Conjugated diene polymer and method for producing conjugated diene polymer
The conjugated diene polymer, produced through a controlled polymerization process, addresses the trade-off in conventional rubber compositions by achieving superior wet grip and low-temperature performance, ensuring effective braking on diverse road conditions.
Patent Information
- Application Number
- PCT/JP2024/016246
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional rubber compositions for tire treads face a trade-off between wet grip performance and low-temperature performance, with existing solutions either compromising on wet grip or low-temperature braking efficiency on icy and snowy roads.
A conjugated diene polymer with a specific microstructure and glass transition temperature range, produced using a method involving continuous reactors and controlled polymerization steps, to achieve both excellent wet grip and low-temperature performance.
The conjugated diene polymer's vulcanizate exhibits a balanced performance with improved wet grip and low-temperature braking capabilities, maintaining flexibility and wear resistance across a wide temperature range.
Smart Images

Figure JPOXMLDOC01-APPB-C000007 
Figure JPOXMLDOC01-APPB-C000008 
Figure JPOXMLDOC01-APPB-C000009
Abstract
Description
Conjugated diene polymer and method for producing conjugated diene polymer
[0001] The present invention relates to a conjugated diene polymer and a method for producing a conjugated diene polymer.
[0002] One of the basic functions required for automobile tire treads is braking performance on road surfaces. With recent climate change, road surfaces can become wet due to sudden rainfall, or turn into icy or snowy surfaces due to sudden snowfall. In such environments, there is a demand for rubber materials used in tire treads that have excellent braking performance not only on dry road surfaces, but also on icy, snowy, and wet surfaces.
[0003] Generally, wet grip performance, which is a required characteristic of rubber for braking on wet roads, and low-temperature performance, which is a required characteristic of rubber for braking on snow, are in conflict with each other, and improving one performance tends to cause a deterioration in the other performance. Tire tread rubber is required to resolve this conflicting property.
[0004] Furthermore, rubber compositions have been known that reduce the modulus of elasticity at low temperatures to improve low-temperature performance and ensure high conformability of tread rubber to snowy road surfaces, and techniques have been proposed to lower the glass transition temperature of rubber materials in order to lower the glass transition temperature of the rubber composition.
[0005] On the other hand, a method of increasing the glass transition temperature of a rubber composition is known to improve wet grip performance, and a technique of increasing the glass transition temperature of a rubber material has been proposed to increase the glass transition temperature of a rubber composition.
[0006] For example, Patent Document 1 discloses a rubber composition containing silica and a modified conjugated diene polymer having a low glass transition temperature, which is obtained by reacting an alkoxysilane containing an amino group with the active terminal of a conjugated diene polymer, and proposes a technology for improving low-temperature performance.
[0007] Furthermore, Patent Document 2 discloses a rubber composition containing a conjugated diene polymer having a high glass transition temperature and silica, and proposes a technology for improving wet grip performance.
[0008] International Publication No. 2021 / 005295 Patent No. 3438317
[0009] In Europe and other regions, all-weather tires that can be used all year round are said to be increasingly popular, and there is a demand for rubber compositions that have improved wet grip performance across a wide temperature range. However, the present inventors conducted a detailed study of the conventional rubber compositions disclosed in Patent Documents 1 and 2 and found that the conventional rubber compositions have a problem in that the balance between the wet grip performance and low-temperature performance of the vulcanized products thereof needs to be improved. In other words, a rubber composition containing a conjugated diene polymer is required to improve the wet grip performance of the vulcanized products thereof without reducing flexibility at low temperatures and to have excellent braking performance even on icy and snowy surfaces.
[0010] Therefore, an object of the present invention is to provide a conjugated diene polymer that can provide a tire having excellent wet grip performance and low-temperature performance, and a method for producing the conjugated diene polymer.
[0011] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, it was found that by providing a rubber having a predetermined physical property with respect to glass transition temperature, it is possible to obtain both wet grip performance and low temperature performance when vulcanized, and this led to the completion of the present invention.
[0012] [1] A conjugated diene polymer having an estimated glass transition temperature (estimated Tg) derived from a microstructure in the conjugated diene polymer of -72°C or higher and -45°C or lower, having only one glass transition temperature (Tg) measured by differential scanning calorimetry (DSC), and having a difference between an extrapolated glass transition onset temperature and an extrapolated glass transition end temperature of the glass transition temperature (Tg) of 15°C or higher and 35°C or lower. [2] The conjugated diene polymer according to [1] above, having a first polymer segment not containing an aromatic vinyl monomer unit and a second polymer segment containing an aromatic vinyl monomer unit, wherein the amount of vinyl bonds Y1 (mol %) in the bound conjugated diene in the first polymer segment satisfies the following formula (2): 10≦Y1≦45... (2) The conjugated diene polymer according to [1] above, having an estimated glass transition temperature (estimated Tg) derived from a microstructure of the second polymer segment of higher than -45°C and lower than -5°C. [3] The conjugated diene polymer according to [1] or [2] above, having a molecular weight distribution, which is the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn, of 1.7 to 2.5. [4] The conjugated diene polymer according to [2] or [3] above, having a segment ratio of the first polymer segment of 20% by mass to 80% by mass. [5] The conjugated diene polymer according to any one of [1] to [4] above, having a weight average molecular weight of 300,000 to 1,350,000. [6] The conjugated diene polymer according to any one of [1] to [5] above, which contains a nitrogen atom. [7] The conjugated diene polymer according to [6] above, having a modification rate of the conjugated diene copolymer of 70% or more. [8] A method for producing a conjugated diene polymer according to any one of [2] to [7] above, using two or more continuous reactors, the method comprising: a first polymerization step (P1) of adding a conjugated diene compound, a polymerization initiator, and a polar substance to the continuous reactors to continuously form a first polymer segment of the conjugated diene polymer; and a second polymerization step (P2) of adding an aromatic vinyl compound and a polar substance to the continuous reactors to form a second polymer segment at an end of the first polymer segment.[9] The method for producing a conjugated diene polymer according to [8] above, further comprising a coupling step (P3) of reacting the conjugated diene polymer with a coupling agent after the second polymerization step (P2).
