Acrylic rubber, acrylic rubber composition for crosslinking, and crosslinked object obtained therefrom

By integrating an organic iodine compound and acrylic acid alkyl ester into the acrylic rubber, the process achieves mechanical strength comparable to secondary crosslinking through primary crosslinking alone, addressing the energy and time inefficiencies in existing methods and ensuring consistent product quality.

WO2024225185A1PCT designated stage expired Publication Date: 2024-10-31OSAKA SODA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015544
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing acrylic rubber crosslinking processes require significant differences in physical properties between primary and secondary crosslinked products, leading to energy-intensive and time-consuming processes, with a need for a method to minimize these differences for improved productivity and energy efficiency.

Method used

Incorporating a structural unit derived from an organic iodine compound with two or more iodine atoms and an acrylic acid alkyl ester into the acrylic rubber, allowing for primary crosslinking to achieve mechanical strength equivalent to secondary crosslinking, thus omitting the secondary crosslinking step and reducing energy consumption.

Benefits of technology

The approach results in a crosslinked acrylic rubber product with minimal differences in physical properties between primary and secondary crosslinked products, enabling faster manufacturing with lower energy consumption and improved product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide: an acrylic rubber which comes to have sufficient mechanical properties through primary crosslinking only without necessitating secondary crosslinking, from the standpoints of energy saving and production efficiency; an acrylic rubber composition for crosslinking; and a crosslinked object obtained therefrom. These inventors have found that a crosslinked acrylic rubber obtained using an acrylic rubber at least including a constituent unit derived from an organic iodine compound having two or more iodine atoms in the molecule and a constituent unit derived from an alkyl ester of acrylic acid, even when being a product of primary crosslinking, has mechanical strength comparable to that of the product of secondary crosslinking.
Need to check novelty before this filing date? Find Prior Art

Description

Acrylic rubber, acrylic rubber crosslinking composition and crosslinked product thereof

[0001] The present invention relates to acrylic rubber and rubber materials thereof, and more particularly to an acrylic rubber, a composition for crosslinking acrylic rubber, and a crosslinked acrylic rubber, which have a small difference in physical properties between the primary crosslinked product and the secondary crosslinked product and have a high crosslinking rate.

[0002] Acrylic rubber exhibits its properties as a rubber material by copolymerizing reactive groups such as halogen groups, epoxy groups, and carboxyl groups on the side chains as crosslinking points and reacting them with various crosslinking agents. However, to obtain sufficient rubber properties, the crosslinking process requires not only primary crosslinking but also secondary crosslinking at high temperatures for a long time, and from the perspective of energy consumption and productivity, a milder and simpler method is needed.

[0003] In response to this situation, Patent Document 1 discloses that an acrylic rubber compound containing a halogen group- and carboxyl group-containing acrylic rubber, trithiocyanuric acid, a metal dithiocarbamate, and / or thiuram sulfide can provide good rubber physical properties even without secondary crosslinking.

[0004] Furthermore, Patent Document 2 discloses that by crosslinking reactive halogen-containing acrylic rubber with an iodide or bromide of an alkali metal or alkaline earth metal, good rubber physical properties can be obtained even if the secondary crosslinking is omitted and the primary crosslinking is shortened.

[0005] However, in the documents 1 and 2, there is a large difference in the physical properties between the primary crosslinked product and the secondary crosslinked product, and it is desirable that the difference in these physical properties be small from the viewpoint of the quality of the final product.

[0006] Patent No. 2622739 Japanese Patent Application Laid-open No. 8-311289

[0007] In view of the above problems, an object of the present invention is to provide an acrylic rubber cross-linked product in which the difference in physical properties between the primary cross-linked product and the secondary cross-linked product is small.

[0008] As a result of extensive investigations conducted by the present inventors in order to achieve the above object, it was found that an acrylic rubber cross-linked product using an acrylic rubber containing at least a structural unit (A) derived from an organic iodine compound containing two or more iodine atoms per molecule and a structural unit (B) derived from an alkyl acrylate ester, even though it is a primary cross-linked product, has mechanical strength equivalent to that of a secondary cross-linked product, and this led to the completion of the present invention.

[0009] That is, the present invention provides the following features: Item 1. An acrylic rubber containing at least a structural unit (A) derived from an organic iodine compound containing two or more iodine atoms per molecule, and represented by the following general formula (1) or the following general formula (2), and a structural unit (B) derived from an alkyl acrylate, wherein the content of the structural unit (A) in 100% by mass of the acrylic rubber is 0.015 to 0.099% by mass. (R1 is a hydrocarbon group having 2 to 4 carbon atoms. R2 and R3 are each a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R2 and R3 may be the same or different. n is an integer of 2 to 4.) (R4 is a hydrocarbon group having 2 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R5 and R6 are a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aromatic hydrocarbon group which may have a substituent, or -COOR7, where R7 is an alkyl group having 1 to 3 carbon atoms. R5 and R6 may be the same or different. R7s may be the same or different. n is an integer of 2 to 4.) Item 2 The acrylic rubber according to Item 1, further comprising a structural unit (C) derived from an alkoxyalkyl acrylate ester. Item 3 The acrylic rubber according to Item 1 or 2, further comprising a structural unit (D) derived from an alkyl methacrylate ester. Item 4 The acrylic rubber according to any one of Items 1 to 3, wherein the acrylic rubber has a weight average molecular weight of 500,000 to 2,300,000. Item 5 A composition for crosslinking acrylic rubber, comprising at least the acrylic rubber according to any one of Items 1 to 4, and a crosslinking agent. Item 6 A crosslinked acrylic rubber obtained by crosslinking the composition for crosslinking acrylic rubber according to Item 5.

[0010] The cross-linked acrylic rubber obtained by cross-linking the acrylic rubber of the present invention has a small difference in mechanical strength between the primary cross-linked product and the secondary cross-linked product, so the secondary cross-linking step can be omitted, which enables shortening of the manufacturing process and industrial production with less energy.

[0011] <Acrylic Rubber> The acrylic rubber of the present invention contains at least a structural unit (A) derived from an organic iodine compound containing two or more iodine atoms per molecule, and a structural unit (B) derived from an alkyl acrylate.

