MnZn-BASED FERRITE

The optimized MnZn-based ferrite composition with specific component ratios achieves high incremental magnetic permeability across -40 to 85°C, addressing temperature-related performance issues and defect rates in pulse transformers.

WO2024225176A1PCT designated stage expired Publication Date: 2024-10-31JFE CHEMICAL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015487
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

MnZn-based ferrites used in pulse transformers face challenges in maintaining high incremental magnetic permeability across a wide temperature range (-40 to 85°C) when a DC magnetic field is applied, particularly at low and high temperatures, due to fluctuations in magnetic properties and Curie temperature limitations, leading to reduced performance and increased defect rates in mass production.

Method used

A MnZn-based ferrite composition with specific ranges of iron, zinc, manganese, and subcomponents like Si, Ca, Co, Nb, and V is optimized to achieve incremental magnetic permeability of 2800 or more when a DC magnetic field of 25 A/m is applied, with the temperature for maximum permeability between 10 to 50°C, ensuring high performance across the temperature range.

Benefits of technology

The optimized MnZn-based ferrite composition achieves high incremental magnetic permeability of 2800 or more across -40 to 85°C, reducing defect rates and improving yield in mass production, while maintaining high performance and stability, thus addressing the limitations of existing compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015487_31102024_PF_FP_ABST
    Figure JP2024015487_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an MnZn-based ferrite that is suitable for electronic components, e.g., pulse transformers, and that yields a higher incremental permeability in the temperature range of -40°C to 85°C when a DC magnetic field of 25 A / m is applied. A MnZn-based ferrite according to the present invention is composed of a base component, an auxiliary component, and unavoidable impurities. The base component is iron: 52.5-53.5 mol% as Fe2O3, zinc: 16.4-18.4 mol% as ZnO, and manganese: balance as MnO; the auxiliary component is, with reference to the base component, Si: 30-100 mass ppm as SiO2, Ca: 50-160 mass ppm as CaO, Co: 1500-3500 mass ppm as Co3O4, Nb: 100-600 mass ppm as Nb2O5, and V: 100-600 mass ppm as V2O5; and the total content of Nb and V is 200-900 mass ppm as Nb2O5 and V2O5.
Need to check novelty before this filing date? Find Prior Art

Description

MnZn ferrite

[0001] The present invention relates to an MnZn-based ferrite suitable for electronic components such as pulse transformers, which exhibits high incremental permeability even when a DC magnetic field of 25 A / m is applied in a temperature range of −40 to 85° C.

[0002] Ethernet® device transformers use pulse transformers with soft magnetic material in the magnetic core for purposes such as matching impedance at input / output terminals or maintaining electrical insulation. These pulse transformers are required to have high inductance, i.e., high incremental permeability, when a DC magnetic field is applied over a wide temperature range of -40 to 85°C. This incremental permeability is a value that indicates the permeability (ease of magnetization) of the magnetic core when a magnetic field is applied. Note that some literature uses the term effective permeability instead of incremental permeability, but since the two terms are synonymous, we will use the term incremental permeability hereafter.

[0003] Toroidal MnZn-based ferrite is generally used for the magnetic core made of the soft magnetic material. Among many soft magnetic materials, MnZn-based ferrite is particularly easy to obtain high magnetic permeability and high inductance. Furthermore, MnZn-based ferrite has the advantage of being inexpensive compared to metallic magnetic materials such as amorphous metals.

[0004] Here, MnZn-based ferrite is an oxide magnetic material, and therefore has the characteristic that its magnetic properties change significantly with temperature fluctuations. Therefore, compared to metal magnetic materials, it has the disadvantage that it is difficult to obtain stable magnetic properties over a wide temperature range.

[0005] Furthermore, pulse transformers may be installed outdoors when used in line termination devices, etc. Therefore, the MnZn-based ferrite used in pulse transformers needs to have high initial permeability over a wide temperature range from low to high, particularly over a temperature range of −40 to 85° C.

[0006] Furthermore, in digital communication equipment, pulse transformers may operate in a magnetized state due to fluctuations in the positive / negative balance of the transmitted pulse voltage, while being subjected to a DC magnetic field. Even under such a DC magnetic field, a high incremental permeability is required for signal conversion. In such applications, the magnitude of the DC magnetic field applied varies depending on the required inductance specification and usage, but a high incremental permeability is required at room temperature. Furthermore, general-purpose MnZn-based ferrite cores are often used under DC magnetic fields of up to 25 A / m.

[0007] Here, the MnZn ferrite used in such fields is Fe 2 O 3 MnZn-based ferrites are composed primarily of MnO, ZnO, and MnO, and exhibit high permeability when the main components have a magnetic anisotropy constant and a magnetostriction constant of zero. For this reason, such MnZn-based ferrites are used as small or thin magnetic cores for transformers, noise filters, and the like. That is, although it is difficult to obtain stable magnetic properties over a wide temperature range, a method has been proposed for achieving high incremental permeability under the application of a DC magnetic field in a temperature range of -40 to 85°C (or -40 to 100°C).

