Laminate and method for producing recycled film

The laminate with an alkali-soluble resin and pigment in the printing layer addresses the high solar transmittance and recycling issues of fluororesin films by allowing easy removal and maintaining weather resistance, ensuring efficient recycling and reduced defects.

WO2024225272A1PCT designated stage expired Publication Date: 2024-10-31AGC INC

Patent Information

Application Number
PCT/JP2024/015924
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Fluororesin films used in membrane structures face issues with high solar transmittance and temperature due to their weather resistance properties, and existing methods for removing printed layers during recycling are inefficient, leading to colored defects and economic concerns.

Method used

A laminate with a fluororesin film and a printing layer containing an alkali-soluble resin and pigment, where the alkali-soluble resin content is between 1.0% to 15.0% by mass, allowing for easy removal with an alkaline solution and maintaining high weather resistance.

Benefits of technology

The laminate enables efficient removal of the printed layer while maintaining excellent weather resistance, preventing color defects and reducing recycling costs, and the recycled film retains mechanical properties similar to the original fluororesin film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The purpose of the present invention is to provide a laminate in which a printed layer can be easily removed and that has high weather resistance, and a method for producing a recycled film. A laminate according to the present invention comprises: a film containing a fluororesin; and a printed layer containing an alkali-soluble resin and a pigment on at least a part of the film. The content of the alkali-soluble resin is 1.0-15.0 mass% with respect to the total mass of the printed layer.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and method for manufacturing recycled film

[0001] The present invention relates to a method for producing a laminate and a recycled film.

[0002] Fluororesin films have excellent weather resistance, stain resistance, and other properties, and are therefore used as membrane materials (roofing materials, exterior wall materials, and the like) in membrane structure facilities (sports facilities (swimming pools, gymnasiums, tennis courts, soccer fields, athletics stadiums, and the like), warehouses, assembly halls, exhibition halls, horticultural facilities (horticultural greenhouses, agricultural greenhouses, and the like)), and the like.

[0003] However, because fluororesin films have a high solar radiation transmittance, when they are used as membrane materials for membrane structures exposed to sunlight, the interior of the membrane structure may become too bright or the temperature inside the membrane structure may become too high. Therefore, paint or ink is printed on the fluororesin film to increase the solar radiation reflectance and reduce the solar radiation transmittance to the interior. In addition, the team colors, logos, etc. of the teams using the sports facilities are sometimes printed on the film with paint or ink.

[0004] Furthermore, since film materials are often used for long periods of time and outdoors, the paints and inks applied to fluororesin films are required to be weather resistant.

[0005] For example, Patent Document 1 discloses a laminate comprising a substrate containing a fluorine-containing polymer and a resin film disposed on at least a partial region of the substrate, and the resin film is formed from a composition containing aluminum-containing composite particles, a fluorine-containing polymer, and a liquid medium. Patent Document 2 discloses a composition for forming a non-curable coating film to be applied to a fluororesin substrate, and the composition contains a fluorine-containing copolymer and a solvent, and the mass average molecular weight (M w ) is 30,000 to 60,000, and the average number of moles of the specific functional group per mole of the fluorine-containing copolymer is 33 or more and less than 54. Patent Document 3 discloses a printing ink containing composite particles having a titanium oxide core and three coating layers, a resin, and a liquid medium.

[0006] International Publication No. 2015 / 152170 Japanese Patent Application Laid-Open No. 2006-152061 International Publication No. 2011 / 013572

[0007] In recent years, there has been an expectation that fluororesin films having a printed layer printed with such paint or ink can be reused after use, etc. In addition to removing the printed layer from the fluororesin film and reusing it in the film form, it is also desirable to heat melt the film to form pellets and process them into fluororesin films for other uses or with different shapes such as thicknesses for reuse.

[0008] However, since the resin components contained in the paint or ink do not have as high heat resistance as the fluororesin film substrate, they become discolored when heated for melting or the like during reprocessing, and so it is necessary to remove the printed layer from the fluororesin film. In fact, paint or ink that has been subjected to a thermal history of approximately 250 to 350°C becomes discolored black, so if the fluororesin film is melted and reprocessed with the printed layer still attached, the resulting film will have black defects or will be darkly discolored overall.

[0009] In view of the above circumstances, it is desirable that the printed layer on the fluororesin film be able to be cleanly removed from the fluororesin film when it is recycled. Possible methods for removing the printed layer include wiping it off with a cloth or the like soaked in an organic solvent such as acetone, or scraping the printed layer off with a grinder. However, in some cases, the printed area accounts for 20 to 95% of the area of ​​the fluororesin film, making the above-mentioned removal methods uneconomical. Furthermore, since the film is often used for long periods of time and outdoors, the printed layer is also required to have excellent weather resistance.

[0010] The present disclosure has been made in view of the above circumstances, and aims to provide a laminate that allows for easy removal of a printed layer and has high weather resistance, and a method for producing a recycled film.

[0011] Specific means for achieving the above object are as follows. <1> A laminate comprising a film containing a fluororesin and a printed layer, at least partially on the film, containing an alkali-soluble resin and a pigment, wherein the content of the alkali-soluble resin is 1.0 to 15.0 mass % relative to the total mass of the printed layer. <2> The laminate according to <1>, wherein the printed layer further contains at least one resin selected from the group consisting of a fluororesin and a (meth)acrylic resin. <3> The laminate according to <2>, wherein the fluororesin in the printed layer is a copolymer having a fluoroolefin unit and a monomer unit having a hydroxyl group. <4> The laminate according to any one of <1> to <3>, wherein the acid value of the alkali-soluble resin is 100 to 500 mgKOH / g. <5> The laminate according to any one of <1> to <4>, wherein the pigment is aluminum composite particles coated with a (meth)acrylic resin or silica. <6> The laminate according to any one of <1> to <5>, wherein the laminate is used outdoors. <7> The laminate according to any one of <1> to <6>, which is at least one material selected from the group consisting of roofing materials, wall covering materials, and display materials. <8> A method for producing a recycled film, comprising impregnating the laminate according to any one of <1> to <7> in an alkaline solution to remove the printed layer and obtain a recycled film containing a fluororesin. <9> A method for producing a recycled film, comprising impregnating the laminate according to any one of <1> to <7> in an alkaline solution to remove the printed layer and obtain a film containing a fluororesin, and melting and molding the obtained film containing a fluororesin to obtain a recycled film containing a fluororesin.

[0012] According to one aspect of the present disclosure, a laminate having a highly weather-resistant property and a method for producing a recycled film, in which a printed layer can be easily removed, can be provided.

[0013] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including element steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the present disclosure.

[0014] In the present disclosure, when a numerical range is indicated using "to", the numerical values ​​before and after "to" are included as the minimum and maximum values, respectively. In the present disclosure, when a numerical range is indicated in a stepped manner, the upper or lower limit value of one numerical range may be replaced with the upper or lower limit value of another stepped numerical range. Furthermore, in the numerical ranges indicated in the present disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple corresponding substances. When multiple substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the particles corresponding to each component may contain multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for the mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, the "unit" of a polymer means a portion derived from a monomer that is present in the polymer and constitutes the polymer. In addition, a unit also refers to a structure of a unit that is chemically converted after polymer formation. In some cases, units derived from individual monomers are called by the name of the monomer with "unit" added. In this disclosure, films and sheets are referred to as "films" regardless of their thickness. In this disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic. In this disclosure, the term "layer" includes cases where the layer is formed over the entire area when the area where the layer is present is observed, as well as cases where the layer is formed only over a portion of the area.

[0015] <Laminate> The laminate of the present disclosure comprises a film containing a fluororesin and a printed layer containing an alkali-soluble resin and a pigment, the printed layer being formed on at least a portion of the film, and the content of the alkali-soluble resin is 1.0 to 15.0 mass% relative to the total mass of the printed layer.

[0016] The above configuration allows the printed layer to be easily removed, resulting in a laminate with high weather resistance. The reason for this is unclear, but is presumed to be as follows: By using a film containing a fluororesin, which has better weather resistance than other resins, the weather resistance is excellent. Furthermore, by using an alkali-soluble resin for the printed layer, the printed layer can be easily removed. In particular, by making the content of the alkali-soluble resin 1.0% by mass or more relative to the total mass of the printed layer, the printed layer can be easily removed. Furthermore, by making the content of the alkali-soluble resin 15.0% by mass or less relative to the total mass of the printed layer, the printed layer has excellent weather resistance. Furthermore, because the printed layer contains a pigment, the laminate provided with the printed layer has high solar reflectance. Therefore, in membrane structure facilities and the like using the laminate of the present disclosure, the indoor temperature, brightness, etc. can be appropriately adjusted.

[0017] (Film containing fluororesin) The laminate of the present disclosure has a film (hereinafter also referred to as "substrate") containing a fluororesin. The fluororesin contained in the substrate is preferably one that can be formed into a film. Furthermore, the fluororesin contained in the substrate is preferably one that has excellent weather resistance. From the above viewpoints, the fluororesin contained in the substrate is preferably a homopolymer or copolymer of a fluoroolefin. Examples of the fluoroolefin include fluoroolefins that will be described later as structural units of specific fluororesins. The fluororesins may be used alone or in combination of two or more.

