Copper alloy sheet material, copper alloy sheet material for drawing, and drawn product
The copper alloy sheet material with specific Ni and Si content, along with optional additives, addresses the challenges of tensile strength, conductivity, and drawing workability, ensuring consistent thickness and improved performance in electronic devices.
Patent Information
- Application Number
- PCT/JP2024/015455
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-31
AI Technical Summary
Copper alloy sheet materials used in electronic devices face challenges in achieving high tensile strength, electrical conductivity, and drawing workability, with existing technologies failing to maintain consistent thickness during drawing processes, leading to increased risk of material breakage and reduced conductivity.
A copper alloy sheet material with a composition of 1.00% to 5.00% Ni, 0.20% to 1.30% Si, and optional additives like Sn, Zn, Mg, and Cr, optimized to reduce α-fiber orientation density on the surface to 3.0 or less, achieving tensile strengths of 500 MPa to 900 MPa and electrical conductivity of 30% IACS or more, thereby enhancing drawing workability and preventing thickness reduction near the punch tip.
The optimized copper alloy sheet material exhibits high tensile strength, high electrical conductivity, and improved drawing workability, reducing the likelihood of material breakage and maintaining consistent thickness during drawing, while also offering enhanced electromagnetic shielding and heat dissipation properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Copper alloy sheets, copper alloy sheets for drawing and drawn products
[0001] The present invention relates to a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product.
[0002] Copper alloy sheet materials are used for, for example, connectors for electronic devices or electronic components, lead frames, relays, switches, sockets, shield cases, shield cans, camera module cases, vibration device cases, heat dissipation parts for liquid crystal and organic EL displays, connectors for batteries and automobiles, shield cases, shield cans, etc., and are often subjected to press working such as punching, bending, drawing, and bulging.
[0003] As an example of a copper alloy sheet material used in such press working, Patent Document 1 discloses an alloy composition containing 0.3 to 1.9 mass% Co and 0.1 to 0.5 mass% Si, with the remainder consisting of Cu and inevitable impurities, and the results of measurement using an EBSD method indicate that the total amount of special grain boundaries Σ7 grain boundaries and Σ9 grain boundaries accounts for 1.5% or more of all crystal grain boundaries, Σ9 / Σ7 is 1.0 to 5.0, and the orientation density of α-fiber (Φ1 = 0 ° to 45 °) is in the range of 3.0 to 25.0. Patent Document 1 discloses a copper alloy sheet material that satisfies the above conditions. By controlling the Σ7, Σ9 grain boundaries and α-fiber (Φ1 = 0 ° to 45 °) in a Cu-Co-Si-based copper alloy, the fluctuation height of the boundary line between the sagging (surface) and the shear surface during press working can be suppressed, thereby improving press punching workability.
[0004] Furthermore, Patent Document 2 discloses a copper alloy sheet for electrical and electronic devices having an alloy composition containing 3.5 to 25 mass% Ni and 0.1 to 9.5 mass% Sn, with the balance being Cu and unavoidable impurities, and having a rolling texture, in which the rolling texture is obtained from texture analysis by EBSD, and the average value of the orientation density of α-fiber (φ1 = 0° to 45°) is in the range of 2.5 to 30.0, and the average value of the orientation density of β-fiber (φ2 = 45° to 90°) is in the range of 2.5 to 30.0. Patent Document 2 discloses that by appropriately controlling the orientation densities of the α-fiber and β-fiber of a Cu-Ni-Sn alloy, it is possible to reduce and maintain a high level of Young's modulus and its anisotropy, thereby enabling predetermined spring characteristics to be stably obtained regardless of the direction in which the product is extracted from the material.
[0005] International Publication No. 2018 / 198995 Japanese Patent Application Laid-Open No. 2017-160513
[0006] In recent years, with the trend toward higher current and smaller size of electronic devices and electronic components, higher mechanical properties and electrical conductivity (or thermal conductivity) have been required for press-formed products, which are one of the components that make up these devices. In particular, for drawn parts used in electronic devices and electronic components, such as connectors, lead frames, relays, switches, sockets, shield cases, shield cans, camera modules, heat dissipation parts for liquid crystal and organic EL displays, batteries, and automotive connectors, shield cases, and shield cans, there is a demand for copper alloy sheet materials made of materials that combine higher mechanical properties and electrical conductivity (or thermal conductivity) than the copper alloys such as brass and nickel silver that have been conventionally used.
[0007] Here, "drawing" refers to a type of metal sheet forming method, and typically refers to a processing method in which a punch is pressed into a sheet of metal to form bottomed containers of various shapes, such as cylinders, square tubes, and cones. Also, "drawn product" refers to a processed product formed by drawing, and is characterized by having no seams in the formed processed product. Note that "drawn product" also includes processed products formed by combining drawing with other processing methods different from drawing, such as bending, crushing, and twisting.
[0008] Generally, when drawing, the closer to the edge of the drawn product, the greater the compressive deformation force of the material, causing the die to float, which tends to result in a thicker drawn product. On the other hand, the area near the tip of the punch used in drawing is stretched by the load applied when the punch is pressed in, resulting in a decrease in thickness. In particular, with materials that tend to lose thickness near the tip of the punch, the thickness of the resulting drawn product varies, making it difficult to finish the drawn product within the specified thickness tolerance.
[0009] Here, in order to finish the thickness of a drawn product within a predetermined tolerance, it was necessary to thicken the sheet material before drawing so that the thickness of the drawn product near the tip of the punch did not fall below a predetermined value. Furthermore, if the sheet material before drawing was thickened, it was also necessary to iron the drawn product to adjust the thickness of the drawn product so that the thickness of the portion near the edge of the drawn product matched the thickness near the tip of the punch. However, when using a material that is prone to thickness reduction near the tip of the punch or when the sheet material before processing is thickened, the ironing thickness becomes large, making the material more susceptible to fracture. Therefore, there is a demand for copper alloy sheet material that has excellent drawing workability, and more specifically, is less likely to reduce its thickness near the tip of the punch during drawing.
[0010] In this regard, although Patent Document 1 describes that the press-punching property of the copper alloy sheet material is improved, it does not consider the drawing workability of the copper alloy sheet material at all, much less discloses that excellent drawing workability can be achieved simultaneously with high tensile strength and high electrical conductivity, and does not show evaluation results of these properties.
[0011] Furthermore, although Patent Document 2 describes that the spring characteristics of the copper alloy sheet are improved, it does not consider the drawing workability of the copper alloy sheet. Furthermore, the copper alloy sheet in Patent Document 2 is made of a Cu-Ni-Sn alloy, but it is desirable that the electrical conductivity be even higher. Furthermore, there is no disclosure about achieving both excellent drawing workability and high tensile strength and high electrical conductivity, and no evaluation results of these properties are shown.
[0012] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product, which have high tensile strength and high electrical conductivity and are capable of obtaining excellent drawing workability.
[0013] The present inventors have discovered that in a copper alloy sheet having an alloy composition containing 1.00 mass % or more and 5.00 mass % or less of Ni, 0.20 mass % or more and 1.30 mass % or less of Si, with the balance being Cu and unavoidable impurities, by setting the average value of the orientation density of α-fibers on at least the sheet surface of the copper alloy sheet, obtained from crystal orientation analysis by the SEM-EBSD method described below, to 3.0 or less, setting the tensile strength to 500 MPa or more and 900 MPa or less, and setting the electrical conductivity to 30% IACS or more, the tensile strength and electrical conductivity of the copper alloy sheet can be increased, and drawing workability can be improved, and in particular, a reduction in sheet thickness near the tip of the punch during drawing can be suppressed, and have completed the present invention.