[10] The method for producing a conjugated diene polymer according to [8] or [9] above, wherein the mass ratio of the conjugated diene compound added in the first polymerization step (P1) to the total amount of the conjugated diene compound and the aromatic vinyl compound added is 20 mass% or more and 80 mass% or less.
[11] The method for producing a conjugated diene polymer according to any one of [8] to
[10] above, wherein the polymerization reaction rate in the first polymerization step (P1) is 75% or more and 95% or less.
[12] The method for producing a conjugated diene polymer according to any one of [8] to
[11] above, wherein the mass ratio of the amount of aromatic vinyl compound added in the second polymerization step (P2) to the amount of conjugated diene compound added is 0.15 or more and 0.70 or less.
[13] The method for producing a conjugated diene polymer according to any one of [8] to
[12] above, wherein a polar substance is added in the second polymerization step (P2) in an amount greater than the amount of polar substance added in the first polymerization step (P1).
[14] The method for producing a conjugated diene polymer according to any one of [9] to
[13] above, wherein the coupling agent is an aminoalkoxysilane compound.
[0013] According to the present invention, a conjugated diene polymer can be provided, the vulcanizate of which exhibits both excellent wet grip performance and low-temperature performance.
[0014] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0015] [Conjugated Diene Polymer] The conjugated diene polymer of the present embodiment contains conjugated diene monomer units and aromatic vinyl monomer units.
[0016] The conjugated diene polymer of this embodiment has an estimated glass transition temperature (hereinafter sometimes referred to as estimated Tg) derived from the microstructure of the conjugated diene polymer of -72°C or more and -45°C or less. The estimated glass transition temperature (estimated Tg) is derived from the microstructure of the conjugated diene polymer, as described below. Furthermore, the conjugated diene polymer of this embodiment has only one glass transition temperature (Tg) measured by differential scanning calorimetry (DSC), and the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature of the glass transition temperature (Tg) is 15°C or more and 35°C or less.
[0017] According to the above-mentioned constitution, a conjugated diene polymer can be obtained which can give a vulcanizate that has both excellent wet grip performance and low-temperature performance.
[0018] (Conjugated Diene Compound) Examples of conjugated diene compounds that form conjugated diene monomer units include, but are not limited to, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-heptadiene. Among these, 1,3-butadiene and isoprene are preferred from the viewpoint of ease of industrial availability. These may be used alone or in combination of two or more. From the viewpoints of ease of availability and ease of structural control during polymer synthesis, the conjugated diene compound is preferably 1,3-butadiene or isoprene, and more preferably 1,3-butadiene.
[0019] (Aromatic vinyl compound) Examples of aromatic vinyl compounds that form aromatic vinyl monomer units include, but are not limited to, styrene, p-methylstyrene, α-methylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, and diphenylethylene. Among these, styrene is preferred from the viewpoint of ease of industrial availability. These compounds may be used alone or in combination of two or more. As the aromatic vinyl compound, styrene is preferred from the viewpoints of ease of availability and ease of structural control during polymer synthesis.
[0020] (Microstructure) In this specification, the microstructure refers to a polymer composition including isomers in a conjugated diene polymer using an aromatic vinyl compound and a conjugated diene compound or in a polymer segment described later. In the conjugated diene polymer of this embodiment, the mass of the copolymer consisting of styrene and butadiene is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more, based on the mass of the entire conjugated diene polymer.
[0021] <Amount of bound aromatic vinyl monomer units (X all The estimated Tg of the conjugated diene polymer of the present embodiment is derived from the microstructure of the conjugated diene polymer. An example of the microstructure is a conjugated diene polymer having a bonded aromatic vinyl monomer unit amount (X all In this specification, the amount of bound aromatic vinyl monomer units (X all ) (mass %) is the mass fraction of bound aromatic vinyl monomer units relative to the total mass of the conjugated diene polymer of the present embodiment.
[0022] Here, the amount of bound aromatic vinyl monomer units can be calculated by measuring the ultraviolet absorption of the phenyl group in the portion of the conjugated diene polymer derived from an aromatic vinyl compound (hereinafter, sometimes referred to as "bound aromatic vinyl monomer units" or "aromatic vinyl monomer units"). Furthermore, when the conjugated diene polymer is composed of bound aromatic vinyl monomer units and bound conjugated diene monomer units, the amount of bound conjugated diene monomer units can be determined from the amount of bound aromatic vinyl monomer units obtained as described above. Specifically, it can be measured by the method described in the Examples below.
[0023] <Amount of vinyl bonds in the bonded conjugated diene (Y all The estimated Tg of the conjugated diene polymer of the present embodiment is derived from the microstructure of the conjugated diene polymer. One example of the microstructure is the amount of vinyl bonds in the bonded conjugated diene (Y all In this specification, the vinyl bond content (Y all) (mol %) is the molar fraction (mol %) of 1,2-bond units relative to the polymer units derived from the conjugated diene compound contained in the conjugated diene-based polymer of the present embodiment.
[0024] When the conjugated diene polymer of the present embodiment is a copolymer of butadiene and styrene, the vinyl bond content in the bound conjugated diene can be obtained by determining the vinyl bond content (1,2-bond content) in the bound butadiene by the Hampton method (R.R. Hampton, Analytical Chemistry, 21, 923 (1949)). Specifically, it can be measured by the method described in the examples below.
