Additive granulated material and method for producing plastic composition

Additive granules with a specific crystal structure and antioxidant composition address the fluidity and stability issues of phenolic antioxidant granules, ensuring improved performance and stability in thermoplastic resins by maintaining fluidity and enhancing heat-resistant properties.

WO2024225160A1PCT designated stage expired Publication Date: 2024-10-31SUMITOMO CHEM CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015419
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The fluidity of phenolic antioxidant granules used in plastics deteriorates over time, affecting their performance and stability, particularly due to the crystal structure of the phenolic antioxidant, which impacts their handling and dispersion in thermoplastic resins.

Method used

The development of additive granules with a specific crystal structure, such as those showing sharp X-ray diffraction peaks at 2θ = 4.2° and 10.6°, which maintain good fluidity and are formulated with a high content of phenolic antioxidants, phosphorous antioxidants, and sulfur antioxidants, along with other additives like neutralizing agents and lubricants, to enhance processing stability and heat resistance.

Benefits of technology

The additive granules exhibit improved fluidity and stability, ensuring uniform dispersion and performance in thermoplastic resins, even after storage, and provide excellent heat-resistant coloring properties when blended with plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015419_31102024_PF_FP_ABST
    Figure JP2024015419_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An additive granulated material is formed from a composition (A) containing an antioxidant (a) containing a phenolic antioxidant (1), and contains 40-100 mass% of a phenolic antioxidant (1-1-1) with respect to the total amount of the phenolic antioxidant (1). The phenolic antioxidant (1-1-1) is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure exhibiting sharp X-ray diffraction peaks at diffraction angles 2θ = 4.2° and 2θ = 10.6°, as measured by powder X-ray diffraction using X-rays having a Cu-Kα wavelength.
Need to check novelty before this filing date? Find Prior Art

Description

Additive granulation and method for producing plastic composition

[0001] The present invention relates to a method for producing an additive granule and a plastic composition.

[0002] 3,9-Bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane is a hydroxyphenylpropionic acid ester known as a phenolic antioxidant, and is known to have an ε-, δ-, αβ-, or γ-crystalline structure (Patent Document 1).

[0003] Among these, the ε crystal has a crystal structure that exhibits a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in powder X-ray diffraction measurement, and a powder of the ε crystal hydroxyphenylpropionic acid ester is also known (Patent Document 2).

[0004] Japanese Patent Application Laid-Open No. 6-87860 Japanese Patent Application Laid-Open No. 2015-157853

[0005] 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane has excellent antioxidant properties. However, when this phenolic antioxidant is added to plastics as a granule, its fluidity may be impaired. In particular, such granules are often used after a certain period of time has passed since production, such as during transportation or storage in a warehouse. It has been found that the fluidity of the granules may be impaired during such storage periods. Therefore, an object of the present invention is to provide a granule containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, which has good fluidity.

[0006] The present inventors conducted a detailed study on factors affecting the fluidity of granules and found that the crystal structure of the phenolic antioxidant affects the fluidity of granules, leading to the completion of the present invention.

[0007] That is, the present invention encompasses the following preferred embodiments: [1] An additive granule formed from a composition (A) containing an antioxidant (a) that contains a phenolic antioxidant (1), the additive granule containing 40 to 100% by mass, based on the total amount of the phenolic antioxidant (1), of the phenolic antioxidant (1-1-1) being 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystalline structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength. [2] The additive granule according to [1], wherein the content of the phenolic antioxidant (1-1-1) is 40 to 100% by mass relative to the total amount of the phenolic antioxidant (1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, contained in the phenolic antioxidant (1). [3] The additive granule according to [1] or [2], wherein the ratio of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure that shows a sharp X-ray diffraction peak at a diffraction angle 2θ = 7.9° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength is (1-1-1):(1-1-2) = 100:0 to 40:60. [4] The additive granule according to any of [1] to [3], wherein the amount of the phenolic antioxidant (1) contained in composition (A) is 2 to 30 mass% based on the total amount of composition (A). [5] The additive granule according to any one of [1] to [4], wherein the amount of the antioxidant (a) contained in the composition (A) is 25 to 100 mass% relative to the total amount of the composition (A).[6] The additive granule according to any one of [1] to [5], wherein the antioxidant (a) further comprises a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3). [7] The additive granule according to [6], wherein the total amount of the phenol-based antioxidant (1) and the phosphorus-based antioxidant (2) and / or sulfur-based antioxidant (3) contained in the composition (A) is 25 to 100% by mass relative to the total amount of the composition (A). [8] The additive granule according to [6] or [7], wherein the amount of the phenol-based antioxidant (1) is 5 to 30% by mass, and the total amount of the phosphorus-based antioxidant (2) and / or sulfur-based antioxidant (3) is 70 to 95% by mass, relative to the total amount of the antioxidant (a). [9] The additive granule according to any one of [6] to [8], wherein the amount of the phenolic antioxidant (1) is 10 to 15% by mass, the amount of the phosphorus-based antioxidant (2) is 48 to 53% by mass, and the amount of the sulfur-based antioxidant (3) is 35 to 40% by mass, relative to the total amount of the antioxidant (a).

[10] The additive granule according to any one of [1] to [9], wherein the composition (A) further contains at least one additive selected from the group consisting of a neutralizing agent, a lubricant, a hindered amine light stabilizer, an ultraviolet absorber, a metal soap, an antistatic agent, an antiblocking agent, a pigment, a flame retardant, a filler, a nucleating agent, a plasticizer, a processing aid, a foaming agent, and an emulsifier.

[11] The additive granule according to any one of [1] to

[10] , wherein the median diameter (by mass) of the additive granule is 0.1 to 7 mm.

[12] A method for producing a plastic composition, comprising a step of blending 0.005 to 10 parts by mass of the additive granules according to any one of [1] to

[11] with respect to 100 parts by mass of plastic.

[13] The method for producing the plastic composition according to

[12] , wherein the plastic is a thermoplastic resin.

[14] The method for producing the plastic composition according to claim

[12] , wherein the plastic is a polyolefin resin.

[0008] According to the present invention, it is possible to provide a granulated product containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, which has good flowability.

[0009] 1 shows the results of powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength for Compound (1-1-1) used in Examples, and Compound (1-1-2) shows the results of powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength for Compound (1-1-2) used in Examples.

[0010] Hereinafter, embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described herein, and various modifications can be made without departing from the spirit of the present invention. Furthermore, when multiple upper and lower limit values ​​are described for a specific feature, any of these upper and lower limit values ​​can be combined to form a suitable numerical range.

[0011] The additive granules of the present invention are granules formed from composition (A), and composition (A) contains at least one or more phenolic antioxidants (1) as antioxidant (a). The phenolic antioxidant (1) contains 40 to 100% by mass, based on the total amount of the phenolic antioxidant (1-1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystalline structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength. 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, which has a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, has a δ crystal structure, and this δ crystal compound is referred to as phenolic antioxidant (1-1-1) in this specification.

[0012] It has been surprisingly found that the fluidity of the additive granules is improved by containing a specific amount of the phenolic antioxidant (1-1-1) in the phenolic antioxidant (1) in the composition (A) forming the additive granules. It has also been found that the fluidity of the additive granules can be maintained even after a certain period of time has elapsed since the production of the granules.

