Resin composition, molded body, and modifier
The combination of polyethylene terephthalate and β-methyl-δ-valerolactone polymers in a resin composition addresses the brittleness and flexibility limitations of polyethylene terephthalate, enhancing impact resistance and preventing bleed-out, thus expanding its application scope.
Patent Information
- Application Number
- PCT/JP2024/016166
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Polyethylene terephthalate resin compositions are brittle and lack sufficient impact resistance and flexibility, limiting their use in applications requiring these properties, and existing modifications with plasticizers often result in bleed-out issues.
A resin composition combining a polyethylene terephthalate polymer with a β-methyl-δ-valerolactone polymer, which enhances impact resistance and flexibility without the need for additional plasticizers and reduces bleed-out.
The resin composition achieves improved impact resistance, flexibility, and bleed-out resistance, making it suitable for a wider range of applications without the drawbacks of traditional plasticizer additions.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition, molded article, and modifier
[0001] The present invention relates to a resin composition containing a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer, a molded article made from the resin composition, and a modifier for polyethylene terephthalate polymers made from the β-methyl-δ-valerolactone polymer.
[0002] From the viewpoint of environmental concerns, there has been a demand for resins to replace polyvinyl chloride resin (PVC), and polyethylene terephthalate (PET) and blends thereof have been proposed as alternatives to polyvinyl chloride. Polyethylene terephthalate-based resins, such as polyethylene terephthalate and glycol-modified PET, which are amorphous copolyesters modified by replacing a portion of the ethylene glycol component of polyethylene terephthalate with cyclohexanedimethanol, are being used in a wide range of applications, such as containers and packaging materials for food, beverages, pharmaceuticals, etc., cases for electronic devices and office supplies, lids for molded containers, and ID card sheets, due to their excellent hardness and transparency. However, products made using polyethylene terephthalate-based resins are brittle, and their use may be limited in fields requiring impact resistance and flexibility. Therefore, improvements have been made to polyethylene terephthalate-based resins to impart physical properties suited to their applications.
[0003] For example, Patent Document 1 describes that an amorphous polyethylene terephthalate resin composition having excellent low-temperature flexibility and bleeding resistance can be obtained by blending an amorphous polyester resin with a plasticizer consisting of an aromatic monocarboxylic acid diester composed of an aromatic monocarboxylic acid and a glycol and / or glycol dimer. For example, Patent Document 2 describes that diacetyl monoacylglycerol, in which the fatty acid constituting the ester has 8 to 14 carbon atoms, can impart flexibility to polyethylene terephthalate products and glycol-modified polyethylene terephthalate products, which are amorphous copolyesters obtained by modifying polyethylene terephthalate by substituting part of the ethylene glycol component with cyclohexanedimethanol, without impairing transparency.
[0004] JP 2005-89630 A JP 2002-53742 A
[0005] The techniques described in Patent Documents 1 and 2 above improve the impact resistance and flexibility of resin compositions containing polyethylene terephthalate polymers to some extent, but are not fully satisfactory. Furthermore, when additives such as plasticizers are added to resin compositions containing polyethylene terephthalate polymers to impart impact resistance and flexibility, there is a problem that the additives such as plasticizers may bleed out from the resin composition. Therefore, an object of the present invention is to provide a resin composition having good impact resistance, flexibility, and bleed-out resistance.
[0006] As a result of intensive research to solve the above problems, the present inventors have conceived the following invention and found that the above problems can be solved.
[0007] [1] A resin composition comprising a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer. [2] The resin composition according to [1] above, wherein the polyethylene terephthalate polymer is amorphous. [3] The resin composition according to [2] above, wherein the polyethylene terephthalate polymer is a modified polyethylene terephthalate polymer obtained by modifying polyethylene terephthalate (PET) with at least one selected from the group consisting of cyclohexanedimethanol and glycol. [4] The resin composition according to any one of [1] to [3] above, wherein the β-methyl-δ-valerolactone polymer is represented by the following general formula (I): [In general formula (I), R 1represents a hydrogen atom, a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms has been substituted with a group represented by the following formula (X), or an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom in a branched alkyl group having 3 to 20 carbon atoms has been substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. R 2 represents a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is 2 to 1,000, and m is 2 to 1,000. R 2 When a plurality of and m are present, they may be the same or different.] [5] The resin composition according to any one of [1] to [4] above, containing 0.1 to 100 parts by mass of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the polyethylene terephthalate polymer. [6] The resin composition according to any one of [1] to [5] above, wherein the number average molecular weight of the β-methyl-δ-valerolactone polymer is 500 to 100,000. [7] A molded article made from the resin composition according to any one of [1] to [6] above. [8] A modifier for polyethylene terephthalate polymer, comprising a β-methyl-δ-valerolactone polymer represented by the following general formula (I): [In general formula (I), R 1represents a hydrogen atom, a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms has been substituted with a group represented by the following formula (X), or an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom in a branched alkyl group having 3 to 20 carbon atoms has been substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. R 2 represents a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is 2 to 1,000, and m is 2 to 1,000. R 2 When a plurality of m's are present, they may be the same or different from each other.
[0008] According to the present invention, it is possible to provide a resin composition having good impact resistance, flexibility and bleed-out resistance.
[0009] The following is a description based on one example of an embodiment of the present invention. However, the embodiment shown below is an example for embodying the technical idea of the present invention, and the present invention is not limited to the following description. Furthermore, although preferred embodiments are shown in this specification, a combination of two or more of the individual preferred embodiments is also a preferred embodiment. For matters shown as numerical ranges, when there are several numerical ranges, the lower limit and upper limit can be selectively combined to form a preferred embodiment. Furthermore, in this specification, when a numerical range is described as "XX to YY," it means "XX or more and YY or less."
[0010] <Resin Composition> The resin composition of this embodiment contains a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer. By including a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer, the resin composition has good impact resistance, flexibility, and bleed-out resistance. Conventionally, in order to impart impact resistance to a polyethylene terephthalate polymer, it was necessary to add an additive that easily bleeds out, such as a plasticizer. In this embodiment, by using a resin composition containing a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer, impact resistance is improved without the addition of an additive such as a plasticizer. As a result, the resin composition of this embodiment also has good bleed-out resistance.
[0011] [Polyethylene terephthalate polymer] The polyethylene terephthalate polymer used in this embodiment is not particularly limited as long as it has a structural unit derived from ethylene glycol and a structural unit derived from at least one selected from the group consisting of terephthalic acid and a terephthalic acid ester. The polyethylene terephthalate polymer may contain a structural unit other than a structural unit derived from polyethylene terephthalate (polyester unit). That is, it may contain a structural unit other than a structural unit derived from ethylene glycol and a structural unit derived from at least one selected from the group consisting of terephthalic acid and a terephthalic acid ester. Examples of structural units other than the structural unit derived from ethylene glycol and the structural unit derived from at least one selected from the group consisting of terephthalic acid and a terephthalic acid ester include units having an ether bond such as a polyethylene glycol unit, a polypropylene glycol unit, and a polytetramethylene ether glycol unit.
[0012] From the viewpoint of obtaining a resin composition having better impact resistance and flexibility, the polyethylene terephthalate polymer is preferably amorphous.
[0013] From the same viewpoint, it is also preferable to use a modified polyethylene terephthalate polymer obtained by modifying polyethylene terephthalate (PET) with at least one selected from the group consisting of cyclohexanedimethanol and glycol.
[0014] In the present invention, the term "amorphous" refers to a polyethylene terephthalate polymer that has been melted, dried, and then kept at room temperature for 5 to 10 days, and then cooled to a temperature of -50°C or lower, preferably -100°C or lower, at a rate of -10°C / min or faster using a differential scanning calorimeter (DSC), and then kept at that temperature for 5 to 15 minutes. When the temperature is then increased at a rate of 10°C / min to a temperature at which melt molding is possible, preferably 150°C or higher, the resulting temperature is increased at a rate of 10°C / min. In this case, no peak of at least 0.5 J / 40 g or higher is observed other than a change in heat capacity due to glass transition.