[0012] Structural unit (A) derived from an organic iodine compound containing two or more iodine atoms per molecule Examples of structural units derived from an organic iodine compound containing two or more iodine atoms per molecule include structural units derived from organic iodine compounds represented by the following general formula (1) or (2). The structural unit (A) may be used alone or in combination of two or more. Among these, structural units derived from an organic iodine compound represented by the following general formula (1) are preferred.

[0013] In the following general formula (1), R1 is preferably a hydrocarbon group having 2 to 4 carbon atoms, more preferably a saturated hydrocarbon group having 2 to 4 carbon atoms, and even more preferably a saturated hydrocarbon group having 2 to 3 carbon atoms. Furthermore, R2 and R3 are preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a phenyl group, more preferably a hydrogen atom, a methyl group, an ethyl group, or a phenyl group, even more preferably a hydrogen atom, a methyl group, or a phenyl group, and particularly preferably a hydrogen atom or a methyl group. Furthermore, R2 and R3 are also preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. R2 and R3 may be the same or different. Preferably, n is an integer of 2 or 3. (R1 is a hydrocarbon group having 2 to 4 carbon atoms. R2 and R3 are each a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R2 and R3 may be the same or different. n is an integer of 2 to 4.)

[0014] Examples of the organic iodine compound represented by general formula (1) include ethylene glycol bisiodoacetic acid, ethylene glycol bis(2-iodopropionic acid), ethylene glycol bis(2-iodoisobutyric acid), ethylene glycol bis(2-iodo-2-phenylacetic acid), ethylene glycol bis(2-iodo-2-phenylpropionic acid), ethylene glycol bis(2-iodo-2-phenylisobutyric acid), glycerol 1,2-bisiodoacetic acid, glycerol 1,3-bisiodoacetic acid, glycerol 1,2-bis(2-iodopropionic acid), glycerol 1,3-bis(2-iodopropionic acid), glycerol 1,2-bis(2-iodoisobutyric acid), glycerol 1,3-bis(2-iodoisobutyric acid), glycerol 1,2- Bis(2-iodo-2-phenylacetic acid), glycerol 1,3-bis(2-iodo-2-phenylacetic acid), glycerol 1,2-bis(2-iodo-2-phenylpropionic acid), glycerol 1,3-bis(2-iodo-2-phenylpropionic acid), glycerol 1,2-bis(2-iodo-2-phenylisobutyric acid), glycerol 1,3-bis(2-iodo-2-phenylisobutyric acid), glycerol trisiodoacetate, glycerol tris(2-iodopropionic acid), glycerol tris(2-iodoisobutyric acid) TBTP, glycerol tris(2-iodo-2-phenylacetic acid), glycerol tris(2-iodo-2-phenylpropionic acid), glycerol tris(2-iodo-2-phenylisobutyric acid). Among these, ethylene glycol bis(2-iodoisobutyric acid), ethylene glycol bis(2-iodo-2-phenylacetic acid), glycerol tris(2-iodoisobutyric acid), and glycerol tris(2-iodo-2-phenylacetic acid) are preferred, and ethylene glycol bis(2-iodoisobutyric acid), ethylene glycol bis(2-iodo-2-phenylacetic acid), and glycerol tris(2-iodoisobutyric acid) are more preferred.

[0015] In the following general formula (2), R4 is preferably a hydrocarbon group or an aromatic hydrocarbon group having 2 to 4 carbon atoms, more preferably a saturated hydrocarbon group or an aromatic hydrocarbon group having 2 to 4 carbon atoms, and even more preferably a saturated hydrocarbon group or an aromatic hydrocarbon group having 2 to 3 carbon atoms. Furthermore, R5 and R6 are preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a phenyl group, and R7 is preferably a methyl group (-COOCH3), an ethyl group (-COOCH2CH3), or a propyl group (-COOCH2CH2CH3), more preferably a hydrogen atom, a methyl group, an ethyl group, or a phenyl group, and R7 is more preferably an ethyl group (-COOCH2CH3), and even more preferably a hydrogen atom, a methyl group, a phenyl group, or R7 is an ethyl group (-COOCH2CH3). R5 and R6 may be the same or different. Preferably, n is an integer of 2 to 3. (R4 is a hydrocarbon group having 2 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R5 and R6 are each a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aromatic hydrocarbon group which may have a substituent, or -COOR7, where R7 is an alkyl group having 1 to 3 carbon atoms. R5 and R6 may be the same or different. R7 may be the same or different. n is an integer of 2 to 4.)

[0016] Examples of the organic iodine compound represented by general formula (2) include 1,4-diiodobutane, 1,1-diiodoisobutane, 1,4-diphenyl-1,4-diiodobutane, diethyl 2,5-diiodoadipate, p-xylylene diiodide, o-xylylene diiodide, m-xylylene diiodide, 1,4-bis(1'-iodoethyl)benzene, 2,2,4-triiodobutane, 1,3,5-tris(1'-iodoethyl)benzene, etc. Among these, diethyl 2,5-diiodoadipate, p-xylylene diiodide, 1,4-bis(1'-iodoethyl)benzene, and 1,3,5-tris(1'-iodoethyl)benzene are preferred.

[0017] The content of the structural unit (A) in 100% by mass of the acrylic rubber of the present invention is preferably 0.015 to 0.099% by mass. More specifically, the lower limit is preferably 0.015% by mass or more, more preferably 0.025% by mass or more, and even more preferably 0.035% by mass or more. The upper limit is preferably 0.099% by mass or less, more preferably 0.09% by mass or less, and even more preferably 0.085% by mass or less. By being in this range, an acrylic rubber having a good balance between crosslinking rate and mechanical strength can be obtained.

[0018] Structural Unit (B) Derived from an Acrylic Acid Alkyl Ester The acrylic rubber of the present invention preferably contains a structural unit derived from an acrylic acid alkyl ester, more preferably a structural unit derived from an acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, even more preferably a structural unit derived from an acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms, and particularly preferably a structural unit derived from an acrylic acid alkyl ester having an alkyl group having 2 to 6 carbon atoms. The structural unit (B) may be used alone or in combination of two or more types.

[0019] Examples of structural units derived from alkyl acrylate esters having an alkyl group of 1 to 8 carbon atoms include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, etc., with structural units derived from ethyl acrylate and n-butyl acrylate being preferred. These may be used alone or in combination of two or more.