[0018] Examples of fluoroolefin copolymers include copolymers of two or more fluoroolefins, copolymers of one or more fluoroolefins with one or more olefins or perfluoro(alkyl vinyl ethers), etc. The fluoroolefins and olefins preferably have 2 or 3 carbon atoms. The perfluoro(alkyl vinyl ether) preferably has 3 to 6 carbon atoms.

[0019] Preferred fluororesins include vinyl fluoride polymer (hereinafter also referred to as "PVF"), vinylidene fluoride polymer (hereinafter also referred to as "PVDF"), vinylidene fluoride-hexafluoropropylene copolymer, THV, tetrafluoroethylene-propylene copolymer, tetrafluoroethylene-vinylidene fluoride-propylene copolymer, ethylene-tetrafluoroethylene copolymer (hereinafter also referred to as "ETFE"), hexafluoropropylene-tetrafluoroethylene copolymer (hereinafter also referred to as "FEP"), ethylene-hexafluoropropylene-tetrafluoroethylene copolymer (hereinafter also referred to as "EFEP"), perfluoro(alkyl vinyl ether)-tetrafluoroethylene copolymer (hereinafter also referred to as "PFA"), chlorotrifluoroethylene polymer (hereinafter also referred to as "PCTFE"), and ethylene-chlorotrifluoroethylene copolymer (hereinafter also referred to as "ECTFE"). As the fluororesin, ETFE is particularly preferred.

[0020] The fluorine atom content of the fluororesin contained in the substrate is preferably 35% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more. When the fluorine atom content is equal to or greater than the lower limit of the above range, the substrate will have even better weather resistance, stain resistance, chemical resistance, and non-stick properties, and will be particularly excellent in non-stick properties and stain resistance. The fluorine atom content of the fluororesin contained in the substrate is preferably 80% by mass or less, more preferably 70% by mass or less. The fluorine atom content of the fluororesin can be determined by burning the fluororesin and then using a fluoride ion selective electrode in combination with gas chromatography.

[0021] The content of the fluororesin is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, relative to the total mass of the substrate, and may be 100% by mass. When the content of the fluororesin is equal to or more than the lower limit of the above range, the weather resistance of the substrate is further improved.

[0022] The substrate may further contain a non-fluorinated resin, known additives, etc. Examples of known additives include colored pigments, UV absorbers, near-infrared absorbing pigments, and near-infrared reflective pigments. Examples of colored pigments include titanium oxide, which is a white pigment, aluminum cobalt oxide, which is a blue pigment, and iron oxide, which is a red pigment. Examples of UV absorbers include inorganic UV absorbers and organic UV absorbers. Examples of inorganic UV absorbers include inorganic particles such as zinc oxide, titanium oxide, cerium oxide, and iron oxide; and inorganic composite particles in which the surfaces of the inorganic particles are coated with an inorganic material such as silica, alumina, or zirconia. Examples of near-infrared absorbing pigments or near-infrared reflective pigments include boron compounds such as lanthanum hexaboride, tungsten compounds such as cesium tungstate, indium tin oxide, and antimony tin oxide.

[0023] The fluorine atom content in the substrate is preferably 27% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 45% by mass or more. When the fluorine atom content is equal to or greater than the lower limit of the above range, the weather resistance, stain resistance, chemical resistance, and non-stickiness of the substrate are further improved, and the non-stickiness and stain resistance are particularly improved. The fluorine atom content in the substrate is preferably 70% by mass or less, more preferably 60% by mass or less. The fluorine atom content in the substrate is determined by combusting the substrate and then using a fluoride ion selective electrode in combination with gas chromatography.

[0024] The stress of the substrate at 10% elongation is preferably 10 MPa or more, more preferably 16 MPa or more. The stress at 10% elongation does not depend on the thickness of the film but on the composition of the fluororesin. When the stress at 10% elongation is 10 MPa or more, the film also has excellent snow load resistance and wind pressure resistance. The stress at 10% elongation of the substrate is preferably 80 MPa or less, more preferably 50 MPa or less.

[0025] In the present disclosure, the stress at 10% elongation is determined by the method specified in JIS K7127:1999 (Plastics - Test methods for tensile properties - Part 3: Test conditions for films and sheets). Using dumbbell 5 as a test specimen, the stress is calculated by dividing the tension when stretched at a tensile speed of 200 mm / min by the cross-sectional area of ​​the film before stretching.

[0026] When the printed layer described below has a light reflecting function, the substrate preferably has light transparency so as not to inhibit the light reflecting function of the printed layer. The total light transmittance of the substrate is preferably 70% or more, more preferably 85% or more. The total light transmittance of the substrate is preferably 99.9% or less, more preferably 98% or less. In the present disclosure, "total light transmittance" is a value measured in accordance with JIS K7375:2008 "Plastics - Determination of total light transmittance and total light reflectance."

[0027] The thickness of the substrate is preferably 25 to 1,000 μm, more preferably 100 to 500 μm. When the thickness of the substrate is equal to or greater than the lower limit of the above range, the mechanical strength of the substrate is excellent. When the thickness of the substrate is equal to or less than the upper limit of the above range, the light transmittance of the substrate is excellent.

[0028] From the viewpoint of improving adhesion to the printing layer, the surface of the substrate on which the printing layer is formed is preferably subjected to a surface treatment to increase surface tension. By performing the surface treatment, polar groups such as formyl groups, carboxy groups, and hydroxyl groups are formed on the surface of the substrate. For example, if the printing layer contains a resin having hydroxyl groups in addition to an alkali-soluble resin, the hydroxyl groups of this resin and the polar groups formed on the surface of the substrate form chemical bonds, further improving adhesion between the substrate and the printing layer. Examples of surface treatments include corona discharge treatment, metallic sodium treatment, mechanical roughening treatment, and excimer laser treatment. Corona discharge treatment is preferred from the viewpoints of fast treatment speed and the elimination of the need for post-treatment cleaning.

[0029] The surface tension of the substrate is preferably 0.035 N / m or more, more preferably 0.04 N / m or more. When the surface tension of the substrate is equal to or greater than the lower limit of the above range, the adhesion between the substrate and the printing layer is further improved. The upper limit of the surface tension of the substrate is not particularly limited, but may be, for example, 0.06 N / m.

[0030] (Printed Layer) The laminate of the present disclosure has a printed layer on at least a portion of the substrate. The printed layer contains an alkali-soluble resin and a pigment, and the content of the alkali-soluble resin is 1.0 to 15.0 mass % relative to the total mass of the printed layer.

[0031] -Alkali-Soluble Resin- In the present disclosure, an alkali-soluble resin refers to a resin that can dissolve 0.1 g or more in 100 mL of a 1.5 mass % aqueous sodium hydroxide solution at 85°C.

[0032] From the viewpoint of improving the removability of the printed layer with an alkaline solution, the acid value of the alkali-soluble resin is preferably 100 mgKOH / g or more, more preferably 150 mgKOH / g or more, and even more preferably 250 mgKOH / g or more. Furthermore, from the viewpoint of adhesion of the printed layer to the substrate, the acid value of the alkali-soluble resin is preferably 500 mgKOH / g or less, more preferably 400 mgKOH / g or less. In the present disclosure, the "acid value" is measured in accordance with JIS K 0070:1992.

[0033] The alkali-soluble resin may be used alone or in combination of two or more. The alkali-soluble resin preferably has an alkali-soluble group such as a phenolic hydroxyl group, a carboxyl group, or an acid anhydride group in the main chain or side chain, more preferably a carboxyl group or an acid anhydride group in the main chain or side chain. The alkali-soluble resin preferably has a structural unit derived from at least one selected from the group consisting of a monomer having a phenolic hydroxyl group, a monomer having an acid anhydride group, and a monomer having a carboxyl group, more preferably a structural unit derived from at least one selected from the group consisting of a monomer having an acid anhydride group and a monomer having a carboxyl group. The alkali-soluble resin may be a homopolymer of these, a copolymer of these, or a copolymer of these monomers or other monomers.

[0034] Examples of monomers having an acid anhydride group or a carboxyl group include unsaturated carboxylic acids such as (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, tetrahydrophthalic anhydride, and itaconic acid, with (meth)acrylic acid being preferred from the viewpoint of excellent copolymerizability. Examples of other monomers include (meth)acrylic monomers such as (meth)acrylic acid esters and hydroxylethyl (meth)acrylate; nitrile monomers such as (meth)acrylonitrile; amide monomers such as (meth)acrylamide; N-alkoxy-substituted amide monomers; N-methylol-substituted amide monomers; styrene-based monomers such as styrene, vinyltoluene, α-methylstyrene, and divinylbenzene; allyl monomers such as diallyl phthalate, allyl glycidyl ether, and triallyl isocyanurate; and monomers having a polymerizable double bond such as vinyl acetate and N-vinylpyrrolidone. Examples of other monomers include acrylic monomers and styrene-based monomers, with styrene-based monomers being more preferred.

[0035] The alkali-soluble resin is preferably a copolymer obtained by copolymerizing one or more monomers having an acid anhydride group or a carboxyl group with one or more other monomers. The alkali-soluble resin is preferably a (meth)acrylic copolymer having an acid anhydride group or a carboxyl group, or a styrene-based monomer copolymer having an acid anhydride group or a carboxyl group, and more preferably a styrene-based monomer copolymer having an acid anhydride group or a carboxyl group.