[0008] For example, Patent Document 1 proposes an MnZn-based ferrite having an incremental permeability of 2000 or more when a DC magnetic field of 33 A / m, which is higher than normal, is applied in a temperature range of -40 to 85° C. Additionally, Patent Document 2 proposes an MnZn-based ferrite having an incremental permeability of 2000 or more when a DC magnetic field of estimated approximately 25 A / m is applied in a temperature range of -40 to 100° C.

[0009] In addition, Patent Document 1 discloses a composition of MnZn ferrite (Fe) that provides high initial permeability. 2 O 3 : 52.0 to 53.0 mol%, ZnO: 22.0 to 23.0 mol%, MnO: balance), 2 and CaO are added at the same time, and Cr as an impurity inevitably mixed in due to the raw material of iron oxide is also added. 2 O 3A method has been proposed in which the content of is reduced to an extremely small amount, thereby controlling the average crystal grain size of MnZn-based ferrite within an appropriate range and obtaining MnZn-based ferrite with an initial permeability of 10,000 or more (23°C) and an incremental permeability of 2,000 or more (-40 to 85°C, when a DC magnetic field of 33 A / m is applied).

[0010] In Patent Document 2, the main component composition of MnZn ferrite (Fe 2 O 3 : 51.0 to 52.0 mol%, ZnO: 18.5 to 22.0 mol%, MnO: balance), and TiO as an accessory component 2 0.5 to 1.5 wt % and SiO 2 , CaO, V 2 O 5 , Nb 2 O 5 A method has been proposed for obtaining an MnZn-based ferrite containing trace amounts of any several of the above, with a relative permeability of 2100 or more in the range of -40 to 100°C and little deterioration in DC superposition characteristics under conditions of a residual magnetic flux density of 50 mT or less and a magnetic bias of 135 mT at room temperature (estimated to be the application of a DC magnetic field of 25 A / m).

[0011] In Patent Document 3, the basic composition of MnCoZn ferrite (Fe 2 O 3 : 51.0 to 53.0 mol%, ZnO: 13.0 to 18.0 mol%, CoO: 0.04 to 0.60 mol%, MnO: balance), with an appropriate amount of SiO 2 and CaO were added at the same time, and TiO 2 A method has been proposed for obtaining an MnCoZn-based ferrite that exhibits an incremental permeability of 2,300 or more when a DC magnetic field of 33 A / m is applied over the entire temperature range of -40 to 85°C by using the above-mentioned elements as the essential elements and reducing the content of P and B, which are unavoidable impurities due to the raw materials of iron oxide, to extremely small amounts. Note that Patent Document 3 contains Co, which has the effect of flattening the temperature characteristic of incremental permeability, and therefore achieves a relatively high Curie temperature of 140 to 210°C over a wide composition range. Therefore, a relatively high incremental permeability can be obtained even at low temperatures (-40°C) and high temperatures (85°C).

[0012] Furthermore, Patent Documents 4 and 5 disclose MnZn-based ferrites having compositions containing Ti and Bi.

[0013] Japanese Patent Publication No. 2013-166663 Japanese Patent Publication No. 2004-319811 Japanese Patent Publication No. 2008-143745 Japanese Patent Publication No. 2022-156991 Chinese Patent Application Publication No. 1686927

[0014] However, the MnZn-based ferrite obtained by the method described in Patent Document 1 does not contain a minor component, such as Co, that flattens the temperature characteristic of incremental permeability. Therefore, even under a mild DC magnetic field condition of 25 A / m, the incremental permeability at low temperatures (-40°C) and high temperatures (85°C) is lower than the value near room temperature. Furthermore, in the composition range described in Patent Document 1, the Curie temperature is low, at around 120 to 130°C, which inevitably results in a problem of low incremental permeability at high temperatures above 85°C.

[0015] Furthermore, the MnZn-based ferrite obtained by the method described in Patent Document 2 also does not contain a subcomponent such as Co that flattens the temperature characteristic of incremental permeability, so there is a problem that the incremental permeability at low temperatures (-40°C) and high temperatures (85°C) is lower than the value near room temperature. Furthermore, even in the composition range described in Patent Document 2, the Curie temperature is low, at 110 to 150°C or lower, so there is a problem that the incremental permeability is low in the high temperature range of 85°C or higher.

[0016] Furthermore, in the invention described in Patent Document 3, SiO 2 CaO, ZrO 2 , Ta 2 O 5 , HfO 2 , Nb 2 O 5 Since it contains a large amount of minor components such as the above, it is thought that even when a DC magnetic field of 25 A / m is applied, the incremental permeability in the range of -40 to 85°C is reduced overall.

[0017] The incremental permeability guaranteed for the MnZn ferrites shown in these documents in the temperature range of -40 to 85°C is often around 2300, which is a level that does not pose any problems in terms of characteristics for use in general pulse transformers, but when a large number of ferrite cores are manufactured, the problem is that the pass rate of the cores is low when considering the variation in characteristics. In order to meet demands such as increasing the pass rate of cores, reducing the number of copper wire windings, and further miniaturizing cores, a higher incremental permeability must be guaranteed, and this was insufficient to address such issues.