[0015] From the viewpoint of obtaining a resin composition having better impact resistance and flexibility, the polyethylene terephthalate polymer preferably contains 70 mol% or more of structural units derived from ethylene glycol and at least one structural unit selected from the group consisting of terephthalic acid and terephthalate esters, and more preferably 90 mol% or more, and may even be 100 mol%. Furthermore, when the polyethylene terephthalate polymer is a modified polyethylene terephthalate polymer obtained by modifying polyethylene terephthalate (PET) with at least one selected from the group consisting of cyclohexanedimethanol and glycol, the polyethylene terephthalate polymer preferably contains 5 to 60 mol%, and more preferably 20 to 40 mol%, of the at least one selected from the group consisting of cyclohexanedimethanol and glycol. One type of polyethylene terephthalate polymer may be used alone, or two or more types may be used in combination.
[0016] From the viewpoints of impact resistance and flexibility, the number average molecular weight of the polyethylene terephthalate polymer is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 15,000 or more. From the viewpoints of moldability and compatibility with the β-methyl-δ-valerolactone polymer, it is preferably 200,000 or less, more preferably 150,000 or less, and even more preferably 100,000 or less. That is, the number average molecular weight of the polyethylene terephthalate polymer is preferably 5,000 to 200,000, more preferably 10,000 to 150,000, and even more preferably 15,000 to 100,000. The number average molecular weight of the polyethylene terephthalate polymer can be determined in terms of standard polystyrene by gel permeation chromatography (GPC) measurement. When using a commercially available product, the catalog value may be used.
[0017] [β-Methyl-δ-valerolactone Polymer] The β-methyl-δ-valerolactone polymer used in this embodiment is preferably a polymer represented by the following general formula (I). The following polymer, due to its structure represented by general formula (I), serves as a superior modifier for polyethylene terephthalate polymers. The following polymer is a polymer obtained by ring-opening polymerization of β-methyl-δ-valerolactone, in which at least one hydroxyl group at the molecular end is modified with another functional group, resulting in a polymer with reduced thermal decomposition properties and capable of suppressing a decrease in the glass transition temperature of the resin composition. Furthermore, the polymer can improve the impact resistance of the resin composition depending on the molecular end structure and number of ends. Furthermore, since the raw material for the polymer represented by the following general formula (I) is β-methyl-δ-valerolactone, the β-methyl-δ-valerolactone polymer is expected to have good biodegradability.
[0018]
[0019] In general formula (I), R 1represents a hydrogen atom, a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms has been substituted with a group represented by formula (X) described below, or an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom in a branched alkyl group having 3 to 20 carbon atoms has been substituted with a group represented by formula (X) described below.
[0020] Examples of the linear alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-icosyl group.
[0021] From the viewpoint of ease of handling, the linear alkyl group having 1 to 20 carbon atoms is preferably a linear alkyl group having 1 to 16 carbon atoms, more preferably a linear alkyl group having 1 to 10 carbon atoms, and even more preferably a linear alkyl group having 1 to 5 carbon atoms. Specifically, at least one selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an n-butyl group, and an n-pentyl group is preferred.
[0022] Examples of the branched alkyl group having 3 to 20 carbon atoms include an isopropyl group, a 1-methylpropyl group, a 2-methylpropyl group, a t-butyl group, a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a 2-ethylpropyl group, a 1,1-diethylpropyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylbutyl group, a 2,2-dimethylbutyl group, a 3,3-dimethylbutyl group, a 1,3,3-trimethylbutyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, a 3, 3-dimethylbutyl group, 1-propylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 4,4-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 4-ethylpentyl group, 1-propylpentyl group, 2-propylpentyl group, 1-butylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 5-methylhexyl group, 5,5-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group ethyl group, 3-ethylhexyl group, 4-ethylhexyl group, 1-propylhexyl group, 2-propylhexyl group, 3-propylhexyl group, 1-butylhexyl group, 2-butylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 5-methylheptyl group, 6-methylheptyl group, 6,6-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 4-ethylheptyl group, 5-ethylheptyl group, 1-propylheptyl group, 2-propylheptyl group, 3-propyl dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 4-ethyloctyl group, 5-methyloctyl group, 6-methyloctyl group, 7-methyloctyl group, 7,7-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 4-ethyloctyl group, 5-ethyloctyl group, 6-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, 5-methylnonyl group, 6-methylnonyl group, 7-methylnonyl group, 8-methylnonyl group, 3,5,5-trimethylhexyl group, etc.
[0023] From the viewpoint of ease of handling, the branched alkyl group having 3 to 20 carbon atoms is preferably a branched alkyl group having 3 to 16 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 5 carbon atoms. Specifically, at least one selected from the group consisting of an isopropyl group, a 1-methylbutyl group, a 3-methylbutyl group, and a 2,2-dimethylpropyl group is preferred.
[0024] Examples of the linear alkenyl group having 2 to 20 carbon atoms include ethenyl, n-propenyl, n-butenyl (e.g., 2-butenyl and 3-butenyl), n-pentenyl (e.g., 3-pentenyl and 4-pentenyl), n-hexenyl (e.g., 1-hexenyl and 5-hexenyl), n-heptenyl (e.g., 1-heptenyl and 1,3-heptadienyl), n-octenyl (e.g., 7-octenyl and 2,7-octadienyl), n-nonenyl (e.g., 3-nonenyl and 3,6-nonadienyl), and n-decenyl (e.g., 1,3-decadienyl and 1,3,5-decatrienyl). n-nyl group), n-undecenyl group (for example, 2-undecenyl and 2,4-undecadienyl group), n-dodecenyl group (for example, 2-dodecenyl group), n-tridecenyl group (for example, 2-tridecenyl group), n-tetradecenyl group (for example, 2-tetradecenyl group), n-pentadecenyl group (for example, 2-pentadecenyl group), n-hexadecenyl group (for example, 2-hexadecenyl group), n-heptadecenyl group (for example, 2-heptadecenyl group), n-octadecenyl group (for example, 2-octadecenyl group), n-nonadecenyl group (for example, 2-nonadecenyl group), n-icosenyl group (for example, 2-icosenyl group), and the like.
[0025] From the viewpoint of handleability, the linear alkenyl group having 2 to 20 carbon atoms is preferably a linear alkenyl group having 2 to 15 carbon atoms, more preferably a linear alkenyl group having 3 to 10 carbon atoms, and even more preferably a linear alkenyl group having 3 to 6 carbon atoms.