[0025] <Content of Bound Aromatic Vinyl Monomer Unit Block> The conjugated diene polymer of this embodiment preferably has a small number of or no blocks in which four or more bound aromatic vinyl monomer units are linked (hereinafter, may be referred to as bound aromatic vinyl monomer unit blocks). When the conjugated diene polymer of this embodiment has a small number of or no bound aromatic vinyl monomer unit blocks, the conjugated diene polymer tends to be less likely to have two or more glass transition temperatures. When the conjugated diene polymer is a butadiene-styrene polymer, the content of the bound aromatic vinyl monomer unit block in the conjugated diene polymer can be measured by a known method in which the conjugated diene polymer is decomposed by the Kolthoff method (the method described in I. M. KOLTHOFF, et al., J. Polym. Sci. 1, 429 (1946)) and the amount of polystyrene insoluble in methanol is analyzed. The content of the bound aromatic vinyl monomer unit block measured by such a method is preferably 1.0 mass% or less, and more preferably 0.1 mass% or less, based on the total amount of the conjugated diene polymer. Since the conjugated diene copolymer and the polymer segments described below do not contain bound aromatic vinyl monomer unit blocks, the conjugated diene polymer of this embodiment tends to exhibit continuous properties with temperature change. As a result, the vulcanizate using the conjugated diene polymer of this embodiment tends to exhibit continuous changes over a wide temperature range and exhibit excellent tensile strength.
[0026] (Method for Estimating Glass Transition Temperature of Conjugated Diene Polymer): Estimated Glass Transition Temperature (Estimated Tg) The glass transition temperature of the conjugated diene polymer of this embodiment can be calculated using the Gordon-Taylor equation (Gordon, M.; Taylor, J.S.J. Appl. Chem. 1952, 2, 493.), which is expanded to a system of two or more components according to the following formula (1). The value calculated by this method is referred to as the estimated glass transition temperature (estimated Tg).
[0027]
[0028] In the formula (1), the variable subscript i represents each component of the microstructure contained in the conjugated diene polymer, and Δα i is the difference in thermal expansion coefficient before and after the glass transition of the homopolymer of component i, w i is the mass ratio of component i in the conjugated diene polymer, Tg i is the glass transition temperature of the homopolymer of component i, ρ i is the density of the homopolymer of component i. Both literature values and actual measurements can be used. For example, when a conjugated diene polymer contains styrene, if one of the i's is a styrene component, the thermal expansion coefficient of polystyrene (J. BRANDRUP et al., Polymer Handbook, 3rd Group, (USA), John Wiley & Sons, Inc., 1966, VI-75) gives Δα i = 3.6 x 10 -4 K -1 , Tg from the measured value of the glass transition temperature i = 105.3°C, and from the measured density value, ρ i = 1.02 g / cm 3 can be used.
[0029] For example, when the conjugated diene polymer is a butadiene-styrene copolymer, the amount of bound aromatic vinyl monomer units X all (mass%), and the vinyl bond amount Y in the bound conjugated diene all (mol%), and the thermal expansion coefficients (Δa i ), glass transition temperature (Tgi ), density (ρ i ) the estimated glass transition temperature (estimated Tg) can be calculated from the following formula (i):
[0030]
[0031] The amount of bound aromatic vinyl monomer units X relative to the denominator of the formula (i) all (mass%), vinyl bond amount Y in the bonded conjugated diene all Since the influence of the product value of (mol%) is very small, it can be approximated by the following formula (ii): Furthermore, the following formula (ii) can be approximated as the following formula (iii):
[0032]
[0033]
[0034] That is, in the case of a butadiene homopolymer or a butadiene-styrene copolymer, the physical properties of the conjugated diene polymer can be predicted by the above formula (iii) from the values usually used in design.
[0035] According to the formula (1), the amount of bound aromatic vinyl monomer units X in the conjugated diene polymer of this embodiment is all (mass%), vinyl bond amount Y in the bonded conjugated diene all The mass proportion of each microstructure component can be calculated from the microstructure such as the mass fraction (mol%) of the conjugated diene polymer, and the glass transition temperature (Tg) of the conjugated diene polymer can be estimated. That is, the estimated Tg is calculated by multiplying the amount of bound aromatic vinyl monomer units X by the mass fraction (mol%) of the conjugated diene polymer. all (mass%), vinyl bond amount Y in the bonded conjugated diene all The estimated Tg is a measure of the change in the glass transition temperature of a conjugated diene polymer relative to a change in the molecular weight (mol%) of the polymer. When the estimated Tg value is small, the glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is low, and when the estimated Tg value is large, the glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is high. For example, when the estimated Tg is -70, the glass transition temperature of the conjugated diene polymer is estimated to be -70°C, and when the estimated Tg is -45, the glass transition temperature of the conjugated diene polymer is estimated to be -45°C.
[0036] As described above, the estimated Tg value determined from the microstructure of a conjugated diene polymer is generally an indicator of the glass transition temperature of the conjugated diene polymer. However, the present inventors have found that when the relaxation temperature of a conjugated diene polymer near its actual glass transition temperature is wide, the viscoelasticity of the actual vulcanizate does not necessarily coincide with the viscoelasticity based on the estimated glass transition temperature calculated from the microstructure. Specifically, when the difference in estimated Tg values between the polymer segments described below is 33 or more, or when the mass ratio of the first polymer segment described below is in the range of 40 to 60, the discrepancy between the glass transition temperature (estimated Tg) estimated from the above formula (1) and the actually measured glass transition temperature (Tg) tends to become significant. Therefore, from the perspective of controlling the performance of a vulcanizate affected by the glass transition temperature, they have found that it is more effective to control the estimated Tg value calculated from the microstructure to a specific value than to control the actually measured glass transition temperature of the conjugated diene polymer to a specific value. The reason for this is thought to be that DSC measurement (differential scanning calorimetry) picks up small energy changes, so that the entire glass transition temperature is pulled up at the start of relaxation of the low Tg portion in the conjugated diene polymer, making the actually measured glass transition temperature lower than the estimated glass transition temperature. For example, it has been experimentally confirmed that even if the microstructure of the entire conjugated diene polymer is the same, the glass transition temperature measured by DSC can differ by about 2 to 5°C depending on the difference in the microstructure of each segment.
