. The mass of the (meth)acrylic acid alicyclic ester may be 25 parts by mass or less.

[0061] The first carboxy group-containing monomer (a1), the second carboxy group-containing monomer (a2), and the reactive solvent (x) are mixed, for example, so that the mass ratio of the hydrophobic resin (A1) to the hydrophilic resin (A2′) in the core-shell resin particles (hydrophobic resin (A1):hydrophilic resin (A2′), mass %) is 95:5 to 60:40.

[0062] When the mass proportion of the hydrophilic resin (A2') is 5% or more, the dispersibility of the resin particles in water is further improved, and the storage stability of the aqueous coating composition is improved. When the mass proportion of the hydrophilic resin (A2') is 40% or less, the water resistance of the coating film can be improved. The ratio of the hydrophobic resin (A1) to the hydrophilic resin (A2') may be 90:10 to 70:30, or 85:15 to 75:25.

[0063] (Reactive Solvent (x)) The reactive solvent (x) chemically reacts with the carboxy group-containing monomer (mainly the first carboxy group-containing monomer (a1)) and has low viscosity, and therefore functions as a solvent for the polymerization reaction.

[0064] The viscosity η of the reactive solvent (x), measured by a Brookfield viscometer at 23°C and a rotation speed of 60 rpm, is, for example, 1 mPa·s or more and 50 mPa·s or less. This allows the reactive solvent (x) to function as an excellent solvent. The viscosity η of the reactive solvent (x) may be 2 mPa·s or more, or 5 mPa·s or more. The viscosity η of the reactive solvent (x) may be 35 mPa·s or less, or 20 mPa·s or less.

[0065] The reactive solvent (x) has a boiling point higher than the solution polymerization temperature (in the range of 130°C or higher and 180°C or lower). The boiling point of the reactive solvent (x) is, for example, 130°C or higher and 300°C or lower. The boiling point of the reactive solvent (x) may be 140°C or higher, or 180°C or higher. The boiling point of the reactive solvent (x) may be 290°C or lower, or 280°C or lower.

[0066] Since the reactive solvent (x) has only one glycidyl group, the reaction between the reactive solvents (x) and the crosslinking reaction are suppressed, and the desired hydrophobic resin (A1) can be obtained. The desired hydrophobic resin (A1) has a carbon-carbon bond as the main chain and a hydrophobic group as a side chain.

[0067] The reactive solvent (x) has one glycidyl group and a hydrophobic group. The reactive solvent (x) may be a monocarboxylic acid glycidyl ester. The monocarboxylic acid glycidyl ester is, for example, a compound represented by the following general formula (1): (wherein R is a monovalent organic group).

[0068] R is a monovalent organic group and contains a hydrophobic group. Examples of the hydrophobic group include hydrocarbon groups. A hydrocarbon group is a group containing carbon and hydrogen, and refers to a group obtained by removing one hydrogen atom from a hydrocarbon. Examples of the hydrocarbon group include aliphatic hydrocarbon groups and aromatic hydrocarbons having 1 to 28 carbon atoms. The aliphatic hydrocarbon group may be linear, branched, or cyclic, and may be saturated or unsaturated. The hydrogen bonded to the carbon may be substituted with a halogen atom or the like.

[0069] The hydrophobic group may be a linear or branched alkyl group having 5 to 24 carbon atoms. This allows the first resin (A1) to have a long-chain alkyl group as a side chain. This long alkyl group imparts plasticity to the first resin (A1), thereby reducing the viscosity of the varnish and allowing the polymerization reaction to proceed more uniformly. Furthermore, this improves the mixability of the first resin (A) with other hydrophobic materials (e.g., crosslinkers and pigments) incorporated into the aqueous coating composition, further improving the water resistance of the resulting coating film. The alkyl group may have 7 to 18 carbon atoms or 8 to 15 carbon atoms. The alkyl group may be saturated. The alkyl group may be branched. In particular, R may be a hydrophobic group, and may be a branched, saturated alkyl group having 5 to 24 carbon atoms.

