Method for producing composite material
The method of discharging a coating liquid with airgel particles, binder resin, and glass fibers onto a target object using a sprayer or dispenser with specific characteristics addresses the cracking issue in composite material formation, achieving high film strength and thermal insulation.
Patent Information
- Application Number
- PCT/JP2024/015640
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
The challenge lies in manufacturing composite materials containing airgel particles, binder resin, and glass fibers without cracking, as the addition of glass fibers to form a coating liquid often results in film formation issues such as cracking during drying.
A method involving the discharge of a coating liquid containing airgel particles, binder resin, glass fibers, and a liquid medium onto a target object using a sprayer or dispenser, with a discharge port diameter of 1.5 mm or more, and incorporating a water-soluble polymer with a hydrophobic group, and emulsified particles to improve dispersibility and reduce cracking.
This method enables the formation of a composite material with reduced cracking, high film strength, and improved thermal insulation properties, suitable for various applications including heat insulation, water repellency, and sound absorption.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Composite material manufacturing method
[0001] The present invention relates to a method for producing a composite material.
[0002] Aerogel is known as a material with excellent thermal insulation properties. Methods of processing aerogel into particles and using the particles as a constituent material of thermal insulation have been proposed (e.g., Patent Documents 1 and 2). Patent Document 1 proposes using particulate aerogel as a filler between resin plates that constitute thermal insulation windows. Patent Document 2 discloses a method of producing a thermal insulation material (molded body) by preparing an aqueous dispersion containing aerogel particles and organic fibers, evaporating the water, and then press-molding the resulting intermediate product.
[0003] JP 2012-091943 A JP 2014-035044 A
[0004] Composite materials containing aerogel particles and binder resins are expected to be applicable to a wider range of applications and uses if they are made into coating liquids.
[0005] The present inventors have investigated the incorporation of additional materials into a composite material and have found that the incorporation of glass fibers can achieve high film strength suitable for use as a thermal insulating material. However, according to the findings of the present inventors, when a composite material containing glass fibers is applied to form a coating liquid, cracks tend to occur during film formation, making it difficult to form a uniform composite material.
[0006] Therefore, an object of the present invention is to provide a method for producing a composite material that contains aerogel particles, a binder resin, and glass fibers and that is capable of easily producing a composite material with few cracks.
[0007] The present invention relates to, for example, the following items [1] to
[10] . [1] A method for producing a composite material, comprising: a coating film forming step of discharging a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium onto an object to form a coating film; and a removing step of removing at least a portion of the liquid medium from the coating film to form a composite material. [2] The production method according to [1], wherein the coating film forming step is a step of discharging the coating liquid onto the object using a discharge device selected from the group consisting of a sprayer and a dispenser. [3] The production method according to [2], wherein the discharge device has a discharge port for discharging the coating liquid, and the inner diameter of the discharge port is 1.5 mm or more. [4] The production method according to any one of [1] to [3], wherein the coating liquid further contains a water-soluble polymer having a hydrophobic group. [5] The production method according to [4], wherein the hydrophobic group is an alkyl group having 6 to 26 carbon atoms. [6] The production method according to any one of [1] to [5], wherein the coating liquid contains emulsified particles containing the binder resin. [7] The manufacturing method according to [6], wherein the emulsified particles further contain a nonionic emulsifier. [8] The manufacturing method according to any one of [1] to [7], wherein at least a portion of the aerogel particles form aggregates. [9] The manufacturing method according to any one of [1] to [8], further comprising: an emulsion preparation step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium; a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing the aerogel particles, the glass fibers, and the second liquid medium; and a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid.
[10] The manufacturing method according to [9], wherein the dispersion preparation step is a step of mixing the aerogel particles, the glass fibers, and the second liquid medium to aggregate at least a portion of the aerogel particles, and the coating liquid contains the aerogel particle aggregates.
[0008] According to the present invention, there is provided a method for producing a composite material, which contains aerogel particles, a binder resin, and glass fibers and is capable of easily producing a composite material with few cracks.
[0009] Preferred embodiments of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments. In this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this embodiment can be used alone or in combination of two or more.
[0010] The method for producing a composite material of this embodiment includes a step of ejecting a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium onto an object to obtain a coating film (coating film formation step), and a step of removing at least a portion of the liquid medium from the coating film to obtain a composite material (removal step).
[0011] According to the findings of the present inventors, when glass fibers are further blended into a composite material containing aerogel particles and a binder resin, a high film strength suitable for use as a thermal insulating material can be achieved. However, when a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium is applied to an object using a roller, trowel, or the like, there is a problem in that the coating film is prone to cracking when it dries.
[0012] In the manufacturing method of this embodiment, a coating film is formed by discharging a coating liquid onto an object. By forming a coating film in this manner, cracks are less likely to occur when the coating film dries, and a composite material with high film strength and few cracks can be easily formed.
[0013] The reason for this effect is thought to be as follows. For example, when a roller is used, components other than glass fibers in the coating liquid mainly penetrate into the roller and are applied, which is thought to reduce the glass fiber density in the coating film and promote the occurrence of cracks. Also, when a trowel is used, the glass fibers are oriented in the application direction, and this orientation is thought to promote the occurrence of cracks. In contrast, in the manufacturing method of this embodiment, the coating film is formed by discharging the coating liquid onto the target object, so the glass fiber density does not decrease and the glass fibers are less likely to be oriented, which is thought to make cracks less likely to occur.
[0014] In this embodiment, the coating liquid may further contain a water-soluble polymer having a hydrophobic group, which improves the dispersibility of the aerogel particles, making it possible to prepare a coating liquid with a higher aerogel particle loading and facilitating the production of a more uniform composite material.
[0015] In the present embodiment, the coating liquid may contain emulsified particles containing a binder resin. By dispersing the binder resin as emulsified particles, the dispersibility of the binder resin is improved, and a more uniform composite material can be easily formed.
[0016] In this embodiment, some or all of the aerogel particles in the coating liquid may form aggregates, which reduces the contact interface between the aerogel particles and the resin component (binder resin) during composite material formation, thereby suppressing penetration of the resin component into the pores of the aerogel particles, and tends to result in a composite material with higher thermal insulation properties.
[0017] The method for producing a composite material of the present embodiment may further include a step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium (emulsion preparation step), a step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, a water-soluble polymer, and the second liquid medium (dispersion preparation step), and a step of mixing the emulsion and the dispersion to obtain a coating liquid (coating liquid preparation step).
[0018] The dispersion preparation step may also be a step of mixing aerogel particles, glass fibers, and a second liquid medium to aggregate at least a portion of the aerogel particles.
[0019] Each step in the method for producing a composite material according to this embodiment will be described in detail below.
[0020] <Coating Film Forming Step> In the coating film forming step, a layer of the coating liquid (coating film) is formed on the object by discharging the coating liquid onto the object.
[0021] The object is not limited to an object to which the composite material is applied, and may be, for example, a resin member, a metal member, a building material, or the like.
[0022] The coating liquid may be discharged using a discharge device selected from the group consisting of a sprayer (e.g., an air sprayer) and a dispenser. The discharge device may have a discharge port for discharging the coating liquid. The inner diameter of the discharge port may be, for example, 1.5 mm or more, 2.0 mm or more, 2.5 mm or more, or 3.0 mm or more. The inner diameter of the discharge port may be, for example, 10.0 mm or less, 7.0 mm or less, 6.0 mm or less, or 5.0 mm or less.
[0023] <Removing Step> In the removing step, a composite material is formed by removing at least a part of the liquid medium from the coating film formed in the coating film forming step.
[0024] The method for removing the liquid medium from the coating film is not particularly limited, and examples thereof include a heating treatment (for example, 40 to 150° C.), a reduced pressure treatment (for example, 10,000 Pa or less), or both of these treatments.
[0025] The thickness of the composite material is not particularly limited and may be, for example, 0.05 mm or more, 0.1 mm or more, 0.5 mm or more, or 1 mm or more. The thickness of the composite material may be, for example, 30 mm or less, 20 mm or less, 10 mm or less, or 5 mm or less.
[0026] The composite material has pores due to the aerogel particles. The pore volume of the composite material is set to 0.15 cm3 in order to obtain higher thermal insulation. 3 / g or more is preferable, and 0.20 cm 3 / g or more is more preferable, and 0.60 cm 3 The upper limit of the pore volume of the composite material is not particularly limited. The pore volume of the composite material is, for example, 5.0 cm 3 / g or less.
[0027] The thermal conductivity of the composite material is, for example, 0.05 W / (m K) or less, preferably 0.04 W / (m K) or less, and more preferably 0.035 W / (m K) or less. There is no particular lower limit to the thermal conductivity of the composite material. The thermal conductivity of the composite material may be, for example, 0.01 W / (m K) or more.
[0028] The composite material has excellent heat insulating properties derived from the aerogel. Therefore, the composite material can be suitably used as a heat insulating material in cryogenic containers, the space field, the architectural field (piping, exterior walls, etc.), the automotive field (car air conditioning units, engines, etc.), the home appliance field (refrigerators, freezers, etc.), the semiconductor field, and industrial facilities (piping, tanks, etc.). In addition to being used as a heat insulating material, the composite material can also be used as a water repellent, sound absorbing material, vibration silencing material, catalyst carrier, etc.
[0029] <Production of Coating Liquid> In this embodiment, the coating liquid may be produced by mixing, for example, aerogel particles, a binder resin, glass fibers, and a liquid medium.
[0030] In this embodiment, the coating liquid may be produced by a production method including, for example, a preparation step of preparing aerogel particles, a binder resin, and a liquid medium, and a mixing step of mixing the aerogel particles, binder resin, and liquid medium prepared in the preparation step to aggregate the aerogel particles, thereby obtaining a coating liquid containing aggregates of aerogel particles, the binder resin, and the liquid medium.
[0031] In the preparation step, components other than the aerogel particles, binder resin, and liquid medium (for example, components described in <Other Components> below) may be further prepared.
[0032] In the mixing step, the components prepared in the preparation step are mixed so as to aggregate the aerogel particles. The mixing method may be any method that can form aggregates of the aerogel particles, and examples thereof include a method in which the components prepared in the preparation step are stirred and mixed.
[0033] The stirring speed affects the size of the aggregates. The higher the stirring speed, the greater the shear stress, which tends to reduce the size of the aggregates. Therefore, from the perspective of obtaining aggregates of a suitable size, as described below, it is desirable to mix at a low stirring speed.
[0034] The viscosity during mixing also affects the size of the aggregates. Even at the same stirring speed, the shear stress changes depending on the viscosity. If the viscosity is high, a larger shear stress is applied, and the aggregates become smaller in size. On the other hand, if the viscosity is low, the shear stress is small, and the aggregates tend to become larger. Therefore, the desired aggregate size can be achieved by adjusting the stirring speed depending on the viscosity.