[0020] The content of the structural unit (B) in 100% by mass of the acrylic rubber of the present invention is preferably 50% by mass to 99.985% by mass. More specifically, the lower limit is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, most preferably 89% by mass or more, and even most preferably 90% by mass or more. The upper limit is preferably 99.985% by mass or less, more preferably 99.975% by mass or less, and even more preferably 99.965% by mass or less. By being in the above range, good physical properties tend to be obtained in terms of the cold resistance and oil resistance of the acrylic rubber.

[0021] Structural Unit (C) Derived from an Alkoxyalkyl Acrylate The acrylic rubber of the present invention may contain a structural unit derived from an alkoxyalkyl acrylate, and in that case, it preferably contains a structural unit derived from an alkoxyalkyl acrylate having an alkoxyalkyl group having 2 to 6 carbon atoms, more preferably contains a structural unit derived from an alkoxyalkyl acrylate having an alkoxyalkyl group having 2 to 5 carbon atoms, and even more preferably contains a structural unit derived from an alkoxyalkyl acrylate having an alkoxyalkyl group having 2 to 4 carbon atoms. The structural unit (C) may be used alone or in combination of two or more types.

[0022] Examples of structural units derived from alkoxyalkyl acrylate esters having an alkoxyalkyl group having 2 to 8 carbon atoms include structural units derived from acrylate esters such as methoxymethyl acrylate, ethoxymethyl acrylate, 2-methoxyethyl acrylate, 2-ethoxyethyl acrylate, 2-propoxyethyl acrylate, 2-butoxyethyl acrylate, 2-methoxypropyl acrylate, 2-ethoxypropyl acrylate, 3-methoxypropyl acrylate, 3-ethoxypropyl acrylate, 4-methoxybutyl acrylate, and 4-ethoxybutyl acrylate, and a structural unit derived from 2-methoxyethyl acrylate is preferred.

[0023] The content of the structural unit (C) in 100% by mass of the acrylic rubber of the present invention is preferably 0% by mass to 30% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and particularly preferably 4% by mass or more. The upper limit is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, particularly preferably 15% by mass or less, and most preferably 10% by mass or less. By being in the above range, good physical properties can be obtained in terms of the mechanical strength of the acrylic rubber, and there is also a tendency for it to be favorable in terms of cold resistance and oil resistance.

[0024] Structural Unit (D) Derived from Alkyl Methacrylate The acrylic rubber of the present invention may contain a structural unit derived from an alkyl methacrylate, and in that case, the structural unit is preferably a structural unit derived from an alkyl methacrylate having an alkyl group having 1 to 8 carbon atoms, more preferably a structural unit derived from an alkyl methacrylate having an alkyl group having 1 to 7 carbon atoms, even more preferably a structural unit derived from an alkyl methacrylate having an alkyl group having 1 to 6 carbon atoms, and particularly preferably a structural unit derived from an alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms. The structural unit (D) may be used alone or in combination of two or more types.

[0025] Examples of structural units derived from alkyl methacrylate esters having an alkyl group of 1 to 8 carbon atoms include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, and cyclohexyl methacrylate, and structural units derived from methyl methacrylate, ethyl methacrylate, and n-butyl methacrylate are preferred. These may be used alone or in combination of two or more.

[0026] The content of the structural unit (D) in 100% by mass of the acrylic rubber of the present invention is preferably 0% by mass to 30% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. The upper limit is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, and particularly preferably 15% by mass or less. When the content is within the above range, good physical properties tend to be obtained in terms of the mechanical strength of the acrylic rubber.

[0027] Furthermore, the acrylic rubber of the present invention may contain, in addition to the above-mentioned structural units, structural units derived from other monomers copolymerizable therewith. Examples of other structural units include structural units derived from ethylenically unsaturated nitriles, structural units derived from acrylamide monomers, structural units derived from aromatic vinyl monomers, structural units derived from conjugated diene monomers, structural units derived from non-conjugated dienes, and structural units derived from other olefins. These may be used alone or in combination of two or more.

[0028] Examples of constituent units derived from ethylenically unsaturated nitriles include constituent units derived from compounds such as acrylonitrile, methacrylonitrile, α-methoxyacrylonitrile, and vinylidene cyanide.

[0029] Examples of structural units derived from acrylamide monomers include structural units derived from compounds such as acrylamide, methacrylamide, diacetone acrylamide, diacetone methacrylamide, N-butoxymethyl acrylamide, N-butoxymethyl methacrylamide, N-butoxyethyl acrylamide, N-butoxyethyl methacrylamide, N-methoxymethyl acrylamide, N-methoxymethyl methacrylamide, N-propioxymethyl acrylamide, N-propioxymethyl methacrylamide, N-methyl acrylamide, N-methyl methacrylamide, N,N-dimethyl acrylamide, N,N-dimethyl methacrylamide, N,N-diethyl acrylamide, N,N-diethyl methacrylamide, N-methylolacrylamide, N-methylol methacrylamide, ethacrylamide, crotonamide, cinnamic acid amide, maleindiamide, itacondiamide, methylmaleamide, methylitaconamide, maleimide, and itaconimide.

[0030] Examples of structural units derived from aromatic vinyl monomers include structural units derived from compounds such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, o-ethylstyrene, p-ethylstyrene, α-fluorostyrene, p-trifluoromethylstyrene, p-methoxystyrene, p-aminostyrene, p-dimethylaminostyrene, p-acetoxystyrene, styrenesulfonic acid or a salt thereof, α-vinylnaphthalene, 1-vinylnaphthalene-4-sulfonic acid or a salt thereof, 2-vinylfluorene, 2-vinylpyridine, 4-vinylpyridine, divinylbenzene, diisopropenylbenzene, and vinylbenzyl chloride.

[0031] Examples of structural units derived from conjugated diene monomers include structural units derived from compounds such as 1,3-butadiene, 2-methyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,2-dichloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-neopentyl-1,3-butadiene, 2-bromo-1,3-butadiene, 2-cyano-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, chloroprene, and piperylene.

[0032] Furthermore, examples of constituent units derived from non-conjugated dienes include constituent units derived from non-conjugated diene compounds such as 1,4-pentadiene, 1,4-hexadiene, ethylidenenorbornene, norbornadiene, and dicyclopentadiene.