[0026] Examples of branched alkenyl groups having 3 to 20 carbon atoms include an isopropenyl group, a 1-methylpropenyl group, a 2-methylpropenyl group, a t-butenyl group, a 1,1-dimethylpropenyl group, a 2,2-dimethylpropenyl group, a 1,2-dimethylpropenyl group, a 1-ethylpropenyl group, a 2-ethylpropenyl group, a 1,1-diethylpropenyl group, a 1-methylbutenyl group, a 2-methylbutenyl group, a 3-methyl-2-butenyl group, a 3-methyl-3-butenyl group, a 1,1-dimethylbutenyl group, a 2,2-dimethylbutenyl group, 3,3-dimethylbutenyl group, 1,3,3-trimethylbutenyl group, 1-ethylbutenyl group, 2-ethylbutenyl group, 3,3-dimethylbutenyl group, 1-propylbutenyl group, 1-methylpentenyl group, 2-methylpentenyl group, 3-methylpentenyl group, 4-methylpentenyl group, 4,4-dimethylpentenyl group, 1-ethylpentenyl group, 2-ethylpentenyl group, 3-ethylpentenyl group, 4-ethylpentenyl group, 1-propylpentenyl group, 2-propylpentenyl group, 1-butylpentenyl group, 1-methylhexenyl group, 2-methylhexenyl group, 3-methylhexenyl group, 4-methylhexenyl group, 5-methylhexenyl group, 5,5-dimethylhexenyl group, 1-ethylhexenyl group, 2-ethylhexenyl group, 3-ethylhexenyl group, 4-ethylhexenyl group, 1-propylhexenyl group, 2-propylhexenyl group, 3-propylhexenyl group, 1-butylhexenyl group, 2-butylhexenyl group, 1-methylheptenyl group, 2-methylheptenyl group, 3-methylheptenyl group, 4-methylheptenyl group a 1-methyloctenyl group, a 5-methylheptenyl group, a 6-methylheptenyl group, a 6,6-dimethylheptenyl group, a 1-ethylheptenyl group, a 2-ethylheptenyl group, a 3-ethylheptenyl group, a 4-ethylheptenyl group, a 5-ethylheptenyl group, a 1-propylheptenyl group, a 2-propylheptenyl group, a 3-propylheptenyl group, a 1-methyloctenyl group, a 2-methyloctenyl group, a 3-methyloctenyl group, a 4-methyloctenyl group, a 5-methyloctenyl group, a 6-methyloctenyl group, a 7-methyloctenyl group, a 7,Examples include a 7-dimethyloctenyl group, a 1-ethyloctenyl group, a 2-ethyloctenyl group, a 3-ethyloctenyl group, a 4-ethyloctenyl group, a 5-ethyloctenyl group, a 6-ethyloctenyl group, a 1-methylnonenyl group, a 2-methylnonenyl group, a 3-methylnonenyl group, a 4-methylnonenyl group, a 5-methylnonenyl group, a 6-methylnonenyl group, a 7-methylnonenyl group, an 8-methylnonenyl group, and a 3,5,5-trimethylhexenyl group.
[0027] From the viewpoint of handleability, the branched alkenyl group having 3 to 20 carbon atoms is preferably a branched alkenyl group having 3 to 15 carbon atoms, more preferably a branched alkenyl group having 3 to 10 carbon atoms, and even more preferably a branched alkenyl group having 3 to 6 carbon atoms.
[0028] Examples of aryl groups having 6 to 12 carbon atoms include phenyl, 2-methylphenyl, 2,4-dimethylphenyl, and 2-naphthyl groups. Phenyl groups are preferred. Examples of arylalkyl groups having 7 to 12 carbon atoms include phenylmethyl, phenylethyl, phenylpropyl, phenylbutyl, phenylpentyl, phenylhexyl, naphthylmethyl, and naphthylethyl groups. Phenylmethyl groups are preferred.
[0029] In formula (I), n represents the average number of repeating units. n is 2 to 1,000, preferably 2 to 800, more preferably 4 to 500, and even more preferably 8 to 300. When n is 2 or more, a more excellent modifying effect can be obtained. Furthermore, when n is 1,000 or less, good moldability and productivity can be obtained.
[0030] In an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom of a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), and in an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X), the bond represented by * in the following formula (X) is bonded to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms:
[0031]
[0032] R in the above formula (X) 2 is R 2 The straight-chain alkyl group having 1 to 20 carbon atoms bonded to formula (X) above can be exemplified by the same groups exemplified above as the "straight-chain alkyl group having 1 to 20 carbon atoms." The straight-chain alkyl group having 1 to 20 carbon atoms bonded to formula (X) above is preferably a straight-chain alkyl group having 1 to 15 carbon atoms, more preferably a straight-chain alkyl group having 1 to 10 carbon atoms, even more preferably a straight-chain alkyl group having 2 to 10 carbon atoms, and even more preferably a straight-chain alkyl group having 2 to 5 carbon atoms. The branched alkyl group having 3 to 20 carbon atoms bonded to formula (X) above can be exemplified by the same groups exemplified above as the "branched alkyl group having 3 to 20 carbon atoms." The branched alkyl group having 3 to 20 carbon atoms bonded to formula (X) above is preferably a branched alkyl group having 3 to 15 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 5 carbon atoms. Alternatively, the oxygen-containing hydrocarbon group may be an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to all terminal carbon atoms of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by formula (X) above, or an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by formula (X) above.
[0033] In formula (X), m represents the average number of repeating units. m is 2 to 1,000, preferably 2 to 800, more preferably 4 to 500, even more preferably 5 to 300, and may be 8 to 300. When m is 2 or more, the viscosity of the β-methyl-δ-valerolactone polymer does not become too low. Furthermore, when m is 1,000 or less, the polymer has good handleability and productivity.
[0034] The average number of repetitions (n and m) is 1It can be calculated from the overall degree of polymerization of the β-methyl-δ-valerolactone polymer determined by H-NMR measurement. More specifically, it can be calculated by the method described in the Examples. The overall degree of polymerization of the β-methyl-δ-valerolactone polymer is the sum of the average number of repeating units contained in the polymer.
[0035] The overall degree of polymerization in the β-methyl-δ-valerolactone polymer is preferably 2 to 10,000, more preferably 4 to 6,000, even more preferably 6 to 3,000, still more preferably 8 to 2,000, and even more preferably 10 to 1,600.
[0036] R 1 In the above formula (I), when a plurality of groups represented by the formula (X) are present, they may be the same or different from each other. 2 There may be a plurality of m and m. That is, there may be two or more groups represented by formula (X) in the above formula (I). 2 When a plurality of m's are present, they may be the same or different from each other. When a plurality of m's are present, that is, when two or more repeating units represented by the average repeat number m are present, they may be the same or different from each other.
[0037] R 1 represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the terminal carbon atom of a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the above formula (X), the following structure can be specifically exemplified as the above general formula (I): Example 1: R 1 However, when the linear alkyl group having carbon number Q represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the terminal carbon atom is substituted with a group represented by formula (X), the general formula (I) is represented by the following general formula (I-a), where Q is 1 to 20.
[0038]
[0039] <Example 2> R 1However, when the ethyl group represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the terminal carbon atom in the ethyl group is substituted with a group represented by the above formula (X), the above general formula (I) is represented by the following general formula (I-b):
[0040]
[0041] R 1 represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the formula (X), the following structure can be specifically exemplified as the general formula (I): Example 3: R 1 However, when all of the terminal carbon atoms of the 2-methylpropyl group represent an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the carbon atom is substituted with a group represented by formula (X), the general formula (I) is represented by the following general formula (I-c):
[0042]
[0043] <Example 4> R 1 represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the carbon atom at each of the two terminal carbon atoms of a 2,2-dimethylpropyl group is substituted with a group represented by formula (X), then general formula (I) is represented by the following general formula (I-d):
[0044]
[0045] <Example 5> R 1 represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the carbon atom at each of the two terminal carbon atoms of a 2,2-dimethylbutyl group is substituted with a group represented by formula (X), then general formula (I) is represented by the following general formula (I-e):
[0046]
[0047] <Example 6> R 1 represents an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to the carbon atom at each terminal carbon atom of a 2,2-dimethylpropyl group is substituted with a group represented by formula (X), the general formula (I) is represented by the following general formula (If):
[0048]
[0049] R 1 From the viewpoint of easily obtaining a modifying effect, is preferably a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms has been substituted with a group represented by formula (X) above, or an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom in a branched alkyl group having 3 to 20 carbon atoms has been substituted with a group represented by formula (X) above.