[0037] The conjugated diene polymer of the present embodiment has an estimated Tg that satisfies the numerical range of −72° C. or more and −45° C. or less, and therefore the actually measured glass transition temperature when vulcanized tends to be an optimum value, and the balance between wet grip performance and low-temperature performance tends to be excellent.
[0038] The conjugated diene polymer of this embodiment has a lower limit of the estimated Tg derived from the microstructure of -72°C or higher, preferably -70°C or higher, and more preferably -68°C or higher. When the lower limit of the estimated Tg is within the above range, the wet grip performance of the vulcanizate of the conjugated diene polymer of this embodiment tends to be improved. Furthermore, the upper limit of the estimated Tg value is -45°C or lower, preferably -48°C or lower, and more preferably -50°C or lower. When the upper limit of the estimated Tg is within the above range, the low-temperature performance of the vulcanizate of the conjugated diene polymer of this embodiment tends to be improved.
[0039] The estimated Tg can be controlled to the above-mentioned range by adjusting the microstructure of the conjugated diene polymer. For example, when the conjugated diene polymer of the present embodiment is a butadiene-styrene copolymer, the bound styrene amount X of the conjugated diene polymer can be calculated by the above-mentioned formula (iii). all (mass%), vinyl bond amount Y in bound butadiene all By adjusting the (mol %), it is possible to control the content within the above-mentioned range.
[0040] (Polymer Segment) The conjugated diene polymer of this embodiment preferably has two or more polymer segments. A polymer segment refers to a portion of a conjugated diene polymer composed of conjugated diene monomer units and aromatic vinyl monomer units, or composed of conjugated diene monomer units. Furthermore, the conjugated diene polymer of this embodiment preferably has a polymer segment with few or no blocks in which four or more linked aromatic vinyl monomer units are chained. The presence of a block in which four or more linked aromatic vinyl monomer units are chained tends to broaden the Tg width. While this is preferable from the perspective of increasing the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature, it also tends to result in the glass transition temperature measured by DSC being easily split into two. The multiple polymer segments contained in the conjugated diene polymer of this embodiment have different microstructures. Each polymer segment may differ, for example, in the amount of linked aromatic vinyl monomer units or the amount of vinyl bonds in the linked conjugated diene. Each polymer segment can be distinguished by the method described in the Examples below.
[0041] <First Polymer Segment> The conjugated diene polymer of this embodiment preferably has a first polymer segment that does not contain an aromatic vinyl monomer unit and a second polymer segment that contains an aromatic vinyl monomer unit. As a result, the estimated Tg value of the first polymer segment is smaller than the estimated Tg value of the conjugated diene polymer of this embodiment (the value of formula (1) for the entire polymer). In such a case, the estimated Tg of the first polymer segment is calculated by substituting each component of the microstructure of the conjugated diene polymer into formula (1). When the conjugated diene polymer is a butadiene-styrene copolymer or a butadiene homopolymer, the estimated Tg of the conjugated diene polymer is calculated by multiplying the bound styrene amount X of the conjugated diene polymer by formula (iii). all (mass%), vinyl bond amount Y in bound butadiene all It is calculated from (mol%).
[0042] The first polymer segment preferably does not contain an aromatic vinyl monomer unit, and the vinyl bond content Y1 (mol %) in the bound conjugated diene satisfies the following formula (2): 10≦Y1≦45 (2) The lower limit of Y1 is more preferably greater than 10, even more preferably 12 or more, and even more preferably 15 or more. The upper limit of Y1 is more preferably less than 45, even more preferably 43 or less, and even more preferably 40 or less. By satisfying formula (2), the flexibility of the conjugated diene polymer of this embodiment at low temperatures is improved, and the vulcanizate thereof tends to have excellent abrasion resistance. The vinyl bond content Y1 (mol %) in the bound conjugated diene can be controlled within the above numerical range by adjusting the amount of polar substance added in the first polymerization step to prepare the first polymer segment.
[0043] <Second Polymer Segment> As described above, the conjugated diene polymer of this embodiment preferably has a first polymer segment that does not contain an aromatic vinyl monomer unit and a second polymer segment that contains an aromatic vinyl monomer unit. The second polymer segment has an estimated Tg value that is greater than the estimated Tg value of the conjugated diene polymer of this embodiment. In such a case, the estimated Tg of the second polymer segment is calculated by substituting each component of the microstructure of the second polymer segment into the above formula (1). When the conjugated diene polymer is a butadiene-styrene copolymer or a butadiene homopolymer, the estimated Tg of the conjugated diene polymer is calculated by multiplying the bound styrene amount X of the conjugated diene polymer by the above formula (iii): all (mass%), vinyl bond amount Y in bound butadiene all It is calculated from (mol%).
[0044] The second polymer segment preferably has an estimated Tg of higher than −45° C. and not higher than −5° C. The estimated Tg of the second polymer segment is calculated by the above-mentioned formula (1) when the amount of bound aromatic vinyl monomer units X all (mass%), vinyl bond amount Y in the bonded conjugated diene all It can be determined from the microstructure such as (mol%).
