Crosslinked product, hydrogel and method for producing same, molded body, and film and method for producing same
Crosslinking high molecular weight polymers with tannic acid enables the creation of materials with self-healing and shape memory properties, addressing the limitations of existing smart material synthesis methods by producing strong, moldable, and eco-friendly hydrogels and films for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/016076
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Current methods for obtaining smart materials with self-healing and shape memory properties often require complex chemical synthesis, generating waste and being unable to be molded, and lack self-repair and shape memory abilities.
A crosslinked product is created by combining a high molecular weight polymer with tannic acid, allowing for easy synthesis, molding, and achieving extensibility, self-healing, and shape memory properties, along with methods for producing hydrogels and films containing these crosslinked products.
The resulting materials exhibit strong tensile and bending stresses, high elongation, self-healing, and shape memory abilities, with minimal waste generation and the ability to be molded into various shapes, suitable for applications in agriculture and medicine.
Smart Images

Figure JP2024016076_31102024_PF_FP_ABST
Abstract
Description
Crosslinked product, hydrogel and its manufacturing method, molded product, and film and its manufacturing method
[0001] The present invention relates to a crosslinked product. The present invention also relates to a hydrogel containing the crosslinked product and a method for producing the same. The present invention also relates to a molded article containing the crosslinked product. The present invention also relates to a film containing the crosslinked product and a method for producing the same.
[0002] Hydrogels are soft materials that contain a large amount of water within a three-dimensional network structure formed by crosslinking hydrophilic polymer chains. Due to their excellent biocompatibility, water absorption, self-healing properties, and extensibility (stretchability), they are widely used in agriculture, food, tissue engineering, and biomedicine. For example, hydrogels have been put to practical use as wound dressings and hemostatic agents, and are also widely used in drug delivery.
[0003] Recently, smart materials with self-repairing and shape-memory properties have been attracting attention, and they can be used in a wide range of applications, such as molecular actuators and paints. Hydrogels have also been attracting attention as such smart materials (e.g., Non-Patent Document 1).
[0004] Meanwhile, tannic acid (TA) has been attracting attention in the medical field, etc. For example, it has been reported that a TA-based supramolecule, TA, can be mixed with polyethylene glycol (PEG) with a molecular weight of 10 kDa or less to form a viscous adhesive through hydrogen bonding between PEG and TA (Non-Patent Documents 2 and 3).
[0005] Advanced Materials, 2016, Vol.28, p.9060-9093Advanced Functional Materials, 2015, Vol.25, p.2402-2410Journal of Visualized Experiments, 2016, 111, 53930
[0006] However, currently, obtaining smart materials often requires chemical synthesis of constituent materials with complex structures, and chemical synthesis generates a large amount of waste, including organic solvents.
[0007] Furthermore, Non-Patent Documents 2 and 3 aim to use a supramolecule consisting of TA and low-molecular-weight PEG as an adhesive, and do not consider self-repairing or shape-memory capabilities, as they are used in a highly fluid state and cannot be molded.
[0008] Under these circumstances, an object of the present invention is to provide a crosslinked product of a high-molecular-weight polymer and tannic acid that can be easily synthesized, molded into any shape, and used to form a material with extensibility, self-repairing properties, and shape memory. Another object of the present invention is to provide a hydrogel, a molded article, and a film containing the crosslinked product of a high-molecular-weight polymer and tannic acid, as well as methods for producing these.
[0009] Another object of the present invention is to provide a plant life-extending agent that can prolong the life of plants.
[0010] The present inventors have conducted extensive research to solve the above problems and have found that the following inventions meet the above objectives, thereby completing the present invention.
[0011] <1> A crosslinked product obtained by crosslinking a high-molecular-weight polymer with tannic acid, wherein the high-molecular-weight polymer has a structural unit containing a group G capable of forming a hydrogen bond with tannic acid and has a weight-average molecular weight of 50 kDa or more. <2> The crosslinked product according to <1>, wherein the molar ratio of tannic acid to the structural unit is 0.02 to 0.1. <3> The crosslinked product according to <1> or <2>, wherein the high-molecular-weight polymer is one or more selected from the group consisting of polyalkylene oxide, polyalkylene oxide copolymer, polyvinyl alcohol, and polyvinyl alcohol copolymer. <4> A hydrogel comprising the crosslinked product according to any one of <1> to <3> and water. <5> The hydrogel according to <4>, wherein the maximum tensile stress is 0.05 MPa or more. <6> The hydrogel according to <4> or <5>, wherein the breaking elongation is 500% or more. <7> The hydrogel according to any one of <4> to <6>, having a swelling ratio of 100% to 120%. <8> The hydrogel according to any one of <4> to <7>, having a maximum bending stress of 10 MPa or more when dried at 40°C for 8 days. <9> The hydrogel according to any one of <4> to <8>, having a self-repairing ability when heated when dried at 40°C for 8 days. <10> The hydrogel according to any one of <4> to <9>, having a shape-memory ability when dried at 40°C for 8 days. <11> A molded article comprising the crosslinked product according to any one of <1> to <3>. <12> A film comprising the crosslinked product according to any one of <1> to <3>, and having a breaking elongation of 500% or more. <13> A method for producing a hydrogel, comprising: a gelation step of mixing an aqueous solution containing a high-molecular-weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high-molecular-weight polymer with tannic acid; and a gel recovery step of recovering a hydrogel containing the crosslinked product from the crosslinked product-containing solution, wherein the high-molecular-weight polymer used is a polymer having a constitutional unit including a group G capable of forming a hydrogen bond with tannic acid and having a weight-average molecular weight of 50 kDa or more.<14> A method for producing a film, comprising: a gelation step of mixing an aqueous solution containing a high-molecular-weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high-molecular-weight polymer with tannic acid; a liquid recovery step of separating the crosslinked product-containing solution into a hydrogel containing the crosslinked product and a liquid component, and then recovering the liquid component; and a film-forming step of drying the liquid component to obtain a film, wherein the high-molecular-weight polymer is a polymer having a structural unit including a group G capable of forming a hydrogen bond with tannic acid and a weight-average molecular weight of 50 kDa or more. <15> A plant life-extending agent comprising the hydrogel according to any one of <4> to <10>. <16> A method for prolonging the life of plants using the hydrogel according to any one of <4> to <10>.
[0012] The present invention provides a crosslinked product of a high-molecular-weight polymer and tannic acid that can be easily synthesized, molded into any shape, and used to form a material with extensibility, self-repairing properties, and shape memory. It also provides a hydrogel, a molded article, and a film containing the crosslinked product of a high-molecular-weight polymer and tannic acid, as well as methods for producing these.
[0013] Another object of the present invention is to provide a plant life-extending agent that can prolong the life of plants.
[0014] Photographs showing the results of observing the morphology of solutions obtained by mixing TA and PEG / PEO of various molecular weights in water. A diagram showing the results of measuring the viscoelasticity of TA / PEG gel and TA / PEO hydrogel. A diagram showing the relationship between TA concentration and turbidity. A diagram showing the relationship between PEG / PEO concentration and turbidity. A diagram showing the results of measuring the turbidity of aqueous TA and PEO solutions after mixing and leaving them to stand at room temperature or 80°C. A diagram showing the results of measuring the turbidity of mixed solutions of aqueous TA and PEO solutions and various hydrogen bond inhibitors. Powder X-ray diffraction measurement results for TA / PEO hydrogel. FT-IR measurement results for TA / PEO hydrogel. TA / PEO hydrogel 11H-NMR measurement results. Photographs of samples at each step during the preparation of a hydrogel molded body. Results of tensile tests on a hydrogel molded body (TaPeO 2 Gel) with PEO 500 kDa and a control gel. Results of tensile tests on a hydrogel molded body (TaPeO 2 Gel) with PEO 500 kDa to 4000 kDa. Results of tensile tests on a hydrogel molded body before (before cutting) and after an adhesion test. Photographs of a hydrogel molded body (TaPeO 2 Gel) before and after immersion in water. Photographs of a dried hydrogel molded body. Results of a three-point bending test on dried hydrogel molded bodies with PEO 500 kDa to 4000 kDa. Photographs showing the evaluation of shape memory ability. Results of a tensile test on a re-swollen gel. Photographs of a TA / high molecular weight PEO film (TaPeO 2 Film) before and after drying. This figure shows the relationship between the molecular weight of PEO and the thickness of a TA / high molecular weight PEO film (TaPeO Film). This figure shows the stress-strain curve of a tensile test of a TA / PEO film (TaPeO Film). This figure shows photographs of a test (left at room temperature for 5 days) of a gerbera daisy planted in a container containing water with hydrogel and a gerbera daisy planted in a container containing water without hydrogel. This figure shows enlarged photographs of the flower portion of a gerbera daisy planted in a container containing water with hydrogel and a gerbera daisy planted in a container containing water without hydrogel after being left at room temperature for 5 days. This figure shows photographs of a gerbera daisy planted in a container containing water with hydrogel and a gerbera daisy planted in a container containing water with added tannic acid. This figure shows photographs of parsley growing 45 and 100 days after the addition of hydrogel.
[0015] The following describes in detail an embodiment of the present invention, but the following description of the constituent elements is one example (typical example) of an embodiment of the present invention, and the present invention is not limited to the following content unless the gist of the present invention is changed. Note that when the expression "~" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0016] <Crosslinked Product> The present invention relates to a crosslinked product in which a high-molecular-weight polymer is crosslinked with tannic acid, in which the high-molecular-weight polymer has a constituent unit containing a group G capable of forming a hydrogen bond with tannic acid, and has a weight-average molecular weight of 50 kDa or more (hereinafter, this may be referred to as the "crosslinked product of the present invention").