[0050] In the general formula (I) and the general formulas (I-a) to (If), R 2 represents a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. 2 The linear alkyl group having 1 to 20 carbon atoms represented by R can be exemplified by the same groups exemplified above as the "linear alkyl group having 1 to 20 carbon atoms". 2 From the viewpoint of ease of handling, the linear alkyl group having 1 to 20 carbon atoms represented by R is preferably a linear alkyl group having 1 to 15 carbon atoms, more preferably a linear alkyl group having 1 to 10 carbon atoms, and even more preferably a linear alkyl group having 1 to 5 carbon atoms. Specifically, at least one selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an n-butyl group, and an n-pentyl group is preferred. 2 The branched alkyl group having 3 to 20 carbon atoms represented by R can be exemplified by the same groups exemplified above as the "branched alkyl group having 3 to 20 carbon atoms". 2From the viewpoint of ease of handling, the branched alkyl group having 3 to 20 carbon atoms is preferably a branched alkyl group having 3 to 15 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, and even more preferably a branched alkyl group having 3 to 5 carbon atoms. Specifically, at least one selected from the group consisting of an isopropyl group, a 1-methylbutyl group, and a 2,2-dimethylpropyl group is preferred.
[0051] R 2 The linear alkenyl group having 2 to 20 carbon atoms represented by R can be exemplified by the same groups exemplified above as the "linear alkenyl group having 2 to 20 carbon atoms". 2 From the viewpoint of ease of handling, the linear alkenyl group having 2 to 20 carbon atoms represented by R is preferably a linear alkenyl group having 2 to 15 carbon atoms, more preferably a linear alkenyl group having 3 to 10 carbon atoms, and even more preferably a linear alkenyl group having 3 to 6 carbon atoms. 2 Examples of the branched alkenyl group having 3 to 20 carbon atoms represented by R include the same groups exemplified above as the "branched alkenyl group having 3 to 20 carbon atoms". 2 From the viewpoint of ease of handling, the branched alkenyl group having 3 to 20 carbon atoms represented by R is preferably a branched alkenyl group having 3 to 15 carbon atoms, more preferably a branched alkenyl group having 3 to 10 carbon atoms, and even more preferably a branched alkenyl group having 3 to 6 carbon atoms. 2 The aryl group having 6 to 12 carbon atoms represented by R can be exemplified by the same groups exemplified above as the "aryl group having 6 to 12 carbon atoms". 2 The aryl group having 6 to 12 carbon atoms represented by R is preferably a phenyl group. 2 The arylalkyl group having 7 to 12 carbon atoms represented by R can be exemplified by the same groups exemplified above as the "arylalkyl group having 7 to 12 carbon atoms". 2 The arylalkyl group having 7 to 12 carbon atoms represented by R is preferably a phenylmethyl group. 2 is preferably a linear alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 12 carbon atoms, from the viewpoint of easily obtaining a modifying effect.
[0052] (Number Average Molecular Weight) The number average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 500 or more, more preferably 1,000 or more, and even more preferably 1,500 or more, from the viewpoint of easily achieving a more excellent modifying effect. Furthermore, from the viewpoint of moldability and productivity, the number average molecular weight of the polymer is preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 50,000 or less. That is, the number average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 500 to 100,000, more preferably 1,000 to 80,000, and even more preferably 1,500 to 50,000. The "number average molecular weight" of the β-methyl-δ-valerolactone polymer described herein is the number average molecular weight in terms of standard polystyrene determined by gel permeation chromatography (GPC). Detailed measurement methods can be performed according to the methods described in the Examples.
[0053] (Weight Average Molecular Weight) The weight average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 1,500 or more and 200,000 or less. A weight average molecular weight of 1,500 or more is likely to exhibit an even more excellent modifying effect. A weight average molecular weight of 200,000 or less is likely to provide excellent handleability and productivity during molding. The weight average molecular weight of the β-methyl-δ-valerolactone polymer is more preferably 2,200 or more, and even more preferably 3,000 or more. Furthermore, the weight average molecular weight of the β-methyl-δ-valerolactone polymer is more preferably 160,000 or less, even more preferably 125,000 or less, and even more preferably 100,000 or less. That is, the weight average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 1,500 to 200,000, more preferably 2,200 to 160,000, even more preferably 3,000 to 125,000, and even more preferably 3,000 to 100,000. Furthermore, the "weight average molecular weight" of the β-methyl-δ-valerolactone polymer described in this specification is the weight average molecular weight calculated in terms of standard polystyrene as determined by gel permeation chromatography (GPC). Details of the measurement method can be found in the methods described in the Examples.
[0054] (Molecular Weight Distribution (Mw / Mn)) The molecular weight distribution (Mw / Mn) of the β-methyl-δ-valerolactone polymer is preferably 1.0 to 3.0, more preferably 1.0 to 2.6, even more preferably 1.1 to 2.5, still more preferably 1.1 to 2.0, and even more preferably 1.2 to 1.8. The "molecular weight distribution" of the β-methyl-δ-valerolactone polymer described in this specification is a value determined from the number average molecular weight and weight average molecular weight in terms of standard polystyrene determined by gel permeation chromatography (GPC) measurement. The detailed method for measuring the number average molecular weight and weight average molecular weight can be according to the methods described in the Examples.
[0055] (Viscosity) In the present invention, "viscosity" refers to the viscosity of a polymer measured with an E-type viscometer. The measurement temperature can be optimized depending on the molecular weight, etc. The viscosity of the β-methyl-δ-valerolactone polymer is preferably 10 mPa·s or more at a measurement temperature of 80°C, and more preferably 50 mPa·s or more at a measurement temperature of 80°C, from the viewpoint of achieving a more excellent modifying effect. Furthermore, from the viewpoint of moldability and productivity, the viscosity is preferably 200,000 mPa·s or less at a measurement temperature of 80°C, and more preferably 150,000 mPa·s or less at a measurement temperature of 80°C. That is, the viscosity of the β-methyl-δ-valerolactone polymer is preferably 10 to 200,000 mPa·s or less, and more preferably 50 to 150,000 mPa·s at a measurement temperature of 80°C. Furthermore, when the β-methyl-δ-valerolactone polymer is measured with an E-type viscometer, the measurement temperature can be set according to the molecular weight, etc. In another preferred embodiment, the β-methyl-δ-valerolactone polymer has a viscosity of preferably 100 to 150,000 mPa·s, more preferably 400 to 150,000 mPa·s, and even more preferably 600 to 100,000 mPa·s at a measurement temperature of 30°C. In another preferred embodiment, the β-methyl-δ-valerolactone polymer has a viscosity of preferably 50 to 150,000 mPa·s, more preferably 200 to 150,000 mPa·s, and even more preferably 600 to 120,000 mPa·s at 60°C.
[0056] (Method for Producing β-methyl-δ-valerolactone Polymer) From the viewpoint of productivity and simplicity, or when producing a high-molecular-weight polymer, it is preferable to employ a method for producing the β-methyl-δ-valerolactone polymer, which includes a step of adding a terminal modifier to a reaction solution obtained by reacting β-methyl-δ-valerolactone with an alcohol compound or water and a base catalyst to carry out a terminal modification reaction (hereinafter also referred to as the "reaction step"). The production method is characterized in that the terminal modifier is added directly to a reaction solution obtained by reacting β-methyl-δ-valerolactone with an alcohol compound or water and a base catalyst. That is, after ring-opening polymerization of β-methyl-δ-valerolactone, the terminal modifier can be added to the reactor in which the ring-opening polymerization was carried out, without first removing the ring-opened polymer, thereby carrying out terminal modification of the ring-opened polymer. Since the reaction step involves carrying out the ring-opening polymerization reaction and the terminal modification reaction in one pot, the production method can be considered a simplified process. Note that the polymer produced is not limited to the above production method.