[0033] Examples of structural units derived from other olefin-based monomers include esters such as dicyclopentadienyl acrylate, dicyclopentadienyl methacrylate, dicyclopentadienyl ethyl acrylate, and dicyclopentadienyl ethyl methacrylate, and structural units derived from compounds such as ethylene, propylene, vinyl chloride, vinylidene chloride, 1,2-dichloroethylene, vinyl acetate, vinyl fluoride, vinylidene fluoride, 1,2-difluoroethylene, vinyl bromide, vinylidene bromide, 1,2-dibromoethylene, ethyl vinyl ether, and butyl vinyl ether.

[0034] In the acrylic rubber of the present invention, when structural units derived from these other copolymerizable monomers are contained, the content of these structural units in all structural units may be 0 to 15% by mass, 0 to 10% by mass, or 0 to 5% by mass.

[0035] In 100% by mass of the acrylic rubber of the present invention, the total content of the structural units (A) and (B) is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more, or may be 100% by mass.

[0036]

[0083] In 100% by mass of the acrylic rubber of the present invention, the total content of the structural units (A), (B), and (C) is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more, or may be 100% by mass.

[0037]

[0083] In 100% by mass of the acrylic rubber of the present invention, the total content of the structural units (A), (B), and (D) is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more, or may be 100% by mass.

[0038]

[0083] In 100% by mass of the acrylic rubber of the present invention, the total content of the structural units (A), (B), (C), and (D) is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more, or may be 100% by mass.

[0039] In the acrylic rubber of the present invention, the content of the structural units can be determined by the nuclear magnetic resonance spectrum of the obtained polymer.

[0040] The weight average molecular weight (Mw) of the acrylic rubber of the present invention obtained as described above is preferably 500,000 to 2,300,000 from the viewpoint of roll kneading properties and moldability. More specifically, the lower limit is preferably 500,000 or more, more preferably 750,000 or more, and even more preferably 1,000,000 or more. The upper limit is preferably 2,300,000 or less, more preferably 2,000,000 or less, and even more preferably 1,900,000 or less.

[0041] The molecular weight distribution (weight average molecular weight / number average molecular weight (Mn)) is preferably 2.0 to 4.5. More specifically, the lower limit is preferably 2.0 or more, more preferably 2.1 or more, and even more preferably 2.2 or more. The upper limit is preferably 4.5 or less, more preferably 4.2 or less, and even more preferably 4.0 or less. A molecular weight distribution within the above range makes it possible to achieve a balance between processability and rubber physical properties. In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the acrylic rubber are measured by the method described in the examples.

[0042] <Method for producing acrylic rubber> The acrylic rubber used in the present invention can be obtained by polymerizing various monomers. The monomers used may be commercially available products and are not particularly limited.

[0043] As the form of the polymerization reaction, any of emulsion polymerization, suspension polymerization, bulk polymerization, and solution polymerization can be used, but from the standpoint of ease of control of the polymerization reaction, it is preferable to use suspension polymerization or emulsion polymerization, which are generally used as conventional methods for producing acrylic rubber.

[0044] In the suspension polymerization method or emulsion polymerization method, the polymerization initiator, chain transfer agent, polymerization terminator, etc., which are commonly used, may be any of the conventionally known and commonly used agents.

[0045] The polymerization initiator is not particularly limited, and a polymerization initiator generally used in suspension polymerization or emulsion polymerization can be used. Specific examples thereof include inorganic polymerization initiators typified by persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate, 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane, 1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 4,4-di(t-butylperoxy)n-butyl valerate, 2,2-di(t-butylperoxy)butane, t-butyl hydroperoxide, and cumene hydroperoxide. Side, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide oxide, benzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, cumyl peroxyneodecanate, 1,1,3,3-tetramethylbutylperoxyneodecanate nate, t-hexylperoxyneodecanate, t-butylperoxyneodecanate, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanate, t-hexylperoxy-2-ethylhexanate, t-butylperoxy-2-ethylhexanate, t-butylperoxylaurate, t-butylperoxy-3,5,Organic peroxide-based polymerization initiators such as 5-trimethylhexanate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, hydroperoxides, azobisisobutyronitrile, 4-4'-azobis(4- Examples of azo initiators include 2-2'-azobis[2-(2-imidazolin-2-yl)propane, 2-2'-azobis(propane-2-carboxamidine), 2-2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide, 2-2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2-2'-azobis(1-imino-1-pyrrolidino-2-methylpropane), and 2-2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}. These polymerization initiators may be used alone or in combination of two or more.

[0046] The amount of polymerization initiator used is preferably in the range of 0.0001 to 0.1 parts by mass per 100 parts by mass of charged monomer. More specifically, the lower limit is preferably 0.0001 parts by mass or more, more preferably 0.0005 parts by mass or more, and even more preferably 0.001 parts by mass or more. The upper limit is preferably 0.1 parts by mass or less, more preferably 0.05 parts by mass or less, and even more preferably 0.01 parts by mass or less. If the amount is less than this range, the polymerization reaction may not be initiated or the polymerization rate may be significantly slowed. On the other hand, if the amount is too high, the polymerization rate may become too fast, or functional groups derived from the polymerization initiator may be introduced at the terminals of the acrylic rubber, making it impossible to obtain the desired acrylic rubber.

[0047] Alternatively, the amount is preferably 0.01 to 200 mol per mol of the organic iodine compound represented by general formula (1) or general formula (2). More specifically, the lower limit is preferably 0.01 mol or more, more preferably 0.02 mol or more, and even more preferably 0.03 mol or more. The upper limit is preferably 40 mol or less, more preferably 20 mol or less, and even more preferably 4 mol or less.

[0048] The chain transfer agent may be a chain transfer agent generally used in suspension polymerization or emulsion polymerization, for example, alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan, xanthogen compounds such as 2,4-diphenyl-4-methyl-1-pentene, 2,4-diphenyl-4-methyl-2-pentene, dimethyl xanthogen disulfide, and diisopropyl xanthogen disulfide, and thiuram compounds such as terpinolene, tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide. Examples of suitable chain transfer agents include phenolic compounds such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol, allyl compounds such as allyl alcohol, halogenated hydrocarbon compounds such as dichloromethane, dibromomethane and carbon tetrabromide, vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile and α-benzyloxyacrylamide, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, and 2-ethylhexyl thioglycolate, and these may be used alone or in combination of two or more. The amount of these chain transfer agents is not particularly limited, but is typically 0 to 0.1 parts by mass, and may be 0.01 to 0.05 parts by mass, per 100 parts by mass of the charged monomer.