[0018] As in the inventions described in Patent Document 4 and Patent Document 5, when Ti is contained, the incremental magnetic permeability μ dc The temperature characteristic of the alloy is shifted to the low temperature side, and the incremental permeability at high temperatures decreases. Furthermore, when Bi is contained, the initial permeability increases when no DC magnetic field is applied, but the effective permeability μ decreases when a DC magnetic field is applied.

[0019] The present invention has been developed in view of the above circumstances, and has an object to provide an MnZn-based ferrite that is suitable for electronic components such as pulse transformers and that can obtain a higher incremental magnetic permeability when a DC magnetic field of 25 A / m is applied in a temperature range of −40 to 85° C.

[0020] The present invention proposes an MnZn-based ferrite having an incremental permeability of 2800 or more when a DC magnetic field of 25 A / m is applied in a temperature range of -40 to 85°C. This incremental permeability needs to be high over a wide temperature range, and it tends to decrease particularly near -40°C and 85°C. Therefore, in the present invention, the incremental permeability is set to 2800 or more near -40°C and 85°C. Furthermore, the temperature at which the incremental permeability reaches its maximum value is preferably in the range of 10 to 50°C. Furthermore, it is preferable that the MnZn-based ferrite has an incremental permeability of 3700 or more in a temperature range of approximately 0 to 60°C and 4100 or more in a temperature range of 23 to 40°C. In the present invention, the initial permeability and incremental permeability values ​​are all expressed as a ratio (relative permeability) to the vacuum permeability μo.

[0021] That is, the gist of the present invention is as follows: [1] An MnZn-based ferrite consisting of a basic component, a subcomponent, and unavoidable impurities, wherein the basic component is Fe, zinc, and manganese in a total amount of Fe 2 O 3 , ZnO, and MnO, calculated as 100 mol %, iron: Fe 2 O 3 52.5 to 53.5 mol% in terms of Si:SiO, 16.4 to 18.4 mol% in terms of zinc:ZnO, and the remainder in terms of manganese:MnO, and the minor components are 2 30 to 100 mass ppm in Ca:CaO equivalent, 50 to 160 mass ppm in Co:Co 3 O 4 Converted to 1500-3500 mass ppm, Nb:Nb 2 O 5 Converted to 100 to 600 mass ppm, and V:V 2 O 5 The total content of Nb and V is 100 to 600 mass ppm in terms of Nb. 2 O 5 and V 2 O 5 MnZn ferrite with a content of 200 to 900 mass ppm.

[0022] [2] The MnZn-based ferrite according to [1] above, wherein the incremental permeability is 2800 or more when a DC magnetic field of 25 A / m is applied in a temperature range of -40 to 85°C, and the temperature at which the incremental permeability shows a maximum value is in the range of 10 to 50°C.

[0023] [3] The MnZn-based ferrite according to [2] above, wherein the incremental permeability is 3700 or more when a DC magnetic field of 25 A / m is applied in a temperature range of 0 to 60°C, and further, the incremental permeability is 4100 or more when a DC magnetic field of 25 A / m is applied in a temperature range of 23 to 40°C.

[0024] According to the present invention, when a DC magnetic field of 25 A / m is applied, in the temperature range of -40 to 85°C, an MnZn ferrite having a high incremental permeability of 2800 or more near -40°C and near 85°C can be obtained.

[0025] The incremental permeability (μ dc ) to Fe 2 O 3 1 is a graph showing the effect of the content of the magnetic flux density (μ m ) at each measurement temperature. dc ) at each measurement temperature. dc ) to SiO 2 1 is a graph showing the effect of the content of the magnetic flux density (μ m ) at each measurement temperature. dc ) at each measurement temperature. dc ) to Co 3 O 4 1 is a graph showing the effect of the content of the magnetic flux density (μ m ) at each measurement temperature. dc ) to Nb 2 O 5 Content and V 2 O 5 1 is a graph showing the influence of the content of the magnetic flux density (μ m ) at each measurement temperature for Comparative Examples 13, 14, and 15. dc ) values.

[0026] An embodiment of the present invention will be described in detail below. Note that the embodiment described below is an example of a specific embodiment of the present invention, and the configuration of the present invention is not limited to this specific example.

[0027] (MnZn-based ferrite) MnZn-based ferrite consists of basic components, minor components, and inevitable impurities. The basic components are iron, zinc, and manganese, which exist as oxides. The mol% below indicates the composition ratio of the basic components.

[0028] [Incremental Permeability] First, each component will be described from the viewpoint of incremental permeability.

[0029] In the present invention, iron is Fe 2 O 3 The iron content is in the range of 52.5 to 53.5 mol % in terms of Fe 2 O 3 The iron content is preferably 52.6 mol % or more, more preferably 52.7 mol % or more, calculated as Fe2 O 3 In the present invention, the iron content is preferably 53.3 mol % or less, more preferably 53.1 mol % or less, calculated as Fe 2 O 3 The reason for the iron content being 52.5 to 53.5 mol% in terms of Fe is as follows. 2 O 3 This is because when the iron content is approximately 53.0 mol %, the magnetostriction constant λ becomes 0, and the incremental magnetic permeability when a DC magnetic field of 25 A / m is applied becomes the highest. 2 O 3 When the iron content is less than 52.5 mol % or exceeds 53.5 mol %, the incremental magnetic permeability is significantly reduced. 2 O 3 The more the equivalent value deviates from 53.0 mol %, the more the core expands and contracts due to deformation caused by the applied magnetic field, which places stress on the core itself, inhibiting domain wall movement and greatly reducing the incremental permeability.