[0035] The amount of liquid medium used during mixing also affects the size of the aggregates. Even if the final composition is the same, the size of the aggregates differs between (A) method, in which the entire amount of liquid medium is added from the beginning of mixing, and (B) method, in which a small amount of liquid medium is mixed at the beginning of mixing and then the liquid medium is added. Method (B) above has a higher initial viscosity than method (A). For this reason, method (B) above tends to produce smaller aggregates than method (A) above. By using these methods appropriately according to conditions such as the composition and mixing device (stirring device), aggregates of the desired size can be formed.
[0036] The average diameter of the aggregates may be, for example, 20 μm or more, or may be 30 μm or more. When the average diameter of the aggregates is large, the contact interface between the aerogel and the binder resin becomes smaller, further suppressing the penetration of the resin into the pores of the aerogel. The average diameter of the aggregates may be, for example, 300 μm or less, or may be 200 μm or less, or 150 μm or less. When the average diameter of the aggregates is small, a decrease in film strength due to the continuity of relatively fragile aerogel is suppressed, making it easier to obtain a stronger composite material.
[0037] The average diameter of the aggregates may be two or more times, or even three or more times, the average diameter of the aerogel particles. When the average diameter of the aggregates is large, the contact interface between the aerogel and the binder resin becomes smaller, further suppressing the penetration of the resin into the pores of the aerogel. Furthermore, the average diameter of the aggregates may be 30 or less times, 20 or less times, or 15 or less times the average diameter of the aerogel particles. When the average diameter of the aggregates is small, a decrease in film strength due to the continuity of relatively fragile aerogel is suppressed, making it easier to obtain a stronger composite material.
[0038] In this specification, the average diameter of aggregates refers to a value measured by the following method. [Method for measuring the average diameter of aggregates in a coating liquid] Approximately 20 g of coating liquid is placed in a 100 mL plastic cup, and water is added in 2 g increments while stirring with a spatula, gradually diluting the solution while mixing. The diluted sample is placed on a glass plate, and a micrograph of the sample is obtained using an optical microscope (manufactured by Olympus, model number: BX51). The obtained micrograph is analyzed using image editing software ImageJ, and the diameters of multiple aggregates in the micrograph are determined. The average of the obtained values is taken as the average diameter of the aggregates.
[0039] In this specification, the average diameter of the aerogel particles has the same meaning as the above-mentioned average particle diameter (D50) of the aerogel particles.
[0040] In this embodiment, when a diluted solution obtained by diluting the coating liquid is observed under an optical microscope, the area occupied by aggregates with a diameter of 20 μm or more (more preferably aggregates with a diameter of 50 μm or more) of the area occupied by aerogel particles (including aggregates) within the observation field is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and may be 100%.
[0041] In this specification, the diluted solution obtained by diluting the coating solution and the method for observing the diluted solution may be the same as the sample prepared in the above-mentioned [Method for measuring the average diameter of aggregates in a coating solution] and the method for observing the sample. Furthermore, the "area within the observation field" is determined by analyzing a micrograph using image editing software ImageJ.
[0042] In this embodiment, the coating liquid may be produced by a production method including, for example, an emulsion preparation step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium, a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, and the second liquid medium, and a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid.
[0043] The emulsion preparation step is a step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium.
[0044] The emulsion preparation step may be, for example, a step of obtaining an emulsion by emulsion polymerization of the monomer components described below in a first liquid medium in the presence of an emulsifier.
[0045] Examples of the first liquid medium include the same liquid mediums as those described below. The first liquid medium is preferably an aqueous solvent.
[0046] The emulsion polymerization may be carried out, for example, by a step (i) of mixing a monomer component and an emulsifier in a first liquid medium to obtain a monomer emulsion, and a step (ii) of mixing the monomer emulsion with a radical polymerization initiator to emulsion-polymerize the monomer component.
[0047] In step (i), the amount of the emulsifier may be, for example, 0.01 parts by mass or more, 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, 0.9 parts by mass or more, or 1 part by mass or more, relative to 100 parts by mass of the monomer component. Also, in step (i), the amount of the emulsifier may be, for example, 15 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, 8 parts by mass or less, or 6 parts by mass or less, relative to 100 parts by mass of the monomer component.
[0048] The radical polymerization initiator is not particularly limited as long as it is a polymerization initiator that can initiate emulsion polymerization of the monomer components, and may be appropriately selected from known radical polymerization initiators.
[0049] Examples of the radical polymerization initiator include hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide].
[0050] In step (ii), the amount of the radical polymerization initiator may be, for example, 0.001 parts by mass or more, 0.01 parts by mass or more, 0.05 parts by mass or more, or 0.1 parts by mass or more, relative to 100 parts by mass of the monomer components. Also, in step (ii), the amount of the radical polymerization initiator may be, for example, 5 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less, relative to 100 parts by mass of the monomer components.
[0051] In step (ii), a reducing agent may be used together with the radical polymerization initiator, if necessary. This promotes the generation of radicals from the radical polymerization initiator. Examples of the reducing agent include reducing organic compounds such as ascorbic acid, tartaric acid, citric acid, and glucose, and reducing inorganic compounds such as thiourea dioxide and hydrazine.
[0052] In step (ii), after the emulsion polymerization is completed, neutralization with a neutralizing agent may be performed. The neutralizing agent is not particularly limited and may be a known neutralizing agent. Examples of the neutralizing agent include aqueous ammonia, morpholine, 2-amino-2-methyl-1-propanol, triethylamine, triethanolamine, sodium hydroxide, and potassium hydroxide. The amount of the neutralizing agent is not particularly limited and may be appropriately adjusted so that the pH of the resulting emulsion is 7 to 11 (preferably 8 to 10).
[0053] The emulsion obtained in step (ii) contains emulsified particles containing a binder resin. The average particle size of the emulsified particles in the emulsion may be, for example, 50 nm or more, 70 nm or more, 90 nm or more, or 100 nm. The average particle size of the emulsified particles in the emulsion may be, for example, 400 nm or less, 350 nm or less, or 300 nm or less.
[0054] In this specification, the average particle size of emulsified particles in an emulsion refers to a value measured at 23°C by dynamic light scattering (DLS) using a MICROTRAC UPA150 (manufactured by Microtrac Bell Co., Ltd.).
[0055] The minimum film-forming temperature (MFT) of the emulsion obtained in step (ii) may be, for example, 25°C or lower, and from the viewpoint of further improving film-forming properties, it is preferably 20°C or lower, and more preferably 15°C or lower. Furthermore, from the viewpoint of further improving film-forming properties at low temperatures, the minimum film-forming temperature (MFT) of the emulsion is preferably 10°C or lower, more preferably 8°C or lower, and may be 6°C or lower. There are no particular restrictions on the lower limit of the minimum film-forming temperature (MFT) of the emulsion. Note that, in the case of a paint containing an aqueous solvent, an MFT of 0°C or lower cannot be measured.
[0056] The dispersion preparation step is a step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, and the second liquid medium.
[0057] The dispersion preparation step may be a step of mixing aerogel particles, glass fibers, and a second liquid medium so that the aerogel particles aggregate, to obtain a dispersion containing aerogel particle aggregates, glass fibers, and the second liquid medium.
[0058] Examples of the second liquid medium include the liquid medium described below, and the second liquid medium is preferably an aqueous solvent.
[0059] The dispersion may further contain a water-soluble polymer having a hydrophobic group. That is, the dispersion preparation step may be a step of mixing aerogel particles, glass fibers, a water-soluble polymer having a hydrophobic group, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, a water-soluble polymer having a hydrophobic group, and the second liquid medium.
[0060] In the dispersion preparation step, the amount of the water-soluble polymer may be, for example, 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, relative to 100 parts by mass of the aerogel particles. Also, in the dispersion preparation step, the amount of the water-soluble polymer may be, for example, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less, relative to 100 parts by mass of the aerogel particles.
[0061] In the dispersion preparation step, the mixing method is not particularly limited, and may be, for example, mixing by stirring.
[0062] The size of the aggregates in the dispersion is not particularly limited, and may be adjusted appropriately so that the size of the aggregates in the coating liquid falls within the preferred range described below.
[0063] The coating liquid preparation step is a step in which an emulsion and a dispersion are mixed to obtain a coating liquid.
[0064] In the coating liquid production step, the mixing method is not particularly limited and may be, for example, mixing by stirring. The mixing method in the coating liquid production step may be appropriately adjusted so that the size of the aerogel particle aggregates falls within the above-mentioned preferred range.
[0065] Each component used in the method for producing a composite material of this embodiment will be described in detail below.
[0066] <Binder Resin> Examples of binder resins include epoxy resins, silicone resins, phenolic resins, urea resins, melamine resins, polyurethane resins, polyethylene resins, polypropylene resins, polystyrene resins, polyester resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, polyamide resins, polyimide resins, and polyvinyl resins.
[0067] In a preferred embodiment, the binder resin may be, for example, a polymer of a monomer component having an ethylenically unsaturated bond. Such a binder resin has structural units (also referred to as monomer units) derived from the monomer component. Examples of the monomer component include acrylic compounds having a (meth)acryloyl group, aromatic vinyl compounds, heterocyclic vinyl compounds, vinyl esters, monoolefins, conjugated diolefins, α,β-unsaturated carboxylic acids, and vinyl cyanides. These may be used alone or in combination of two or more.
[0068] Examples of acrylic compounds include (meth)acrylic acid alkyl esters. The alkyl group of the (meth)acrylic acid alkyl ester may be linear, branched, or cyclic. The number of carbon atoms of the alkyl group of the (meth)acrylic acid alkyl ester may be, for example, 1 to 20, 1 to 18, 1 to 16, or 1 to 14. Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate.
[0069] Examples of the acrylic compound include polar-group-containing acrylic compounds having a (meth)acryloyl group and a polar group (a polar group other than a (meth)acryloyl group). Examples of the polar group include a hydroxy group, an amino group, a substituted amino group (e.g., a dialkylamino group, a hydroxyalkylamino group, etc.), an amide group, a substituted amide group (e.g., a dialkylamide group, a hydroxyalkylamide group, etc.), an epoxy group, a silyl group (e.g., a trialkoxysilyl group, etc.), a cyano group, an isocyanate group, a phosphate group, and a carbonyl group.
[0070] Examples of polar group-containing acrylic compounds include compounds in which a polar group is substituted on the alkyl group of a (meth)acrylic acid alkyl ester. Examples of such compounds include hydroxyalkyl(meth)acrylates (e.g., hydroxyethyl(meth)acrylate), dialkylaminoalkyl(meth)acrylates (e.g., dimethylaminoethyl(meth)acrylate), glycidyl(meth)acrylate, trialkoxysilylalkyl(meth)acrylate, isocyanatoalkyl(meth)acrylates (e.g., 2-isocyanatoethyl(meth)acrylate), and 2-(meth)acryloyloxyethyl acid phosphate.
