Epoxy resin composition particle, tablet, and method for producing columnar tablet

Incorporating fibrous or acicular fillers into epoxy resin compositions enhances the mechanical properties and fracture toughness, addressing the limitations of conventional compositions by preventing gap formation in skewed structures, particularly in magnet fixation and sealing applications.

WO2024225223A1PCT designated stage expired Publication Date: 2024-10-31SUMITOMO BAKELITE CO LTD

Patent Information

Application Number
PCT/JP2024/015723
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-22
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional epoxy resin compositions used for molding semiconductor elements and sealing applications have limitations in flexural modulus and exhibit gaps when filling skewed structures due to inadequate fracture toughness, particularly in rotor cores with magnet fixing materials.

Method used

Incorporating fibrous or acicular fillers with specific properties, such as wollastonite fibers, into the epoxy resin composition, and optimizing kneading conditions to achieve a fracture toughness value of 3.0 MPa·m^(1/2) or higher, which enhances the mechanical properties and prevents gap formation during the filling of skewed structures.

Benefits of technology

The modified epoxy resin composition particles demonstrate improved flexural modulus and fracture toughness, effectively preventing gap formation when filling skewed structures, making them suitable for magnet fixation, electronic control unit sealing, and stator core sealing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

This epoxy resin composition particle is used for fixing a magnet, sealing an electronic control unit, sealing a coil, or sealing a stator core, and contains an epoxy resin and a fibrous or needle-like filler.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing epoxy resin composition particles, tablets, and columnar tablets

[0001] The present invention relates to a method for producing epoxy resin composition particles, tablets, and pillar-shaped tablets.

[0002] Various methods for molding tablet-shaped epoxy resin compositions have been developed. One such technique is known from Patent Document 1. Patent Document 1 describes a transfer molding method for encapsulating semiconductor elements using a tablet-shaped epoxy resin composition containing an inorganic filler such as quartz glass powder, talc, silica powder, alumina powder, or calcium carbonate (see, for example, claim 1 and paragraphs 0005 and 0030 of Patent Document 1).

[0003] Japanese Patent Application Publication No. 9-208805

[0004] However, as a result of investigations by the present inventors, it was found that there is room for improvement in the flexural modulus of the tablet-form epoxy resin composition described in Patent Document 1. Furthermore, in a molded article having a skew structure using a conventional epoxy resin composition, a phenomenon was confirmed in which gaps were generated at the discontinuous surfaces of the molded article (misaligned portions of the molded article).

[0005] As a result of further investigation, the present inventors found that epoxy resin composition particles containing an epoxy resin and a fibrous or needle-like filler can improve the mechanical properties such as the flexural modulus of a molded article, thereby realizing a molding material that is suitable for any of magnet fixing, electronic control unit sealing, coil sealing, and stator core sealing, and thus completed the first invention.

[0006] The present inventors also focused on molded articles having a skewed structure using conventional epoxy resin compositions. It is believed that when a magnet fixing material is filled into a rotor core having a skewed structure, fracture occurs in the magnet fixing material, originating from the corners of the magnets, which hinder the flow of the material, resulting in the formation of gaps. Further investigation led the present inventors to discover that the degree of gap formation when a skewed structure is filled can be reliably evaluated by using the fracture toughness value of the magnet fixing material as an index. Based on this knowledge, further research led to the discovery that by using a fibrous or needle-like filler and adopting a moderately high mixing temperature, the fracture toughness value of the epoxy resin composition particles can be increased to a predetermined level or higher, thereby suppressing the formation of gaps when the skewed structure is filled. This led to the completion of the second invention.

[0007] According to the present invention, the following epoxy resin composition particles and related techniques are provided.

[0008] [1] Epoxy resin composition particles used for fixing a magnet, sealing an electronic control unit, sealing a coil, or sealing a stator core, the epoxy resin composition particles comprising: an epoxy resin; and a fibrous or needle-like filler. [2] Epoxy resin composition particles used for fixing a magnet, the epoxy resin composition particles comprising: an epoxy resin; and a fibrous or needle-like filler, the epoxy resin composition particles having a fracture toughness (K1c) of 3.0 MPa m as measured by the following procedure i. 1/2Epoxy resin composition particles having the above structure. (Step i) Using a transfer molding machine, a molded article is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the obtained molded article is cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm. A notch 3.5 mm deep in the thickness direction is formed in the center of the length direction, and the article is cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch 0.1 mm deep in the thickness direction is made with a razor at the tip of the notch in the cured product to prepare a test piece having a total crack length a = 3.6 mm. Thereafter, a three-point bending test is performed on the obtained test piece using a tension-compression testing machine at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S = 40 mm, and the fracture toughness value (K1c (MPa m 1/2 )) is calculated. Q is the maximum load (N). C = ((P Q × S) / (B × W 3/2 ) × f(a / W) where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2) [3] The epoxy resin composition particles according to [1] or [2], wherein the number average fiber length of the fibrous or acicular filler, measured by the following procedure A, is 5 μm or more and 500 μm or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and then the insoluble matter is dispersed on a glass plate. The filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The number average fiber length is the average value of the fiber lengths of the 100 longest fiber pieces of the filler. [4] The epoxy resin composition particles according to any one of [1] to [3], wherein the number average fiber length of the fibrous or acicular filler, measured by the following procedure A, is L, and the number average fiber diameter of the fibrous or acicular filler, measured by the following procedure B, is D, and the ratio L / D is 3 or more and 100 or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and the insoluble portion is dispersed on a glass plate. The filler in the insoluble portion is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The fiber lengths are measured in descending order of fiber length, and the average value of 100 fillers is defined as the number-average fiber length. (Procedure B) A scanning electron microscope is used to measure 100 cross sections of fibrous fillers from the cross section of the epoxy resin composition particles, and the average of the smallest diameters of each fiber cross section is determined as the number-average fiber diameter. [5] The epoxy resin composition particles according to any one of [1] to [4], wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fiber, glass fiber, metal fiber, carbon fiber, fibrous aluminum oxide, aramid fiber, silicon carbide whisker, silicon nitride whisker, and potassium titanate whisker. [6] The epoxy resin composition particles according to any one of [1] to [5], wherein the spiral flow measured according to the following procedure ii is 30 cm or more.(Step ii) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured. [7] The epoxy resin composition particles according to any one of [1] to [6], wherein the content of the fibrous or acicular filler is 5% by mass or more and 80% by mass or less, based on 100% by mass of the epoxy resin composition particles. [8] The epoxy resin composition particles according to any one of [1] to [7], wherein the epoxy resin comprises a cresol novolac epoxy resin and / or a bisphenol A epoxy resin. [9] The epoxy resin composition particles according to any one of [1] to [8], wherein the epoxy resin comprises one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts.

[10] The epoxy resin composition particles according to any one of [1] to [9], which are used to be molded into tablets through a process of feeding the epoxy resin composition particles into a heated extruder and kneading them while melting to obtain an epoxy resin molding material, and a process of continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder while cutting the epoxy resin molding material to obtain tablets.

[11] The epoxy resin composition particles according to any one of [1] to

[10] , which are injection molding epoxy resin composition particles that are introduced into a cylinder in injection molding using an injection molding machine comprising an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold connected to the injection unit and having a cavity.

[12] The epoxy resin composition particles according to any one of [1] to

[11] , which contain an epoxy resin or a curing agent having a softening point of less than 110°C.

[13] A tablet formed using the epoxy resin composition particles according to any one of [1] to

[12] , which has a diameter of 5 cm. 3 More than 1500cm 3

[14] A method for producing an epoxy resin composition comprising the steps of: preparing epoxy resin composition particles according to any one of [1] to

[12] ; supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and cutting the molten epoxy resin molding material while continuously extruding it from an opening at the tip of the extruder to obtain pillar-shaped tablets, wherein the cross-sectional area of ​​the pillar-shaped tablets is 3 cm or less. 2 More than 100cm 2 A method for producing a pillar-shaped tablet, which is as follows.

[15] A structure using the epoxy resin composition particles according to any one of [1] to

[12] .

[16] A method for producing the structure according to

[15] , comprising the steps of: using an injection molding apparatus comprising an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold connected to the injection unit and having a cavity, melting the epoxy resin composition particles in the cylinder to form a molten resin composition; and injecting the molten resin composition from the tip of the screw to fill the cavity.