[0057] <Alcohol Compound or Water> The alcohol compound that can be used in this embodiment is not particularly limited as long as the effects of the present invention can be obtained. Examples of alcohol compounds include linear or branched aliphatic hydrocarbon alcohols having 1 to 20 carbon atoms, aromatic hydrocarbon alcohols having 6 to 12 carbon atoms, and alkylaromatic hydrocarbon alcohols having 7 to 12 carbon atoms. These alcohol compounds may have a saturated or unsaturated hydrocarbon group. Note that the above-mentioned "branched aliphatic hydrocarbon alcohols" have 3 to 20 carbon atoms. That is, examples of alcohol compounds include linear aliphatic hydrocarbon alcohols having 1 to 20 carbon atoms, branched aliphatic hydrocarbon alcohols having 3 to 20 carbon atoms, aromatic hydrocarbon alcohols having 6 to 12 carbon atoms, and alkylaromatic hydrocarbon alcohols having 7 to 12 carbon atoms. These alcohol compounds may have a saturated or unsaturated hydrocarbon group. Furthermore, the alcohol compound may be a monohydric alcohol or a polyhydric alcohol such as a dihydric alcohol or a trihydric alcohol. The water that can be used in this embodiment is not particularly limited as long as the effects of the present invention can be obtained. For example, tap water, distilled water, ion-exchanged water, industrial water, deionized water, etc. can be used.
[0058] <Base Catalyst> Examples of base catalysts that can be used in this embodiment include metal catalysts such as alkali metals and alkali metal compounds, as well as organic base compounds. A single base catalyst may be used alone, or two or more may be used in combination. Examples of alkali metal compounds include organic alkali metal compounds, alkali metal hydroxide compounds, and alkali metal hydrides, with organic lithium compounds such as butyllithium being preferred. Examples of organic base compounds include amine compounds having an amidine skeleton or a guanidine skeleton. Metal catalysts such as organomagnesium compounds and organozinc compounds can also be used as base catalysts. In the reaction step, it is preferable to add 0.005 to 1.5 molar equivalents of the base catalyst relative to the hydroxyl groups of the alcohol compound. When water is used, it is preferable to add 0.005 to 3 molar equivalents of the base catalyst relative to the water.
[0059] <β-Methyl-δ-valerolactone> β-Methyl-δ-valerolactone that can be used in this embodiment can be produced by a known method. For example, it can be produced by a known method using 2-hydroxy-4-methyltetrahydropyran or the like as a raw material (see, for example, Japanese Patent Publication No. 6-53691). Furthermore, commercially available β-methyl-δ-valerolactone can be used, and it can be derived from either petroleum or biomass. In the reaction step, it is preferable to add 5 to 1,500 molar equivalents of β-methyl-δ-valerolactone relative to the hydroxyl groups of the alcohol compound. Furthermore, when water is used, it is preferable to add 5 to 1,500 molar equivalents of β-methyl-δ-valerolactone relative to the water.
[0060] <Terminal Modifier> Examples of terminal modifiers that can be used in this embodiment include acid anhydrides and acid halides (acid halides are also referred to as "halogenated esters"). The acid anhydrides and acid halides (halogenated esters) are not particularly limited as long as the effects of the present invention can be obtained. For example, acid anhydrides and acid halides (halogenated esters) having at least one group selected from the group consisting of a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an arylalkyl group having 7 to 12 carbon atoms can be used. Note that in the case of the "branched alkyl group," the number of carbon atoms is 3 to 20, and in the case of the "branched alkenyl group," the number of carbon atoms is 3 to 20. That is, acid anhydrides and acid halides (halogenated esters) having at least one group selected from the group consisting of a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an arylalkyl group having 7 to 12 carbon atoms can be used.
[0061] Specific examples of acid anhydrides include acetic anhydride, oxalic anhydride, propionic anhydride, succinic anhydride, maleic anhydride, benzoic anhydride, phthalic anhydride, glutaric anhydride, methacrylic anhydride, butyric anhydride, isobutyric anhydride, 1,8-naphthalic anhydride, trifluoroacetic anhydride, and cyclohexanecarboxylic anhydride. Specific examples of acid halides (halogenated esters) include acetyl chloride, propionyl chloride, butyroyl chloride, trifluoroacetyl chloride, benzoyl chloride, 2-furoyl chloride, hexanoyl chloride, phenylacetyl chloride, acetyl bromide, propionyl bromide, and benzoyl bromide. In the reaction step, it is preferable to add 1 to 20 molar equivalents of a terminal modifier relative to the hydroxyl groups of the alcohol compound. Furthermore, when water is used, it is preferable to add 1 to 20 molar equivalents of a terminal modifier relative to the water.
[0062] <Co-catalyst> In the reaction step, a co-catalyst may be added as necessary. Examples of the co-catalyst that can be used include amine compounds such as triethylamine, tributylamine, trioctylamine, imidazole, pyridine, aminopyridine, and 4-dimethylaminopyridine. In the reaction step, the co-catalyst can be added in an amount of 0.001 to 10 molar equivalents relative to the hydroxyl groups of the alcohol compound. Furthermore, when water is used, the co-catalyst can be added in an amount of 0.001 to 10 molar equivalents relative to the water.
[0063] The reaction step can be carried out in the presence of a solvent inert to the ring-opening polymerization reaction. Examples of the solvent include aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, n-hexane, and n-pentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.
[0064] <Reaction Conditions> In the reaction step, the reaction temperature when reacting β-methyl-δ-valerolactone with an alcohol compound or water and a base catalyst is usually 20 to 100°C, and the reaction time is usually 1 minute to 24 hours. In addition, in the reaction step, the reaction temperature when carrying out the terminal modification reaction after adding a terminal modifying agent to the reaction solution is usually 20 to 80°C, and the reaction time is usually 1 minute to 24 hours.
[0065] <Post-treatment step> The polymer represented by the general formula (I) can be produced through the above reaction step. If necessary, a post-treatment step may be carried out to isolate the produced polymer. As the post-treatment step, a suitable method can be adopted from known methods. For example, the reaction mixture after the reaction step can be washed with a reaction solvent or water, concentrated, and purified by a method typically used for separating and purifying organic compounds, such as distillation.
[0066] The resin composition of this embodiment preferably contains 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, and even more preferably 10 to 30 parts by mass of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the polyethylene terephthalate polymer. This content ratio allows for a resin composition with even better impact resistance.
[0067] Furthermore, the total content of the polyethylene terephthalate polymer and the β-methyl-δ-valerolactone polymer in the resin composition of this embodiment is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, still more preferably 98% by mass or more, and may be 100% by mass. With this content, the effects of the present invention are more significantly exhibited.
[0068] The content of the polyethylene terephthalate polymer in the resin composition of this embodiment is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less. That is, the content of the polyethylene terephthalate polymer in the resin composition of this embodiment is preferably 60 to 99% by mass, more preferably 70 to 98% by mass, and even more preferably 80 to 97% by mass. With the above content ratios, the effects of the present invention are more significantly exhibited.
[0069] The content of the β-methyl-δ-valerolactone polymer in the resin composition of this embodiment is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. That is, the content of the β-methyl-δ-valerolactone polymer in the resin composition of this embodiment is preferably 1 to 40% by mass, more preferably 2 to 30% by mass, and even more preferably 3 to 20% by mass. With the above content ratios, the effects of the present invention are more significantly exhibited.
[0070] The resin composition of this embodiment may contain resins other than polyethylene terephthalate polymers and β-methyl-δ-valerolactone polymers within the range that does not impair its physical properties. Examples of resins other than polyethylene terephthalate polymers and β-methyl-δ-valerolactone polymers include thermoplastic elastomers such as polyolefin thermoplastic elastomers, polystyrene thermoplastic elastomers, polyester thermoplastic elastomers, polyamide thermoplastic elastomers, and polyurethane thermoplastic elastomers, ABS resins, polyamide resins, polyolefin resins, polycarbonates, polyvinyl chloride, polystyrene resins, (meth)acrylic resins, fluorinated resins, polylactic acid (PLA), polycaprolactone (PCL), and polybutylene terephthalate. cellulose acetate (CA), starch polyester (Mater-Bi (registered trademark)), etc.).