[0071] The polar group-containing acrylic compound also includes a compound in which a (meth)acryloyl group is bonded to a polar group, such as (meth)acrylic acid, (meth)acrylamide, n-methylol(meth)acrylamide, and diacetone acrylamide.
[0072] Examples of polar group-containing acrylic compounds also include diacetone (meth)acrylate and acetoacetoxyalkyl (meth)acrylate (for example, acetoacetoxyethyl (meth)acrylate).
[0073] Examples of the acrylic compound include acrolein and vinyl alkyl ketones (for example, vinyl methyl ketone).
[0074] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, and ethylvinylbenzene.
[0075] Examples of heterocyclic vinyl compounds include vinylpyrrolidone, vinylfuran, vinylthiophene, vinyloxazoline, and vinylpyrrole.
[0076] Examples of vinyl esters include vinyl acetate, vinyl alkanoate, and vinyl versatate.
[0077] Examples of monoolefins include ethylene, propylene, butylene, and isobutylene.
[0078] Examples of conjugated diolefins include butadiene, isoprene, and chloroprene.
[0079] Examples of the α,β-unsaturated carboxylic acid include crotonic acid, itaconic acid, maleic acid, fumaric acid, and anhydrides thereof.
[0080] Examples of vinyl cyanides include acrylonitrile and methacrylonitrile.
[0081] As the monomer component, from the viewpoint of more significantly exhibiting the above-mentioned effects, a compound selected from the group consisting of an acrylic compound, an aromatic vinyl compound, a heterocyclic vinyl compound, and an α,β-unsaturated carboxylic acid is preferred.
[0082] The monomer component preferably contains an acrylic compound, from the viewpoint of achieving the above-mentioned effects more significantly. The content of the acrylic compound may be, for example, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or even 100% by mass, based on the total amount of the monomer component.
[0083] From the viewpoint of more significantly achieving the above-mentioned effects, the acrylic compound preferably contains a (meth)acrylic acid alkyl ester. The content of the (meth)acrylic acid alkyl ester may be, for example, 50% by mass or more based on the total amount of the monomer components. From the viewpoint of further improving the water resistance of the composite material, it may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. Furthermore, the content of the (meth)acrylic acid alkyl ester may be, for example, 99% by mass or less, 97% by mass or less, or 95% by mass or less based on the total amount of the monomer components.
[0084] The acrylic compound may further contain a polar group-containing acrylic compound. The content of the polar group-containing acrylic compound may be, for example, 1% by mass or more, 3% by mass or more, or 5% by mass or more, based on the total amount of the monomer components. Furthermore, the content of the polar group-containing acrylic compound may be, for example, 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, or 10% by mass or less, based on the total amount of the monomer components.
[0085] The monomer component may be selected, for example, from the group consisting of methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylic acid, and styrene.
[0086] The monomer component may be appropriately selected so that the glass transition temperature (Tg) of the binder resin falls within the preferred range described below. The glass transition temperature (Tg) of the binder resin can be measured by the method described in the examples described below.
[0087] The glass transition temperature (Tg) of the binder resin can be estimated by the FOX formula from the weight ratio of each monomer unit constituting the binder resin and the Tg of the homopolymer of each monomer. With reference to the values estimated by the FOX formula, the monomer components may be appropriately selected so that the glass transition temperature (Tg) of the binder resin falls within a suitable range.
[0088] The glass transition temperature (Tg) of the binder resin may be, for example, 25°C or lower, and from the viewpoint of further improving film-formability, it is preferably 20°C or lower, and more preferably 15°C or lower. Furthermore, from the viewpoint of further improving film-formability at low temperatures, the glass transition temperature (Tg) of the binder resin is preferably 10°C or lower, more preferably 8°C or lower, and may be 6°C or lower. There is no particular restriction on the lower limit of the glass transition temperature (Tg) of the binder resin, and it may be, for example, -40°C or higher, or -20°C or higher.
[0089] The binder resin can be produced, for example, by emulsion polymerization of monomer components in a liquid medium (preferably an aqueous solvent) in the presence of an emulsifier, which results in the formation of emulsion particles containing the binder resin and the emulsifier.
[0090] The emulsifier may be any known emulsifier that can emulsify the binder resin, such as an anionic emulsifier or a nonionic emulsifier.
[0091] From the viewpoint of easily obtaining a coating liquid with low corrosiveness to metals, the emulsifier is preferably a nonionic emulsifier. By selecting a nonionic emulsifier, it is thought that corrosion of metals caused by ions contained in other emulsifiers (e.g., anionic emulsifiers) can be suppressed.
[0092] The nonionic emulsifier may be any known nonionic emulsifier as long as it is capable of emulsifying the binder resin. Examples of the nonionic emulsifier include polyoxyalkylene alkyl ethers, polyoxyalkylene alkylphenol ethers, polyoxyalkylene fatty acid esters, and polyoxyalkylene sorbitan fatty acid esters. Polyoxyalkylene alkyl ethers are preferred, and polyoxyethylene alkyl ethers are more preferred.
[0093] The HLB value of the emulsifier is preferably 13 or more, more preferably 14 or more, from the viewpoint of making it easier to emulsify the binder resin, and is preferably 15 or more, more preferably 16 or more, from the viewpoint of further improving the film-forming properties of the coating liquid. Furthermore, the HLB value of the emulsifier is preferably 19 or less, from the viewpoint of preventing a decrease in the water resistance of the composite material.
[0094] The content of the emulsifier may be, for example, 0.01 parts by mass or more relative to 100 parts by mass of the binder resin, and from the viewpoint of delaying the surface drying of the coating film and improving film-forming properties and core drying properties, it may be 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, 0.9 parts by mass or more, or 1 part by mass or more. Furthermore, the content of the emulsifier may be, for example, 15 parts by mass or less relative to 100 parts by mass of the binder resin, and from the viewpoint of further improving the water resistance of the composite material, it may be 12 parts by mass or less, 10 parts by mass or less, 8 parts by mass or less, or 6 parts by mass or less.
[0095] The average particle size of the emulsified particles may be, for example, 50 nm or more, 70 nm or more, 90 nm or more, or 100 nm or more, and may be, for example, 400 nm or less, 350 nm or less, or 300 nm or less.
[0096] The content of the binder resin in the coating liquid may be, for example, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more, based on the total amount of nonvolatile content in the coating liquid. The content of the binder resin in the coating liquid may be, for example, 80% by mass or less, 75% by mass or less, or 70% by mass or less, based on the total amount of nonvolatile content in the coating liquid.
[0097] The content of the binder resin in the coating liquid may be adjusted as appropriate so that the content of the binder resin in the composite material falls within a suitable range described below.
[0098] The content of the binder resin in the composite material may be, for example, 1 vol% or more, 3 vol% or more, 5 vol% or more, or 10 vol% or more, based on the total volume of the composite material. The content of the binder resin in the composite material may be, for example, 40 vol% or less, 30 vol% or less, 25 vol% or less, or 20 vol% or less, based on the total volume of the composite material.
[0099] <Glass Fiber> Glass fiber functions as an anchor between aerogel particles, and can further improve the strength of the composite material.
[0100] The fiber diameter of the glass fiber may be, for example, 0.01 μm or more, and from the viewpoint of coating film strength, may be 0.1 μm or more, 1 μm or more, or 3 μm or more. The fiber diameter of the glass fiber may be, for example, 100 μm or less, and from the viewpoint of coating film smoothness, may be 50 μm or less or 30 μm or less.
[0101] The fiber length of the glass fiber may be, for example, 0.1 mm or more, and from the viewpoint of coating film strength, may be 1 mm or more, 1.5 mm or more, 2 mm or more, or 3 mm or more. The fiber diameter of the glass fiber may be, for example, 20 mm or less, and from the viewpoint of dispersibility and coating liquid dischargeability, may be 7 mm or less, or 5 mm or less.
[0102] The content of glass fibers in the coating liquid may be, for example, 0.5% by mass or more based on the total amount of nonvolatile content in the coating liquid, and from the viewpoint of coating film strength, may be 2% by mass or more, 3% by mass or more, or 5% by mass or more. The content of glass fibers in the coating liquid may be, for example, 15% by mass or less based on the total amount of nonvolatile content in the coating liquid, and from the viewpoint of dispersibility and coating liquid dischargeability, may be 12% by mass or less, or 10% by mass or less.
[0103] The content of glass fiber in the coating liquid may be adjusted as appropriate so that the contents of binder resin and emulsifier in the composite material fall within the preferred ranges described below.
[0104] The content of the glass fiber in the composite material may be, for example, 0.1 vol% or more, 0.2 vol% or more, 0.3 vol% or more, or 0.4 vol% or more, based on the total volume of the composite material. The content of the glass fiber in the composite material may be, for example, 5 vol% or less, 3 vol% or less, or 2 vol% or less, based on the total volume of the composite material.
[0105] <Water-Soluble Polymer> The water-soluble polymer may be any polymer as long as it has a hydrophobic group and is water-soluble.
[0106] Examples of the hydrophobic group include an alkyl group (preferably a long-chain alkyl group having 6 to 26 carbon atoms), an ester group, an alkoxy group, a halogen atom, etc. Of these, the hydrophobic group is preferably an alkyl group, more preferably a long-chain alkyl group having 6 to 26 carbon atoms, even more preferably a long-chain alkyl group having 8 to 26 carbon atoms, still more preferably a long-chain alkyl group having 10 to 26 carbon atoms, or may be a long-chain alkyl group having 12 to 26 carbon atoms or a long-chain alkyl group having 15 to 26 carbon atoms.
[0107] Examples of water-soluble polymers include modified carboxyl vinyl polymers, modified polyether urethane, cellulose-based resins, polyethylene oxide, polyvinyl alcohol, polyacrylates, polyvinylpyrrolidone, dextrin-based resins, chitin-based resins, and chitosan-based resins.
[0108] As the water-soluble polymer, a cellulose-based resin can be suitably used, such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, and modified products thereof that have been further modified (e.g., hydrophobized).
[0109] The cellulose-based resin is preferably a cellulose-based resin having an alkyl group, and more preferably a cellulose-based resin having a long-chain alkyl group having 6 to 26 carbon atoms. The effects of the present invention are more pronounced when using such a cellulose-based resin. The number of carbon atoms in the long-chain alkyl group is preferably 6 to 26, more preferably 8 to 26, even more preferably 10 to 26, still more preferably 12 to 26, and even more preferably 15 to 26.
[0110] In the cellulose-based resin, the content of long-chain alkyl groups having 6 to 26 carbon atoms is preferably 0.01 to 5 mass %, more preferably 0.01 to 3 mass %, based on the total amount of the cellulose-based resin.