[17] A method for producing the structure according to

[16] , wherein in the filling step, the temperature T of the tip of the screw is 60 to 100°C.

[18] A method for producing the structure according to

[16] or

[17] , wherein in the filling step, the temperature inside the cavity is 150 to 180°C.

[0009] According to the present invention, there are provided epoxy resin composition particles that can be used to form a molded article having an excellent flexural modulus, or epoxy resin composition particles that are excellent in suppressing gaps when filled in a skew structure.

[0010] It is a longitudinal sectional view of an extruder in an example of this embodiment. It is a sectional schematic view showing an example of an injection molding apparatus according to this embodiment. It is a sectional view explaining an outline of a tension and compression testing machine.

[0011] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In all drawings, similar components are designated by similar reference numerals, and descriptions thereof will be omitted where appropriate. Furthermore, the drawings are schematic diagrams and do not correspond to actual dimensional proportions.

[0012] First Embodiment The epoxy resin composition particles of this embodiment are particulate epoxy resin compositions containing an epoxy resin and a fibrous or needle-like filler.

[0013] Such epoxy resin composition particles are used for magnet fixation, electronic control unit (ECU) sealing, coil sealing, or stator core sealing. Specifically, a tablet-shaped molding material is produced from the epoxy resin composition particles, and the obtained tablet-shaped molding material can be used for magnet fixation, electronic control unit (ECU) sealing, coil sealing, or stator core sealing by a known molding method. The epoxy resin composition particles of this embodiment can improve the mechanical properties, such as the flexural modulus, of the resulting molded article. That is, the entanglement of the fibrous or needle-like filler particles with each other facilitates improving the toughness of the molded article, thereby making it easier to obtain elasticity that is more suitable for magnet fixation, electronic control unit (ECU) sealing, coil sealing, or stator core sealing.

[0014] Second Embodiment The epoxy resin composition particles of this embodiment contain an epoxy resin and a fibrous or needle-like filler, and have a fracture toughness value (K1c) of 3.0 MPa m as measured by the following procedure i. 1/2 It satisfies the above.

[0015] By setting the fracture toughness value (K1c) of the epoxy resin composition particles to the above-mentioned lower limit or more, it is possible to suppress the occurrence of gaps when a magnet fixing material using the epoxy resin composition particles is filled in a rotor core having a skew structure. Although the details of the reason for this are not clear, it is thought that the fracture toughness value can highly control the degree of crack progression. Therefore, even if cracks occur when epoxy resin composition particles are filled in a rotor core having a skew structure, it is thought that the occurrence of gaps can be suppressed because the fracture toughness value can appropriately control the progression of the cracks.

[0016] The upper limit of the fracture toughness value (K1c) is not particularly limited, but is, for example, 10.0 MPa m 1/2 The following may also be used.

[0017] (Procedure i for measuring fracture toughness) Using a transfer molding machine, a molded article is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the Klc method specified in ASTM D5045-14, the obtained molded article is cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm. A notch 3.5 mm deep in the thickness direction is formed in the center of the length direction, and the article is cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch 0.1 mm deep in the thickness direction is made with a razor at the tip of the notch in the cured product to prepare a test specimen having a total crack length a = 3.6 mm. Thereafter, a three-point bending test is performed on the obtained test specimen using a tension-compression testing machine at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S = 40 mm, and the fracture toughness value (Klc (MPa m 1/2 )) is calculated. Q is the maximum load (N). C = ((P Q × S) / (B × W 3/2 ) × f(a / W) where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2 )

[0018] In this embodiment, the fracture toughness value can be controlled by, for example, appropriately selecting the type and amount of each component contained in the epoxy resin composition particles, the method for preparing the epoxy resin composition particles, etc. Among these, for example, improving the kneadability of the materials and increasing the fiber length of the fibrous filler can be cited as factors for setting the fracture toughness value within a desired numerical range.

[0019] Hereinafter, the common configuration, action, etc. of the epoxy resin composition particles of the first and second embodiments will be described.

[0020] [Mold of Epoxy Resin Composition Particles] The epoxy resin composition particles of the present embodiment can be suitably used for producing a tablet-shaped, preferably columnar tablet-shaped, epoxy resin molding material. The epoxy resin composition particles enable stable production of tablet-shaped epoxy resin molding materials.

[0021] A method for producing a tablet-shaped epoxy resin molding material may include, for example, an extrusion molding method including a step of supplying epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material, and a step of continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder while cutting the epoxy resin molding material to obtain tablets.

[0022] As a specific example, an extruder shown in FIG. 1 can be used to produce the tablet-shaped epoxy resin molding material. FIG. 1 shows a longitudinal cross-sectional view of one example of the extruder configuration. The extruder includes a hopper 2 into which epoxy resin composition particles 1 are introduced, a heater 41 for heating the epoxy resin composition particles 1 via a cylinder 43, a screw 42, and a temperature-controlled die 5 attached to the tip of the extruder, having an opening with the same shape as the desired tablet cross section. A temperature regulator 51 for controlling the temperature of the die 5 may also be connected to the extruder. The extruder extrudes the epoxy resin composition particles 1 into the cylinder 43 and the input cylinder 43a, and kneads the epoxy resin molding material obtained by melting the epoxy resin composition particles 1 with heat using the screw 42 while extruding. The extruder then continuously extrudes the melt-kneaded epoxy resin molding material from the opening of the die 5. The extruder produces an extruded material 6. The extruded material 6 is cut to a desired tablet length using a cutter (not shown) or the like to obtain a tablet-shaped epoxy resin molding material (tablet).

[0023] The particles of the epoxy resin composition particles 1 include powder and / or granules. For example, relatively fine particles (powder) can be obtained by pulverizing and / or classifying relatively coarse particles (granules). The particle shape of the epoxy resin composition particles 1 is not particularly limited, and may be spherical, polygonal, irregular, or the like. These may be used alone or in combination of two or more.

[0024] In this embodiment, the opening shape of the die 5 attached to the tip of the extruder is the same as the cross-sectional shape of the tablet-shaped epoxy resin molding material (tablet). Furthermore, when the opening shape is circular, the dimensions of the opening shape are, for example, 20 mm to 200 mm in diameter, and preferably 40 mm to 120 mm. The opening shape, including its dimensions, is appropriately selected according to the desired tablet shape. Furthermore, the extruded material 6 extruded from the extruder is cut to the desired length with a cutter. This length is, for example, 10 mm to 300 mm, and preferably 20 mm to 200 mm.

[0025] The volume of the tablet (tablet-shaped epoxy resin molding material) is, for example, 5 cm 3 More than 1500cm 3 Less than 10 cm, preferably 3 More than 1000cm 3 The cross-sectional area of ​​the pillar-shaped tablet is, for example, 3 cm 2 More than 100cm 2 Less than 10 cm, preferably 2 Over 95cm 2 The following is the result.

[0026] By using the epoxy resin composition particles of this embodiment, tablet-shaped epoxy resin molding materials can be continuously obtained, and therefore, tall tablet-shaped epoxy resin molding materials can be efficiently produced.

[0027] The method for producing tablets using the epoxy resin composition particles of this embodiment is not limited to the above-mentioned extrusion molding method, but may also be a compression molding method, a transfer molding method, an injection molding method, or the like.

[0028] [Physical Properties of Epoxy Resin Composition Particles] The lower limit of the spiral flow of the epoxy resin composition particles is, for example, 30 cm or more, preferably 50 cm or more. On the other hand, the upper limit of the spiral flow of the epoxy resin composition particles is, for example, 250 cm or less, preferably 200 cm or less. The spiral flow can be measured according to the following procedure ii. (Procedure ii) Using a low-pressure transfer molding machine, epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured.

[0029] [Uses and Methods of Use] Various structures can be manufactured using known molding methods such as transfer molding and injection molding using tablet-shaped epoxy resin molding materials. In particular, the epoxy resin composition particles of this embodiment are preferably used for injection molding. Specifically, the epoxy resin composition particles are preferably used for injection molding using an injection molding machine equipped with an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold connected to the injection unit and having a cavity, in which the epoxy resin composition particles are introduced into the cylinder. For example, when manufacturing a magnet fixing structure using the epoxy resin composition particles of this embodiment, the epoxy resin composition particles may be introduced into an injection molding machine and melted in the cylinder, and the molten resin may be directly filled between the hole in the mold and the permanent magnet.

