Blank, method for manufacturing structural member, and structural member

The hot stamping blank with higher emissivity on the outer surfaces of the minimum thickness steel plates in the overlap region addresses the challenge of maintaining a process window and ensuring strength and corrosion resistance, enhancing productivity and energy efficiency in the manufacturing of structural members.

WO2024225330A1PCT designated stage expired Publication Date: 2024-10-31NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/016120
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In hot stamping processes for manufacturing structural members, such as automobile body components, it is challenging to maintain a process window for heating conditions, especially when using composite blanks with overlapping portions, which can lead to uneven temperature distribution and reduced productivity due to excessive alloying of the plating layer, resulting in compromised strength and corrosion resistance.

Method used

A blank for hot stamping is designed with a plurality of steel plates arranged in an annular shape, where the steel plate with the minimum thickness has a higher emissivity on its outer surfaces than other surfaces, allowing for increased temperature rise in the overlap portion, thus ensuring both the strength of the maximum thickness overlap and the corrosion resistance of the minimum thickness portion.

Benefits of technology

This approach allows for a more efficient heating process, reducing the heating time and energy consumption, improving productivity, and maintaining the corrosion resistance of the structural member, while also eliminating the need for post-processing treatments like shot blasting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016120_31102024_PF_FP_ABST
    Figure JP2024016120_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A blank (20) comprises a plurality of steel sheets. The plurality of steel sheets are arranged and joined so as to have an annular shape in a plan view of the blank (20). The plurality of steel sheets include steel sheets (21, 22). An edge portion of a first steel sheet (21) and an edge portion of a second steel sheet (22) form an overlap portion (241). Among the plurality of steel sheets, the steel sheet that constitutes a part of the blank (20) having a minimum plate thickness (tmin) is a plated steel sheet. A maximum plate thickness (tmax) of the blank (20) is in the overlap portion (241). The emissivity of surfaces (216, 226) of the steel sheets (21, 22), respectively, positioned outside the overlap portion (241) is greater than the emissivity of at least one of the other surfaces of the plurality of steel sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Blank, manufacturing method of structural member, and structural member

[0001] The present disclosure relates to a blank for hot stamping, a method for manufacturing a structural member using the blank, and the structural member.

[0002] Structures such as automobile bodies are formed from multiple structural members. Structural members are manufactured, for example, by press-forming a blank. To ensure high strength and good dimensional accuracy, structural members are sometimes manufactured by a press-forming method called hot stamping. Hot stamping is a technique in which a blank, which is a steel plate, is heated to a temperature in the austenite range, and then press-formed using a die. The blank is then held in the die and quenched by removing heat (rapid cooling).

[0003] Patent Document 1 discloses a steel sheet (blank) for hot stamping. The steel sheet of Patent Document 1 has a surface treatment film on the entire surface of at least one surface, the surface treatment film having an emissivity of 60% or more at a wavelength of 8.0 μm at 25° C. According to Patent Document 1, the surface of the steel sheet to which the surface treatment film is applied has an increased emissivity, and the heat transfer effect by radiation is large. Therefore, when the steel sheet is heated during hot stamping, the steel sheet undergoes a transformation into an austenite phase, where the metal structure of the steel sheet is transformed into an austenite phase. c3 Patent Document 1 describes that this makes it possible to shorten the heating time and improve the productivity of hot stamped members.

[0004] Patent Document 2 discloses a method for manufacturing an automobile body side structural frame from a plurality of blanks. In Patent Document 2, the plurality of blanks are joined to form a composite blank, and the composite blank is press-formed to manufacture the body side structural frame. Patent Document 2 also describes hot forming (hot stamping) the composite blank.

[0005] International Publication No. 2022 / 215229 Special Publication No. 2021-528248

[0006] In recent years, in order to simplify the manufacturing process of structures, it has been considered to integrate two or more components from the blank stage. Patent Document 2, for example, discloses a method of hot stamping a composite blank having an annular shape in a plan view to form an annular body side structural frame integrated with pillars, rockers, etc. Patent Document 2 also describes a method of overlapping adjacent steel sheets in the composite blank and joining them by spot welding. When a composite blank includes an overlap portion, it is difficult to ensure a process window in the manufacturing of structural components. Specifically, during hot stamping, the blank is heated until its microstructure is austenitized. However, the overlap portion formed by partial overlapping of steel sheets is thicker than the non-overlapping portion, and therefore is difficult to heat. For example, if the steel sheet having the smallest sheet thickness in the blank is a plated steel sheet, while the overlap portion having the largest sheet thickness in the blank is being heated to ensure its strength by hot stamping, excessive alloying of the plating layer may occur in the thinnest plated steel sheet, which was heated first, resulting in a thick diffusion layer and a decrease or loss of the corrosion resistance (rust prevention) of the plating layer. Therefore, when an overlap portion is present in the blank, it is difficult to ensure a process window for the heating conditions. Furthermore, the temperature rise rate of the overlap portion having the largest sheet thickness in the blank may become a bottleneck, potentially reducing the productivity of the structural component.

[0007] An object of the present disclosure is to provide a blank for hot stamping that can be used to manufacture structural components that combine the strength of the overlap portion, which has the maximum plate thickness, with the rust prevention function of the portion, which has the minimum plate thickness.

[0008] A hot stamping blank according to the present disclosure comprises a plurality of steel sheets. The plurality of steel sheets are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel sheets include a first steel sheet and a second steel sheet. The second steel sheet has an end portion. The end portion of the second steel sheet is overlapped and joined to the end portion of the first steel sheet, thereby forming an overlap portion together with the end portion of the first steel sheet. Of the plurality of steel sheets, the steel sheet constituting the portion having the smallest sheet thickness in the blank is a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet. The overlap portion has the largest sheet thickness in the blank. The emissivity of the surface located outside the overlap portion in each of the first steel sheet and the second steel sheet is greater than the emissivity of at least one of the other surfaces in the plurality of steel sheets.

[0009] The hot stamping blank according to the present disclosure makes it possible to manufacture a structural component that combines the strength of the overlap portion having the greatest thickness with the rust prevention function of the portion having the smallest thickness.

[0010] FIG. 1 is a plan view of a structural member according to an embodiment. FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 3A is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment, showing a blank according to an embodiment. FIG. 3B is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment, showing a blank according to an embodiment. FIG. 3C is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment, showing a blank according to an embodiment. FIG. 3D is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment, showing a blank according to an embodiment. FIG. 3E is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment. FIG. 3F is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment. FIG. 3G is a schematic diagram illustrating a method for manufacturing a structural member according to an embodiment. FIG. 4 is a cross-sectional view of a structural member manufactured by a manufacturing method according to an embodiment. FIG. 5 is a plan view of a structural member according to a modified example of the above embodiment. FIG. 6A is a diagram illustrating a division pattern of a structural member according to a first example. FIG. 6B is a diagram illustrating another division pattern of a structural member according to the first example. FIG. 6C is a diagram illustrating yet another division pattern of a structural member according to the first example. Fig. 6D is a diagram showing yet another division pattern of a structural member in the first embodiment. Fig. 6E is a diagram showing yet another division pattern of a structural member in the first embodiment. Fig. 6F is a diagram showing yet another division pattern of a structural member in the first embodiment. Fig. 6G is a diagram showing yet another division pattern of a structural member in the first embodiment. Fig. 7A is a diagram showing a division pattern of a structural member in the second embodiment. Fig. 7B is a diagram showing another division pattern of a structural member in the second embodiment. Fig. 7C is a diagram showing yet another division pattern of a structural member in the second embodiment. Fig. 7D is a diagram showing yet another division pattern of a structural member in the second embodiment.

[0011] A blank for hot stamping according to an embodiment includes a plurality of steel sheets. The plurality of steel sheets are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel sheets include a first steel sheet and a second steel sheet. The second steel sheet has an end portion. The end portion of the second steel sheet is overlapped and joined to the end portion of the first steel sheet, thereby forming an overlap portion together with the end portion of the first steel sheet. Of the plurality of steel sheets, the steel sheet constituting the portion having the smallest sheet thickness in the blank is a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet. The overlap portion has the largest sheet thickness in the blank. The emissivity of the surface located outside the overlap portion in each of the first steel sheet and the second steel sheet is greater than the emissivity of at least one of the other surfaces in the plurality of steel sheets (first configuration).

[0012] In the blank according to the first configuration, the end of the first steel sheet and the end of the second steel sheet form an overlap portion having the maximum sheet thickness in the blank. The emissivity of the surface of each of the first steel sheet and the second steel sheet located outside the overlap portion is higher than the emissivity of at least one other surface in the blank. That is, the emissivity of both outer surfaces of the overlap portion in the blank is relatively high. This allows the heating rate of the overlap portion to be increased when the blank is heated during hot stamping, thereby shortening the heating time of the overlap portion. Therefore, the heating of the blank required for hot stamping can be completed before excessive alloying of the coating layer in the steel sheet with the smallest sheet thickness, which has been heated first, progresses and the diffusion layer becomes thick. As a result, the strength of the overlap portion with the largest sheet thickness can be ensured by hot stamping, and the corrosion resistance (rust resistance) of the steel sheet with the smallest sheet thickness can be ensured.

[0013] Thus, the blank according to the first configuration enables the manufacture of structural components that combine the strength of the overlap portion having the greatest thickness with the rust prevention function of the portion having the smallest thickness. In other words, the blank allows the temperature rise rate of the overlap portion having the greatest thickness to be increased, thereby making it easier to ensure the process window of heating conditions in the manufacture of structural components. Furthermore, by increasing the temperature rise rate of the overlap portion, the heating time of the blank for hot stamping can be shortened, thereby improving the productivity of structural components. Furthermore, shortening the heating time of the blank reduces energy consumption in the manufacture of structural components and reduces the amount of greenhouse gases generated when heating the blank for hot stamping.