[0036] As the other monomer, a monomer having a group that is easily saponified by an alkaline solution to increase hydrophilicity (hereinafter also referred to as a "hydrophilicity-improving group") may be used. Examples of the monomer having a hydrophilicity-improving group include lower alkyl esters of polymerizable unsaturated carboxyl compounds, and methyl acrylate is preferred from the viewpoint of excellent saponification rate by an alkaline solution.

[0037] Commercially available alkali-soluble resins that can be used include SMA17352P (styrene-maleic anhydride copolymer resin, manufactured by Kawahara Oil Chemical Co., Ltd., weight average molecular weight: 7000, acid value: 270 mgKOH / g) and Joncryl 682 (styrene-acrylic acid copolymer resin, manufactured by BASF, weight average molecular weight: 1750, acid value: 238 mgKOH / g).

[0038] The proportion of the total amount of units derived from monomers having an alkali-soluble group relative to the entire molecule of the alkali-soluble resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, and the proportion of the total amount of units derived from monomers having an alkali-soluble group relative to the entire molecule of the alkali-soluble resin is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.

[0039] The weight average molecular weight of the alkali-soluble resin is preferably from 500 to 50,000, more preferably from 1,000 to 10,000, and even more preferably from 2,000 to 8,000, from the viewpoint of solubility.

[0040] The content of the alkali-soluble resin relative to the total mass of the printed layer is 1.0 to 15.0% by mass. From the viewpoint of removability of the printed layer with an alkaline solution, the content of the alkali-soluble resin relative to the total mass of the printed layer is preferably 1.2% by mass or more, more preferably 1.5% by mass or more. Furthermore, from the viewpoint of improving adhesion between the substrate and the printed layer in a long-term humidity test, the content of the alkali-soluble resin relative to the total mass of the printed layer is preferably 14% by mass or less, more preferably 12% by mass or less, even more preferably 9.0% by mass or less, and particularly preferably 6.0% by mass or less.

[0041] Pigment The pigment contained in the printing layer may be either an organic pigment or an inorganic pigment. Examples of pigments include titanium oxide and zinc oxide (white pigments), carbon black, bismuth oxide, and chromium compounds (black pigments), iron oxide and perylene (red pigments), aluminum cobalt oxide (blue pigments), copper phthalocyanine (blue or green pigments), and bismuth vanadate (yellow pigments). Other examples include pearlescent mica, which is a flat substrate such as mica, silica, or alumina coated with titanium oxide or iron oxide, as well as pearlescent silica, pearlescent glass, and pearlescent alumina. Furthermore, the pigment may be a near-infrared absorbing pigment or a near-infrared reflective pigment. Examples of near-infrared absorbing or near-infrared reflective pigments include boron compounds such as lanthanum hexaboride (green pigments), tungsten compounds such as cesium tungstate (blue pigments), indium tin oxide (light blue pigments), antimony tin oxide (blue pigments), and so-called pearlescent pigments that utilize the interference color of light. One pigment may be used alone, or two or more pigments may be used in combination.

[0042] Furthermore, aluminum-based pigments or stainless steel-based pigments may be used to adjust the visible light reflectance and solar radiation reflectance. Aluminum-based pigments are most commonly used as inks for printing on the surface of fluororesin films. Examples include aluminum particles such as aluminum flakes, or aluminum particles coated with an organic or inorganic substance (surface-treated aluminum particles). Examples of organic substances in the surface-treated aluminum particles include resins, fatty acids, silane coupling agents, etc., and examples of inorganic substances include inorganic oxides such as silica, metals other than aluminum, etc. Among these, aluminum composite particles coated with (meth)acrylic resin or silica are particularly preferred from the viewpoint of preventing the visible light reflectance and solar radiation reflectance of the laminate of the present disclosure from decreasing over a long period of time.

[0043] The total coating amount of (meth)acrylic resin and silica in the aluminum composite particles is more preferably 3 to 35 parts by mass, even more preferably 3 to 33 parts by mass, and particularly preferably 4 to 30 parts by mass, per 100 parts by mass of the aluminum particles. When the total coating amount of (meth)acrylic resin and silica is at or above the lower limit of the above range, the aluminum particles are sufficiently protected by the (meth)acrylic resin or silica, and the solar reflectance of the laminate of the present disclosure is less likely to decrease over the long term. When the total coating amount of (meth)acrylic resin and silica is at or below the upper limit of the above range, the laminate of the present disclosure tends to be prevented from dissolving due to deterioration of the (meth)acrylic resin during long-term use, and from cracking inside the silica and causing moisture to penetrate and dissolve the aluminum particles. As a result, the solar reflectance of the laminate of the present disclosure is less likely to decrease over the long term. In another embodiment, the total coating amount of the (meth)acrylic resin and silica on the aluminum composite particles is preferably 30 to 45 parts by mass, more preferably 32 to 40 parts by mass, and even more preferably 34 to 38 parts by mass, per 100 parts by mass of the aluminum particles. When the total coating amount of the (meth)acrylic resin and silica is at least the lower limit of the above range, the aluminum particles are sufficiently protected by the (meth)acrylic resin or silica, and the solar reflectance of the laminate of the present disclosure is unlikely to decrease over the long term. When the total coating amount of the (meth)acrylic resin and silica is at most the upper limit of the above range, dissolution of aluminum by halogen ions or hydrogen halide generated from the substrate, alkali-soluble resin, other resins described below, and dissolution of aluminum by water is unlikely to occur, and the solar reflectance of the laminate of the present disclosure is unlikely to decrease over the long term.

[0044] It is desirable that the aluminum composite particles are insoluble in an alkaline solution, since dissolving the aluminum composite particles in an alkaline aqueous solution may result in the generation of hydrogen gas.

[0045] The average major axis of the aluminum composite particles is preferably 6 to 25 μm, more preferably 8 to 15 μm. The average major axis of the aluminum composite particles is the arithmetic mean value when 20 particles are measured using a scanning electron microscope (SEM). Commercially available products containing aluminum composite particles include EMR-D5660, BP-280PA, BPZ-6370, WZA-7670, BPA-6390, EMR-B5680, EMR-D6390, and EMR-D4690 (all trade names, manufactured by Toyo Aluminum K.K.).

[0046] When the printing layer contains aluminum composite particles, from the viewpoint of the balance between solar reflectance, viscosity of the resin composition, adhesion, and the like, the content of the aluminum composite particles is preferably 10 to 60 mass%, more preferably 15 to 50 mass%, and even more preferably 20 to 40 mass%, relative to the total mass of the printing layer.

[0047] The pigment content is preferably 0.1 to 60% by mass, more preferably 5 to 55% by mass, based on the total mass of the printed layer. In the case of a white pigment, the content is preferably 20 to 60% by mass, more preferably 30 to 55% by mass. In the case of a black pigment, the content is preferably 0.1 to 10% by mass, more preferably 1 to 5% by mass.

[0048] -Other Resins- The printing layer may contain other resins other than the alkali-soluble resin. The other resins may be used alone or in combination of two or more. Examples of the other resins include fluororesins, (meth)acrylic resins, polyester-based resins, vinyl-based resins, styrene-based resins, cellulose-based resins, carbonate-based resins, amide-based resins, polyolefin-based resins such as propylene resins, vinyl alcohol-based resins, imide-based resins, phenol-based resins, and urethane-based resins. Among these, the other resin preferably contains at least one selected from the group consisting of fluororesins and (meth)acrylic resins, from the viewpoint of excellent adhesion to the substrate. When the printing layer contains at least one of fluororesins and (meth)acrylic resins, the laminate of the present disclosure has excellent weather resistance, and hardening of the printing layer is suppressed even after long-term use. This suppresses a decrease in conformity to the substrate, thereby maintaining adhesion. In particular, when the printing layer contains a fluororesin, it is preferable because it has excellent adhesion, even better weather resistance, and also excellent contamination resistance.

[0049] [Fluororesin] As the fluororesin as the other resin, known fluororesins can be used, and among them, a copolymer having a fluoroolefin unit and a monomer unit having a hydroxyl group (hereinafter also referred to as "specific fluororesin") is preferred. The specific fluororesin has a monomer unit having a hydroxyl group in addition to the fluoroolefin unit, and therefore has excellent properties inherent to fluororesins, such as weather resistance and contamination resistance, as well as excellent adhesion to substrates. The specific fluororesin may also be a copolymer with other monomers. The specific fluororesin may be used alone or in combination of two or more types.

[0050] The fluoroolefin in the fluoroolefin unit is preferably a fluoroolefin having 10 or less carbon atoms. Specific examples include vinyl fluoride, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene (hereinafter also referred to as "CTFE"), tetrafluoroethylene (hereinafter also referred to as "TFE"), hexafluoropropylene, perfluorobutene-1, perfluorohexene-1, perfluorononene-1, and (perfluoroalkyl)ethylene, with (perfluoroalkyl)ethylene being preferred.

[0051] (Perfluoroalkyl)ethylene is CH 2 =CH-R f (However, R f represents a perfluoroalkyl group). Specific examples include (perfluoromethyl)ethylene, (perfluorobutyl)ethylene, etc. As the (perfluoroalkyl)ethylene, a (perfluoroalkyl)ethylene having 3 to 8 carbon atoms is preferred. As the fluoroolefin other than the (perfluoroalkyl)ethylene, a fluoroolefin having 2 or 3 carbon atoms (however, CH 2 =CH-R f ) is preferred.

