Laminate, method for producing laminate, and method for producing printed wiring board

The laminate with a silicone resin film and polyurethane/polyamide-based protective layer addresses uniformity and peel strength issues, enabling effective lamination and transfer processes for printed wiring boards.

WO2024225364A1PCT designated stage expired Publication Date: 2024-10-31TATSUTA ELECTRICWIRE & CABLE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016187
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing methods for forming a protective layer on a separator film used in printed wiring boards face issues with uniformity and high peel strength, leading to adhesion problems and damage during thermocompression bonding.

Method used

A laminate is developed with a silicone resin film as a mold release surface and a protective layer containing polyurethane resin, polyamideimide resin, or polyamide resin, ensuring a water contact angle of 107.1° or more, which allows for uniform lamination and reduces peel strength, enabling easy peeling without resin repulsion.

Benefits of technology

The solution ensures a uniformly formed protective layer with reduced peel strength, facilitating the transfer of conductive and adhesive layers onto a substrate, enhancing the precision and reliability of printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016187_31102024_PF_FP_ABST
    Figure JP2024016187_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a laminate in which a protective layer is evenly laminated on a separator, and the separator does not have a too high peel strength after thermal press bonding. This laminate comprises: a separator which comprises a substrate and a silicone resin film formed on a surface of the substrate and serving as a release surface; and a protective layer laminated on the separator so as to be in contact with the release surface. The laminate is characterized in that the release surface has a water contact angle of 107.1° or greater, and that the protective layer includes at least one resin selected from the group consisting of polyurethane resins, polyamide-imide resins, and polyamide resins.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate, method for manufacturing laminate, and method for manufacturing printed wiring board

[0001] The present invention relates to a laminate, a method for manufacturing a laminate, and a method for manufacturing a printed wiring board.

[0002] In recent years, the integration of electrical circuits associated with the increasing performance of electronic devices has led to increased precision and density in printed wiring boards. One method for forming electrical circuits on printed wiring boards involves transferring an electrical circuit formed on a transfer film to a substrate. An example of such a transfer film is one in which a separator is laminated with a protective layer, a conductive paste that forms the electrical circuit, and an adhesive resin, in that order. When transferring an electrical circuit to a substrate using such a transfer film, the transfer film is first placed on the substrate so that the adhesive resin of the transfer film contacts the substrate. Next, the transfer film is bonded to the substrate by thermocompression bonding. During this process, the conductive paste hardens to form an electrical circuit. Then, by peeling off the separator film, a printed wiring board can be produced in which the adhesive resin, electrical circuit, and protective layer have been transferred onto the substrate.

[0003] Regarding the separator for such a transfer film, Patent Document 1 discloses the following polyester film: That is, Patent Document 1 discloses a film having a polyester A layer on at least one side of a polyester B layer, the polyester A layer forming at least one surface layer of the polyester film and containing 5% by mass to 30% by mass of a polyester having butylene terephthalate as a repeating unit, the center line average roughness Ra of the surface of the polyester A layer being 0.20 μm to 1.00 μm and the water contact angle being 70° to 84°.

[0004] Japanese Patent Application Laid-Open No. 2022-1431

[0005] A method for improving the releasability of a separator is known in which a silicone resin film is formed on the surface of the separator. When attempting to laminate a protective layer on the silicone resin film of the separator, the separator repels the protective layer, resulting in an uneven formation of the protective layer. Furthermore, when peeling the separator from the transfer film after thermocompression bonding, the peel strength becomes too high, resulting in problems such as part of the protective layer adhering to the separator or damage to the protective layer.

[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a laminate in which a protective layer is uniformly laminated on a separator and the peel strength of the separator after thermocompression bonding is not too high.

[0007] That is, the laminate of the present invention comprises a substrate, a separator having a silicone resin film formed on the surface of the substrate and serving as a release surface, and a protective layer laminated on the separator so as to come into contact with the release surface, wherein the release surface has a water contact angle of 107.1° or more, and the protective layer contains at least one resin selected from the group consisting of polyurethane resins, polyamideimide resins, and polyamide resins.

[0008] Silicone resin films have the property of repelling resins laminated thereon by printing or the like. Furthermore, typically, the larger the water contact angle of the silicone resin film (i.e., the release surface), the more easily the resin is repelled. However, surprisingly, it was discovered that when the resin is at least one selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin, the resin is less likely to be repelled by the silicone resin film. The present invention is based on the above findings.