[0017] The present inventors have surprisingly discovered that crosslinking a high-molecular-weight polymer having a specific weight-average molecular weight or more with tannic acid produces a material with properties completely different from the viscous material obtained by crosslinking a low-molecular-weight polyethylene glycol (PEG) with tannic acid (TA), which has been reported to date. Furthermore, they have discovered that hydrogels containing crosslinked high-molecular-weight polymers crosslinked with tannic acid and their dried products possess a variety of functions, such as self-repairing and shape-memory capabilities. The present invention was made based on these findings.
[0018] (High-Molecular-Weight Polymer) The high-molecular-weight polymer constituting the crosslinked product of the present invention is a polymer having a structural unit (hereinafter sometimes referred to as "structural unit (A)") containing a group G (hereinafter sometimes simply referred to as "group G") capable of forming a hydrogen bond with tannic acid, and is usually a water-soluble polymer. The high-molecular-weight polymer is crosslinked by tannic acid through the formation of a hydrogen bond between this group G and tannic acid.
[0019] The group G is not particularly limited as long as it is a group capable of forming a hydrogen bond with tannic acid, but examples of groups capable of forming a hydrogen bond with the hydroxyl group of tannic acid include groups having an oxygen atom such as an ether group or a carbonyl group, and groups having a nitrogen atom such as an amino group. Examples of groups capable of forming a hydrogen bond with the ether group or carbonyl group of tannic acid include a hydroxyl group. The structural unit (A) of the high-molecular-weight polymer may contain one or more of these groups G.
[0020] Examples of the structural unit (A) include those represented by the following formulae (1) to (3).
[0021]
[0022] In formula (1), R1 represents an alkylene group, preferably having 1 to 6 carbon atoms, more preferably 2 to 3 carbon atoms. X is —O— or —NH—.
[0023]
[0024] In formula (2), R 2 is a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group. 3 is a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group.
[0025]
[0026] In formula (3), R 4 is a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group. Y is OH, OR 40 OH (R 40 is an alkylene group or an oxyalkylene group. 41 R 42 (R 41 , R 42 are each independently a hydrogen atom or an alkyl group.
[0027] Among these, the structural unit (A) is preferably represented by the following formula (4) and / or formula (5): The structural unit represented by formula (4) is capable of forming a hydrogen bond between the ether bond in the structural unit and the hydroxyl group of tannic acid. The structural unit represented by formula (5) is capable of forming a hydrogen bond between the hydroxyl group in the structural unit and the ether group (oxygen atom) of tannic acid.
[0028]
[0029] R in formula (4) 1 represents an alkylene group, preferably having 1 to 5 carbon atoms, more preferably having 2 or 3 carbon atoms.
[0030]
[0031] The high molecular weight polymer only needs to contain the structural unit (A), and may be a homopolymer, a copolymer containing a plurality of structural units (A), or a copolymer containing other than the structural unit (A), but if the structural unit (A) is too small, it is considered that it is difficult to react with tannic acid.Therefore, the proportion of the structural unit (A) in the total structural units in the high molecular weight polymer is preferably 50 mol% or more, and may be 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, etc.
[0032] Specifically, examples of the high molecular weight polymer include polyalkylene oxides such as polyethylene oxide and polypropylene oxide, polyalkylene oxide copolymers, polyvinyl alcohol, polyvinyl alcohol copolymers, etc. The high molecular weight polymer is preferably one or more selected from the group consisting of polyethylene oxide (PEO), polyethylene oxide copolymers, polyvinyl alcohol (PVA), and polyvinyl alcohol copolymers.
[0033] The weight-average molecular weight of the high-molecular-weight polymer constituting the crosslinked product of the present invention is 50 kDa or more. By using such a high-molecular-weight polymer, the product does not become a viscous liquid as when a low-molecular-weight PEG is used, but becomes a solid form such as a hydrogel or a dried hydrogel. Considering the balance between hardness and elongation when the product is made into a hydrogel or a dried hydrogel, the weight-average molecular weight of the high-molecular-weight polymer is preferably 100 kDa or more, more preferably 500 kDa or more. The upper limit is not particularly limited, and may be 5000 kDa or less or 4000 kDa or less, but from the viewpoint of ease of production, 2000 kDa or less or 1000 kDa or less is preferred.
[0034] Therefore, the weight average molecular weight of the high molecular weight polymer is preferably 50 kDa to 5000 kDa, 100 kDa to 5000 kDa, 500 kDa to 5000 kDa, 500 kDa to 4000 kDa, 500 kDa to 2000 kDa, or 500 kDa to 1000 kDa.
[0035] The weight-average molecular weight of a high-molecular-weight polymer is a weight-average molecular weight calculated in terms of polyethylene oxide by gel permeation chromatography (GPC) using polyethylene oxide as a standard sample, and may also be simply referred to as "molecular weight."
[0036] Tannic acid (TA) is a natural polyphenol consisting of a central glucose unit to which 19 gallic acid units are bound, and which contains both catechol and pyrogallol groups. Tannic acid is the third most abundant natural compound after cellulose, semicellulose, and lignin, and is readily available and inexpensive. Tannic acid has also been approved by the U.S. Food and Drug Administration (FDA) as a food additive. It is highly soluble in water and is a safe and environmentally friendly material.
[0037] In the crosslinked product of the present invention, the molar ratio of tannic acid to the structural unit (A) in the high molecular weight polymer (number of moles of tannic acid in the crosslinked product / number of moles of structural unit (A) in the high molecular weight polymer in the crosslinked product) is preferably 0.02 to 0.1, and more preferably 0.03 to 0.06.
[0038] The crosslinked product of the present invention can be used as a constituent component of a hydrogel or a molded article. Hereinafter, the hydrogel or molded article containing the crosslinked product of the present invention will be described.
[0039] <Hydrogel> The present invention relates to a hydrogel containing the above-described crosslinked product of the present invention and water (hereinafter, may be referred to as "hydrogel of the present invention").
[0040] The hydrogel of the present invention typically has a water content of 15% by mass or more. The water content can be determined from the difference in mass before and after drying of the hydrogel of the present invention when the hydrogel is dried to a constant mass at 120°C and the mass before drying, and is expressed as a percentage by dividing the "difference in mass of the hydrogel of the present invention before and after drying at 120°C" by the "mass of the gel before drying." The water content of the hydrogel of the present invention may be 15% to 30% by mass, or 18% to 25% by mass, for example.
[0041] The hydrogel of the present invention is a rubbery elastic gel in which the storage modulus (G') is greater than the loss modulus (G") at 25°C and 0.1 Hz to 100 Hz, and which exhibits strong elastic properties. Such a rubbery elastic gel is obtained by forming a hydrogel containing water and a crosslinked product obtained by crosslinking a high-molecular-weight polymer having a weight-average molecular weight of 50 kDa or more with tannic acid. Note that a gel of a low-molecular-weight polymer and tannic acid has a loss modulus (G") greater than the storage modulus (G') and exhibits strong viscous properties, and the behavior of these gels is completely different.
[0042] The hydrogel of the present invention can achieve a maximum tensile stress of 0.05 MPa or more, and is stronger than general agarose gels and gelatin gels. The maximum tensile stress of the hydrogel of the present invention is preferably 0.07 MPa or more, more preferably 0.10 MPa or more, and even more preferably 0.12 MPa or more.
[0043] There is no particular upper limit to the maximum tensile stress of the hydrogel of the present invention, but the maximum tensile stress of the hydrogel of the present invention can be, for example, 0.05 MPa to 0.5 MPa, 0.07 MPa to 0.40 MPa, 0.10 MPa to 0.30 MPa, or 0.12 MPa to 0.25 MPa.
[0044] The hydrogel of the present invention has excellent extensibility and can achieve a breaking elongation of 500% or more, preferably 600% or more, and more preferably 700% or more.
[0045] There is no particular upper limit to the breaking elongation of the hydrogel of the present invention, but the breaking elongation of the hydrogel of the present invention can be, for example, 500% to 2000%, 600% to 1800%, or 700% to 1500%.
[0046] The maximum tensile stress and breaking elongation (breaking strain) of the hydrogel of the present invention can be calculated from a stress-strain curve measured by a tensile test using a 10 mm × 30 mm × 2 mm hydrogel of the present invention as a test piece, as described later in the Examples.
[0047] The hydrogel of the present invention can achieve a maximum bending stress of 10 MPa or more when dried at 40°C for 8 days, and having such a maximum bending stress makes it strong even when dried, which is preferable. The maximum bending stress when dried at 40°C for 8 days is preferably 15 MPa or more, and more preferably 18 MPa or more. This maximum bending stress can be calculated from a stress-strain curve measured by a three-point bending test using a 10 mm x 30 mm x 2 mm test piece of the hydrogel of the present invention, as described below in the Examples.
[0048] The hydrogel of the present invention exhibits excellent swelling resistance. The closer the swelling ratio is to 100%, the less likely it is to swell. When the hydrogel of the present invention is immersed in water for 48 hours, the swelling ratio is approximately 100% to 120%, or 105% to 115%. The swelling ratio can be determined from the mass of the hydrogel before and after immersion in water for 48 hours, and is expressed as a percentage by dividing the "mass of the gel after immersion in water for 48 hours" by the "mass of the gel before immersion."
[0049] The hydrogel of the present invention has adhesive properties, and when wounded or cut surfaces of the hydrogel of the present invention are brought into contact with each other and allowed to stand for about 24 hours, the hydrogel can recover its shape and physical properties to those before the wound or cut occurred.