[0111] As the cellulose-based resin, for example, a cellulose-based resin having a structural unit represented by the following formula (A-1) is preferred.
[0112] In formula (A-1), R A represents a hydrogen atom, an alkyl group, a hydroxyalkyl group, -R A1 -O-R A2 A group represented by R A1 represents an alkanediyl group or a hydroxyalkanediyl group, and R A2 represents an alkyl group, or -(R A3 O) n A group represented by H (R A3 represents an alkanediyl group, and n represents an integer of 2 or more. A may be the same or different from each other, provided that three R A At least one of the groups is an alkyl group or -R A1 -O-R A2 It is a group represented by the following formula:
[0113] In formula (A-1), R A The alkyl group in R is preferably an alkyl group having 1 to 26 carbon atoms. AThe alkyl group in the formula (I) is more preferably a short-chain alkyl group having 1 to 3 carbon atoms or a long-chain alkyl group having 6 to 26 carbon atoms. The long-chain alkyl group preferably has 8 to 26 carbon atoms, more preferably 10 to 26 carbon atoms, even more preferably 12 to 26 carbon atoms, and even more preferably 15 to 26 carbon atoms.
[0114] In formula (A-1), R A The hydroxyalkyl group in is preferably a hydroxyalkyl group having 1 to 26 carbon atoms, more preferably a hydroxyalkyl group having 1 to 10 carbon atoms, and even more preferably a hydroxyalkyl group having 1 to 5 carbon atoms.
[0115] In formula (A-1), R A1 The alkanediyl group in R is preferably an alkanediyl group having 1 to 26 carbon atoms, more preferably an alkanediyl group having 1 to 10 carbon atoms, and even more preferably an alkanediyl group having 1 to 5 carbon atoms. A1 The hydroxyalkanediyl group in the formula (I) is preferably a hydroxyalkanediyl group having 1 to 26 carbon atoms, more preferably a hydroxyalkanediyl group having 1 to 10 carbon atoms, and even more preferably a hydroxyalkanediyl group having 1 to 5 carbon atoms.
[0116] In formula (A-1), R A2 is preferably an alkyl group having 1 to 26 carbon atoms. A2 The alkyl group in the formula (I) is more preferably a short-chain alkyl group having 1 to 3 carbon atoms or a long-chain alkyl group having 6 to 26 carbon atoms, and more preferably a long-chain alkyl group. The number of carbon atoms in the long-chain alkyl group is preferably 8 to 26, more preferably 10 to 26, even more preferably 12 to 26, and even more preferably 15 to 26.
[0117] In formula (A-1), R A3 As the alkyl group, an alkanediyl group having 2 to 3 carbon atoms is preferred, and an alkanediyl group having 3 carbon atoms is more preferred.
[0118] In formula (A-1), three R A At least one of the R A At least one of them is -R A1 -O-RA2 and R A2 is preferably a long chain alkyl group.
[0119] The content of the water-soluble polymer in the coating liquid may be, for example, 0.03 mass% or more based on the total amount of nonvolatile content in the coating liquid, and from the viewpoint of further improving the dispersibility of the aerogel particles, it may be 0.05 mass% or more, 0.07 mass% or more, 0.09 mass% or more, 0.2 mass% or more, 0.4 mass% or more, 0.6 mass% or more, or 0.8 mass% or more. Furthermore, the content of the water-soluble polymer in the coating liquid may be, for example, 6 mass% or less based on the total amount of nonvolatile content in the coating liquid, and from the viewpoint of further improving the water resistance of the composite material, it may be 5 mass% or less, 4 mass% or less, or 3 mass% or less.
[0120] The content of the water-soluble polymer in the coating liquid may be, for example, 0.1 parts by mass or more relative to 100 parts by mass of the aerogel particles, and from the viewpoint of further improving the dispersibility of the aerogel particles, it may be 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more. Furthermore, from the viewpoint of further improving the water resistance of the composite material, the content of the water-soluble polymer in the coating liquid may be, for example, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less relative to 100 parts by mass of the aerogel particles.
[0121] The content of the water-soluble polymer in the coating liquid may be adjusted as appropriate so that the content of the water-soluble polymer in the composite material falls within a suitable range described below.
[0122] The content of the water-soluble polymer in the composite material may be, for example, 0.01 vol% or more, 0.05 vol% or more, 0.1 vol% or more, or 0.15 vol% or more, based on the total volume of the composite material. The content of the water-soluble polymer in the composite material may be, for example, 1.5 vol% or less, or 1 vol% or less, based on the total volume of the composite material.
[0123] <Aerogel> In this embodiment, the term "aerogel" refers to a broad aerogel, namely, "a gel composed of a microporous solid in which the dispersed phase is a gas (a gel composed of a microporous solid in which the dispersed phase is a gas)."
[0124] The aerogel of this embodiment is, for example, a silica aerogel containing silica as a main component. Examples of the silica aerogel include so-called organic-inorganic hybrid silica aerogels into which an organic group (e.g., a methyl group) or an organic chain has been introduced.
[0125] The aerogel of this embodiment may have the following aspects, for example. By employing each aspect, it is possible to obtain an aerogel having the heat insulating properties, flame retardancy, heat resistance, and flexibility appropriate for each aspect.
[0126] (First Aspect) The aerogel according to the present embodiment can have a structure represented by the following general formula (1): The aerogel according to the present embodiment can have a structure represented by the following general formula (1a) as a structure including the structure represented by formula (1).
[0127] In formula (1) and formula (1a), R 1 and R 2 each independently represents an alkyl group or an aryl group, R 3 and R 4 each independently represents an alkylene group. Here, examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. p represents an integer of 1 to 50. In formula (1a), when two or more R 1 may be the same or different, and similarly, two or more R 2 In formula (1a), two R 3 may be the same or different, and similarly, two R 4 may be the same or different.
[0128] By introducing the structure represented by the above formula (1) or formula (1a) into the skeleton of an aerogel as an aerogel component, an aerogel having low thermal conductivity and flexibility can be obtained. 1 and R 2 are each independently an alkyl group having 1 to 6 carbon atoms, a phenyl group, etc., and examples of the alkyl group include a methyl group, etc. In addition, in formula (1) and formula (1a), R 3 and R 4 are each independently an alkylene group having 1 to 6 carbon atoms, and examples of the alkylene group include an ethylene group, a propylene group, etc. In formula (1a), p can be 2 to 30, and may be 5 to 20.
[0129] (Second Aspect) The aerogel of this embodiment has a ladder-type structure including struts and bridges, and the bridges can have a structure represented by the following general formula (2). By introducing such a ladder-type structure into the skeleton of the aerogel as an aerogel component, it is possible to improve heat resistance and mechanical strength. Note that in this embodiment, the "ladder-type structure" refers to one having two struts and bridges connecting the struts (a structure having a so-called "ladder" shape). In this aspect, the skeleton of the aerogel may have a ladder-type structure, or the aerogel may partially have a ladder-type structure.
[0130] In formula (2), R 5 and R 6 are each independently an alkyl group or an aryl group, and b is an integer of 1 to 50. Here, examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. In addition, in formula (2), when b is an integer of 2 or more, two or more R 5 may be the same or different, and similarly, two or more R 6 may be the same or different.
[0131] By introducing the above structure into the skeleton of an aerogel as an aerogel component, an aerogel having greater flexibility than, for example, aerogels having a structure derived from conventional ladder-type silsesquioxanes can be obtained.
[0132] The structure that forms the support portion and its chain length, as well as the spacing between the structures that form the bridging portion, are not particularly limited. From the viewpoint of further improving heat resistance and mechanical strength, the ladder structure may have a ladder structure represented by the following general formula (3):
[0133] In formula (3), R 5 , R 6 , R 7 and R 8 each independently represents an alkyl group or an aryl group, a and c each independently represent an integer of 1 to 3000, and b represents an integer of 1 to 50. Here, examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. In addition, in formula (3), when b is an integer of 2 or more, two or more R 5 may be the same or different, and similarly, two or more R 6 In addition, in formula (3), when a is an integer of 2 or more, two or more R 7 may be the same or different, and similarly, when c is an integer of 2 or more, two or more R 8 may be the same or different.
[0134] In order to obtain better flexibility, R 5 , R 6 , R 7 and R 8 (However, R 7 and R 8(only in formula (3)) each independently includes an alkyl group having 1 to 6 carbon atoms, a phenyl group, etc., and examples of the alkyl group include a methyl group, etc. In formula (3), a and c each independently can be 6 to 2000, but may be 10 to 1000. In formulas (2) and (3), b can be 2 to 30, but may be 5 to 20.
[0135] (Third Aspect) The aerogel of this embodiment may be a dried product of a wet gel (obtained by drying a wet gel produced from a sol) that is a condensate of a sol containing at least one selected from the group consisting of a silicon compound having a hydrolyzable functional group or a condensable functional group and a hydrolysis product of a silicon compound having a hydrolyzable functional group. Note that the aerogels described so far may also be obtained by drying a wet gel produced from a sol containing a silicon compound or the like.
[0136] A polysiloxane compound can be used as the silicon compound having a hydrolyzable functional group or a condensable functional group. That is, the sol can contain at least one compound selected from the group consisting of polysiloxane compounds having a hydrolyzable functional group or a condensable functional group and hydrolysis products of polysiloxane compounds having a hydrolyzable functional group (hereinafter sometimes referred to as "polysiloxane compound group").
[0137] The functional groups in the polysiloxane compound are not particularly limited, and may be groups that react with the same functional groups or with other functional groups. Examples of hydrolyzable functional groups include alkoxy groups. Examples of condensable functional groups include hydroxyl groups, silanol groups, carboxyl groups, and phenolic hydroxyl groups. The hydroxyl groups may be contained in hydroxyl group-containing groups such as hydroxyalkyl groups. Note that polysiloxane compounds having hydrolyzable or condensable functional groups may further contain reactive groups different from the hydrolyzable and condensable functional groups (functional groups that do not fall under the category of hydrolyzable or condensable functional groups). Examples of reactive groups include epoxy groups, mercapto groups, glycidoxy groups, vinyl groups, acryloyl groups, methacryloyl groups, and amino groups. The epoxy groups may be contained in epoxy group-containing groups such as glycidoxy groups. Polysiloxane compounds having these functional groups and reactive groups may be used alone or in combination of two or more types. Among these functional groups and reactive groups, for example, groups that improve the flexibility of the aerogel include alkoxy groups, silanol groups, and hydroxyalkyl groups. Of these, alkoxy groups and hydroxyalkyl groups can further improve the compatibility of the sol. Furthermore, from the viewpoint of improving the reactivity of the polysiloxane compound and reducing the thermal conductivity of the aerogel, the number of carbon atoms in the alkoxy groups and hydroxyalkyl groups can be 1 to 6. However, from the viewpoint of further improving the flexibility of the aerogel, the number of carbon atoms may be 2 to 5 or 2 to 4.