[0014] (1) A copper alloy sheet having an alloy composition containing 1.00% by mass or more and 5.00% by mass or less of Ni, 0.20% by mass or more and 1.30% by mass or less of Si, with the balance being Cu and inevitable impurities, wherein the average value of the orientation density of α-fibers at least on the sheet surface of the copper alloy sheet obtained by crystal orientation analysis using an EBSD method is 3.0 or less, the tensile strength is 500 MPa or more and 900 MPa or less, and the electrical conductivity is 30% IACS or more.
[0015] (2) With respect to the accumulation of crystal planes facing the normal direction (ND) of the sheet surface obtained from the crystal orientation analysis, the area of a region having crystal planes whose angle between the normal direction (ND) and the normal direction of the (100) plane is within 10° is 10% or less, The copper alloy sheet material according to (1) above.
[0016] (3) The copper alloy sheet material according to (1) or (2), wherein the alloy composition further contains at least one optional additional component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a total amount of 0.10 mass% or more and 1.00 mass% or less.
[0017] (4) A copper alloy sheet material for drawing, comprising the copper alloy sheet material according to any one of (1) to (3) above.
[0018] (5) A drawn product obtained by drawing the copper alloy sheet material according to any one of (1) to (3) above.
[0019] According to the present invention, it is possible to provide a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product, which have high tensile strength and high electrical conductivity and are capable of obtaining excellent drawing workability.
[0020] Fig. 1 is a schematic diagram showing a main part of an example of a processing machine used in a repeated bending back processing step among the steps of manufacturing a copper alloy sheet material of the present invention. Fig. 2 is a diagram illustrating a method for measuring a sheet thickness near the tip of a punch.
[0021] Next, an embodiment of the present invention will be described. The following description shows examples of embodiments of the present invention and does not limit the scope of the claims.
[0022] The copper alloy sheet according to the present invention has an alloy composition containing Ni in the range of 1.00 mass% to 5.00 mass%, Si in the range of 0.20 mass% to 1.30 mass%, and the balance consisting of Cu and unavoidable impurities, and has an average orientation density of α-fibers at least on the sheet surface of the copper alloy sheet obtained from crystal orientation analysis by an EBSD method of 3.0 or less, a tensile strength in the range of 500 MPa to 900 MPa, and an electrical conductivity of 30% IACS or more.
[0023] The copper alloy sheet of the present invention contains at least appropriate amounts of Ni and Si and is produced under appropriate production conditions, thereby reducing the orientation density of α-fibers at least on the sheet surface to 3.0 or less, thereby suppressing a decrease in sheet thickness near the tip of the punch in a drawn product. Furthermore, the copper alloy sheet of the present invention contains at least appropriate amounts of Ni and Si, thereby increasing the tensile strength and electrical conductivity of the copper alloy sheet. Therefore, the copper alloy sheet of the present invention can provide a copper alloy sheet, a copper alloy sheet for drawing, and a drawn product that have high tensile strength and high electrical conductivity and are capable of achieving excellent drawing workability.
[0024] [1] Alloy composition of copper alloy sheet The copper alloy sheet of the present invention has an alloy composition containing, as essential components, Ni in the range of 1.00 mass% to 5.00 mass% and Si in the range of 0.20 mass% to 1.30 mass%. The reasons for limiting the alloy composition of the copper alloy sheet will be explained below.
[0025] (Ni: 1.00 mass% or more and 5.00 mass% or less) Ni (nickel) is an important component that has the effect of increasing the tensile strength of a copper alloy sheet material, and is contained in a range of 1.00 mass% or more and 5.00 mass% or less. Here, if the Ni content is less than 1.00 mass%, the desired high tensile strength cannot be obtained. Furthermore, if the Ni content is more than 5.00 mass%, a coarse second phase consisting of a compound with Si is likely to be generated, and this second phase is likely to become the starting point of cracks during drawing. Furthermore, if the Ni content is more than 5.00 mass%, the electrical conductivity of the copper alloy sheet material decreases. Therefore, from the viewpoint of increasing the tensile strength and electrical conductivity of the copper alloy sheet and making it difficult for cracks to occur in the drawn product, the Ni content is in the range of 1.00 mass% to 5.00 mass%, preferably in the range of 1.00 mass% to 4.50 mass%, more preferably in the range of 1.50 mass% to 4.50 mass%, and even more preferably in the range of 2.00 mass% to 4.00 mass%. In particular, from the viewpoint of increasing the electrical conductivity of the copper alloy sheet, the Ni content is preferably 4.50 mass% or less.
[0026] (Si: 0.20 mass% or more and 1.30 mass% or less) Si (silicon) is an important component that has the effect of increasing the tensile strength of a copper alloy sheet material, and is contained in a range of 0.20 mass% or more and 1.30 mass% or less. Here, if the Si content is less than 0.10 mass%, the desired high tensile strength cannot be obtained. Furthermore, if the Si content is more than 1.30 mass%, a coarse second phase consisting of a compound with Ni is likely to be generated, and this second phase is likely to become the starting point of cracks during drawing. Furthermore, if the Si content is more than 1.30 mass%, the electrical conductivity of the copper alloy sheet material decreases. Therefore, from the viewpoint of increasing the tensile strength and electrical conductivity of the copper alloy sheet and making it difficult for cracks to occur in the drawn product, the Si content is in the range of 0.20 mass% to 1.30 mass%, preferably in the range of 0.20 mass% to 1.10 mass%, more preferably in the range of 0.30 mass% to 1.10 mass%, and more preferably in the range of 0.50 mass% to 1.00 mass%. In particular, from the viewpoint of increasing the electrical conductivity of the copper alloy sheet, the Si content is preferably 1.10 mass% or less.
[0027] <Optionally Added Component> Furthermore, the copper alloy sheet material of the present invention may further contain, as an optional added component, at least one optional added component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a range of 0.10 mass% or more and 1.00 mass% or less in total.
[0028] (Sn: 0.10% by mass or more and 0.30% by mass or less) Sn (tin) is a component that has the effect of improving stress relaxation resistance. To exert this effect, the Sn content is preferably 0.10% by mass or more. On the other hand, if the Sn content exceeds 0.30% by mass, the electrical conductivity tends to decrease. For this reason, the Sn content is preferably in the range of 0.10% by mass or more and 0.30% by mass or less.
[0029] (Zn: 0.10% by mass or more and 0.50% by mass or less) Zn (zinc) is a component that has the effect of improving the adhesion and migration properties of Sn plating. To exert this effect, the Zn content is preferably 0.10% by mass or more. On the other hand, if the Zn content exceeds 0.50% by mass, the electrical conductivity tends to decrease. For this reason, the Zn content is preferably in the range of 0.10% by mass or more and 0.50% by mass or less.
[0030] (Mg: 0.10% by mass or more and 0.30% by mass or less) Mg (magnesium) is a component that has the effect of improving stress relaxation resistance. To exert this effect, the Mg content is preferably 0.10% by mass or more. On the other hand, if the Mg content exceeds 0.30% by mass, the electrical conductivity tends to decrease. Therefore, the Mg content is preferably in the range of 0.10% by mass or more and 0.30% by mass or less.