[0070] The amount of reactive solvent (x) used may be, for example, 20 parts by mass or more and 60 parts by mass or less, relative to 100 parts by mass of the total mass of the first monomer mixture, the second monomer mixture, the reactive solvent, and other solvents (hereinafter sometimes referred to as the "total charged amount"). This makes it easy to control the reaction heat and allows the polymerization reaction to proceed uniformly. The amount of reactive solvent (x) used may be 25 parts by mass or more. The amount of reactive solvent (x) used may be 40 parts by mass or less. The total charged amount may be considered to be the same as the mass of the resulting varnish.

[0071] (Polymerization initiator) A polymerization initiator may be used in the first step, the second step, and the aging step. The total amount of the polymerization initiator used is appropriately set, for example, depending on the type and amount of the raw material monomers. The total amount of the polymerization initiator used may be, for example, 0.2 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the total of the first monomer mixture and the second monomer mixture. The amount of the polymerization initiator used may be 0.2 parts by mass or more. The amount of the polymerization initiator used may be 1.5 parts by mass or less.

[0072] Examples of the polymerization initiator include 2,2'-azobisisobutyronitrile, benzoyl peroxide, 2,2-di(t-amylperoxy)butane, di-t-butyl peroxide, di-t-amyl peroxide (DTA), t-butyl peroctoate, and 2,2'-azobis(2-methylbutyronitrile).

[0073] (Organic Solvent) The varnish may contain an organic solvent other than the reactive solvent (x) at a mass ratio of less than 15 mass %. Examples of the other organic solvent include high-boiling point solvents having a boiling point higher than the solution polymerization temperature (in the range of 130°C to 180°C).

[0074] Examples of high-boiling point solvents include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, 3-butoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, ethylene glycol, propylene glycol, glycerin, dimethylcarbitol, butylcarbitol, butyl dicarbitol, butyl cellosolve, 1,4-butanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, diethylene glycol monomethyl ether, and dipropylene glycol monomethyl ether.

[0075] From the viewpoint of reducing environmental impact, it is also desirable for aqueous coating compositions to have low-temperature curing properties. From the viewpoint of low-temperature curing properties, it is desirable for the mass proportion of high-boiling point solvents to be small. The mass proportion of high-boiling point solvents in the varnish may be less than 13 mass%, or may be less than 10 mass%.

[0076] (1-2) Second embodiment of the step of obtaining a varnish In this embodiment, the step of obtaining a varnish includes a step of adding dropwise a monomer mixture containing a carboxy group-containing ethylenically unsaturated monomer (a) into a reactive solvent (x) at a temperature of 50°C or higher and lower than 130°C to polymerize the monomer mixture to obtain a precursor of the first resin (A), and a step of raising the temperature to 130°C or higher and 180°C or lower to react the reactive solvent (x) with the precursor to obtain a varnish containing the first resin (A).

[0077] In this embodiment, the polymerization reaction of the ethylenically unsaturated monomer and the ring-opening reaction are carried out in a stepwise manner, taking advantage of the fact that the ring-opening reaction of the epoxy ring is unlikely to occur at low temperatures. According to this embodiment, even when a highly volatile raw material monomer is used, the polymerization reaction can be reliably carried out, and the first resin (A) can contain a hydrophobic moiety.

[0078] The temperature in the step of obtaining a precursor of the first resin (A) may be 50° C. or higher. The temperature in the step of obtaining a precursor of the first resin (A) may be 110° C. or lower.

[0079] The raw material monomer, reactive solvent (x), polymerization initiator, and organic solvent contained in the monomer mixture may be the same as those exemplified in Embodiment 1. The amount of each component used may be in the same range as in Embodiment 1, with the total mass of the first monomer mixture and the second monomer mixture in Embodiment 1 being read as the mass of the monomer mixture in this embodiment.

[0080] (2) Neutralization and Phase Inversion Emulsification Step First, a basic compound is added to the varnish at a temperature of 70°C to 98°C to neutralize the remaining carboxy groups in the first resin (A). This makes the first resin (A) water-dispersible. Then, deionized water is added to the varnish at a temperature of 70°C to 98°C to cause phase inversion emulsification. This produces a colloidal dispersion containing resin particles.