[0030] [Structure] The structure of this embodiment is formed using the above-mentioned epoxy resin composition particles. Specific examples include a fixing structure or a sealing structure selected from the group consisting of a magnet fixing structure, an electronic control unit sealing structure, a coil sealing structure, and a stator core sealing structure.

[0031] Regarding the above-mentioned fixed structure or sealing structure, for example, International Publication No. 2012 / 029278 etc. can be used as a rotor core to which a magnet is fixed, International Publication No. 2016 / 139985 etc. can be used as a reference for an in-vehicle electronic control unit, and Japanese Patent Application Laid-Open No. 2020-094092 etc. can be used as a reference for a stator core.

[0032] The following describes a case where an epoxy resin molding material is used for the magnet fixing structure. The rotor core has a plurality of holes and a permanent magnet inserted into each of the holes. The permanent magnet can be fixed to the rotor core by filling the gaps between the holes and the permanent magnets with epoxy resin molding material.

[0033] The use of an epoxy resin molding material in a sealing structure for an automotive electronic control unit will be described. The automotive electronic control unit includes a substrate on which electronic components and the like are mounted. In the automotive electronic control unit, at least a portion of the substrate together with the electronic components can be encapsulated with the epoxy resin molding material.

[0034] This section explains the use of epoxy resin molding material in a coil sealing structure. Coils have windings such as copper wire and are used in motors and transformers. These coils are molded (sealed) with epoxy resin molding material to provide insulation.

[0035] A case where an epoxy resin molding material is used in a stator core sealing structure will be described. The stator core includes multiple teeth and coils (windings) wound around each of the multiple teeth. The coils wound around the teeth are sealed with epoxy resin molding material, thereby insulating the coils from the stator core. Furthermore, if the teeth formed in the stator core have housings, the coils wound around the teeth can be housed in the housings and the spaces between them can be filled with epoxy resin molding material, thereby insulating the coils from the stator core. As a manufacturing example, an insulating layer is formed on the surface of the stator core using epoxy resin molding material. Then, a coil is inserted into the teeth and sealed with epoxy resin molding material. The windings used in the coils and stator core may be round or rectangular wire.

[0036] The step of manufacturing the fixed structure or the sealing structure may be carried out, for example, using a tablet-shaped epoxy resin molding material at a temperature of 120°C or higher and 200°C or lower and a pressure of 3 MPa or higher and 15 MPa or lower, preferably at a temperature of 140°C to 180°C and a pressure of 5 to 12 MPa.

[0037] [Method for Manufacturing a Structure] An example of a method for manufacturing a structure will be described in detail below. The following description will be made with reference to FIG. 2. FIG. 2 shows an injection molding apparatus 1 equipped with an injection unit 20 consisting of a cylinder 21 and a screw 22 inserted into the cylinder 21, and a mold 10 having a cavity 12. The injection molding apparatus 1 includes the mold 10 having a molding space (cavity 12) including a gate, a runner, and a gate, and an injection molding machine 20 for performing injection molding. The injection molding machine 20 includes, for example, the cylinder 21, a screw 22 rotatable within the cylinder 21, a hopper 23 into which epoxy resin composition particles can be introduced into the cylinder 21, a heater 24 for melting and heating the epoxy resin composition particles via the cylinder 21, and a nozzle 25 for delivering the epoxy resin composition particles melted and kneaded in the cylinder 21 to the mold 10. Although FIG. 2 shows the screw 22 equipped with a check valve 26 at its tip, the screw 22 is not limited to this. The screw 22 may not be provided with a backflow valve 26 .

[0038] The method for producing a structure includes the steps of melting epoxy resin composition particles in a cylinder 21 to form a molten resin composition, and injecting the molten resin composition from the tip of a screw 22 to fill the cavity 12. Specifically, epoxy resin composition particles are first introduced into a heated injection molding machine 20. The epoxy resin composition particles are then heated and melted in the cylinder 21 by a heater 24 while being kneaded by the screw 22. The temperature at the tip of the screw 22 in the cylinder 21 is preferably 60 to 100°C in order to ensure satisfactory heating and melting of the epoxy resin composition particles. Next, the molten resin composition melted by the screw 22 is sent toward the nozzle 25 while being compressed and kneaded, while the screw 22 moves backward (in the opposite direction from the nozzle 25). At this time, back pressure is applied to the screw 22 from the rear, so that the molten resin composition collected at the nozzle 25 can be pressurized. The molten resin composition collected at the nozzle 25 at the tip of the screw 22 is then metered to a set position. The measured molten resin composition is then injected into the cavity 12 of the mold 10 through the nozzle 25 by the pressure of the screw 22 as the screw 22 moves forward. The temperature inside the cavity 12 when the molten resin composition is filled is preferably 150 to 180°C in order to ensure that the molten resin composition is filled appropriately. Next, the molten resin composition is cured in the cavity 12, and then the mold 10 is opened and the structure is removed from the cavity 12.

[0039] For example, when manufacturing a magnet fixing structure using the epoxy resin composition particles of this embodiment, the epoxy resin composition particles may be introduced into an injection molding machine and melted in the cylinder 21, and the molten resin may be directly filled between the hole in the mold 10 and the permanent magnet.

[0040] Each component of the epoxy resin composition particles of this embodiment will be described in detail below.

[0041] [Epoxy Resin] The epoxy resin composition particles contain an epoxy resin. Examples of the epoxy resin include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, and resol-type phenolic resin, novolac-type epoxy resins such as phenol novolac-type epoxy resin and cresol novolac-type epoxy resin, bisphenol A-type epoxy resin and bisphenol F-type epoxy resin, aromatic glycidylamine-type epoxy resins such as N,N-diglycidylaniline, N,N-diglycidyltoluidine, diaminodiphenylmethane-type glycidylamine, and aminophenol-type glycidylamine, hydroquinone-type epoxy resin, biphenyl-type epoxy resin, and stilbene. Examples of epoxy resins include aralkyl-type epoxy resins such as aryl aryl epoxy resins, triphenolmethane-type epoxy resins, triphenolpropane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthol-type epoxy resins, naphthalene-type epoxy resins, phenol aralkyl-type epoxy resins having a phenylene and / or biphenylene skeleton, and naphthol aralkyl-type epoxy resins having a phenylene and / or biphenylene skeleton; and aliphatic epoxy resins such as vinylcyclohexene dioxide, dicyclopentadiene oxide, and alicyclic diepoxy adipide. These may be used alone or in combination of two or more. Among these, the epoxy resin preferably includes a cresol novolac-type epoxy resin and / or a bisphenol A-type epoxy resin.

[0042] The epoxy resin preferably has a softening point of less than 80° C. The softening point is measured by the ball and ring method.

[0043] The content of the epoxy resin is preferably 5% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 20% by mass or less, based on the total amount of the epoxy resin composition particles.

[0044] [Curing Agent] The epoxy resin composition particles may contain a curing agent that cures the epoxy resin. A preferred curing agent is, for example, a phenolic resin-based curing agent. Examples of phenolic resin-based curing agents include novolac-type resins such as phenol novolac resin, cresol novolac resin, and naphthol novolac resin; multifunctional phenolic resins such as triphenolmethane-type phenolic resin; modified phenolic resins such as terpene-modified phenolic resin and dicyclopentadiene-modified phenolic resin; aralkyl-type resins such as phenol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton and naphthol aralkyl resins having a phenylene and / or biphenylene skeleton; and bisphenol compounds such as bisphenol A and bisphenol F. These may be used alone or in combination of two or more. Such phenolic resin-based curing agents provide a good balance of flame resistance, moisture resistance, electrical properties, curability, storage stability, and the like.

[0045] Further, examples of curing agents that can be used in combination include polyaddition type curing agents and condensation type curing agents.

[0046] Examples of polyaddition curing agents include aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylenediamine (MXDA), aromatic polyamines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS), as well as polyamine compounds including dicyandiamide (DICY) and organic acid dihydrazides; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polyphenol compounds such as novolac phenolic resins and phenol polymers; polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins.