[0014] In the first configuration, each of the plurality of steel sheets may be a plated steel sheet. The plated steel sheet has a base steel sheet and a plating layer provided on the base steel sheet (second configuration).

[0015] In the second configuration, each steel sheet included in the blank is a plated steel sheet. In this case, when the blank is formed into a structural component by hot stamping, the formation of oxide scale can be suppressed. Therefore, after hot stamping, it is not necessary to subject the structural component to a process for removing oxide scale, such as shot blasting. This can improve the productivity of the structural component.

[0016] In the second configuration, the plating layer may be an aluminum-based plating layer (third configuration).

[0017] When each steel sheet is a plated steel sheet having an aluminum-based plating layer, as in the third configuration, when the blank is heated during hot stamping, a difference in temperature rise rate is likely to occur, particularly between the overlap portion having the largest sheet thickness and the steel sheet having the smallest sheet thickness. Because the aluminum-based plating layer is nearly white, it easily reflects heat energy and inhibits temperature rise in the overlap portion. However, even when each steel sheet is a plated steel sheet having an aluminum-based plating layer, by increasing the emissivity of both outer surfaces of the overlap portion, temperature rise in the overlap portion can be promoted when the blank is heated during hot stamping, thereby shortening the heating time of the overlap portion. As a result, corrosion resistance of the steel sheet with the smallest sheet thickness can be ensured and productivity of structural components manufactured from the blank can be improved.

[0018] In any of the first to third configurations, the surfaces of the first steel plate and the second steel plate located outside the overlapping portion may be coated with a coating, which has, for example, an emissivity of 60% or more at 25°C and a wavelength of 8.0 μm (fourth configuration).

[0019] In any one of the first to third configurations, the surfaces of the first steel plate and the second steel plate located outside the overlapping portion may be coated with a coating, which comprises carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a coating weight of 0 to 0.30 g / m 2 The carbon black and oxide may be dispersed throughout the coating. The carbon black content in the coating may be X CB (g / m 2 ), the oxide content is X Oxide (g / m 2 ) and then X CB and X Oxide It is preferable that the following formula (1) (see Patent Document 1) is satisfied (fifth configuration): 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )≦332.0 (1)

[0020] In any one of the first to fifth configurations, the plurality of steel plates may include two or more steel plates having different plate thicknesses. In this case, the plate thickness of the overlapping portion may be t max , the thickness of the steel plate constituting the part with the smallest plate thickness in the blank is t min When this is the case, t max / t min It is preferable that the ratio is ≦3.2 (sixth configuration).

[0021] When two or more steel plates with different thicknesses are included in a blank, the difference in thickness between the overlap portion and the steel plate constituting the portion with the smallest thickness in the blank becomes larger compared to when all the steel plates included in the blank have the same thickness. If the difference in thickness is excessive, when a structural component is manufactured from the blank by hot stamping, the temperature rise in the overlap portion becomes slower than that of the steel plate constituting the portion with the smallest thickness in the blank, making it more difficult to ensure the process window of the heating conditions. Therefore, in the sixth configuration, the thickness t of the overlap portion is max and minimum plate thickness t min Ratio to: t max / t min is set to 3.2 or less. As a result, even when two or more steel sheets having different thicknesses are included in a blank, it becomes easier to complete heating of the thickest overlap portion before alloying of the coating layer of the thinnest steel sheet progresses excessively, and the process window of the heating conditions becomes easier to ensure.

[0022] A method for manufacturing a structural component according to an embodiment includes the steps of preparing a blank according to any one of the first to sixth configurations, heating a plurality of steel plates included in the blank to a temperature equal to or higher than the austenite transformation completion temperature, and using a mold to form the heated blank into a structural component that is annular in plan view and quenching it (seventh configuration).

[0023] A structural member according to an embodiment comprises a member body and a coating. The member body is formed by a plurality of steel plates joined together and has an annular shape in plan view. The plurality of steel plates include a first steel plate and a second steel plate. The second steel plate has an end portion. The end portion of the second steel plate is overlapped and joined to the end portion of the first steel plate, thereby forming an overlap portion together with the end portion of the first steel plate. The coating is provided on a surface of each of the first steel plate and the second steel plate that is positioned outside the overlap portion. The coating contains one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide at a concentration of 0.001 g / m 2 or more (eighth configuration).

[0024] A structural member according to an embodiment comprises a member body and a coating. The member body is formed by a plurality of steel plates joined together and has an annular shape in plan view. The plurality of steel plates include a first steel plate and a second steel plate. The second steel plate has an end portion. The end portion of the second steel plate is overlapped and joined to the end portion of the first steel plate, thereby forming an overlap portion together with the end portion of the first steel plate. The coating is provided on the surface of each of the first steel plate and the second steel plate that is positioned outside the overlap portion. The coating contains carbon black at 0.500 g / m 2 The following is contained (ninth configuration).

[0025] In the eighth or ninth configuration, the structural member may be a door ring part of an automobile. In this case, the member body may include a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar (tenth configuration).

[0026] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or equivalent components are designated by the same reference numerals, and the same description will not be repeated.

[0027] [Structural Member] Fig. 1 is a diagram (plan view) of a structural member 10 according to this embodiment, viewed from above in a state where it is placed on a horizontal surface. The structural member 10 is used, for example, in the body of an automobile. The structural member 10 is typically a door ring component of the automobile. In this embodiment, an example in which the structural member 10 is a door ring component will be described.

[0028] The structural member 10 is a hot-stamped member. That is, the structural member 10 is formed by hot stamping (hot press processing) a blank made of multiple steel plates. The structural member 10 includes a member main body 11. The member main body 11 has an annular shape in a plan view of the structural member 10. The member main body 11 includes a front pillar 111, a center pillar 112, and a rocker 113. When the structural member 10 is assembled to the body of an automobile, the center pillar 112 is disposed rearward of the front pillar 111. The center pillar 112 extends generally in the vertical direction of the vehicle body. The front pillar 111 extends toward the center pillar 112. When the structural member 10 is assembled to the body of an automobile, the rocker 113 is disposed below the front pillar 111 and the center pillar 112. The rocker 113 connects the front pillar 111 and the center pillar 112.

[0029] In this embodiment, the member body 11 is formed of a plurality of steel plates 21, 22, and 23 joined together. In the example of FIG. 1 , the front pillar 111 is mainly formed of the steel plates 21 and 23. The center pillar 112 is mainly formed of the steel plate 22. The rocker 113 is also formed of the steel plates 22 and 23.

[0030] FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1 . FIG. 2 shows a cross-section of the structural member 10 cut in the thickness direction at the position of the steel plate 21. As shown in FIG. 2 , the steel plate 21 has an open cross-section. In a cross-sectional view of the structural member 10, the steel plate 21 has, for example, a generally hat-shaped shape. More specifically, the steel plate 21 includes a top plate 211, vertical walls 212 and 213, and flanges 214 and 215. The vertical wall 212 is disposed on the opposite side of the vertical wall 213 with respect to the top plate 211. In a cross-sectional view of the structural member 10, one end of the vertical walls 212 and 213 is connected by the top plate 211. In a cross-sectional view of the structural member 10, the other end of the vertical walls 212 and 213 is connected to flanges 214 and 215, respectively. The flanges 214 and 215 protrude from the vertical walls 212 and 213, respectively, to the outside of the structural member 10.

[0031] In the structural member 10, the width W of the steel plate 21, i.e., the portion located above the front pillar 111 (FIG. 1), may be 15 mm or more and 300 mm or less. The height H of the steel plate 21, i.e., the portion located above the front pillar 111, may be 10 mm or more and 150 mm or less. The width W is the distance from the end of the rounded corner between the top plate 211 and the vertical wall 212 on the vertical wall 212 side to the end of the rounded corner between the top plate 211 and the vertical wall 213 on the vertical wall 213 side in the cross section of the structural member 10. The height H is the distance from the top plate 211 to the flanges 214, 215 in the thickness direction of the top plate 211.

[0032] Although not shown, the other steel plates 22, 23 also have an open cross section similar to the steel plate 21. The steel plates 22, 23 may also have, for example, a generally hat-shaped cross section in the cross section of the structural member 10. The width of the portion of the steel plate 22 corresponding to the center pillar 112 ( FIG. 1 ) may be 15 mm or more and 300 mm or less. The height of the portion of the steel plate 22 corresponding to the center pillar 112 may be 10 mm or more and 150 mm or less. The width of the portion of the steel plate 23 corresponding to the lower part of the front pillar 111 ( FIG. 1 ) may be, for example, 30 mm or more and 750 mm or less. The height of the portion of the steel plate 23 corresponding to the lower part of the front pillar 111 may be 25 mm or more and 150 mm or less. The width of the portion of the steel plate 23 corresponding to the rocker 113 ( FIG. 1 ) may be, for example, 30 mm or more and 300 mm or less. The height of the portion of the steel plate 23 corresponding to the rocker 113 may be 25 mm or more and 150 mm or less.

[0033] The size of the annular structural member 10 in a plan view is, for example, 1.0 m or more. The size of the structural member 10 may be, for example, 4.0 m or less. The size of the structural member 10 is the length of a line segment connecting any two points on the outer periphery of the structural member 10 that are farthest apart when the structural member 10 is placed on a horizontal surface and viewed vertically.