[0030] It is known that the Curie temperature and secondary peak of MnZn-based ferrite change depending on the ratio of iron to zinc. In the present invention, the zinc content is 16.4 to 18.4 mol% in terms of ZnO. Furthermore, the zinc content is preferably 16.5 mol% or more, more preferably 16.6 mol% or more, in terms of ZnO. On the other hand, the zinc content is preferably 18.3 mol% or less, more preferably 18.2 mol% or less, in terms of ZnO. The reason for setting the zinc content in the range of 16.4 to 18.4 mol% in terms of ZnO is that the Curie temperature in this range is approximately 160 to 190°C, and good incremental permeability can be obtained even at high temperatures (85°C). In addition, if the zinc content is below 16.4 mol% in terms of ZnO, although the Curie temperature increases, the initial permeability itself decreases, and therefore the incremental permeability when a DC magnetic field is applied also decreases. On the other hand, if the zinc content exceeds 18.4 mol % in terms of ZnO, the Curie temperature decreases, and the incremental permeability at high temperatures (85° C.) decreases.

[0031] Manganese is the balance of the basic components. The manganese content is preferably in the range of 28.0 to 31.0 mol% in terms of MnO. The manganese content is more preferably 28.5 mol% or more and 30.7 mol% or less in terms of MnO.

[0032] That is, the basic components of MnZn ferrite are Fe, which is the sum of iron, zinc, and manganese. 2 O 3 , ZnO, and MnO, which is calculated as 100 mol %.

[0033] Next, the auxiliary components will be described. In addition to the above basic components, the MnZn ferrite of the present invention preferably contains Si, Ca, Co, Nb, and V as auxiliary components, and is composed of these. These are each SiO 2 , CaO, Co 3 O 4 , Nb 2 O 5 , and V 2 O 5 The contents of the minor components are expressed in mass ppm relative to the base component.

[0034] Both Si and Ca are elements that promote the formation of grain boundaries, suppress grain growth, and increase resistivity. By containing appropriate amounts of Si and Ca, it is possible to suppress the decrease in initial permeability over the entire wide temperature range of -40 to 85°C, and by increasing the incremental permeability in the low and high temperature ranges when a DC magnetic field is applied, it is possible to obtain a high incremental permeability over the wide temperature range of -40 to 85°C.

[0035] Si is SiO 2 It is essential that the content of Ca is in the range of 30 to 100 mass ppm, preferably 40 mass ppm or more, and preferably 95 mass ppm or less, calculated as CaO. It is also essential that the content of Ca is in the range of 50 to 160 mass ppm, preferably 90 mass ppm or more, and preferably 150 mass ppm or less, calculated as CaO. 2If the content of Si is less than 30 mass ppm in terms of SiO or if the content of Ca is less than 50 mass ppm in terms of CaO, the incremental permeability in both the low and high temperature ranges decreases, and an incremental permeability of 2800 or more cannot be obtained in the wide temperature range of -40 to 85°C. 2 When the Ca content is more than 100 mass ppm in terms of CaO or when the Ca content is more than 160 mass ppm in terms of CaO, the initial permeability decreases significantly, and the incremental permeability also decreases significantly accordingly, making it impossible to obtain an incremental permeability of 2800 or more in the wide temperature range of -40 to 85 ° C.

[0036] Co is an effective component for improving the temperature dependence of the magnetic properties of MnZn-based ferrite. By including an appropriate amount of Co, the change in incremental permeability with temperature when a DC magnetic field is applied is reduced, improving the incremental permeability in both the low and high temperature ranges. However, Co also has the effect of shifting the temperature dependence of permeability toward lower temperatures. Therefore, if the Co content is too low or too high, the balance of permeability between the low and high temperature ranges is disrupted, the incremental permeability in the low or high temperature range decreases, and it becomes impossible to obtain a high incremental permeability over a wide temperature range from -40 to 85°C.

[0037] Co is Co 3 O 4 It is important that Co is contained in the range of 1500 to 3500 mass ppm in terms of Co. 3 O 4 The content of Co is preferably 1800 mass ppm or more, more preferably 2000 mass ppm or more, calculated as Co. 3 O 4 The content of Co is preferably 3000 mass ppm or less, more preferably 2900 mass ppm or less, calculated as Co. 3 O 4 If the content is less than 1500 mass ppm in terms of Co, the maximum point of the temperature characteristic of the incremental permeability shifts to the high temperature side, and although the incremental permeability at high temperatures improves, the characteristics at low temperatures deteriorate, making it impossible to obtain an incremental permeability of 2800 or more over a wide temperature range from -40 to 85°C. 3 O 4If the converted content is more than 3500 mass ppm, the maximum point of the temperature characteristic of the incremental permeability shifts to the low temperature side, and although the low temperature characteristic of the incremental permeability improves, the high temperature characteristic deteriorates, making it impossible to obtain an incremental permeability of 2800 or more over a wide temperature range of -40 to 85°C.