[0047] Examples of condensation type curing agents include resol resins, urea resins such as methylol group-containing urea resins, and melamine resins such as methylol group-containing melamine resins.

[0048] The curing agent preferably has a softening point of less than 110° C., more preferably less than 105° C. The softening point is measured by the ball and ring method.

[0049] The phenolic resin as a curing agent and the epoxy resin are preferably blended so that the equivalent ratio (EP) / (OH) of the number of epoxy groups (EP) in the epoxy resin composition particles to the number of phenolic hydroxyl groups (OH) in the total phenolic resin is 0.8 or more and 1.3 or less. When the equivalent ratio is within the above range, sufficient curing properties can be obtained when the resulting epoxy resin composition particles are molded. However, when a resin other than the phenolic resin that can react with the epoxy resin is used in combination, the equivalent ratio can be adjusted appropriately.

[0050] [Inorganic Filler] (Fibrous or Acicular Filler) The epoxy resin composition particles contain a fibrous or acicular filler as the inorganic filler.

[0051] The lower limit of the number average fiber length of the fibrous or acicular filler is, for example, 5 μm or more, preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. This can improve the strength of the material. On the other hand, the upper limit of the number average fiber length of the fibrous or acicular filler is, for example, 500 μm or less, preferably 450 μm or less, and more preferably 400 μm or less. This can improve the moldability of the material.

[0052] When the number average fiber length of the fibrous or acicular filler is L and the number average fiber diameter of the fibrous or acicular filler is D, the aspect ratio is defined as L / D. The lower limit of L / D of the fibrous or acicular filler is, for example, 3 or more, preferably 10 or more, and more preferably 15 or more. This can further improve the flexural modulus. Furthermore, toughness can be improved. On the other hand, the upper limit of L / D of the fibrous or acicular filler is, for example, 100 or less, preferably 70 or less, and more preferably 50 or less. This can improve the moldability of the material.

[0053] (Procedure A for Measuring Number Average Fiber Length) After dissolving epoxy resin composition particles in acetone to remove the resin component, the insoluble matter is dispersed on a glass plate, the filler particles in the insoluble matter are photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average fiber length of the 100 longest filler particles is taken as the number average fiber length.

[0054] (Procedure B for Measuring Number Average Fiber Diameter) Using a scanning electron microscope, 100 cross sections of the fibrous filler are measured from the cross section of an epoxy resin composition particle, and the average of the smallest diameters of each fiber cross section is determined as the number average fiber diameter.

[0055] The fibrous or acicular filler may contain, for example, one or more selected from the group consisting of wollastonite fiber, glass fiber, metal fiber, carbon fiber, fibrous aluminum oxide, aramid fiber, silicon carbide whisker, silicon nitride whisker, and potassium titanate whisker. Among these, it is preferable to contain at least one of wollastonite fiber and glass fiber, and it is more preferable to contain wollastonite fiber.

[0056] The lower limit of the content of the fibrous or needle-like filler is, for example, 5% by mass or more, preferably 10% by mass or more, and more preferably 30% by mass or more, based on 100% by mass of the epoxy resin composition particles. This allows for a further improvement in the flexural modulus. Furthermore, toughness can also be improved. On the other hand, the upper limit of the content of the fibrous or needle-like filler is not particularly limited, but may be 80% by mass or less, preferably 75% by mass or less, based on 100% by mass of the epoxy resin composition particles.

[0057] The lower limit of the content of the fibrous or needle-like filler in all inorganic fillers is, for example, 30% by mass or more, preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 72% by mass or more. This can further improve the flexural modulus. Furthermore, toughness can be improved. On the other hand, the upper limit of the content of the fibrous or needle-like filler in all inorganic fillers is not particularly limited, but may be 100% by mass or less.

[0058] (Other inorganic fillers other than fibrous or needle-like fillers) The epoxy resin composition particles may contain other inorganic fillers other than fibrous or needle-like fillers. The other inorganic fillers are not particularly limited as long as they have a shape such as spherical, polygonal, or irregular. Specifically, the other inorganic fillers preferably have an aspect ratio of 2 or less, and more preferably are spherical.

[0059] Examples of other inorganic fillers include silica, alumina, kaolin, talc, clay, mica, rock wool, glass powder, glass flakes, glass beads, silicon carbide, silicon nitride, aluminum nitride, carbon black, graphite, titanium dioxide, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, and barium sulfate. These may be used alone or in combination of two or more. Examples of silica that can be used include fused silica such as fused crushed silica and fused spherical silica, and crystalline silica.

[0060] Average particle size D of inorganic filler 50 is preferably 0.01 μm or more and 75 μm or less, more preferably 0.05 μm or more and 50 μm or less. By setting the average particle size of the inorganic filler within the above range, the filling property in the mold is improved. Furthermore, by setting the upper limit of the average particle size of the inorganic filler to 75 μm or less, the filling property is further improved. Average particle size D 50 is the volume-converted average particle diameter measured by a laser diffraction measuring device RODOS SR type (SYMPATEC HEROS & RODOS).

[0061] The content of the inorganic filler is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, and particularly preferably 75% by mass or more, based on the total amount of the epoxy resin composition particles, while the content of the inorganic filler is preferably 93% by mass or less, more preferably 91% by mass or less, and even more preferably 90% by mass or less, based on the total amount of the epoxy resin composition particles.

[0062] Furthermore, when an inorganic filler is used in combination with a metal hydroxide such as aluminum hydroxide or magnesium hydroxide, or an inorganic flame retardant such as zinc borate, zinc molybdate, or antimony trioxide, as described below, it is desirable that the total amount of these inorganic flame retardants and the inorganic filler be within the range of the content of the inorganic filler.

[0063] [Curing Catalyst] The epoxy resin composition particles may contain a curing catalyst, if necessary. As the curing catalyst, it is preferable to use one or more selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts.

[0064] As the imidazole catalyst, for example, imidazoles are preferably used. Examples of imidazoles include imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxyimidazole, 2-phenyl-4,5-dihydroxydimethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. The compound may include one or more compounds selected from imidazole compounds such as midazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2-phenylimidazole, and an isocyanuric acid adduct of 2-methylimidazole.

[0065] When the curing catalyst contains an imidazole catalyst, the lower limit of the content of the imidazole catalyst is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and particularly preferably 0.05 mass% or more, based on the total epoxy resin composition particles, and the upper limit of the content of the imidazole catalyst is preferably 2.0 mass% or less, more preferably 1.0 mass% or less, and particularly preferably 0.5 mass% or less, based on the total epoxy resin composition particles.

[0066] Examples of phosphorus-based catalysts include phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds.

[0067] Examples of organic phosphines that can be used in the epoxy resin composition particles include primary phosphines such as ethylphosphine and phenylphosphine; secondary phosphines such as dimethylphosphine and diphenylphosphine; and tertiary phosphines such as trimethylphosphine, triethylphosphine, tributylphosphine and triphenylphosphine.

[0068] Examples of the tetra-substituted phosphonium compound that can be used in the epoxy resin composition particles include compounds represented by the following general formula (4).

[0069] (In the above general formula (4), P represents a phosphorus atom. R 4 , R 5 , R 6 and R 7 represents an aromatic group or an alkyl group. A represents the anion of an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on the aromatic ring. AH represents an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on the aromatic ring. x and y are numbers from 1 to 3, z is a number from 0 to 3, and x = y.

[0070] The compound represented by general formula (4) can be obtained, for example, but not limited to, as follows. First, a tetra-substituted phosphonium halide, an aromatic organic acid, and a base are mixed uniformly in an organic solvent, and an aromatic organic acid anion is generated in the solution system. Next, water is added to precipitate the compound represented by general formula (4). In the compound represented by general formula (4), the R bonded to the phosphorus atom 4 , R 5 , R 6 and R 7is preferably a phenyl group, AH is a compound having a hydroxyl group on an aromatic ring, i.e., a phenol, and A is an anion of the phenol. Examples of the phenol include monocyclic phenols such as phenol, cresol, resorcinol, and catechol, condensed polycyclic phenols such as naphthol, dihydroxynaphthalene, and anthraquinol, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, and polycyclic phenols such as phenylphenol and biphenol.