[0052] The monomer unit having a hydroxyl group may be a monomer unit having a fluorine atom or a monomer unit not having a fluorine atom, and is preferably a monomer unit not having a fluorine atom. Examples of the monomer unit having a hydroxyl group include units derived from allyl alcohol, hydroxyalkyl vinyl ether, hydroxyalkyl allyl ether, hydroxyalkyl (meth)acrylate, hydroxyalkyl vinyl carboxylate, hydroxyalkyl allyl carboxylate, etc. The hydroxyalkyl group of the monomer unit having a hydroxyalkyl group may be a hydroxycycloalkyl group, a hydroxyalkyl-substituted cycloalkyl group, etc. The number of carbon atoms of the hydroxyalkyl group is preferably 10 or less, more preferably 6 or less.

[0053] Examples of hydroxyalkyl vinyl ethers include 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 4-hydroxycyclohexyl vinyl ether. Examples of hydroxyalkyl allyl ethers include 2-hydroxyethyl allyl ether, 3-hydroxypropyl allyl ether, 4-hydroxybutyl allyl ether, and 4-hydroxycyclohexyl allyl ether. Examples of hydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate. Examples of hydroxyalkyl vinyl carboxylates include vinyl hydroxyacetate, vinyl hydroxyisobutyrate, vinyl hydroxypropionate, vinyl hydroxybutyrate, vinyl hydroxyvalerate, and vinyl hydroxycyclohexanecarboxylate. Examples of hydroxyalkyl allyl carboxylates include allyl hydroxyacetate, allyl hydroxypropionate, allyl hydroxybutyrate, allyl hydroxyisobutyrate, and allyl hydroxycyclohexanecarboxylate.

[0054] Examples of monomer units other than fluoroolefin units and monomer units having a hydroxyl group include units derived from fluorine-containing monomers other than fluoroolefins and units derived from monomers not having fluorine atoms (all of which exclude monomer units having a hydroxyl group). Examples of fluorine-containing monomers other than fluoroolefins include perfluoro(alkyl vinyl ether) and perfluorounsaturated cyclic ether. As perfluoro(alkyl vinyl ether), perfluoro(alkyl vinyl ether) having 10 or less carbon atoms is preferred, and perfluoro(alkyl vinyl ether) having 6 or less carbon atoms is more preferred. Specific examples include perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), perfluoro(propyl vinyl ether), and perfluoro(heptyl vinyl ether).

[0055] Examples of monomers not containing fluorine atoms include olefins, vinyl ethers, allyl ethers, vinyl carboxylates, allyl carboxylates, and unsaturated carboxylic acid esters. The number of carbon atoms in the vinyl ethers, allyl ethers, vinyl carboxylates, allyl carboxylates, and unsaturated carboxylic acid esters is preferably 16 or less, and more preferably 12 or less. Preferred olefins have 2 to 4 carbon atoms, such as ethylene, propylene, and isobutylene. Examples of vinyl ethers include cycloalkyl vinyl ethers (cyclohexyl vinyl ether, etc.) and alkyl vinyl ethers (nonyl vinyl ether, 2-ethylhexyl vinyl ether, hexyl vinyl ether, ethyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, etc.). Examples of allyl ethers include alkyl allyl ethers (ethyl allyl ether, hexyl allyl ether, etc.). Examples of vinyl carboxylates include vinyl esters of carboxylic acids (acetic acid, butyric acid, pivalic acid, benzoic acid, propionic acid, etc.). Furthermore, as a vinyl ester of a carboxylic acid having a branched alkyl group, Veova 9 (registered trademark) and Veova 10 (registered trademark) manufactured by Oxalis Chemicals Co., Ltd. may be used. Examples of allyl carboxylates include allyl esters of carboxylic acids (acetic acid, butyric acid, pivalic acid, benzoic acid, propionic acid, etc.). Examples of unsaturated esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate.

[0056] The specific fluororesin may further contain a monomer unit having a crosslinkable group other than a hydroxyl group, such as a carboxy group, an amide group, or an epoxy group.

[0057] In the specific fluororesin, a particularly preferred combination of a fluoroolefin unit and a monomer unit having a hydroxyl group is a combination of at least one selected from the group consisting of tetrafluoroethylene and chlorotrifluoroethylene with a hydroxyalkyl vinyl ether.

[0058] The proportion of fluoroolefin units in the specific fluororesin is preferably 30 to 70 mol %, more preferably 40 to 60 mol %, of all units in the specific fluororesin. When the proportion of fluoroolefin units is equal to or greater than the lower limit of the above range, a printed layer with excellent weather resistance, stain resistance, etc. tends to be obtained. When the proportion of fluoroolefin units is equal to or less than the upper limit of the above range, the adhesion between the substrate and the printed layer tends to be even better.

[0059] The proportion of hydroxyl group-containing monomer units in the specific fluororesin is preferably 0.5 to 20 mol %, more preferably 1 to 15 mol %, of all units in the specific fluororesin. When the proportion of hydroxyl group-containing monomer units is equal to or greater than the lower limit of the above range, the adhesion between the printed layer and the substrate tends to be even better. When the proportion of hydroxyl group-containing monomer units is equal to or less than the upper limit of the above range, the flexibility of the printed layer tends to be excellent.

[0060] The proportion of the monomer units in the fluororesin can be confirmed by nuclear magnetic resonance (NMR) spectroscopy.

[0061] In one embodiment, the specific fluororesin is preferably a copolymer having a fluoroolefin unit, a hydroxyl group-containing monomer unit, and a hydroxyl-free non-fluorine-containing monomer unit. Hereinafter, such a copolymer will also be referred to as "copolymer (A)."

[0062] As the combination of monomers constituting copolymer (A), the following combinations (1) to (3) are preferred, and combination (2) or (3) is more preferred, from the viewpoints of preventing the solar reflectance of the printed layer from decreasing over the long term, of providing excellent adhesion between the printed layer and the substrate, and of providing excellent flexibility of the printed layer.

[0063] Combination (1) Fluoroolefin: tetrafluoroethylene or chlorotrifluoroethylene Monomer having a hydroxyl group: hydroxyalkyl vinyl ether Non-fluorine-based monomer not having a hydroxyl group: at least one selected from the group consisting of cycloalkyl vinyl ether, alkyl vinyl ether, and vinyl carboxylic acid ester

[0064] Combination (2) Fluoroolefin: tetrafluoroethylene Monomer having a hydroxyl group: hydroxyalkyl vinyl ether Non-fluorine-based monomer not having a hydroxyl group: at least one selected from the group consisting of tert-butyl vinyl ether and vinyl carboxylic acid ester

[0065] Combination (3) Fluoroolefin: chlorotrifluoroethylene Monomer having a hydroxyl group: hydroxyalkyl vinyl ether Non-fluorine-based monomer not having a hydroxyl group: at least one selected from the group consisting of tert-butyl vinyl ether and vinyl carboxylic acid ester

[0066] The proportion of fluoroolefin units in copolymer (A) is preferably 30 to 70 mol %, more preferably 40 to 60 mol %, of all units (100 mol %) in copolymer (A). When the proportion of fluoroolefin units is equal to or greater than the lower limit of the above range, a printed layer with excellent weather resistance, stain resistance, etc. tends to be obtained. When the proportion of fluoroolefin units is equal to or less than the upper limit of the above range, the adhesion between the substrate and the printed layer tends to be even better.

[0067] The proportion of hydroxyl group-containing monomer units in copolymer (A) is preferably 0.5 to 20 mol %, more preferably 1 to 15 mol %, of all units in copolymer (A). When the proportion of hydroxyl group-containing monomer units is equal to or greater than the lower limit of the above range, the adhesion between the printed layer and the substrate tends to be even better. When the proportion of hydroxyl group-containing monomer units is equal to or less than the upper limit of the above range, the flexibility of the printed layer tends to be excellent.

[0068] The proportion of non-fluorine-based monomer units not having a hydroxyl group in copolymer (A) is preferably 20 to 60 mol %, more preferably 30 to 50 mol %, of all units in copolymer (A). When the proportion of these monomer units is equal to or greater than the lower limit of the above range, the flexibility of the printed layer tends to be excellent. When the proportion of these monomer units is equal to or less than the upper limit of the above range, the adhesion between the printed layer and the substrate tends to be even better.

[0069] The copolymer (A) is preferably an alternating copolymer of a fluoroolefin unit, a hydroxyl group-containing monomer unit, and a hydroxyl-free non-fluorine-containing monomer unit, in which case the printed layer tends to have excellent weather resistance.

[0070] Commercially available copolymers (A) include the Lumiflon (registered trademark) series (LF200, LF200MEK, LF100, LF710, LF600, etc.) (AGC Inc.), the Zeffle (registered trademark) GK series (GK-500, GK-510, GK-550, GK-570, GK-580, etc.) (Daikin Industries, Ltd.), the Fluonate (registered trademark) series (K-700, K-702, K-703, K-704, K-705, K-707, etc.) (DIC Corporation), and the ETERFLOON series (4101, 41011, 4102, 41021, 4261A, 4262A, 42631, 4102A, 41041, 41111, 4261A, etc.) (Eternal Examples include PEG-100 (manufactured by PEG-100 Chemical Co., Ltd.).