[0038] Nb and V are elements that, when present together, suppress the generation of coarse crystal grains, obtain fine and uniform crystal grains, and have the effect of increasing the resistivity. By containing appropriate amounts of Nb and V, the incremental permeability when a DC magnetic field is applied can be increased.

[0039] Nb is Nb 2 O 5 It is essential that V is contained in the range of 100 to 600 mass ppm in terms of V, preferably 200 mass ppm or more, and more preferably 575 mass ppm or less. 2 O 5 It is essential that the content is in the range of 100 to 600 mass ppm, preferably 200 mass ppm or more, and more preferably 400 mass ppm or less.

[0040] Furthermore, the total content of Nb and V in the MnZn ferrite is Nb 2 O 5 and V 2 O 5 It is important that the total content of Nb and V is in the range of 200 to 900 mass ppm. 2 O 5 and V 2 O 5 In terms of carbon dioxide equivalent, the carbon dioxide content is preferably 250 mass ppm or more, and preferably 750 mass ppm or less.

[0041] Nb is Nb 2 O 5 When the converted value is less than 100 mass ppm, V is V 2 O 5When the content of Nb is less than 100 mass ppm in terms of Nb content, or when the total content of Nb and V is less than 200 mass ppm, the suppression of the generation of coarse crystal grains is insufficient and the resistivity is low, so that the incremental permeability when a DC magnetic field is applied also decreases. 2 O 5 When the converted amount is more than 600 mass ppm, V is V 2 O 5 When the Nb content is more than 600 mass ppm or when the total content of Nb and V is more than 900 mass ppm, the crystal grains become finer and the resistivity increases, making it difficult for the domain walls to move, and the initial permeability decreases. Accordingly, the incremental permeability when a DC magnetic field is applied also decreases.

[0042] [Failure Rate Due to Abnormal Grain Growth] Next, we will explain each component from the perspective of the failure rate due to abnormal grain growth. Generally, minor components such as Si or Ca added to MnZn-based ferrite significantly affect not only the properties but also the formation of crystal grains. When an appropriate amount of minor component is added, the minor component segregates at grain boundaries, suppressing grain coarsening, homogenizing the crystalline structure, and increasing resistivity. However, because minor components also have the effect of promoting sintering, excessive minor component content increases the likelihood of abnormal grain growth, leading to grain coarsening. The formation of coarse, abnormal grains reduces resistivity and, particularly, the incremental permeability at low and high temperatures. Ferrite cores containing abnormal grains larger than a certain size are therefore treated as defective products due to poor appearance and properties. Abnormal grains present on the surface of a sintered core can be visually identified because their color differs from that of a healthy ferrite sintered core.

[0043] On the other hand, when the Si and Ca contents of the MnZn-based ferrite are low, the generation of abnormal grains is suppressed, and the defective rate due to abnormal grain growth tends to be low. Also, although the influence is not as great as that of Si or Ca, abnormal grain growth is also likely to occur when the MnZn-based ferrite contains excessive amounts of Nb, V, Ti, Bi, etc. Therefore, in order to reduce the defective rate due to abnormal grain growth on the surface of the ferrite sintered core, it is important to reduce the contents of minor components that greatly contribute to the generation of abnormal grains.

[0044] In the present invention, the contents of the basic components and the subcomponents such as Si and Ca are appropriately selected so as to increase the initial permeability μi, so that the occurrence of abnormal grains is basically small and the defect rate due to abnormal grain growth of the ferrite core is also low. 2 When Si is contained in the range of 30 to 100 mass ppm in terms of SiO and Ca is contained in the range of 50 to 160 mass ppm in terms of CaO, the generation of abnormal grains is suppressed and the defective rate of the ferrite core is reduced. 2 If the Ca content exceeds 100 mass ppm in terms of CaO, or if the Ca content exceeds 160 mass ppm in terms of CaO, the generation of abnormal grains increases, and the defect rate due to abnormal grain growth in the ferrite core tends to increase.

[0045] Similarly, the content of Nb or V is Nb 2 O 5 Conversion value and V 2 O 5 If the total of the converted values ​​exceeds 900 mass ppm, the defect rate due to abnormal grain growth of the ferrite core increases. 2 O 5 Conversion value and V 2 O 5 The total converted value is preferably 900 mass ppm or less. 2 O 5 Conversion value and V 2 O 5 The total converted value is preferably 200 mass ppm or more.

[0046] [Process Capability Index Cpk] Next, each component will be described from the perspective of the process capability index Cpk. Since the MnZn-based ferrite according to one embodiment of the present invention has a low content of a subcomponent such as Si or Ca, the incremental permeability is lowest at either −40°C or 85°C in the temperature range of −40 to 85°C. This MnZn-based ferrite is characterized by a smaller variation in incremental permeability at that temperature than ferrites with a higher content of Si or Ca. Therefore, this MnZn-based ferrite also has a good margin for the lower limit specification of incremental permeability, taking variation into account. Therefore, from the perspective of the rate of defects below the lower limit specification of incremental permeability, it is preferable that the content of subcomponents such as Si or Ca is low. That is, MnZn-based ferrites with a low content of subcomponents such as Si or Ca can achieve a high process capability index Cpk. Generally, Cpk is preferably 1.33 or higher.