[0050] The hydrogel of the present invention exhibits heat-induced self-repairing ability when dried at 40°C for 8 days. Specifically, when the cut surfaces of a dried hydrogel of the present invention dried at 40°C for 8 days are heated and then brought into contact with each other, the cut surfaces adhere to each other, allowing the shape and physical properties to be restored to those before cutting. For example, a hydrogel of the present invention can be dried at 40°C for 8 days, cut at any position, and heated by contacting the cut surfaces with hot water (water at approximately 90°C to 110°C), followed by bringing the cut surfaces into contact with each other and adhering them to obtain a self-repairing product. The maximum bending stress of this self-repairing product is 70% or more, or 80% or more, of the maximum bending stress of the dried product before cutting.
[0051] The hydrogel of the present invention has shape memory ability when dried at 40°C for 8 days. Shape memory ability is a property in which the hydrogel can be heated to a predetermined temperature, deformed into any shape, and then cooled, thereby memorizing the deformed shape, and can be restored to its pre-deformed shape by heating the deformed shape again. After drying the hydrogel of the present invention at 40°C for 8 days, immersion in hot water makes it flexible and allows it to be deformed into any shape. Allowing the deformed hydrogel to stand at room temperature allows it to memorize the deformation. Then, immersion in hot water again allows it to recover from the deformed state to its pre-deformed shape.
[0052] <Dried Hydrogel> The hydrogel of the present invention can be converted into a lightweight, highly tough, plastic-like material by drying. The dried hydrogel (i.e., the dried product of the hydrogel of the present invention) does not need to be completely free of water, but the water content of the dried hydrogel is lower than that of the hydrogel of the present invention, for example, a water content of 5 mass % or less.
[0053] The dried hydrogel has excellent toughness and can achieve a maximum bending stress of 10 MPa or more. The maximum bending stress of the dried hydrogel is preferably 15 MPa or more, and more preferably 18 MPa or more.
[0054] There is no particular upper limit to the maximum bending stress of the dry hydrogel, but the maximum bending stress of the dry hydrogel can be, for example, 10 MPa to 60 MPa, 15 MPa to 50 MPa, or 18 MPa to 35 MPa.
[0055] The extensibility of the dried hydrogel is smaller than that of the hydrogel of the present invention, and the breaking strain (%) in a bending test is about 2 to 10%.
[0056] Dry hydrogels have excellent self-repairing properties, such that damaged or cut portions are repaired by heating the damaged or cut portions and then bringing the damaged or cut surfaces into contact with each other. For example, by bringing the cut surfaces of a dry hydrogel into contact with water at approximately 90°C to 110°C and then bringing the cut surfaces into contact with each other, the cut surfaces adhere to each other, and the shape and physical properties can be restored to those before the damage or cut. In particular, by cutting a dry hydrogel at a desired position, heating the cut surfaces, and bringing the cut surfaces into contact with each other to allow self-repair, the maximum bending stress can be restored to 70% or more or 80% or more of the maximum bending stress before the cut.
[0057] Dried hydrogels have excellent shape memory. Specifically, they can be immersed in boiling water, deformed into any shape, and then left at room temperature to memorize the deformation. When the hydrogel is then immersed in boiling water again, it can recover from the deformed state to its original shape.
[0058] <Reswelling of dried hydrogel> A dried hydrogel can be reswelled to form the hydrogel of the present invention by immersing it in water. For example, the hydrogel can be restored to its pre-drying mechanical properties in about one day in water at room temperature, or in about 1 to 5 hours in water at about 30°C to 50°C.
[0059] <Molded Article> The molded article of the present invention is a molded article containing the crosslinked product of the present invention, and is the hydrogel of the present invention itself, the dried hydrogel of the present invention itself, or the hydrogel of the present invention or its dried product used as part of the constituent materials of the molded article. The shape of the molded article of the present invention is not particularly limited, and it can be in the form of a film, a plate, particles, various components, or the like, depending on the intended use.
[0060] The molded article of the present invention can have functionality attributable to the hydrogel of the present invention, its dried product, the high-molecular-weight polymers that constitute these, and tannic acid. For example, by utilizing functionalities such as toughness, high extensibility, adhesive ability, anti-swelling ability, self-healing ability, shape-memory ability, sustained-release ability, UV-blocking ability, anti-inflammatory activity, antibacterial activity, antiviral activity, and biocompatibility, the molded article of the present invention can be used as a tough material, a highly extensible material, an adhesive material, an anti-swelling material, a self-healing material, a shape-memory material, a sustained-release carrier, a UV-blocking material, an anti-inflammatory material, an antibacterial material, an antiviral material, a biocompatible material, and the like. Specifically, the molded article of the present invention can be used as a molecular actuator; a paint; household goods such as eyeglass frames and sunglasses lenses; cosmetics; toiletries; tissue adhesives, hemostatic materials, wound dressings, drug carriers, and other medical materials.
[0061] <Film> An example of the molded article of the present invention is a film. The thickness of the film is not particularly limited, but is, for example, 0.1 μm to 0.5 μm. The film can be used, for example, as a highly extensible film by taking advantage of its high extensibility. Specifically, it can be a film containing the crosslinked product of the present invention and having a breaking elongation of 500% or more. This film can also achieve a breaking elongation of 1000% or more, or even 1500% or more. As described below, such a highly extensible film can be produced by using the supernatant liquid separated during the production of the hydrogel of the present invention.
[0062] <Method for Producing Hydrogel> Hereinafter, the method for producing the hydrogel of the present invention will be described.
[0063] Although the method for producing the hydrogel of the present invention is not particularly limited, it is preferably a production method including a gelation step of mixing an aqueous solution containing a high-molecular-weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high-molecular-weight polymer with tannic acid, and a gel recovery step of recovering a hydrogel containing the crosslinked product from the crosslinked product-containing solution. By using such a hydrogel production method, the hydrogel of the present invention can be easily obtained without performing complicated operations such as purification.
[0064] (Gelling process) The gelling process is a process of mixing an aqueous solution containing a high molecular weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product in which the high molecular weight polymer is crosslinked with tannic acid.
[0065] The high-molecular-weight polymer is a polymer having a structural unit (structural unit (A)) containing a group G capable of forming a hydrogen bond with a hydroxyl group and a weight-average molecular weight of 50 kDa or more. The high-molecular-weight polymer used in the gelation step is similar to the high-molecular-weight polymer constituting the crosslinked product of the present invention, and its structure, molecular weight, and preferred examples thereof are as explained in the crosslinked product of the present invention. Simply mixing an aqueous solution containing such a high-molecular-weight polymer with an aqueous solution containing tannic acid causes hydrogen bonding between the group G in the high-molecular-weight polymer and the tannic acid, crosslinking the high-molecular-weight polymer and precipitating the crosslinked product as a solid. Therefore, the crosslinked product-containing solution obtained in the gelation step is a heterogeneous solution in which the crosslinked product has precipitated.
[0066] Although it depends on the molecular weight of the high-molecular-weight polymer, the concentration of the high-molecular-weight polymer in the aqueous solution containing the high-molecular-weight polymer used in the gelation step is preferably 5 g / L or more. Therefore, the high-molecular-weight polymer is preferably a polymer that dissolves 5 g or more in 1 L of water at 25° C. Taking into consideration the reactivity, the amount of waste liquid, and the like, the concentration of the high-molecular-weight polymer may be 10 g / L to 100 g / L or 20 g / L to 50 g / L.
[0067] The concentration of tannic acid in the aqueous solution containing tannic acid is preferably 5 g / L or more. Taking into consideration the reactivity, the amount of waste liquid, and the like, the concentration of tannic acid may be 50 g / L to 150 g / L or 80 g / L to 120 g / L.
[0068] The mixing ratio of the aqueous solution containing the high-molecular-weight polymer to the aqueous solution containing tannic acid is not particularly limited, but it is preferable to mix so that tannic acid is 0.045 mol or more, more preferably 0.047 mol or more or 0.050 mol or more per mol of the structural unit (A) in the high-molecular-weight polymer. The upper limit can be 0.7 mol or less, 0.3 mol or less, or 0.1 mol or less of tannic acid per mol of the structural unit (A) in the high-molecular-weight polymer.
[0069] Therefore, the mixing ratio of the aqueous solution containing the high molecular weight polymer to the aqueous solution containing tannic acid can be set to 0.045 mol to 0.7 mol, 0.047 mol to 0.3 mol, or 0.050 mol to 0.1 mol of tannic acid per 1 mol of the structural unit (A) in the high molecular weight polymer.
[0070] The order of mixing is not particularly limited, and the aqueous solution containing a high molecular weight polymer may be supplied to the reaction vessel after which the aqueous solution containing tannic acid is supplied and mixed therewith, or the aqueous solution containing a high molecular weight polymer may be supplied to the reaction vessel after which the aqueous solution containing tannic acid is supplied and mixed therewith, or the aqueous solution containing a high molecular weight polymer and the aqueous solution containing tannic acid may be supplied to the reaction vessel in parallel and mixed therewith. Furthermore, the mixing of the aqueous solution containing a high molecular weight polymer and the aqueous solution containing tannic acid is usually carried out with stirring.
[0071] If the mixing temperature is too high, the formation of hydrogen bonds is inhibited, so the temperature is preferably 10° C. to 60° C., more preferably 15° C. to 45° C., and even more preferably a temperature around room temperature of 20° C. to 30° C. Since a precipitate forms when a hydrogel is formed, the mixing time may be adjusted appropriately to any time at least until a precipitate forms, depending on the concentration of each aqueous solution and the mixing temperature.