[0009] In the laminate of the present invention, the protective layer contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin. As described above, these resins are not easily repelled by the silicone resin film. Therefore, the protective layer is formed uniformly. In this specification, "the protective layer is uniform" means that when the laminate is viewed from the protective layer side, there are no repelled portions of the protective layer formed on the release surface of the separator, and the release surface of the separator is not visible.

[0010] In the laminate of the present invention, if the water contact angle of the release surface is 107.1° or more, the peel strength of the separator after thermocompression bonding of the laminate of the present invention can be reduced. On the other hand, if the water contact angle of the release surface is less than 107.1°, the resin is likely to be repelled by the silicone resin film, making it difficult to form a uniform protective layer.

[0011] The laminate of the present invention may further include a conductive material layer laminated on the protective layer so that the separator is located on the opposite side of the protective layer. By using the laminate of the present invention, the conductive material layer can be transferred to a substrate.

[0012] In the laminate of the present invention, the conductive material layer may be a conductive paste layer for forming an electric circuit. Forming a conductive paste layer for forming an electric circuit on the laminate that will become the transfer film and transferring the conductive paste layer for forming an electric circuit to the substrate to form the electric circuit allows for the formation of a finer electric circuit than forming the electric circuit directly on the substrate.

[0013] The laminate of the present invention may further include an adhesive resin layer laminated on the separator on the opposite side of the protective layer and covering the conductive material layer. The presence of such an adhesive resin layer makes it possible to transfer the transfer target laminated on the separator to the substrate.

[0014] The method for producing a laminate of the present invention includes a separator preparation step of forming a silicone resin film that serves as a release surface on the surface of a substrate to form a separator, and a protective layer formation step of laminating a protective layer on the release surface, wherein in the separator preparation step, the silicone resin film is formed so that the water contact angle of the release surface is 107.1° or more, and the protective layer contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin. The laminate production method of the present invention allows the production of the laminate of the present invention.

[0015] The method for producing a printed wiring board of the present invention includes the following steps: a laminate preparation step of preparing a laminate including: a substrate; a separator having a silicone resin film formed on the surface of the substrate and serving as a release surface; a protective layer laminated on the separator so as to be in contact with the release surface; a conductive material layer laminated on the protective layer so as to sandwich the protective layer between the separator and the protective layer; and an adhesive resin layer laminated on the conductive material layer between the separator and the protective layer and to cover the conductive material layer; a laminate arrangement step of arranging the laminate on a substrate so as to adhere the adhesive resin layer; a thermocompression bonding step of thermocompression bonding the laminate to the substrate; and a peeling step of peeling off the separator; wherein the release surface has a water contact angle of 107.1° or more; and the protective layer contains at least one resin selected from the group consisting of polyurethane resins, polyamideimide resins, and polyamide resins.

[0016] In the method for producing a printed wiring board of the present invention, the water contact angle of the release surface (silicone resin film) of the separator is 107.1° or more, and the protective layer contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin. Because these resins are compatible with each other, after thermocompression bonding of the laminate, the peel strength between the release surface of the separator and the protective layer does not become too high, and the separator can be suitably peeled off in the peeling step.

[0017] According to the present invention, it is possible to provide a laminate in which a protective layer is uniformly laminated on a separator and the peel strength of the separator after thermocompression bonding is not too high.

[0018] FIG. 1A is a perspective view schematically showing an example of a laminate of the present invention. FIG. 1B is a cross-sectional view taken along line A-A in FIG. 1A. FIG. 2A is a schematic diagram of an example of a separator preparation step in the method for producing a laminate of the present invention. FIG. 2B is a schematic diagram of an example of a separator preparation step in the method for producing a laminate of the present invention. FIG. 3 is a schematic diagram of an example of a protective layer formation step in the method for producing a laminate of the present invention. FIG. 4 is a schematic diagram of an example of a transfer target lamination step in the method for producing a laminate of the present invention. FIG. 5A is a schematic diagram of an example of a lamination step in the method for producing a printed wiring board of the present invention. FIG. 5B is a schematic diagram of an example of a thermocompression bonding step in the method for producing a printed wiring board of the present invention. FIG. 5C is a schematic diagram of an example of a peeling step in the method for producing a printed wiring board of the present invention. FIG. 6A is a photograph of an example of a sample rated "Good" in the repellency evaluation. FIG. 6B is a photograph of an example of a sample rated "Triple" in the repellency evaluation. FIG. 6C is a photograph of an example of a sample rated "Poor" in the repellency evaluation.