[0071] [Additives] The resin composition of this embodiment may contain additives other than the polyethylene terephthalate polymer and the β-methyl-δ-valerolactone polymer. Examples of additives include inorganic fillers, softeners, heat aging inhibitors, antioxidants, hydrolysis resistance inhibitors, light stabilizers, antistatic agents, release agents, flame retardants, foaming agents, pigments, dyes, brighteners, UV absorbers, lubricants, and impact modifiers. These may be used alone or in combination of two or more. When using the above additives, the content of the additives in the resin composition may be determined appropriately depending on the desired physical properties of the resin composition.
[0072] [Method for Producing Resin Composition] The method for producing the resin composition of this embodiment is not particularly limited, and it is sufficient to uniformly mix the polyethylene terephthalate polymer, β-methyl-δ-valerolactone polymer, and, if necessary, additives. Examples of mixing methods include melt-kneading using a single-screw extruder, multi-screw extruder, Banbury mixer, heated roll, Brabender, various kneaders, etc., or melt-kneading by feeding each component through a separate inlet. Pre-blending may also be performed before melt-kneading. Examples of pre-blending methods include using a mixer such as a Henschel mixer, high-speed mixer, V-blender, ribbon blender, tumbler blender, or conical blender. The temperature during melt-kneading can be selected arbitrarily, preferably within the range of 140 to 280°C, taking into account the melting point, glass transition point (Tg), and decomposition temperature of the polyethylene terephthalate polymer.
[0073] <Molded Article> The present invention also provides a molded article made from a resin composition. The shape of the molded article may be any molded article that can be produced using the resin composition of this embodiment. Examples of molded articles include molded articles in various shapes such as pellets, films, sheets, plates, pipes, tubes, bottles, fibers, rods, fine particles, particles, and foams. The method for producing this molded article is not particularly limited, and it can be molded by various known molding methods, such as injection molding, blow molding, press molding, extrusion molding, calendar molding, and molding using a 3D printer.
[0074] <Applications> By mixing a polyethylene terephthalate polymer with a β-methyl-δ-valerolactone polymer represented by the above general formula (I) to form a resin composition, the impact resistance and flexibility (elongation) can be improved without the β-methyl-δ-valerolactone polymer bleeding out. Therefore, the present invention provides a modifier for polyethylene terephthalate polymers, comprising the β-methyl-δ-valerolactone polymer represented by the above general formula (I). Furthermore, a preferred embodiment is the use of the β-methyl-δ-valerolactone polymer represented by the above general formula (I) as a modifier for polyethylene terephthalate polymers.
[0075] The resin composition of this embodiment can be used in a variety of applications. Examples of uses of the resin composition include pharmaceutical packaging materials, food packaging materials, food packaging containers, sheets, flooring materials, automotive interior materials, agricultural materials, gardening materials, fishing materials, civil engineering and construction materials, stationery, medical supplies, and electrical and electronic components. The resin composition of this embodiment can also be used as a textile product. Examples of uses of textile products using the resin composition of this embodiment include construction materials, waterproofing, heat insulation, soundproofing, roofing materials, consumer apparel, interior decoration materials and the clothing industry, industrial apparel, medical products, household fixtures, protective equipment, packaging materials, cosmetic products, sanitary products, filtration materials, agricultural applications, construction applications, geotechnical applications, industrial applications, medical applications, transportation, eco-technology applications, packaging applications, personal protection, property protection, and sports applications.
[0076] The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to these.
[0077] <Measurement and Evaluation Methods> Various physical properties were measured or evaluated by the following methods.
[0078] [Total Degree of Polymerization of β-methyl-δ-valerolactone Polymer] In the Production Examples, the total degree of polymerization of the obtained β-methyl-δ-valerolactone polymer was 1The degree of polymerization was determined by H-NMR measurement. The proton signal of the raw material alcohol was used as a reference and the overall degree of polymerization was calculated from the ratio of the proton signals of the repeating units in the polymer. The average repeat numbers n and m are the values obtained by dividing the overall degree of polymerization calculated here by the number of hydroxyl groups in the raw material alcohol. The specific measurement method is as follows. (Measurement conditions) Apparatus: 400YH (manufactured by JEOL Ltd.) Solvent: deuterated chloroform (CDCl 3 ) Measurement temperature: 23°C Number of times of accumulation: 32 (Method of calculating the overall degree of polymerization) For example, in the case of Production Example 1, the terminal CH 3 (0.90-0.92 ppm, d) Proton number X and methyl branch CH of β-methyl-δ-valerolactone, which is a repeating structural unit 3 Using the number of protons Y of (0.98-1.00 ppm, d), the overall degree of polymerization was calculated using the following formula (1). The average repeat number n is calculated by dividing the overall degree of polymerization calculated here by 1, which is the number of hydroxyl groups in the raw material isoamyl alcohol. Overall degree of polymerization = 2 x Y / X (1)
[0079] [Number-Average Molecular Weight, Weight-Average Molecular Weight, and Molecular Weight Distribution of β-Methyl-δ-valerolactone Polymer] Using the β-methyl-δ-valerolactone polymer obtained in the Production Examples as a sample, the number-average molecular weight (Mn), weight-average molecular weight (Mw), and molecular weight distribution (Mw / Mn) were determined using standard polystyrene equivalent molecular weights by gel permeation chromatography (GPC). The specific measurement methods are as follows. <For Mn Less than 15,000> Samples with Mn less than 15,000 were measured as follows to determine Mn and Mw. Using a tetrahydrofuran (THF) solution as the eluent, 10 mg of the sample, calculated as resin, was weighed and dissolved in 1 mL of the eluent. The solution was passed through a 0.2 μm membrane filter to prepare a measurement sample. The specific measurement method is as follows. (Measurement conditions) Apparatus: HLC-EcoSEC8320GPC (manufactured by Tosoh Corporation) Column: Three columns, KF-803 (manufactured by Resonac Corporation), KF-802.5 (manufactured by Resonac Corporation), and KF-802 (manufactured by Resonac Corporation), were connected in series. Eluent: tetrahydrofuran Flow rate: 0.9 mL / min Sample injection amount: 30 μL Column temperature: 40°C Standard polystyrene: PSt Oligomer Kit (molecular weight 589 to 98,900) manufactured by Tosoh Corporation was used for cubic approximation. Detector: RI detector Mw / Mn was calculated from the obtained Mn and Mw.
[0080] <For Mn of 15,000 or More> Samples with an Mn of 15,000 or more were measured as follows to determine Mn and Mw. A tetrahydrofuran (THF) solution was used as the eluent. 1.0 mg of the sample, calculated as resin, was weighed and dissolved in 1 mL of the eluent. The solution was passed through a 0.2 μm membrane filter to prepare a measurement sample. The measurement conditions were as follows: (Measurement Conditions) Apparatus: HLC-8220 GPC (manufactured by Tosoh Corporation) Column: Two TSK-gel (registered trademark) SuperMultipore HZ-M (manufactured by Tosoh Corporation) columns were connected in series. Eluent: tetrahydrofuran Flow rate: 0.35 mL / min Sample injection volume: 10 μL Column temperature: 40°C Standard polystyrene: Polystyrene molecular weight standard (molecular weight 580 to 1,214,000) manufactured by GL Sciences Inc. was used for cubic approximation. Detector: RI detector Mw / Mn was calculated from the obtained Mn and Mw.
[0081] [Viscosity] In accordance with JIS K 7117-2:1999, the viscosity (unit: mPa s) of the polymers obtained in the Production Examples was measured at the measurement temperatures shown in Table 1 using an E-type viscometer ("TVE-25 type viscometer" manufactured by Toki Sangyo Co., Ltd.).