[0045] In the conjugated diene polymer of this embodiment, the lower limit of the estimated Tg of the second polymer segment is preferably higher than −45° C., more preferably −44° C. or higher, and even more preferably −43° C. or higher. The upper limit of the estimated Tg of the second polymer segment is preferably −5° C. or lower, more preferably −10° C. or lower, and even more preferably −15° C. or lower. When the estimated Tg of the second polymer segment is within the above-mentioned range, the conjugated diene polymer of this embodiment tends to have increased hysteresis loss in the high temperature range, and the vulcanizate thereof tends to have excellent wet grip performance.
[0046] The estimated Tg of the second polymer segment of the conjugated diene-based polymer of this embodiment, calculated by the formula (1), can be controlled to fall within the above-mentioned numerical range by adjusting the microstructure of the second polymer segment.
[0047] The conjugated diene polymer of this embodiment may contain a polymer segment other than the first polymer segment and the second polymer segment. For example, after synthesis of the first and second polymer segments, the conjugated diene polymer may contain a third polymer segment made of a conjugated diene compound in order to increase the reactivity of the conjugated diene polymer with a coupling agent. The polymer segments may be bonded to each other directly or via a coupling agent.
[0048] (Polymer Segment Ratio) The polymer segment ratio in a conjugated diene polymer represents the average mass fraction of each polymer segment relative to the entire conjugated diene polymer. The first and second polymer segment ratios in the conjugated diene polymer of this embodiment are defined as the ratio of the mass of the polymer segments obtained in the first polymerization step (P1), which is a step for preparing the first polymer segment, and the second polymerization step (P2), which is a step for forming the second polymer segment, to the total mass of the conjugated diene polymer. The first polymer segment ratio (r 1 ), and the second polymer segment ratio (r 2 ) in which the segment ratio (r 1The first polymer segment ratio (r ) is preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 40% by mass or more and 60% by mass or less. 1 When the lower limit of the first polymer segment ratio (r 1 ) satisfies the upper limit range, the second polymer segment ratio (r 2 ) falls within a preferable range, and wet grip performance tends to be excellent.
[0049] In the conjugated diene-based polymer of this embodiment, the segment ratio (r 1 ) can be controlled within the above-mentioned numerical range by adjusting the polymerization conditions such as the amount of monomer added and polymerization time in the first polymerization step (P1).
[0050] The method for introducing multiple polymer segments into the molecule of the conjugated diene-based polymer of this embodiment is not particularly limited, but examples thereof include a method using a continuous solution polymerization method in which multiple reactors are arranged in series, as described below, and sequentially adding a conjugated diene compound, an aromatic vinyl compound, a polar substance, and a solvent to each reactor. The sequentially added substances may be the same or different between reactors.
[0051] (Glass Transition Temperature (Tg) and Difference Between Extrapolated Glass Transition Onset Temperature and Extrapolated Glass Transition End Temperature of the Glass Transition Temperature (Tg)) The conjugated diene polymer of this embodiment has only one glass transition temperature (Tg) measured by differential scanning calorimetry (DSC), and the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature of the glass transition temperature (Tg) is 15°C or more and 35°C or less. When a single conjugated diene polymer undergoes glass transition over a wide temperature range, that is, has a region in which it relaxes from an elastic body to a viscous body over a wide temperature range, the vulcanizate thereof tends to become viscous in a low temperature range, resulting in excellent low-temperature performance. In addition, the elastic region of the vulcanizate continues even in a high temperature range, resulting in excellent wet grip performance, resulting in an excellent balance between both properties.
[0052] As described above, the conjugated diene polymer of this embodiment has only one glass transition temperature (Tg) as measured by DSC. To achieve a single glass transition temperature (Tg), it is effective to ensure that the conjugated diene polymer does not contain isolated aromatic vinyl monomer units (aromatic vinyl monomer blocks, segments consisting only of aromatic vinyl monomer units) or that random conjugated diene polymers with a high proportion of aromatic vinyl monomer units are not locally distributed unevenly. For example, if only the terminal 30% by mass of the conjugated diene polymer contains bonds of aromatic vinyl monomer units, and 40% by mass of these are aromatic vinyl monomer units, the conjugated diene polymer will have two glass transition temperatures. Having a single glass transition temperature (Tg) means that the conjugated diene polymer is not phase-separated, and tends to exhibit good low-temperature properties when vulcanized.
[0053] The glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is approximately halfway between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature in differential scanning calorimetry (DSC). The measured Tg value is preferably −75°C or higher, more preferably −70°C or higher. The glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is preferably −45°C or lower, more preferably −50°C or lower. The glass transition temperature (Tg) may be within a range that combines any of the above upper and lower limits. The glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is measured in accordance with ISO 22768:2006. More specifically, a DSC curve is recorded by differential scanning calorimetry (DSC) while increasing the temperature within a predetermined temperature range, and the inflection point of the DSC curve is taken as the glass transition temperature. Specifically, it can be measured by the method described in the Examples below. The conjugated diene polymer of the present embodiment may contain plasticizing components such as resins and process oils described below, but these components must be removed in the DSC measurement for determining the Tg of the conjugated diene polymer of the present embodiment.
[0054] The glass transition temperature (Tg) of a conjugated diene polymer varies depending on the amount of bound aromatic vinyl monomer units in the conjugated diene polymer and the amount of vinyl bonds in the bound conjugated diene. Specifically, the glass transition temperature (Tg) increases by increasing the amount of bound aromatic vinyl monomer units and the amount of vinyl bonds in the bound conjugated diene, while the glass transition temperature (Tg) decreases by decreasing the amount of bound aromatic vinyl monomer units and the amount of vinyl bonds in the bound conjugated diene. In the conjugated diene polymer of this embodiment, the estimated Tg can be controlled to a preferred range by adjusting the microstructure to control the actually measured glass transition temperature (Tg).