[0034] 3A to 3G, a method for manufacturing the structural member 10 will be described. The method for manufacturing the structural member 10 according to this embodiment includes the steps of preparing a blank 20, heating the blank 20, and forming the heated blank 20 into the structural member 10.

[0035] 3A , in the preparation step, a blank 20 having a shape obtained by unfolding the structural member 10 is prepared. The blank 20 includes a plurality of steel plates 21, 22, and 23. The steel plates 21, 22, and 23 are arranged and joined together so as to have an annular shape when the blank 20 is viewed from above.

[0036] 3B, 3C, and 3D are cross-sectional views of the blank 20 showing the joints between the steel plates 21, 22, and 23. FIGS. 3B, 3C, and 3D are cross-sectional views taken along lines IIIB-IIIB, IIIC-IIIC, and IIID-IIID in FIG. 3A, respectively. Referring to FIGS. 3B and 3C, the steel plate 21 is lap-joined to each of the steel plates 22 and 23. That is, the end of the steel plate 22 is lap-joined to the end of the steel plate 21, thereby forming an overlap portion 241 together with the end of the steel plate 21. Similarly, the end of the steel plate 23 is lap-joined to the end of the steel plate 21, thereby forming an overlap portion 242 together with the end of the steel plate 21. Referring to FIG. 3D, the steel plate 22 is lap-joined to the steel plate 23 in addition to the steel plate 21. The end of the steel plate 22 is overlapped and joined to the end of the steel plate 23, thereby forming an overlap portion 243 together with the end of the steel plate 23. The steel plates 21, 22, and 23 are joined by, for example, spot welding or laser welding.

[0037] 3B to 3D, the steel plate 21 has a plate thickness t 1 The steel plate 22 has a plate thickness t 2 The steel plate 23 has a plate thickness t 3 In the example of this embodiment, the steel plate 21 has a plate thickness t 1 and t of the steel plate 22 2 is the thickness t of the steel plate 23 3 Therefore, the overlap portion 241 of the steel plates 21 and 22 has a maximum plate thickness t maxThe thickness t of the overlap portion 241 max is larger than the plate thickness of the overlap portion 242 of the steel plates 21 and 23 and the plate thickness of the overlap portion 243 of the steel plates 22 and 23.

[0038] In the example of this embodiment, among the plurality of steel plates 21, 22, and 23 included in the blank 20, the plate thickness t 3 Therefore, the steel plate 23 has a minimum thickness t min That is, the portion of the steel plate 23 that is not overlapped with the other steel plates 21 and 22 constitutes a portion having the minimum plate thickness t min and the thickness t of the steel plate 23 3 is the minimum thickness t of the blank 20 min is.

[0039] As in this embodiment, the plurality of steel plates 21, 22, and 23 have different plate thicknesses t 1 , t 2 , t 3 When having the maximum plate thickness t max and minimum plate thickness t min Ratio of: t max / t min In this case, the maximum plate thickness t max and minimum plate thickness t min For example, t max / t min <4.0 Maximum plate thickness t max and minimum plate thickness t min is t max / t min It is preferable that the maximum plate thickness t satisfies ≦3.2. max and minimum plate thickness t min is t max / t min The maximum plate thickness t may be ≧2.5. max is, for example, 4.2 mm or less. max may be 1.6 mm or more.

[0040] The steel plates 21 and 22 have a maximum plate thickness t maxThe surfaces 216, 226 of the steel plates 21, 22 located outside the overlap portion 241 have a higher emissivity than at least one of the other surfaces of the steel plates 21, 22, 23 included in the blank 20. That is, the emissivity of the surfaces 216, 226 of the steel plates 21, 22 located outside the overlap portion 241 is higher than the emissivity of the surfaces 217, 227 of the steel plates 21, 22 located inside the overlap portion 241 and / or the emissivity of one or both surfaces of the other steel plate 23. The surfaces 216, 226 of the steel plates 21, 22 located outside the overlap portion 241 have a thickness of 1 / 2 mm that is less than the maximum thickness t max In this embodiment, the emissivity of the surfaces 216 and 226 located outside the overlap portion 241 of the steel plates 21 and 22 is greater than the emissivity of the surfaces 217 and 227 located inside the overlap portion 241. In addition, the emissivity of the surfaces 216 and 226 located outside the overlap portion 241 of the steel plates 21 and 22 is greater than the emissivity of the surfaces 217 and 227 located inside the overlap portion 241 of the steel plates 21 and 22 when the steel plates 21 and 22 have a minimum plate thickness t minThe emissivity at 25°C is greater than the emissivity at both surfaces of the steel plate 23 constituting the portion having the overlapping portion 241. For example, the emissivity at 25°C at a wavelength of 8.0 μm is 60% or more for the surfaces 216, 226 of the steel plates 21, 22. The emissivity at 25°C at a wavelength of 8.0 μm for the surfaces 216, 226 of the steel plates 21, 22 is more preferably 70% or more, and even more preferably 80% or more. The emissivity at 25°C at a wavelength of 8.0 μm for at least one surface other than the surfaces 216, 226 of the steel plates 21, 22, 23 included in the blank 20 may be less than 60%. The difference in emissivity at 25°C at a wavelength of 8.0 μm between the surfaces 216, 226 on both outer sides of the overlapping portion 241 and at least one surface other than the surfaces 216, 226 is preferably greater than 5%, more preferably greater than 10%, and even more preferably greater than 20%. The emissivity can be measured in accordance with JIS R 1801 (2002). In this case, a sample taken from the steel sheet to be measured is placed in a Fourier transform infrared spectrophotometer, and the radiation intensity at a wavelength of 8.0 μm is measured at 25° C. to calculate the emissivity. Alternatively, it is also possible to measure the radiation intensity of a target area at 25° C. using a radiation thermometer set to a measurement wavelength of 8.0 μm, and calculate the emissivity from the ratio to the radiation intensity of a black body.

[0041] In this embodiment, the entire surface 216 of the steel plate 21 opposite the steel plate 22 is covered with the coating 25. Also, the entire surface 226 of the steel plate 22 opposite the steel plate 21 is covered with the coating 25. On the other hand, the steel plate 23 is not provided with the coating 25. As a result, the emissivity of both outer surfaces of the overlap portion 241 is higher than the emissivity of the surface of the steel plate 23.

[0042] The coating 25 is, for example, a black coating. The coating 25 may be a carbon-based surface treatment coating (a coating containing carbon (C)). For example, the brightness L * Value (CIE 1976 lightness index L defined in JIS Z8781-4 (2013) *If the emissivity (Emissivity) of the coating 25 at a wavelength of 8.0 μm at 25°C is 60% or more, preferably 70% or more, and more preferably 80% or more. That is, the emissivity of the surfaces 216, 226 of the steel sheets 21, 22 to which the coating 25 is applied at a wavelength of 8.0 μm at 25°C is 60% or more, preferably 70% or more, and more preferably 80% or more. The coating 25 may have an emissivity of 60% or more at a wavelength of 8.0 μm at 700°C. For example, the surface treatment coating described in Patent Document 1 can be used as the coating 25. Specifically, the coating 25 can contain carbon black and one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide. The coating 25 may or may not contain silica. That is, the silica content of the coating 25 is 0 g / m or less. 2 The silica content of the coating 25 is 0.30 g / m 2 The silica content may be more preferably 0.10 g / m or less. 2 More preferably, it is 0.05 g / m or less. 2 The following is the result.

[0043] The carbon black and oxides can be dispersed throughout the entire surface of the coating 25 that is perpendicular to the thickness direction of the steel sheet 21. CB (g / m 2 ), the content of one or more oxides (metal oxides) selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide is X Oxide (g / m 2 ) and then X CB and X Oxide It is preferable that the following formula (1) is satisfied: 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )≦332.0 (1)

[0044] In formula (1), the central formula: 24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide)) is preferably 119.0 or more, more preferably 170.0 or more, and even more preferably 220.0 or more. The value calculated by the middle formula is preferably 330.0 or less, more preferably 310.0 or less, and even more preferably 300.0 or less.

[0045] The dispersion state of the carbon black and metal oxide in the coating 25 can be confirmed by performing an area analysis of the coating 25 with an electron probe micro analyzer (EPMA) for elements derived from the carbon black (e.g., C) and elements derived from the oxide (Zr, Zn, and Ti). CB can be measured by cross-sectional analysis of the coating 25 using a transmission electron microscope (TEM). That is, a cross-sectional analysis of the coating 25 is performed by TEM-EDS analysis on an area of ​​a predetermined size (thickness of the coating 25 × 5 μm), and the thickness of the coating 25 and the area ratio of particles with a carbon content of 70 mass % or more in that area are measured. The density of carbon black is defined as ρ (ton / m 3 ), the film thickness is d (μm), and the area ratio is a (%), the value expressed by ρ×d×a is the carbon black content X CB (g / m 2 ) The oxide content X Oxide can be determined by performing elemental analysis on the surface of the coating 25 using an X-ray fluorescence analyzer (ZSX Primus, manufactured by RIGAKU Corporation) and quantifying the amounts of metal Zr, metal Zn, and metal Ti.

[0046] Carbon black content X in the coating 25 CB is 0.030 g / m 2 It is preferable that the content is 0.100 g / m or more. 2 It is more preferable that the content X is equal to or greater than this. CB is set within a range that satisfies the formula (1), but is preferably 0.800 g / m 2 or less, more preferably 0.600 g / m 2 The following is the result.

[0047] Coating 25 may contain 5.0% or more, preferably 8.0% or more, by volume of carbon black. Coating 25 may contain 40.0% or less, preferably 30.0% or less, by volume of carbon black.