[0013] [Antioxidant (a)] (Phenol-based antioxidant (1)) In the present invention, the composition (A) contains an antioxidant (a) containing at least a phenol-based antioxidant (1). Examples of the phenol-based antioxidant (1) include compounds represented by the formula (I): and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (1-1), which is a phenolic antioxidant represented by the formula (I). As described in JP-A-6-87860, the phenolic antioxidant (1-1) is known to have crystal structures such as a δ crystal that shows sharp X-ray diffraction peaks at diffraction angles of 2θ=4.2° and 2θ=10.6°, an ε crystal that shows a sharp X-ray diffraction peak at a diffraction angle of 2θ=7.9°, an αβ crystal that shows sharp X-ray diffraction peaks at diffraction angles of 2θ=2.8°, 2θ=8.7°, and 2θ=11.7°, and a γ crystal that shows no specific X-ray diffraction peak, in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength. In this specification, among the phenolic antioxidants represented by formula (I) (1-1), a δ-crystalline compound having a crystal structure that exhibits sharp X-ray diffraction peaks at diffraction angles 2θ = 4.2 ° and 2θ = 10.6 ° is also referred to as a phenolic antioxidant (1-1-1), an ε-crystalline compound having a crystal structure that exhibits sharp X-ray diffraction peaks at diffraction angles 2θ = 7.9 ° is also referred to as a phenolic antioxidant (1-1-2), an αβ-crystalline compound having a crystal structure that exhibits sharp X-ray diffraction peaks at diffraction angles 2θ = 2.8 °, 2θ = 8.7 °, and 2θ = 11.7 ° is also referred to as a phenolic antioxidant (1-1-3), and a γ-crystalline compound having a crystal structure that does not exhibit a specific X-ray diffraction peak is also referred to as a phenolic antioxidant (1-1-4). Note that the phenolic antioxidants having a crystal structure that exhibits the above-mentioned specific X-ray diffraction peaks are each a single crystal system and typically have a specific melting point. Specifically, the melting point of the δ-crystalline phenolic antioxidant (1-1-1), which has a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, is usually about 124 to 127° C. Similarly, the melting point of the phenolic antioxidant (1-1-2) is usually about 116 to 119° C., the melting point of the phenolic antioxidant (1-1-3) is usually about 104 to 109° C., and the melting point of the phenolic antioxidant (1-1-4) is usually about 45 to 55° C.

[0014] The composition (A) may contain, as the antioxidant (a), one type of phenolic antioxidant, two or more types of phenolic antioxidants, or an antioxidant other than a phenolic antioxidant, but it at least contains a δ-crystalline compound represented by formula (I) having a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, i.e., a phenolic antioxidant (1-1-1).

[0015] The amount of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1) contained in the composition (A) is 40 to 100% by mass. If the amount is less than 40% by mass, it becomes difficult to obtain the effect of the phenolic antioxidant (1-1-1) in improving the fluidity of the granules. The amount of the phenolic antioxidant (1-1-1) is 40% by mass or more, but from the viewpoint of improving fluidity, it is preferably 50% by mass or more, more preferably 75% by mass or more, even more preferably 90% by mass or more, and even more preferably 99% by mass or more. There is no particular upper limit to the amount, as long as it is 100% by mass or less.

[0016] In one embodiment of the present invention, the content of the phenolic antioxidant (1-1-1) is preferably 40 to 100% by mass, more preferably 50 to 100% by mass, even more preferably 75 to 100% by mass, even more preferably 90 to 100% by mass, and still more preferably 99 to 100% by mass, based on the total amount of the phenolic antioxidant (1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, contained in the phenolic antioxidant (1), from the viewpoint of flowability of the granules.

[0017] The phenolic antioxidant (1) contained in the composition (A) may be, in addition to the above-mentioned phenolic antioxidant (1-1-1), an antioxidant having a crystal system other than the δ crystal represented by formula (I) (for example, the above-mentioned phenolic antioxidants (1-1-2), (1-1-3), or (1-1-4)), or a compound represented by formula (II): [In formula (II), R 1represents an alkyl group having 1 to 9 carbon atoms, X represents an n-valent alcohol residue having 1 to 18 carbon atoms which may contain a heteroatom and / or a cyclic group, and n represents an integer of 2 or 4] (excluding the phenolic antioxidants represented by formula (I)), 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, 4,4'-thiobis(2-t-butyl-5-methylphenol), 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propanamide], and 4,4'-butylidenebis(6-t-butyl-m-cresol).

[0018] R in formula (II) 1 Examples of R include a linear alkyl group having 1 to 8 carbon atoms, such as a methyl group, a t-butyl group, a t-pentyl group, and a t-octyl group, and a branched alkyl group having 3 to 8 carbon atoms. 1 is preferably a methyl group or a t-butyl group.

[0019] In formula (II), n is 2 or 4.

[0020] X in formula (II) is an n-valent alcohol residue, and X contains 1 to 18 carbon atoms. Here, the alcohol residue refers to a substituent obtained by removing a hydroxyl group from an alcohol. X may contain a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom, or may contain a cyclic group such as an alicyclic group such as a cyclopentane structure or a cyclohexane structure, or an aromatic group such as a benzene structure. A carbon atom of the cyclic group may be substituted with a heteroatom.

[0021] Examples of alcohols that provide the alcohol residue include stearyl alcohol, decyl alcohol, octyl alcohol, triethylene glycol, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, and pentaerythritol. Of these, stearyl alcohol, triethylene glycol, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, and pentaerythritol are preferred.

[0022] Examples of the phenolic compound (II) include bis{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionic acid}triethylene glycolyl ester, tetrakis{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionic acid}pentaerythrityl ester, etc. However, the phenolic antioxidant represented by formula (I) is not included in the phenolic antioxidant represented by formula (II).

[0023] The composition (A) forming the additive granules contains a phenolic antioxidant (1). From the viewpoint of heat discoloration resistance (the property of suppressing discoloration even when kneaded and molded at high temperatures), the total amount of the phenolic compound represented by formula (I) and the compound represented by formula (II) contained in the phenolic antioxidant (1) is preferably 90 parts by mass or more, more preferably 95 parts by mass or more, and even more preferably 99 parts by mass or more, per 100 parts by mass of the phenolic antioxidant (1) contained in the composition (A).

[0024] The amount of the phenolic antioxidant (1) contained in the composition (A) forming the additive granules is preferably 2% by mass or more, more preferably 2.5% by mass or more, and even more preferably 3% by mass or more, based on the total amount of the composition (A), from the viewpoint of improving processing stability; and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the total amount of the composition (A), from the viewpoint of cost reduction.

[0025] The amount of antioxidant (a) contained in composition (A) forming the additive granules is preferably 25% by mass or more, more preferably 26% by mass or more, and even more preferably 27% by mass or more, based on the total amount of composition (A), from the viewpoint of improving processing stability. The upper limit of this amount is not particularly limited, and it is sufficient if it is 100% by mass or less based on the total amount of composition (A). However, from the viewpoint of cost reduction, it is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.