[0072] (Gel recovery step) The gel recovery step is a step of recovering a hydrogel containing the crosslinked product from the crosslinked product-containing solution obtained in the gelation step. The method for recovering the hydrogel from the crosslinked product-containing solution is not particularly limited, and the solid hydrogel can be recovered using a method that can separate solids and liquid components, such as decantation, filtration, or centrifugation.
[0073] The recovered hydrogel may be used as is, or may be further subjected to a molding method such as compression molding to form a molded article of a desired shape. When the recovered hydrogel or a molded article formed from the hydrogel is dried for use, it may be dried by a known method until it reaches the desired water content. The drying method is not particularly limited, and any method such as natural drying, heat drying, or freeze drying may be used.
[0074] In the liquid component separated from the solids in the gel recovery step, crosslinked products usually remain. Therefore, it is preferable to use the liquid component separated from the solids in the gel recovery step for the production of a film or the like. By using the liquid component for the production of a film or the like, almost no waste components other than water are generated, making this an environmentally friendly (eco-friendly) production method. Furthermore, by reusing water, zero-wasted production is also possible.
[0075] <Film Manufacturing Method> Hereinafter, a method for manufacturing a film containing the crosslinked product of the present invention will be described, which utilizes the liquid component separated from the solid matter in the gel recovery step.
[0076] The method for producing a film that utilizes the liquid component separated from the solid matter in the gel recovery process specifically includes a gelation process in which an aqueous solution containing a high-molecular-weight polymer is mixed with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high-molecular-weight polymer with tannic acid, a liquid recovery process in which the crosslinked product-containing solution is separated into a hydrogel containing the crosslinked product and a liquid component, and then the liquid component is recovered, and a film formation process in which the liquid component is formed into a film.
[0077] (Gelling Step) The gelling step is the same as the gelling step in the method for producing the hydrogel of the present invention.
[0078] (Liquid recovery step) The liquid recovery step corresponds to the gel recovery step in the method for producing a hydrogel of the present invention, and is a step of separating a solid from a liquid component using decantation, filtration, centrifugation, or the like, and then recovering the liquid component. This liquid component contains cross-linked products with a low degree of cross-linking. Decantation is one of the preferred methods because it easily removes cross-linked products with a low degree of cross-linking from the solids and leaves them in the supernatant liquid.
[0079] (Film Forming Process) The film forming process is a process in which the liquid component recovered in the liquid recovery process is formed into a film. For example, a film can be obtained by placing the liquid component in an appropriate mold and drying it. There are no particular limitations on the drying conditions as long as the water in the liquid component can be removed, but in order to obtain a highly extensible film, it is preferable to dry at 40°C or higher and then condition the humidity at 15 to 35°C. For example, in order to obtain a highly extensible film, it is preferable to dry at 40 to 60°C for about 1 to 10 days and then condition the humidity at 15 to 35°C and a relative humidity of 60 to 90%.
[0080] <Plant life-extending agent> The present invention also relates to a plant life-extending agent containing the hydrogel of the present invention (hereinafter, sometimes referred to as the "plant life-extending agent of the present invention"). By using the hydrogel of the present invention, it is possible to prolong the life of plants, maintain their freshness for a long period of time, and prevent them from wilting.
[0081] The method of using the plant life-extending agent of the present invention is not particularly limited, and when growing plants in soil or a solid medium, the plant life-extending agent of the present invention can be mixed with the soil or a solid medium or placed on top of the soil or a solid medium. When used for hydroponics or for cut flowers in a vase, the plant life-extending agent of the present invention can be added to water or a culture solution. The cut parts of cut flowers, etc., during transportation may also be brought into contact with the plant life-extending agent of the present invention.
[0082] When the hydrogel of the present invention is applied to soil, solid medium, water, or culture solution, the size (maximum length) of the hydrogel of the present invention in a dried state can be 5 cm or less, 3 cm or less, or 1.5 cm or less, and is preferably, for example, about 0.1 cm to 5 cm, about 0.3 cm to 3 cm, or about 0.5 cm to 1.5 cm.
[0083] The amount of the plant life-extending agent of the present invention used can be set appropriately depending on the method of use, etc., but for example, when applied to soil, solid culture medium, water or culture solution, the amount of the plant life-extending agent of the present invention used can be 1 g to 30 g, 3 g to 20 g, 3.5 g to 15 g, etc. per 100 g of soil, culture medium, water or culture solution.
[0084] The plant to which the plant life-extending agent of the present invention is applied may be not only the plant itself, but also a part of the plant, such as an organ or tissue. Plant organs or tissues include flowers, leaves, stems, roots, branches, bulbs, etc. For example, the plant life-extending agent of the present invention can be applied to crops, trees, lawns, potted flowers, cut flowers, cut leaves, branches, etc.
[0085] Target plants include, but are not limited to, vegetables such as parsley, herb, spinach, komatsuna, mizuna, mibuna, asparagus, swiss cabbage, lettuce, thyme, sage, Italian parsley, rosemary, oregano, lemon balm, chives, lavender, salad burnet, lamb's ear, rocket, dandelion, nasturtium, basil, arugula, watercress, mulukhiyah, celery, kale, leeks, cabbage, Chinese cabbage, chrysanthemum, lettuce, lettuce, lettuce, butterbur, turnip, bok choy, mitsuba, Japanese parsley, Brussels sprouts, broccoli, cauliflower, myoga, radish, carrot, burdock, radish, turnip, sweet potato, potato, nagaimo, yam, taro, jinenjo, and yamatoimo; citrus fruits, apples, pears, grapes, blueberries, and other fruits. Fruits such as berries, persimmons, strawberries, pineapples, cherries, lychees, pomegranates, loquats, bananas, melons, mangoes, papayas, kiwifruit, cherimoya, avocados, guavas, plantains, plums, peaches, passion fruit, apricots, breadfruit, jackfruit, pawpaw, durian, feijoa, dragon fruit, star fruit, rambutan, jujubes, bell peppers, paprika, shishito peppers, cucumbers, eggplants, tomatoes, cherry tomatoes, pumpkins, bitter melons, okra, sweet corn, edamame, snow peas, green beans, and broad beans; fungi; and cut flowers such as gerberas, carnations, roses, hydrangeas, sweet peas, baby's breath, chrysanthemums, lilies, stocks, statice, gentians, gladioli, eustomas, tulips, and orchids.
[0086] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not changed.
[0087] [Reagents] The following reagents and solvents were used. Polyethylene glycol (PEG) (0.4 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. Polyethylene glycol (PEG) (0.6 kDa): Sigma Aldrich Polyethylene glycol (PEG) (1 kDa): Sigma Aldrich Polyethylene glycol (PEG) (6 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. Polyethylene glycol (PEG) (10 kDa): Sigma Aldrich Polyethylene glycol (PEG) (20 kDa): Sigma Aldrich Polyethylene glycol (PEG) (40 kDa): Serva Electrophoresis GmbH Polyethylene oxide (PEO) (100 kDa): Alfa Aesar Polyethylene oxide (PEO) (200 kDa): polysciences, Inc.・Polyethylene glycol (PEG) (500 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. ・Polyethylene oxide (PEO) (1000 kDa): Sigma Aldrich ・Polyethylene glycol (PEG) (2000 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. ・Polyethylene glycol (PEG) (4000 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. ・Tannic acid: Fujifilm Wako Pure Chemical Industries, Ltd. ・Guanidine hydrochloride: Nacalai Tesque ・Borax: Kenei Pharmaceutical ・Urea: Fujifilm Wako Pure Chemical Industries, Ltd. ・Polyvinyl alcohol (PVA) (22 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. ・Polyvinyl alcohol (PVA) (66 kDa): Fujifilm Wako Pure Chemical Industries, Ltd. ・Comazi Brilliant Blue R-250 (CBBR-250): Nacalai Tesque ・Gelatin: Nitta Gelatin Agarose: Nippon Gene 30 w / v% Acrylamide / Bis Mixed Solution (37.5:1): Wako Chemical USA Ammonium persulfate (APS): Tokyo Chemical Industry Co., Ltd. N,N,N',N'-Tetramethylethylenediamine: Nacalai Tesque, Dulbecco's Modified Eagle Medium (DMEM) high glucose: Fujifilm Wako Pure Chemical Industries, Ltd., Streptomycin sulfate for injection 1g "Meiji": Meiji Seika Pharma, Penicillin G potassium for injection 200,000 units: Meiji Seika Pharma, Fetal Bovine Serum (FBS): Sigma Aldrich, Trypsin: Nacalai Tesque, Cell counting Kit-8 (WST-8): Dojindo Chemical Industries, Ltd.
[0088] The other reagents used were commercially available special grade products. MilliQ (pure water with a resistivity of 18.3 MΩ cm or more produced by a milliQ (registered trademark) ultrapure water production system (Millipore)) was used as the solvent.
[0089] It should be noted that "polyethylene glycol" and "polyethylene oxide" are generally classified as "polyethylene glycol" when the molecular weight is low, 20 kDa or less, and "polyethylene oxide" when the molecular weight is higher. Regarding polyethylene glycol and polyethylene oxide, in the above [Reagent] description, even if the reagent name is "polyethylene glycol," it is described as "polyethylene glycol." However, hereinafter, those with a molecular weight of 20 kDa or less will be described as "PEG," those with a molecular weight of 40 kDa or more will be described as "PEO," and polyethylene glycol and polyethylene oxide will be collectively described as "PEG-PEO." Tannic acid will be described as "TA."