[0071] Examples of the phosphobetaine compound used as the curing catalyst include compounds represented by the following general formula (5).

[0072] (In the above general formula (5), R 8 is an alkyl group having 1 to 3 carbon atoms, R 9 represents a hydroxyl group, f is a number from 0 to 5, and g is a number from 0 to 3.

[0073] The compound represented by general formula (5) can be obtained, for example, as follows: First, a triaromatic-substituted phosphine, which is a tertiary phosphine, is brought into contact with a diazonium salt to substitute the diazonium group of the diazonium salt with the triaromatic-substituted phosphine. However, the method is not limited to this.

[0074] Examples of the adduct of a phosphine compound and a quinone compound used as a curing catalyst include compounds represented by the following general formula (6).

[0075] (In the above general formula (6), P represents a phosphorus atom. R 10 , R 11 and R 12 represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and may be the same or different. 13 , R 14 and R 15 represent a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, and may be the same or different from each other; R 14 and R 15may be bonded to form a cyclic structure.)

[0076] The phosphine compound used in the adduct of a phosphine compound and a quinone compound is preferably, for example, triphenylphosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, trinaphthylphosphine, tris(benzyl)phosphine, etc., which is unsubstituted or has a substituent such as an alkyl group or alkoxy group on the aromatic ring, and the substituent such as the alkyl group or alkoxy group has a carbon number of 1 to 6. From the viewpoint of availability, triphenylphosphine is preferred.

[0077] The quinone compound used in the adduct of a phosphine compound and a quinone compound includes benzoquinone and anthraquinones, and among these, p-benzoquinone is preferred from the viewpoint of storage stability.

[0078] The adduct of a phosphine compound and a quinone compound can be produced by contacting and mixing the organic tertiary phosphine and the benzoquinone in a solvent that can dissolve both of them. The solvent is preferably a ketone such as acetone or methyl ethyl ketone, which has low solubility in the adduct, but is not limited thereto.

[0079] In the compound represented by general formula (6), R bonded to the phosphorus atom 10 , R 11 and R 12 is a phenyl group, and R 13 , R 14 and R 15 is a hydrogen atom, that is, a compound obtained by adding 1,4-benzoquinone and triphenylphosphine, is preferred in that it reduces the elastic modulus of the cured product of the epoxy resin composition particles when heated.

[0080] Examples of the adduct of a phosphonium compound and a silane compound used as a curing catalyst include compounds represented by the following general formula (7).

[0081] (In the above general formula (7), P represents a phosphorus atom, and Si represents a silicon atom. R 16 , R17 , R 18 and R 19 and each represent an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group, and may be the same or different. 20 is the group Y 2 and Y 3 is an organic group that bonds to 21 is the group Y 4 and Y 5 is an organic group that bonds to 2 and Y 3 represents a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 represents a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 , and R 21 may be the same or different, and Y 2 , Y 3 , Y 4 and Y 5 may be the same or different. 1 is an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group.

[0082] In general formula (7), R 16 , R 17 , R 18 and R 19 Examples of the alkyl group include a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, a naphthyl group, a hydroxynaphthyl group, a benzyl group, a methyl group, an ethyl group, an n-butyl group, an n-octyl group, and a cyclohexyl group. Among these, an aromatic group having a substituent such as an alkyl group, an alkoxy group, or a hydroxyl group, such as a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, or a hydroxynaphthyl group, or an unsubstituted aromatic group is more preferred.

[0083] In addition, in the general formula (7), R 20 Is Y 2 and Y 3 Similarly, R 21 is the group Y 4 and Y 5 is an organic group that bonds to 2 and Y 3 is a group formed by releasing a proton from a proton-donating group, and the group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 is a group formed by releasing a proton from a proton-donating group, and the group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 and R 21 may be the same or different, and the group Y 2 , Y 3 , Y 4 , and Y 5 may be the same or different. 2 -R 20 -Y 3 - and -Y 4 -R 21 -Y 5The group represented by - is constituted by a group formed by a proton donor releasing two protons, and as the proton donor, an organic acid having at least two carboxyl groups or hydroxyl groups in the molecule is preferred, and an aromatic compound having at least two carboxyl groups or hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferred, and an aromatic compound having at least two hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferred, and examples thereof include catechol, pyrogallol, 1,2-dihydro- Examples of the dihydroxynaphthalene include xynaphthalene, 2,3-dihydroxynaphthalene, 2,2'-biphenol, 1,1'-bi-2-naphthol, salicylic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, chloranilic acid, tannic acid, 2-hydroxybenzyl alcohol, 1,2-cyclohexanediol, 1,2-propanediol, and glycerin. Of these, catechol, 1,2-dihydroxynaphthalene, and 2,3-dihydroxynaphthalene are more preferred.

[0084] In addition, Z in the general formula (7) 1 represents an organic group or an aliphatic group having an aromatic ring or a heterocyclic ring, and specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, hexyl, and octyl groups; aromatic hydrocarbon groups such as phenyl, benzyl, naphthyl, and biphenyl groups; glycidyloxy groups such as glycidyloxypropyl, mercaptopropyl, and aminopropyl groups; mercapto groups; alkyl groups having amino groups; and reactive substituents such as vinyl groups. Among these, methyl, ethyl, phenyl, naphthyl, and biphenyl groups are more preferred in terms of thermal stability.

[0085] In a method for producing an adduct of a phosphonium compound and a silane compound, a silane compound such as phenyltrimethoxysilane and a proton donor such as 2,3-dihydroxynaphthalene are dissolved in a flask containing methanol, and then a sodium methoxide-methanol solution is added dropwise to the solution with stirring at room temperature. A previously prepared solution of a tetra-substituted phosphonium halide such as tetraphenylphosphonium bromide dissolved in methanol is then added dropwise to the solution with stirring at room temperature, resulting in the precipitation of crystals. The precipitated crystals are filtered, washed with water, and vacuum dried to obtain an adduct of a phosphonium compound and a silane compound. However, the method is not limited to this.

[0086] The content of the curing catalyst is preferably 0.05% by mass or more, more preferably 0.08% by mass or more, and particularly preferably 0.10% by mass or more, based on the total epoxy resin composition particles. By setting the content of the curing catalyst to the above-mentioned lower limit or more, it is possible to effectively improve the curability of the epoxy resin composition particles during transfer molding. On the other hand, the content of the curing catalyst is preferably 2.0% by mass or less, more preferably 1.0% by mass or less, and particularly preferably 0.5% by mass or less, based on the total epoxy resin composition particles. Setting the content of the curing catalyst to the above-mentioned upper limit or less can improve the fluidity during encapsulation, contributing to improved filling properties.

[0087] [Wax] The epoxy resin composition particles may contain wax as a release agent, if necessary. Examples of wax include natural waxes such as carnauba wax, synthetic waxes such as ester wax, Montan acid ester wax, and oxidized polyethylene wax, and higher fatty acids and metal salts thereof such as zinc stearate.

[0088] The amount of wax blended is, for example, 0.05% by mass or more and 2.0% by mass or less, based on the total amount of epoxy resin composition particles. The lower limit of the amount of wax blended is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, based on the total amount of epoxy resin composition particles. The upper limit of the amount of wax blended is preferably 1.5% by mass or less, more preferably 1.0% by mass or less, based on the total amount of epoxy resin composition particles. By blending the wax within the above range, the obtained epoxy resin composition particles have excellent fluidity and filling ability during transfer molding.

[0089] [Coupling Agent] The epoxy resin composition particles may contain a coupling agent such as a silane coupling agent, if necessary, such as epoxysilane, aminosilane, ureidosilane, or mercaptosilane.

[0090] Examples of epoxy silanes include γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Examples of aminosilanes include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenylγ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-benzenedimethanane. Examples of ureidosilanes include γ-ureidopropyltriethoxysilane and hexamethyldisilazane. Primary aminosilanes include Latent aminosilane coupling agents in which the amino moiety is protected by reaction with a ketone or aldehyde may also be used. Furthermore, the aminosilane may have a secondary amino group. Examples of mercaptosilanes include γ-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and silane coupling agents that exhibit the same function as mercaptosilane coupling agents upon thermal decomposition, such as bis(3-triethoxysilylpropyl)tetrasulfide and bis(3-triethoxysilylpropyl)disulfide. These silane coupling agents may also be blended after being subjected to a hydrolysis reaction in advance. These silane coupling agents may be used alone or in combination of two or more.