[0026] In the composition (A) forming the additive granules, the ratio (1-1-1):(1-1-2) of the amount of the phenolic antioxidant (1-1-1) contained as the phenolic antioxidant (1) to the amount of the phenolic antioxidant (1-1-2) is preferably 100:0 to 40:60, more preferably 100:0 to 45:55, and even more preferably 100:0 to 50:50. In this embodiment, the additive granules may contain the above components as a whole. Therefore, the additive granules may be, for example, an additive granules made of a composition (A) containing a phenolic antioxidant (1-1-1), an additive granules made of a composition (A) containing a phenolic antioxidant (1-1-1) and a phenolic antioxidant (1-1-2), or a mixture obtained by mixing an additive granule (a1) made of a composition (A) containing a phenolic antioxidant (1-1-1) with an additive granule (b1) made of a composition (B) containing a phenolic antioxidant (1-1-2) in such a ratio that the ratio of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2), (1-1-1):(1-1-2), is preferably 100:0 to 40:60, more preferably 100:0 to 45:55, and even more preferably 100:0 to 50:50.

[0027] The composition (A) forming the additive granules may contain only the phenolic antioxidant (1) as the antioxidant (a), or may further contain an antioxidant other than the phenolic antioxidant (1). Examples of antioxidants other than the phenolic antioxidant (1) include phosphorus-based antioxidants (2), sulfur-based antioxidants (3), and hindered amine-based antioxidants. The composition (A) may further contain, for example, the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) as the antioxidant (a).

[0028] (Phosphorus-Based Antioxidant (2)) Examples of the phosphorus-based antioxidant (2) include 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite and triisodecyl phosphite. The composition (A) may contain one type of phosphorus-based antioxidant or two or more types of phosphorus-based antioxidants as the phosphorus-based antioxidant (2). From the viewpoint of improving heat discoloration resistance and antioxidant properties, the phosphorus-based antioxidant is preferably a compound represented by the formula (III): [In formula (III), R 3 , R 4 , and R 5 each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom], a phosphorus-based antioxidant represented by formula (IV): [In formula (IV), R 6 , R 7 , and R 8 each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom], and / or a phosphorus-based antioxidant represented by formula (V): [In formula (V), R 9 , R 10 , and R 11 and each independently represent a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group.

[0029] In formula (III), R3 , R 4 , and R 5 R each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. Examples of linear alkyl groups and branched alkyl groups include a methyl group, a t-butyl group, a t-pentyl group, and a t-octyl group. 3 , R 4 , R 5 is preferably a hydrogen atom, a methyl group, or a t-butyl group. Examples of the phosphorus-based antioxidant represented by formula (III) include tris(nonylphenyl)phosphite and tris(2,4-di-t-butylphenyl)phosphite.

[0030] In formula (IV), R 6 , R 7 , and R 8 each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. The linear alkyl group and the branched alkyl group are, for example, R 3 Examples of R include the same groups as those exemplified for R etc. 6 , R 7 , R 8 is preferably a hydrogen atom, a methyl group, or a t-butyl group. Examples of the phosphorus-based antioxidant represented by formula (IV) include bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite and bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite.

[0031] In formula (V), R 9 , R 10 , and R 11 each independently represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. The linear alkyl group and the branched alkyl group include R 3Examples of the cycloalkyl group having 5 to 8 carbon atoms include a cyclopentyl group, a cyclohexyl group, and a cyclopentyl group, examples of the alkylcycloalkyl group having 6 to 12 carbon atoms include a methylcyclopentyl group, a methylcyclohexyl group, and a dimethylcyclohexyl group, and examples of the aralkyl group having 7 to 12 carbon atoms include a benzyl group.

[0032] In formula (V), R 9 preferably represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms, and more preferably represents a t-alkyl group, a cyclohexyl group, or a 1-methylcyclohexyl group.

[0033] In formula (V), R 10 preferably represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms, and more preferably represents a methyl group, a t-butyl group, or a t-pentyl group.

[0034] In formula (V), R 11 preferably represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, or a branched alkyl group having 3 to 8 carbon atoms, and more preferably represents a hydrogen atom or a methyl group.

[0035] In formula (V), B is a single bond, a sulfur atom, or —CHR 12 represents a - group, and R 12 represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. The linear alkyl group having 1 to 8 carbon atoms, the branched alkyl group having 3 to 8 carbon atoms, and the cycloalkyl group having 5 to 8 carbon atoms are the same as those described above for R 9 Examples include the same groups as those shown in —CHR 12 Examples of the - group include a methylene group, an ethylidene group, a propylidene group, a 1-cyclohexylmethyl group, etc. B preferably represents a single bond, a methylene group, or an ethylidene group.

[0036] In formula (V), A is an alkylene group having 2 to 8 carbon atoms or *-C(=O)-R 13 represents a - group, and R 13 represents a single bond or an alkylene group having 1 to 8 carbon atoms, and * represents a bond to the oxygen atom side of the >P-O- portion. Examples of alkylene groups having 1 to 8 carbon atoms include methylene, ethylene, trimethylene, and tetramethylene. A represents an alkylene group having 2 to 4 carbon atoms or the aforementioned *-C(=O)-R 13 The carbon-carbon bond of the alkylene group having 2 to 4 carbon atoms may be interrupted by a group containing a heteroatom. In this case, examples of the group containing a heteroatom include an -O-C(=O)- or -C(=O)-O- group. R 13 is preferably an alkylene group having 1 to 4 carbon atoms.

[0037] Either Y or Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, or a branched alkyl group having 3 to 8 carbon atoms. When Y is a hydroxyl group, R 12 and R 13 Preferably, either one of the groups is a linear alkyl group having 3 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. Examples of alkoxy groups having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, and a t-butoxy group, and examples of aralkyloxy groups having 7 to 12 carbon atoms include a benzyloxy group.

[0038] When Y in formula (V) is a hydroxyl group, Z is more preferably a hydrogen atom or a methyl group, and R 12 and R 13 More preferably, one of the groups is a t-butyl group.

[0039] When Z in formula (V) is a hydroxyl group, R 13 is a methyl group, Y is a hydrogen atom, and R 12is preferably a t-butyl group.

[0040] Furthermore, R in formula (V) 9 , R 10 , R 11 may be the same as or different from each other.

[0041] Preferred examples of the phosphorus-based antioxidant represented by formula (V) include the following: 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine, oxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphine and the like.

[0042] (Sulfur-Based Antioxidant (3)) Examples of the sulfur-based antioxidant (3) include bis[2-methyl-4-{3-n-alkyl(C12 or C14)thiopropionyloxy}-5-t-butylphenyl]sulfide. The composition (A) may contain one type of sulfur-based antioxidant or two or more types of sulfur-based antioxidants as the sulfur-based antioxidant (3). From the viewpoint of improving heat discoloration resistance and antioxidation properties, the sulfur-based antioxidant is preferably a compound represented by the formula (VI): (R 14 -D-S-C 2 H 4 CO 2 ) m -E (VI) [In formula (VI), R 14 represents a linear alkyl group having 12 to 18 carbon atoms or a branched alkyl group having 12 to 18 carbon atoms, and D represents a single bond or -C 2 H 4 CO 2- group, m is an integer of 1 to 4, and E is an m-valent alcohol residue having 5 to 18 carbon atoms.