[0048] Metal oxide content X in the coating 25 Oxide is 0.030 g / m 2 It is preferable that the content is 0.060 g / m or more. 2 It is more preferable that the content X is equal to or greater than this. Oxide is set within a range that satisfies the formula (1), but is preferably 0.500 g / m 2 More preferably, it is 0.300 g / m or less. 2 The following is the result.

[0049] The coating 25 may contain 1.0% or more metal oxide by volume. The coating 25 may also contain 30.0% or less metal oxide by volume, and preferably contains 25.0% or less metal oxide by volume.

[0050] Carbon black content X CB (g / m 2 ) and the metal oxide content X Oxide (g / m 2 ) ratio: X Oxide / X CB is preferably 0.20 or more and 200.00 or less. Oxide / X CB is more preferably 0.40 or more and 10.00 or less, and further preferably 0.60 or more and 5.00 or less.

[0051] The coating 25 may contain various binder components and additives in addition to the carbon black and metal oxides described above.

[0052] The binder component is preferably a water-dispersible or water-soluble resin. The content of the binder component is preferably 40% by volume or more relative to the total volume of the coating 25. As the binder component selected from water-dispersible or water-soluble resins, various known resins exhibiting water dispersibility or water solubility can be used. Examples of such water-dispersible or water-soluble resins include polyurethane resins, polyester resins, acrylic resins, epoxy resins, fluororesins, polyamide resins, polyolefin resins, and polymer compounds obtained by hydrolysis and condensation polymerization of silane coupling agents. The binder component is more preferably one or more selected from the group consisting of polyester resins, polyurethane resins, polyolefin resins, acrylic resins, epoxy resins, fluororesins, and polyamide resins. When a polyurethane resin is used as the binder component, the polyurethane resin is preferably a polyether-based polyurethane resin.

[0053] Examples of additives include leveling agents, water-soluble solvents, metal stabilizers, and etching inhibitors. The leveling agent is, for example, a nonionic or cationic surfactant. Examples of nonionic or cationic surfactants include polyethylene oxide or polypropylene oxide adducts, acetylene glycol compounds, and the like. Examples of water-soluble solvents include alcohols such as ethanol, isopropyl alcohol, t-butyl alcohol, and propylene glycol; cellosolves such as ethylene glycol monobutyl ether and ethylene glycol monoethyl ether; esters such as ethyl acetate and butyl acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of metal stabilizers include chelate compounds such as EDTA (ethylenediaminetetraacetic acid) and DTPA (diethylenetriaminepentaacetic acid). Examples of etching inhibitors include amine compounds such as ethylenediamine, triethylenepentamine, guanidine, and pyrimidine.

[0054] The coating 25 can be formed by applying an organic or inorganic treatment liquid containing, for example, carbon black and a metal oxide to the entire surfaces 216, 226 of the steel sheets 21, 22, and then drying the volatile components in the treatment liquid. The treatment liquid can be applied to the surfaces 216, 226 of the steel sheets 21, 22, for example, by a roll coater, a curtain coater, or an inkjet. In the case of inkjet application, the thickness of the coating 25 can also be changed continuously. The thickness of the coating 25 is, for example, 0.5 μm or more and 5.0 μm or less. The thickness of the coating 25 is preferably 1.0 μm or more and 3.0 μm or less. The thickness of the coating 25 is determined based on the thickness t of the steel sheets 21, 22. 1 , t 2 Therefore, the thicknesses of the steel plates 21 and 22 measured including the coating 25 are respectively set to the thickness t 1 , t 2 can be treated as

[0055] The minimum thickness t of the blank 20 min The steel sheet 23 having the above-mentioned characteristic is a plated steel sheet. In this case, the steel sheet 23 has a base steel sheet 23a and a plated layer 23b. The type of the base steel sheet 23a is not particularly limited. The plated layer 23b is provided on the base steel sheet 23a. The plated layer 23b covers the entire or almost the entire surface of both sides of the base steel sheet 23a. The plated layer 23b is a metal plated layer. The plated layer 23b may be, for example, hot-dip aluminum plating, hot-dip galvanneal plating, or electro-galvanized plating. As the steel sheet 23, a known aluminum-plated steel sheet, zinc-plated steel sheet, etc. may be used. The thickness t of the steel sheet 23 min is the combined thickness of the base steel sheet 23a and the plating layer 23b.

[0056] The steel sheets 21 and 22 may be known plated steel sheets, similar to the steel sheet 23. That is, the steel sheet 21 may have a base steel sheet 21a and a plated layer 21b provided on the base steel sheet 21a. The steel sheet 22 may have a base steel sheet 22a and a plated layer 22b provided on the base steel sheet 22a. The type of the base steel sheets 21a and 22a is not particularly limited. The plated layers 21b and 22b cover the entire or almost the entire surfaces of the base steel sheets 21a and 22a, respectively. The plated layers 21b and 22b are metal plated layers. The plated layers 21b and 22b may be the same as the plated layers exemplified for the steel sheet 23. That is, the steel sheets 21 and 22 may be aluminum plated steel sheets or zinc plated steel sheets, similar to the steel sheet 23. When the steel sheet 21 is a plated steel sheet, the thickness t of the steel sheet 21 may be 0.05 mm. 1 Similarly, when the steel sheet 22 is a plated steel sheet, the thickness t 2 is the combined thickness of the base steel sheet 22a and the plating layer 22b.

[0057] The plating layers 21b, 22b, and 23b are typically plating layers containing aluminum as a main component (aluminum-based plating layers). The configuration of the aluminum-based plating layers is not particularly limited. Known aluminum-based plating layers can be used as the plating layers 21b, 22b, and 23b.

[0058] The steel sheets 21, 22, and 23 may be plated steel sheets of the same type as the other steel sheets, or may be plated steel sheets of a different type from the other steel sheets. The steel sheets 21 and 22 may be steel sheets (bare materials) that do not have plating layers 21 b and 22 b on their surfaces. When two or more of the steel sheets 21, 22, and 23 are plated steel sheets, the coating weight of each steel sheet may be the same as or different from the other steel sheets.

[0059] (Heating Step) The prepared blank 20 is formed into the structural member 10 (FIGS. 1 and 2) by hot stamping (hot press working). During the hot stamping, the blank 20 is subjected to a heating step. Referring to FIG. 3E, in the heating step, the blank 20 is heated, for example, by a heating furnace 30. The plurality of steel plates 21, 22, and 23 included in the blank 20 are heated to an austenite transformation completion temperature (A c3 The steel plates 21, 22, and 23 are heated to, for example, 900° C. or higher, so that the microstructures of the steel plates 21, 22, and 23 are transformed, for example, entirely or almost entirely into an austenite phase.

[0060] (Forming Process) Referring to Fig. 3F, in the forming process, a die 40 is used to form the heated blank 20 into a structural member 10 (Figs. 1 and 2) that is annular in plan view and quench it. The blank 20 heated in the heating process is removed from the heating furnace 30 (Fig. 3E) and transported to the die 40. The die 40 is attached to a known press device. The die 40 includes, for example, a punch 41 and a die 42. The blank 20 is placed between the punch 41 and the die 42.

[0061] 3G , after the blank 20 is placed between the punch 41 and the die 42, the die 42 moves relatively close to the punch 41. The blank 20 is clamped (pressed) between the punch 41 and the die 42 and formed into a shape that conforms to the forming surfaces of the punch 41 and the die 42. The blank 20 remains clamped between the punch 41 and the die 42. The blank 20 is cooled (quenched) by the die 40, and its microstructure is transformed into martensite. This allows the structural member 10 to be manufactured from the blank 20.

[0062] FIG. 4 is a cross-sectional view of the structural member 10 after hot stamping. FIG. 4 shows a cross-section of the structural member 10 at the position of the steel plate 21 ( FIGS. 3B and 3C ) to which the black coating 25 was applied at the blank 20 stage. This structural member 10 includes a member body 11 and a coating 12. The coating 12 is provided on the steel plate 21. The black coating 25 ( FIGS. 3B and 3C ) that was applied to the steel plate 21 in the blank 20 becomes the coating 12 through hot stamping. Although not shown, the black coating 25 ( FIGS. 3B and 3D ) that was applied to the steel plate 22 in the blank 20 becomes the coating 12 through hot stamping. The coating 12 is provided on surfaces 216, 226 ( FIG. 3B ) of each of the steel plates 21, 22 that are located outside the overlap portion 241. If the coating 25 before hot stamping contains carbon black, this carbon black will be almost completely removed by the high temperature heating during hot stamping, but may remain on the member body 11. If the coating 25 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping may not contain carbon black or may contain 0.500 g / m 2 In some cases, the coating 12 after hot stamping contains carbon black. When the coating 12 contains carbon black, the carbon black content in the coating 12 is 0 g / m 2 Furthermore, when the coating 26 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping satisfies the central formula: 24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )} is, for example, 120.0 or more and 150.0 or less.

[0063] When the coating 25 (FIGS. 3B and 3C) before hot stamping satisfies the above formula (1), the coating 12 after hot stamping contains one or more oxides (metal oxides) selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide at a concentration of, for example, 0 g / m 2 More preferably, 0.001 g / m 2 The metal oxide content of the coating 12 is, for example, 0.500 g / m 2In this way, when the metal oxide remains on the structural member 10, that is, when the coating 12 is 0 g / m or less, 2 When the coating 25 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping has a metal oxide content of 0 to 0.30 g / m or more, which is more desirable because it improves the corrosion resistance of the structural member 10. 2 Contains silica.