[0049] The polymerization terminator may be any of those commonly used in suspension polymerization and emulsion polymerization. Examples include hydroxylamine, hydroxyamine sulfate, diethylhydroxyamine, hydroxyamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, and quinone compounds such as hydroquinone. The amount of the polymerization terminator used is not particularly limited, but is usually 0 to 2 parts by mass per 100 parts by mass of the charged monomer.

[0050] The emulsifier used in emulsion polymerization is not particularly limited, and commonly used nonionic emulsifiers and anionic emulsifiers can be used. Nonionic emulsifiers include, for example, polyoxyethylene alkyl ethers, polyoxyethylene alcohol ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene sorbitan fatty acid esters. Anionic emulsifiers include alkylbenzenesulfonates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, polyoxyalkylene alkyl ether phosphates or their salts, fatty acid salts, and the like, and these may be used alone or in combination of two or more. Typical examples of anionic emulsifiers include sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, and triethanolamine dodecyl sulfate.

[0051] The amount of emulsifier used in the present invention may be an amount generally used in emulsion polymerization. Specifically, it is preferably 0.01 to 10% by mass relative to the amount of charged monomer. More specifically, the lower limit is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and even more preferably 0.05% by mass or more. The upper limit is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less. When a reactive surfactant is used as a monomer component, the addition of an emulsifier is not necessarily required.

[0052] The dispersant used in the suspension polymerization method is not particularly limited, and a commonly used dispersant can be used. For example, the above-mentioned emulsifiers used in emulsion polymerization can also be used as the dispersant, and examples thereof include nonionic polymer compounds such as polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, and cellulose derivatives, anionic polymer compounds such as polyacrylic acid and its salts, polymethacrylic acid and its salts, and rubbers of methacrylic acid esters and methacrylic acid and / or its salts, and poorly water-soluble inorganic compounds such as calcium phosphate, calcium carbonate, and aluminum hydroxide.

[0053] These dispersants can be used alone or in combination of two or more. The amount of dispersant used in the present invention may be any amount generally used in suspension polymerization. Specifically, the amount is preferably in the range of 0.01 to 10% by mass relative to the amount of charged monomer. More specifically, the amount is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and even more preferably 0.05% by mass or more. The upper limit is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less.

[0054] Furthermore, the pH of the polymer obtained by the above method can be adjusted, if necessary, by using a base as a pH adjuster. Specific examples of bases include sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, inorganic ammonium compounds, and organic amine compounds. The pH range is preferably 1 to 11, more preferably 1.5 or higher, even more preferably 2 or higher, and more preferably 10.5 or lower, even more preferably 10 or lower.

[0055] In addition, if necessary, polymerization secondary materials such as particle size adjusters, chelating agents, and oxygen scavengers can be used.

[0056] Suspension polymerization and emulsion polymerization may be carried out in a batch, semi-batch, or continuous manner. The polymerization time and temperature are not particularly limited. They can be appropriately selected depending on the type of polymerization initiator used, etc., but generally, the polymerization temperature is 10 to 100°C, and the polymerization time is 0.5 to 100 hours.

[0057] There is no particular limitation on the method for recovering the polymer obtained by the above method, and a commonly used method can be adopted. One example of such a method is to continuously or batchwise supply the polymerization solution to an aqueous solution containing a coagulant, and a coagulated slurry is obtained by this operation. In this case, the temperature of the aqueous solution containing the coagulant is affected by coagulation conditions such as the type and amount of monomer used, and shear force due to stirring, etc., so it cannot be uniformly specified, but it is generally 50°C or higher, preferably in the range of 60°C to 100°C.

[0058] The coagulated slurry obtained by the above method is preferably washed with water to remove the coagulant. If washing with water is not performed at all or washing is insufficient, ion residues derived from the coagulant may be precipitated during the molding process.

[0059] The acrylic rubber can be obtained by removing water from the coagulated slurry after washing with water and drying it. The drying method is not particularly limited, but is generally carried out using a flash dryer or a fluidized bed dryer. Furthermore, a dehydration step using a centrifuge or the like may be carried out before the drying step.

[0060] <Composition for Cross-Linking Acrylic Rubber> The composition for cross-linking acrylic rubber of the present invention can be obtained by containing at least the above-mentioned acrylic rubber and cross-linking agent.

[0061] In the composition for acrylic rubber cross-linking of the present invention, the content of the acrylic rubber of the present invention in 100% by mass of the acrylic rubber is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, particularly preferably 98% by mass or more, and may be 100% by mass.

[0062] As the crosslinking agent, any of the conventionally known crosslinking agents commonly used for crosslinking rubber, such as organic peroxides, polyamine compounds, polyepoxy compounds, polyisocyanate compounds, aziridine compounds, sulfur compounds, basic metal oxides, and organometallic halides, can be used. Of these, organic peroxides are preferably used because the acrylic rubber of the present invention contains iodine.

[0063] The organic peroxide may be any organic peroxide that can easily generate peroxy radicals in the presence of heat or a redox system, and examples thereof include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3, benzoyl peroxide, t-butylperoxybenzene, t-butylperoxymaleic acid, t-butylperoxyisopropyl carbonate, and t-butylperoxybenzoate. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3 are preferred.

[0064] Examples of the polyvalent amine compound include aliphatic polyvalent amine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine; and aromatic polyvalent amine compounds such as 4,4'-methylenedianiline, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, 1,3,5-benzenetriamine, 1,3,5-benzenetriaminomethyl, and isophthalic acid dihydrazide.

[0065] Examples of the polyfunctional epoxy compound include glycidyl ether type epoxy compounds such as phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, cresol type epoxy compounds, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, brominated bisphenol A type epoxy compounds, brominated bisphenol F type epoxy compounds, and hydrogenated bisphenol A type epoxy compounds, as well as other polyfunctional epoxy compounds such as alicyclic epoxy compounds, glycidyl ester type epoxy compounds, glycidyl amine type epoxy compounds, and isocyanurate type epoxy compounds.

[0066] Examples of polyisocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, 1,5-naphthylene diisocyanate, 1,3,6-hexamethylene triisocyanate, 1,6,11-undecane triisocyanate, and bicycloheptane triisocyanate.

[0067] Examples of the aziridine compound include tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, tris[1-(2-methyl)aziridinyl]phosphinoxide, and hexa[1-(2-methyl)aziridinyl]triphosphatriazine.