[0090] Experimental Example 1: Effect of PEG / PEO Molecular Weight (1) TA was dissolved in water to prepare a 100 mg / mL TA aqueous solution. PEG / PEO of various molecular weights (0.4 kDa, 0.6 kDa, 1.6 kDa, 10 kDa, 20 kDa, 40 kDa, 100 kDa, 200 kDa, 500 kDa, 1000 kDa, and 2000 kDa) were dissolved in water to prepare 25 mg / mL PEG / PEO aqueous solutions. 0.5 mL of the 100 mg / mL TA aqueous solution was added to 1 mL of each 25 mg / mL PEG / PEO aqueous solution, vortex-mixed, and centrifuged to obtain samples. Figure 1 shows the morphology of the solutions obtained by mixing TA and PEG / PEO of various molecular weights in water.
[0091] As shown in Figure 1, PEG-PEO alone was a colorless, transparent solution (see Figure 1(A)), whereas when TA was mixed, a precipitate formed in both solutions (see Figure 1(B)). As shown in Figure 1(C), when an aqueous solution of PEO with a molecular weight of 100 kDa or more was mixed with TA, clumps formed. When the liquid portion was removed by decantation, an elastic gel was obtained. As shown in Figure 1(C), when the molecular weight of PEG-PEO was 40 kDa or less, a highly dispersible suspension was obtained, and these precipitates disappeared by decantation. On the other hand, when the suspension of Figure 1(B) was centrifuged without decanting, the white precipitate turned brown (see Figure 1(D)), and when the supernatant after centrifugation was removed, a highly viscous gel was obtained (see Figure 1(E)).
[0092] [Experimental Example 2]: Evaluation of viscoelasticity of hydrogels PEG with a molecular weight of 10 kDa was selected as the PEG that forms a viscous gel, and PEO with a molecular weight of 500 kDa was selected as the PEO that forms an elastic gel. Gels were prepared, and the viscoelasticity of the gels was evaluated using a rheometer.
[0093] (Experimental Example 2-1): Preparation of Hydrogels Aqueous solutions of PEG and PEO (25 mg / mL) of each molecular weight were mixed with an aqueous solution of TA (100 mg / mL) at a ratio of 2:1 (v / v). In the case of PEG 10 kDa, simply mixing the aqueous PEG and TA solutions did not form a gel, so the mixture was centrifuged and the precipitated gel was used in the experiment. In the case of PEO 500 kDa, the precipitated gel mass formed by mixing the aqueous PEO and TA solutions was collected and used for measurement.
[0094] (Experimental Example 2-2): Evaluation of Viscoelasticity The viscoelasticity of the TA / PEG gel and TA / PEO hydrogel was measured using an MCR-101 rheometer manufactured by Anton Paar Japan under the following conditions: parallel plate diameter: 25 mm, fixed strain: 15.8% (10 kDa), 4.0% (500 kDa), measurement temperature: 25°C.
[0095] Figure 2 shows the results of measuring the viscoelasticity of the TA / PEG gel and TA / PEO hydrogel. As shown in Figure 2, for 10 kDa PEG, the loss modulus (G") exceeded the storage modulus (G'), indicating a strong viscous property. On the other hand, for 500 kDa PEO, the storage modulus was higher, suggesting a strong elastic property. The reason for this is thought to be that the higher the molecular weight of PEO, the longer the molecular chains are and the more entangled they are, which increases the ability to return to their original state when an external force is applied, i.e., increases the elasticity.
[0096] Experimental Example 3: Effect of TA Concentration PEG·PEO solutions of various molecular weights (10 kDa, 500 kDa) were dissolved in water to prepare 5 mg / mL PEG·PEO aqueous solutions. TA was dissolved in water to prepare TA aqueous solutions of various concentrations (0.125 mg / mL, 0.25 mg / mL, 0.5 mg / mL, 1 mg / mL, 2 mg / mL, 4 mg / mL, 8 mg / mL, 16 mg / mL, 32 mg / mL). 0.4 mL of the PEG·PEO aqueous solution was added to 1.6 mL of the TA aqueous solution and mixed by vortexing. The resulting mixture was incubated at room temperature for 24 hours, and then the absorbance at 600 nm was measured using a JASCO UV-Visible Spectrophotometer (V-630 (BIO)). Figure 3 shows the relationship between TA concentration and turbidity (average of three experiments). As shown in FIG. 3, in the case of PEO 500 kDa, the turbidity increased significantly at a TA concentration of 4 mg / mL or more.
[0097] Experimental Example 4: Effect of PEG·PEO Concentration TA was dissolved in water to prepare a 5 mg / mL TA aqueous solution. PEG·PEO (10 kDa, 500 kDa) was dissolved in water to prepare PEG·PEO aqueous solutions of various concentrations (0.125 mg / mL, 0.25 mg / mL, 0.5 mg / mL, 1 mg / mL, 1.25 mg / mL, 1.5 mg / mL, 1.75 mg / mL, 2 mg / mL, 4 mg / mL, 8 mg / mL, 16 mg / mL). 0.4 mL of the TA aqueous solution was added to 1.6 mL of the PEG·PEO aqueous solution and mixed by vortexing. The mixture was incubated at room temperature for 24 hours, and then the absorbance at 600 nm was measured. Figure 4 shows the relationship between PEG·PEO concentration and turbidity (average of three experiments). As shown in FIG. 4, for 500 kDa PEO, the turbidity increased significantly at PEO concentrations of 4 mg / mL or higher.
[0098] [Experimental Example 5]: Evaluation of whether hydrogen bonding is involved in the TA / PEO interaction To investigate whether hydrogen bonding is involved in the TA / PEO interaction, the formation of precipitates upon heating or in the presence of a hydrogen bond inhibitor was examined.
[0099] Experimental Example 5-1: Effect of Temperature on the Turbidity of TA / PEO Mixtures TA or 500 kDa PEO was dissolved in water to prepare a 5 mg / mL TA aqueous solution or a 5 mg / mL 500 kDa PEO aqueous solution. 0.4 mL of each of the TA aqueous solution and the 500 kDa PEO aqueous solution was added to 1.2 mL of water and mixed by vortexing. The mixture was incubated at room temperature or 80°C for 24 hours, and then the absorbance at 600 nm was measured.
[0100] Experimental Example 5-2: Effect of Hydrogen Bond Inhibitors on the Turbidity of TA / PEO Mixtures TA or 500 kDa PEO was dissolved in water to prepare a 5 mg / mL TA aqueous solution or a 5 mg / mL 500 kDa PEO aqueous solution. 0.4 mL of the TA aqueous solution was added to 1.2 mL of water, followed by the addition of either guanidine hydrochloride (50 mg), borax (50 mg), or urea (1 g). Then, 0.4 mL of the 500 kDa PEO aqueous solution was added and mixed by vortexing. The mixture was incubated at room temperature for 24 hours, and the absorbance at 600 nm was measured.
[0101] Figure 5 shows the results of turbidity measurements after mixing aqueous TA and PEO solutions and allowing them to stand at room temperature or 80°C (mean ± SE for three experiments; * (asterisk) indicates p<0.05 compared to room temperature). Figure 6 shows the results of turbidity measurements of mixtures of aqueous TA and PEO solutions and various hydrogen bond inhibitors (mean ± SE for three experiments; * indicates p<0.05 compared to the control). As shown in Figure 5, when the mixture was allowed to stand at 80°C, where hydrogen bonds are broken, the turbidity decreased compared to room temperature. Furthermore, as shown in Figure 6, the addition of hydrogen bond inhibitors such as guanidine hydrochloride and urea also reduced the turbidity. Furthermore, the addition of borax, which forms a boronate ester with the hydroxyl groups of TA, also reduced the turbidity. These results suggest that the hydroxyl groups of TA interact with PEG and PEO via hydrogen bonds.
[0102] Experimental Example 6: Evaluation of Hydrogel Structure (Experimental Example 6-1): Preparation of Hydrogel A 500 kDa PEO aqueous solution (25 mg / mL) and a TA aqueous solution (100 mg / mL) were mixed at a ratio of 2:1 (v / v). The precipitated hydrogel formed by mixing was dried under reduced pressure and used for the following evaluation.
[0103] (Experimental Example 6-2): Powder X-ray Diffraction A sample obtained by preparing a mixed solution of TA and 500 kDa PEO was dried under reduced pressure and then subjected to powder X-ray diffraction measurement. Powder X-ray diffraction was measured using a Rigaku horizontal sample multipurpose X-ray diffractometer (Ultima IV) with the sample fixed in a glass cell. The measurement conditions were as follows: X-ray source: Cu-Kα radiation (1.542 Å), tube voltage: 40 kV, tube current: 20 mA, scanning speed: 10° / min, diffraction angle: 5 to 35°, slit: 1 / 2-open-open
[0104] Figure 7 shows the results of powder X-ray diffraction analysis of the TA / PEO hydrogel. While the physical mixture of TA and PEO exhibited peaks similar to those of PEO alone, the TA / PEO hydrogel exhibited a halo pattern, suggesting an amorphous structure. This suggests that the PEO-derived crystallinity of TA / PEO disappears upon formation of the hydrogel, resulting in an amorphous structure.