[0091] From the viewpoint of continuous moldability, mercaptosilane is preferred, from the viewpoint of flowability, aminosilane is preferred, and from the viewpoint of adhesion, epoxysilane is preferred.

[0092] The lower limit of the content of the coupling agent, such as a silane coupling agent, that can be used in the epoxy resin composition particles is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and particularly preferably 0.1 mass% or more, based on the total epoxy resin composition particles. When the lower limit of the content of the coupling agent, such as a silane coupling agent, is within the above range, the interfacial strength between the epoxy resin and the inorganic filler is not reduced, and good vibration resistance can be obtained. Furthermore, the upper limit of the content of the coupling agent, such as a silane coupling agent, is preferably 1 mass% or less, more preferably 0.8 mass% or less, and particularly preferably 0.6 mass% or less, based on the total epoxy resin composition particles. When the upper limit of the content of the coupling agent, such as a silane coupling agent, is within the above range, the interfacial strength between the epoxy resin and the inorganic filler is not reduced, and good vibration resistance can be obtained. Furthermore, when the content of the coupling agent, such as a silane coupling agent, is within the above range, an increase in the water absorption of the cured product of the epoxy resin composition particles is prevented.

[0093] [Other Additives] In addition to the above components, the epoxy resin composition particles of the present embodiment may further contain, as necessary, other additives such as a colorant, a flame retardant, a stress reducing agent, etc. These may be used alone or in combination of two or more.

[0094] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0095] A first embodiment of the present invention will be described below. 1. Epoxy resin composition particles used for fixing a magnet, comprising an epoxy resin and a fibrous or needle-like filler, and having a fracture toughness (K1c) of 3.0 MPa m as measured by the following procedure. 1/2Epoxy resin composition particles having the above structure. (Procedure) Using a transfer molding machine, a molded article is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the obtained molded article is cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm. A notch 3.5 mm deep in the thickness direction is formed in the center of the length direction, and the article is cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch 0.1 mm deep in the thickness direction is made with a razor at the tip of the notch in the cured article to prepare a test piece having a total crack length a = 3.6 mm. Thereafter, a three-point bending test is performed on the obtained test piece using a tension-compression testing machine at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S = 40 mm, and the fracture toughness value (K1c (MPa m)) is calculated based on the following formula: 1/2 )) is calculated. Q is the maximum load (N). C = ((P Q × S) / (B × W 3/2 ) × f(a / W) where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2) 2. Epoxy resin composition particles according to 1., wherein the number average fiber length of the fibrous or acicular filler, measured by the following procedure A, is 5 μm or more and 500 μm or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and then the insoluble matter is dispersed on a glass plate. The filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average fiber length of the 100 longest fiber pieces is defined as the number average fiber length. 3. Epoxy resin composition particles according to 1. or 2., wherein, when the number average fiber length of the fibrous or acicular filler, measured by the following procedure A, is L, and the number average fiber diameter of the fibrous or acicular filler, measured by the following procedure B, is D, L / D is 3 or more and 100 or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and then the insoluble matter is dispersed on a glass plate. The filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The fiber lengths are measured in descending order of length, and the average value of 100 fillers is taken as the number average fiber length. (Procedure B) A scanning electron microscope is used to measure 100 cross sections of fibrous fillers from the cross section of the epoxy resin composition particles, and the average of the smallest diameters of each fiber cross section is determined as the number average fiber diameter. 4. Epoxy resin composition particles according to any one of 1. to 3., wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fiber, glass fiber, metal fiber, carbon fiber, fibrous aluminum oxide, aramid fiber, silicon carbide whisker, silicon nitride whisker, and potassium titanate whisker. 5. 1. to 4. Epoxy resin composition particles according to any one of the above, having a spiral flow of 30 cm or more as measured according to the following procedure: (Procedure) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured.6. Epoxy resin composition particles according to any one of 1. to 5., wherein the content of the fibrous or acicular filler is 5% by mass or more and 80% by mass or less, based on 100% by mass of the epoxy resin composition particles. 7. Epoxy resin composition particles according to any one of 1. to 6., wherein the epoxy resin comprises a cresol novolac epoxy resin and / or a bisphenol A epoxy resin. 8. Epoxy resin composition particles according to any one of 1. to 7., wherein the epoxy resin comprises one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts. 9. 1. to 8. 10. Epoxy resin composition particles according to any one of 1. to 9., which are used to be molded into tablets through a process of feeding the epoxy resin composition particles into a heated extruder and kneading them while melting to obtain an epoxy resin molding material, and a process of cutting the molten epoxy resin molding material while continuously extruding it from an opening at the tip of the extruder to obtain tablets. 3 More than 1500cm 3 11. A method for producing an epoxy resin composition comprising the steps of: preparing epoxy resin composition particles according to any one of 1. to 9.; supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and cutting the molten epoxy resin molding material while continuously extruding it from an opening at the tip of the extruder to obtain pillar-shaped tablets, wherein the cross-sectional area of ​​the pillar-shaped tablets is 3 cm or less. 2 More than 100cm 2 The following is a method for manufacturing a columnar tablet.

[0096] A second reference form of this embodiment is described below. 1. Epoxy resin composition particles used for magnet fixation, electronic control unit sealing, coil sealing, or stator core sealing, comprising: an epoxy resin; and a fibrous or needle-like filler. 2. Epoxy resin composition particles according to 1., wherein the number-average fiber length of the fibrous or needle-like filler measured by the following procedure A is 5 μm or more and 500 μm or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and then the insoluble matter is dispersed on a glass plate. An image of the filler in the insoluble matter is taken using an optical microscope, and the fiber length is measured using an image analyzer. The fiber lengths are measured in descending order, and the average value of 100 fillers is taken as the number-average fiber length. 3. 1. or 2. Epoxy resin composition particles according to 4., wherein L is the number average fiber length of the fibrous or acicular filler measured by the following procedure A, and D is the number average fiber diameter of the fibrous or acicular filler measured by the following procedure B, and L / D is 3 or more and 100 or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and then the insoluble matter is dispersed on a glass plate. The filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average fiber length of the 100 longest fiber pieces is taken as the number average fiber length. (Procedure B) A scanning electron microscope is used to measure 100 cross sections of the fibrous filler from the cross section of the epoxy resin composition particle, and the average of the smallest diameters of each fiber cross section is determined as the number average fiber diameter. 4.1. to 3. Epoxy resin composition particles according to any one of 1. to 4., wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fiber, glass fiber, metal fiber, carbon fiber, fibrous aluminum oxide, aramid fiber, silicon carbide whisker, silicon nitride whisker, and potassium titanate whisker. 5. Epoxy resin composition particles according to any one of 1. to 4., wherein the spiral flow measured according to the following procedure is 30 cm or more.(Procedure) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured. 6. Epoxy resin composition particles according to any one of 1. to 5., wherein the content of the fibrous or acicular filler is 5% by mass or more and 80% by mass or less, based on 100% by mass of the epoxy resin composition particles. 7. Epoxy resin composition particles according to any one of 1. to 6., wherein the epoxy resin comprises a cresol novolac epoxy resin and / or a bisphenol A epoxy resin. 8. Epoxy resin composition particles according to any one of 1. to 7., wherein the epoxy resin comprises one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts. 9. Epoxy resin composition particles according to any one of 1. to 8. 10. Epoxy resin composition particles according to any one of 1. to 9., which are used to be molded into tablets through a process of feeding the epoxy resin composition particles into a heated extruder and kneading them while melting to obtain an epoxy resin molding material, and a process of cutting the molten epoxy resin molding material while continuously extruding it from an opening at the tip of the extruder to obtain tablets. 3 More than 1500cm 3 11. A method for producing an epoxy resin composition comprising the steps of: preparing epoxy resin composition particles according to any one of 1. to 9.; supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and cutting the molten epoxy resin molding material while continuously extruding it from an opening at the tip of the extruder to obtain pillar-shaped tablets, wherein the cross-sectional area of ​​the pillar-shaped tablets is 3 cm or less. 2 More than 100cm 2 The following is a method for manufacturing a columnar tablet.