[0019] The laminate of the present invention, the method for manufacturing the laminate, and the method for manufacturing a printed wiring board using the laminate will be specifically described below. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.

[0020] FIG. 1A is a perspective view schematically illustrating an example of a laminate of the present invention. FIG. 1B is a cross-sectional view taken along line A-A in FIG. 1A. The laminate 10 shown in FIGS. 1A and 1B includes a substrate 21, a separator 20 having a silicone resin film 22 formed on the surface of the substrate 21 and serving as a release surface 22a, and a protective layer 30 laminated on the separator 20 so as to contact the release surface 22a. The laminate 10 further includes a conductive material layer 40 and an adhesive resin layer 50 laminated in this order on the protective layer 30. That is, the conductive material layer 40 is laminated on the protective layer 30 so as to sandwich the separator 20 on the opposite side of the protective layer 30. The adhesive resin layer 50 is laminated so as to sandwich the separator 20 on the opposite side of the protective layer 30, and to cover the conductive material layer 40.

[0021] In the laminate 10, the protective layer 30 contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin. These resins are compatible with the silicone resin film 22 and are not easily repelled by the silicone resin film 22. Therefore, the protective layer 30 is formed uniformly.

[0022] In the laminate 10, the water contact angle of the release surface 22a is 107.1° or more. The water contact angle of the release surface 22a is preferably 109 to 120°, more preferably 110 to 115°, and even more preferably 110 to 113.5°. As will be described in detail below, the laminate 10 is thermocompression bonded to a substrate. If the water contact angle of the release surface 22a is 107.1° or more, the peel strength of the separator 20 after thermocompression bonding of the laminate 10 can be reduced. This makes it easier to peel the separator 20. Furthermore, if the water contact angle of the release surface is less than 107.1°, the silicone resin film will be more likely to repel the resin, making it difficult to form a uniform protective layer.

[0023] In this specification, the "water contact angle of the release surface" means the contact angle of the release surface with pure water measured using a contact angle meter (product name: Portable Contact Angle Meter PCA-11, manufacturer: Kyowa Interface Science Co., Ltd.).

[0024] Each component of the laminate will be described in detail below.

[0025] (Separator) The substrate 21 constituting the separator 20 is not particularly limited, but examples thereof include polyethylene naphthalate (PEN) and polyethylene terephthalate (PET).

[0026] The substrate 21 is preferably in the form of a sheet, and its thickness is preferably 6 to 100 μm, and more preferably 12 to 100 μm. If the thickness of the substrate is less than 6 μm, the substrate itself is prone to breakage. If the thickness of the substrate is more than 100 μm, heat is not easily transferred, and poor compression bonding is likely to occur.

[0027] A silicone resin film 22 is formed on the surface of the substrate 21. The silicone resin film 22 forms a release surface 22a of the separator 20. Examples of the silicone resin film 22 include emulsion types in which silicone oil is emulsified, solution types in which silicone resin is diluted with toluene or a petroleum hydrocarbon, baked types in which silicone resin diluted with a petroleum hydrocarbon is baked at high temperature after the solvent has evaporated to form a film, and spray types that can be used as is. However, in the present invention, it is preferable to use a solution type. Specific examples of separators 20 having a release surface on which the silicone resin film 22 is formed include NS-75-G manufactured by Nakamoto Pax Co., Ltd., E7001 manufactured by Toyobo Co., Ltd., E7002 manufactured by Toyobo Co., Ltd., and E7006 manufactured by Toyobo Co., Ltd.

[0028] The weight of the silicone resin film 22 after drying is, in particular, 0.01 to 1 g / m 2 is preferably 0.05 to 0.8 g / m 2 It is more preferable that:

[0029] The weight of the silicone resin film after drying is 0.01 g / m 2 If the weight of the silicone resin film after drying is less than 1 g / m, it becomes difficult to obtain the effect of the silicone resin film, and the peel strength becomes high. 2 If the thickness exceeds this value, the effect obtained by forming the silicone resin film approaches its upper limit, which is not economical.