[0043] In formula (VI), R 14 is preferably a dodecyl group, a tetradecyl group, or an octadecyl group. The alcohol residue in E refers to the portion of the alcohol other than the hydroxyl group. Examples of alcohols that provide the alcohol residue include dodecyl alcohol, tetradecyl alcohol, octadecyl alcohol, and pentaerythritol.

[0044] In particular, in the sulfur-based antioxidant represented by formula (VI), when D in formula (VI) is a single bond, R 14 is a dodecyl group, m is 4, and E is a pentaerythritol residue. 2 H 4 CO 2 - group, R 14 is a dodecyl group, a tetradecyl group, or an octadecyl group, m is 1, and E is the above R 14 Preferably, the alcohol residue has 12, 14 or 18 carbon atoms, corresponding to:

[0045] In addition, D is -C 2 H 4 CO 2 When E is a - group, the alcohol residue and D are usually bonded via an ester group. 2 H 4 CO 2 It is set to -Z.

[0046] Examples of the sulfur-based antioxidant represented by formula (VI) include 3,3'-thiodipropionic acid di-n-dodecyl ester, 3,3'-thiodipropionic acid di-n-tetradecyl ester, 3,3'-thiodipropionic acid di-n-octadecyl ester, and tetrakis(3-dodecylthiopropionic acid) pentaerythrityl ester.

[0047] In a preferred embodiment of the present invention, when the composition (A) forming the additive granules contains, as the antioxidant (a), a phenolic antioxidant (1), a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3), the total amount of the phenolic antioxidant (1), the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) is preferably 25 to 100% by mass, more preferably 26 to 90% by mass, and even more preferably 27 to 80% by mass, based on the total amount of the composition (A).

[0048] In a more preferred embodiment of the present invention, when the composition (A) forming the additive granule contains, as the antioxidant (a), a phenolic antioxidant (1) and a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3), the amount of the phenolic antioxidant (1) relative to the total amount of the antioxidants (a) is preferably 5 to 30% by mass, more preferably 8 to 20% by mass, and even more preferably 10 to 15% by mass, and the total amount of the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) relative to the total amount of the antioxidants (a) is preferably 70 to 95% by mass, more preferably 80 to 92% by mass, and even more preferably 85 to 90% by mass. Furthermore, the composition (A) contains 40 to 100% by mass of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1).

[0049] In a more preferred embodiment of the present invention, when the composition (A) forming the additive granule contains, as antioxidants (a), a phenolic antioxidant (1), a phosphorus-based antioxidant (2), and a sulfur-based antioxidant (3), the amount of the phenolic antioxidant (1) relative to the total amount of the antioxidants (a) is preferably 10 to 15% by mass, more preferably 10 to 14% by mass, and even more preferably 11 to 14% by mass, the amount of the phosphorus-based antioxidant (2) is preferably 48 to 53% by mass, more preferably 49 to 52% by mass, and even more preferably 49 to 51% by mass, and the amount of the sulfur-based antioxidant (3) is preferably 35 to 40% by mass, more preferably 36 to 39% by mass, and even more preferably 36 to 38% by mass. Furthermore, the composition (A) contains 40 to 100% by mass of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1).

[0050] From the viewpoint of improving heat discoloration resistance and antioxidant properties, the phenolic antioxidant (1) is preferably a compound selected from the group consisting of phenolic antioxidants represented by formula (I) and phenolic antioxidants represented by formula (II). However, from the viewpoint of obtaining an additive granule with high fluidity, the phenolic antioxidant (1-1-1) is contained in an amount of 40 to 100 mass% based on the total amount of the phenolic antioxidant (1). From the viewpoint of improving heat discoloration resistance and antioxidant properties, the phosphorus-based antioxidant (2) is preferably a compound selected from the group consisting of phosphorus-based antioxidants represented by formula (III), phosphorus-based antioxidants represented by formula (IV), and phosphorus-based antioxidants represented by formula (V), and is more preferably a phosphorus-based antioxidant represented by formula (III). From the viewpoint of improving heat discoloration resistance and antioxidant properties, the sulfur-based antioxidant (3) is preferably a compound selected from the group consisting of sulfur-based antioxidants represented by formula (VI), and in which D in formula (VI) is -C 2 H 4 CO 2 - group, and R 14 is a dodecyl group, a tetradecyl group, or an octadecyl group, m is 1, and E is the above R 14More preferred are sulfur-based antioxidants which are alcohol residues having 12, 14 or 18 carbon atoms corresponding to the following:

[0051] (Other Additives) In addition to the antioxidant (a), the composition (A) forming the additive granules may further contain various additives known in the art. Examples of such additives include at least one additive selected from the group consisting of neutralizing agents, lubricants, hindered amine light stabilizers, UV absorbers, metal soaps, antistatic agents, antiblocking agents, pigments, flame retardants, fillers, nucleating agents, plasticizers, processing aids, foaming agents, and emulsifiers. The composition (A) may further contain one of these additives or a combination of two or more of them. The content of the above additives in the composition (A) is not particularly limited, but from the viewpoint of processing stability, it is preferably 10 to 75% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 65% by mass based on the total amount of the composition (A).

[0052] Examples of the neutralizing agent include calcium stearate, zinc stearate, magnesium stearate, zinc oxide, synthetic hydrotalcite, natural hydrotalcite, and calcium hydroxide.

[0053] Examples of the lubricant include oleic acid amide, erucic acid amide, propylene glycol monostearate, stearyl stearate, and sorbitan stearate.

[0054] Examples of the hindered amine light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (melting point 81 to 86°C), bis(2,2,6,6-tetramethyl-4-piperidyl)ester, 2,2,6,6-tetramethyl-4-piperidyl methacrylate (melting point 58°C), and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}-1,6-hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}] (melting point 100 to 135°C).

[0055] Examples of the ultraviolet absorber include 2-hydroxy-4-n-octyloxybenzophenone (melting point of 45°C or higher), 2-(2H-benzotriazol-2-yl)-4,6-di-t-pentylphenol (melting point of 77°C or higher), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl-]-5-(octyloxy)phenol (melting point of 87 to 89°C), 2-(2-hydroxy-5-methylphenyl)benzotriazole (melting point of 127°C), 2-(3-t-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole (melting point of 137°C), and 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate (melting point of 192°C).

[0056] Metal soaps include fatty acid metal salts such as calcium stearate.

[0057] Examples of antistatic agents include cationic surfactants such as quaternary ammonium salt-type cationic surfactants, betaine-type amphoteric surfactants, alkyl phosphate-type anionic surfactants, primary amine salts, secondary amine salts, tertiary amine salts, quaternary amine salts, and pyridine derivatives; anionic surfactants such as sulfated oils, soaps, sulfated ester oils, sulfated amide oils, sulfated ester salts of olefins, fatty alcohol sulfate salts, alkyl sulfate ester salts, fatty acid ethyl sulfonates, alkyl naphthalene sulfonates, alkyl benzene sulfonates, succinic acid ester sulfonates, and phosphate ester salts; nonionic surfactants such as ethylene oxide adducts of partial fatty acid esters of polyhydric alcohols, ethylene oxide adducts of fatty alcohols, ethylene oxide adducts of fatty aminos or fatty acid amides, ethylene oxide adducts of alkylphenols, ethylene oxide adducts of partial fatty acid esters of polyhydric alcohols, and polyethylene glycol; and amphoteric surfactants such as carboxylic acid derivatives and imidazoline derivatives.