[0097] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0098] (1) First Embodiment (Examples 1 to 6, Comparative Example 1) <Preparation of Epoxy Resin Composition Particles> A material mixture containing the components in the amounts shown in Table 1 below was kneaded with a heated roll, cooled into a sheet, and pulverized to obtain epoxy resin composition particles (granular molding material). The kneading conditions for the heated roll were a rotation speed of 20 rpm, a temperature of 120°C, and a kneading time of 5 to 10 minutes.

[0099] Details of each component in Table 1 are as follows: Fibrous or needle-like filler 1: glass fiber (manufactured by Nitto Boseki Co., Ltd., CS3E479) Fibrous or needle-like filler 2: wollastonite fiber (manufactured by NYCO Corporation, NYAD325) Spherical inorganic filler 1: glass beads (manufactured by Unitika Ltd., Unibeads UB-13L) Spherical inorganic filler 2: fused silica (manufactured by Fumitec Co., Ltd., FMT-15C) Colorant: carbon black (manufactured by Mitsubishi Chemical Corporation, #750B) Low-stress agent: epoxy-polyether-modified silicone oil (manufactured by Dow Corning Toray Co., Ltd., FZ-3730) Epoxy resin: cresol novolac epoxy resin (manufactured by DIC Corporation, N-673), softening point 78°C Curing agent 1: phenol-based curing agent (novolac phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-51470), softening point 104°C Curing agent 2: Phenol-based curing agent (novolac-type phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-HF-3) softening point 80°C Curing catalyst: Imidazole-based catalyst (2-phenyl-4,5-dihydroxyimidazole, manufactured by Shikoku Chemical Industry Co., Ltd., 2PHZ-PW) Mold release agent: Ester wax (manufactured by Clariant Chemical Japan, Licowax OP) Coupling agent: Aminosilane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., KBE-903)

[0100] <Number Average Fiber Length> After dissolving the epoxy resin composition particles in acetone to remove the resin component, the insoluble matter was dispersed on a glass plate, and the filler particles in the insoluble matter were photographed using an optical microscope and the fiber length was measured using an image analyzer. The average value of the fiber lengths of the 100 longest filler particles was taken as the number average fiber length (μm).

[0101]

[0102] The obtained epoxy resin composition particles were evaluated for the following items.

[0103] <Spiral flow> Using a low-pressure transfer molding machine (KTS-15, manufactured by Kotaki Seiki Co., Ltd.), the obtained epoxy resin composition particles were injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a pressure dwell time of 120 seconds, and the flow length was measured.

[0104] <Bending Test: Bending Modulus> The epoxy resin composition particles obtained above were tableted to obtain tablets. The obtained tablets were injection molded using a transfer molding machine under conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds to obtain test specimens as cured products measuring 10 mm wide x 4 mm thick x 80 mm long. The flexural modulus (GPa) of the obtained test specimens at room temperature was measured in accordance with JIS K 6911.

[0105] <K1c> Using a transfer molding machine, a molded article was formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the resulting molded article was cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm. A notch 3.5 mm deep in the thickness direction was formed in the longitudinal center, and the article was cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch 0.1 mm deep in the thickness direction was made with a razor at the tip of the notch in the cured product to prepare a test specimen with a total crack length a = 3.6 mm. Thereafter, as shown in FIG. 3, a three-point bending test was performed on the obtained test piece 10 using a tension and compression testing machine (STB-1225S Tensilon manufactured by Orientec Co., Ltd.) at a measurement temperature of 25° C., a speed of 10 mm / min, and a support distance S of 40 mm, and the fracture toughness value (K1c (MPa m 1/2 )) was calculated. Q is the maximum load (N). The tension and compression testing machine in FIG. 3 is equipped with a loading pin 12 with a diameter of 10 mm and two round supports 14 with rounded edges. C = ((P Q × S) / (B × W 3/2 ) × f(a / W) where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2 When the fracture toughness value of Comparative Example 1 calculated as above is normalized to 1.0, the relative fracture toughness values ​​of Examples 1 to 6 are shown in Table 1.

[0106] The above results show that the epoxy resin composition particles of Examples 1 to 6 in Table 1 exhibited higher flexural modulus than Comparative Example 1. It was also found that the epoxy resin composition particles of Examples 1 to 6 in Table 1 also exhibited excellent fracture toughness. The epoxy resin composition particles of Examples 1 to 6 in Table 1 can be suitably used for magnet fixing, electronic control unit sealing, coil sealing, or stator core sealing.

[0107] (2) Second Embodiment (Examples 1 to 5, Comparative Example 1) <Preparation of Epoxy Resin Composition Particles> A material mixture prepared by blending the components according to the blending amounts shown in Table 2 below was kneaded with a heated roll, cooled into a sheet, and pulverized to obtain epoxy resin composition particles (granular molding material). The kneading conditions for the heated roll were a rotation speed of 20 rpm, a temperature of 120°C, and a kneading time of 5 to 10 minutes.

[0108] Comparative Example 2 Epoxy resin composition particles (granular molding material) were obtained in the same manner as in Example 1 using the blending amounts and components shown in Table 2, except that the temperature was set to 90° C. in the heating roll kneading conditions.

[0109] Details of each component in Table 2 are as follows: Fibrous or needle-like filler 1: glass fiber (manufactured by Nitto Boseki Co., Ltd., CS3E479) Fibrous or needle-like filler 2: wollastonite fiber (manufactured by NYCO Corporation, NYAD325) Spherical inorganic filler 1: glass beads (manufactured by Unitika Ltd., Unibeads UB-13L) Spherical inorganic filler 2: fused silica (manufactured by Fumitec Co., Ltd., FMT-15C) Colorant: carbon black (manufactured by Mitsubishi Chemical Corporation, #750B) Low-stress agent: epoxy-polyether-modified silicone oil (manufactured by Dow Corning Toray Co., Ltd., FZ-3730) Epoxy resin: cresol novolac epoxy resin (manufactured by DIC Corporation, N-673), softening point 78°C Curing agent 1: phenol-based curing agent (novolac phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-51470), softening point 104°C Curing agent 2: Phenol-based curing agent (novolac-type phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-HF-3) softening point 80°C Curing catalyst: Imidazole-based catalyst (2-phenyl-4,5-dihydroxyimidazole, manufactured by Shikoku Chemical Industry Co., Ltd., 2PHZ-PW) Mold release agent: Ester wax (manufactured by Clariant Chemical Japan, Licowax OP) Coupling agent: Aminosilane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., KBE-903)

[0110] <Number Average Fiber Length> After dissolving the epoxy resin composition particles in acetone to remove the resin component, the insoluble matter was dispersed on a glass plate, and the filler particles in the insoluble matter were photographed using an optical microscope and the fiber length was measured using an image analyzer. The average value of the fiber lengths of the 100 longest filler particles was taken as the number average fiber length (μm).

[0111]

[0112] The obtained epoxy resin composition particles shown in Table 2 were evaluated for the following items.

[0113] <Spiral flow> Using a low-pressure transfer molding machine (KTS-15, manufactured by Kotaki Seiki Co., Ltd.), the obtained epoxy resin composition particles were injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a pressure dwell time of 120 seconds, and the flow length was measured.

[0114] <Bending Test: Bending Modulus> The epoxy resin composition particles obtained above were tableted to obtain tablets. The obtained tablets were injection molded using a transfer molding machine under conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds to obtain test specimens as cured products measuring 10 mm wide x 4 mm thick x 80 mm long. The flexural modulus (GPa) of the obtained test specimens at room temperature was measured in accordance with JIS K 6911.