[0031] (Fe: 0.05% by mass or more and 0.30% by mass or less) Fe (iron) is a component that has the effect of suppressing coarsening of crystal grains after dynamic recrystallization and the effect of preventing roughness of the surface of a drawn product in the hot rolling step [Step 3] described below. To exert this effect, the Fe content is preferably 0.05% by mass or more. Furthermore, if the Fe content exceeds 0.30% by mass, coarse crystallized products containing Fe are likely to be generated during casting, which makes it easier for cracks to form. For this reason, the Fe content is preferably in the range of 0.05% by mass or more and 0.30% by mass or less.
[0032] (Cr: 0.05% by mass or more and 0.30% by mass or less) Cr (chromium) is a component that has the effect of suppressing coarsening of crystal grains after dynamic recrystallization and the effect of preventing roughness of the surface of a drawn product in the hot rolling step [Step 3] described below. To exert this effect, the Cr content is preferably 0.05% by mass or more. Furthermore, if the Cr content exceeds 0.30% by mass, coarse crystallized products containing Cr are likely to be generated during casting, which makes it easier for cracks to form. For this reason, the Cr content is preferably in the range of 0.05% by mass or more and 0.30% by mass or less.
[0033] (Total content of optional components: 0.10 mass % or more and 1.00 mass % or less) In order to obtain the effects of the optional components described above, it is preferable that the total content of these optional components be 0.10 mass % or more. On the other hand, if these optional components are contained in large amounts, the electrical conductivity decreases, so it is preferable that the total content of the optional components be 1.00 mass % or less.
[0034] (Balance: Cu and inevitable impurities) The copper alloy constituting the copper alloy sheet material has an alloy composition consisting of the above-mentioned components, with the balance being Cu (copper) and inevitable impurities. The term "unavoidable impurities" as used herein generally refers to impurities present in raw materials for metal products or unavoidably mixed in during the manufacturing process. These impurities are essentially unnecessary but are tolerated in trace amounts because they do not affect the properties of the metal product. Examples of inevitable impurities include non-metallic elements such as sulfur (S), carbon (C), and oxygen (O), and metallic elements such as antimony (Sb). The upper limit of the content of these components can be, for example, 0.05% by mass for each of the above components, or 0.20% by mass for the total amount of the above components.
[0035] [2] Average value of α-fiber orientation density In the copper alloy sheet of the present invention, the average value of the α-fiber orientation density at least on the sheet surface of the copper alloy sheet obtained by crystal orientation analysis using the EBSD method is 3.0 or less. Here, if the average value of the α-fiber orientation density exceeds 3.0, a reduction in sheet thickness is likely to occur near the tip of the punch in a drawn product. On the other hand, if the average value of the α-fiber orientation density is less than 0.5, the peak height of the waviness in the drawn product will be low, making it difficult to form bridges during progressive pressing. Therefore, the average value of the α-fiber orientation density is preferably 0.5 or more. Note that, if no bridges are formed, the average value of the α-fiber orientation density may be less than 0.5. From the viewpoint of preventing a reduction in sheet thickness near the tip of the punch in a drawn product, the average value of the α-fiber orientation density is preferably 2.8 or less, more preferably 2.3 or less, and even more preferably 2.0 or less. Therefore, the average orientation density of the α-fibers is preferably in the range of 0.5 to 2.8, more preferably in the range of 0.5 to 2.3, and even more preferably in the range of 0.5 to 2.0.
[0036] Here, the average value of the orientation density of α-fibers can be obtained from crystal orientation analysis data calculated using analysis software (OIM Analysis, manufactured by TSL) from crystal orientation data continuously measured using an EBSD detector attached to a high-resolution scanning analytical electron microscope (JEOL Ltd., JSM-7001FA). "EBSD" stands for Electron Backscatter Diffraction, and refers to a crystal orientation analysis technique that utilizes reflected electron Kikuchi diffraction, which occurs when an electron beam is irradiated onto a copper plate sample in a scanning electron microscope (SEM). "OIM Analysis" is software for analyzing data measured by EBSD. Measurements can be performed on a cross section along the rolling direction of a copper alloy plate embedded in resin and finished by mechanical polishing and buffing (colloidal silica). Measurements may also be performed on the surface of an electropolished copper alloy plate. The measurement area on these cross sections and plate surfaces is approximately 400 μm × 800 μm, and measurements can be performed with a step size of 0.5 μm. In both cross-sectional and plate surface measurements, if the above field of view size cannot be obtained due to the sample size, measurements can be taken in multiple fields of view and the average value can be used.
[0037] In this way, among the crystal orientation data obtained by the EBSD method, measurement points where the reliability index CI value is 0.1 or more are analyzed to obtain a crystal orientation distribution function (ODF) expressed by Euler angles (φ1, Φ, φ2).For α-fiber orientations where φ1 is in the range of 0 to 35°, the average value of the ODF intensity when a randomly oriented sample is used as the reference (reference value = 1) can be calculated as the average value of the α-fiber orientation density.
[0038] [3] Area ratio of the region having a crystal plane where the angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane is within 10°. Regarding the accumulation of crystal planes facing the normal direction (ND) of the sheet surface obtained by crystal orientation analysis using the EBSD method, the copper alloy sheet of the present invention preferably has an area of the region having a crystal plane where the angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane is within 10°, as a ratio to the area of the measured region of the sheet surface, of 10% or less. Here, if the area of the region where the angle difference between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane is within 10° is greater than 10% of the area of the measured region of the sheet surface, a reduction in sheet thickness is likely to occur near the tip of the punch in a drawn product. This is because, in materials where the (100) plane of the crystal is oriented on or near the sheet surface, compressive deformation is difficult during flange deformation during drawing due to the characteristics of crystal slip deformation, so a large force is required for flange deformation. As a result, it is thought that a reduction in plate thickness is likely to occur near the tip of the punch, which pulls the load during drawing.
[0039] Here, the area of the region having a crystal plane where the angle between the normal direction (ND) of the plate surface and the normal direction of the (100) plane is within 10° can be determined by analyzing measurement points among the crystal orientation data obtained by the above-mentioned EBSD method where the reliability index CI value is 0.1 or more, and calculating the proportion of the area of the region having a crystal plane (atomic plane) where the angle between the normal direction (ND) of the (100) plane and the normal direction of the plate surface is within 10° to the area of the measurement region.
[0040] [4] Tensile strength of copper alloy sheet The copper alloy sheet of the present invention has a tensile strength in the range of 500 MPa or more and 900 MPa or less. As a result, even when the copper alloy sheet is used for small or thin parts such as electrical and electronic components or automotive components, the desired tensile strength can be obtained, making the copper alloy sheet suitable for use in various drawn products. On the other hand, if the tensile strength exceeds 900 MPa, the fracture resistance of the copper alloy sheet increases, but the deformation resistance during drawing also increases, and the sheet thickness reduction rate in drawing tests tends to increase. Therefore, the tensile strength of the copper alloy sheet is in the range of 500 MPa or more and 900 MPa or less, and preferably in the range of 550 MPa or more and 900 MPa or less. Here, the tensile strength can be, for example, the tensile strength when pulled in a direction parallel to the rolling direction. The tensile strength is measured using two test pieces of No. 13B specified in JIS Z2241, cut out so that the longitudinal direction is parallel to the rolling direction, and the average value of the tensile strength obtained from the two test pieces is taken as the measured value of the tensile strength.
[0041] In particular, from the viewpoint of further improving the drawing workability by further reducing the sheet thickness reduction rate in the drawing work test, it is preferable that the average value of the orientation density of α-fibers in the copper alloy sheet is in the range of 0.5 or more and 2.3 or less, and that the tensile strength of the copper alloy sheet is in the range of 780 MPa or more and 900 MPa or less.