[0058] Examples of the antiblocking agent include inorganic antiblocking agents such as aluminum silicate, synthetic silica, natural silica, zeolite, kaolin, and diatomaceous earth, and organic antiblocking agents such as crosslinked polymethyl methacrylic acid.

[0059] Examples of pigments include carbon black, titanium oxide, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, perylene or perinine pigments, quinophthalone pigments, diketopyrrolo-pyrrole pigments, dioxazine pigments, disazo condensation pigments, and benzimidazolone pigments.

[0060] Examples of the flame retardant include decabromobiphenyl, antimony trioxide, phosphorus-based flame retardants, and aluminum hydroxide.

[0061] Examples of fillers include calcium carbonate, silicates, glass fibers, talc, kaolin, mica, barium sulfate, carbon black, carbon fibers, zeolite, metal powders, and metal oxides.

[0062] Examples of nucleating agents include Na salt of α-naphthalenesulfonic acid, Mg salt of α-naphthalenesulfonic acid, Ca salt of α-naphthalenesulfonic acid, Al salt of α-naphthalenesulfonic acid, Na salt of 8-aminonaphthalenesulfonic acid, Na salt of benzenesulfonic acid, Mg salt of benzenesulfonic acid, Ca salt of benzenesulfonic acid, Al salt of benzenesulfonic acid, Ca salt of 2,5-dichlorobenzenesulfonic acid, Mg salt of 2,5-dichlorobenzenesulfonic acid, Ca salt of m-xylenesulfonic acid, and Al salt of m-xylenesulfonic acid. Mg salt, benzoic acid (melting point 122°C), sodium benzoate (melting point 147°C), p-isopropylbenzoic acid, o-t-butylbenzoic acid, p-t-butylbenzoic acid, monophenylacetic acid (melting point 77°C), diphenylacetic acid, Li salt of diphenylacetic acid, Al salt, Na salt, Na salt of diphenylacetic acid, Mg salt of diphenylacetic acid, Ca salt of diphenylacetic acid, Ba salt of diphenylacetic acid, Al salt of diphenylacetic acid, phenyldimethylacetic acid, Li salt of phenyldimethylacetic acid, Na salt of phenyldimethylacetic acid, phenyldimethyl Mg salt of phenyldimethylacetic acid, Ca salt of phenyldimethylacetic acid, Ba salt of phenyldimethylacetic acid, Mg salt of phthalic acid, succinic acid (melting point 185°C), Li salt of succinic acid, Na salt of succinic acid, Mg salt of succinic acid, Ca salt of succinic acid, Ba salt of succinic acid, glutaric acid (melting point 95-99°C), Li salt of glutaric acid, Na salt of glutaric acid, Mg salt of glutaric acid, Ca salt of glutaric acid, Ba salt of glutaric acid, adipic acid (melting point 151-153°C), suberic acid, Li salt of suberic acid, Na salt of suberic acid, Mg salt of suberic acid salt, Ca salt of suberic acid, Ba salt of suberic acid, sebacic acid, Li salt of sebacic acid, Na salt of sebacic acid, Mg salt of sebacic acid, Ca salt of sebacic acid, Al salt of sebacic acid, diphenylphosphinic acid (melting point 193-196°C), Li salt of diphenylphosphinic acid, Na salt of diphenylphosphinic acid, K salt of diphenylphosphinic acid, Ca salt of diphenylphosphinic acid, Mg salt of diphenylphosphinic acid, Al salt of diphenylphosphinic acid, Li salt of 4,4'-dichlorodiphenylphosphinic acid, 4,Examples of the dinaphthylphosphinic acid include a sodium salt of 4'-dimethyldiphenylphosphinic acid, dinaphthylphosphinic acid, a lithium salt of dinaphthylphosphinic acid, a sodium salt of dinaphthylphosphinic acid, a magnesium salt of dinaphthylphosphinic acid, a calcium salt of dinaphthylphosphinic acid, and an aluminum salt of dinaphthylphosphinic acid.

[0063] Examples of the plasticizer include polyethylene glycol and polypropylene glycol.

[0064] Processing aids include ricinoleic acid, stearic acid, palmitic acid, lauric acid, and the like.

[0065] Examples of foaming agents include chemical foaming agents and physical foaming agents. Examples of chemical foaming agents include inorganic compounds and organic compounds. Examples of inorganic compounds include hydrogen carbonates such as sodium hydrogen carbonate, and ammonium carbonate. Examples of organic compounds include polycarboxylic acids, azo compounds, sulfonhydrazide compounds, nitroso compounds, p-toluenesulfonylsemicarbazide, and isocyanate compounds. Examples of physical foaming agents include inert gases, volatile organic compounds such as butane and pentane, and examples of inert gases include carbon dioxide, nitrogen, argon, neon, and helium.

[0066] Examples of the emulsifier include polyoxyethylene sorbitan monolaurate, polyethylene glycol monolaurate, and sorbitan tristearate.

[0067] In a preferred embodiment of the present invention, the composition (A) contains 25 to 100% by mass of the antioxidant (a) relative to the total amount of the composition (A), and the antioxidant (a) contains a phenolic antioxidant (1), a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3), and it is preferred that the amount of the phenolic antioxidant (1) contained in the antioxidant is 2 to 30% by mass relative to the total amount of the composition (A), and the amount of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidants (1) is 40 to 100% by mass.

[0068] [Additive Granules] The additive granules of the present invention are granules formed from composition (A). Examples of the shape of the additive granules include "pellets" obtained by granulation using a semi-dry extruder such as a single-screw or multi-screw melt extruder or a disc pelletizer, "granules" obtained by agitation granulation, and "flakes" obtained by granulation using a compression granulator such as a roller compactor. The shape of the additive granules described above refers to the shapes classified according to the definitions described in Section 10 of JIS-Z8841 (1993), Explanatory Table 1, Shape and Name of Granules. Furthermore, the additive granules do not refer to a single granule, but rather to an aggregate of granules. Among the above shapes, "granules" are preferred from the viewpoints of excellent flowability and excellent dispersibility in thermoplastic resins. Granular additive granules can be obtained by either extrusion granulation or agitation granulation, but "granules" obtained by agitation granulation of composition (A) are more preferred.

[0069] The method for producing the additive granules is not particularly limited, and examples thereof include a method in which composition (A) is subjected to stirring granulation or extrusion granulation within an appropriate temperature range, for example, 40°C to 80°C, preferably 40°C to 70°C, and particularly preferably 40°C to 60°C.

[0070] Examples of equipment used for stirring granulation include high-speed rotating equipment such as a Henschel mixer, a super mixer, and a high-speed mixer, stirring mixer granulators such as a vertical granulator, and a tumbling fluidized coating device. Granules may also be produced by the production method described in JP-A-2010-254958.

[0071] Examples of the stirring granulation method include a method in which the raw materials constituting composition (A) are charged into a mixer such as a Henschel mixer and then stirred and mixed at high speed. Methods for setting the temperature within the above range include a method in which a hot water jacket is attached to the Henschel mixer to heat it, and a method in which the temperature is increased by utilizing shear heat generated by high-speed stirring.