[0115] <K1c> Using a transfer molding machine, a molded article was formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the resulting molded article was cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm. A notch 3.5 mm deep in the thickness direction was formed in the longitudinal center, and the article was cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch 0.1 mm deep in the thickness direction was made with a razor at the tip of the notch in the cured product to prepare a test specimen with a total crack length a = 3.6 mm. Thereafter, as shown in FIG. 3, a three-point bending test was performed on the obtained test piece 10 using a tension and compression testing machine (STB-1225S Tensilon manufactured by Orientec Co., Ltd.) at a measurement temperature of 25° C., a speed of 10 mm / min, and a support distance S of 40 mm, and the fracture toughness value (K1c (MPa m 1/2 )) was calculated. Q is the maximum load (N). The tension and compression testing machine in FIG. 3 is equipped with a loading pin 12 with a diameter of 10 mm and two round supports 14 with rounded edges. C = ((P Q × S) / (B × W 3/2 ) × f(a / W) where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2 The fracture toughness values ​​calculated as above are shown in Table 1.

[0116] <Evaluation of Gap at Filling> Forty electromagnetic steel sheets, each 130 mm in diameter and 0.35 mm thick, were stacked, and magnets were inserted into the holes in the stacked steel sheets. A total of five stacked layers, each with a 2 mm circumferential phase shift between layers of different heights, were used to prepare a rotor structure with a skewed structure. The workpiece was attached to a mold, and the epoxy resin composition particles were injected into the gaps between the holes and magnets in the rotor structure using a transfer molding machine at a mold temperature of 175°C, an injection pressure of 4 MPa, and a dwell time of 180 seconds. The presence or absence of gaps in each layer of the resulting molded product was confirmed using a feeler gauge. A 0.02 mm feeler gauge that could not be inserted was considered good, and a 0.02 mm or greater feeler gauge insertion was considered bad. In the evaluation of the gap at filling described above, Examples 1 to 5 showed good results, while Comparative Examples 1 and 2 showed bad results.

[0117] The above results show that the epoxy resin composition particles of Examples 1 to 5 in Table 2 exhibit higher K1c values ​​than Comparative Examples 1 and 2, and suppress the occurrence of gaps when filled into a skew structure. Such epoxy resin composition particles of Examples 1 to 5 in Table 2 can be suitably used for fixing magnets.

[0118] This application claims priority based on Japanese Patent Application No. 2023-071045 filed on April 24, 2023, and Japanese Patent Application No. 2023-071046 filed on April 24, 2023, the disclosures of which are incorporated herein in their entireties.

[0119] REFERENCE SIGNS LIST 1 Epoxy resin composition particles 2 Hopper 41 Heater 42 Screw 43 Cylinder 43a Input cylinder 5 Die 51 Temperature regulator 6 Extrusion material 10 Test piece 12 Loading pin 14 Round support 100 Injection molding device 15 Mold 16 Cavity 20 Injection molding machine 21 Cylinder 22 Screw 23 Hopper 24 Heater 25 Nozzle 26 Reverse flow valve 30 On-vehicle electronic control unit 32 Wiring board 34 Sealing resin 36 Electronic component 38 Connection terminal 40 Through hole

Claims

1. Epoxy resin composition particles used for either magnet fixing, electronic control unit sealing, coil sealing, or stator core sealing, the epoxy resin composition particles comprising: an epoxy resin; and a fibrous or needle-like filler.

2. An epoxy resin composition particle used for fixing a magnet, comprising an epoxy resin and a fibrous or needle-like filler, and having a fracture toughness value (K1c) of 3.0 MPa m or less as measured by the following procedure i. 1/2 The epoxy resin composition particles are as above. (Step i) Using a transfer molding machine, a molded body is molded from the epoxy resin composition particles under molding conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds. In accordance with the KIc method specified in ASTM D5045-14, the obtained molded body is sized to have a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm, and a notch of 3.5 mm in depth in the thickness direction is formed in the center of the length direction, and cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch of 0.1 mm in depth in the thickness direction is made with a razor at the tip of the notch of the cured product, and a test piece having a total crack length a = 3.6 mm is prepared. Thereafter, a three-point bending test is performed on the obtained test piece using a tension and compression tester at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S = 40 mm, and the fracture toughness value (K1c (MPa m 1/2 In the following formula, P Q is the maximum load (N). C = ((P Q x S) / (B x W 3/2 ) × f(a / W), where f(a / W) = (3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2 ) 3. Epoxy resin composition particles according to claim 1 or 2, wherein the number average fiber length of the fibrous or needle-like filler is 5 μm or more and 500 μm or less, as measured by the following procedure A. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin components, and then the insoluble matter is dispersed on a glass plate, and the filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average value of the fiber lengths of the 100 longest fiber lengths of the filler is regarded as the number average fiber length.

4. Epoxy resin composition particles according to claim 1 or 2, wherein L / D is 3 or more and 100 or less, where L is the number average fiber length of the fibrous or needle-like filler measured by the following procedure A, and D is the number average fiber diameter of the fibrous or needle-like filler measured by the following procedure B. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin components, and then the insoluble matter is dispersed on a glass plate, and the filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The fiber lengths are measured in order from longest to smallest, and the average value of 100 of the fillers is taken as the number average fiber length. (Procedure B) A scanning electron microscope is used to measure 100 cross sections of the fibrous filler from the cross section of the epoxy resin composition particle, and the average of the minimum diameter of each fiber cross section is calculated as the number average fiber diameter.

5. Epoxy resin composition particles according to claim 1 or 2, wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fibers, glass fibers, metal fibers, carbon fibers, fibrous aluminum oxide, aramid fibers, silicon carbide whiskers, silicon nitride whiskers, and potassium titanate whiskers.

6. Epoxy resin composition particles according to claim 1 or 2, which have a spiral flow of 30 cm or more as measured according to the following procedure ii: (Procedure ii) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured.

7. An epoxy resin composition particle according to claim 1 or 2, wherein the content of the fibrous or needle-like filler is 5% by mass or more and 80% by mass or less based on 100% by mass of the epoxy resin composition particle.

8. Epoxy resin composition particles according to claim 1 or 2, wherein the epoxy resin comprises a cresol novolac type epoxy resin and / or a bisphenol A type epoxy resin.

9. Epoxy resin composition particles according to claim 1 or 2, comprising one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts.

10. Epoxy resin composition particles according to claim 1 or 2, which are used to be molded into tablets through a process in which the epoxy resin composition particles are supplied to a heated extruder and kneaded while melting to obtain an epoxy resin molding material, and a process in which the molten epoxy resin molding material is continuously extruded from an opening at the tip of the extruder while being cut to obtain tablets.

11. Epoxy resin composition particles according to claim 1 or 2, which are used in injection molding by being poured into a cylinder in an injection molding apparatus equipped with an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold having a cavity and connected to the injection unit.

12. An epoxy resin composition particle according to claim 1 or 2, comprising an epoxy resin having a softening point of less than 110°C or a curing agent.

13. A tablet formed using the epoxy resin composition particles according to claim 1 or 2, the tablet having a size of 5 cm 3 More than 1500cm 3 Tablets having the following volumes:

14. A method for producing an epoxy resin molding material, comprising the steps of: preparing the epoxy resin composition particles according to claim 1 or 2; supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and cutting the epoxy resin molding material while continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder to obtain columnar tablets, the columnar tablets having a cross-sectional area of ​​3 cm or less. 2 More than 100cm 2 The manufacturing method of the columnar tablet is as follows:

15. A structure using the epoxy resin composition particles according to claim 1 or 2.

16. A method for producing a structure as described in claim 15, comprising the steps of: using an injection molding device equipped with an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold connected to the injection unit and having a cavity, melting the epoxy resin composition particles in the cylinder to form a molten resin composition; and injecting the molten resin composition from the tip of the screw to fill the cavity.

17. A method for producing a structure according to claim 16, wherein the temperature T of the tip of the screw is 60 to 100°C in the filling step.

18. A method for producing a structure according to claim 16, wherein the temperature inside the cavity is 150 to 180°C in the filling step.

Citation Information

Patent Citations

  • Epoxy resin composition for sealing optical semiconductor device

    JP1997208805A

  • Resin composition for stator core insulation

    JP2020094092A

  • Joint

    JP2023071045A

  • Double structure container

    JP2023071046A

  • Fixing resin composition for use in rotor

    WO2012029278A1

Cited By

  • Tablet-shaped epoxy resin molding material, columnar tablet, and method for manufacturing columnar tablet

    JP7845585B2

  • JPWO2025211171A1

  • Tablet-shaped epoxy resin molding material, columnar tablet, and method for producing columnar tablet

    WO2025211171A1