[0081] When the temperature of the varnish during neutralization and phase inversion emulsification is 70°C or higher and 98°C or lower, the first resin (A) can be sufficiently softened while suppressing the volatilization of the basic compound and deionized water. This makes it easier for the first resin (A) to be finely dispersed in deionized water. In particular, when the temperature of the varnish is equal to or higher than the Tg of the first resin (A), the first resin (A) is even more easily finely dispersed.

[0082] The average particle size of the resin particles formed by phase inversion emulsification is 20 nm or more and 200 nm or less. The average particle size of the resin particles may be 180 nm or less, 160 nm or less, or 150 nm or less. The average particle size of the resin particles may be 25 nm or more, or 30 nm or more. In one embodiment, the average particle size of the resin particles may be 20 nm or more and 150 nm or less.

[0083] The phase inversion emulsification is carried out, for example, by stirring a mixture of the varnish containing the neutralized first resin (A) and deionized water. Stirring can reduce the average particle size of the resin particles.

[0084] The average particle size of the resin particles can be adjusted by, for example, the conditions of radical polymerization, the type of raw material monomer, and the stirring conditions during phase inversion emulsification. For example, a lower neutralization rate tends to increase the average particle size of the resin particles, while a higher neutralization rate tends to decrease the average particle size of the resin particles.

[0085] The solid content concentration of the colloidal dispersion is, for example, 30% by mass or more and 45% by mass or less. The solid content concentration of the colloidal dispersion may be 34% by mass or more, or 36% by mass or more. The solid content concentration of the colloidal dispersion may be 42% by mass or less, or 40% by mass or less.

[0086] The solid content concentration of the colloidal dispersion is calculated from the residue when the colloidal dispersion is heated at 150°C.

[0087] The viscosity η of the colloidal dispersion measured by a Brookfield viscometer at 23°C and a rotation speed of 60 rpm 60 is, for example, 50 mPa·s or more and 700 mPa·s or less. This allows the colloidal dispersion to be blended into the aqueous coating composition without diluting it with a solvent. 60 The viscosity η of the colloidal dispersion may be 80 mPa·s or more, or may be 100 mPa·s or more. 60may be 630 mPa·s or less, may be 600 mPa·s or less, may be 500 mPa·s or less, may be 300 mPa·s or less, may be 295 mPa·s or less, or may be 290 mPa·s or less.

[0088] Viscosity η 60 is measured using a Brookfield viscometer (for example, trade name: Viscometer VT-06, No. 2 rotor, manufactured by Rion Co., Ltd.) under conditions of 23°C and a rotation speed of 60 rpm, in accordance with JIS-Z8803 "Methods for measuring viscosity of liquids, 9. Viscosity measurement method using a single cylindrical rotational viscometer."

[0089] (Basic Compound) Examples of the basic compound include secondary aliphatic amine compounds such as diethylamine, di-n-propylamine, diisopropylamine, diisobutylamine, di-n-butylamine, di-sec-butylamine, diamylamine, N-ethyl-1,2-dimethylpropylamine, N-methylhexylamine, di-n-octylamine, and diallylamine; tertiary aliphatic amine compounds such as triethylamine, tributylamine, triallylamine, N,N-dimethylethanolamine, N-methyldiallylamine, and N,N-dimethylallylamine; secondary cyclic amine compounds such as piperidine, 2-pipecoline, 3-pipecoline, 4-pipecoline, 2,4-lupetidine, 2,6-lupetidine, 3,5-lupetidine, and 3-piperidinemethanol; tertiary cyclic amine compounds such as N-methylpiperidine, N-methylpiperazine, and N-methylmorpholine; and aromatic amine compounds such as pyridine and 4-ethylpyridine.

[0090] The basic compound is added in an amount such that the neutralization rate of the carboxyl groups in the first resin (A) is 70% or more and 100% or less. When the neutralization rate is within this range, the water dispersibility of the first resin (A) is improved, and the average particle size can be smaller. The neutralization rate may be 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more.