[0072] The size of the additive granules is not particularly limited, but when produced by agitation granulation, for example, the median diameter (mass basis) is preferably 0.1 to 7 mm, more preferably 0.15 to 6 mm, even more preferably 0.18 to 6 mm, and even more preferably 0.20 to 6 mm. The median diameter (mass basis) is determined by mechanical sieving of about 100 g of a sample using a low-tap shaker (for example, low-tap shaker RL-1, Kagaku Kyoeisha) for 15 minutes, with a shaking speed of 290 rpm / 60 Hz, a swing width of 25 mm, and a stroke rate of 156 tpm / 60 Hz.

[0073] Examples of methods for producing additive granules having the above-mentioned median diameter (by mass) include a method using an agitation granulator having an agitation blade, in which the clearance between the tip of the agitation blade inside the agitation granulator and the wall surface inside the agitation granulator is adjusted to 30 mm or less. The additive granules having the above-mentioned median diameter (by mass) are preferably in the form of granules.

[0074] Examples of equipment used for extrusion granulation include single-screw or multi-screw melt extruders, and semi-dry extruders such as disc pelleters.

[0075] In the extrusion granulation method, for example, the raw materials constituting composition (A) are mixed in a mixer such as a Henschel mixer or a super mixer to prepare a mixture, and the mixture is then fed into an extruder from a hopper or the like. The material temperature inside the extruder is adjusted to 40°C to 80°C using the shear heat generation or heating equipment of the extruder, allowing for easy extrusion to produce cylindrical granules. The extruded cylindrical granules can be cut to an appropriate length with a cutter or the like to obtain pellet-shaped additive granules. By adjusting the die diameter, extrusion speed, and cutting speed, pellet-shaped additive granules of any size can be produced, but from the viewpoint of dispersibility, a diameter of 2 to 5 mm and a length of 2 to 5 mm are preferred.

[0076] The additive granules of the present invention contain 40 to 100% by mass of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1). The ratio of the amount of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1) contained in the additive granules may be calculated, for example, from the charge ratio when producing the additive granules, or the amount of the phenolic antioxidant (1) contained in the additive granules may be identified and quantified by HPLC and the amount of the phenolic antioxidant (1-1-1) may be calculated from the endothermic heat at the time of melting at around 124 to 127°C by DSC, and the ratio may be calculated from these amounts.

[0077] The additive granules according to one embodiment of the present invention are used by blending them with plastics, such as thermoplastic resins. The blending ratio of the additive granules to the plastic can be, for example, 0.005 to 10 parts by mass of the additive granules per 100 parts by mass of the plastic, preferably 0.01 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass. The present invention also provides a method for producing a plastic composition by blending the additive granules of the present invention with a plastic, preferably blending 0.005 to 10 parts by mass of the additive granules of the present invention per 100 parts by mass of the plastic, as well as the plastic composition. The plastic composition obtained by the above-described manufacturing method contains a highly fluid additive granule, and therefore has advantages such as minimal variation in the additive amount and uniform dispersion of the additive. The present invention also provides a method for stabilizing plastics, including blending 0.005 to 10 parts by mass of the additive granules of the present invention per 100 parts by mass of the plastic.

[0078] The plastic to be blended with the additive granules is preferably a thermoplastic resin. The thermoplastic resin is not particularly limited as long as it is a commercially available resin, but examples thereof include polypropylene resins such as ethylene-propylene copolymers, polyethylene resins (high density polyethylene (HD-PE), low density polyethylene (LD-PE), linear low density polyethylene (LLDPE), etc.), methylpentene polymers, ethylene-ethyl acrylate copolymers, ethylene-vinyl acetate copolymers, polystyrenes (polystyrenes such as poly(p-methylstyrene) and poly(α-methylstyrene), acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, special acrylic rubber-acrylonitrile-styrene copolymers, acrylonitrile-chlorinated polyethylene-styrene copolymers, styrene-butadiene copolymers, etc.), chlorinated polyethylene, polychloroprene, chlorinated rubber, polyvinyl chloride, polychloride, etc. Examples of the resin include vinylidene chloride, methacrylic resin, ethylene-vinyl alcohol copolymer, fluororesin, polyacetal, grafted polyphenylene ether resin, polyphenylene sulfide resin, polyurethane, polyamide, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate, etc.), polycarbonate, polyacrylate, polysulfone, polyether ether ketone, polyether sulfone, aromatic polyester resin, diallyl phthalate prepolymer, silicone resin, 1,2-polybutadiene, polyisoprene, butadiene / acrylonitrile copolymer, ethylene-methyl methacrylate copolymer, etc., and from the viewpoint of good moldability, polyolefin resins such as polyethylene resins and polypropylene resins, and polystyrene resins are preferred, with polyolefin resins being more preferred.

[0079] Here, polypropylene-based resin means a polyolefin-based resin containing structural units derived from propylene, and specific examples include crystalline propylene homopolymer, propylene-ethylene random copolymer, propylene-α-olefin random copolymer, propylene-ethylene-α-olefin copolymer, polypropylene-based block copolymer consisting of a propylene homopolymer component or a copolymer component mainly composed of propylene, and a copolymer component of propylene and ethylene and / or an α-olefin, etc. When a polypropylene-based resin is used as the thermoplastic resin, one type of polypropylene-based resin may be used, or two or more types may be blended and used.

[0080] Examples of the α-olefin include α-olefins having 4 to 12 carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, and 1-octene.

[0081] Examples of the propylene-α-olefin random copolymer include a propylene-1-butene random copolymer, a propylene-1-hexene random copolymer, and a propylene-1-octene random copolymer.

[0082] Examples of the propylene-ethylene-α-olefin copolymer include a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and a propylene-ethylene-1-octene copolymer.

[0083] In the polypropylene-based block copolymer comprising a propylene homopolymer component or a copolymer component mainly composed of propylene and a copolymer component of propylene and ethylene and / or an α-olefin, examples of the copolymer component mainly composed of propylene include a propylene-ethylene copolymer component, a propylene-1-butene copolymer component, a propylene-1-hexene copolymer component, etc., and examples of the copolymer component of propylene and ethylene and / or an α-olefin include a propylene-ethylene copolymer component, a propylene-ethylene-1-butene copolymer component, a propylene-ethylene-1-hexene copolymer component, a propylene-ethylene-1-octene copolymer component, a propylene-1-butene copolymer component, a propylene-1-hexene copolymer component, a propylene-1-octene copolymer component, etc. The content of ethylene and / or an α-olefin having 4 to 12 carbon atoms in the copolymer component of propylene and ethylene and / or an α-olefin is, for example, 0.01 to 20% by weight.

[0084] Furthermore, examples of polypropylene block copolymers comprising a propylene homopolymer component or a copolymer component mainly consisting of propylene and a copolymer component of propylene and ethylene and / or an α-olefin include propylene-ethylene block copolymers, (propylene)-(propylene-ethylene) block copolymers, (propylene)-(propylene-ethylene) block copolymers, (propylene)-(propylene-ethylene-1-butene) block copolymers, (propylene)-(propylene-ethylene-1-hexene) block copolymers, (propylene)-(propylene-1-butene) block copolymers, (propylene)-(propylene-1-hexene) block copolymers, and (propylene-ethylene)-(propylene-ethylene-1-butene) block copolymers. polymer, (propylene-ethylene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-ethylene)-(propylene-1-butene) block copolymer, (propylene-ethylene)-(propylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-ethylene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-1-hexene) block copolymer, and the like.