[0030] The silicone resin film 22 may contain, in addition to the above resin, a crosslinking agent, a catalyst, a reaction inhibitor, an adhesion improver, and the like.

[0031] The water contact angle of the release surface 22 a of the separator 20 can be adjusted by selecting the amount and type of the silicone resin film 22 applied.

[0032] (Protective Layer) In the laminate 10, the protective layer 30 contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin.

[0033] When the protective layer 30 contains a polyurethane resin, the elasticity of the protective layer 30 is improved. Therefore, this is useful when elasticity is required for the printed wiring board manufactured using the laminate 10. When the protective layer 30 contains a polyamideimide resin and / or a polyamide resin, the heat resistance of the protective layer 30 is improved. Therefore, this is useful when heat resistance is required for the printed wiring board manufactured using the laminate 10.

[0034] Furthermore, in the case where the protective layer 30 is required to have elasticity in the printed wiring board manufactured using the laminate 10, the protective layer 30 may contain a polyurethane-based elastomer. The polyurethane-based elastomer is composed of a hard segment and a soft segment, and the soft segment may be a carbonate, ester, ether, or the like, and the physical properties thereof are such that the breaking elongation is preferably 20 to 500%, and more preferably 30 to 500%.

[0035] The thickness of the protective layer 30 is preferably 3 to 60 μm, and more preferably 5 to 50 μm. If the thickness of the protective layer is less than 3 μm, the protective layer is more likely to be damaged. Therefore, in a printed wiring board manufactured using the laminate, it becomes difficult to adequately protect the electrical circuit that the protective layer is intended to protect. If the thickness of the protective layer exceeds 60 μm, the flexibility of the protective layer is likely to decrease. Therefore, it becomes difficult to apply the protective layer to components that require bending resistance.

[0036] The protective layer 30 may contain, as needed, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, an antiblocking agent, and the like.

[0037] (Conductive Material Layer) The conductive material layer 40 is not particularly limited as long as it can form an electrical circuit when a printed wiring board is manufactured using the laminate 10. For example, the conductive material layer 40 may be a conductive paste layer or a metal layer. Examples of the metal layer include a vapor deposition layer, a plating layer, and a metal layer formed by etching or the like.

[0038] The conductive paste layer may contain a conductive filler and a resin.

[0039] Examples of conductive fillers include copper powder, silver powder, silver-coated copper powder, silver-coated nickel powder, copper-coated nickel powder, graphite, and carbon nanotubes. The conductive filler may have a dendritic, coiled, blocky, spherical, flake-like, needle-like, fibrous, or other shape. A dendritic shape refers to a shape in which rod-like branched branches extend from a rod-like main branch in two or three dimensions. The dendritic shape also includes a shape in which the branched branch is bent midway and a shape in which further rod-like branched branches extend from the midway of the branched branch.

[0040] The particle size of the conductive filler (average particle size D 50 ) is preferably 0.01 to 50 μm, and more preferably 0.02 to 30 μm. When the particle size of the conductive filler is 0.01 μm or more, the conductive fillers are likely to come into contact with each other, resulting in good conductivity of the conductive composition. When the particle size of the conductive filler is 50 μm or less, the printability and smoothness of the conductive material layer can be ensured.

[0041] The content of the conductive filler in the conductive paste layer is preferably 50 to 95% by weight.

[0042] Examples of the resin include epoxy resin, phenol resin, polyimide resin, and polyamide-imide resin.

[0043] Furthermore, in the case where stretchability is required for the electrical circuit in the printed wiring board manufactured using the laminate 10, the resin may be an elastomer resin. Examples of elastomer resins include elastic resins such as styrene-based elastomers, olefin-based elastomers, polyester-based elastomers, polyurethane-based elastomers, polyamide-based elastomers, and silicone-based elastomers. Polyurethane-based elastomers are composed of hard segments and soft segments, and the soft segments include carbonates, esters, ethers, and the like. As for physical properties, the breaking elongation is preferably 20 to 500%, and more preferably 30 to 500%.

[0044] The metal constituting the metal layer formed by vapor deposition, plating, etching or the like is not particularly limited, but copper is generally used.