[0091] The neutralization rate is equivalent to the amount of the basic compound used relative to the carboxyl group, and is calculated by the following formula:

[0092] The acid value of the first resin (A) may be, for example, 10 mgKOH / g or more and 50 mgKOH / g or less. The acid value of the first resin (A) may be 15 mgKOH / g or more, or 20 mgKOH / g or more. The acid value of the first resin (A) may be 40 mgKOH / g or less, or 35 mgKOH / g or less.

[0093] The acid value of the first resin (A) may be calculated from the composition of the raw material monomers in accordance with JIS regulations, or may be determined by neutralization titration using an aqueous potassium hydroxide solution in accordance with JIS K 0070. Since the acid value of the first resin (A) is approximately the same as the acid value of the resin particles, the acid value of the resin particles may be regarded as the acid value of the first resin (A). The acid value of the resin particles can be calculated by dividing the acid value determined by the neutralization titration method using a colloidal dispersion by the solids concentration of the colloidal dispersion.

[0094] (Aqueous Coating Composition) The colloidal dispersion obtained by the method according to the present disclosure is suitable for use in preparing an aqueous coating composition. The aqueous coating composition contains water as a solvent in an amount of 50 mass % or more (particularly 80 mass % or more) of the total solvent.

[0095] The colloidal dispersion can be incorporated into an aqueous coating composition as a film-forming resin or as a pigment dispersant. When the resin particles have hydroxyl groups (when the monomer mixture contains a hydroxyl-containing monomer), they can react with the crosslinker contained in the aqueous coating composition. Therefore, the use of the colloidal dispersion obtained by the present disclosure can improve various physical properties of the resulting coating film.

[0096] The aqueous coating composition contains, for example, the colloidal dispersion, a crosslinker, a pigment, and, if necessary, deionized water and various additives. The aqueous coating composition may contain, if necessary, a conventionally known film-forming resin and / or a pigment dispersant. Examples of the pigment include color pigments, luster pigments, and extender pigments. Examples of the additives include surface conditioners, viscosity control agents, thickeners, antioxidants, ultraviolet inhibitors, and defoamers.

[0097] The present invention will be described in more detail with reference to the following examples, but is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0098] Example 1 (1) First Step (Preparation of Hydrophobic Acrylic Resin (A1)) A reaction vessel equipped with a stirrer, a temperature controller, a condenser, and a dropping device was charged with 30 parts of a reactive solvent (CAE, a glycidyl ester of a monocarboxylic acid having a branched alkyl group having 9 carbon atoms, trade name: Cardurer E10P, manufactured by Hexion Corporation, viscosity 7 mPa s, boiling point 251 to 278°C), and the mixture was heated to 165°C with stirring and refluxed. Separately, a mixture of 9.47 parts of acrylic acid (AA), 5.8 parts of 2-hydroxyethyl methacrylate (HEMA), 11.6 parts of cyclohexyl methacrylate (CHMA), 7.5 parts of n-butyl acrylate (NBA), 16.9 parts of styrene (ST), 0.28 parts of a polymerization initiator (DTA, trade name: Luperox DTA, manufactured by Arkema Yoshitomi Co., Ltd.), and 6.5 parts of a high-boiling point solvent (dipropylene glycol monomethyl ether (DPM)) was prepared. This mixture was added dropwise to the reaction vessel at 165°C over 3.5 hours to carry out a polymerization reaction and a ring-opening addition reaction.

[0099] (2) Second step (preparation of carboxyl group-containing acrylic resin (A2)) and aging Separately, a mixture of 3.43 parts of AA, 3.8 parts of HEMA, 2.7 parts of CHMA, 2.9 parts of NBA, 5.8 parts of ST, 0.11 parts of polymerization initiator (Luperox DTA), and 2.4 parts of high-boiling solvent (DPM) was prepared. This mixture was added dropwise to the reaction vessel over 1 hour at 165 ° C. with stirring, and allowed to polymerize for 1 hour. Furthermore, a mixture of 0.1 parts of polymerization initiator (Luperox DTA) and 0.1 parts of high-boiling solvent (DPM) was added to the reaction vessel, and the mixture was allowed to polymerize for 1 hour at 165 ° C. with stirring.