[0105] (Experimental Example 6-3): Fourier transform infrared spectroscopy (FT-IR) After drying the sample obtained by preparing a mixed solution of TA and 500 kDa PEO under reduced pressure, it was measured by the ATR method using a PerkinElmer Fourier transform infrared spectrophotometer (Frontier MIR / NIR). The measurement conditions were as follows: Number of scans: 32, Resolution: 4
[0106] FT-IR measurement results of the TA / PEO hydrogel are shown in Figure 8. In the spectrum of the TA / PEO hydrogel, -1 The C-O-C stretching vibration band derived from PEG in the vicinity shifted to the lower wavenumber side. -1 The peaks derived from the hydroxyl groups of TA in the vicinity also shifted to the lower wavenumber side, suggesting that the oxygen of the ether of PEO and the hydroxyl groups of TA were hydrogen bonded in the gel.
[0107] (Experimental Example 6-4): Nuclear magnetic resonance spectroscopy ( 1 The sample obtained by preparing a mixed solution of TA and 500 kDa PEO was dried under reduced pressure, dissolved in DMSO-d6, and measured at 25°C using a JEOL JIM-α-500 nuclear magnetic resonance spectrometer (external magnetic field: 500 MHz). 1 The results of H-NMR are shown below. Peaks derived from TA and PEO were observed in the spectrum of the TA / PEO hydrogel. Furthermore, the ratio of TA hydroxyl groups to PEO ether groups was calculated from the integrals of the TA hydroxyl proton peaks around 9-10 ppm and the PEO ethylene proton peaks around 3.5 ppm. The stoichiometric ratio (molar ratio) of TA hydroxyl groups to PEO ether groups was found to be 1:1.
[0108] The samples obtained were similarly analyzed except that PEG / PEO with different molecular weights was used instead of 500 kDa. 1 H-NMR was measured. In the case of 0.4 kDa PEG, the molar ratio of hydroxyl groups of TA to ethylene groups of PEG was approximately 3:1, but this decreased with increasing PEG molecular weight, and in the case of PEG-PEO from 6 kDa to 4000 kDa, the molar ratio of ethylene groups of PEG to hydroxyl groups of TA was 1:1. These results suggest that the hydroxyl groups of TA may form hydrogen bonds with the ether of PEG-PEO in a 1:1 ratio.
[0109] Experimental Example 7: Evaluation of PVA Polymer TA was dissolved in water to prepare a 100 mg / mL TA aqueous solution. PVA (22 kDa, 60 kDa) was dissolved in water to prepare a 25 mg / mL PVA aqueous solution. 0.5 mL of the 100 mg / mL TA aqueous solution was added to 1 mL of the 25 mg / mL PVA aqueous solution, mixed by vortexing, and then centrifuged to obtain a sample.
[0110] As a result, while each PVA alone produced a colorless, transparent solution, mixing with TA resulted in the formation of a precipitate. Mixing 66 kDa PVA with TA yielded clumps similar to those obtained with ultra-high molecular weight PEO, and decanting the liquid yielded an elastic gel. Mixing 22 kDa PVA with TA, on the other hand, produced a highly dispersed suspension similar to that of PEG-PEO with a molecular weight of 40 kDa or less, and further centrifugation yielded a highly viscous, brown gel. These results suggest that in order to form an elastic gel with the addition of TA, it may be important for the polymer chains to be able to form hydrogen bonds with TA and for the polymer chain to have an ultra-high molecular weight.
[0111] Example 8: Evaluation of Hydrogel Molded Articles (Experimental Example 8-1): Preparation of Hydrogel Molded Articles Figure 10 shows photographs of samples taken at each stage during the preparation of hydrogel molded articles. First, a 100 mg / mL TA solution was added to 25 mg / mL PEO solutions of various molecular weights (500 kDa, 1000 kDa, 2000 kDa, and 4000 kDa) in a volume ratio of 1:2. After stirring, a hydrogel precipitate formed. The supernatant was removed from the hydrogel-containing solution by decantation to obtain the hydrogel (Figure 10(A)). The hydrogel was then sandwiched between glass or stainless steel plates for 5 or 30 minutes, respectively, and compressed to a thickness of 2 mm to form a molded article (Figure 10(B)). After molding, the molded product was dried at 40°C for 5 hours using an AS ONE constant temperature dryer (OF-300B) to remove excess water, and then cut into a predetermined size to obtain a hydrogel molded product (hydrogel molded product before drying) (Figure 10 (C)).
[0112] As shown in Figure 10, the hydrogel obtained by mixing TA / PEO could be molded into a plate by compressing it. Furthermore, by removing excess water, the color changed from cream to brown, and a highly uniform gel exhibiting permeability was obtained.
[0113] (Experimental Example 8-2): Preparation of control gel Preparation of gelatin gel Water was added to gelatin and heated at 80°C for 3 hours to prepare a gelatin solution (500 mg / mL). The gelatin solution was poured into a mold and allowed to stand overnight at 4°C to obtain a gelatin gel with a thickness of 2 mm.
[0114] Preparation of agarose gel: Water was added to agarose and heated in a microwave oven to prepare an agarose solution (25 mg / mL). The agarose solution was poured into a mold and allowed to stand at room temperature to obtain an agarose gel.
[0115] Preparation of acrylamide gel: Water was added to 30 w / v% Acrylamide / Bis Mixed Solution to adjust the final acrylamide concentration to 100 mg / mL, and then 10% APS (final concentration: 0.05 v / v%) and TEMED (final concentration: 0.1 v / v%) were added and stirred. The mixture was then poured into a mold and allowed to stand at room temperature for 30 minutes or more to obtain a 2 mm thick acrylamide gel.
[0116] (Experimental Example 8-3): Tensile Test of Hydrogel Molded Articles Stress-strain measurements in the tensile test were performed at room temperature using an A&D tabletop tension-compression testing machine (MCT-2150, 500N load cell). When the control gel was rectangular, the gel broke at the fixed position, so a dumbbell-shaped sample was used. For other tensile tests, rectangular (10mm x 30mm) samples (2mm thick) were used. PEO 1000kDa to 4000kDa hydrogel molded articles were directly set in the clamp of the testing machine. For the PEO 500kDa hydrogel molded article, an acrylic plate was sandwiched between the fixed part and the clamp was set via the acrylic plate, because a rectangular shape would cause stress to concentrate at the fixed position due to the structure of the fixing device of the testing machine, leading to breakage at the fixed part. Maximum stress indicates the maximum stress until breakage. Breaking elongation indicates the strain (%) at breakage. Stress (Pa) is calculated by multiplying the load (N) by the area (m 2 The strain (%) is the value obtained by dividing the distance displacement (m) between the two clamps when the gel was deformed by the distance (m) before deformation, expressed as a percentage. The tensile speed was 300 mm / min.
[0117] Figure 11 shows the results of tensile tests of a 500 kDa PEO hydrogel (TaPeO Gel) and a control gel. Figure 11(A) shows the stress-strain curves of the tensile tests, Figure 11(B) shows the maximum stress of each gel (mean ± SE of 10 experiments; * indicates p<0.05 compared to acrylamide gel, † (dagger) indicates p<0.05 compared to agarose gel, and ‡ (double dagger) indicates p<0.05 compared to gelatin gel), and Figure 11(C) shows the strain of each gel (mean ± SE of 10 experiments; * indicates p<0.05 compared to acrylamide gel, † indicates p<0.05 compared to agarose gel, and ‡ indicates p<0.05 compared to gelatin gel). 11, the PEO 500 kDa hydrogel specimen exhibited a maximum tensile stress of approximately 0.135 MPa and a breaking strain of 817%, which were higher than those of any of the control gels. This suggests that the hydrogel specimen is a tough and highly stretchable gel.
[0118] Figure 12 shows the results of tensile tests on hydrogel specimens with PEO 500 kDa to 4000 kDa. Figure 12(A) shows the stress-strain curves of the tensile tests, Figure 12(B) shows the maximum stress of each specimen (mean ± SE of 7 to 10 experiments, * indicates p<0.05 compared to the PEO 500 kDa hydrogel specimen, † indicates p<0.05 compared to the PEO 1000 kDa hydrogel specimen), and Figure 12(C) shows the strain of each specimen (mean ± SE of 7 to 10 experiments, * indicates p<0.05 compared to the PEO 500 kDa hydrogel specimen). As shown in Figure 12, the maximum tensile stress of each hydrogel specimen increased depending on the PEO molecular weight and reached a plateau above 2000 kDa. On the other hand, the breaking strain was not significantly affected by the PEO molecular weight, and all showed high values of 700% or more.
[0119] (Experimental Example 8-4): Adhesion of Hydrogel Molded Articles Adhesion of cut surfaces was evaluated using an undyed hydrogel molded article (PEO 500 kDa) and a hydrogel molded article (PEO 500 kDa) dyed blue with Commercial Brilliant Blue R-250 (CBBR-250) to make the adhesion site easier to visualize. First, 10 x 30 mm undyed and dyed hydrogel molded articles were each cut in half at the center. Next, the cut surfaces of the undyed and dyed hydrogel molded articles were brought into contact with each other and allowed to stand at room temperature for 24 hours. Thereafter, a tensile test was performed and evaluated using the same method as in the tensile test described above.
[0120] Figure 13 shows the results of tensile tests of hydrogel molded articles before and after the adhesion test (before cutting). Figure 13(A) shows the stress-strain curves of the tensile test, Figure 13(B) shows the maximum stress of each molded article, and Figure 13(C) shows the strain of each molded article. As shown in Figure 13, the hydrogel molded articles (PEO 500 kDa) were bonded simply by contacting the cut surfaces. The bonded hydrogel molded articles were stretched using a tensile tester to the measurement limit of the tester without fracture. Furthermore, the maximum tensile stress and fracture strain of the bonded hydrogel molded articles were comparable to those of the uncut articles, suggesting that the hydrogel molded articles (PEO 500 kDa) have excellent adhesive properties. The reason why the hydrogel molded article (PEO 500 kDa) showed adhesiveness is thought to be that although the bond between TA and PEO at the cut surface was broken when the gel was cut, the hydrogen bond between TA and PEO was reformed by adhesion. Furthermore, since such adhesion was weak on the uncut surface, it is inferred that this adhesive ability is selective for the cut surface.