[0064] The carbon black content, metal oxide content, and silica content in the coating 12 can be measured in the same manner as for the coating 25 at the blank 20 stage. Specifically, a vehicle body part is disassembled to obtain an annular structural member 10, and an analytical sample is obtained from the structural member 10, for example, by laser cutting. For example, an analytical sample is obtained from each of the multiple steel plates included in the structural member 10. The analytical sample is obtained from the center or its vicinity of the top plate of each steel plate having an open cross section. The obtained analytical sample is adjusted by polishing the cross section to outside the heat-affected zone during laser cutting, to prepare a sample for coating analysis. Surface analysis of the coating 12 for elements derived from carbon black (e.g., C) and elements derived from oxides (Zr, Zn, and Ti) can be performed using EPMA to confirm the dispersion state of carbon black and metal oxide in the coating 12. Because the coating 12 is present on the front and / or back side of the structural member 10 depending on the location, both the front and back sides of the analytical sample are analyzed.

[0065] In many cases, the outermost surface layer of the structural member 10 is, for example, an electrodeposition coating film. In such cases, the coating layer that is below the electrodeposition coating film layer and above the alloyed metal plating layer is analyzed. The carbon black content X in the coating 12 is CB can be measured by cross-sectional analysis of the coating 25 using a TEM. That is, a cross-sectional analysis of the coating 12 is performed by TEM-EDS analysis on an area of ​​a predetermined size (thickness of the coating 12 × 5 μm), and the thickness of the coating 12 and the area ratio of particles with a carbon content of 70 mass % or more in that area are measured. The density of carbon black is defined as ρ (ton / m 3), the film thickness is d (μm), and the area ratio is a (%), the value expressed by ρ×d×a is the carbon black content X CB (g / m 2 ) The oxide content X Oxide can be determined by performing elemental analysis of the coating layer that is present below the electrodeposition coating layer and above the alloyed metal plating layer using the above-mentioned X-ray fluorescence analyzer, and quantifying the amounts of metal Zr, metal Zn, and metal Ti.

[0066] After the forming process (hot stamping), the steel sheet 21 can have a tensile strength of, for example, 0.5 GPa or more, and preferably has a tensile strength of 1.0 GPa or more. Similarly, after the forming process (hot stamping), the steel sheets 22 and 23 ( FIG. 1 ) can have a tensile strength of, for example, 0.5 GPa or more, and preferably has a tensile strength of 1.0 GPa or more. At least one of the steel sheets 21, 22, and 23 may have a tensile strength of 1.5 GPa or more after the forming process. The tensile strength of each of the steel sheets 21, 22, and 23 may be the same as or different from the tensile strength of the other steel sheets.

[0067] [Effect] When the blank 20 is heated during hot stamping, the minimum plate thickness t min In the steel sheet 23 having the above-mentioned thickness, iron diffuses from the base steel sheet 23a to the plating layer 23b, forming a diffusion layer. The diffusion layer becomes thicker as the heating time of the blank 20 becomes longer, which may reduce the corrosion resistance or weldability of the steel sheet 23 due to the plating layer 23b. In order to ensure the corrosion resistance and weldability of the steel sheet 23, it is preferable that the thickness of the diffusion layer be kept below a predetermined value. For example, when the steel sheet 23 has a plating layer 23b with a coating weight of 50 to 80 g / m 2 In the case of a steel sheet having a thickness of about 15 μm, the thickness of the diffusion layer is preferably 15 μm or less. 2 In the case of a thin steel sheet, the thickness of the diffusion layer is preferably 10 μm or less. maxThe emissivity of the surfaces 216, 226 of the steel sheets 21, 22 located outside the overlap portion 241 having a thickness of 1000 Å is higher than the emissivity of at least one of the other surfaces of the steel sheets 21, 22, 23. That is, the surfaces 216, 217 on both sides of the overlap portion 241 of the steel sheets 21, 22 are treated to increase the emissivity. As a result, when the blank 20 is heated during hot stamping, the temperature rise rate of the overlap portion 241 can be increased, and the heating time of the overlap portion 241 can be shortened. Therefore, in the thinnest steel sheet 23, which has been heated first, excessive alloying of the plating layer 23b progresses, and heating of the blank 20 can be terminated before the diffusion layer grows to a thickness exceeding a predetermined thickness. As a result, the maximum sheet thickness t max The strength of the overlap portion 241 having the minimum thickness t min This ensures the corrosion resistance (rust prevention) of the steel plate 23. Furthermore, by reducing the thickness of the diffusion layer, the weldability of the steel plate 23 is more easily ensured.

[0068] As described above, according to the blank 20 of this embodiment, the maximum plate thickness t max Therefore, it is possible to heat the entire blank 20 to the temperature required for hot stamping before the alloying of the plating layer 23b in the thinnest steel sheet 23 progresses excessively, and it is possible to secure a process window for the heating conditions in the manufacture of the structural member 10. Therefore, it is possible to increase the temperature rise rate of the overlap portion 241 having the maximum sheet thickness t max The strength of the overlap portion 241 and the minimum plate thickness t min This allows the manufacture of a structural member 10 that also has a rust prevention function at the position of the steel plate 23. Furthermore, by increasing the temperature rise rate of the overlap portion 241, the heating time of the blank 20 can be shortened, thereby improving the productivity of the structural member 10. Furthermore, by shortening the heating time of the blank 20, energy consumption in the manufacture of the structural member 10 is suppressed, and the amount of greenhouse gases generated during heating can be reduced.

[0069] In this embodiment, the steel sheets 21, 22, and 23 included in the blank 20 may all be plated steel sheets. In this case, when the blank 20 is formed into the structural member 10 by hot stamping, the generation of oxide scale can be suppressed. Therefore, after hot stamping, it is not necessary to subject the structural member 10 to a process for removing oxide scale, such as shot blasting. This allows for increased productivity of the structural member 10.

[0070] For example, when the plating layers 21b, 22b, and 23b of the steel sheets 21, 22, and 23 are aluminum-based plating layers, the maximum plate thickness t max The overlap portion 241 has a minimum plate thickness t min The aluminum-based plating layer is white, which tends to reflect heat energy and inhibit the temperature rise of the overlap portion 241. However, in the blank 20 according to the present embodiment, the surfaces 216, 226 of the steel sheets 21, 22 arranged on both sides of the overlap portion 241 are treated to increase the emissivity. Therefore, even if the steel sheets 21, 22 forming the overlap portion 241 are plated steel sheets having an aluminum-based plating layer, the temperature rise of the overlap portion 241 in the heating process can be promoted and the heating time of the overlap portion 241 can be shortened. Therefore, the corrosion resistance and weldability of the thin-walled steel sheet 23 can be ensured, and the productivity of the structural member 10 can be improved.

[0071] In this embodiment, in the heating process, first, the blank 20 is heated to the minimum thickness t min The steel plate 23 having a maximum plate thickness t reaches the temperature in the austenite region, and then the portions of the steel plate 23 having a maximum plate thickness t reach the temperature in the austenite region in order. max In the case where the steel plates 21, 22, and 23 included in the blank 20 have different thicknesses as in the present embodiment, the overlap portion 241 having the minimum thickness t min and maximum plate thickness t max If there is too much difference between the thickness t min For a steel plate 23 having a plate thickness t maxThe temperature rise of the overlap portion 241 having the minimum thickness t min and maximum plate thickness t max Ratio to: t max / t min is preferably 3.2 or less. This allows the overlap portion 241 to be sufficiently heated until the phase transformation to austenite is completed before the alloying of the plating layer 23b of the thinnest steel sheet 23 progresses and the diffusion layer becomes thicker, causing a loss of corrosion resistance, even if there is a difference in thickness between the steel sheets 21, 22, and 23. This makes it easier to ensure a process window in the manufacture of the structural member 10.

[0072] In this embodiment, in order to increase the emissivity of the overlap portion 241, a coating 25 can be applied to the surfaces 216, 226 of the steel sheets 21, 22 opposite the mating steel sheet. The emissivity of the coating 25 (at a temperature of 25°C and a wavelength of 8.0 μm) is, for example, 60% or more. This allows efficient radiative heating of the overlap portion 241, making it easier to increase the temperature rise rate of the overlap portion 241 during the heating process.

[0073] In this embodiment, the coating 25 is made of a material containing carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a carbon black content of 0 to 0.30 g / m 2 The carbon black content X may be the following: CB (g / m 2 ), and the oxide content X Oxide (g / m 2 ) preferably satisfies the above formula (1). As described in Patent Document 1, formula (1) is a function of the ratio (%) of the increase in the temperature rise rate (°C / s) and the carbon black content X CB and oxide content X OxideEquation (1) defines the relationship between the carbon black and the oxide. Equation (1) indicates that carbon black primarily functions as a heat absorbing material in the temperature range up to 700°C, and that oxide primarily functions as a heat absorbing material in the temperature range of 700°C or higher. When coating 25 satisfies equation (1), the emissivity at a wavelength of 8.0 μm at 25°C tends to be 60% or higher for both outer surfaces 216, 226 of overlap portion 241 to which coating 25 is applied.

[0074] The carbon black and oxides can be dispersed throughout the entire surface of the coating 25 that is perpendicular to the thickness direction of the steel sheet 21. This facilitates uniform emissivity of the surfaces 216, 226 of the steel sheets 21, 22 located on both outer sides of the overlap portion 241. Therefore, the overlap portion 241, which is the thickest, can be heated quickly and uniformly in the heating process.