[0100] In this way, a varnish containing a hydrophobic resin (A1) and an acrylic resin (A) having a carboxyl group-containing resin (A2) and having a solids concentration of 91% by mass was obtained. The weight-average molecular weight of the obtained acrylic resin (A) was 32,000.

[0101] (Weight-Average Molecular Weight) The weight-average molecular weight was measured using a GPC apparatus "HLC8220GPC" (trade name, manufactured by Tosoh Corporation) and four columns, "Shodex KF-606M" and "Shodex KF-603" (both trade names, manufactured by Showa Denko K.K.), under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 0.6 cc / min, and detector: RI.

[0102] (3) Neutralization and Phase Inversion Emulsification: A basic compound (dimethylethanolamine, DMEA) was added to the varnish at a ratio of 5.33 parts per 100 parts of acrylic resin at 80°C, and the mixture was stirred for 15 minutes. The neutralization rate of the carboxyl group was adjusted to 90%. Subsequently, 150 parts of deionized water was added dropwise to the neutralized varnish at 80°C while stirring, to obtain a milky white colloidal dispersion.

[0103] The solid concentration of the colloidal dispersion was 38% by mass, and the viscosity was η 60The viscosity was 130 mPa s and the pH was 8.2. The acrylic resin particles contained in the colloidal dispersion were expected to have a core-shell structure, with an average particle size of 85 nm, a Tg of 20°C, and an acid value of 34 mgKOH / g. The Tg and acid value of the acrylic resin particles may be considered to be the Tg and acid value of the first resin (A).

[0104] (Acid Value (AV)) 1 g of the colloidal dispersion was dissolved in 50 ml of tetrahydrofuran (THF), and the acid value of the colloidal dispersion was determined by neutralization titration using an aqueous potassium hydroxide solution in accordance with JIS K 0070. Next, the acid value was divided by the solid content concentration of the colloidal dispersion to calculate the solid content acid value of the resin particles, which was defined as the acid value of the acrylic resin (A).

[0105] (Glass Transition Temperature (Tg)) The colloidal dispersion was heated at 150°C for 1 hour to obtain a heating residue. Data was obtained using a DSC (Differential Scanning Calorimeter) manufactured by Seiko Instruments, Inc. at a heating rate of 10°C / min, and the intersection of the baseline and the tangent to the inflection point was taken as the Tg. This Tg was taken as the Tg of the acrylic resin (A).

[0106] (SP Value) The SP value of the neutralized resin particles was calculated as described above.

[0107] Examples 2-11, Comparative Examples 1 and 2 Colloidal dispersions were obtained in the same manner as in Example 1, except that the types of raw material monomers, neutralization rates, etc. were changed as shown in Tables 1 and 2.

[0108]

[0109]

[0110] Comparative Example 3 A dispersion containing particles of a core-shell type acrylic resin (B) was obtained as follows without using a reactive solvent.

[0111] (a) Preparation of Macromonomer (Core Portion) A reaction vessel equipped with a stirrer, temperature controller, condenser, and dropping device was charged with 23.7 parts of methyl isobutyl ketone (MIBK) and heated to 110°C. Subsequently, the raw material monomers listed in Table 3 and a solution of 8.3 parts of tert-butylperoxy-2-ethylhexanate dissolved in 4.8 parts of MIBK were added dropwise in parallel at a constant rate over 90 minutes. After maintaining the reaction vessel at 110°C for 30 minutes, a solution of 0.3 parts of tert-butylperoxy-2-ethylhexanate dissolved in 3.2 parts of MIBK was added dropwise at a constant rate over 30 minutes. Subsequently, the mixture was stirred at 110°C for 60 minutes. While maintaining the reaction vessel at 110°C, 0.8 parts of methacrylic anhydride was added and the mixture was maintained for 2 hours. The mixture was then cooled to 60°C to obtain a macromonomer.