[0042] [5] Electrical Conductivity of Copper Alloy Sheet The copper alloy sheet of the present invention has an electrical conductivity of 30% IACS or more. This allows the copper alloy sheet to have high electrical conductivity, and therefore the copper alloy sheet can also be used for drawn products that require electromagnetic wave shielding and heat dissipation. Therefore, the electrical conductivity of the copper alloy sheet is 30% IACS or more, and preferably 35% IACS or more. Here, the electrical conductivity (IACS; International Annealed Copper Standard) is measured twice using a four-terminal method, and the average of the electrical conductivities obtained by the two measurements is used as the measured electrical conductivity.
[0043] [6] Example of a manufacturing method for a copper alloy sheet The above-mentioned copper alloy sheet can be realized by controlling the alloy composition and the manufacturing process in combination, and the manufacturing process is not particularly limited. Among them, the following method can be mentioned as an example of a manufacturing process that can obtain such high tensile strength and excellent drawing workability.
[0044] In one example of the method for producing a copper alloy sheet of the present invention, a copper alloy material having an alloy composition equivalent to that of the above-mentioned copper alloy sheet is sequentially subjected to at least a melting and casting step (step 1), a reheating step (step 2), a hot rolling step (step 3), a first cold rolling step (step 4), an intermediate annealing step (step 5), a repeated bending back processing step (step 6), a solution treatment step (step 7), an aging heat treatment step (step 8), a second cold rolling step (step 9), and a low-temperature annealing step (step 10).
[0045] (i) Melting and Casting Step [Step 1] In the melting and casting step [Step 1], a copper alloy material having an alloy composition equivalent to the above-mentioned alloy composition is melted and cast to produce an ingot of a predetermined shape (e.g., thickness 30 mm, width 100 mm, length 150 mm). In the melting and casting step [Step 1], the copper alloy material is preferably melted and cast in air, an inert gas atmosphere, or a vacuum using a high-frequency melting furnace. Note that the alloy composition of the copper alloy material may not necessarily be completely identical to that of the copper alloy sheet material produced due to the addition of components that adhere to or volatilize the melting furnace in each manufacturing step, but it has substantially the same alloy composition as the copper alloy sheet material.
[0046] (ii) Reheating Step [Step 2] The reheating step [Step 2] is a step of heat treating the ingot after the casting step [Step 1]. The conditions for the heat treatment in the reheating step [Step 2] are preferably a temperature (heat treatment temperature) in the range of 900 ° C. to 1050 ° C., and a holding time (heat treatment time) at the temperature in the range of 1 hour to 10 hours. If the temperature is less than 900 ° C., the temperature drop at the time of entering the hot rolling step [Step 3] described later will cause coarse precipitates to form, and the solid solubility will decrease in the solution treatment step [Step 7]. Furthermore, the amount of precipitation strengthening in the aging heat treatment step [Step 8] will decrease, making it difficult to obtain a copper alloy sheet material with high tensile strength. On the other hand, if the temperature exceeds 1050 ° C., the grain boundaries will be weakened, and cracks will easily occur in the hot-rolled material after the hot rolling step [Step 3].
[0047] (iii) Hot Rolling Step [Step 3] The hot rolling step [Step 3] is a step in which the ingot that has been subjected to the reheating step [Step 2] is hot rolled until it reaches a predetermined thickness to produce a hot-rolled material. The conditions for the hot rolling step [Step 3] can be set so that dynamic recrystallization occurs, and for example, the rolling temperature can be set to 700°C or higher and the total processing rate (total reduction rate) can be set to 50% or higher. On the other hand, if dynamic recrystallization does not occur sufficiently in the hot rolling step [Step 3], the resulting copper alloy sheet material is likely to have a non-uniform structure.
[0048] The "working rate" (rolling reduction) in this specification is a value obtained by subtracting the cross-sectional area after rolling from the cross-sectional area before rolling, dividing the value by the cross-sectional area before rolling, and multiplying the result by 100, expressed as a percentage, and is expressed by the following formula: [Working rate] = {([cross-sectional area before rolling] - [cross-sectional area after rolling]) / [cross-sectional area before rolling]} x 100 (%)
[0049] As an example, when the rolling temperature in the hot rolling step [Step 3] is 700°C, the sum of the processing rate calculated from the cross-sectional area before the start of rolling and the cross-sectional area after the passes completed before reaching 700°C can be used as the total processing rate (total rolling reduction), and the total processing rate (total rolling reduction) in the temperature range from the heat treatment temperature to 700°C in the reheating step [Step 2] can be set to 50% or more.
[0050] The temperature of the ingot during the hot rolling step [step 3] can be measured with a radiation thermometer.
[0051] The hot-rolled material is preferably cooled after the hot working step [Step 3]. Here, the means for cooling the hot-rolled material is not particularly limited, but from the viewpoint of, for example, making it difficult for crystal grains to become coarse, it is preferable to use a means for increasing the cooling rate as much as possible, and for example, it is preferable to set the cooling rate to 10°C / second or more by means such as water cooling.
[0052] Here, the cooled hot-rolled material may be subjected to facing, in which the surface is scraped off. By performing facing, it is possible to remove oxide films and defects on the surface that have occurred in the hot working step [Step 3]. The conditions for facing may be any conditions that are normally used, and are not particularly limited. The amount of material scraped off from the surface of the hot-rolled material by facing can be appropriately adjusted based on the conditions of the hot working step [Step 3], and can be, for example, about 1 mm to 5 mm from both the front and back sides of the hot-rolled material.
[0053] (iv) First cold rolling step [step 4] The first cold rolling step [step 4] is a step of cold rolling the hot-rolled material after the hot working step [step 3]. The rolling in the first cold rolling step [step 4] can be performed at any reduction rate according to the plate thickness of the product, and for example, the total working rate can be in the range of 70.0% to 99.9%.
[0054] (v) Intermediate Annealing Step [Step 5] The intermediate annealing step [Step 5] is a step in which the cold-rolled material after the first cold rolling step [Step 4] is subjected to a heat treatment according to the alloy composition.
[0055] The annealing conditions in the intermediate annealing step [Step 5] are preferably such that the ultimate temperature is in the range of 600 ° C. or higher and 800 ° C. or lower, and the holding time at the ultimate temperature is in the range of 10 seconds to 1 hour, from the viewpoint of efficiently recovering dislocations generated in the cold-rolled material. Here, if the ultimate temperature is less than 600 ° C., NiSi compounds are precipitated, and in the solution treatment step [Step 7] described later, the area having a crystal plane in which the angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane is within 10 ° is likely to increase on at least the sheet surface of the copper alloy sheet. In particular, the ultimate temperature in the intermediate annealing step [Step 5] is preferably 650 ° C. or higher, from the viewpoint of further improving the drawing workability of the copper alloy sheet. On the other hand, in order to recover dislocations generated in the cold-rolled material, the ultimate temperature in the intermediate annealing step [Step 5] is sufficient at 800 ° C., and heat treatment at a higher temperature is not desirable from the viewpoint of productivity.
[0056] Furthermore, if the holding time at the reached temperature in the intermediate annealing step [Step 5] is less than 10 seconds, the recovery of dislocations generated in the cold-rolled material is likely to be insufficient. On the other hand, since a holding time at the reached temperature in the intermediate annealing step [Step 5] of 1 hour is sufficient to recover the dislocations generated in the cold-rolled material, heat treatment for a longer time than this is not desirable from the viewpoint of productivity.