[0071] From the viewpoint of obtaining good adhesion, the hydroxyl value of the specific fluororesin is preferably from 10 to 150 mgKOH / g, more preferably from 15 to 120 mgKOH / g, still more preferably from 20 to 100 mgKOH / g, and particularly preferably from 20 to 50 mgKOH / g. The hydroxyl value of the fluororesin can be measured by Method A of ISO 14900:2001.

[0072] When the print layer contains a fluororesin as another resin, the content of the fluororesin is preferably 40 to 99 mass %, more preferably 45 to 98 mass %, based on the total mass of the print layer.

[0073] [(Meth)acrylic Resin] As the (meth)acrylic resin as the other resin, a known (meth)acrylic resin can be used. When a (meth)acrylic resin is used as the other resin contained in the printed layer, the printed layer has excellent adhesion to the substrate.

[0074] The (meth)acrylic resin preferably contains units derived from acrylic monomers such as alkyl(meth)acrylate, hydroxyl group-containing alkyl(meth)acrylate, carboxyl group-containing acrylic monomer, amide bond group-containing acrylic monomer, amino group-containing acrylic monomer, alkylene oxide group-containing acrylic monomer, aromatic ring-containing acrylic monomer, epoxy group-containing acrylic monomer, acrylic polyol, etc. The units derived from acrylic monomers may be used alone or in combination of two or more.

[0075] Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, methylcyclohexyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and octadecyl (meth)acrylate. Among these, methyl (meth)acrylate is preferred because it easily provides good adhesion to the substrate.

[0076] Examples of hydroxyl group-containing alkyl (meth)acrylates include hydroxyalkyl (meth)acrylate esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; glycol mono(meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and 1,4-cyclohexanedimethanol mono(meth)acrylate; caprolactone-modified (meth)acrylate; and hydroxyethyl acrylamide. Of these, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred.

[0077] Examples of carboxyl group-containing acrylic monomers include (meth)acrylic acid, monohydroxyethyl phthalate acrylate, p-carboxybenzyl acrylate, ethylene oxide-modified (number of moles added: 2 to 18) acrylate phthalate, monohydroxypropyl phthalate acrylate, monohydroxyethyl succinate acrylate, β-carboxyethyl acrylate, and 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate.

[0078] Examples of acrylic monomers containing an amide bond group include N-isopropyl(meth)acrylamide and N,N-diethylacrylamide.

[0079] Examples of the amino group-containing acrylic monomer include monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, and monoethylaminopropyl (meth)acrylate.

[0080] For example, examples of alkylene oxide group-containing acrylic monomers include 2-methoxyethyl acrylate, 2-ethoxyethyl acrylate, 2-phenoxyethyl acrylate, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenoxypolypropylene glycol (meth)acrylate.

[0081] Examples of aromatic ring-containing acrylic monomers include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0082] Examples of epoxy group-containing acrylic monomers include glycidyl (meth)acrylate, α-methylglycidyl acrylate, α-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl acrylate, and 3,4-epoxycyclohexylmethyl methacrylate.

[0083] The (meth)acrylic resin may have an acid value, and in this case, the acid value is preferably 20 mgKOH / g or less, more preferably 10 mgKOH / g or less. An acid value of 20 mgKOH / g or less can further improve the durability of the printed layer and the laminate. A method for imparting an acid value to the (meth)acrylic resin is to copolymerize an acrylic monomer having an acid value with another acrylic monomer. Examples of acrylic monomers having an acid value include (meth)acrylic acid, maleic anhydride, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, and 2-(meth)acryloyloxyethyl acid phosphate.

[0084] The glass transition temperature (Tg) of the (meth)acrylic resin is preferably 20 to 100° C., more preferably 30 to 90° C., and even more preferably 30 to 80° C. When the glass transition temperature is 20° C. or higher, blocking properties are improved, and when the glass transition temperature is 100° C. or lower, good adhesion is maintained.

[0085] The weight-average molecular weight (Mw) of the (meth)acrylic resin is preferably 3,000 to 300,000. By making the weight-average molecular weight 3,000 or more, pigment sedimentation can be suppressed, and both moldability and surface hardness can be achieved. By making the weight-average molecular weight 300,000 or less, a printing layer with good chemical resistance can be obtained.

[0086] The (meth)acrylic resin may be synthesized or commercially available. For example, an acrylic polyol may be the 6000 series manufactured by Taisei Fine Chemical Co., Ltd. Examples of homopolymers of acrylate monomers such as alkyl acrylate and alkyl methacrylate, and copolymers thereof with other monomers include Dianal solution type and Dianal beads type manufactured by Mitsubishi Chemical Corporation.

[0087] When the printing layer contains a (meth)acrylic resin as another resin, the content of the (meth)acrylic resin is preferably 40 to 99 mass %, more preferably 45 to 98 mass %, based on the total mass of the printing layer.

[0088] - Other Components - In addition to the components described above, the printing layer may contain additives such as anti-blocking agents, lubricants, curing agents, UV absorbers, anti-settling agents, plasticizers, dispersion stabilizers, fillers, antioxidants, antistatic agents, matting agents (silica, alumina, etc.), tack improvers (polyolefins, etc.), adhesion improvers (silane coupling agents, etc.), etc. Furthermore, the printing layer may contain solvents (solvents, water, etc.), curing agents, etc., contained in the ink used to form the printing layer.

[0089] [Anti-blocking agent] When the printed layer contains an anti-blocking agent, the problem of printed surfaces coming into contact with each other and adhering to each other when the laminate of the present disclosure is spread can be effectively avoided. Note that if the blocking temperature of the printed layer itself exceeds 45°C, it may not be necessary to add an anti-blocking agent.

[0090] Examples of anti-blocking agents include silicon compounds, chlorinated polyethylene, (meth)acrylic resin beads, and esterified cellulose resins. Among these, esterified cellulose resins are preferred. Examples of esterified cellulose resins include cellulose acetate resin, cellulose acetate butyrate (CAB) resin, and cellulose acetate propionate (CAP) resin. CAP is generally obtained by triesterifying cellulose with acetic acid and propionic acid, followed by hydrolysis. CAB is also obtained by triesterifying cellulose with acetic acid and butyric acid, followed by hydrolysis. The esterified cellulose resin is preferably at least one selected from the group consisting of CAB and CAP. The esterified cellulose resin may be used alone or in combination with two or more. When the printing layer contains an esterified cellulose resin, adhesion between the printing layer and the functional layer, as described below, tends to be improved when the functional layer is provided. One of the reasons for this is thought to be that the esterified cellulose resin present on the surface of the printing layer is partially dissolved or compatible with the components in the functional layer.

[0091] When the printing layer contains an anti-blocking agent, the content of the anti-blocking agent is preferably 0.5 to 20 mass %, and more preferably 1 to 10 mass %, relative to the total mass of the printing layer. When the content is equal to or greater than the lower limit, the anti-blocking effect is exerted, and when the content is equal to or less than the upper limit, initial poor adhesion to the substrate tends to be suppressed.

[0092] [Lubricant] Examples of lubricants include various waxes such as polyolefin waxes such as polyethylene wax, fatty acid amides, fatty acid esters, paraffin wax, polytetrafluoroethylene (PTFE) wax, carnauba wax, etc. When the printing layer contains a lubricant, the content of the lubricant can be adjusted as appropriate and is, for example, preferably 0.05 to 3 mass %, and more preferably 0.2 to 1 mass %, relative to the total mass of the printing layer.

[0093] [UV Absorber] Examples of the UV absorber include inorganic UV absorbers, organic UV absorbers, etc. Examples of the organic UV absorber include triazine-based UV absorbers and benzophenone-based UV absorbers, with triazine-based UV absorbers being preferred. Among these, hydroxyphenyltriazine-based UV absorbers such as 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (manufactured by BASF Japan Ltd., trade name: TINUVIN 479), 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (manufactured by BASF Japan Ltd., trade name: TINUVIN 460), and 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyloxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (manufactured by BASF Japan Ltd., trade name: TINUVIN 405) are preferred. When the printed layer contains a UV absorber, the content of the UV absorber can be appropriately adjusted. For example, the total content of the UV absorber and pigment is preferably 1 to 15% by mass, and more preferably 2 to 10% by mass, relative to the total mass of the printed layer.

[0094] [Curing Agent] When the printed layer contains a curing agent, improvements in water resistance, solvent resistance, and blocking resistance tend to be observed. On the other hand, if the printed layer does not contain a curing agent, the printed layer is easily removed with an alkaline solution. Therefore, it is preferable that the printed layer does not contain a curing agent, or if it does contain a curing agent, it contains only a small amount. The curing agent can be appropriately selected from curing agents known as curing agents for paints. Specific examples include isocyanate-based curing agents, blocked isocyanate-based curing agents, aminoplast-based curing agents, polycarboxylic acid-based curing agents, and polyamine-based curing agents. The curing agent is preferably selected taking into consideration the type of curing reactive site possessed by the fluororesin, curing characteristics, etc. As the curing agent, isocyanate-based curing agents, blocked isocyanate-based curing agents, or aminoplast-based curing agents are preferred. One type of curing agent may be used alone, or two or more types may be used in combination.