[0112] (b) Preparation of Core-Shell Acrylic Resin (B) Separately, 39.7 parts of MIBK was charged into a reactor equipped with a cooling and heating device and heated to 110° C. Thereafter, the raw material monomers shown in Table 3 and a solution prepared by dissolving 2.1 parts of tert-butylperoxy-2-ethylhexanate in 8.6 parts of MIBK were added dropwise at a constant rate in parallel over 90 minutes.

[0113] After the reaction vessel was maintained at 110°C for 30 minutes, a solution of 0.3 parts of tert-butylperoxy-2-ethylhexanate in 2.9 parts of MIBK was added dropwise at a constant rate over 30 minutes. Subsequently, the mixture was stirred at 110°C for 60 minutes, and then cooled to 70°C.

[0114] In this way, a varnish v1 containing a core-shell acrylic resin (B) and having a solids concentration of 55% by mass was obtained. The weight average molecular weight of the obtained acrylic resin (B) was 15,000.

[0115] (c) Solvent Removal From varnish v1 (181.8 parts), 81.8 parts of MIBK was distilled off under reduced pressure. 15 parts of DPM was then added to obtain varnish v2. The reduced pressure distillation was carried out at approximately 5 kPa and a temperature of 90°C for 120 minutes.

[0116] (d) Neutralization and Phase Inversion Emulsification DMEA was added to varnish v2 at a ratio of 2.53 parts per 100 parts of acrylic resin (B) at 80°C, and the mixture was stirred for 15 minutes (neutralization rate 75%). Subsequently, 155 parts of deionized water was added dropwise to the neutralized varnish at 80°C while stirring, to prepare a milky white colloidal dispersion. The resin solids content of the resulting dispersion of acrylic resin (B) was 36% by mass.

[0117] The conditions for (c) solvent removal and (d) neutralization and phase inversion emulsification are shown in Table 4.

[0118]

[0119]

[0120] [Evaluation] The colloidal dispersions were evaluated as follows. The results are shown in Table 6.

[0121] (1) Dispersion Stability The colloidal dispersion was allowed to stand for one month at a temperature of 40° C. The presence or absence of sedimentation was visually observed and evaluated according to the following criteria.

[0122] A: No settling after one month. B: No settling after one week. C: Settling was observed after 24 hours. D: Settling was observed after one hour.

[0123] (2) Odor The presence or absence of odor of the colloidal dispersion was evaluated by sensory evaluation according to the following criteria: None: No irritating odor that stings the nose, almost no odor Present: Smell of thinner and / or irritating odor

[0124] (3) Dispersibility of Colloidal Dispersion for Hydrophobic Resin Sample Preparation A hydrophobic melamine resin (SP value: 10.1, product name: Cymel 250, manufactured by Allnex), a surfactant (acetylene glycol-based, product name: Surfynol 465, manufactured by Evonik Industries), and an organic solvent (isoparaffin, product name: Merveille 30, manufactured by Idemitsu Kosan Co., Ltd.) were mixed to a solid content ratio as shown in the table below. Next, the colloidal dispersion was added while stirring with a disperser, and the mixture was further stirred for 10 minutes. Next, pure water was added while stirring with a disperser so that the total amount became 100% by mass, and the mixture was further stirred for 3 minutes. In this manner, a sample was prepared.

[0125]

[0126] Initial Dispersion Performance The above sample was diluted with water to a solids concentration of 0.01% by mass. The particle size of the resin contained in the diluted sample was measured three times using dynamic light scattering (instrument name: ELSZ-2000ZS, Otsuka Electronics), and the cumulant diameter was obtained by cumulant analysis. The obtained cumulant diameters were averaged to determine the dispersion diameter of the melamine resin. If the dispersion diameter is 300 nm or less, the colloidal dispersion can be said to have excellent initial dispersion performance.

[0127] Dispersion Stability The above sample was placed in a transparent bottle and allowed to stand at room temperature. After one day and five days, the bottle was tilted and visually inspected for the presence of precipitate at the bottom. If no precipitate was observed after five days, the colloidal dispersion was deemed to have excellent dispersion stability.