[0082] [Impact Resistance Test] (1) Preparation of Test Pieces for Impact Resistance Test The resin compositions obtained in the Examples and Comparative Examples were each subjected to a reduced pressure hot press ("IMC-183B" manufactured by Imoto Machinery Co., Ltd.) using an oil rotary pump to reduce the pressure to -0.1 MPaG, preheated at 200°C for 5 minutes, and pressed at 50 kN for 3 minutes. Thereafter, the resin compositions were subjected to a cooling press equipped with water flow cooling at 70 kgf / cm. 2The specimens were pressed at 100°C for 3 minutes to produce a 1.0 mm thick press plate. A 50 x 50 mm specimen was cut from the resulting press plate to prepare a test specimen. (2) Impact Resistance Test: Impact resistance was evaluated with reference to JIS K 7211-1:2006. Specifically, the test specimens were stored for 10 hours or more in a low-temperature constant temperature bath (ETAC Corporation's "HIFLEX FL714C") adjusted to the test temperature (0°C) shown in Table 2, for humidity control. After humidity control, the test specimens were measured using a DuPont impact tester (manufactured by Taiyu Kizai Co., Ltd.) according to the following steps (a) to (e) to evaluate their impact resistance. (a) Using a support bar, a 1 kg weight was set 0.5 m from the support base. (b) The test specimen was removed from the constant temperature bath and placed in an environment of 23°C and 49% humidity, and the test specimen was placed between the support base and the hammer. (c) The pressure rod is pulled out and the weight is dropped towards the hammer. At this time, the time from removing the test piece in (b) to dropping the weight in (c) must be completed in 5 seconds or less. (d) After the weight is dropped, the test piece is checked to see if it "breaks" or "does not break." (e) The operations (a) to (d) are performed on 20 test pieces, and 10 or more test pieces that did not break are considered to have passed ("G"), and less than 10 test pieces are considered to have failed ("NG").
[0083] [Tensile Test] (1) Preparation of Tensile Test Specimens The resin compositions obtained in the Examples and Comparative Examples were injection molded at a cylinder temperature of 200°C using an injection molding machine ("SE18DU" manufactured by Sumitomo Heavy Industries, Ltd.) to prepare JIS No. 3 (dumbbell-shaped No. 3) dumbbell test specimens in accordance with JIS K 6251:2017. (2) Tensile Test The breaking elongation of the obtained dumbbell test specimens was measured in accordance with JIS K 7127:1999. Specifically, the specimens were stored for 24 hours or more under conditions of 23°C and 49% humidity, and the breaking elongation (%) was measured using a universal testing machine ("INSTRON 5900R-5666" manufactured by Instron) at 23°C, 49% humidity, and a tensile speed of 200 mm / min. The measured value was the average of five measurements.
[0084] [Bleeding Resistance Test] The resin compositions obtained in the examples and comparative examples were injection molded at a cylinder temperature of 200°C using an injection molding machine ("SE18DU" manufactured by Sumitomo Heavy Industries, Ltd.) to prepare JIS No. 3 (dumbbell-shaped No. 3) dumbbell test pieces in accordance with JIS K 6251:2017. The obtained dumbbell test pieces were stored at 50°C for one week or more, and the surface condition was evaluated visually and by touch according to the following evaluation criteria. VG: No clear bleedout or stickiness was observed. G: At least one selected from the group consisting of slight bleedout and slight stickiness was observed, but this was at a level that was acceptable for practical use. NG: At least one selected from the group consisting of significant bleedout and significant stickiness was observed, and the product was not suitable for practical use.
[0085] <Materials> The materials used in the examples and comparative examples are as follows.
[0086] (Polyethylene terephthalate polymer) PET-1: Eastar 6763 Copolyester (manufactured by Eastman Chemical Co.) (Plasticizer) Plasticizer 1: Diacetyl monolauryl glycerol (manufactured by Tokyo Chemical Industry Co., Ltd.) (Impact modifier) Impact modifier 1: Kane Ace B-56 (manufactured by Kaneka Corporation)
[0087] [Production Example 1] A 500 mL four-neck glass flask was purged with nitrogen, and 7.9 g (90 mmol) of isoamyl alcohol and 231 g (2.0 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.84 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 11.0 g (108 mmol) of acetic anhydride and 0.55 g (4.5 mmol) of 4-dimethylaminopyridine dissolved in 5.5 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a β-methyl-δ-valerolactone polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 155 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-1") were measured as described above. The results are shown in Table 1. The obtained PMVL-1 is a β-methyl-δ-valerolactone polymer represented by the above-mentioned general formula (I), 1 , R 2 , n, and the overall degree of polymerization are as shown in Table 1.
[0088] [Production Example 2] A 500 mL four-neck glass flask was purged with nitrogen, and 11.3 g (183 mmol) of ethylene glycol and 184 g (1.6 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 1.18 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 44.2 g (433 mmol) of acetic anhydride and 2.23 g (18.3 mmol) of 4-dimethylaminopyridine dissolved in 20.8 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a β-methyl-δ-valerolactone polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), to obtain 150 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-2") were measured as described above. The results are shown in Table 1. The obtained PMVL-2 is a β-methyl-δ-valerolactone polymer represented by the above-mentioned general formula (I), 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1.
[0089] [Production Example 3] A 500 mL four-necked glass flask was purged with nitrogen, and 1.6 g (18.2 mmol) of isoamyl alcohol and 231 g (2.0 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.83 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 2.3 g (22.5 mmol) of acetic anhydride and 0.11 g (0.9 mmol) of 4-dimethylaminopyridine dissolved in 1.1 g of β-methyl-δ-valerolactone were added to the four-necked glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 162 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-3") were measured as described above. The results are shown in Table 1. The obtained PMVL-3 is a β-methyl-δ-valerolactone polymer represented by the above-mentioned general formula (I), 1 , R 2 , n, and the overall degree of polymerization are as shown in Table 1.
[0090] [Production Example 4] A 1,000 mL four-necked glass flask was purged with nitrogen, and 1.6 g (18.2 mmol) of isoamyl alcohol and 623 g (5.5 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 2.21 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 2.2 g (21.8 mmol) of acetic anhydride and 0.11 g (0.9 mmol) of 4-dimethylaminopyridine dissolved in 1.1 g of β-methyl-δ-valerolactone were added to the four-necked glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 450 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-4") were measured as described above. The results are shown in Table 1. The obtained PMVL-4 is a β-methyl-δ-valerolactone polymer represented by the above-mentioned general formula (I), 1 , R 2 , n, and the overall degree of polymerization are as shown in Table 1.
[0091] A 2000 mL four-neck glass flask was purged with nitrogen, and 1.8 g (29 mmol) of ethylene glycol, 202 g (1.8 mol) of β-methyl-δ-valerolactone, and 86.8 g of toluene were added and heated to 30°C. 1.5 mL of n-butyllithium (1.6 M hexane solution) was added and stirred at 30°C for 210 minutes. Next, 7.1 g (69 mmol) of acetic anhydride and 0.4 g (2.9 mmol) of 4-dimethylaminopyridine dissolved in 3.5 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 30°C for 60 minutes to obtain a reaction solution containing a polymer. The resulting reaction solution containing the polymer was purified by extraction with toluene and water and distillation using a thin-film evaporator (Shibata Scientific Instruments, Inc., "Molecular Distillation Apparatus MS-300"), yielding 139 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter, sometimes referred to as "PMVL-5") were measured as described above. The results are shown in Table 1. The obtained PMVL-5 is a polymer represented by the general formula (I) above, 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1.