[0047] Therefore, from the viewpoint of obtaining a high process capability index Cpk, the total content of Si and Ca in the MnZn ferrite is SiO 2 On the other hand, the total content of Si and Ca in the MnZn ferrite is preferably 260 mass ppm or less in terms of SiO 2 and the CaO equivalent can be 80 mass ppm or more.

[0048] The MnZn-based ferrite of the present invention may contain unavoidable impurities such as P, B, S, Cl, etc. The total content of such unavoidable impurities is controlled to 500 mass ppm or less.

[0049] (Method for producing MnZn-based ferrite) Next, a method for producing MnZn-based ferrite according to the present invention will be described. A known general production method can be used for producing the MnZn-based ferrite according to the present invention. The general production method is as follows.

[0050] First, the basic component, Fe 2 O 3 , ZnO, and Mn 3 O 4 (The composition ratio is Mn 3 O4 The powder raw materials (treated as MnO rather than as MnO) are weighed out in amounts that satisfy the specifications of the present invention, and mixed in an attritor or ball mill to obtain a mixed powder. The mixing method may be either a dry method or a wet method.

[0051] The mixed powder is then heated to a temperature in the range of 800 to 1000°C and calcined to obtain a calcined powder. This calcined powder is then wet-pulverized using an attritor or ball mill until the pulverized particle size is approximately 0.8 to 1.6 μm. Sub-components are added in amounts that satisfy the amounts specified in the present invention before pulverization. This pulverization process requires homogenization to avoid uneven concentration of the sub-components.

[0052] An organic binder such as polyvinyl alcohol is added to the slurry obtained by the wet milling, and the mixture is granulated using a spray dryer or the like to obtain a granulated powder. The granulated powder is then filled into a mold of a predetermined shape and molded into a molded body. The molded body thus obtained is fired to obtain a MnZn-based ferrite core according to the present invention.

[0053] The MnZn-based ferrite obtained by the present invention has an incremental permeability of 2800 or more when a DC magnetic field of 25 A / m is applied in the temperature range of -40 to 85°C. Furthermore, it is preferable that the temperature at which the incremental permeability takes a maximum value is in the range of 10 to 50°C. Furthermore, it is preferable that the incremental permeability is 3700 or more when a DC magnetic field of 25 A / m is applied in the temperature range of 0 to 60°C, and that the incremental permeability is high, being 4100 or more when a DC magnetic field of 25 A / m is applied in the temperature range of 23 to 40°C. Furthermore, since the MnZn-based ferrite has a high incremental permeability of 2800 or more, when mass-produced, the number of products that have previously been rejected due to not achieving the required characteristics will decrease, resulting in an increased yield.

[0054] Furthermore, the incremental permeability of the MnZn ferrite core of the present invention when a DC magnetic field of 25 A / m is applied in the temperature range of -40 to 85°C is an upwardly convex curve showing a maximum value. Here, the temperature at which the incremental permeability shows a maximum value is different from the temperature at which the secondary peak of the initial permeability appears. 3 O 4By adding appropriate amounts of such minor components and by selecting an appropriate temperature at which the maximum value is exhibited, the incremental permeability at low temperatures (near -40°C) and high temperatures (near 85°C) can be balanced, and the high incremental permeability mentioned above can be stably obtained. In other words, in the present invention, it is essential to set the temperature at which the maximum value of incremental permeability is exhibited within an appropriate range (10 to 50°C) by including appropriate basic components and minor components. The temperature at which the maximum value of incremental permeability is exhibited is preferably 15°C or higher, and preferably 45°C or lower.

[0055] [Incremental Permeability] First, the influence of the basic components and the subcomponents on the incremental permeability was investigated. 2 O 3 , ZnO, and Mn 3 O 4 (The compounding ratio is treated as converted to MnO) Each raw material powder was weighed so as to have the composition ratio shown in Tables 1 to 3. High purity raw material powder was used in all cases.

[0056] Here, Comparative Example 13 had a composition corresponding to Example 11 of Patent Document 4, Comparative Example 14 had a composition corresponding to Example 1 of Patent Document 5, and Comparative Example 15 had a composition corresponding to Example 2 of Patent Document 5. That is, Fe 2 O 3 and ZnO were in the composition ratios described in the respective patent documents, and the remainder, MnO, was appropriately adjusted so that the total of the basic components was 100 mol %.