[0075] However, the configuration of the coating 25 is not limited thereto. The coating 25 may be a substantially black coating in order to increase the emissivity of both outer surfaces 216, 226 of the overlap portion 241 compared to an untreated coating. For example, the coating 25 may contain graphite or soot instead of or in addition to carbon black. Alternatively, the coating 25 may contain, for example, an acicular compound having a hexagonal crystal structure with an aspect ratio of 4 to 50 inclusive in order to increase the emissivity of both outer surfaces 216, 226 of the overlap portion 241. The compound having a hexagonal crystal structure is typically graphite (C), but may also be lanthanum silicate, magnesium diboride, beryllium oxide (beryllia), zinc oxide, β-quartz, goethite (NiS), wurtzite (ZnS), or the like.

[0076] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0077] In the above embodiment, the minimum plate thickness t minThe emissivity of both surfaces of the steel plate 23 having the minimum thickness t is smaller than the emissivity of the surfaces 216 and 226 located outside the overlap portion 241 of the steel plates 21 and 22. That is, the steel plate 23 is not provided with the coating 25 like the overlap portion 241. However, min In the steel plate 23 having the above structure, the emissivity of at least one surface may be substantially equal to the emissivity of the surfaces 216, 226 located on both outer sides of the overlap portion 241. For example, one or both surfaces of the steel plate 23 may be coated with the same coating 25 as the overlap portion 241. However, from the viewpoint of ensuring the process window, it is preferable that the black coating 25 is not applied to at least one surface of the steel plate 23. That is, the thickness t at which the emissivity of the surfaces 216, 226 located on the outer sides of the overlap portion 241 of each of the steel plates 21, 22 is minimum min It is preferable that the emissivity is greater than that of at least one surface of the steel plate 23 having the emissivity.

[0078] In the above embodiment, in the steel sheets 21 and 22, the emissivity of the surfaces 217 and 227 located inside the overlap portion 241 is lower than the emissivity of the surfaces 216 and 226 located outside the overlap portion 241. That is, in the steel sheets 21 and 22, the surfaces 217 and 227 located inside the overlap portion 241 are not provided with the coating 25. However, in the steel sheet 21, the surface 217 located inside the overlap portion 241 may be coated with the coating 25. Similarly, in the steel sheet 22, the surface 227 located inside the overlap portion 241 may be coated with the coating 25. However, from the viewpoint of uniformly heating the blank 20 during hot stamping, it is preferable that in each of the steel sheets 21 and 22, the surfaces 216 and 226 outside the overlap portion 241 are coated with the substantially black coating 25, and the surfaces 217 and 227 located inside the overlap portion 241 are not coated with the coating 25. When both surfaces 216, 217 of the steel plate 21 are coated with the coating 25, heating of the portion of the steel plate 21 that is not overlapped with the steel plate 22 progresses, the diffusion layer becomes thicker, and it may become difficult to ensure the corrosion resistance and weldability of the steel plate 21. Similarly, when both surfaces 226, 227 of the steel plate 22 are coated with the coating 25, heating of the portion of the steel plate 22 that is not overlapped with the steel plate 21 progresses, the diffusion layer becomes thicker, and it may become difficult to ensure the corrosion resistance and weldability of the steel plate 22. Therefore, in order to more easily ensure good corrosion resistance and weldability, it is preferable that the coating 25 is provided on the surfaces 216, 226 located outside the overlap portion 241 of the steel plates 21, 22, while the coating 25 is not provided on the surfaces 217, 227 located inside the overlap portion 241.

[0079] In the above embodiment, the presence of the substantially black coating 25 reduces the maximum plate thickness t maxThe emissivity of both outer surfaces 216, 226 of the overlap portion 241 having the coating 25 is higher than the emissivity of one or more other surfaces of the steel plates 21, 22, 23. However, the method of increasing the emissivity of a selected portion of the blank 20 is not limited to the coating 25. For example, the emissivity of the selected portion can be made higher than that of the other portions by increasing the surface roughness of the selected portion compared to the surface roughness of the other portions.

[0080] In the above embodiment, the steel plates 21, 22, and 23 included in the blank 20 may each be a single layer or multiple layers. That is, the steel plates 21, 22, and 23 may each be a single steel plate or a plate material formed by overlapping a plurality of steel plates.

[0081] In the above embodiment, the ends of the steel plates 21 and 22 are overlapped and joined to form an overlap portion 241. Similarly, the ends of the steel plates 21 and 23 are overlapped and joined to form an overlap portion 242. Furthermore, the ends of the steel plates 22 and 23 are overlapped and joined to form an overlap portion 243. However, it is sufficient for the blank 20 to include at least one overlap portion. In other words, the steel plate 23 does not necessarily have to be overlapped and joined to the steel plates 21 and 22. The steel plate 23 may be butt-joined to one or both of the steel plates 21 and 22.

[0082] In the above embodiment, the blank 20 includes three steel plates 21, 22, and 23. However, the number of steel plates included in the blank 20 is not limited to this. The blank 20 may be made up of two steel plates, or may include four or more steel plates. The blank 20, which is annular in plan view, typically includes three or more steel plates. The maximum plate thickness t maxThe steel sheets 21, 22 forming the overlap portion 241 having the above-mentioned structure are treated to increase the emissivity on the surfaces 216, 226 located outside the overlap portion 241. The other steel sheets may or may not be treated to increase the emissivity. The blank 20 may include one or more steel sheets that have not been treated to increase the emissivity on one or both sides.

[0083] In the blank 20 according to the above embodiment, the minimum plate thickness t min The steel plates 21 and 22, which are different from the steel plate 23 constituting the portion having the maximum plate thickness t max However, the steel plate 21 or the steel plate 22 forming the overlap portion 241 has a minimum thickness t min The steel plate may have the following structure.

[0084] In the above embodiment, the maximum plate thickness t max However, in the blank 20, there is only one overlap portion 241 having the maximum plate thickness t max In this case, there may be a plurality of overlapping portions having the maximum plate thickness t max Preferably, all overlapping portions having a thickness of 100 Å are treated on both outer surfaces to enhance emissivity.

[0085] In the blank 20 according to the above embodiment, the plurality of steel plates 21, 22, 23 have different thicknesses. However, two or more of the steel plates included in the blank 20 may have the same thickness, or all of the steel plates may have the same thickness. When all of the steel plates included in the blank 20 have the same thickness, the portions of each steel plate that do not form the overlap portion have the smallest thickness t min Each overlap portion has a maximum plate thickness t max In this case, the maximum plate thickness t max The emissivity of both outer surfaces of the overlapping portion is greater than the emissivity of at least one of the other surfaces. max / tmin is 2.0.

[0086] In the above embodiment, the mold 40 used for hot stamping the blank 20 includes a punch 41 and a die 42. However, the configuration of the mold 40 is not limited to the example described in the above embodiment. The mold 40 may further include, for example, a pad and a blank holder.

[0087] In the above embodiment, the main body 11 of the structural member 10 includes a front pillar 111, a center pillar 112, and a rocker 113. However, the member main body 11 may further include other components. For example, as shown in FIG. 5 , the member main body 11 may further include a rear pillar 114. The structural member 10 according to the above embodiment is a door ring component having a single ring shape (single door ring component). On the other hand, the structural member shown in FIG. 5 is a door ring component having a double ring shape (double door ring component). When manufacturing a double door ring component, the blank used as the raw material also has a double ring shape.

[0088] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.

[0089] [First Example] In order to confirm the effects of the present disclosure, a CAE analysis was performed on a press-formed (hot stamped) structural member that is a single door ring part, using commercially available software (AUTOFORM R.10, manufactured by AUTOFORM) while changing the type (material type) and thickness of the steel plate included in the structural member, as well as the division pattern of the structural member.

[0090] The steel plates used in this analysis are shown in Table 1.

[0091]

[0092] In Table 1, the material type is listed in the order of plating type, tensile strength, and application (hot stamping). Regarding the coating specifications, the black coating is a black coating containing carbon black and metal oxide. "Black coating - one side" means that one entire side of the steel sheet is coated with a black coating. "Black coating - both sides" means that both entire sides of the steel sheet are coated with a black coating.

[0093] The division patterns of the structural members are shown in Figures 6A to 6G. Figures 6A to 6G show the number of steel plates (materials) included in the structural member, which is a single door ring part, and the positions of the joints between the steel plates in the structural member. In Figures 6A to 6G, each steel plate is given a number in parentheses.

[0094] The analysis conditions and results for division patterns 1 and 2 shown in Figures 6A and 6B are shown in Table 2. In Figures 6A and 6B, the structural member is formed from three materials (1) to (3). Each of materials (1) to (3) is overlapped and joined with the adjacent material.

[0095]

[0096] In Table 2, the "time to reach 910°C" is the time required for the blank to reach 910°C. min The material having the above temperature reaches 910°C (A c3 The "heating completion time" is the time required for the part of the blank that has the slowest temperature rise to reach 910°C from the start of heating the blank until it becomes hot stampable. The "process window (PW)" is the time required for the part of the blank that has the slowest temperature rise to reach 910°C from the start of heating the blank until it becomes hot stampable. min This is the value obtained by adding the allowable heating time (245 seconds) after a material having the above temperature reaches 910°C to the time it takes to reach 910°C, and subtracting the time it takes to complete heating. The larger this value, the wider the process window of heating conditions is for hot stamping structural members.