[0128] (Evaluation criteria) A: No settling even after 5 days B: Settling can be confirmed after 5 days C: Settling can be confirmed after 1 day D: The sample had no fluidity during preparation, and dispersion could not be confirmed

[0129]

[0130] The production method of the present disclosure can obtain a colloidal dispersion with excellent dispersion stability while reducing the use of organic solvents. The obtained colloidal dispersion is suitable for use in an aqueous coating composition.

[0131] This application claims priority based on Japanese Patent Application No. 2023-074538, filed on April 28, 2023, the entire contents of which are incorporated herein by reference.

Claims

1. A method for producing a colloidal dispersion, comprising: a step of dropping a monomer mixture containing a carboxy group-containing ethylenically unsaturated monomer (a) into a reactive solvent (x) having one glycidyl group at a temperature of 50°C or higher and 180°C or lower to obtain a varnish containing a first resin (A); and a step of adding a basic compound to the varnish at a temperature of 70°C or higher and 98°C or lower to neutralize the carboxy groups remaining in the first resin (A), and then adding deionized water to perform phase inversion emulsification to obtain a colloidal dispersion containing particles of the neutralized first resin (A), wherein the solids concentration of the varnish is 85 mass% or higher, the weight average molecular weight of the first resin (A) contained in the varnish is 13,000 or higher and 80,000 or lower, and the average particle size of the neutralized particles of the first resin (A) is 20 nm or higher and 200 nm or lower.

2. The method for producing a colloidal dispersion according to claim 1, which does not include a step of removing the organic solvent.

3. The method for producing a colloidal dispersion according to claim 1 or 2, wherein the average particle size of the neutralized particles of the first resin (A) is 20 nm or more and 150 nm or less.

4. The method for producing a colloidal dispersion according to any one of claims 1 to 3, wherein the mass of the reactive solvent (x) used in the step of obtaining the varnish is 20 parts by mass or more and 60 parts by mass or less relative to 100 parts by mass of the varnish.

5. The method for producing a colloidal dispersion according to any one of claims 1 to 4, wherein the reactive solvent (x) further has a hydrophobic group, and the step of obtaining the varnish comprises: a first step of dropping a first monomer mixture containing a first carboxy group-containing ethylenically unsaturated monomer (a1) into the reactive solvent (x) at a temperature of 130°C or higher and 180°C or lower to synthesize a hydrophobic resin (A1) and obtain a liquid material containing the hydrophobic resin (A1); and a second step of dropping a second monomer mixture containing a second carboxy group-containing ethylenically unsaturated monomer (a2) into the liquid material at a temperature of 70°C or higher and 180°C or lower to synthesize a carboxy group-containing resin (A2) and obtain the varnish containing the first resin (A) having the hydrophobic resin (A1) and the carboxy group-containing resin (A2).

6. The method for producing a colloidal dispersion according to claim 5, wherein the reactive solvent (x) has, as the hydrophobic group, a linear or branched alkyl group having 5 to 24 carbon atoms.

7. The method for producing a colloidal dispersion according to any one of claims 1 to 4, wherein the step of obtaining the varnish comprises: a step of dropping the monomer mixture containing the carboxy group-containing ethylenically unsaturated monomer (a) into the reactive solvent (x) at a temperature of 50°C or higher and lower than 130°C, polymerizing the monomer mixture to obtain a precursor of the first resin (A); and a step of raising the temperature to 130°C or higher and 180°C or lower, reacting the reactive solvent (x) with the precursor to obtain a varnish containing the first resin (A).

8. A method for producing a colloidal dispersion according to any one of claims 1 to 7, wherein the solubility parameter of the particles of the first resin (A) is 10.0 or more and 11.3 or less.

Citation Information

Patent Citations

  • Low-solvent hydroxyl-containing polyacrylate aqueous dispersion and preparation method thereof

    CN106008790A

  • Formation of paint film

    JP1986120667A

  • Resin composition for normal-temperature cross-linking two-pack type coating compound

    JP1995113063A