[0045] The thickness of the conductive material layer 40 is preferably 3 to 60 μm, and more preferably 5 to 50 μm.

[0046] (Adhesive Resin Layer) The adhesive resin layer 50 preferably contains a hot-melt adhesive resin. Examples of hot-melt adhesive resins include thermoplastic resins such as polyester-based resins, polyurethane-based resins, polyamide-based resins, olefin-based resins, and ethylene vinyl acetate-based resins. The thermoplastic resin preferably has a softening point of 170°C or less and a breaking elongation of 300% or more, and more preferably a softening point of 150°C or less and a breaking elongation of 500% or more. More specifically, the thermoplastic resin may be a polyurethane-based thermoplastic resin such as "SHM101-PUR" manufactured by Sheedom Co., Ltd.

[0047] Next, a method for producing a laminate of the present invention will be described. The method for producing a laminate of the present invention includes a separator preparation step and a protective layer formation step. The method for producing a laminate of the present invention may also include a transfer target lamination step in which a transfer target is further laminated on the protective layer. Each step will be described in detail below.

[0048] 2A and 2B are schematic diagrams showing an example of the separator preparation step in the laminate manufacturing method of the present invention. In the separator preparation step, first, a substrate 21 is prepared as shown in Fig. 2A. The substrate 21 can be formed by extrusion molding a material to have a desired shape and size.

[0049] 2B, a silicone resin film 22 that will become the release surface 22a is formed on the surface of the substrate 21. At this time, the silicone resin film 22 is formed so that the water contact angle of the release surface 22a is 107.1° or more. The water contact angle of the release surface 22a is preferably formed to be 109 to 120°, more preferably 110 to 115°, and even more preferably 110 to 113.5°.

[0050] The silicone resin film 22 can be formed by applying a silicone resin film-forming composition containing a silicone resin and a solvent, followed by heating and drying. Examples of the solvent include toluene, acetone, methyl ethyl ketone, methanol, ethanol, propanol, and dimethylformamide. The concentration of solids in the silicone resin film-forming composition is preferably determined appropriately depending on the thickness of the silicone resin film 22, etc.

[0051] The method for applying the silicone resin film-forming composition is not particularly limited, and any known coater can be used. For example, the silicone resin film 22 may be formed using a coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a lip coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, a direct coater, or a slot die coater.

[0052] The preferred materials for the substrate 21 and the silicone resin film 22 have already been described, and therefore will not be described here.

[0053] (Protective Layer Forming Step) In the protective layer forming step, a protective layer 30 is laminated on the release surface 22a, as shown in Fig. 3. The protective layer 30 may be formed by applying a protective layer forming composition containing a protective layer resin and a solvent by coating, followed by heating and drying, or by applying the protective layer forming composition by printing.

[0054] The preferred resin for the protective layer contained in the composition for forming the protective layer is the same as the resin constituting the protective layer described above, and therefore, the description thereof will be omitted here.

[0055] Examples of solvents contained in the protective layer-forming composition include toluene, acetone, methyl ethyl ketone, methanol, ethanol, propanol, dimethylformamide, N-methylpyrrolidone, γ-butyrolactone, butyl carbitol acetate, butyl cellosolve, etc. When the concentration of solids in the protective layer-forming composition is within the above range, the protective layer-forming composition is less likely to be repelled by the silicone resin film 22, and the protective layer 30 can be formed uniformly.

[0056] The method for coating the protective layer-forming composition is not particularly limited, and a known coater can be used. For example, the protective layer 30 may be formed using a coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a lip coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, a direct coater, or a slot die coater.

[0057] Examples of methods for printing the protective layer-forming composition include gravure printing, flexographic printing, offset printing, screen printing, and rotary screen printing.

[0058] The conditions for heating and drying the protective layer-forming composition are preferably 100 to 250° C. and 2 to 60 minutes.

[0059] Through the above steps, it is possible to manufacture the laminate 11 in which the separator 20 and the protective layer 30 are laminated together. The laminate 11 manufactured in this manner is also the laminate of the present invention.

[0060] (Transfer Receiving Material Laminating Step) Fig. 4 is a schematic diagram of an example of a transfer receiving material laminating step in the laminate manufacturing method of the present invention. Next, as shown in Fig. 4, a conductive material layer 40 and an adhesive resin layer 50, which are transfer receiving materials, are laminated in this order on the protective layer 30. A conventionally known method can be used to laminate the conductive material layer 40 and the adhesive resin layer 50.