[0068] Examples of sulfur compounds include sulfur, 4,4'-dithiomorpholine, tetramethylthiuram disulfide, and tetraethylthiuram disulfide.

[0069] Examples of basic metal oxides include zinc oxide, lead oxide, calcium oxide, and magnesium oxide.

[0070] The organic metal halide may be, for example, a dicyclopentadienyl metal dihalide, and the metal may be titanium, zirconium, or the like.

[0071] The amount of the crosslinking agent to be added is preferably 0.05 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the acrylic rubber of the present invention. The crosslinking agents can be used alone or in combination of two or more.

[0072] When the crosslinking agent is an organic peroxide, the acrylic rubber crosslinking composition preferably further contains a crosslinking aid. Examples of the crosslinking aid include triallyl cyanurate, triallyl isocyanurate (TAIC), triacryl formal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalate amide, triallyl phosphate, bismaleimide, and fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine). N,N-diallyl acrylamide, 1,6-divinyldodecafluorohexane, hexaallyl phosphoramide, N,N,N',N'-tetraallylphthalamide, N,N,N',N'-tetraallylmalonamide, trivinyl isocyanurate, 2,4,6-trivinylmethyltrisiloxane, tri(5-norbornene-2-methylene) cyanurate, triallyl phosphite, etc. Among these, triallyl isocyanurate (TAIC) is preferred because of its excellent crosslinkability, mechanical properties, and flexibility.

[0073] The amount of cross-linking aid blended is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 7.0 parts by mass, and even more preferably 0.1 to 5.0 parts by mass, per 100 parts by mass of acrylic rubber. If the amount of cross-linking aid is less than 0.01 part by mass, mechanical properties and flexibility tend to decrease. If the amount exceeds 10 parts by mass, heat resistance tends to be poor and the durability of the molded product also tends to decrease. The cross-linking aids can be used alone or in combination of two or more types.

[0074] The acrylic rubber cross-linking composition of the present invention can also be optionally blended with other additives commonly used in the art, such as lubricants, antioxidants, light stabilizers, fillers, reinforcing agents, plasticizers, processing aids, pigments, colorants, cross-linking accelerators, cross-linking retarders, antistatic agents, foaming agents, etc. These can be used alone or in combination of two or more.

[0075] An example of the reinforcing agent is carbon black, and the content thereof is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 30 parts by mass or more, relative to 100 parts by mass of the acrylic rubber, and is preferably 120 parts by mass or less, and more preferably 100 parts by mass or less.

[0076] Examples of lubricants include metal soaps such as zinc stearate, calcium stearate, and magnesium stearate, higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and oleic acid, higher fatty acid esters such as methyl esters, isopropyl esters, butyl esters, and octyl esters of higher fatty acids, higher alcohols such as myristyl alcohol, cetyl alcohol, and stearyl alcohol, and hydrocarbon lubricants such as liquid paraffin, paraffin wax, and synthetic polyethylene wax. Among these, higher fatty acids are preferred in the present invention, and stearic acid is more preferred.

[0077] The amount of lubricant blended is preferably 0.1 to 10 parts by mass per 100 parts by mass of acrylic rubber. More specifically, the lower limit is preferably 0.1 part by mass or more, more preferably 0.5 part by mass or more, and even more preferably 1 part by mass or more. The upper limit is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less.

[0078] Examples of antioxidants include amine-based, phosphate-based, quinoline-based, cresol-based, phenol-based, and dithiocarbamate metal salts. In the present invention, it is preferable to use amine-based and phenol-based antioxidants. These antioxidants may be used alone or in combination of two or more.

[0079] Examples of amine-based antiaging agents include phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonylamido)-diphenylamine, 4,4′-bis(α,α-dimethylbenzyl)diphenylamine, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N′-phenyl-p-phenylenediamine, and butyraldehyde-aniline condensates.

[0080] Examples of phenolic antioxidants include 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butylphenol, butylhydroxyanisole, 2,6-di-t-butyl-α-dimethylamino-p-cresol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, styrenated phenol, 2,2'-methylene-bis(6-α-methyl-benzyl-p-cresol), 4,4'-methylenebis( 2,6-di-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, 2,2'-thiobis-(4-methyl-6-t-butylphenol), 4,4'-thiobis-(6-t-butyl-o-cresol), 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, and the like.

[0081] The content of the antioxidant is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and particularly preferably 0.03 to 3 parts by mass, relative to 100 parts by mass of the acrylic rubber.

[0082] Furthermore, it is also possible to blend with rubbers, resins, etc., as is commonly done in the technical field, without departing from the spirit of the present invention. Examples of rubbers that can be used in the present invention include butadiene rubber, styrene-butadiene rubber, isoprene rubber, natural rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-isoprene rubber, acrylic rubber, ethylene acrylic rubber, ethylene-propylene-diene rubber, epichlorohydrin rubber, etc., and examples of resins that can be used in the present invention include PMMA (polymethyl methacrylate) resin, PS (polystyrene) resin, PUR (polyurethane) resin, PVC (polyvinyl chloride) resin, EVA (ethylene / vinyl acetate) resin, AS (styrene / acrylonitrile) resin, PE (polyethylene) resin, etc. These can be used alone or in combination of two or more.

[0083] The total amount of the rubber and resin is 50 parts by mass or less, preferably 10 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the acrylic rubber of the present invention.

[0084] The acrylic rubber crosslinking composition of the present invention can be compounded using any means conventionally used in the field of polymer processing, such as an open roll, a Banbury mixer, or various kneaders.

[0085] The compounding procedure can be a conventional procedure used in the field of polymer processing, for example, by first kneading only the polymer, then adding compounding ingredients other than the crosslinking agent and crosslinking aid to prepare kneaded compound A, and then kneading compound B to add the crosslinking agent and crosslinking aid.

[0086] A rubber material can be produced from the composition of the present invention (specifically, a crosslinked product can usually be obtained by heating to 100 to 250°C). The crosslinking time varies depending on the temperature, but is usually between 0.5 and 300 minutes. Crosslinking molding may be performed by integrally performing crosslinking and molding, by heating a previously molded acrylic rubber crosslinking composition again to obtain a crosslinked product, or by first heating the crosslinked product and then processing it for molding. Specific methods for crosslinking molding include compression molding using a mold, injection molding, heating using a steam can, an air bath, infrared radiation, or microwaves, among other methods.