[0085] When a polypropylene-based resin is used as the thermoplastic resin, preferably, a crystalline propylene homopolymer, a polypropylene-based block copolymer consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or an α-olefin having 4 to 12 carbon atoms is used, and more preferably, a polypropylene-based block copolymer consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or an α-olefin having 4 to 12 carbon atoms is used.

[0086] Examples of methods for blending the additive granules with plastics include a method in which the additive granules and plastic are mixed together and then melt-kneaded using a single-screw or multi-screw extruder, a method in which the additive granules are added by feeding them into a solution obtained after polymerizing a thermoplastic resin, etc. The thermoplastic resin obtained in this way can be processed into products such as films, molding materials, and pipes.

[0087] The additive granules of the present invention have good fluidity, and therefore are easy to handle when blended with plastics such as thermoplastic resins, and variations in the amount of additive are unlikely to occur, making it possible to produce highly uniform plastic compositions. Furthermore, when the additive granules of the present invention are blended with plastics, the effects of the additive granules are uniformly exerted, and a thermoplastic resin composition with excellent heat discoloration resistance can be obtained.

[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0089] The components used in the examples and comparative examples are listed below. Compound (1-1-1): 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystalline structure that exhibits sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength. (The results of powder X-ray diffraction measurement are shown in FIG. 1. The left end of the horizontal axis in FIGS. 1 and 2 is 4°.) Compound (1-1-2): 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure that exhibits a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength (the results of powder X-ray diffraction measurement are shown in FIG. 2). Compound (2-1): Tris(2,4-di-t-butylphenyl)phosphite "Irgafos 168 (registered trademark)" (manufactured by BASF) Compound (3-1): 3,3'-thiodipropionic acid di-n-tetradecyl ester "Sumilizer TPM (registered trademark)" (manufactured by Sumitomo Chemical)

[0090] (Example 1: Production of additive granules A-1) 187.5 g of compound (1-1-1), 750.0 g of compound (2-1), and 562.5 g of compound (3-1) were charged into a 10 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-GS-10J). After charging, the temperature of the stirring tank equipped with the high-speed mixer was raised by passing hot water at 50°C through the jacket of the high-speed mixer. Thereafter, the rotation speed of the stirring blade was set to 450 rpm, and the rotation speed of the chopper blade was set to 2000 rpm, and the compounds were mixed. Stirring was stopped when the agitator current reached 4.7 A, and additive granules A-1 having a median diameter (by mass) of 241 μm was obtained.

[0091] (Comparative Example 2: Production of additive granule A-2) Additive granule A-2 was obtained in the same manner as in the production of additive granule A-1, except that compound (1-1-2) was used instead of compound (1-1-1) used in the production of additive granule A-1.

[0092] (Examples 2 to 3, Comparative Example 1) A total of 80.0 g of additive granules A-1 and / or additive granules A-2 in the proportions shown in Table 1 was placed in a 20 L plastic bag and mixed uniformly to obtain additive granules B-1 to B-3.

[0093] (Fluidity) 80.0 g of each of the obtained additive granules of Examples 1 to 3 and Comparative Examples 1 and 2 was placed into a funnel (with stopper) with an opening diameter of 95 mm and a leg outer diameter of 20 mm. The fluidity of the additive granules in their initial state when the stopper was removed was evaluated. After evaluating the initial state, the samples were stored in a constant temperature and humidity chamber at a temperature of 35°C and a humidity of 80% RH for 7 days, and then the fluidity was evaluated in the same manner. The results are shown in Table 1. Evaluation criteria for fluidity: ○: The entire amount flows down. ×: The entire amount does not flow down due to bridging phenomenon.

[0094] (Median diameter based on mass) Each of the additive granules A-1 and A-2 was used as a measurement sample, and 100 g of the sample was mechanically sieved using a low-tap shaker RL-1 (Kagaku Kyoei-sha) under the conditions of a sieving time of 15 minutes, a shaking rate of 290 rpm / 60 Hz, an oscillation width of 25 mm, and a hitting rate of 156 tpm / 60 Hz, to determine the median diameter based on mass. The median diameters of the additive granules A-1 and A-2 were within the range of 0.1 to 7 mm.

[0095]

[0096] The components used in the production examples are listed below. Compound (4-1): calcium stearate "Calcium Stearate WLC (registered trademark)" (manufactured by Faci) Compound (5-1): sodium benzoate "Sodium Benzoate 20M (registered trademark)" (manufactured by BASF) Compound (6-1): hydrotalcite "DHT-4C (registered trademark)" (manufactured by Kyowa Chemical Industry Co., Ltd.) Compound (7-1): talc "Micron White 5000S (registered trademark)" (manufactured by Hayashi Kasei Co., Ltd.) Compound (8-1): oleic acid amide "Kemamide VO (registered trademark)" (manufactured by PMC)

[0097] (Production Example: Additive Granule A-3) A 100 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: Model No. FS-100) was charged with raw materials (15 kg total) consisting of 8.9 parts by weight of compound (1-1-1), 35.7 parts by weight of compound (2-1), 26.8 parts by weight of compound (3-1), 25.0 parts by weight of compound (5-1), and 3.6 parts by weight of compound (6-1). The temperature of the stirring vessel equipped with the high-speed mixer was raised by passing hot water at 50°C through the jacket of the high-speed mixer. The rotation speed of the stirring blades inside the stirring vessel of the high-speed mixer was set to 165 rpm (6 m / s as impeller tip speed) and the rotation speed of the chopper was set to 1500 rpm (10 m / s as impeller tip speed), and the high-speed mixer was operated for approximately 20 minutes while maintaining this condition. In this way, additive granule A-3 was obtained by stirring and granulating the mixture consisting of the raw materials.

[0098] (Production Example: Additive Granule A-4) Additive Granule A-4 was obtained in the same manner as in Additive Granule A-3, except that Compound (1-1-2) was used instead of Compound (1-1-1) used in Additive Granule A-3.

[0099] (Production Example: Additive Granule A-5) A 100 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: Model No. FS-100) was charged with raw materials (15 kg total) consisting of 9.6 parts by weight of compound (1-1-1), 38.2 parts by weight of compound (2-1), 29.1 parts by weight of compound (3-1), 19.3 parts by weight of compound (4-1), and 3.8 parts by weight of compound (7-1). The temperature of the stirring vessel equipped with the high-speed mixer was raised by passing hot water at 50°C through the jacket of the high-speed mixer. The rotation speed of the stirring blades inside the stirring vessel of the high-speed mixer was set to 165 rpm (6 m / s as impeller tip speed) and the rotation speed of the chopper was set to 1500 rpm (10 m / s as impeller tip speed), and the high-speed mixer was operated for approximately 1 minute 20 seconds while maintaining this condition. In this way, additive granule A-5 was obtained by stirring and granulating the mixture consisting of the raw materials.

[0100] (Production Example: Additive Granule A-6) Additive Granule A-6 is obtained in the same manner as additive granule A-5, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-5.