[0055] The conjugated diene polymer of this embodiment has an extrapolated glass transition onset temperature of a glass transition temperature (Tg) of preferably −90° C. or higher, more preferably −85° C. or higher. The extrapolated glass transition onset temperature is preferably −60° C. or lower, more preferably −65° C. or lower. When the extrapolated glass transition onset temperature is within the above range, the vulcanizate of the conjugated diene polymer of this embodiment tends to have even more excellent tensile properties. The conjugated diene polymer of this embodiment has an extrapolated glass transition end temperature of a glass transition temperature (Tg) of preferably −70° C. or higher, more preferably −65° C. or higher. The extrapolated glass transition end temperature is preferably −40° C. or lower, more preferably −45° C. or lower. When the extrapolated glass transition end temperature is within the above range, the vulcanizate of the conjugated diene polymer of this embodiment tends to have even more excellent low hysteresis loss properties.
[0056] The conjugated diene polymer of this embodiment has only one glass transition temperature (Tg) measured by DSC, and the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature of the glass transition temperature is 15°C or more and 30°C or less. This increases the hysteresis loss in the temperature range higher than the glass transition temperature, resulting in excellent wet grip performance, and also provides a wide range of flexibility at temperatures lower than the glass transition temperature, tending to result in excellent low-temperature performance. From the viewpoint of achieving both wet grip performance and low-temperature performance, the conjugated diene polymer of this embodiment is a conjugated diene polymer in which the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature for the single glass transition temperature is 15°C or more. The lower limit of the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature is preferably 15.5°C or more, more preferably 18°C or more. The upper limit is preferably 35°C or less, more preferably 30°C or less.
[0057] The extrapolated glass transition onset temperature is calculated by multiplying the vinyl bond amount Y in the bonded conjugated diene of the first polymer segment by 1. 1 Specifically, the vinyl bond amount Y in the bonded conjugated diene 1 On the other hand, the amount of the bound aromatic vinyl monomer unit X of the first polymer segment increases.1 and the amount of vinyl bonds in the bonded conjugated diene Y 1 The extrapolated glass transition onset temperature decreases as Y decreases. For example, when Y is 20 (mol%), the extrapolated glass transition onset temperature is -76.5°C, while Y 1 When the amount of the bound aromatic vinyl monomer unit X of the second polymer segment is 15 (mol %), the extrapolated glass transition onset temperature is −78.0° C. Furthermore, the extrapolated glass transition end temperature is 2 , the amount of vinyl bonds in the bonded conjugated diene Y 2 , and the second polymer segment ratio r 2 Specifically, the amount of bound aromatic vinyl monomer units X 2 and the amount of vinyl bonds in the bonded conjugated diene Y 2 or the increase in the second polymer segment ratio r 2 On the other hand, the amount of bound aromatic vinyl monomer units X 2 and the amount of vinyl bonds in the bonded conjugated diene Y 2 or the decrease in the second polymer segment ratio r 2 The extrapolated glass transition finish temperature decreases as r decreases. 2 When r is 50 (mass%), if the value calculated by the formula (iii) is −23, the extrapolated glass transition end temperature is −53.0° C., and r 2 When the value calculated by the formula (iii) is −38, r 2 is 55, the extrapolated glass transition finish temperature is -46.0°C.
[0058] (Weight Average Molecular Weight) The weight average molecular weight (Mw) of the conjugated diene polymer of the present embodiment measured by GPC measurement method is preferably 27×10 4 More preferably, 30×10 4 More preferably, it is 40×10 4 or more, and even more preferably 45×10 4When the lower limit of the weight average molecular weight measured by GPC measurement method is within the above range, the vulcanizate tends to have excellent abrasion resistance. In addition, the weight average molecular weight is preferably 135×10 4 or less, more preferably 90×10 4 More preferably, 70×10 4 or less. When the upper limit of the weight-average molecular weight satisfies the above range, the dispersibility of the filler in the vulcanizate tends to be even better. The weight-average molecular weight may be set within a range that arbitrarily combines the above upper and lower limits. The weight-average molecular weight of the conjugated diene polymer can be measured by GPC measurement, specifically, by the method described in the examples below.
[0059] (Number Average Molecular Weight) The number average molecular weight of the conjugated diene polymer of the present embodiment measured by GPC measurement is preferably 17×10 4 More preferably, 19×10 4 More preferably, it is 23×10 4 When the lower limit of the number average molecular weight measured by GPC measurement method is within the above range, the vulcanizate tends to have excellent abrasion resistance. In addition, the number average molecular weight is preferably 80×10 4 or less, more preferably 50×10 4 or less, and more preferably 40×10 4 The number average molecular weight is as follows. When the upper limit of the number average molecular weight satisfies the above range, the dispersibility of the filler in the vulcanizate tends to be even better. The number average molecular weight may be set within a range that combines any of the above upper and lower limits. The number average molecular weight of the conjugated diene polymer can be measured by GPC measurement, specifically, by the method described in the examples below.
[0060] The weight average molecular weight and number average molecular weight of the conjugated diene polymer can be controlled within the above-mentioned ranges by adjusting the ratio between the amount of polymerization initiator used and the amount of monomer used, and the type and amount of coupling agent used.
[0061] (Molecular Weight Distribution) The molecular weight distribution of the conjugated diene polymer of this embodiment is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn). The conjugated diene polymer of this embodiment preferably has a molecular weight distribution of 1.7 or more and 2.5 or less. Conjugated diene polymers with a molecular weight distribution in this range tend to have better processability when vulcanized. The molecular weight distribution of the conjugated diene polymer of this embodiment is more preferably 1.75 or more, and even more preferably 1.8 or more. Furthermore, the molecular weight distribution is more preferably 2.4 or less, and even more preferably 2.2 or less.