[0057] These raw material powders were mixed and pulverized in a ball mill for 16 hours, and then calcined in air at 925°C for 3 hours to obtain calcined powder. 2 , CaCO 3 , Co 3 O 4 , Nb 2 O 5 , V 2 O 5 , TiO 2 , and Bi 2 O 5The components were added to the powder in the composition ratios shown in Tables 1 to 3, and the powder was pulverized for 12 hours in a ball mill to obtain a pulverized powder. Polyvinyl alcohol was then added to the pulverized powder, granulated, and a pressure of 118 MPa was applied to form a toroidal core. This pulverized powder was then loaded into a sintering furnace and sintered at a maximum temperature of 1350°C to obtain a sintered sample with an outer diameter of 30.5 mm, an inner diameter of 19 mm, and a height of 6.5 mm. The content of P, B, S, Cl, and other unavoidable impurities was quantified according to JIS K0102 (ICP mass spectrometry) and confirmed to be 500 mass ppm or less. Each sample thus obtained was wound with 20 turns, and the initial permeability and incremental permeability were measured using a Precision LCR Meter E4980A (manufactured by Keysight Technologies). The initial permeability was measured at 23°C and 100 kHz without superimposing a DC magnetic field. The temperature characteristics of incremental permeability were measured at a frequency of 100 kHz under a superimposed DC magnetic field of 25 A / m at temperatures of -40°C, 0°C, 23°C, 40°C, 60°C, and 85°C. The results are shown in Tables 1 to 3 and Figures 1 to 7. The solid lines in the figures represent the incremental permeability (μ dc ) is 2800.

[0058]

[0059]

[0060]

[0061] <Basic Component> As shown in Table 1 and Figures 1 and 2, the results of Examples 1 to 8 and Comparative Examples 1 to 4 show that the basic component, Fe, 2 O 3 is in the range of 52.5 to 53.5 mol % and ZnO is in the range of 16.4 to 18.4 mol %, when a DC magnetic field of 25 A / m is applied, an increased magnetic permeability of 2800 or more is obtained in the temperature range of -40 to 85° C., and it can be seen that the temperature at which the maximum value of the incremental magnetic permeability is shown is in the range of 10 to 50° C. Furthermore, it can also be seen that in Examples 1 to 8, the incremental magnetic permeability when a DC magnetic field of 25 A / m is applied in the temperature range of 0 to 60° C. is 3700 or more, and the incremental magnetic permeability when a DC magnetic field of 25 A / m is applied in the temperature range of 23 to 40° C. is 4100 or more.

[0062] <Subcomponent SiO 2 As shown in Table 2 and FIG. 3, the results of Examples 9 to 11 and Comparative Examples 5 and 6 show that the secondary component SiO 2 If the range is 30 to 100 mass ppm, when a DC magnetic field of 25 A / m is applied, an increased permeability of 2800 or more is obtained in the temperature range of -40 to 85 ° C., and it can be seen that the temperature showing the maximum value of the incremental permeability is in the range of 10 to 50 ° C.

[0063] <Subsidiary Component CaO> As shown in Table 2 and FIG. 4 , from the results of Examples 12 to 15 and Comparative Examples 7 and 8, it can be seen that if the amount of CaO as a subcomponent is in the range of 50 to 160 mass ppm, an increased magnetic permeability of 2800 or more is obtained in the temperature range of −40 to 85° C. when a DC magnetic field of 25 A / m is applied, and the temperature at which the maximum value of the incremental magnetic permeability is shown is in the range of 10 to 50° C.

[0064] <Subcomponent Co 3 O 4 As shown in Table 2 and FIG. 5, the results of Examples 16 to 20 and Comparative Examples 9 to 10 show that the auxiliary component Co 3 O 4 is in the range of 1500 to 3500 mass ppm, when a DC magnetic field of 25 A / m is applied, an increased permeability of 2800 or more is obtained in the temperature range of -40 to 85 ° C. In particular, it can be seen that in Examples 17 to 20 of the present invention, the temperature at which the maximum value of the incremental permeability is shown is in the range of 10 to 50 ° C.

[0065] <Subcomponent Nb 2 O 5 and V 2 O 5 As shown in Table 2 and FIG. 6, the results of Examples 21 to 24 and Comparative Examples 11 to 12 show that the auxiliary component Nb 2 O 5 and V 2 O 5 are all in the range of 100 to 600 mass ppm, and Nb 2 O 5 and V 2 O 5If the total is in the range of 200 to 900 mass ppm, when a DC magnetic field of 25 A / m is applied, an increased permeability of 2800 or more is obtained in the temperature range of -40 to 85 ° C. It can be seen that the temperature showing the maximum value of the incremental permeability is in the range of 10 to 50 ° C.

[0066] <Case corresponding to Patent Document 4: Comparative Example 13> As shown in Table 3 and FIG. 7, in Comparative Example 13 (corresponding to Example 11 of Patent Document 4), the temperature characteristic curve is shifted to the low temperature side, the incremental permeability in the high temperature range is less than 2800, and it is not possible to obtain an incremental permeability of 2800 or more in the temperature range of −40 to 85° C.

[0067] <Cases corresponding to Patent Document 5: Comparative Examples 14 and 15> As shown in Table 3 and Fig. 7, in Comparative Example 14 (corresponding to Example 1 of Patent Document 5) and Comparative Example 15 (corresponding to Example 2 of Patent Document 5), the temperature characteristic curves are shifted to the high temperature side, the incremental permeability in the low temperature range is less than 2800, and an incremental permeability of 2800 or more cannot be obtained in the temperature range of -40 to 85°C. Furthermore, it can be seen that the rate of change in incremental permeability is large because Co is not added.