[0092] [Production Example 6] A 5000 mL four-neck glass flask was purged with nitrogen, and 7.6 g (122 mmol) of ethylene glycol and 1457 g (12.8 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 1.18 mL of n-butyllithium (1.6 M hexane solution) was added thereto, and the mixture was stirred at 60°C for 11 hours. Next, 29.98 g (294 mmol) of acetic anhydride and 1.50 g (12.0 mmol) of 4-dimethylaminopyridine dissolved in 13.5 g of β-methyl-δ-valerolactone were added to the four-neck glass flask, and the mixture was stirred at 60°C for 30 minutes to obtain a reaction solution containing a polymer. The resulting reaction solution containing the polymer was purified by extraction with toluene and water and distillation using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 955 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter, sometimes referred to as "PMVL-6") were measured as described above. The results are shown in Table 1. The obtained PMVL-6 is a polymer represented by the general formula (I) above, 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1.
[0093] [Production Example 7] A 500 mL four-neck glass flask was purged with nitrogen, and 7.9 g (58.6 mmol) of trimethylolpropane and 130 g (1.1 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.76 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 33.45 g (328 mmol) of acetic anhydride and 1.65 g (13.5 mmol) of 4-dimethylaminopyridine dissolved in 14.9 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a β-methyl-δ-valerolactone polymer. The reaction solution containing the obtained polymer was purified by extraction with toluene and water and distillation using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 77 g of polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-7") were measured as described above. The results are shown in Table 1. The obtained PMVL-7 is represented by the general formula (I) described above, and specifically, by the general formula (I-e) described above. R 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1. In Production Example 7, the starting alcohol has three hydroxyl groups and two m's.
[0094] [Production Example 8] A 500 mL four-neck glass flask was purged with nitrogen, and 5.6 g (90 mmol) of ethylene glycol and 231 g (2,025 mmol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.79 mL of n-butyllithium (1.6 M hexane solution) was added and stirred at 60°C for 60 minutes. Next, 34.2 g (216 mmol) of butyric anhydride and 1.1 g (9.0 mmol) of 4-dimethylaminopyridine dissolved in 11 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a polymer. The resulting reaction solution containing the polymer was purified by extraction with toluene and water and distillation using a thin-film evaporator (Shibata Scientific Instruments, Inc., "Molecular Distillation Apparatus MS-300"), yielding 158 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter, sometimes referred to as "PMVL-8") were measured as described above. The results are shown in Table 1. The obtained PMVL-8 is a polymer represented by the general formula (I) above, 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1.
[0095] [Production Example 9] A 500 mL four-neck glass flask was purged with nitrogen, and 5.6 g (90 mmol) of ethylene glycol and 231 g (2,025 mmol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.84 mL of n-butyllithium (1.6 M hexane solution) was added and stirred at 60°C for 60 minutes. Next, 48.9 g (216 mmol) of benzoic anhydride and 1.1 g (9.0 mmol) of 4-dimethylaminopyridine dissolved in 11 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a polymer. The resulting reaction solution containing the polymer was purified by extraction with toluene and water and distillation using a thin-film evaporator (Shibata Scientific Instruments, Inc., "Molecular Distillation Apparatus MS-300"), yielding 153 g of a β-methyl-δ-valerolactone polymer. The physical properties of the obtained β-methyl-δ-valerolactone polymer (hereinafter, sometimes referred to as "PMVL-9") were measured as described above. The results are shown in Table 1. The obtained PMVL-9 is a polymer represented by the general formula (I) above, 1 , R 2 , n, m, and the overall degree of polymerization are as shown in Table 1.
[0096]
[0097] The notations in Table 1 are as follows: 1 In the column, "(X)" indicates the above formula (X).
[0098] [Examples 1 to 12] Polyethylene terephthalate polymer 1 and the β-methyl-δ-valerolactone polymer obtained in the Production Examples were charged into a twin-screw kneader ("ULTnano 50" manufactured by Technovel Co., Ltd.) in the formulations shown in Table 2, extruded into strands at a cylinder temperature of 200°C, a screw rotation speed of 50 rpm, and a residence time of 1 to 10 minutes, and the resulting strands were cut into pellets to obtain resin compositions. The resulting resin compositions were evaluated as described above. The results are shown in Table 2.
[0099] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that the β-methyl-δ-valerolactone polymer was not used. The obtained resin composition was evaluated as described above. The results are shown in Table 2.
[0100] Comparative Example 2 A resin composition was obtained in the same manner as in Example 1, except that Plasticizer 1 was used instead of the β-methyl-δ-valerolactone polymer. The obtained resin composition was evaluated as described above. The results are shown in Table 2.
[0101] Comparative Example 3 A resin composition was obtained in the same manner as in Example 1, except that Impact Resistance Improver 1 was used instead of the β-methyl-δ-valerolactone polymer. The obtained resin composition was evaluated as described above. The results are shown in Table 2.
[0102]
[0103] [Examples 13 to 27] Polyethylene terephthalate polymer 1 and the β-methyl-δ-valerolactone polymer obtained in the Production Examples were charged into a twin-screw kneader ("ULTnano 50" manufactured by Technovel Co., Ltd.) in the formulations shown in Table 3, extruded into strands at a cylinder temperature of 200°C, a screw rotation speed of 50 rpm, and a residence time of 1 to 10 minutes, and the resulting strands were cut into pellets to obtain resin compositions. The resulting resin compositions were evaluated as described above. The results are shown in Table 3.
[0104]
[0105] A comparison of Examples 1 to 27 with Comparative Examples 1 to 3 reveals that the resin compositions obtained in the Examples are resin compositions with an excellent balance of impact resistance, flexibility, and bleed-out resistance. It also reveals that the β-methyl-δ-valerolactone polymers obtained in Production Examples 1 to 4 are useful as modifiers for polyethylene terephthalate polymers.
Claims
1. A resin composition containing a polyethylene terephthalate polymer and a β-methyl-δ-valerolactone polymer.
2. The resin composition according to claim 1, wherein the polyethylene terephthalate polymer is amorphous.
3. The resin composition according to claim 2, wherein the polyethylene terephthalate polymer is a modified polyethylene terephthalate polymer obtained by modifying polyethylene terephthalate (PET) with at least one selected from the group consisting of cyclohexanedimethanol and glycol.
4. The resin composition according to any one of claims 1 to 3, wherein the β-methyl-δ-valerolactone polymer is represented by the following general formula (I): [In general formula (I), R 1 represents a hydrogen atom, a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), or an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. R 2 represents a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is 2 to 1,000, and m is 2 to 1,000. R 2 When a plurality of and m are present, they may be the same or different from each other.
5. A resin composition according to any one of claims 1 to 3, comprising 0.1 to 100 parts by mass of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the polyethylene terephthalate polymer.
6. The resin composition according to any one of claims 1 to 3, wherein the β-methyl-δ-valerolactone polymer has a number average molecular weight of 500 to 100,000.
7. A molded article made of the resin composition according to any one of claims 1 to 3.
8. A modifier for polyethylene terephthalate polymers, comprising a β-methyl-δ-valerolactone polymer represented by the following general formula (I): [In general formula (I), R 1 represents a hydrogen atom, a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), or an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. R 2 represents a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, a linear alkenyl group having 2 to 20 carbon atoms, a branched alkenyl group having 3 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is 2 to 1,000, and m is 2 to 1,000. R 2 When a plurality of and m are present, they may be the same or different from each other.
Citation Information
Patent Citations
Preparation method and application of polylactic acid for producing extinction biaxially oriented film
CN115057997A
Highly crystalline polyester copolymer
JP1990097519A
Dispersion composition, curable composition, light-shielding film, color filter, solid-state imaging device, image display device, resin, and method for manufacturing cured film
WO2017150112A1
Β-methyl-δ-valerolactone polymer
WO2023068346A1
Resin composition
WO2023068348A1