[0101] (Production Example: Additive Granules A-7) A 100 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: Model No. FS-100) was charged with raw materials (15 kg in total) consisting of 3.9 parts by weight of compound (1-1-1), 15.4 parts by weight of compound (2-1), 11.5 parts by weight of compound (3-1), 7.7 parts by weight of compound (4-1), 46.1 parts by weight of compound (7-1), and 15.4 parts by weight of compound (8-1). The stirring vessel equipped with the high-speed mixer was heated by passing 50°C hot water through the jacket of the high-speed mixer. The rotation speed of the stirring blades inside the stirring vessel of the high-speed mixer was set to 165 rpm (6 m / s as impeller tip speed) and the rotation speed of the chopper was set to 1500 rpm (10 m / s as impeller tip speed), and the high-speed mixer was operated for approximately 40 minutes while maintaining this condition. In this manner, the mixture of the raw materials is stirred and granulated to obtain additive granule A-7.

[0102] (Production Example: Additive Granule A-8) Additive Granule A-8 was obtained in the same manner as in Additive Granule A-7, except that Compound (1-1-2) was used instead of Compound (1-1-1) used in Additive Granule A-7.

[0103] (Production Example: Additive Granule A-9) A raw material consisting of 8.9 parts by weight of compound (1-1-1), 35.7 parts by weight of compound (2-1), 26.8 parts by weight of compound (3-1), 25.0 parts by weight of compound (5-1), and 3.6 parts by weight of compound (6-1) was mixed in a 100 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100) using a Henschel mixer. Thereafter, this mixture was charged into a disc pelletizer (manufactured by Dalton: model number F-5) and operated. The extruded material was extruded from a disc die under a roller and immediately cut into pellets to obtain additive granule A-9.

[0104] (Production Example: Additive Granule A-10) Additive Granule A-10 is obtained in the same manner as additive granule A-9, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-9.

[0105] (Production Example: Additive Granule A-11) A raw material consisting of 9.6 parts by weight of compound (1-1-1), 38.2 parts by weight of compound (2-1), 29.1 parts by weight of compound (3-1), 19.3 parts by weight of compound (4-1), and 3.8 parts by weight of compound (7-1) is mixed in a 100 L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100) using a Henschel mixer. Thereafter, this mixture is charged into a disc pelletizer (manufactured by Dalton: model number F-5) and operated. The extruded material is extruded from a disc die under a roller and immediately cut into pellets to obtain additive granule A-11.

[0106] (Production Example: Additive Granule A-12) Additive Granule A-12 is obtained in the same manner as Additive Granule A-11, except that Compound (1-1-2) is used instead of Compound (1-1-1) used in Additive Granule A-11.

[0107] (Production Example: Additive Granule A-13) Raw materials consisting of 3.9 parts by weight of compound (1-1-1), 15.4 parts by weight of compound (2-1), 11.5 parts by weight of compound (3-1), 7.7 parts by weight of compound (4-1), 46.1 parts by weight of compound (7-1), and 15.4 parts by weight of compound (8-1) are mixed using a Henschel mixer. Thereafter, this mixture is charged into a disc pelleter (manufactured by Dalton: model number F-5) and operated. The extruded material is extruded from a disc die under a roller and immediately cut into pellets to obtain additive granule A-13.

[0108] (Production Example: Additive Granule A-14) Additive Granule A-14 is obtained in the same manner as Additive Granule A-13, except that Compound (1-1-2) is used instead of Compound (1-1-1) used in Additive Granule A-13.

[0109] The additive granules A-3, A-5, A-7, A-9, A-11 and A-13 obtained in the above Production Examples are considered to have the same initial flowability and flowability after 7 days as in Example 1. Furthermore, the additive granules A-4, A-6, A-8, A-10, A-12 and A-14 obtained in the above Production Examples are considered to have the same initial flowability and flowability after 7 days as in Comparative Example 2.

[0110] The present invention provides an additive granule having excellent flowability.

Claims

1. An additive granule formed from a composition (A) containing an antioxidant (a) containing a phenolic antioxidant (1), the additive granule containing 40 to 100 mass% of a phenolic antioxidant (1-1-1) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure which shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength.

2. The additive granule according to claim 1, wherein the content of the phenolic antioxidant (1-1-1) is 40 to 100 mass% based on the total amount of the phenolic antioxidant (1-1) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane contained in the phenolic antioxidant (1).

3. The additive granule according to claim 1 or 2, wherein in the phenolic antioxidant (1), the ratio of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure which shows a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in powder X-ray diffraction measurement using X-rays of Cu-Kα wavelength is (1-1-1):(1-1-2)=100:0 to 40:

60.

4. The additive granule according to any one of claims 1 to 3, wherein the amount of the phenolic antioxidant (1) contained in composition (A) is 2 to 30 mass% based on the total amount of composition (A).

5. The additive granule according to any one of claims 1 to 4, wherein the amount of the antioxidant (a) contained in the composition (A) is 25 to 100 mass% based on the total amount of the composition (A).

6. The additive granule according to any one of claims 1 to 5, wherein the antioxidant (a) further comprises a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3).

7. The additive granule according to claim 6, wherein the total amount of the phenol-based antioxidant (1), the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) contained in composition (A) is 25 to 100 mass% based on the total amount of composition (A).

8. The additive granule according to claim 6 or 7, wherein the amount of the phenol-based antioxidant (1) is 5 to 30 mass% and the total amount of the phosphorus-based antioxidant (2) and / or sulfur-based antioxidant (3) is 70 to 95 mass% based on the total amount of the antioxidant (a).

9. The additive granule according to any one of claims 6 to 8, wherein the amount of the phenol-based antioxidant (1) is 10 to 15 mass%, the amount of the phosphorus-based antioxidant (2) is 48 to 53 mass%, and the amount of the sulfur-based antioxidant (3) is 35 to 40 mass%, relative to the total amount of the antioxidant (a).

10. The additive granule according to any one of claims 1 to 9, wherein composition (A) further contains at least one additive selected from the group consisting of neutralizing agents, lubricants, hindered amine light stabilizers, ultraviolet absorbers, metal soaps, antistatic agents, antiblocking agents, pigments, flame retardants, fillers, nucleating agents, plasticizers, processing aids, foaming agents, and emulsifiers.

11. The additive granule according to any one of claims 1 to 10, wherein the additive granule has a median diameter (by mass) of 0.1 to 7 mm.

12. A method for producing a plastic composition, comprising the step of blending 0.005 to 10 parts by mass of the additive granules according to any one of claims 1 to 11 with respect to 100 parts by mass of plastic.

13. The method of producing a plastic composition according to claim 12, wherein the plastic is a thermoplastic resin.

14. The method for producing a plastic composition according to claim 12, wherein the plastic is a polyolefin resin.

Citation Information

Patent Citations

  • Hydroxyphenylpropionic acid ester having novel crystal structure and production thereof

    JP1987149679A

  • Hydroxyphenylpropionic acid ester having new crystalline structure

    JP1994087860A

  • Composition for discoloring inhibitor of organic polymer materials by nitrogen oxide gas and organic polymer materials containing the same

    JP2001310972A

  • Polyamide laminated biaxially oriented film

    JP2002160334A

  • Granule mass and method for producing the same

    JP2007161997A