[0061] Through the above steps, a laminate 10 as shown in FIG. 1A can be manufactured.

[0062] Next, a method for manufacturing a printed wiring board using the laminate of the present invention will be described. The method for manufacturing a printed wiring board of the present invention includes a laminate preparation step, a laminate placement step, a thermocompression bonding step, and a peeling step. Each step will be described below.

[0063] (Laminate Preparation Step) In the method for manufacturing a printed wiring board of the present invention, first, the laminate 10 is prepared. The configuration of the laminate 10 has already been described, so a description thereof will be omitted here.

[0064] (Laminate placement step) Fig. 5A is a schematic diagram of an example of the lamination step in the printed wiring board manufacturing method of the present invention. In the laminate placement step, as shown in Fig. 5A, the laminate 10 is placed on the substrate 60 so that the adhesive resin layer 50 adheres to the substrate 60. Note that the laminate 10 shown in Fig. 5A is shown in a state in which the laminate 10 shown in Fig. 1A is turned upside down.

[0065] The material of the substrate 60 is not particularly limited, but is preferably made of engineering plastics. Examples of engineering plastics include resins such as polypropylene, cross-linked polyethylene, polyester, polybenzimidazole, polyimide, polyimideamide, polyetherimide, and polyphenylene sulfide (PPS), as well as woven fabrics, stretch woven fabrics, nonwoven fabrics, and stretch nonwoven fabrics.

[0066] (Thermocompression bonding step) Figure 5B is a schematic diagram of an example of the thermocompression bonding step in the printed wiring board manufacturing method of the present invention. Next, as shown in Figure 5B, the laminate 10 is thermocompression bonded to the substrate 60 (the arrows in Figure 5B indicate the direction of pressure). The thermocompression bonding conditions are preferably determined appropriately depending on the composition of the adhesive resin layer 50, the thickness of the separator 20, etc. For example, thermocompression bonding is preferably performed under conditions of 60 to 300°C, 0.1 to 3.0 MPa, and 5 to 300 seconds.

[0067] By carrying out this step, the adhesive resin layer 50 , the conductive material layer 40 and the protective layer 30 can be transferred onto the substrate 60 .

[0068] When the conductive material layer 40 is made of a conductive paste layer, the conductive paste layer hardens by thermocompression bonding to form an electric circuit.

[0069] (Peeling Step) Figure 5C is a schematic diagram of an example of the peeling step in the printed wiring board manufacturing method of the present invention. Next, as shown in Figure 5C, the separator 20 is peeled off. In the laminate 10, the release surface 22a made of the silicone resin film 22 has a water contact angle of 107.1° or more, and the protective layer 30 contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin. Because these resins are compatible with each other, the peel strength between the release surface 22a of the separator 20 and the protective layer 30 after thermocompression bonding is not too high, and the separator 20 can be peeled off suitably in the peeling step.

[0070] The peel strength when peeling the separator is preferably 0.01 to 2 N / 50 mm or more, and more preferably 0.05 to 1 N / 50 mm. The peel strength is measured at room temperature using a peel strength tester (PFT50S, manufactured by Palmec Co., Ltd.) at a tensile speed of 1000 mm / min and a peel angle of 170°.

[0071] Through the above steps, a printed wiring board 70 can be manufactured in which the adhesive resin layer 50, the conductive material layer 40 which is an electric circuit, and the protective layer 30 are laminated in this order on the substrate 60.

[0072] (Other Embodiments) The laminate 10 is used to transfer an electrical circuit of a printed wiring board 70. However, as long as the laminate of the present invention includes a separator and a protective layer, the material to be transferred that is laminated on the protective layer does not have to be a material for forming an electrical circuit. For example, the laminate of the present invention may be a laminate in which a separator, a protective layer, and a shielding layer are laminated in this order. Alternatively, the laminate of the present invention may be a laminate in which a separator, a protective layer, and a polarizing film are laminated in this order.

[0073] In addition, in the laminate of the present invention, other layers such as functional material layers such as anchor coat layers may be laminated between the protective layer and the conductive material layer, or between the conductive material layer and the adhesive resin layer.