[0097] Referring to Table 2 and FIG. 6A, in Example 1, the material (1) and the material (2) have the maximum plate thickness t maxAn overlap portion having a thickness of t = 2.8 mm is formed, and a black coating is applied to the surface located outside the overlap portion in each of the raw materials (1) and (2). On the other hand, a black coating is not applied to the surface located inside the overlap portion in each of the raw materials (1) and (2). In Example 1, the raw material (3) has a minimum plate thickness t min = 1.2 mm, and a black coating was applied to only one side of the blank (3). In Comparative Example 1, which had the same combination of material type and plate thickness as Example 1, a black coating was not applied to any of the blanks (1) to (3). In Example 1, a black coating was applied to both outer sides of the thickest overlap portion, which promoted the temperature rise of this overlap portion and significantly reduced the time to complete heating of the blank compared to Comparative Example 1. In Example 1, although the time to reach 910°C was faster than in Comparative Example 1 due to the application of a black coating to the thinnest blank (3), the process window was expanded by nearly 60 seconds compared to Comparative Example 1.

[0098] Referring to Table 2 and FIG. 6B, in Example 3, the material (1) and the material (3) have the maximum plate thickness t max In Example 3, the blank (2) has a minimum thickness t = 3.4 mm, and the surfaces of the blanks (1) and (3) located outside the overlapping portions are provided with a black coating. On the other hand, the surfaces of the blanks (1) and (3) located inside the overlapping portions are not provided with a black coating. min = 1.2 mm, and a black coating was applied to only one side of the raw material (2). In Comparative Example 2, which had the same combination of material type and plate thickness as Example 3, a black coating was not applied to any of the raw materials (1) to (3). In Example 3, a black coating was applied to both outer sides of the thickest overlap portion, which promoted the temperature rise of this overlap portion and significantly reduced the time to complete heating of the blank compared to Comparative Example 2. In Example 3, a black coating was applied to the thinnest raw material (2), which resulted in an earlier time to reach 910°C than in Comparative Example 2, but the process window was expanded by more than 70 seconds compared to Comparative Example 2. In Comparative Example 2, the process window of the heating conditions was eliminated (negative).

[0099] In Example 2, the material (2) and the material (3) have the maximum plate thickness t max An overlap portion having a thickness of t = 2.9 mm is formed, and a black coating is applied to the surface located outside the overlap portion in each of the raw materials (2) and (3). On the other hand, a black coating is not applied to the surface located inside the overlap portion in each of the raw materials (2) and (3). In Example 2, the raw material (1) has a minimum plate thickness t min = 1.2 mm. It was also confirmed that the process window was sufficiently secured in Example 2.

[0100] The analysis conditions and results for division patterns 3 and 4 shown in Figures 6C and 6D are shown in Table 3. In Figures 6C and 6D, the structural member is formed from four materials (1) to (4). Each of materials (1) to (4) is overlapped and joined with the adjacent material.

[0101]

[0102] In Examples 4 to 10 in Table 3, as in Examples 1 to 3 (Table 2), at least the maximum plate thickness t max A black coating was placed on both outer surfaces of the overlapping portion. Therefore, a sufficient process window for the heating conditions was ensured for Examples 4 to 10. When each Example was compared with the corresponding Comparative Example, it was found that the process window was expanded.

[0103] For example, in Example 8, the material (1) and the material (3) have the maximum plate thickness t max An overlap portion having a thickness of 4.0 mm was formed, and a black coating was applied to the surface located outside the overlap portion in each of raw materials (1) and (3) (Table 3 and FIG. 6D). On the other hand, in Comparative Example 4, the combination of material type and plate thickness was the same as in Example 8, but a black coating was not applied to any of the materials, including the overlap portion. In Example 8, the temperature rise in the overlap portion was accelerated, and the time to complete heating of the blank was significantly shortened compared to Comparative Example 4. In Example 8, the process window was expanded by more than 100 seconds compared to Comparative Example 4. In Comparative Example 4, the process window of the heating conditions was eliminated (negative).

[0104] For example, in Example 9, the materials (1) and (3), and the materials (3) and (4) have the maximum plate thickness t max An overlap portion having a thickness of 2.6 mm was formed, and a black coating was applied to the surfaces of each of the raw materials (1), (3), and (4) located outside the overlap portion (Table 3 and FIG. 6D). On the other hand, in Comparative Example 7, the combination of material type and plate thickness was the same as in Example 9, but the raw materials (1) and (3) forming the overlap portion were not provided with a black coating. In Example 9, the temperature rise in the overlap portion was accelerated, and the blank heating completion time was significantly shortened compared to Comparative Example 7. In Example 9, the process window was expanded by more than 80 seconds compared to Comparative Example 7. In Comparative Example 7, a black coating was applied to both sides of the thinnest raw material (4), and the time to reach 910°C was slightly more than 10 seconds earlier than in Example 9. However, in Example 9, the blank heating completion time was shortened by more than 70 seconds compared to Comparative Example 7. Therefore, even considering the difference in the time to reach 910°C, it can be said that the process window was expanded compared to Comparative Example 7.

[0105] The analysis conditions and results for division patterns 5 and 6 shown in Figures 6E and 6F are shown in Table 4. In Figures 6E and 6F, the structural member is formed from five materials (1) to (5). Each of materials (1) to (5) is overlapped and joined with the adjacent material.

[0106]

[0107] In Examples 11 to 16 in Table 4, as in Examples 1 to 10 (Tables 2 and 3), at least the maximum plate thickness t max A black coating was placed on both outer surfaces of the overlapping portion. Therefore, a sufficient process window for the heating conditions was ensured for Examples 11 to 16. When each Example was compared with the corresponding Comparative Example, it was found that the process window was expanded.

[0108] For example, in Example 13, the material (1) and the material (2) have the maximum plate thickness t maxAn overlap portion having a thickness of 3.2 mm was formed, and a black coating was applied to the surface located outside the overlap portion of each of the raw materials (1) and (2) (Table 4 and FIG. 6F). On the other hand, in Comparative Example 9, the combination of material type and plate thickness was the same as in Example 13, but a black coating was not applied to any of the raw materials, including the overlap portion. In Example 13, the temperature rise in the overlap portion was accelerated, and the time to complete heating of the blank was significantly shortened compared to Comparative Example 9. In Example 13, the process window was expanded by more than 90 seconds compared to Comparative Example 9. In Comparative Example 9, the process window of the heating conditions was eliminated (negative).

[0109] For example, in Example 15, the material (1) and the material (3) have the maximum plate thickness t max In Example 15, the blanks (1) and (3) had overlapping portions with a thickness of t = 3.0 mm, and a black coating was applied to the surface located outside the overlapping portion (Table 4 and Figure 6F). max An overlap portion having a thickness of 3.0 mm was formed, and a black coating was applied to the surface of each of the raw materials (3) and (4) located outside the overlap portion. On the other hand, in Comparative Example 11, the combination of material type and plate thickness was the same as in Example 15, but a black coating was not applied to any of the raw materials, including the overlap portion. In Example 15, the temperature rise in the overlap portion was accelerated, and the time to complete heating of the blank was significantly shortened compared to Comparative Example 11. In Example 15, the process window was extended by more than 60 seconds compared to Comparative Example 11.

[0110] Second Example Regarding the press forming (hot stamping) of a structural member that is a double door ring part, an analysis similar to that of the first example was carried out while changing the material type and plate thickness of the structural member, as well as the division pattern of the structural member.

[0111] As with the first embodiment, the steel plates used as raw materials were selected from those shown in Table 1. The division patterns of the structural members are as shown in Figures 7A to 7D. Figures 7A to 7D show the number of steel plates (raw materials) included in the structural members that are double door ring components, and the positions of the joints between the steel plates in the structural members. In Figures 7A to 7D, each steel plate used as raw material is given a number in parentheses.

[0112] The analysis conditions and results for division patterns 8 and 9 shown in Figures 7A and 7B are shown in Table 5. In Figures 7A and 7B, the structural member is formed from six materials (1) to (6). Each of materials (1) to (6) is overlapped and joined with the adjacent material.

[0113]

[0114] Referring to Table 5, in Examples 17 to 19, materials (1) and (3) have the maximum plate thickness t max = 3.4 mm, and a black coating was applied to the surfaces of materials (1) and (3) located outside the overlapping portion. On the other hand, in Comparative Examples 12 and 13, no black coating was applied to any of materials (1) to (6), including the overlapping portion.

[0115] From Table 5, in Examples 17 to 19, the maximum plate thickness t max The temperature rise in the overlapping portion was promoted, and the time to complete heating of the blank was significantly shortened compared to Comparative Examples 12 and 13. As a result, in Examples 17 to 19, the process window of the heating conditions was significantly expanded compared to Comparative Examples 12 and 13.

[0116] The analysis conditions and results for division patterns 10 and 11 shown in Figures 7C and 7D are shown in Table 6. In Figures 7C and 7D, the structural member is formed from seven materials (1) to (7). Each of materials (1) to (7) is overlapped and joined with the adjacent material.

[0117]

[0118] Referring to Table 6, in Examples 20 to 22, materials (1) and (3) have the maximum plate thickness t max= 3.4 mm, and a black coating was applied to the surfaces of materials (1) and (3) located outside the overlapping portion. On the other hand, in Comparative Examples 14 and 15, no black coating was applied to any of materials (1) to (7), including the overlapping portion.

[0119] From Table 6, in Examples 20 to 22, the maximum plate thickness t max The temperature rise in the overlapping portion was promoted, and the time to complete heating of the blank was significantly shortened compared to Comparative Examples 14 and 15. As a result, in Examples 20 to 22, the process window of the heating conditions was significantly expanded compared to Comparative Examples 14 and 15.

[0120] [Third Example] Regarding press forming (hot stamping) of a structural member that is a single door ring part, the maximum plate thickness t max and minimum plate thickness t min In order to check the effect of the difference between max / t min The analysis conditions and results are shown in Table 7.