[0121] (Experimental Example 8-5): Measurement of Moisture Content The moisture content was measured using a moisture meter (MOC63u) manufactured by Shimadzu Corporation, and calculated using the following formula: Moisture content (%) = (W - D) / W x 100, where W is the weight of the compact before drying and D is the weight of the compact after drying to a constant weight at 120°C.
[0122] As a result, all of the hydrogel molded articles ranging from 500 kDa to 4000 kDa showed a water content of approximately 20%.
[0123] (Experimental Example 8-6): Measurement of swelling ratio The weight (W1) of the hydrogel molded article (500 kDa PEO) before swelling was measured. Next, the hydrogel molded article (500 kDa PEO) was immersed in water at room temperature for 24 hours or 48 hours, and the weight (W2) was measured. The swelling ratio was calculated using the following formula: Swelling ratio (%) = W2 / W1 × 100
[0124] Figure 14 shows photographs of the hydrogel molded article before and after immersion in water. As shown in Figure 14, no change in the shape of the molded article was observed even after 48 hours. Furthermore, the swelling ratio of the hydrogel molded article (500 kDa PEO) was low, at 105% and 107% after 24 and 48 hours, respectively, suggesting that it hardly swelled at all.
[0125] (Experimental Example 8-7): Cytotoxicity of TA / PEO Hydrogel HeLa cells, which are human cervical cancer cells, were cultured in 10% (v / v) FBS-containing DMEM high glucose medium (200 U / mL penicillin, 0.2 mg / mL streptomycin) at 37°C under 5% CO2 concentration. Semi-confluent cells were detached from the dish using the trypsin-EDTA method and centrifuged at 3000 rpm for 3 minutes. The supernatant was removed, and the resulting pellet was suspended in 10% (v / v) FBS-containing DMEM medium for use in subculture or seeding. 3 x 10 HeLa cells were cultured in a 6-well plate. 5Cells were seeded at 1000 cells / well and cultured in 10% FBS-containing DMEM high glucose medium (3 mL) for 24 hours. After washing with serum-free medium, the TA / PEO hydrogel molded article (length: width: thickness = 1 cm: 1 cm: 2 mm) was placed on the upper layer of a trans-well, and the cells were cultured in serum-free cell medium in the lower layer for 6 hours. After culture, the trans-well was removed, washed with serum-free medium, and then cultured in 10% FBS-containing medium (3 mL) for 18 hours. After washing with HBSS (1 mL), 10 v / v% WST-8-containing HBSS (2 mL) was added. The mixture was incubated at 37°C for 30 minutes, and the absorbance was measured using a Biotec microplate spectrophotometer (Epoch) (measurement wavelength: 450 nm, reference wavelength: 655 nm). The results showed that regardless of the molecular weight of PEO used, between 500 kDa and 4,000 kDa, the TA / PEO hydrogel showed nearly 100% cell viability and induced almost no cytotoxicity. Therefore, the application of TA / PEO hydrogel as a biomaterial is promising.
[0126] [Experimental Example 9]: Evaluation of Dried Hydrogel Molded Body (Experimental Example 9-1): Preparation of Dried Hydrogel Molded Body A hydrogel molded body (hydrogel molded body before drying) prepared in the same manner as in Experimental Example 8-1 was dried at 40°C for approximately 8 days to obtain a dried hydrogel molded body. Figure 15 is a photograph of the obtained dried hydrogel molded body. As shown in Figure 15, the transparency of the hydrogel molded body (500 kDa PEO) increased upon drying. Furthermore, the dried hydrogel molded body was a plastic-like material that was lightweight and had excellent toughness.
[0127] (Experimental Example 9-2): Load-bearing test When a load-bearing test was carried out on the dried hydrogel molded body (500 kDa PEO), the dried hydrogel molded body (500 kDa PEO) was able to support a weight of 500 g.
[0128] (Experimental Example 9-3): Three-point bending test A three-point bending test was performed using a dried hydrogel molded body to evaluate deformability. The stress-strain measurement in the three-point bending test was performed at room temperature using an A&D tabletop tension-compression testing machine (MCT-2150, 500N load cell). The sample used was a specimen (2mm thick) cut to 10 x 30mm. The indentation speed was 100mm / min. The maximum stress indicates the maximum stress until breakage. The breaking strain indicates the strain at breakage. The stress and strain were defined by the following formula: Stress (Pa) = 3 x distance between supports (m) x load (N) / 2 x sample width (m) x sample thickness (m) 2 Strain (%) = 6 x gel thickness (m) x displacement (m) / {distance between supports (m)} 2 ×100
[0129] The results of the three-point bending test for the dried hydrogel molded bodies of PEO 500 kDa to 4000 kDa are shown in Figure 16. Figure 16(A) shows the stress-strain curve of the three-point bending test, Figure 16(B) shows the maximum stress of each molded body in the three-point bending test (mean ± SE of 5 to 10 experiments, * indicates p<0.05 compared to the dried hydrogel molded body of PEO 500 kDa, and † indicates p<0.05 compared to the dried hydrogel molded body of PEO 1000 kDa), and Figure 16(C) shows the strain of each molded body in the three-point bending test (mean ± SE of 5 to 10 experiments, ‡ indicates p<0.05 compared to the dried hydrogel molded body of PEO 4000 kDa). The maximum bending stress and breaking strain of the dried hydrogel specimen (500 kDa PEO) were approximately 18 MPa and 2.4%, respectively. The maximum stress of the dried hydrogel specimen tended to increase with increasing PEO molecular weight. On the other hand, the breaking strain was not significantly affected by the PEO molecular weight and remained within a ±2% range.
[0130] (Experimental Example 9-4): Adhesion of dried hydrogel molded body A cross section of a broken sample of dried hydrogel molded body (500 kDa PEO) was immersed in boiling water for 30 seconds, and then the cross section was brought into contact with the surface and allowed to stand at room temperature for 24 hours. Thereafter, visual evaluation, a load test, and a three-point bending test were performed.
[0131] (Experimental Example 9-5): Adhesion of dried hydrogel molded body - visual evaluation and load test Visual observation of the sample after the adhesion test showed that the two gel pieces had adhered and had recovered to the point where the adhesion site was no longer visible. Furthermore, even when a 500 g weight was hung from the adhered gel, it did not break. Furthermore, no adhesion was observed unless the cross section was immersed in boiling water. When the cut surface of a dried hydrogel molded body (500 kDa PEO) was immersed in boiling water, the hydrogen bonds between the TA / PEO at the cut surface were broken, and when another cut surface was brought into contact with the cut surface in this state, the TA / PEO reformed hydrogen bonds between the cut surfaces, resulting in adhesion.
[0132] (Experimental Example 9-6): Adhesion of dried hydrogel shaped body - three-point bending test A three-point bending test of the adhered dried hydrogel shaped body (500 kDa PEO) was carried out under the same conditions as above. As a result, compared to the uncut dried hydrogel shaped body, the maximum bending stress was slightly reduced, but the bending stress was maintained at 80% or more.
[0133] (Experimental Example 9-7): Shape Memory Ability of Dried Hydrogel Molded Articles First, a 500 kDa PEO hydrogel molded article was prepared and cut out. After cutting, it was dried for 8 days either in a plate shape (I-shaped) or in a folded state (L-shaped or U-shaped), to obtain dried hydrogel molded articles molded into each shape. Next, each molded article was immersed in room temperature water or boiling water for 30 seconds. The "I-shaped" sample was transformed into an "L-shaped" sample, and the "L-shaped" or "U-shaped" sample was flattened into an "I-shape." The shape was then fixed by leaving it to stand for 60 seconds. After that, the sample was again immersed in boiling water for 60 seconds, and the change in shape was observed.
[0134] Figure 17 shows the evaluation of shape memory ability. As shown in Figure 17, when the "I-shaped," "L-shaped," and "U-shaped" molded bodies were immersed in boiling water for 30 seconds and stress was applied, they were able to deform into the "L-shaped," "I-shaped," and "I-shaped" shapes, respectively. On the other hand, when the dried hydrogel molded body (500 kDa PEO) was immersed in water at room temperature and stress was applied, it failed to deform and broke. After immersion in boiling water, the deformed gel was able to fix its shape by leaving it for 60 seconds. When immersed in boiling water again, it gradually changed shape and returned to its original shape. This suggests that the dried hydrogel molded body (500 kDa PEO) has shape memory ability. The reason why the dried hydrogel molded body (500 kDa PEO) exhibited deformability is thought to be that immersion in boiling water for 30 seconds partially cleaved the hydrogen bonds between TA and PEO, making the gel flexible. On the other hand, it is thought that after leaving it still for 60 seconds, hydrogen bonds were reformed and the shape was fixed. When it was immersed in hot water again, the reformed hydrogen bonds were broken again, and it is thought that the original shape was restored by some of the hydrogen bonds that were not broken by the first immersion in hot water.
[0135] (Experimental Example 9-8): Swelling ratio of dried hydrogel shaped body Dried hydrogel shaped body (500 kDa PEO) was immersed in water to re-swell. The dried hydrogel shaped body showed no change in shape even after immersion in water for 24 or 48 hours, but in both cases it showed a swelling ratio of approximately 130%. The water content of the gel after swelling calculated from this value was approximately 20%, which closely matched the water content of the hydrogel shaped body (500 kDa PEO) before drying.