[0074] Examples will be given below to explain the present invention more specifically, but the present invention is not limited to these examples.

[0075] (Example 1) (Separator preparation process) A substrate made of a 75 μm thick sheet of polyethylene terephthalate was prepared. Next, a silicone resin film-forming composition (release surface-forming composition) shown in Table 1 was applied to one side of the substrate, heated, and dried to form a silicone resin film, which served as a release surface. In this way, a separator according to Example 1 was prepared.

[0076] Using a contact angle meter (product name: Portable Contact Angle Meter PCA-11, manufacturer: Kyowa Interface Science Co., Ltd.), 2 μL of distilled water was dropped by the sessile drop method, and the contact angle of the release surface was measured after 1 second. The results are shown in Table 1.

[0077] (Protective Layer Forming Step) Next, the protective layer forming composition shown in Table 1 was printed on the release surface of the separator so that the length x width was 60 mm x 60 mm. The printing conditions were manual screen printing at 150°C for 3 minutes and drying, so that the thickness of the protective layer was 10 µm. Through the above steps, the laminate according to Example 1 was manufactured.

[0078] (Example 2) to (Example 6) and (Comparative Example 1) to (Comparative Example 8) Laminates according to Examples 2 to 6 and Comparative Examples 1 to 8 were produced in the same manner as in Example 1, except that the compositions were changed to those shown in Tables 1 and 2.

[0079]

[0080]

[0081] The separators in Tables 1 and 2 in which the release surface-forming composition is formed from a silicone resin are as follows: Silicone resin 1: NS-75-G manufactured by Nakamoto Pax Co., Ltd. Silicone resin 2: NS-75-G with adjusted water contact angle 1 manufactured by Nakamoto Pax Co., Ltd. Silicone resin 3: NS-75-G with adjusted water contact angle 2 manufactured by Nakamoto Pax Co., Ltd. Silicone resin 4: NS-75-G with adjusted water contact angle 3 manufactured by Nakamoto Pax Co., Ltd. Silicone resin 5: E7001 manufactured by Toyobo Co., Ltd. Silicone resin 6: E7002 manufactured by Toyobo Co., Ltd. Silicone resin 7: E7006 manufactured by Toyobo Co., Ltd. The separators in which the release surface-forming composition is formed from a non-silicone resin are as follows: Non-silicone resin 1: R02N2 manufactured by Nakamoto Pax Co., Ltd. Non-silicone resin 2: F05N manufactured by Nakamoto Pax Co., Ltd. The protective layer-forming compositions are as follows: Acrylic urethane resin: TPTF-9001N manufactured by GOO Chemical Industry Co., Ltd. Polyurethane resin: Lezamin CU-4104E manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. Polyamide-imide resin: HR-16NN manufactured by Toyobo Co., Ltd. Acrylic resin: PTF-60N manufactured by GOO Chemical Industry Co., Ltd. Polycarbonate resin: TPTF-9500 manufactured by GOO Chemical Industry Co., Ltd. Polyimide resin: PIAD200 manufactured by Arakawa Chemical Industries Co., Ltd.

[0082] <Appearance Evaluation> The laminates according to each of the Examples and Comparative Examples were observed from the protective layer side to visually check whether the protective layer had been repelled. The results are shown in Tables 1 and 2.

[0083] The evaluation criteria for the appearance evaluation are as described below and shown in Figures 6A to 6C. Figure 6A is a photograph of an example of a "good" rating in the repellency evaluation. Figure 6B is a photograph of an example of a "fair" rating in the repellency evaluation. Figure 6C is a photograph of an example of an "unacceptable" rating in the repellency evaluation. A rating of "good" means that the protective layer is not repelled, the separation film is not visible, and the protective layer is uniformly formed, as shown in Figure 6A. A rating of "fair" means that, as shown in Figure 6B, some of the protective layer is uniformly formed, but there are also areas where the protective layer is repelled and the separation film is visible, and the protective layer is not uniformly formed. A rating of "bad" means that the protective layer is repelled overall, the separation film is visible, and the protective layer is not uniformly formed, as shown in Figure 6C. A rating of "good" means that there is no problem in actual use, while ratings of "fair" and "unacceptable" mean that problems will occur in actual use.