[0057] After the intermediate annealing step [Step 5] is performed, it is preferable to cool the cold-rolled material from the temperature reached in the intermediate annealing step [Step 5] to a temperature of 300°C or less, which is a temperature at which new precipitation is unlikely to occur. At this time, it is preferable to cool the cold-rolled material at a cooling rate of 1°C / s or more. By increasing the cooling rate, it becomes difficult for precipitation strengthening of the cold-rolled material to progress, so that it is possible to easily perform repeated bending back on the cooled cold-rolled material.
[0058] (vi) Repeated Bending-Back Process [Step 6] The repeated bending-back process [Step 6] is a process in which the cold-rolled material after the intermediate annealing process [Step 5] is repeatedly bent back. More specifically, this is a process in which the cold-rolled material is alternately bent back repeatedly from both sheet surfaces. For example, this can be performed using a processing machine 1 as shown in FIG. 1 by alternately pressing work rolls 2 against both sheet surfaces of the cold-rolled material to bend back the cold-rolled material 3. By performing this repeated bending-back process, the deformation form of the material can be changed compared to conventional cold rolling, and the strain state (distribution, density, etc.) and crystal orientation in the structure after the bending-back process can be made different from those obtained by conventional cold rolling. As a result, the orientation density of α-fiber can be reduced at least on the sheet surface of the copper alloy sheet. In this regard, it has been difficult to reduce the orientation density of α-fiber in conventional cold-rolled materials because a recrystallized texture is formed based on the strain and rolling texture of the cold rolling when the material is recrystallized in a solution treatment process, etc. In this regard, the recrystallized texture obtained by heat-treating the cold-rolled material that has been subjected to the repeated bending back process [Step 6] can control the α-fiber within a specified range.
[0059] In this repeated bending-back processing step [Step 6], a cycle of bending deformation so that the ratio of the bending radius to the thickness of the cold-rolled material (ratio of bending radius / thickness) is in the range of 8.0 to 10.0, and then unbending this bending deformation is repeated 4 to 10 times.
[0060] Here, when the ratio of the bending radius to the thickness of the cold-rolled material is less than 8.0, cracks are likely to occur on the surface of the cold-rolled material. On the other hand, when the ratio of the bending radius to the thickness of the cold-rolled material is greater than 10.0 or when the number of repeated bending back processes is less than four, the amount of strain caused by the repeated bending back process step [Step 6] is reduced, resulting in an excessive increase in the orientation density of α-fibers, and therefore a decrease in the drawing workability of the copper alloy sheet. In particular, the ratio of the bending radius to the thickness of the cold-rolled material is preferably in the range of 8.0 to 9.0. Note that the bending back process in the repeated bending back process step [Step 6] may be repeated 10 or more times, but since the work hardening saturates and the effect of further bending becomes smaller, repeating it 10 or more times is not desirable from the viewpoint of productivity.
[0061] In particular, when using a processing machine 1 as shown in Fig. 1 in which work rolls 2 are pressed alternately against both plate surfaces of the cold-rolled material, the bending radius in the unbending process may be approximated to the radius of the work rolls 2. Note that the processing machine 1 shown in Fig. 1 is an example in which a cycle of bending deformation and unbending processing is performed seven times.
[0062] (vii) Solution Treatment Step [Step 7] The solution treatment step [Step 7] is a step in which the cold-rolled material after the repeated bending back processing step [Step 6] is subjected to heat treatment to recrystallize and then cooled. Here, the heat treatment conditions in the solution treatment step [Step 7] can be, for example, a temperature range of 700 ° C. to 1000 ° C., and a holding time at the temperature range of 10 seconds to 60 seconds. Here, if the temperature is less than 700 ° C. or the holding time is less than 10 seconds, the amount of precipitation strengthening in the aging heat treatment step [Step 8] described below decreases, thereby reducing the tensile strength of the copper alloy sheet. On the other hand, if the temperature exceeds 1000 ° C. or the holding time exceeds 60 seconds, the crystal grain size tends to coarsen, resulting in a decrease in the tensile strength of the copper alloy sheet. Therefore, from the viewpoint of increasing the tensile strength of the copper alloy sheet, it is preferable to set the temperature to 950 ° C. or less.
[0063] The solution-treated material after the solution treatment step [Step 7] is preferably cooled immediately. More specifically, the solution-treated material after the solution treatment step [Step 7] is preferably cooled at a cooling rate of 40°C / s or more. Here, if the cooling rate is less than 40°C / s, coarse precipitates are formed during cooling, which reduces the amount of precipitation strengthening in the aging heat treatment step [Step 8], and the tensile strength of the copper alloy sheet tends to decrease.
[0064] (viii) Aging Heat Treatment Step [Step 8] The aging heat treatment step [Step 8] is a step of precipitation strengthening by heat treatment of the cooled solution-treated material. Here, the conditions for the heat treatment in the aging heat treatment step [Step 8] are that the ultimate temperature is in the range of 400°C or higher and 600°C or lower, and the holding time at the ultimate temperature is in the range of 1 hour or higher and 10 hours or lower. Here, if the ultimate temperature is lower than 400°C or the holding time is shorter than 1 hour, precipitation strengthening is difficult to achieve, and the tensile strength and electrical conductivity of the copper alloy sheet material are likely to decrease. On the other hand, if the ultimate temperature exceeds 600°C or the holding time exceeds 10 hours, the precipitates become coarse, and the tensile strength of the copper alloy sheet material is likely to decrease.
[0065] (ix) Second Cold Rolling Step [Step 9] The second cold rolling step [Step 9] is a step of further cold rolling the cold-rolled material after the aging heat treatment step [Step 8]. Here, the total working ratio in the second cold rolling step [Step 9] is preferably in the range of 5% to 50%, and more preferably in the range of 5% to 40%. Here, if the total working ratio is less than 5%, the amount of work hardening is small, so the tensile strength of the copper alloy sheet is likely to decrease. Furthermore, if the total working ratio is greater than 50%, the drawing workability of the copper alloy sheet is reduced. In particular, from the viewpoint of further increasing the tensile strength of the copper alloy sheet and further improving the drawing workability of the copper alloy sheet, the total working ratio in the second cold rolling step [Step 9] is preferably 40% or less. This second cold rolling step [Step 9] can be performed according to the desired tensile strength.
[0066] The second cold rolling step [Step 9] is preferably performed at a relatively high working ratio of 20% or more in applications such as connector hold-down, where a part having a spring mechanism is combined into a drawn structure, where the drawing depth is relatively shallow, at 5 mm or less, and tensile strength is prioritized over drawing workability, thereby increasing the tensile strength of the copper alloy sheet material. On the other hand, in applications such as camera module cases, shielding cases, vibration device cases, and battery cases, where the drawing depth is relatively deep, at 5 mm or more, and drawing workability is prioritized over tensile strength, the second cold rolling step [Step 9] is preferably performed at a low working ratio of 20% or less.
[0067] (x) Low-Temperature Annealing Step [Step 10] The low-temperature annealing step [Step 10] is an annealing step in which the cold-rolled material after the second cold rolling step [Step 9] is subjected to heat treatment. The conditions for the heat treatment in this low-temperature annealing step [Step 10] are preferably such that the ultimate temperature is in the range of 300 ° C. or higher and 500 ° C. or lower, and the holding time at the ultimate temperature is in the range of 10 seconds or higher and 30 minutes or lower. Here, if the ultimate temperature is lower than 300 ° C. or the holding time is shorter than 10 seconds, excessive strain remains in the cold-rolled material after annealing, thereby reducing the drawing workability of the copper alloy sheet material. On the other hand, if the ultimate temperature exceeds 500 ° C. or the holding time at the ultimate temperature exceeds 30 minutes, the work hardening due to cold rolling disappears.