[0062] (Mooney Viscosity) The Mooney viscosity of the modified conjugated diene polymer of this embodiment, measured at 100°C, is preferably 30 or more and 150 or less, more preferably 60 or more and 130 or less, and even more preferably 60 or more and 115 or less. When the Mooney viscosity is within the above range, the fluidity of the conjugated diene copolymer of this embodiment decreases, resulting in excellent moldability, and the fracture properties and abrasion resistance of the vulcanizate thereof tend to be further improved. The Mooney viscosity of the conjugated diene polymer of this embodiment can be measured by the method described in the examples below.
[0063] (Modification Ratio) The conjugated diene polymer of this embodiment preferably has a nitrogen atom, and more specifically, preferably has a modifying group having a nitrogen atom. In this specification, the term "modification ratio" refers to the content, expressed in mass %, of a conjugated diene polymer component having a specific functional group in the polymer molecule that has affinity or binding reactivity with a filler relative to the total amount of the conjugated diene polymer mixture, when a conjugated diene polymer is modified with a modifying agent having a nitrogen atom to obtain a mixture of a modified conjugated diene polymer and an unmodified conjugated diene polymer. Therefore, when the specific functional group contains a nitrogen atom, the "modification ratio" refers to the mass ratio of the nitrogen-containing conjugated diene polymer relative to the total amount of the conjugated diene polymer mixture.
[0064] For example, when a conjugated diene polymer containing a modified conjugated diene polymer is obtained by reacting a nitrogen atom-containing modifying agent with the terminal end of a conjugated diene polymer, the modification rate is the mass ratio of the conjugated diene polymer having a nitrogen atom-containing functional group resulting from the nitrogen atom-containing modifying agent to the total amount of the conjugated diene polymer.
[0065] The modification rate can be measured by chromatography, which can separate functional group-containing modified components from unmodified components. Examples of methods using chromatography include a method using a gel permeation chromatography column packed with a polar substance such as silica that adsorbs specific functional groups, and quantifying the unadsorbed components using an internal standard for comparison. More specifically, the modification rate can be obtained by measuring the amount of adsorption to the silica column from the difference between a chromatogram measured on a polystyrene-based gel column and a chromatogram measured on a silica-based column for a sample solution containing a sample and a low-molecular-weight internal standard polystyrene. More specifically, the modification rate can be measured by the method described in the Examples.
[0066] In the conjugated diene polymer of this embodiment, the modification rate can be controlled by adjusting the amount of modifier added and the reaction method. For example, a desired modification rate can be achieved by combining a method of polymerization using an organolithium compound having at least one nitrogen atom in the molecule described below as a polymerization initiator, a method of copolymerizing a monomer having at least one nitrogen atom in the molecule, and a method of using a modifier represented by the structural formula described below, and controlling the polymerization conditions.
[0067] From the viewpoint of low hysteresis loss of the vulcanizate, the conjugated diene polymer of the present embodiment preferably has a modification rate of 60% or more, more preferably 65% or more, and even more preferably 70% or more, based on the total amount of the conjugated diene polymer.
[0068] [Method for Producing Conjugated Diene Polymer] The method for producing a conjugated diene polymer of this embodiment is not limited to the following, but may include, for example, a method using two or more continuous reactors, comprising a first polymerization step (P1) in which a conjugated diene compound, a polymerization initiator, and a polar substance are added to the continuous reactors to continuously form a first polymer segment of a conjugated diene polymer, and a second polymerization step (P2) in which an aromatic vinyl compound and a polar substance are added to the continuous reactors to form a second polymer segment at an end of the first polymer segment. It is preferable that the continuous reactors have a configuration of two or more.
[0069] (Polymerization Initiator) At least an organic monolithium compound can be used as the polymerization initiator. Examples of organic monolithium compounds include, but are not limited to, low molecular weight compounds and solubilized oligomeric organic monolithium compounds. Furthermore, examples of organic monolithium compounds include compounds having a carbon-lithium bond, a nitrogen-lithium bond, and a tin-lithium bond in the bonding mode between the organic group and the lithium. The amount of the organic monolithium compound used as the polymerization initiator is preferably determined based on the target molecular weight of the conjugated diene polymer or modified conjugated diene polymer. The amount of monomer, such as a conjugated diene compound, used relative to the amount of polymerization initiator used is related to the degree of polymerization. In other words, it tends to be related to the number-average molecular weight and weight-average molecular weight. Therefore, to increase the molecular weight, it is effective to reduce the amount of polymerization initiator used, and to decrease the molecular weight, it is effective to increase the amount of polymerization initiator used.
[0070] When introducing nitrogen atoms into a conjugated diene polymer using a polymerization initiator, the organic monolithium compound is preferably an alkyllithium compound having a substituted amino group or a dialkylaminolithium compound, from the viewpoint that it can be used as one method for introducing nitrogen atoms into a conjugated diene polymer. In this case, a conjugated diene polymer having a nitrogen atom consisting of an amino group at the polymerization initiation terminal is obtained. The substituted amino group is an amino group that does not have an active hydrogen or has a structure in which the active hydrogen is protected. Examples of alkyllithium compounds having an amino group without an active hydrogen include, but are not limited to, 3-dimethylaminopropyllithium, 3-diethylaminopropyllithium, 4-(methylpropylamino)butyllithium, and 4-hexamethyleneiminobutyllithium. Examples of alkyllithium compounds having an amino group with a structure in which the active hydrogen is protected include, but are not limited to, 3-bistrimethylsilylaminopropyllithium and 4-trimethylsilylmethylaminobutyllithium. Examples of dialkylaminolithiums include, but are not limited to, lithium dimethylamide, lithium diethylamide, lithium dipropylamide, lithium dibutylamide, lithium di-n-hexylamide, lithium diheptylamide, lithium diisopropylamide, lithium dioctylamide, lithium-di-2-ethylhexylamide, lithium didecylamide, lithium ethylpropylamide, lithium ethylbutylamide, lithium ethylbenzylamide, lithium methylphenethylamide, lithium hexamethyleneimide, lithium pyrrolidide, lithium piperidide, lithium heptamethyleneimide, lithium morpholide, 1-lithioazacyclooctane, 6-lithio-1,3,3-trimethyl-6-azabicyclo[3.2.1]octane, and 1-lithio-1,2,3,6-tetrahydropyridine. These organomonolithium compounds having a substituted amino group can also be used as solubilized oligomeric organomonolithium compounds by reacting them with a small amount of a polymerizable monomer, such as 1,3-butadiene, isoprene, or styrene.