[0084] <Evaluation of Peel Strength After Thermocompression Bonding> An adhesive resin, SHM101-PUR manufactured by Seedum, was applied to the protective layer of each laminate according to each Example and Comparative Example using a wire bar to a thickness of 10 μm to form an adhesive resin layer. Next, the laminate according to each Example and Comparative Example was placed on a polyimide substrate so that the adhesive resin layer was in contact with the substrate, and thermocompression bonded using a press under conditions of a temperature of 150°C, a time of 5 seconds, and a pressure of 0.5 MPa. After the laminate returned to room temperature, the separator's peel strength was measured using a peel strength tester (PFT50S manufactured by Palmec Co., Ltd.). Measurements were performed at room temperature, with a tensile speed of 1000 mm / min and a peel angle of 170°. Ten measurements were performed, and the average value was calculated. The results are shown in Tables 1 and 2.

[0085] As shown in Table 1, the separators according to Examples 1 to 6, in which the water contact angle of the release surface was 107.1° or more and the protective layer contained a polyurethane resin or a polypolyamideimide resin, had good appearance evaluations and low peel strength after thermocompression bonding. As shown in Comparative Examples 1 to 3 in Table 2, even if the water contact angle of the release surface was 107.1° or more, the appearance evaluation was poor when the protective layer did not contain any of a polyurethane resin, a polyamideimide resin, or a polyamide resin. Furthermore, as shown in Comparative Examples 4 to 8 in Table 2, even if the protective layer contained a urethane resin, the appearance evaluation was poor when the water contact angle of the release surface was less than 107.1°.

[0086] REFERENCE SIGNS LIST 10, 11 Laminate 20 Separator 21 Substrate 22 Silicone resin film 22a Release surface 30 Protective layer 40 Conductive material layer 50 Adhesive resin layer 60 Substrate 70 Printed wiring board

Claims

1. A laminate comprising: a substrate; a separator having a silicone resin film formed on the surface of the substrate and serving as a release surface; and a protective layer laminated on the separator so as to be in contact with the release surface, wherein the release surface has a water contact angle of 107.1° or more; and the protective layer contains at least one resin selected from the group consisting of polyurethane resins, polyamideimide resins, and polyamide resins.

2. The laminate according to claim 1, further comprising a conductive material layer laminated on said protective layer so that said separator is positioned on the opposite side of said protective layer.

3. The laminate according to claim 2, wherein said conductive material layer is a conductive paste layer for forming an electric circuit.

4. The laminate according to claim 2 or 3, further comprising an adhesive resin layer laminated so as to cover said conductive material layer and to sandwich said protective layer between said separator and said adhesive resin layer.

5. A method for producing a laminate, comprising: a separator preparation step of forming a silicone resin film that serves as a release surface on the surface of a substrate to form a separator; and a protective layer formation step of laminating a protective layer on the release surface, wherein in the separator preparation step, the silicone resin film is formed so that the water contact angle of the release surface is 107.1° or more, and the protective layer contains at least one resin selected from the group consisting of polyurethane resin, polyamideimide resin, and polyamide resin.

6. A method for producing a printed wiring board, comprising: a laminate preparation step of preparing a laminate comprising: a substrate and a separator having a silicone resin film formed on a surface of the substrate to serve as a release surface; a protective layer laminated on the separator so as to be in contact with the release surface; a conductive material layer laminated on the protective layer so as to sandwich the protective layer between the separator and the protective layer; and an adhesive resin layer laminated so as to cover the conductive material layer and to sandwich the protective layer between the separator and the protective layer; a laminate arrangement step of arranging the laminate on a substrate so that the adhesive resin layer is adhered to the substrate; a thermocompression bonding step of thermocompression bonding the laminate to the substrate; and a peeling step of peeling off the separator, wherein the release surface has a water contact angle of 107.1° or more, and the protective layer contains at least one resin selected from the group consisting of polyurethane resins, polyamideimide resins, and polyamide resins.

Citation Information

Patent Citations

  • Polyester film

    JP2022001431A

  • Water-based varnish composition and laminate

    JP7348416B1

  • Articles comprising durable icephobic coatings

    US20210017395A1

  • Release film for use in forming green sheet

    WO2005087493A1

  • Printing plate, method for producing printing plate, method for manufacturing functional element and printing apparatus

    WO2015186386A1