[0121]

[0122] The division pattern of Test Examples 1 and 3 is division pattern 7 shown in FIG. 6G. The division pattern of Test Example 2 and the Reference Example is division pattern 5 shown in FIG. 6E. In Test Examples 1 to 3 and the Reference Example, each material forms an overlap portion at the joint with the other material. In all of Test Examples 1 to 3, the maximum plate thickness t max A black coating is applied to both outer surfaces of the overlapping portion. In each of Test Examples 1 to 3, each of the raw materials (1) to (5) has a thickness difference between it and one or more other raw materials. On the other hand, in the Reference Example, the raw materials (1) to (5) all have the same thickness. In addition, in the Reference Example, a black coating is not applied to any of the raw materials (1) to (5), including the overlapping portion.

[0123] In the reference example, there is no difference in thickness between the materials (1) to (5), so the minimum thickness t min Maximum thickness t for (thickness of materials (1) to (5)) max (Thickness of overlapping portion) ratio: tmax / t min In the reference example, the maximum plate thickness t max and minimum plate thickness t min The difference between (t max / t min ) is not large, so it is possible to secure a certain process window for the heating conditions without increasing the emissivity of both outer surfaces of the overlapping part. On the other hand, if there is a difference in thickness between materials (1) to (5), the maximum thickness t max and minimum plate thickness t min The difference between (t max / t min In this case, the effect of increasing the emissivity of both outer surfaces of the overlap portion (by providing a black coating) is likely to be significantly achieved.

[0124] From Table 7, the maximum plate thickness t max When a black coating is applied to both outer surfaces of the overlapping portion having max / t min It can be seen that even when t exceeds 2.0, the heating completion time is unlikely to be long, and the process window can be secured (Test Examples 1 and 2). max / t min Although the value of t is relatively large at 3.2, the process window was secured. max / t min In Test Example 3, where the value exceeded 4.0, the process window was negative.

[0125] According to the results of this analysis, when there is a difference in thickness between materials, t max / t min It is preferable that t≦3.2. max / t min >2.0, but t max / t min It may be ≧2.5.

[0126] The productivity of the structural members and the greenhouse gas emission ratio were evaluated for Test Examples 1 to 3. The rust prevention performance of the structural members was also evaluated for Test Examples 1 to 3. The evaluation results are shown in Table 8.

[0127]

[0128] As shown in Table 8, in Test Examples 1 and 2, the time required to complete heating of the blank was shorter than in Test Example 3, and therefore the productivity of the structural components was improved compared to Test Example 3. In addition, in Test Examples 1 and 2, the time required to complete heating of the blank was shorter than in Test Example 3, and the amount of energy consumed in manufacturing the structural components was reduced, so the greenhouse gas emission rate during manufacturing was also reduced. In Table 8, "Productivity" is the number of blanks (structural components) that can be heat-treated per minute in a heating furnace. "Greenhouse gas emission rate" is the rate of greenhouse gas emission compared to Test Example 3. The amount of greenhouse gases generated during the heating process was calculated by setting the hourly power consumption of the multi-stage electric heating furnace for heating hot stamp blanks at 450 kWh, the furnace temperature at 920 °C, the daily operating time at 15 hours, and the heating and waiting time in the heating furnace at 3 hours, assuming component production at the productivity shown in Table 8. The amount was allocated to the power consumption per structural component and multiplied by the greenhouse gas intensity per kWh of the average electricity in Japan in 2018 (from the LCA database, AIST IDEA v3.2). Other greenhouse gas emissions (other than the heating process) during the manufacture of structural components were calculated using the method described in a published literature on LCA calculations for automotive parts (Masahiro Kubo and two others, "Evaluation of Greenhouse Gas Emissions over the Life Cycle of Lightweight Steel Bodies and Parts," Spring Meeting Academic Lecture Proceedings, Society of Automotive Engineers of Japan, 2022).

[0129] In Test Examples 1 and 2, the blank heating completion time was shortened compared to Test Example 3. Therefore, excessive alloying of the thinnest plating layer of the material during blank heating did not proceed, and the deterioration of the material's rust prevention performance (corrosion resistance) was suppressed. Test Examples 1 and 2 were able to maintain high rust prevention performance compared to Test Example 3. Corrosion prevention performance was evaluated by cutting corrosion evaluation test pieces (evaluation samples) from the overlap portion and other portions of the hot-stamped structural member. The corrosion prevention performance was evaluated by performing a combined cycle test (CCT) under cycle conditions similar to those in a real environment, as specified in the accelerated corrosion test method (VDA233-102) of the German Association of the Automotive Industry (VDA). In Table 8, "○" indicates that all evaluation samples obtained from multiple portions of the structural member had no problems with rust prevention performance and were evaluated as good, and "×" indicates that even one of the evaluation samples was evaluated as having poor rust prevention.

[0130] Test Example 3 was evaluated as low in comparison with Test Examples 1 and 2. However, as explained in Examples 1 to 3, the maximum plate thickness t max By increasing the emissivity of both outer surfaces of the overlapping portion, it is possible to obtain the effect of accelerating the temperature rise of the overlapping portion and shortening the heating completion time. max Since the emissivity of both outer surfaces of the overlapping portion is increased, it is estimated that the time required to complete heating of the blank is shorter, and that the productivity, greenhouse gas generation rate, and rust prevention performance are improved, compared to a case where, for example, the combination of material type and plate thickness is the same as in Test Example 3 and no treatment is applied to the both outer surfaces of the overlapping portion to increase the emissivity.

[0131] 10: Structural member 11: Member body 111: Front pillar 112: Center pillar 113: Rocker 12: Coating 20: Blank 21: Steel plate (first steel plate) 22: Steel plate (second steel plate) 23: Steel plate 21a, 22a, 23a: Base steel plate 21b, 22b, 23b: Plating layer 241, 242, 243: Overlap portion 25: Coating 40: Mold

Claims

1. A blank for hot stamping, comprising a plurality of steel sheets which are arranged and joined to have a ring shape in a plan view of the blank, the plurality of steel sheets including: a first steel sheet; and a second steel sheet having an end which is overlapped and joined to an end of the first steel sheet to form an overlap portion together with the end of the first steel sheet, wherein of the plurality of steel sheets, a steel sheet constituting a portion having a smallest sheet thickness in the blank is a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet, the overlap portion has the largest sheet thickness in the blank, and the emissivity of a surface located outside the overlap portion in each of the first steel sheet and the second steel sheet is greater than the emissivity of at least one of the other surfaces in the plurality of steel sheets.

2. A blank according to claim 1, wherein each of the plurality of steel sheets is a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet.

3. A blank according to claim 2, wherein the plating layer is an aluminum-based plating layer.

4. A blank according to claim 1, wherein the surfaces of the first steel plate and the second steel plate located outside the overlapping portion are covered with a coating having an emissivity of 60% or more at a wavelength of 8.0 μm at 25°C.

5. A blank according to claim 1, wherein the surfaces of the first steel plate and the second steel plate located outside the overlapping portion are coated with a coating, and the coating is a mixture of carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a metal oxide having a concentration of 0 to 0.30 g / m 2 and silica, and the content of the carbon black in the coating is X CB (g / m 2 ), the content of the oxide is X Oxide (g / m 2 ) and then X CB and X Oxide A blank that satisfies the following formula (1). 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide ))≦332.0 (1) 6. A blank according to claim 1, wherein the plurality of steel plates include two or more steel plates having different plate thicknesses, and the plate thickness of the overlapping portion is t max The thickness of the steel plate constituting the part having the smallest thickness in the blank is t min Then, t max / t min ≦3.2, blank.

7. A method for manufacturing a structural component, comprising the steps of: preparing a blank as described in any one of claims 1 to 6; heating the plurality of steel plates contained in the blank to a temperature equal to or higher than the austenite transformation completion temperature; and using a die to form the heated blank into a structural component that is annular in plan view and quenching it.

8. A structural member comprising: a first steel plate; and a second steel plate having an end portion which is overlapped and joined to an end portion of the first steel plate to form an overlap portion together with the end portion of the first steel plate, the main body being formed by a plurality of steel plates joined to each other and having an annular shape in a plan view; and one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, each of which is provided on a surface located outside the overlap portion of each of the first steel plate and the second steel plate, at a concentration of 0.001 g / m 2 A structural member comprising:

9. A structural member comprising: a first steel plate; and a second steel plate having an end portion which is overlapped and joined to an end portion of the first steel plate to form an overlap portion together with the end portion of the first steel plate, the main body being formed by a plurality of steel plates joined to each other and having an annular shape in a plan view; and a carbon black content of 0.500 g / m2 provided on the surface of each of the first steel plate and the second steel plate positioned outside the overlap portion. 2 A structural member comprising:

10. A structural member as claimed in claim 8 or 9, which is a door ring part of an automobile, and the member body includes a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar.

Citation Information

Patent Citations

  • Vehicle body side structural frame

    JP2021528248A

  • Overlapped blank and method for manufacturing hot stamp molding using the same

    JP2021154370A

  • Method of manufacturing blank for hot-press, and blank for hot-press

    JP2023180687A

  • Manufacturing method of hot press-formed product and steel plate

    JP7260765B2

  • Steel sheet for hot stamping and hot-stamped member

    WO2022215229A1

Cited By

  • Method for manufacturing welded steel sheets, method for manufacturing tailored blanks, method for manufacturing hot press-formed products, welded steel sheets, tailored blanks, and hot press-formed products

    JP2026166184A