[0068] The heating and cooling rates before and after the annealing in the low-temperature annealing step [step 10] are not particularly limited, but can be, for example, in the range of 1° C. / s to 100° C. / s.
[0069] [7] Uses of Copper Alloy Sheet The copper alloy sheet of the present invention preferably constitutes a copper alloy sheet for drawing. That is, the copper alloy sheet of the present invention is particularly suitable for obtaining drawn products by drawing, and is suitable for forming, for example, parts for electronic devices, electronic components, automotive components, etc. More specifically, it is suitable for use in connectors, lead frames, relays, switches, sockets, shield cases, shield cans, camera module cases, vibration device cases, heat dissipation parts for liquid crystal and organic EL displays, battery and automotive connectors, shield cases, shield cans, etc. for electronic devices or electronic components that require miniaturization and high current.
[0070] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, but includes all aspects encompassed by the concept of the present invention and the scope of the claims, and can be modified in various ways within the scope of the present invention.
[0071] Next, in order to further clarify the effects of the present invention, examples of the present invention and comparative examples will be described, but the present invention is not limited to these examples of the present invention.
[0072] (Inventive Examples 1 to 18 and Comparative Examples 1 to 17) Various copper alloy materials having the alloy compositions shown in Table 1 were melted, cooled in an air atmosphere, and cast to obtain ingots in a melting and casting process [Step 1]. The ingots were then subjected to a reheating process [Step 2] in which they were heat-treated at an ultimate temperature (heat treatment temperature) of 1000°C and held at that temperature for 1 hour (heat treatment time), followed by a hot-rolling process [Step 3] in which the temperature was immediately raised to a range of 700°C to 1000°C and the ingot was rolled such that the longitudinal direction of the ingot was the rolling direction, resulting in a total processing rate of 50% or more, to obtain hot-rolled materials. The ingots were then cooled to room temperature by water cooling.
[0073] The cooled hot-rolled material was subjected to facing to remove approximately 1 mm to 2 mm from both the front and back surfaces to remove the oxide film on the surface, and then subjected to a first cold-rolling step [step 4] in which the hot-rolled material was rolled so that the longitudinal direction of the hot-rolled material was the rolling direction under conditions where the total processing rate was 98.0%.
[0074] The rolled material after the first cold rolling step [step 4] was subjected to an intermediate annealing step [step 5] in which heat treatment was performed at the attained temperature and holding time shown in Table 2. Next, using the processing machine 1 shown in FIG. 1, a repeated bending back processing step [step 6] was performed in which the cold rolled material was repeatedly bent back under the conditions of the ratio of the bending radius to the plate thickness of the cold rolled material and the number of bending backs [times] shown in Table 2.
[0075] The cold-rolled material after the repeated bending back processing step [step 6] was subjected to a solution treatment step [step 7] in which heat treatment was performed at the attained temperature and holding time shown in Table 2, and then cooled to room temperature at a cooling rate of 100°C / s.
[0076] The cooled solution-treated material was subjected to an aging heat treatment step [Step 8] in which heat treatment was performed at the ultimate temperature and for the holding time shown in Table 2, and then to a second cold rolling step [Step 9] in which rolling was performed in the longitudinal direction under the total working ratio conditions shown in Table 2.
[0077] The rolled material after the second cold rolling step [step 9] was subjected to a low-temperature annealing step [step 10] in which heat treatment was performed at the attained temperature and holding time shown in Table 2, thereby producing the copper alloy sheet material of the present invention.
[0078] On the other hand, for Comparative Example 15, a copper alloy sheet was produced without performing the repeated bending back process [Step 6]. For Comparative Example 16, a copper alloy sheet was produced without performing the intermediate annealing process [Step 5] and the repeated bending back process [Step 6], similar to the copper alloy sheet of Patent Document 1. For Comparative Example 17, a copper alloy sheet was produced without performing the repeated bending back process [Step 6] and the aging heat treatment process [Step 8], similar to the copper alloy sheet of Patent Document 2.
[0079] In Table 1, among the constituent elements other than copper (Cu), Ni (nickel), and Si (silicon), Sn (tin), Zn (zinc), Mg (magnesium), Fe (iron), and Cr (chromium) are listed as optional added elements and are separated from the other elements. In Table 1, a horizontal line "-" is entered in the column for an element not included in the alloy composition of the copper alloy material, indicating that the element is not included, or if it is included, its amount is below the detection limit.
[0080] [Various Measurement and Evaluation Methods] The copper alloy sheets according to the above-described invention examples and comparative examples were used to carry out the following characteristic evaluations. The evaluation conditions for each characteristic were as follows.
[0081] [1] Average value of α-fiber orientation density of copper alloy sheet The average value of the α-fiber orientation density of the copper alloy sheet was obtained from crystal orientation analysis data calculated using analysis software (manufactured by TSL, OIM Analysis) from crystal orientation data continuously measured using an EBSD detector attached to a high-resolution scanning analytical electron microscope (manufactured by JEOL Ltd., JSM-7001FA) for the copper alloy sheets obtained in the present invention examples and comparative examples. The surface (plate surface) of the copper alloy sheet was electrolytically polished, and the measurement was performed in a field of view of approximately 400 μm × 800 μm on the electrolytically polished surface with a step size of 0.5 μm.
[0082] Among the crystal orientation data obtained by the EBSD method in this way, measurement points where the reliability index CI value was 0.1 or more were used as the analysis targets, and when a crystal orientation distribution function (ODF) expressed by Euler angles (φ1, Φ, φ2) was obtained as crystal orientation analysis data, for α-fiber orientations where φ1 was in the range of 0 to 35°, the average value of the ODF intensity when a randomly oriented sample was used as the reference (reference value = 1) was calculated as the average orientation density of α-fiber. In this example, an average value of the orientation density of α-fiber of 3.0 or less was considered to be acceptable. The results are shown in Table 3.
[0083] [2] Area ratio of the region having a crystal plane where the angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane is within 10° The area ratio of the region having a crystal plane where the angle between the normal direction (ND) of the sheet surface of the copper alloy sheet and the normal direction of the (100) plane is within 10° was determined by analyzing measurement points where the reliability index CI value was 0.1 or more among the crystal orientation data obtained by the EBSD method described above. The area ratio of the region having a crystal plane (atomic plane) where the angle between the normal direction (ND) of the (100) plane and the normal direction of the sheet surface is within 10° was calculated. The results are shown in Table 3.
[0084] [3] Measurement of tensile strength of copper alloy sheet material Tensile strength was measured using two test pieces of No. 13B specified in JIS Z2241, cut out from the test material so that the longitudinal direction was parallel to the rolling direction, and the average value of the tensile strength obtained from the two test pieces was taken as the measured value. In this example, a tensile strength in the range of 500 MPa or more and 900 MPa or less was considered to be acceptable. The results are shown in Table 3.
[0085] [4] Measurement of electrical conductivity of copper alloy sheet The electrical conductivity of the copper alloy sheet was measured twice using the four-terminal method, and the average value of the two measurements was used as the measured electrical conductivity. In this example, a conductivity of 30% IACS or more was considered to be acceptable. The results are shown in Table 3.