[0087] The acrylic rubber of the present invention and the acrylic rubber cross-linking composition of the present invention containing the acrylic rubber of the present invention can provide an acrylic rubber cross-linked product with small differences in physical properties between the primary cross-linked product and the secondary cross-linked product. Therefore, since the acrylic rubber of the present invention and the acrylic rubber cross-linking composition of the present invention can produce an acrylic rubber cross-linked product with sufficient physical properties through the primary cross-linking process, it is preferable not to perform the secondary cross-linking process. In other words, the acrylic rubber cross-linked product of the present invention is preferably produced by performing only the primary cross-linking process on the acrylic rubber of the present invention and the acrylic rubber cross-linking composition of the present invention as a cross-linking process, without performing the secondary cross-linking process. In this specification, the primary cross-linking process refers to a process in which the acrylic rubber of the present invention and the acrylic rubber cross-linking composition of the present invention are allowed to stand, preferably at 140 to 200°C, more preferably at 150 to 180°C, for preferably 5 to 50 minutes, more preferably 10 to 40 minutes. The secondary cross-linking process refers to a process in which, after the primary cross-linking process, the acrylic rubber of the present invention and the acrylic rubber cross-linking composition of the present invention are allowed to stand, preferably at 140 to 200°C, more preferably at 150 to 180°C, for preferably 1 to 5 hours, more preferably 1 to 3 hours.

[0088] The crosslinked product prepared from the composition containing the acrylic rubber of the present invention thus obtained has excellent scorch resistance at high temperatures and a high crosslinking rate.

[0089] Therefore, the rubber material of the present invention can obtain hardness and rubber physical properties equivalent to those of secondary crosslinking through primary crosslinking alone, and therefore can be used to produce, with lower energy consumption than ever before, various gaskets such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing seals, mechanical seals, wellhead seals, seals for electric and electronic devices, seals for pneumatic equipment, cylinder head gaskets attached to the joint between a cylinder block and a cylinder head, rocker cover gaskets attached to the joint between a rocker cover and a cylinder head, oil pan gaskets attached to the joint between an oil pan and a cylinder block or a transmission case, gaskets for fuel cell separators attached between a pair of housings sandwiching a unit cell comprising a positive electrode, an electrolyte plate, and a negative electrode, and gaskets for the top cover of a hard disk drive, as well as various hoses such as extrusion-molded products and mold-crosslinked products used in automobiles, including fuel oil hoses around fuel tanks such as fuel hoses, filler neck hoses, vent hoses, vapor hoses, and oil hoses, air hoses such as turbo air hoses and emission control hoses, radiator hoses, heater hoses, brake hoses, and air conditioner hoses. Furthermore, the crosslinking rate is fast, and hardness and rubber physical properties equivalent to those of secondary crosslinking can be obtained with only primary crosslinking, so there is little lot-to-lot variation in the physical properties of the crosslinked product, and there is little variation in the quality of the final product.

[0090] The present invention will be specifically explained using examples and comparative examples. However, the present invention is not limited to these. In the event of any discrepancy between the description in the text and the description in the tables, the description in the tables takes precedence.

[0091] [Production Example 1] (Production of Acrylic Rubber A) A polymerization reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a pressure reducing device was charged with 200 parts by mass of water, 1.9 parts by mass of polyoxyalkylene alkyl ether phosphate ester, 50 parts by mass of ethyl acrylate and 50 parts by mass of n-butyl acrylate as monomers, and 0.05 parts by mass of ethylene glycol bis(2-iodoisobutyrate) (manufactured by Godo Shigen Co., Ltd., hereinafter abbreviated as BBDG) as an organic iodine compound. After sufficient removal of oxygen by repeated degassing under reduced pressure and nitrogen substitution, 0.004 parts by mass of benzoyl peroxide was added, the polymerization reactor was heated to 65°C, and a polymerization reaction was carried out until the polymerization conversion reached 80%. The resulting polymerization liquid was coagulated with an aqueous sodium sulfate solution, washed with water, and dried to obtain Acrylic Rubber A. The resulting acrylic rubber was subjected to the following tests, and the results are shown in Table 1.

[0092] <Molecular Weight Measurement> The weight average molecular weight (Mw) and number average molecular weight (Mn) of the acrylic rubber were measured by gel permeation chromatography (GPC), and the molecular weight distribution was calculated from Mw and Mn. Specifically, the measurement was carried out using a liquid chromatograph (manufactured by Waters Corporation) with two TSKgel Super HM-H columns (manufactured by Tosoh Corporation, column size 6.0 mm x 15 cm) connected in series. Tetrahydrofuran was used as the eluent, and the column temperature was set to 50°C. The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured as polystyrene equivalent values.

[0093] <Polymer Mooney viscosity (ML 1+4 , 100°C)> For acrylic rubber, the Mooney viscosity (ML) was measured at a measurement temperature of 100°C using a Mooney Viscometer AM-3 manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with the Mooney viscosity test of the physical testing method for uncrosslinked rubber in JIS K6300. 1+4 ) was measured.

[0094] <Mooney Scorch Time t5 (Scorch Stability)> The acrylic rubber composition was kneaded using a kneader and an open roll to prepare an uncrosslinked sheet having a thickness of 2 to 2.5 mm, and the Mooney scorch test specified in JIS K 6300 was carried out using a Mooney Viscometer AM-3 manufactured by Toyo Seiki Seisakusho, Ltd. at 145°C, measuring the time required for the Mooney viscosity to increase by 5 points from the minimum Mooney viscosity, and the scorch stability was evaluated.

[0095] [Production Example 2] (Production of Acrylic Rubber B) The same procedure as in Production Example 1 was carried out, except that the iodine compound charged was changed to 0.08 parts by mass of glycerol tris(2-iodoisobutyric acid) (manufactured by Godo Shigen Co., Ltd., hereinafter abbreviated as TBTP), to obtain Acrylic Rubber B. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0096] [Production Example 3] (Production of Acrylic Rubber C) The same procedure as in Production Example 1 was carried out, except that the iodine compound charged was changed to 0.05 parts by mass of TBTP, to obtain Acrylic Rubber C. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0097] [Production Example 4] (Production of Acrylic Rubber D) The same procedure as in Production Example 1 was carried out, except that the monomers charged and their amounts were changed to 40 parts by mass of ethyl acrylate and 60 parts by mass of n-butyl acrylate, to obtain Acrylic Rubber D. The obtained acrylic rubber was subjected to the above tests, and the results are shown in Table 1.