[0095] [Solvent] Any solvent capable of dissolving or dispersing resins, pigments, etc. may be used, and may be appropriately selected depending on the application method, taking into consideration the repellency of the coating on the substrate, transfer rate, drying properties, storage stability, etc. Examples of solvents include aqueous solvents and organic solvents, and these may be used alone or in combination of two or more. Examples of organic solvents include toluene, xylene, ethylbenzene, methyl ethyl ketone, ethyl acetate, isopropyl alcohol, etc. In gravure printing, a solvent that gives the ink a No. 3 Zahn Cup viscosity of 15 to 30 seconds is preferred to reduce printing defects such as uneven application and bleeding. When forming a printed layer by an inkjet method, a high-boiling point solvent may also be added to prevent the ink outlet from drying out.

[0096] (Configuration, physical properties, etc. of laminate) In the laminate of the present disclosure, the printed layer may be provided over the entire surface of one side of the substrate, or may be provided over a portion of the surface. Furthermore, the printed layer may be provided on one side of the substrate, or on both sides.

[0097] The ratio of the area of ​​the printed layer to the total area of ​​one surface of the substrate may be appropriately selected depending on the purpose, etc., and may be, for example, 10 to 100%, or may be less than 95%, less than 90%, or less than 80%. Furthermore, the ratio of the area of ​​the printed layer to the total area of ​​one surface of the substrate may be 80% or more, 90% or more, or 95% or more.

[0098] The printed layer may be one layer or two or more layers. The thickness of the printed layer (total thickness when two or more layers are present) is preferably 0.5 to 10 μm, more preferably 1 to 6 μm. When the thickness of the printed layer is equal to or less than the upper limit of the above range, the printed layer can follow deformation of the substrate such as expansion, contraction, bending, etc., and tends to be less likely to peel off from the substrate. When the thickness of the printed layer is equal to or greater than the lower limit of the above range, the printed layer is not too thin and has an excellent effect of reducing solar radiation transmittance, etc.

[0099] The laminate may further include layers other than the substrate and the printed layer. For example, the laminate may further include a functional layer on the printed layer. The functional layer can be formed by coating, transfer using a transfer film, sputtering, or the like. The functional layer may include one layer or two or more layers. In the present disclosure, the functional layer refers to a layer that imparts a desired function to the laminate. Examples of the desired function imparted to the laminate include design, optical properties (ultraviolet absorption, ultraviolet reflectivity, near-infrared absorption, near-infrared reflectivity, etc.), durability, etc. Components of the functional layer include the aforementioned pigments, UV absorbers, near-infrared absorbing pigments, near-infrared reflective pigments, curing agents, etc. The laminate may also include an adhesive layer between the substrate and the printed layer, or between the printed layer and any other layer. Examples of the adhesive layer include a layer formed by applying a silane coupling agent.

[0100] The solar reflectance of the laminate of the present disclosure is preferably 20% or more, more preferably 40% or more, and is preferably 90% or less, more preferably 80% or less.

[0101] When the laminate of the present disclosure is used as a membrane material for roofs, walls, etc., it is constantly deforming and recovering due to deformation of the film caused by snow load, vibration caused by wind, stamping caused by raindrops, etc. It is desirable that the printed layer provided on such a laminate have high adhesion so that it does not peel off even when the substrate is deformed. It is also expected that the printed layer will be wetted with water for a long time due to condensation or rain blown in by wind. Therefore, it is desirable that the laminate has excellent durability when exposed to water (retention of adhesion, maintenance of solar reflectance, etc.). From this perspective, the solar reflectance retention rate of the laminate after the 80°C steam test described in the examples is preferably 85% or more, more preferably 90% or more, and even more preferably 92% or more. The upper limit of the solar reflectance retention rate after the 80°C steam test is 100%. Furthermore, it is preferable that the laminate has high resistance to outdoor ultraviolet rays. From this perspective, the solar reflectance retention rate of the laminate after the accelerated weathering test described in the examples is preferably 85% or more, more preferably 90% or more, and even more preferably 91% or more. The upper limit of the solar reflectance maintenance rate after the accelerated weather resistance test is 100%.

[0102] <Method for manufacturing laminate> The method for manufacturing the laminate of the present disclosure is not particularly limited. For example, the laminate may be obtained by applying an ink containing an alkali-soluble resin and a pigment to at least a portion of a film containing a fluororesin. The ink may be in the form of a solution, a dispersion, a varnish, or the like. The printed layer may be a coated layer obtained by applying the ink to a substrate, or may be an ink layer obtained by drying the ink as needed to remove at least a portion of the solvent, or may even be a cured layer obtained by curing the ink by heating or the like.

[0103] The ink components preferably contain other resins in addition to the alkali-soluble resin and pigment, and may further contain other components such as a solvent. When the ink contains a solvent, the content of the solvent is preferably 30 to 90% by mass, and more preferably 40 to 80% by mass, based on the total mass of the ink.

[0104] The method for applying the ink to the substrate is not particularly limited, and examples include the following methods: - A method in which the ink is applied to the substrate by a known application method such as gravure printing, screen printing, pad printing, inkjet, brush coating, spray coating, or die coating - A method in which a transfer film having a printing layer is used, and the printing layer on the transfer film is transferred to the substrate by a heated roll or the like As a method for applying the ink to the substrate, from the viewpoints of accuracy of alignment, productivity, etc., gravure printing, screen printing, pad printing, and inkjet methods are preferred, and gravure printing is more preferred.

[0105] In the coating method, methods for removing the solvent after applying the ink to the substrate include heat drying, reduced-pressure drying, and heat-and-reduced-pressure drying. In the case of heat drying or heat-and-reduced-pressure drying, the heating temperature is preferably 30 to 150° C., and more preferably 60 to 120° C. Drying may be carried out once or multiple times.

[0106] When the ink is a resin composition containing a curing agent, the ink may be cured by heating at, for example, 40 to 80° C. to form a printed layer.

[0107] The surface of the printing layer may be subjected to a surface treatment to improve adhesion, taking into consideration the formation of a functional layer thereon, which will be described later. Examples of the surface treatment include the same treatments as those that can be applied to the substrate.

[0108] <Method for producing recycled film> In one embodiment of the method for producing a recycled film of the present disclosure, the laminate of the present disclosure is impregnated with an alkaline solution to remove the printed layer, thereby obtaining a recycled film containing a fluororesin. Since the printed layer of the laminate of the present disclosure can be easily removed with the alkaline solution, the film containing the fluororesin can be easily removed from the laminate of the present disclosure. This manufacturing method is particularly useful when reusing the substrate in the form of a film contained in the laminate.

[0109] In another embodiment of the method for producing a recycled film according to the present disclosure, the laminate according to the present disclosure is immersed in an alkaline solution to remove the printed layer, thereby obtaining a film containing a fluororesin. The obtained film containing a fluororesin is then melted and molded to obtain a recycled film containing a fluororesin. The film may be melted and formed into pellets, which may then be molded. In this embodiment of the method, the film can be processed into a film of a different shape than the film contained in the laminate and reused.

[0110] The pH of the alkaline solution used to remove the printed layer from the laminate is preferably 10 to 14, and more preferably 10 to 13. Specific examples of the alkaline solution include an aqueous solution of sodium hydroxide and an aqueous solution of potassium hydroxide. The alkaline solution may be heated before use, for example, to 70 to 90°C.

[0111] The laminate may be cut and then impregnated in an alkaline solution. Alternatively, the printed layer may be removed from the laminate, and then the fluororesin-containing film may be cut. The cut size and shape are not particularly limited. After the printed layer is removed from the laminate, the resulting fluororesin-containing film may be washed with water and dried.

[0112] The recycled film obtained by the manufacturing method of the present disclosure is suppressed in black defects and discoloration due to the printed layer. Furthermore, the obtained film containing a fluororesin may be reused in the laminate of the present disclosure or may be used for other purposes.

[0113] The decrease in visible light transmittance of the recycled film depends on the thickness, but is preferably within 2%, more preferably within 1%, of an unrecycled film of the same thickness that does not have a printed layer. The method for measuring visible light transmittance is as described in the Examples. In the Examples, the visible light transmittance of the 250 μm film before printing is 91%, so the visible light transmittance of the recycled film in this case is preferably 89% or more. A small decrease in visible light transmittance indicates that coloration is suppressed.

[0114] The change in stress of the recycled film at 10% elongation varies slightly depending on the thickness of the film to be molded, but a change of ±2 MPa or less is preferable, and a change of ±1 MPa or less is even more preferable, compared to an unrecycled film of the same thickness that does not have a printed layer. In the example, the stress of a 250 μm film before printing at 10% elongation is 21 MPa, so in this case, the stress of the recycled film at 10% elongation is preferably 19 MPa or more. Furthermore, 20 MPa or more is even more preferable.

[0115] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure. Examples 2 to 4, 6 to 9, and 11 to 13 are working examples, and Examples 1, 5, and 10 are comparative examples.

[0116] <Ink Preparation> The inks of Examples 1 to 13 were prepared by incorporating the components shown in Table 1 below in the formulations (parts by mass) shown in Table 1. The viscosity of the inks of Examples 1 to 13 was 24 to 25 seconds using a No. 3 Zahn cup. The components are as follows:

[0117] [Aluminum Paste 1] EMR-D5660 (trade name, manufactured by Toyo Aluminum K.K.) was used as aluminum paste 1. This aluminum paste contained 49.5 mass% of aluminum composite particles 1 in which the surfaces of flat aluminum particles were coated with 25 mass% of silica relative to 100 mass% of aluminum, and 50.5 mass% of propylene glycol monomethyl ether as a solvent. The average major axis of these aluminum composite particles 1 was 9 μm.