[0086] [5] Evaluation of drawing workability of copper alloy sheet material The drawing workability of copper alloy sheet material was evaluated by using a 40 mm diameter blank formed by press punching from a copper alloy sheet material with a thickness of 0.2 mm, applying a lubricant (product name: Preton R-303P, manufactured by Sugimura Chemical Industry Co., Ltd.) to the sheet surface, and using a die with a shoulder curvature radius of 3 mm and a cylindrical punch with a tip diameter of 20 mm and a tip corner curvature radius of 3 mm, with a punch-to-die clearance of 0.27 mm, the punch was pressed into the center of the blank to form a cylindrical cup. The reduction in sheet thickness near the tip of the punch in the cup was evaluated. At this time, the blank holder pressure, which is the pressure pressing the copper alloy sheet material as the workpiece, was 1500 N.
[0087] Here, the thickness near the tip of the punch was measured by embedding a cylindrical cup, which was a drawn product, in resin, mechanically polishing a cross section 10 along the rolling direction of the bottom surface including the central axis of the cylinder as shown in Figure 2, and observing the R portion 11 near the tip of the punch in the cross section 10 with an optical microscope. At this time, a tangent line A was drawn that forms an angle of 45° with the bottom surface 12 of the drawn product so as to be in contact with the R portion 11, and a perpendicular line B was drawn that passes through the tangent line A and the apex of the R portion 11 and is perpendicular to the tangent line A, and the length of the perpendicular line B, which is a line segment that crosses the cross section 10, was determined as the thickness t near the tip of the punch. 1 It was decided.
[0088] This plate thickness t 1 and the thickness t of the copper alloy sheet before drawing. 0 The reduction rate [%] of the plate thickness near the tip of the punch was calculated using the following formula (1): Plate thickness reduction rate [%] = ((t 0 -t 1 ) / t 0 ) × 100 ... (1)
[0089] The calculated reduction rate of the plate thickness was evaluated according to the following evaluation criteria. The results are shown in Table 3.
[0090] <Evaluation criteria for thickness reduction rate near the tip of the punch> "4" (Excellent): When the thickness reduction rate is 2% or less "3" (Good): When the thickness reduction rate is more than 2% but not more than 4% "2" (Acceptable): When the thickness reduction rate is more than 4% but not more than 6% "1" (Unacceptable): When the thickness reduction rate is more than 6% or when the blank breaks during drawing
[0091]
[0092]
[0093]
[0094] From the results in Tables 1 to 3, the copper alloy sheet materials of Inventive Examples 1 to 18 had alloy compositions within the appropriate range of the present invention, an average orientation density of α-fiber of 3.0 or less, a tensile strength in the range of 500 MPa or more and 900 MPa or less, and an electrical conductivity of 30% IACS or more, and at this time, the evaluation of drawing workability was also "2", "3", or "4".
[0095] Therefore, the copper alloy sheets of Examples 1 to 18 of the present invention had high tensile strength and high electrical conductivity, and were able to obtain excellent drawing workability.
[0096] In particular, in the copper alloy sheet materials of Inventive Examples 2 to 18, the temperature reached in the intermediate annealing step [Step 5] was 700°C or higher, so that the region having a crystal plane with a small angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane was reduced, and as a result, in Inventive Examples 2 to 8 and 10 to 18 in particular, the evaluation of drawing workability was higher than that of Inventive Example 1.
[0097] Furthermore, when comparing the copper alloy sheets of Inventive Examples 2, 4, and 5, the ratio of the bending radius to the sheet thickness of the cold-rolled material in the repeated bending back processing step [Step 6] (ratio of bending radius / sheet thickness) of Inventive Examples 4 and 5 was 9 or less, which was smaller than that of Inventive Example 2. It is considered that this introduced a larger amount of bending strain, and therefore the average orientation density of α-fiber on the sheet surface of the copper alloy sheet was smaller, resulting in a higher evaluation of drawing workability compared to Inventive Example 2.
[0098] Furthermore, the copper alloy sheets of Examples 5 to 7, 11, and 17 of the present invention had an average orientation density of α-fiber of 2.3 or less and a tensile strength in the range of 780 MPa or more and 900 MPa or less, and at this time, the reduction rate of the sheet thickness near the tip of the punch was less than 2.0%, and thus, sheets with even better drawing workability were obtained.
[0099] Furthermore, when comparing the copper alloy sheet materials of Inventive Examples 5 and 7, the copper alloy sheet material of Inventive Example 5 reached a temperature of 800°C in the solution treatment step [Step 7], which was lower than that of Inventive Example 7. This is thought to have made it difficult for crystal grains to become coarse, and therefore a tensile strength higher than that of Inventive Example 7 was obtained.
[0100] Furthermore, when comparing the copper alloy sheet materials of Inventive Examples 5 and 8, the copper alloy sheet material of Inventive Example 5 reached a temperature of 480°C in the aging heat treatment step [Step 8], which was lower than that of Inventive Example 8. This is thought to have made it difficult for precipitates to become coarse, and therefore a copper alloy sheet material of Inventive Example 5 had a higher tensile strength than Inventive Example 8.
[0101] Furthermore, when comparing the copper alloy sheets of Inventive Examples 4 and 9, the copper alloy sheet of Inventive Example 4 had a total working ratio of 5% in the second cold rolling step [Step 9], which was lower than that of Inventive Example 9, resulting in a sheet with lower tensile strength than that of Inventive Example 9. Furthermore, because the total working ratio in the second cold rolling step [Step 9] was lower than that of Inventive Example 9, the average orientation density of α-fibers on the sheet surface of the copper alloy sheet was smaller, resulting in a sheet with higher evaluation of drawing workability than that of Inventive Example 9.
[0102] Furthermore, when comparing the copper alloy sheets of Inventive Examples 4 and 10, the copper alloy sheet of Inventive Example 4 reached a temperature of 500°C in the low-temperature annealing step [Step 10], which was higher than that of Inventive Example 10, and therefore had a lower tensile strength than Inventive Example 10. Furthermore, since the reached temperature in the low-temperature annealing step [Step 10] was higher than that of Inventive Example 10, a smaller reduction rate of the sheet thickness near the tip of the punch was obtained compared to Inventive Example 10.
[0103] Moreover, the copper alloy sheet material of Inventive Example 11 had smaller amounts of Ni (nickel) and Si (silicon) added than Inventive Examples 1 to 10 and 12 to 18, and therefore had higher electrical conductivity than Inventive Examples 1 to 10 and 12 to 18. Moreover, the copper alloy sheets of Inventive Examples 1 to 15, 17, and 18 had smaller amounts of Ni (nickel) and Si (silicon) added than Inventive Example 16, and therefore had higher electrical conductivity than Inventive Example 16.
[0104] Furthermore, the copper alloy sheet materials of Inventive Examples 1 to 17 contain at least one optional added component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a total amount of 0.10 mass% or more and 1.00 mass% or less. However, similar to Inventive Example 18 which does not contain any optional added component, the copper alloy sheet materials have high tensile strength and high electrical conductivity, and are highly evaluated for drawing workability.
[0105] Furthermore, the copper alloy sheet materials of the present invention are suitable for forming components for electronic devices, electronic components, automotive components, etc. In particular, for applications in which a spring mechanism is added to a drawn shape, such as the hold-down portion of a connector, the copper alloy sheet materials of Present Invention Examples 8 and 16, which have high tensile strength, are considered to be suitable, and can be selected based on the required characteristics of electrical conductivity and drawing workability. Furthermore, for case applications such as shielding cases, camera module cases, vibration device cases, and vibration device cases, the copper alloy sheet materials of Present Invention Examples 4, 5, 6, 7, 8, and 10, which have high drawing workability, are suitable. Among these, since battery cases generate heat, the copper alloy sheet material of Present Invention Example 11, which has high thermal conductivity proportional to electrical conductivity, is considered to be particularly suitable from the perspective of heat dissipation measures.