[0098] [Production Example 5] (Production of Acrylic Rubber E) The same procedure as in Production Example 1 was carried out, except that the monomers charged and their amounts were changed to 70 parts by mass of ethyl acrylate, 25 parts by mass of n-butyl acrylate, and 5 parts by mass of 2-methoxyethyl acrylate, to obtain Acrylic Rubber E. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0099] [Production Example 6] (Production of Acrylic Rubber F) The same procedure as in Production Example 1 was carried out, except that the monomers charged and their amounts were changed to 50 parts by mass of ethyl acrylate, 40 parts by mass of n-butyl acrylate, and 10 parts by mass of n-butyl methacrylate, to obtain Acrylic Rubber F. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0100] [Production Example 7] (Production of Acrylic Rubber G) The same procedure as in Production Example 1 was carried out, except that the amount of BBDG, an iodine compound, charged was changed to 0.01 parts by mass, to obtain Acrylic Rubber G. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0101] [Production Example 8] (Production of Acrylic Rubber H) The same procedure as in Production Example 1 was carried out except that the amount of BBDG, an iodine compound, charged was changed to 0.1 parts by mass, to obtain Acrylic Rubber H. The above tests were carried out using the obtained acrylic rubber, and the results are shown in Table 1.

[0102]

[0103] Example 1 To 100 parts by mass of the acrylic rubber obtained in Production Example 1, 60 parts by mass of carbon black N550, 2 parts by mass of stearic acid, and 4 parts by mass of triallyl isocyanurate were added and kneaded to obtain kneaded compound A. To this kneaded compound A, 1.5 parts by mass of Perhexa 25B (manufactured by NOF Corporation, chemical name 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) was added and kneaded with an open roll to obtain kneaded compound B, from which an uncrosslinked sheet 2 to 2.5 mm thick was prepared. The obtained uncrosslinked sheet was evaluated as follows, and the results are shown in Table 2.

[0104] <Normal State Physical Property Test> The uncrosslinked sheet obtained above was pressed at 180°C for 15 minutes to obtain a primary crosslinked sheet. This was further heated in an air oven at 180°C for 3 hours to obtain a secondary crosslinked sheet. Using each of the primary crosslinked and secondary crosslinked crosslinked sheets, a tensile test (strength TB, elongation EB) was performed in accordance with the method described in JIS K 6251 using an AGS-5KNY manufactured by Shimadzu Corporation. In addition, Type A durometer hardness HS (JIS A) was performed in accordance with the method described in JIS K6253. A comparative evaluation of the primary crosslinked product and the secondary crosslinked product was performed as follows. The smaller the rate and amount of change in physical properties between the primary crosslinked product and the secondary crosslinked product, the more sufficient normal state physical properties were obtained with the primary crosslinked product. ΔTB = (strength of primary crosslinked product - strength of secondary crosslinked product) / strength of secondary crosslinked product x 100 ΔEB = (elongation of primary crosslinked product - elongation of secondary crosslinked product) / elongation of secondary crosslinked product x 100 ΔHS = (hardness of primary crosslinked product - hardness of secondary crosslinked product)

[0105] [Examples 2 to 6, Comparative Examples 1 and 2] Examples 2 to 6 and Comparative Examples 1 and 2 were carried out as shown in Table 2 to obtain acrylic rubber cross-linking compositions, and were evaluated as described above. The respective results are shown in Table 2.

[0106]

[0107] As shown in Examples 1 to 6, the acrylic rubbers A to F of the present invention obtained in Production Examples 1 to 6 showed a small change in physical properties between the primary crosslinked product and the secondary crosslinked product of ±10% compared to Comparative Examples 1 and 2, suggesting that sufficient crosslinking had progressed with only the primary crosslinking. Therefore, it was found that the acrylic rubber crosslinked product obtained by crosslinking the acrylic rubber of the present invention has small differences in physical properties between the primary crosslinked product and the secondary crosslinked product, making it possible to omit the secondary crosslinking step, shortening the manufacturing process, and enabling industrial production with less energy.

[0108] The acrylic rubber, acrylic rubber cross-linking composition, and cross-linked product thereof of the present invention show only small changes in physical properties between the primary cross-linked product and the secondary cross-linked product, and therefore can be used to produce materials for various rubber products and resin products by primary cross-linking alone, making them extremely useful from the perspectives of low energy consumption and labor savings.

Claims

1. An acrylic rubber comprising at least a structural unit (A) derived from an organic iodine compound containing two or more iodine atoms in one molecule, represented by the following general formula (1) or the following general formula (2), and a structural unit (B) derived from an alkyl acrylate, wherein the content of structural unit (A) in 100% by mass of the acrylic rubber is 0.015 to 0.099% by mass. (R1 is a hydrocarbon group having 2 to 4 carbon atoms. R2 and R3 are a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R2 and R3 may be the same or different. n is an integer from 2 to 4. (R4 is a hydrocarbon group having 2 to 4 carbon atoms, or an aromatic hydrocarbon group which may have a substituent. R5 and R6 are a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aromatic hydrocarbon group which may have a substituent, or -COOR7, where R7 is an alkyl group having 1 to 3 carbon atoms. R5 and R6 may be the same or different. R7 may be the same or different. n is an integer from 2 to 4.

2. The acrylic rubber according to claim 1, further comprising a structural unit (C) derived from an alkoxyalkyl acrylate.

3. The acrylic rubber according to claim 1, further comprising a structural unit (D) derived from an alkyl methacrylate ester.

4. The acrylic rubber according to claim 1, wherein the weight average molecular weight of the acrylic rubber is 500,000 to 2,300,000.

5. A composition for crosslinking acrylic rubber, comprising at least the acrylic rubber according to any one of claims 1 to 4 and a crosslinking agent.

6. A cross-linked acrylic rubber product obtained by cross-linking the acrylic rubber cross-linking composition according to claim 5.

Citation Information

Patent Citations

  • Crosslinking composition

    JP2021123623A

  • Acrylic elastomer, acrylic elastomer composition, laminate, cross-linking substance, and molding member

    WO2014080948A1

  • Magnetic rubber composition, magnetic rubber molded article, and magnetic encoder

    WO2016052598A1

  • Acrylic rubber, acrylic rubber-containing composition, and crosslinked rubber

    WO2021201009A1