[0138] (Fourth Aspect) The aerogel according to this embodiment may further contain silica particles in addition to the aerogel component in order to further increase toughness and achieve even better heat insulation and flexibility. An aerogel containing the aerogel component and silica particles can also be called an aerogel composite. The aerogel composite is a composite of the aerogel component and the silica particles, but it still has a cluster structure that is characteristic of aerogel, and is considered to have a three-dimensionally fine porous structure.
[0139] The aerogel containing the aerogel component and silica particles can be said to be a dried product of a wet gel that is a condensate of a sol containing silica particles and at least one selected from the group consisting of silicon compounds having hydrolyzable functional groups or condensable functional groups and hydrolysis products of silicon compounds having hydrolyzable functional groups. Therefore, the descriptions of the first to third aspects can also be applied mutatis mutandis to the aerogel according to this embodiment.
[0140] The silica particles can be used without any particular limitation, and examples thereof include amorphous silica particles. Examples of amorphous silica particles include fused silica particles, fumed silica particles, and colloidal silica particles. Among these, colloidal silica particles have high monodispersity and are easy to suppress aggregation in the sol. The silica particles may also be silica particles having a hollow structure, a porous structure, or the like.
[0141] The shape of the silica particles is not particularly limited, and examples include spherical, cocoon-shaped, and association-type silica particles. Among these, the use of spherical silica particles makes it easier to suppress aggregation in the sol. The average primary particle diameter of the silica particles may be 1 nm or more, 5 nm or more, or 20 nm or more, from the viewpoint of easily imparting appropriate strength and flexibility to the aerogel and easily obtaining an aerogel with excellent shrinkage resistance during drying. The average primary particle diameter of the silica particles may be 500 nm or less, 300 nm or less, or 100 nm or less, from the viewpoint of easily suppressing the solid-state thermal conductivity of the silica particles and easily obtaining an aerogel with excellent thermal insulation properties. From these viewpoints, the average primary particle diameter of the silica particles may be 1 to 500 nm, 5 to 300 nm, or 20 to 100 nm.
[0142] In this embodiment, the average particle size of the aerogel components and the average primary particle size of the silica particles can be obtained by directly observing the aerogel using a scanning electron microscope (hereinafter abbreviated as "SEM"). The "diameter" here refers to the diameter of a particle exposed on the cross section of the aerogel when the cross section is considered to be a circle. Furthermore, the "diameter when the cross section is considered to be a circle" refers to the diameter of a perfect circle when the area of the cross section is replaced with a perfect circle of the same area. The average particle size is calculated by determining the diameter of circles for 100 particles and averaging them.
[0143] The average particle size of silica particles can also be measured from the raw material. For example, the biaxial average primary particle size is calculated as follows from the results of observing 20 random particles using an SEM. Taking colloidal silica particles, which are typically dispersed in water with a solids concentration of about 5 to 40% by mass, as an example, a wafer with patterned wiring is cut into 2 cm square chips, which are immersed in a dispersion of colloidal silica particles for about 30 seconds, then the chips are rinsed with pure water for about 30 seconds and dried with nitrogen blowing. The chips are then placed on a sample stage for SEM observation, an accelerating voltage of 10 kV is applied, and the silica particles are observed at a magnification of 100,000 times, and an image is taken. From the obtained image, 20 silica particles are randomly selected, and the average particle size of these particles is taken as the average particle size.
[0144] <Aerogel Particles> The aerogel particles in this embodiment can be obtained, for example, by pulverizing bulk aerogel as described below.
[0145] The average particle size (D50) (also referred to as the average diameter) of the aerogel particles can be 0.1 to 1000 μm, but may also be 0.5 to 700 μm, 1 to 500 μm, 3 to 100 μm, or 5 to 50 μm. When the average particle size (D50) of the aerogel particles is large, it becomes easier to obtain aerogel particles with excellent dispersibility, handleability, etc. On the other hand, when the average particle size (D50) is small, it becomes easier to obtain aerogel particles with excellent dispersibility. The average particle size (D50) of the aerogel particles can be appropriately adjusted by the pulverization method and pulverization conditions, sieving, classification method, etc.
[0146] The average particle diameter (D50) of aerogel particles can be measured by laser diffraction / scattering. For example, aerogel particles are added to a solvent (ethanol) so that the content is 0.05 to 5% by mass, and the aerogel particles are dispersed by vibrating with a 50W ultrasonic homogenizer for 15 to 30 minutes. Approximately 10 mL of the dispersion is then injected into a laser diffraction / scattering particle size distribution analyzer, and the particle size is measured at 25°C, with a refractive index of 1.3 and an absorption of 0. The particle size at an integrated value of 50% (volume basis) in this particle size distribution is taken as the average particle diameter D50. For example, a Microtrac MT3000 (manufactured by Nikkiso Co., Ltd.) can be used as the measuring device.
[0147] Commercially available aerogel particles may also be used, such as ENOVA MT1100 (manufactured by CABOT Corporation) and AeroVa (manufactured by JIS AEROGEL CORPORATION).
[0148] In this embodiment, the amount of aerogel particles in the coating liquid is preferably such that the content of the aerogel particles in the composite material is 70 vol% or more, more preferably 72 vol% or more, and even more preferably 74 vol% or more, based on the total volume of the composite material. Alternatively, the amount of aerogel particles in the coating liquid may be such that the content of the aerogel particles in the composite material is, for example, 99 vol% or less, 98 vol% or less, or 97 vol% or less, based on the total volume of the composite material.
[0149] <Method for Producing Aerogel Particles> The method for producing aerogel particles is not particularly limited, but for example, they can be produced by the following method.
[0150] The aerogel particles of this embodiment can be produced by a production method mainly including a sol production step, a wet gel production step in which the sol obtained in the sol production step is gelled and then aged to obtain a wet gel, a washing and solvent substitution step in which the wet gel obtained in the wet gel production step is washed and (if necessary) solvent-substituted, a drying step in which the washed and solvent-substituted wet gel is dried, and a crushing step in which the aerogel obtained by drying is crushed.
[0151] Alternatively, the composition may be produced by a production method mainly including a sol production process, a wet gel production process, a wet gel crushing process for crushing the wet gel obtained in the wet gel production process, a washing and solvent substitution process, and a drying process.
[0152] The size of the obtained aerogel particles can be further uniformed by sieving, classification, etc. Uniform particle size can improve dispersibility. The term "sol" refers to the state before the gelation reaction occurs, and in this embodiment, refers to the state in which the silicon compound and, optionally, silica particles are dissolved or dispersed in a solvent. The term "wet gel" refers to a gel solid in a wet state that contains a liquid medium but does not have fluidity.
[0153] (Sol generation process) The sol generation process is a process in which a silicon compound and, optionally, silica particles (or a solvent containing silica particles) are mixed to undergo a hydrolysis reaction, followed by generation of a sol. In this process, an acid catalyst may be further added to the solvent to promote the hydrolysis reaction. As shown in Japanese Patent No. 5250900, a surfactant, a thermally hydrolyzable compound, etc. may also be added to the solvent. Furthermore, for the purpose of suppressing heat radiation, etc., components such as carbon graphite, an aluminum compound, a magnesium compound, a silver compound, a titanium compound, etc. may also be added to the solvent.
[0154] As the solvent, for example, water or a mixture of water and alcohol can be used. Examples of alcohol include methanol, ethanol, n-propanol, 2-propanol, n-butanol, 2-butanol, and t-butanol. Among these, examples of alcohols that have low surface tension and low boiling points, from the viewpoint of reducing the interfacial tension with the gel wall, include methanol, ethanol, and 2-propanol. These may be used alone or in combination of two or more.
[0155] For example, when alcohol is used as the solvent, the amount of alcohol can be 4 to 8 moles per mole of the total amount of the silicon compounds and the polysiloxane compounds, but may also be 4 to 6.5, or 4.5 to 6 moles. By using an alcohol amount of 4 moles or more, good compatibility can be more easily obtained, and by using an alcohol amount of 8 moles or less, shrinkage of the gel can be more easily suppressed.
[0156] Examples of acid catalysts include inorganic acids such as hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, hypophosphorous acid, bromic acid, chloric acid, chlorous acid, and hypochlorous acid; acidic phosphates such as aluminum acid phosphate, magnesium acid phosphate, and zinc acid phosphate; and organic carboxylic acids such as acetic acid, formic acid, propionic acid, oxalic acid, malonic acid, succinic acid, citric acid, malic acid, adipic acid, and azelaic acid. Among these, organic carboxylic acids are preferred as acid catalysts that further improve the water resistance of the resulting aerogel. Examples of such organic carboxylic acids include acetic acid, but they may also include formic acid, propionic acid, oxalic acid, and malonic acid. These may be used alone or in combination of two or more.
[0157] By using an acid catalyst, the hydrolysis reaction of the silicon compound can be accelerated, and the sol can be obtained in a shorter time.
[0158] The amount of the acid catalyst added can be 0.001 to 0.1 parts by mass per 100 parts by mass of the total amount of the polysiloxane compounds and silicon compounds.
[0159] The surfactant may be a nonionic surfactant, an ionic surfactant, etc. These may be used alone or in combination of two or more.
[0160] Examples of nonionic surfactants that can be used include compounds containing a hydrophilic portion such as polyoxyethylene and a hydrophobic portion mainly composed of an alkyl group, and compounds containing a hydrophilic portion such as polyoxypropylene. Examples of compounds containing a hydrophilic portion such as polyoxyethylene and a hydrophobic portion mainly composed of an alkyl group include polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, and polyoxyethylene alkyl ether. Examples of compounds containing a hydrophilic portion such as polyoxypropylene include polyoxypropylene alkyl ether and block copolymers of polyoxyethylene and polyoxypropylene.
[0161] Examples of ionic surfactants include cationic surfactants, anionic surfactants, and amphoteric surfactants. Examples of cationic surfactants include cetyltrimethylammonium bromide and cetyltrimethylammonium chloride, and examples of anionic surfactants include sodium dodecylsulfonate. Examples of amphoteric surfactants include amino acid surfactants, betaine surfactants, and amine oxide surfactants. Examples of amino acid surfactants include acyl glutamic acid. Examples of betaine surfactants include lauryl dimethyl amino acetate betaine and stearyl dimethyl amino acetate betaine. Examples of amine oxide surfactants include lauryl dimethyl amine oxide.
[0162] These surfactants are thought to act to reduce the difference in chemical affinity between the solvent in the reaction system and the growing siloxane polymer, thereby suppressing phase separation in the wet gel formation process described below.