[0106] On the other hand, in the copper alloy sheets of Comparative Examples 1 to 17, at least one of the alloy composition, tensile strength, electrical conductivity, and average value of the orientation density of α-fibers on the sheet surface was outside the appropriate range of the present invention, and therefore the tensile strength or electrical conductivity did not reach an acceptable level, or the overall evaluation of drawing workability was evaluated as "1".
[0107] In particular, in the copper alloy sheet material of Comparative Example 1, the temperature reached in the intermediate annealing step [Step 5] was high, which resulted in an increase in the region having a crystal plane in which the angle between the normal direction (ND) of the sheet surface and the normal direction of the (100) plane was within 10°. Therefore, the copper alloy sheet material of Comparative Example 1 was evaluated as "1" in overall evaluation of drawing workability.
[0108] Furthermore, in the copper alloy sheet material of Comparative Example 2, it is considered that the ratio of the bending radius to the sheet thickness of the cold-rolled material (ratio of bending radius / sheet thickness) was large in the repeated bending back processing step [Step 6], and therefore sufficient bending strain was not introduced. As a result, the average orientation density of α-fiber exceeded 3.0, and the overall evaluation of drawing workability was evaluated as "1".
[0109] Furthermore, it is believed that the copper alloy sheet material of Comparative Example 3 was not subjected to sufficient bending strain due to an insufficient number of repetitions of the bending-back process in the repeated bending-back process step [Step 6]. As a result, the average orientation density of the α-fiber exceeded 3.0, and the overall evaluation of the drawing workability was rated as "1".
[0110] In addition, the copper alloy sheet material of Comparative Example 4 had a high temperature reached in the solution treatment step [Step 7], and the tensile strength did not reach an acceptable level. This is thought to be because the temperature reached in the solution treatment step [Step 7] was too high, causing coarsening of crystal grains.
[0111] In addition, the copper alloy sheet material of Comparative Example 5 had a high temperature reached in the aging heat treatment step [Step 8], and the tensile strength did not reach an acceptable level. This is thought to be because the high temperature reached in the aging heat treatment step [Step 8] caused coarsening of precipitates.
[0112] In addition, the copper alloy sheet material of Comparative Example 6 had a low temperature reached in the aging heat treatment step [Step 8], and the tensile strength did not reach an acceptable level. This is thought to be because the temperature reached in the aging heat treatment step [Step 8] was too low, resulting in insufficient precipitation.
[0113] Furthermore, the copper alloy sheet material of Comparative Example 7 had a low total working ratio in the second cold rolling step [Step 9], and the tensile strength did not reach an acceptable level. This is thought to be because the total working ratio in the second cold rolling step [Step 9] was too low, resulting in insufficient work hardening.
[0114] Furthermore, the copper alloy sheet material of Comparative Example 8 had a high total working ratio in the second cold rolling step [step 9], and the blank broke during drawing. This is thought to be because the total working ratio in the second cold rolling step [step 9] was too high, which reduced the ductility of the copper alloy sheet material.
[0115] In addition, the copper alloy sheet material of Comparative Example 9 had a low attained temperature in the low-temperature annealing step [step 10], and the tensile strength was higher than the acceptable level, and the blank broke during drawing. This is thought to be because the attained temperature in the low-temperature annealing step [step 10] was low, resulting in insufficient tempering of the copper alloy sheet material.
[0116] The copper alloy sheet material of Comparative Example 10 is an example in which the electrical conductivity does not reach the acceptable level.
[0117] In addition, the copper alloy sheet material of Comparative Example 11 had a Si (silicon) content in the alloy composition that was greater than the range of the present invention, and the electrical conductivity did not reach an acceptable level.
[0118] In addition, the copper alloy sheet material of Comparative Example 12 had a Ni (nickel) content in the alloy composition that was greater than the range of the present invention, and the electrical conductivity did not reach an acceptable level.
[0119] In addition, the copper alloy sheet material of Comparative Example 13 had a Si (silicon) content in the alloy composition that was lower than the range of the present invention, and the tensile strength did not reach an acceptable level.
[0120] In addition, the copper alloy sheet material of Comparative Example 14 had a Ni (nickel) content in the alloy composition that was lower than the range of the present invention, and the tensile strength did not reach an acceptable level.
[0121] In addition, since the copper alloy sheet material of Comparative Example 15 was not subjected to the repeated bending-back processing step [Step 6], the average orientation density of the α-fiber exceeded 3.0, and the overall evaluation of the drawing workability was evaluated as "1".
[0122] The copper alloy sheet material of Comparative Example 16 was produced in accordance with Patent Document 1, but the intermediate annealing step [Step 5] and the repeated bending back processing step [Step 6] were not performed, and the average orientation density of α-fiber exceeded 3.0, and the overall evaluation of drawing workability was evaluated as "1." The copper alloy sheet material of Comparative Example 16 also differs in alloy composition from the copper alloy sheet material of the present invention.
[0123] The copper alloy sheet of Comparative Example 17 was produced in accordance with Patent Document 2, but the repeated bending back process [Step 6] was not performed, the average orientation density of α-fiber exceeded 3.0, and the overall evaluation of drawing workability was rated as "1". The copper alloy sheet of Comparative Example 17 was also not subjected to the aging heat treatment process [Step 8], and the electrical conductivity did not reach an acceptable level. The copper alloy sheet of Comparative Example 17 also has an alloy composition different from that of the copper alloy sheet of the present invention.
[0124] REFERENCE SIGNS LIST 1 Processing machine 2 Work roll 3 Cold-rolled material 10 Cross section of drawn product 11 R portion 12 Bottom surface of drawn product A Tangent line forming an angle of 45° with the bottom surface of the drawn product B Perpendicular line perpendicular to tangent line A, passing through tangent line A and the apex of the R portion
Claims
1. A copper alloy sheet material having an alloy composition containing Ni in the range of 1.00 mass% to 5.00 mass%, Si in the range of 0.20 mass% to 1.30 mass%, and the balance consisting of Cu and unavoidable impurities, wherein the average orientation density of α-fibers at least on the sheet surface of the copper alloy sheet material obtained by crystal orientation analysis using an EBSD method is 3.0 or less, the tensile strength is in the range of 500 MPa to 900 MPa, and the electrical conductivity is 30% IACS or more.
2. The copper alloy sheet material according to claim 1, wherein, with respect to the accumulation of crystal planes facing the normal direction (ND) of the sheet surface obtained from the crystal orientation analysis, the area of a region having crystal planes whose angle between the normal direction (ND) and the normal direction of the (100) plane is within 10° is a ratio of 10% or less to the area of the measurement region of the sheet surface.
3. The copper alloy sheet material according to claim 1, wherein the alloy composition further contains at least one optional added component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a range of 0.10 mass% or more and 1.00 mass% or less in total.
4. A copper alloy sheet material for drawing, comprising the copper alloy sheet material according to any one of claims 1 to 3.
5. A drawn product obtained by drawing the copper alloy sheet material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Copper alloy strip and method for producing the same
JP2013082968A
Copper alloy sheet material and manufacturing method therefor
JP2017160513A
Copper alloy for electronic material
JP2019077889A