[0068] [Failure Rate Due to Abnormal Grain Growth] Next, the failure rate due to abnormal grain growth was investigated. For Examples 3, 11, and 15 and Comparative Examples 6, 8, and 13-18 shown in Table 4, ferrite pulverized powder was prepared in the same manner as described above. Polyvinyl alcohol was added to the pulverized powder and granulated. A pressure of 118 MPa was applied to form a toroidal core. The pulverized powder was then placed in a sagger and loaded into a firing furnace. The sintered core was fired at a maximum temperature of 1350°C, yielding a sintered core (core) with an outer diameter of 6.0 mm, an inner diameter of 3.0 mm, and a height of 4.0 mm. The initial permeability and incremental permeability of the resulting sintered core were determined using the method described above. Furthermore, 100 sintered samples were prepared, and the number of sintered samples with abnormal grains of 0.5 mm or larger on the surface was visually inspected to determine the failure rate. The results are shown in Table 4.

[0069] Here, Comparative Example 16 had a component equivalent to Example 7 of Patent Document 1, Comparative Example 17 had a component equivalent to Compliant Example 1 of Patent Document 2, and Comparative Example 18 had a component equivalent to Sample No. 1-5 (invention example) of Patent Document 3.

[0070]

[0071] As shown in Table 4, in Examples 3, 11, and 15, cores were produced using ferrite powder consisting of the basic components and subcomponents of the present invention, and an incremental permeability of 2800 or more was obtained in the temperature range of -40 to 85°C. Furthermore, no cores with abnormal grains were produced, indicating a low rate of defects due to abnormal grain growth.

[0072] As shown in Table 4, in Comparative Examples 6, 8, and 13 to 17, an incremental permeability of 2800 or more could not be obtained in the temperature range of -40 to 85°C, and the defective rate due to abnormal grain growth was higher than in the Examples of the present invention. In Comparative Example 18, an incremental permeability of 2800 or more could be obtained in the temperature range of -40 to 85°C, but there were cores that were defective due to abnormal grain growth, and the defective rate due to abnormal grain growth was higher than in the Examples of the present invention.

[0073] [Process Capability Index Cpk] Next, the process capability index Cpk of the present invention was investigated. 100 sintered body samples (cores) were produced by the above-mentioned method for Inventive Example 15 and Comparative Example 18, which have approximately the same incremental permeability at -40°C. The incremental permeability of each core was measured, and the standard deviation σ of the incremental permeability at -40°C, where the incremental permeability was lowest, was determined. Then, the lower limit specification of the incremental permeability at -40°C was set to 2700 (one-sided specification), and the process capability index Cpk, taking into account the bias, was calculated using the following formula (1). The results are shown in Table 5. Cpk = (average value - lower limit specification) / 3σ (1)

[0074]

[0075] As shown in Table 5, Example 15, which has a low content of Si or Ca, had a high Cpk of 1.35, while Comparative Example 18, which has a high Ca content, had a low Cpk of 0.82. From these results, it can be seen that Example 15 has a higher Cpk than Comparative Example 18, and has a margin below the standard lower limit of incremental permeability. From this, it can be seen that the present invention, which has a low content of Si or Ca, has a lower incremental permeability defect rate than the conditions of the invention examples of Patent Document 3, and is therefore more preferable.

[0076] The present invention makes it possible to obtain an MnZn-based ferrite that exhibits high incremental permeability even when a DC magnetic field of 25 A / m is applied in the temperature range of −40 to 85° C., making it suitable for electronic components such as pulse transformers. This makes it possible to reduce the size of ferrite cores and the number of copper wire windings.

Claims

1. MnZn-based ferrite consisting of basic components, auxiliary components, and unavoidable impurities, wherein the basic components are Fe, Zn, and Mn in total. 2 O 3 , ZnO, and MnO calculated as 100 mol % Iron: Fe 2 O 3 52.5 to 53.5 mol % in terms of ZnO, zinc: 16.4 to 18.4 mol % in terms of ZnO, and manganese: the balance in terms of MnO, and the auxiliary components are 2 Ca: 30 to 100 mass ppm in CaO equivalent, Co: 50 to 160 mass ppm in CaO equivalent 3 O 4 Converted to 1500 to 3500 mass ppm, Nb: Nb 2 O 5 Converted to 100 to 600 mass ppm, and V:V 2 O 5 The total content of Nb and V is 100 to 600 mass ppm in terms of Nb. 2 O 5 and V 2 O 5 MnZn ferrite, equivalent to 200 to 900 mass ppm.

2. The MnZn-based ferrite according to claim 1, wherein the incremental permeability is 2800 or more when a DC magnetic field of 25 A / m is applied in the temperature range of -40 to 85°C, and the temperature at which the incremental permeability shows a maximum value is in the range of 10 to 50°C.

3. The MnZn-based ferrite according to claim 2, wherein the incremental permeability is 3700 or more when a DC magnetic field of 25 A / m is applied in the temperature range of 0 to 60°C, and further, the incremental permeability is 4100 or more when a DC magnetic field of 25 A / m is applied in the temperature range of 23 to 40°C.

Citation Information

Patent Citations

  • Mn-Zn soft magnetic ferrite material having wide-temperature high-DC superposition characteristic

    CN103086705A

  • Mn-Zn-BASED FERRITE, MAGNETIC CORE FOR TRANSFORMER AND TRANSFORMER

    JP2004196632A

  • Ferrite composition, electronic component and power supply