[0163] The amount of surfactant added will depend on the type of surfactant and the type and amount of silicon compound, but can be, for example, 1 to 100 parts by mass per 100 parts by mass of the total amount of polysiloxane compounds and silicon compounds, or 5 to 60 parts by mass.
[0164] The thermally hydrolyzable compound is thought to generate a base catalyst by thermal hydrolysis, making the reaction solution basic and accelerating the sol-gel reaction in the wet gel production step described below. Therefore, the thermally hydrolyzable compound is not particularly limited as long as it is a compound that can make the reaction solution basic after hydrolysis, and examples thereof include urea; acid amides such as formamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-methylacetamide, and N,N-dimethylacetamide; and cyclic nitrogen compounds such as hexamethylenetetramine. Among these, urea is particularly likely to provide the accelerating effect.
[0165] The amount of the thermally hydrolyzable compound added is not particularly limited, as long as it is an amount that can sufficiently promote the sol-gel reaction in the wet gel formation step described below. For example, when urea is used as the thermally hydrolyzable compound, the amount added can be 1 to 200 parts by mass relative to 100 parts by mass of the total amount of the polysiloxane compounds and the silicon compounds. The amount added may also be 2 to 150 parts by mass. By adding an amount of 1 part by mass or more, good reactivity can be more easily obtained, and by adding an amount of 200 parts by mass or less, crystal precipitation and a decrease in gel density can be more easily suppressed.
[0166] The hydrolysis in the sol production step depends on the types and amounts of the silicon compound, silica particles, acid catalyst, surfactant, etc. in the mixed solution, but may be carried out, for example, in a temperature environment of 20 to 60° C. for 10 minutes to 24 hours, or in a temperature environment of 50 to 60° C. for 5 minutes to 8 hours. This allows the hydrolyzable functional groups in the silicon compound to be sufficiently hydrolyzed, making it possible to more reliably obtain a hydrolysis product of the silicon compound.
[0167] However, when a thermally hydrolyzable compound is added to a solvent, the temperature environment in the sol formation step may be adjusted to a temperature that suppresses hydrolysis of the thermally hydrolyzable compound and suppresses gelation of the sol. The temperature at this time may be any temperature as long as it can suppress hydrolysis of the thermally hydrolyzable compound. For example, when urea is used as the thermally hydrolyzable compound, the temperature environment in the sol formation step may be 0 to 40°C, but may also be 10 to 30°C.
[0168] (Wet Gel Formation Step) In the wet gel formation step, the sol obtained in the sol formation step is gelled, and then aged to obtain a wet gel. In this step, a base catalyst can be used to promote gelation.
[0169] Examples of the base catalyst include carbonates such as calcium carbonate, potassium carbonate, sodium carbonate, barium carbonate, magnesium carbonate, lithium carbonate, ammonium carbonate, copper (II) carbonate, iron (II) carbonate, and silver (I) carbonate; hydrogen carbonates such as calcium hydrogen carbonate, potassium hydrogen carbonate, sodium hydrogen carbonate, and ammonium hydrogen carbonate; alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, and cesium hydroxide; ammonium compounds such as ammonium hydroxide, ammonium fluoride, ammonium chloride, and ammonium bromide; basic sodium phosphates such as sodium metaphosphate, sodium pyrophosphate, and sodium polyphosphate; allylamine, diallylamine, triallylamine, isopropylamine, diisopropylamine, ethylamine, diethylamine, Examples of suitable base catalysts include aliphatic amines such as ethanol, triethylamine, 2-ethylhexylamine, 3-ethoxypropylamine, diisobutylamine, 3-(diethylamino)propylamine, di-2-ethylhexylamine, 3-(dibutylamino)propylamine, tetramethylethylenediamine, t-butylamine, sec-butylamine, propylamine, 3-(methylamino)propylamine, 3-(dimethylamino)propylamine, 3-methoxyamine, dimethylethanolamine, methyldiethanolamine, diethanolamine, and triethanolamine; and nitrogen-containing heterocyclic compounds such as morpholine, N-methylmorpholine, 2-methylmorpholine, piperazine and its derivatives, piperidine and its derivatives, and imidazole and its derivatives. Among these, ammonium hydroxide (aqueous ammonia) is highly volatile and unlikely to remain in the aerogel particles after drying, thereby preventing deterioration of water resistance and being economical. The above-mentioned base catalysts may be used alone or in combination of two or more.
[0170] The use of a base catalyst can promote the dehydration condensation reaction or dealcoholization condensation reaction of the silicon compound and silica particles in the sol, thereby enabling the gelation of the sol to be completed in a shorter time. This also allows a wet gel with higher strength (rigidity) to be obtained. In particular, since ammonia is highly volatile and does not easily remain in the aerogel particles, the use of ammonia as a base catalyst allows the production of aerogel particles with better water resistance.
[0171] The amount of base catalyst added can be 0.5 to 5 parts by mass, but may also be 1 to 4 parts by mass, per 100 parts by mass of the total amount of the polysiloxane compounds and silicon compounds. By using an amount of 0.5 parts by mass or more, gelation can be carried out in a shorter time, and by using an amount of 5 parts by mass or less, deterioration in water resistance can be further suppressed.
[0172] The gelation of the sol in the wet gel formation step may be carried out in a sealed container to prevent the solvent and base catalyst from volatilizing. The gelation temperature can be set to 30 to 90°C, but may also be set to 40 to 80°C. By setting the gelation temperature to 30°C or higher, gelation can be carried out in a shorter time, and a wet gel with higher strength (rigidity) can be obtained. Furthermore, by setting the gelation temperature to 90°C or lower, it is easier to suppress the volatilization of the solvent (especially alcohol), and therefore gelation can be carried out while suppressing volumetric shrinkage.
[0173] The aging in the wet gel production step may be carried out in a sealed container to prevent the solvent and base catalyst from volatilizing. The aging strengthens the bonds between the components that make up the wet gel, resulting in a wet gel with sufficient strength (rigidity) to suppress shrinkage during drying. The aging temperature can be 30 to 90°C, but may also be 40 to 80°C. By setting the aging temperature to 30°C or higher, a wet gel with higher strength (rigidity) can be obtained, and by setting the aging temperature to 90°C or lower, volatilization of the solvent (especially alcohol) can be easily suppressed, allowing gelation while suppressing volumetric shrinkage.
[0174] Since it is often difficult to determine the time when the gelation of the sol is completed, the gelation of the sol and the subsequent aging may be carried out in a continuous series of operations.
[0175] The gelation time and aging time can be appropriately set depending on the gelation temperature and aging temperature. When silica particles are contained in the sol, the gelation time can be particularly shortened compared to when silica particles are not contained. This is presumably because the silanol groups or reactive groups of the silicon compound in the sol form hydrogen bonds or chemical bonds with the silanol groups of the silica particles. The gelation time can be set to 10 to 120 minutes, but may also be set to 20 to 90 minutes. Setting the gelation time to 10 minutes or more makes it easier to obtain a homogeneous wet gel, while setting it to 120 minutes or less enables simplification of the washing and solvent substitution process to the drying process described below. The total time for the gelation and aging process as a whole can be set to 4 to 480 hours, but may also be set to 6 to 120 hours. Setting the total gelation time and aging time to 4 hours or more makes it possible to obtain a wet gel with higher strength (rigidity), and setting it to 480 hours or less makes it easier to maintain the aging effect.
[0176] To decrease the density of the resulting aerogel particles or increase the average pore size, the gelation temperature and aging temperature may be increased within the above ranges, or the total time of the gelation time and aging time may be increased within the above ranges. Alternatively, to increase the density of the resulting aerogel particles or decrease the average pore size, the gelation temperature and aging temperature may be decreased within the above ranges, or the total time of the gelation time and aging time may be decreased within the above ranges.
[0177] (Wet Gel Crushing Step) When the wet gel crushing step is performed, the wet gel obtained in the wet gel production step is crushed. Crushing can be performed, for example, by placing the wet gel in a Henshall mixer, or by performing the wet gel production step in a mixer and operating the mixer under appropriate conditions (rotation speed and time). Alternatively, more simply, the wet gel can be placed in a sealable container, or by performing the wet gel production step in a sealable container and shaking for an appropriate period of time using a shaking device such as a shaker. If necessary, the particle size of the wet gel can also be adjusted using a jet mill, roller mill, bead mill, or the like.
[0178] (Washing and Solvent Replacement Step) The washing and solvent replacement step includes a step of washing the wet gel obtained by the wet gel production step or the wet gel crushing step (washing step), and a step of replacing the washing liquid in the wet gel with a solvent suitable for drying conditions (the drying step described below) (solvent replacement step). The washing and solvent replacement step can be carried out in a form in which only the solvent replacement step is performed without performing the step of washing the wet gel. However, from the viewpoint of reducing impurities such as unreacted substances and by-products in the wet gel and enabling the production of aerogel particles with higher purity, the wet gel may be washed.
[0179] In the washing step, the wet gel obtained in the wet gel generating step or the wet gel crushing step is washed. The washing can be performed repeatedly using, for example, water or an organic solvent. In this case, the washing efficiency can be improved by heating.
[0180] As the organic solvent, various organic solvents can be used, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, acetone, methyl ethyl ketone, 1,2-dimethoxyethane, acetonitrile, hexane, toluene, diethyl ether, chloroform, ethyl acetate, tetrahydrofuran, methylene chloride, N,N-dimethylformamide, dimethyl sulfoxide, acetic acid, formic acid, etc. The above organic solvents may be used alone or in combination of two or more.
[0181] In the solvent substitution step described below, a low surface tension solvent can be used to suppress gel shrinkage due to drying. However, low surface tension solvents generally have extremely low mutual solubility with water. Therefore, when a low surface tension solvent is used in the solvent substitution step, the organic solvent used in the washing step can be a hydrophilic organic solvent that has high mutual solubility with both water and the low surface tension solvent. The hydrophilic organic solvent used in the washing step can serve as a preliminary replacement for the solvent substitution step. Among the above organic solvents, examples of hydrophilic organic solvents include methanol, ethanol, 2-propanol, acetone, and methyl ethyl ketone. Methanol, ethanol, methyl ethyl ketone, and the like are economically advantageous.
[0182] The amount of water or organic solvent used in the washing step can be an amount that can sufficiently replace the solvent in the wet gel and wash it. This amount can be 3 to 10 times the volume of the wet gel. Washing can be repeated until the water content in the wet gel after washing is 10 mass% or less relative to the mass of silica.
[0183] The temperature environment in the washing step can be a temperature below the boiling point of the solvent used for washing. For example, when methanol is used, the temperature can be raised to about 30 to 60°C.