[0136] (Experimental Example 9-9): Tensile test of reswelled gel A dried hydrogel molded body (500 kDa PEO) was immersed in water for 24 hours. Then, it was dried at 40°C for 1 to 5 hours using an AS ONE constant temperature dryer (OF-300B) or left to stand at room temperature for 24 hours, and then a tensile test was carried out under the same conditions as in Experimental Example 8-3.
[0137] Figure 18 shows the results of tensile tests on the reswelled gels. Figure 18(A) shows the stress-strain curves of the tensile tests, Figure 18(B) shows the maximum stress of each gel (mean ± SE of 6 to 10 experiments), and Figure 18(C) shows the strain of each gel (mean ± SE of 6 to 10 experiments; * indicates p<0.05 compared to the control (before drying)). As shown in Figure 18, the hydrogel specimens hardened like plastic upon drying, but upon swelling with water, they exhibited a maximum tensile stress equivalent to that of the hydrogel specimens before drying. The fracture strain was also equal to or greater than that of the specimens before drying, suggesting that the hydrogel specimens can be transformed into rubber-like elastic gels by reswelling, even after drying. This is thought to be due to the fact that water penetrated deep into the gels during prolonged water immersion, restoring the reversibility of the hydrogen bonds between TA and PEO. Furthermore, the precise reason why the breaking strain was slightly improved compared to the hydrogel molded body before drying is unknown, but the hydrogel molded body before drying was obtained by immediately molding and drying a heterogeneous gel obtained by mixing a TA solution and a PEO solution, so it is possible that the hydrogen bonds were uneven and the PEO chains were distorted.However, it is thought that the swelling process increased uniformity and made the crosslinking points uniform, which eliminated the distortion of the PEO chains and resulted in a more extensible gel.These results suggest that the dried hydrogel molded body exhibits physical properties roughly equivalent to those of the molded body before drying due to swelling.
[0138] Experimental Example 10: Evaluation of TA / PEO Films (Experimental Example 10-1): Preparation of TA / High Molecular Weight PEO Films. A 100 mg / mL aqueous solution of TA was added to a 25 mg / mL aqueous solution of various molecular weight PEOs (500 kDa, 1000 kDa, 2000 kDa) at a volume ratio of 1:2 and stirred, resulting in the formation of a hydrogel precipitate. The supernatant was removed from the hydrogel-containing solution by decantation, and the hydrogel and supernatant were separated. 100 mL of the supernatant was poured into a mold and dried at 40°C and 60% humidity for 4 days using a Tokyo Rikakikai thermo-hygrostat (KCL-2000W). The dried film was cut out and then allowed to stand at 25°C and 70% humidity for 1 day to reabsorb moisture. This film was used as a TA / high molecular weight PEO film (TaPeO Film).
[0139] Figure 19 shows photographs of the TA / high molecular weight PEO film before and after drying. As shown in Figure 19, the supernatant, which was a white suspension, formed a film upon drying. Although the film was brittle immediately after drying, it exhibited extensibility upon re-absorbing moisture. Figure 20 shows the relationship between the molecular weight of PEO and the thickness of the TA / high molecular weight PEO film (mean ± SE of 5 to 10 experiments, * indicates p<0.05 compared to TaPeO Film (PEO 500 kDa)). The thickness of the TA / high molecular weight PEO film decreased with increasing PEO molecular weight.
[0140] (Experimental Example 10-2): Tensile test of TA / PEO film Stress-strain measurements in the tensile test of the TA / PEO film were performed at room temperature using an A&D tabletop tension-compression tester (MCT-2150, 500 N load cell). The sample used was a TA / PEO film cut to a size of 10 x 40 mm. The maximum stress indicates the maximum stress until breakage. The elongation (strain) (%) is the value expressed as a percentage, obtained by dividing the distance displacement between the two clamps when the film is deformed by the distance before deformation. The tensile speed was 50 mm / min.
[0141] The stress-strain curves of the tensile test of the TA / PEO film are shown in Figure 21. As shown in Figure 21, in all of the TA / ultra-high molecular weight PEO films using PEO of 500 to 2000 kDa, the films were elongated to the measurement limit.
[0142] [Experimental Example 11]: Evaluation of the Effect on Plants (1) An aqueous solution of 10 g of PEO (500 kDa) dissolved in 400 mL of water was mixed with an aqueous solution of 20 g of tannic acid dissolved in 200 mL of water, and the supernatant was removed by decantation to obtain a hydrogel. Next, the entire amount of the obtained hydrogel was torn into approximately 1 cm pieces and placed in a container containing 800 mL of water containing a gerbera (cut flower) and left at room temperature. For comparison, a gerbera placed in a container containing water without hydrogel and a gerbera placed in a container containing water with added tannic acid were left at room temperature and observed.
[0143] Figure 22 is a photograph showing a test (left at room temperature for 5 days) of a gerbera placed in a container of water with hydrogel and a gerbera placed in a container of water without hydrogel. Figure 23 is a magnified photograph of the flower portion of a gerbera placed in a container of water with hydrogel and a gerbera placed in a container of water without hydrogel after being left at room temperature for 5 days. As shown in Figures 22 and 23, the condition of the flowers with hydrogel was better after 5 days and they lived longer than those without hydrogel.
[0144] Figure 24 is a photograph showing a gerbera plant in a container with water containing hydrogel and a gerbera plant in a container with water containing tannic acid. As shown in Figure 24, adding tannic acid to the water makes the gerbera plant more likely to wither.
[0145] [Experimental Example 12]: Evaluation of Effect on Plants (2) An aqueous solution of 10 g of PEO (500 kDa) dissolved in 400 mL of water was mixed with an aqueous solution of 20 g of tannic acid dissolved in 200 mL of water, and the supernatant was removed by decantation to obtain a hydrogel. Next, the entire amount of the obtained hydrogel was torn into pieces of approximately 1 cm and mixed with soil. The soil mixed with the hydrogel was placed in a pot, and parsley seedlings were planted and grown. For comparison, parsley was grown in the soil without adding hydrogel.
[0146] Figure 25 is a photograph showing the growth of parsley 45 and 100 days after adding hydrogel. As shown in Figure 25, the plants that used hydrogel lived longer than those that did not use hydrogel.
[0147] The crosslinked product of the present invention and hydrogels containing the same can be used as smart materials and medical materials by taking advantage of their functionalities such as self-repairing ability and shape memory ability, and are therefore industrially useful. Furthermore, the use of the crosslinked product of the present invention and hydrogels containing the same can prolong the life of plants, making them useful in the fields of agriculture and horticulture.
Claims
1. A crosslinked product in which a high molecular weight polymer is crosslinked with tannic acid, the high molecular weight polymer having a structural unit containing a group G capable of forming a hydrogen bond with tannic acid, and having a weight average molecular weight of 50 kDa or more.
2. The crosslinked product according to claim 1, wherein the molar ratio of tannic acid to said constituent units is 0.02 to 0.
1.
3. The crosslinked product according to claim 1, wherein the high molecular weight polymer is one or more selected from the group consisting of polyalkylene oxide, polyalkylene oxide copolymer, polyvinyl alcohol and polyvinyl alcohol copolymer.
4. A hydrogel comprising the crosslinked product according to any one of claims 1 to 3 and water.
5. The hydrogel described in claim 4, having a maximum tensile stress of 0.05 MPa or more.
6. The hydrogel according to claim 4, having a breaking elongation of 500% or more.
7. The hydrogel according to claim 4, having a swelling ratio of 100% to 120%.
8. The hydrogel described in claim 4, which has a maximum bending stress of 10 MPa or more when dried at 40°C for 8 days.
9. The hydrogel according to claim 4, which has a self-repairing ability upon heating when dried at 40°C for 8 days.
10. The hydrogel according to claim 4, which has shape memory ability when dried at 40°C for 8 days.
11. A molded article comprising the crosslinked product according to any one of claims 1 to 3.
12. A film comprising the crosslinked product according to any one of claims 1 to 3, and having a breaking elongation of 500% or more.
13. A method for producing a hydrogel, comprising: a gelling step of mixing an aqueous solution containing a high molecular weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high molecular weight polymer with tannic acid; and a gel recovery step of recovering a hydrogel containing the crosslinked product from the crosslinked product-containing solution, wherein the high molecular weight polymer used is a polymer having a constituent unit including a group G capable of forming a hydrogen bond with tannic acid and having a weight average molecular weight of 50 kDa or more.
14. A method for producing a film, comprising: a gelling step of mixing an aqueous solution containing a high molecular weight polymer with an aqueous solution containing tannic acid to obtain a crosslinked product-containing solution containing a crosslinked product formed by crosslinking the high molecular weight polymer with tannic acid; a liquid recovery step of separating the crosslinked product-containing solution into a hydrogel containing the crosslinked product and a liquid component, and then recovering the liquid component; and a film formation step of drying the liquid component to obtain a film, wherein the high molecular weight polymer used is a polymer having a constituent unit including a group G capable of forming a hydrogen bond with tannic acid and having a weight average molecular weight of 50 kDa or more.
15. A plant life-extending agent comprising the hydrogel according to claim 4.
Citation Information
Patent Citations
Film and method for producing film
JP2021014533A
Polymeric binders for silicon or silicon-graphite composite electrodes and their use in electrochemical cells
JP2021536523A
Cited By
High-strength degradable self-healing hydrogel and preparation method thereof
CN120718300A