[0118] [Aluminum Paste 2] BP-280PA (trade name, manufactured by Toyo Aluminum K.K.) was used as aluminum paste 2. This aluminum paste contained 50 mass% of aluminum composite particles 2 in which the surfaces of flat aluminum particles were coated with 12 mass% (meth)acrylic resin relative to 100 mass% of aluminum, and 50 mass% of n-propyl acetate as a solvent. The average major axis of these aluminum composite particles 2 was 9 μm.

[0119] [Aluminum Paste 3] EMR-D6390 (trade name, manufactured by Toyo Aluminum K.K.) was used as the aluminum paste 3. This aluminum paste contained 54.5 mass% of aluminum composite particles 3 in which the surfaces of flat aluminum particles were coated with 34.5 mass% of silica relative to 100 mass% of aluminum, and 45.5 mass% of propylene glycol monomethyl ether n-propyl acetate as a solvent. The average major axis of these aluminum composite particles 3 was 9 μm.

[0120] [Aluminum Paste 4] EMR-D4690 (trade name, manufactured by Toyo Aluminum K.K.) was used as aluminum paste 4. This aluminum paste contains 50 mass% of aluminum composite particles 4 in which the surfaces of flat aluminum particles are coated with 37 mass% of silica relative to 100 mass% of aluminum, and 50 mass% of propylene glycol monomethyl ether as a solvent. The average major axis of these aluminum composite particles 4 is 9 μm.

[0121] [Fluororesin Varnish] LF200MEK (manufactured by AGC Inc., solid content: 60 mass%, solvent: methyl ethyl ketone, hydroxyl value: 31 mg (KOH) / g) was used as the fluororesin varnish. The resin of LF200MEK (specific fluororesin) is an alternating copolymer of fluoroethylene and vinyl ether, and contains units derived from hydroxyalkyl vinyl ether.

[0122] [(Meth)acrylic Resin Varnish] As a (meth)acrylic resin, Dianal BR115 (manufactured by Mitsubishi Chemical Corporation, (meth)acrylic resin, Tg 48°C, acid value 0 mgKOH / g, weight average molecular weight 5000) was dissolved in ethyl acetate, and an ethyl acetate solution with a solid content of 40 mass% was used as a (meth)acrylic resin varnish.

[0123] [Anti-blocking agent solution] An esterified cellulose resin (trade name: CAB-381-2, manufactured by Eastman Chemical Japan, glass transition point 133°C, number average molecular weight 40,000, hydroxyl group content 1.3% by mass) was used as the anti-blocking agent. This resin was dissolved in methyl ethyl ketone (MEK) to prepare an anti-blocking agent solution with a solids concentration of 20% by mass.

[0124] [Alkali-soluble resin liquid 1] A styrene-maleic anhydride copolymer resin (product name: SMA17352P, manufactured by Kawahara Oil Chemical Co., Ltd., weight average molecular weight: 7000, acid value: 270 mg KOH / g, soluble in an amount of 0.1 g or more in 100 mL of 1.5 mass % aqueous sodium hydroxide solution at 85°C) was used as the alkali-soluble resin 1. This was dissolved in MEK to prepare alkali-soluble resin liquid 1 with a solid content of 20 mass %.

[0125] [Alkali-soluble resin liquid 2] A styrene-acrylic acid copolymer resin (trade name: Joncryl 682: manufactured by BASF, weight average molecular weight 1750, acid value: 238 mg KOH / g, soluble in an amount of 0.1 g or more in 100 mL of 1.5 mass % aqueous sodium hydroxide solution at 85°C) was used as the alkali-soluble resin 2. This was dissolved in ethyl acetate (EA) to prepare alkali-soluble resin liquid 2 with a solid content of 50 mass %.

[0126] [Curing Agent] A polyisocyanate of hexamethylene diisocyanate (trade name: Duranate A201H, manufactured by Asahi Kasei Corporation) was used as the curing agent. The NCO content of this curing agent was 17.2% by mass.

[0127] [Dilution Solvent] A mixed solvent of MEK and toluene (MEK:toluene=50:50 (by mass)) was used as the dilution solvent.

[0128] <Production of Laminate> A 250 μm ETFE film (manufactured by AGC Inc., product name: Fluon ETFE Film 250NJ, fluorine atom content of ETFE is 46% by mass, ETFE content is 100% by mass, stress at 10% elongation is 21 MPa, total light transmittance is 92.0%) was applied to the surface of the film at 150 W·min / m in air. 2The corona discharge treatment was carried out at a treatment density of 0.054 N / m. The surface tension of the corona discharge treated surface was 0.054 N / m. Subsequently, the prepared ink was printed by gravure printing on the corona discharge treated surface of the ETFE film, and dried at 120°C for 1 minute. The gravure printing plate had a dot design with a diameter of 16 mm, and the printing area ratio was 58%. The mass of the printing layer per unit area of ​​the substrate was 1.4 g / m. 2 ~1.6g / m 2 The thickness of the printed layer was 2 μm.

[0129] <Evaluation> The initial physical properties of the obtained laminate were measured for solar reflectance, evaluated for adhesion by a peel test, and evaluated by an alkali elimination test. Furthermore, the laminate was subjected to an accelerated weathering test, and then the solar reflectance retention rate was measured, the adhesion strength was evaluated by a peel test, and the alkali elimination test was also performed. Furthermore, the laminate was subjected to an 80°C steam test, and then the solar reflectance retention rate was measured, and the adhesion strength was evaluated by a peel test. A recycled film was then produced from the obtained laminate, and the visible light transmittance and stress at 10% elongation of this recycled film were measured. The respective measurement and evaluation methods were as follows. The results are shown in Table 2.

[0130] (Solar reflectance) The solar reflectance was measured using a spectrophotometer (UV-3100PC, manufactured by Shimadzu Corporation) in accordance with JIS R3106:1998 ("Test methods for transmittance, reflectance, emissivity, and solar heat gain coefficient of plate glass"). These optical properties were measured by irradiating light from the substrate side.

[0131] (Peel test) In accordance with JIS K5600-5-6:1999, 10 x 10 lattice cuts of 1 mm squares were made in a printed layer formed on a substrate (100 squares in total), and Cellophane Tape (registered trademark) (manufactured by Nichiban Co., Ltd.: product name CT18) was attached, and then the tape was peeled off. The number of peeled squares out of the 100 squares was counted, and the adhesion strength was evaluated according to the following criteria. A rating of A or B was considered to be acceptable. A (excellent): 0 or more squares but less than 2 squares peeled off. B (good): 2 or more squares but less than 20 squares peeled off. C (poor): 20 or more squares peeled off.

[0132] (Alkali Desorption Test) The laminate was cut into a piece of 5 cm x 30 cm, immersed in a 1% by mass aqueous solution of sodium hydroxide (pH: 13.2) at 85°C, and stirred for 20 minutes. The state of desorption of the printed layer was observed and evaluated according to the following criteria. An evaluation result of A was considered to be pass. A (Good): The entire printed layer was desorbed. B (Bad): At least a part of the printed layer remained.

[0133] (Accelerated Weathering Test) The laminate was subjected to an accelerated weathering test using an accelerated weathering tester (for example, manufactured by Iwasaki Electric Co., Ltd., trade name: Eye UV Tester SUV-W231) at a wavelength of 300 to 450 nm and an intensity of 1500 mW / cm. 2 The test piece was exposed to ultraviolet light for 500 hours (one cycle lasting 12 hours and 20 seconds), with the cycle consisting of (i) 10 hours of ultraviolet light irradiation at a black panel (BP) temperature of 63°C and a relative humidity of 50%RH, (ii) a 10-second shower, (iii) 2 hours of dark condensation at a BP temperature of 30°C and a relative humidity of 100%RH, and (iv) a 10-second shower. The cumulative ultraviolet light dose under these conditions was 2,400 MJ / m. 2 The annual UV dose in Choshi City, Japan is approximately 250 MJ / m 2 This is equivalent to approximately 10 years of outdoor exposure.

[0134] (80°C steam test) A water tank with water temperature maintained at 80°C was placed indoors at 23°C, and the top of the water tank was covered with the laminate. At this time, the printed layer of the laminate was placed on the inside (the water side of the water tank). In this state, exposure was carried out for 5 days.

[0135] (Solar reflectance maintenance rate after accelerated weather resistance test) The solar reflectance was measured before and after the accelerated weather resistance test, and the solar reflectance maintenance rate was calculated and evaluated according to the following criteria. An evaluation result of A was judged to be pass. A (good): Solar reflectance maintenance rate of 85% or more B (poor): Solar reflectance maintenance rate of less than 85%

[0136] (Solar reflectance maintenance rate after 80°C steam test) The solar reflectance was measured before and after the 80°C steam test, and the solar reflectance maintenance rate was calculated and evaluated according to the following criteria. An evaluation result of A was judged to be pass. A (good): Solar reflectance maintenance rate of 85% or more B (poor): Solar reflectance maintenance rate of less than 85%

[0137] (Production and Evaluation of Recycled Film) The laminate was cut into a piece of 5 cm x 30 cm and immersed in a 1% by mass aqueous solution of sodium hydroxide at 85°C for 20 minutes to remove the printed layer. The obtained substrate was taken out, washed with water and dried.