[0184] In the solvent substitution process, the solvent in the washed wet gel is replaced with a predetermined substitution solvent to suppress shrinkage of the aerogel during the drying process. Heating the solvent during this process can improve substitution efficiency. Specifically, when drying is performed under atmospheric pressure at a temperature below the critical point of the solvent used for drying in the drying process, low-surface-tension solvents, as described below, are used as the substitution solvent. On the other hand, when supercritical drying is performed, examples of the substitution solvent include ethanol, methanol, 2-propanol, dichlorodifluoromethane, carbon dioxide, etc., or a mixture of two or more of these solvents.
[0185] Examples of solvents with low surface tension include solvents having a surface tension of 30 mN / m or less at 20° C. The surface tension may be 25 mN / m or less, or 20 mN / m or less. Examples of low surface tension solvents include aliphatic hydrocarbons such as pentane (15.5), hexane (18.4), heptane (20.2), octane (21.7), 2-methylpentane (17.4), 3-methylpentane (18.1), 2-methylhexane (19.3), cyclopentane (22.6), cyclohexane (25.2), and 1-pentene (16.0); aromatic hydrocarbons such as benzene (28.9), toluene (28.5), m-xylene (28.7), and p-xylene (28.3); and hydrocarbons such as dichloromethane (27.9), chloroform (27.2), carbon tetrachloride (26.9), 1-chloropropane (21.8), and 2-chloropropane (18.1). Examples of suitable solvents include halogenated hydrocarbons; ethers such as ethyl ether (17.1), propyl ether (20.5), isopropyl ether (17.7), butyl ethyl ether (20.8), and 1,2-dimethoxyethane (24.6); ketones such as acetone (23.3), methyl ethyl ketone (24.6), methyl propyl ketone (25.1), and diethyl ketone (25.3); and esters such as methyl acetate (24.8), ethyl acetate (23.8), propyl acetate (24.3), isopropyl acetate (21.2), isobutyl acetate (23.7), and ethyl butyrate (24.6). (The values in parentheses indicate the surface tension at 20°C, in units of mN / m.) Among these, aliphatic hydrocarbons (e.g., hexane and heptane) have low surface tension and are excellent in terms of work environment. Furthermore, hydrophilic organic solvents such as acetone, methyl ethyl ketone, and 1,2-dimethoxyethane can be used in combination with the organic solvent used in the cleaning step. Among these, solvents having a boiling point of 100° C. or less at normal pressure may be used because they are easy to dry in the drying step described below. The above solvents may be used alone or in combination of two or more.
[0186] The amount of solvent used in the solvent substitution step can be an amount that can sufficiently substitute the solvent in the wet gel after washing, and can be 3 to 10 times the volume of the wet gel.
[0187] The temperature environment in the solvent substitution step can be a temperature below the boiling point of the solvent used for substitution. For example, when heptane is used, the temperature can be raised to about 30 to 60°C.
[0188] It should be noted that when silica particles are contained in the gel, the solvent substitution step is not essential. The presumed mechanism is as follows: The silica particles function as a support for the three-dimensional network skeleton, thereby supporting the skeleton and suppressing gel shrinkage during the drying step. Therefore, it is believed that the gel can be directly subjected to the drying step without replacing the solvent used for washing. In this way, the use of silica particles makes it possible to simplify the washing and solvent substitution steps to the drying step.
[0189] (Drying Step) In the drying step, the wet gel that has been washed and (if necessary) solvent-substituted as described above is dried. This allows aerogel (aerogel blocks or aerogel particles) to be obtained. In other words, the aerogel can be obtained by drying the wet gel produced from the sol.
[0190] The drying method is not particularly limited, and known methods such as atmospheric drying, supercritical drying, or freeze drying can be used. Among these, atmospheric drying or supercritical drying can be used from the viewpoint of ease of producing a low-density aerogel. Furthermore, atmospheric drying can be used from the viewpoint of low-cost production. In this embodiment, atmospheric pressure means 0.1 MPa (atmospheric pressure).
[0191] Aerogel can be obtained by drying a washed and (optionally) solvent-substituted wet gel at atmospheric pressure at a temperature below the critical point of the solvent used for drying. The drying temperature varies depending on the type of substituted solvent (or the solvent used for washing if solvent substitution is not performed), but can be set to 20 to 150°C, taking into account that drying at high temperatures can accelerate the evaporation rate of the solvent and cause large cracks in the gel. The drying temperature may be 60 to 120°C. The drying time varies depending on the volume of the wet gel and the drying temperature, but can be set to 4 to 120 hours. Accelerating drying by applying a pressure below the critical point within a range that does not impair productivity is also considered to be atmospheric pressure drying.
[0192] Aerogels can also be obtained by supercritical drying a wet gel that has been washed and (if necessary) solvent-substituted. Supercritical drying can be performed using known techniques. Examples of supercritical drying methods include removing the solvent at a temperature and pressure equal to or higher than the critical point of the solvent contained in the wet gel. Alternatively, examples of supercritical drying methods include immersing the wet gel in liquefied carbon dioxide at, for example, 20 to 25°C and approximately 5 to 20 MPa, thereby replacing all or part of the solvent contained in the wet gel with carbon dioxide having a lower critical point than the solvent, and then removing the carbon dioxide alone or a mixture of carbon dioxide and the solvent.
[0193] The aerogel obtained by such atmospheric drying or supercritical drying may be further dried at atmospheric pressure at 105 to 200°C for about 0.5 to 2 hours. This makes it easier to obtain an aerogel with low density and small pores. The additional drying may be performed at atmospheric pressure at 150 to 200°C.
[0194] (Crushing step) When the wet gel crushing step is not performed, the aerogel (aerogel block) obtained by drying is crushed to obtain aerogel particles. For example, this can be done by placing the aerogel in a jet mill, roller mill, bead mill, hammer mill, etc. and operating it at an appropriate rotation speed for an appropriate time.
[0195] <Liquid Medium> The liquid medium is preferably an aqueous solvent containing water. The aqueous solvent may contain an organic solvent in addition to water. The organic solvent may be any organic solvent as long as it is compatible with water, and examples thereof include alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, and propylene glycol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and methyl ethyl ketone; carboxylic acids such as acetic acid and propionic acid; and nitrogen-containing compounds such as acetonitrile, dimethylformamide, and triethylamine.
[0196] In this embodiment, the content of the liquid medium in the coating liquid is not particularly limited and may be changed appropriately depending on the desired viscosity of the coating liquid, etc. For example, the content of the liquid medium may be an amount that causes the nonvolatile content of the coating liquid to fall within a suitable range described below.
[0197] The nonvolatile content of the coating liquid may be, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more, and may be, for example, 70% by mass or less, preferably 60% by mass or less, and more preferably 50% by mass or less.
[0198] <Other Components> In this embodiment, the coating liquid may further contain other components in addition to those described above.
[0199] The coating liquid of this embodiment may further contain, for example, a thickener, a pigment, a leveling agent, etc. Examples of the thickener include fine particles of fumed silica, clay minerals, etc.
[0200] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above embodiments.
[0201] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0202] (Example 1) (1) Production of emulsion A reaction vessel equipped with a stirrer, a thermometer, a condenser, and a dropping funnel was charged with 160 parts by mass of ion-exchanged water and 1.2 parts by mass of a nonionic emulsifier (Emulgen 1150S-60, a 60% aqueous solution of polyoxyethylene alkyl ether, manufactured by Kao Corporation, HLB value: 18.5), and the mixture was stirred and heated to 65°C. After that, nitrogen was passed through the reaction vessel to remove dissolved oxygen.
[0203] Next, 274 parts by mass of butyl acrylate, 173.5 parts by mass of methyl methacrylate, 24 parts by mass of 2-hydroxyethyl methacrylate, 9 parts by mass of methacrylic acid, 215 parts by mass of ion-exchanged water, and 48.8 parts by mass of a nonionic emulsifier (Emulgen 1150S-60, a 60% aqueous solution of polyoxyethylene alkyl ether, manufactured by Kao Corporation, HLB value: 18.5) were mixed and emulsified in a homomixer to obtain a monomer emulsion.
[0204] 3% of this monomer emulsion was added to the reaction vessel under stirring, and 0.7 parts by weight of "Trigonox A-W70" (70% aqueous solution of tert-butyl hydroperoxide, manufactured by Kayaku Nouryon Co., Ltd.) and 0.23 parts by weight of ascorbic acid were added as a radical polymerization initiator and allowed to react for 15 minutes. Next, the remaining 97% of the monomer emulsion, a solution of 0.9 parts by weight of "Trigonox A-W70" dissolved in 60 parts by weight of ion-exchanged water, and a solution of 0.37 parts by weight of ascorbic acid dissolved in 60 parts by weight of ion-exchanged water were each added dropwise to the reaction vessel over a period of 4 hours and allowed to react. After completion of the dropwise addition, the mixture was stirred for another hour at 65°C, cooled to below 40°C, and 2.9 parts by weight of 26% aqueous ammonia was added as a neutralizer. This resulted in an emulsion containing emulsified particles containing a binder resin and a nonionic emulsifier, and water.
[0205] The properties of the emulsion were as follows: Nonvolatile content: 49.5% by mass Viscosity at 23°C: 35 mPa·s pH at 23°C: 8.6 Minimum film formation temperature (MFT): 5°C Glass transition temperature of binder resin: 9°C Average particle size of emulsion particles: 210 nm
[0206] [Measurement of non-volatile content of emulsion] 1 g of emulsion was weighed, placed on an aluminum dish with a diameter of 5 cm, and placed in a dryer. While circulating air in the dryer, the emulsion was dried at 1 atmosphere (1013 hPa) and a temperature of 105°C for 1 hour, and the mass of the remaining components was measured. The mass ratio (mass%) of the above components remaining after drying relative to the mass (1 g) of the emulsion before drying was calculated, and this was taken as the non-volatile content concentration (mass%).
[0207] [Measurement of Emulsion Viscosity] Measurement was carried out using a BL type viscometer as a measuring instrument under conditions of a temperature of 23° C. and a rotation speed of 60 rpm.
[0208] [Measurement of pH of emulsion] The pH at 23°C was measured using a pH meter (glass electrode type hydrogen ion concentration indicator HM-30G, manufactured by DKK-TOA Corporation).
[0209] [Measurement of Average Particle Diameter of Emulsified Particles] The average particle diameter (d50) of emulsified particles was measured at 23°C by dynamic light scattering (DLS) using a MICROTRAC UPA150 (manufactured by Microtrac Bell Co., Ltd.).
[0210] [Measurement of minimum film formation temperature (MFT)] The emulsion was applied to the measurement surface of a thermal gradient MFT measuring instrument using a 0.3 mm applicator and allowed to dry in a windless environment. The dried film was visually observed for cracks due to film formation failure, and the MFT was measured.
[0211] [Glass transition temperature (Tg) of binder resin] The glass transition temperature (Tg) of the binder resin was determined by measuring the temperature dependence of the loss tangent using a rheometer (MCR-102, manufactured by Anton Paar). A parallel plate with a diameter of 12 mm was used, and the vibration mode was set at a frequency of 1 Hz and a strain of 2%. After dispensing a small amount of the emulsion onto the measurement plate, the plate was brought into contact with the plate and heated from 30 ° C to 180 ° C at a rate of 10 ° C / min, thereby removing the volatile components of the emulsion and adhering the resin to the plate. The temperature was then lowered from 180 ° C to 0 ° C at a rate of 2 ° C / min, and the loss tangent was measured at intervals of 1 point / ° C. The temperature at which the loss tangent was maximum was taken as the glass transition temperature.
[0212] (2) Preparation of coating liquid In a 500 mL separable flask, 1 part by mass of Sangelose 90L (manufactured by Daido Chemical Industry Co., Ltd.) as a water-soluble polymer, 9 parts by mass of isopropyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent), 179 parts by mass of hot water, and 4 parts by mass of glass fiber (manufactured by Nitto Boseki Co., Ltd., product name: CS 3J-891) were placed and stirred at 200 rpm using a mechanical stirrer for 1 minute to obtain a dispersion. Subsequently, while cooling the flask in an ice-water bath, the Sangelose 90L was dissolved by stirring at 200 rpm using a mechanical stirrer to obtain a pregel, which was an aqueous solution of Sangelose 90L. 188 parts by mass of the pregel and 21 parts by mass of aerogel particles (manufactured by CABOT, product name: ENOVA MT1100, particle diameter 2-24 μm, average particle size (D50) 10 μm) were added to a planetary mixer (Primix Corporation, Model 2P-1) and stirred at 25 rpm for 10 minutes. Next, 86 parts by mass of the emulsion obtained in (1) was added, and the mixture was stirred at 25 rpm for 15 minutes to obtain a coating liquid. Based on the total volume of solids in the coating liquid, the aerogel particle content was 84.9 vol%, the water-soluble polymer content was 0.3 vol%, and the acrylic resin content was 14.1 vol%. The average diameter of the aerogel particle aggregates in the resulting coating liquid was measured using the following method. The results are shown in Table 1.
[0213] <Measurement of the average diameter of aerogel particle aggregates> Approximately 20 g of the coating liquid was placed in a 100 mL plastic cup, and water was added in 2 g increments while stirring with a spatula, gradually diluting the mixture. The diluted sample was placed on a glass plate, and the aerogel particle aggregates in the coating liquid were observed using an optical microscope (manufactured by Olympus, model number: BX51) to obtain micrographs. The obtained micrographs were analyzed using image editing software ImageJ to determine the average diameter of the aerogel particle aggregates.
[0214] <Crack Evaluation> The coating liquid was applied to a stainless steel plate (100 mm x 70 mm x 0.8 mm) using an air spray (hopper gun, model 25D496, manufactured by Graco Corporation) to a thickness of 2 mm, and the coating liquid was left to stand at room temperature of 23°C for 12 hours to remove the liquid medium, yielding a stainless steel plate with a 1 mm thickness composite material. The resulting composite material was evaluated for cracking, with A representing no cracks throughout, B representing localized cracks, and C representing cracks throughout.
[0215] <Evaluation of pore volume of composite material> A composite material was produced in the same manner as in the above <Evaluation of cracking>. 100 mg of the obtained composite material was sampled, and the pore volume was calculated using a high-sensitivity gas adsorption analyzer (AutoSorb iQ, manufactured by Quantachrome).
[0216] <Evaluation of thermal conductivity of composite material> A composite material was prepared in the same manner as in the above <Crack evaluation>. This procedure was repeated to obtain a composite material with a thickness of 3.0 m. The thermal conductivity of the obtained composite material was measured by a steady-state method using a thermal conductivity measuring device "HFM-446" (product name, manufactured by NETZSCH).
[0217] Example 2 A coating liquid was prepared in the same manner as in Example 1. The obtained coating liquid was used to draw a line at 30 kPa and a speed of 20 mm / s using a dispenser (ML-808GX (dispenser) / SHOTMASTER Ωx (motion unit) manufactured by Musashi Engineering) equipped with a tapered nozzle having an inner diameter of 1.6 mm. The line was then left at room temperature of 23°C for 12 hours to remove the liquid medium from the coating liquid, yielding a stainless steel plate with a composite material line having a width of 1.6 mm and a maximum thickness of 0.8 mm. The degree of cracking of the obtained composite material was evaluated, with A being the case where there were no cracks throughout, B being the case where there were localized cracks, and C being the case where there were cracks throughout. The evaluation was otherwise carried out in the same manner as in Example 1. The results are shown in Table 1.
[0218] Comparative Example 1 A coating liquid was prepared in the same manner as in Example 1. 15 g of the obtained coating liquid was placed on a stainless steel plate, swept several times using a disposable spatula (made by PP, manufactured by AS ONE), and left at room temperature of 23°C for 12 hours to remove the liquid medium from the coating liquid, yielding a stainless steel plate with a thickness of 1 mm and a composite material. The degree of cracking of the obtained composite material was evaluated, with A being when there were no cracks throughout, B being when there were localized cracks, and C being when there were cracks throughout. The rest of the evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1.
[0219] Comparative Example 2 A coating liquid was prepared in the same manner as in Example 1. The resulting coating liquid was applied to a stainless steel plate using a roller (for interior paint finishes, bristle length 5 mm) and left to stand at room temperature of 23°C for 12 hours to remove the liquid medium from the coating liquid, yielding a stainless steel plate with a composite material of 0.2 mm in thickness. The degree of cracking of the resulting composite material was evaluated, with A being when there were no cracks overall, B being when there were localized cracks, and C being when there were cracks overall. The evaluation was otherwise carried out in the same manner as in Example 1. The results are shown in Table 1.
[0220]
[0221] (Example 3) (1) Preparation of aerogel particles A 100.0 parts by mass of PL-2L (manufactured by Fuso Chemical Co., Ltd., product name) as a silica particle-containing raw material, 80.0 parts by mass of water, 0.5 parts by mass of acetic acid as an acid catalyst, 1.0 parts by mass of cetyltrimethylammonium bromide (manufactured by Wako Pure Chemical Industries, Ltd.) as a cationic surfactant, and 150.0 parts by mass of urea as a thermal hydrolysis product were mixed, to which 60.0 parts by mass of methyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-13) as a silicon compound, 20.0 parts by mass of dimethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KMB-22), and 20.0 parts by mass of a bifunctional alkoxy-modified polysiloxane compound (hereinafter referred to as "polysiloxane compound A") were added, and the mixture was allowed to react for 2 hours at 25 ° C. to obtain a sol. The obtained sol was gelled at 60 ° C. and then aged for 48 hours at 60 ° C. to obtain a wet gel. The "polysiloxane compound A" was synthesized as follows. First, in a 1-liter three-neck flask equipped with a stirrer, a thermometer, and a Dimroth condenser, 100.0 parts by mass of dimethylpolysiloxane XC96-723 (manufactured by Momentive Performance Materials Japan LLC, product name) having silanol groups at both ends, 181.3 parts by mass of methyltrimethoxysilane, and 0.50 parts by mass of t-butylamine were mixed and reacted at 30 ° C. for 5 hours. Thereafter, this reaction solution was heated at 140 ° C. for 2 hours under a reduced pressure of 1.3 kPa, and the volatiles were removed to obtain a polysiloxane compound modified with bifunctional alkoxy at both ends (polysiloxane compound A). Thereafter, the obtained wet gel was transferred to a plastic bottle, sealed, and then pulverized at 27,000 rpm for 10 minutes using an extreme mill (manufactured by AS ONE Corporation, MX-1000XTS) to obtain a particulate wet gel. The obtained particulate wet gel was immersed in 2500.0 parts by mass of methanol and washed at 25°C for 24 hours. This washing operation was repeated three times while replacing with fresh methanol. Next, the washed particulate wet gel was immersed in 2500.0 parts by mass of heptane, a low surface tension solvent, and solvent substitution was carried out at 25°C for 24 hours. This solvent substitution operation was repeated three times while replacing with fresh heptane.The washed and solvent-substituted particulate wet gel was dried at 40° C. under normal pressure for 96 hours, and then further dried at 150° C. for 2 hours. Finally, the wet gel was passed through a sieve (manufactured by Tokyo Screen Co., Ltd., mesh size 45 μm, wire diameter 32 μm) to obtain aerogel particles A.
[0222] (2) Preparation of Coating Liquid A coating liquid was prepared in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, and the results are shown in Table 2.
[0223] Example 4 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracks were evaluated in the same manner as in Example 2. The results are shown in Table 2.
[0224] Comparative Example 3 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracks were evaluated in the same manner as in Comparative Example 1. The results are shown in Table 2.
[0225] Comparative Example 4 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracking was evaluated in the same manner as in Comparative Example 2. The results are shown in Table 2.
[0226]
Claims
1. A method for producing a composite material, comprising: a coating film forming step of discharging a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium toward an object to obtain a coating film; and a removal step of removing at least a portion of the liquid medium from the coating film to obtain a composite material.
2. The manufacturing method according to claim 1, wherein the coating film forming step is a step of discharging the coating liquid toward the object by a discharging device selected from the group consisting of a sprayer and a dispenser.
3. The manufacturing method according to claim 2, wherein the discharge device has a discharge port for discharging the coating liquid, and the inner diameter of the discharge port is 1.5 mm or more.
4. The manufacturing method according to claim 1, wherein the coating liquid further contains a water-soluble polymer having a hydrophobic group.
5. The method according to claim 4, wherein the hydrophobic group is an alkyl group having 6 to 26 carbon atoms.
6. The manufacturing method according to claim 1, wherein the coating liquid contains emulsified particles containing the binder resin.
7. The method according to claim 6, wherein the emulsion particles further contain a nonionic emulsifier.
8. The method of claim 1, wherein at least a portion of the aerogel particles form agglomerates.
9. The manufacturing method according to claim 1, further comprising: an emulsion preparation step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium; a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing the aerogel particles, the glass fibers, and the second liquid medium; and a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid.
10. The manufacturing method according to claim 9, wherein the dispersion liquid preparation step is a step of mixing the aerogel particles, the glass fibers, and the second liquid medium to aggregate at least a portion of the aerogel particles, and the coating liquid contains the aggregates of the aerogel particles.
Citation Information
Patent Citations
aerogel
JP2012091943A
Method for producing alkylsiloxane aerogel, and method for producing alkylsiloxane aerogel, apparatus for producing the same, and method for producing a panel containing the same.
JP5250900B2
Heat insulating material and method for producing the same
JP2014035044A
Aqueous dispersion of hydrophobic silica aerogel particles, solid composite material, heat insulating material and sound absorbing material
JP2018043927A
Coating liquid, production method for coating film, and coating film
WO2019069492A1