[0138] The obtained substrate was placed in a 15 mm diameter co-rotating twin-screw extruder (manufactured by Technovel Co., Ltd.), and the cylinder and head temperatures were set to 280°C to obtain pellets with a diameter of 2 mm and a length of 3 mm. The extrusion rate was 2 kg / h. The obtained pellets were extruded into a 250 μm thick recycled film using a 30 mm single-screw extruder equipped with a 150 mm wide T-die at the tip.

[0139] The visible light transmittance and stress at 10% elongation of the recycled film were measured. The stress at 10% elongation was measured in accordance with JIS K7127:1999 (Plastics - Test methods for tensile properties - Part 3: Test conditions for films and sheets) at a pulling rate of 200 mm / min. Type V test specimens with a gauge length of 25 mm were used for the stress at 10% elongation.

[0140] The visible light transmittance of the virgin ETFE film having a thickness of 250 μm used as the raw material for the laminate was 91%, and the stress at 10% elongation was 21 MPa, so the recycled film was evaluated according to the following criteria.

[0141] - Visible light transmittance of recycled film - A (good): 89% or more B (poor): less than 89%

[0142] - Stress of recycled film at 10% elongation - A (good): 19 MPa or more B (bad): Less than 19 MPa

[0143]

[0144]

[0145] <Discussion> [Example 1] The initial solar reflectance was 58.6%. The peel test results were judged to be pass, with not a single square peeling. In the alkali desorption test, no desorption occurred after 20 minutes of immersion and agitation. Furthermore, after 500 hours of accelerated weathering testing, the solar reflectance was 58.0%, and the solar reflectance retention rate was 99%. The peel test after the accelerated weathering testing was pass, with not a single square peeling. However, in the alkali desorption test after the accelerated weathering testing, no ink was desorbed. Furthermore, after an 80°C steam exposure test, the solar reflectance retention rate was 92%, with not a single square peeling, also passing. The peel test also passed. The visible light transmittance of the recycled film was 86%, and it was clearly colored brown. Furthermore, holes were observed in the recycled film, likely due to gas generation. The stress at 10% elongation of the recycled film was 16.2 MPa, which did not meet the 19 MPa requirement and therefore failed. Because the ink was not sufficiently removed by the alkaline solution, the recycled film had insufficient visible light transmittance and mechanical properties.

[0146] [Example 2] The initial solar reflectance was 56.6%. The peel test results were good, with not a single square peeling. In the alkali desorption test, the printed layer completely peeled off after 20 minutes of immersion and agitation. Furthermore, the solar reflectance retention rate after a 500-hour accelerated weathering test was 99%. The peel test after the accelerated weathering test passed, with not a single square peeling off. Furthermore, in the alkali desorption test after the accelerated weathering test, the ink was completely desorbed. Furthermore, the solar reflectance retention rate after an 80°C steam exposure test was 92%, and the peel test also passed, with not a single square peeling off. The visible light transmittance of the recycled film was 90%, and no coloring was observed. The stress at 10% elongation of the recycled film was 20.8 MPa, which exceeded 19 MPa and therefore passed. The ink was sufficiently removed by alkaline hot water, and it was determined that the mechanical properties and visible light transmittance of the recycled film were comparable to those of the virgin ETFE film used as the raw material for the laminate.

[0147] [Examples 3 and 4] Examples 3 and 4, in which the alkali-soluble resin contents were 3.4% by mass and 10.9% by mass, respectively, showed good results in solar reflectance, peel test, alkali desorption test, etc., initially, after an accelerated weathering test, and after an 80°C steam test. Furthermore, it was found that the recycled films of Examples 3 and 4 had little coloring and also maintained sufficient mechanical properties.

[0148] [Example 5] In the case of Example 5, in which the content of alkali-soluble resin was 16.1% by mass, problems were observed in the solar reflectance retention rate after an accelerated weather resistance test, the reflectance retention rate after a steam test at 80°C, and the peel test. It was found that the recycled film of Example 5 had little coloring and also maintained sufficient mechanical properties.

[0149] [Example 6] The solar reflectance or solar reflectance retention rate, peel test, and detachment test showed good results initially, after an accelerated weathering test, and after a steam test at 80°C. Furthermore, the recycled film showed little coloring and maintained sufficient mechanical properties.

[0150] [Examples 7 to 9] Examples 7 to 9 showed good results in solar reflectance, solar reflectance retention, peel test, and detachment test, initially, after an accelerated weathering test, and after an 80°C steam test. Furthermore, the recycled films showed little discoloration and maintained sufficient mechanical properties. It was also found that the recycled films of Examples 7 to 9 showed little discoloration and maintained sufficient mechanical properties.

[0151] [Example 10] In the case of Example 10, in which the alkali-soluble resin content was 18.3% by mass, defects were observed in the solar reflectance retention rate after an accelerated weathering test and in the peel test, and in the solar reflectance retention rate after a steam test at 80°C and in the peel test. It was found that the recycled film of Example 10 had little coloring and also maintained sufficient mechanical properties.

[0152] [Example 11] The solar reflectance, solar reflectance retention, peel test, and detachment test showed good results initially, after the accelerated weathering test, and after the 80°C steam test. Furthermore, the recycled film showed little coloring and maintained sufficient mechanical properties.

[0153] [Example 12] The solar reflectance, solar reflectance retention, peel test, and detachment test showed good results initially, after the accelerated weathering test, and after the 80°C steam test. Furthermore, the recycled film showed little coloring and maintained sufficient mechanical properties.

[0154] [Example 13] The solar reflectance, solar reflectance retention, peel test, and detachment test showed good results initially, after the accelerated weathering test, and after the 80°C steam test. Furthermore, the recycled film showed little coloring and maintained sufficient mechanical properties.

[0155] The laminate of the present disclosure has excellent weather resistance and can be suitably used outdoors. The use of the laminate of the present disclosure is not particularly limited, but it is suitably used as a roofing material, a wall covering material, and a display material. Specifically, it can be used as a membrane material (roofing material, exterior wall material, skylight, waterproof sheet, protective sheet, etc.) in membrane structure facilities (sports facilities (swimming pools, gymnasiums, tennis courts, soccer fields, athletics stadiums, etc.), warehouses, assembly halls, exhibition halls, horticultural facilities (horticultural greenhouses, agricultural greenhouses, etc.), arcades, etc.); membrane material for screens; soundproof walls; windbreak fences; overtopping fences; highway side walls; garage canopies; membrane material for shopping malls; walkway walls; glass shatterproof film; heat-resistant sheet; water-resistant sheet; tent material for tent warehouses; membrane material for adjusting solar radiation; light Examples of suitable applications include partial roofing materials for removal, window materials as an alternative to glass, membrane materials for fire-retardant partitions, curtains, membrane materials for reinforcing exterior walls, waterproof membranes, smoke-proof membranes, non-flammable transparent partitions, membrane materials for reinforcing roads, interiors (lighting, walls, brands, etc.), exteriors (tents, signs, etc.), automotive materials (canopies, vibration-damping materials, bodies, etc.), aircraft materials, ship materials, exteriors for home appliances, tanks, filters, membrane materials for construction work, etc. In one embodiment, the laminate of the present disclosure is particularly suitable for use as a membrane material for membrane structure facilities, screens, signs, or for adjusting solar radiation.

Claims

1. A laminate comprising: a film containing a fluororesin; and a printed layer containing an alkali-soluble resin and a pigment on at least a portion of the film, wherein the content of the alkali-soluble resin is 1.0 to 15.0 mass % relative to the total mass of the printed layer.

2. The laminate according to claim 1, wherein the printed layer further contains at least one resin selected from the group consisting of fluororesins and (meth)acrylic resins.

3. The laminate according to claim 2, wherein the fluororesin in the printed layer is a copolymer having a fluoroolefin unit and a monomer unit having a hydroxyl group.

4. The laminate according to claim 1 or 2, wherein the alkali-soluble resin has an acid value of 100 to 500 mgKOH / g.

5. The laminate according to claim 1 or 2, wherein the pigment is an aluminum composite particle coated with a (meth)acrylic resin or silica.

6. The laminate according to claim 1 or 2, which is used outdoors.

7. The laminate according to claim 1 or 2, which is at least one material selected from the group consisting of roofing materials, wall covering materials, and display materials.

8. A method for producing a recycled film, comprising the steps of: immersing the laminate according to claim 1 or 2 in an alkaline solution to remove the printed layer, thereby obtaining a recycled film containing a fluororesin.

9. A method for producing a recycled film, comprising the steps of: immersing the laminate according to claim 1 or 2 in an alkaline solution to remove the printed layer, obtaining a film containing the fluororesin; and melting and molding the obtained film containing the fluororesin to obtain a recycled film containing the fluororesin.

Citation Information

Patent Citations

  • Recycling of fluororesin film

    JP1999323008A

  • Laminated film

    JP2004142305A

  • Method for manufacturing laminate

    JP2012076079A

  • Laminated article and method for manufacturing same

    WO2016175058A1

  • Packaging material, recycled molding material, and methods for manufacturing same

    WO2023032997A1

Cited By

  • Resin composition, liquid composition, laminate, and method for removing printed layer

    JP2026165915A

  • Resin composition, liquid composition, laminate, and method for removing printed layer

    JP7777710B1