[0071] The polymerization initiator may be one produced by reacting an aromatic vinyl compound and / or a conjugated diene compound having a substituted amino group with an organomonolithium compound, or may be one capable of introducing a functional group into one end of a polymer chain. The organomonolithium compound is preferably an alkyllithium compound from the viewpoints of industrial availability and ease of control of the polymerization reaction. In this case, a conjugated diene polymer having an alkyl group at the polymerization initiation end is obtained. Examples of the alkyllithium compound include, but are not limited to, n-butyllithium, sec-butyllithium, tert-butyllithium, n-hexyllithium, benzyllithium, phenyllithium, and stilbenelithium. Examples of the alkyllithium compound include n-butyllithium and sec-butyllithium from the viewpoints of industrial availability and ease of control of the polymerization reaction. These organomonolithium compounds may be used alone or in combination of two or more. Furthermore, they may be used in combination with other organometallic compounds. Examples of the other organometallic compounds include alkaline earth metal compounds, other alkali metal compounds, and other organometallic compounds. Examples of alkaline earth metal compounds include, but are not limited to, organomagnesium compounds, organocalcium compounds, and organostrontium compounds. Also included are alkaline earth metal alkoxides, sulfonates, carbonates, and amides. Examples of organomagnesium compounds include dibutylmagnesium and ethylbutylmagnesium. Other organometallic compounds include organoaluminum compounds.
[0072] In the method for producing a conjugated diene polymer of this embodiment, a coupling step (P3) of reacting the conjugated diene polymer with a coupling agent may be carried out after the second polymerization step (P2).
[0073] The weight-average molecular weight of the conjugated diene polymer before the coupling step (P3) can be controlled by adjusting the amount of polymerization initiator used relative to the conjugated diene compound and aromatic vinyl compound, and the weight-average molecular weight tends to decrease as the amount of polymerization initiator used decreases. The amount of polymerization initiator used is preferably 0.15 mol or more and 1.5 mol or less, assuming that the total mass of the conjugated diene compound and aromatic vinyl compound used is 100 kg.
[0074] (Polar Substance) A polar substance may be added in the polymerization step. The polar substance allows the aromatic vinyl compound to be randomly copolymerized with the conjugated diene compound, and the polar substance tends to be usable as a vinylating agent for controlling the microstructure of the conjugated diene portion. The polar substance also tends to be effective in accelerating the polymerization reaction.
[0075] Examples of polar substances include, but are not limited to, ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-oxolanyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidinoethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butylate, sodium tert-butylate, and sodium amylate; and phosphine compounds such as triphenylphosphine. These polar substances may be used alone or in combination of two or more. The amount of polar substance used is not particularly limited and can be selected depending on the purpose, but is preferably 0.01 mol to 100 mol per mol of the polymerization initiator.
[0076] Such polar substances (vinylating agents) can be used in an appropriate amount depending on the desired vinyl bond content as an adjuster for the microstructure of the conjugated diene portion of the conjugated diene polymer. Many polar substances also exhibit an effective randomizing effect in the copolymerization of a conjugated diene compound and an aromatic vinyl compound, and tend to be able to adjust the randomness of the aromatic vinyl monomer units and conjugated diene monomer units in each polymer segment. A method for randomizing the conjugated diene monomer units and the aromatic vinyl monomer units, as described in JP-A-59-140211, for example, may be used in which a copolymerization reaction is initiated with all of the styrene and a portion of the 1,3-butadiene, and the remaining 1,3-butadiene is intermittently added during the copolymerization reaction. The 1,3-butadiene added here is added to achieve a high modification rate in the coupling step (P3) and does not necessarily need to form a polymer segment.
[0077] The polymerization temperature in the polymerization step is preferably a temperature at which living anionic polymerization proceeds, and from the viewpoint of productivity, is preferably 0°C or higher, and more preferably 120°C or lower. By keeping the temperature in this range, it tends to be possible to ensure a sufficient amount of the modifying agent reacting with the active terminals after the polymerization is completed. More preferably, it is 50°C or higher and 100°C or lower.
[0078] (Polymer Segment Polymerization Step) In a preferred embodiment of the method for producing a conjugated diene-based polymer of this embodiment, the polymerization step is carried out in a continuous reactor system using two or more continuous reactors, and as described above, a first polymerization step (P1) for obtaining a first polymer segment and a second polymerization step (P2) for obtaining a second polymer segment are carried out. The first polymerization step (P1) and the second polymerization step (P2) can each be carried out using one or two or more connected reactors. The reactor may have any shape, such as a tank type or a tubular type equipped with a stirrer. It is not essential that the first polymerization step (P1) and the second polymerization step (P2) be assigned to each reactor. For example, the second polymerization step (P2) may be set to start downstream of the first reactor. Each reactor may have a temperature control function.
[0079] In the continuous reactor system, one or two or more connected reactors can be used. The continuous reactor may be, for example, a tank-type or tubular reactor equipped with a stirrer. In the continuous reactor system, preferably, the monomers, the inert solvent, and the polymerization initiator are continuously fed to the reactor, a polymer solution containing a conjugated diene polymer is obtained in the reactor, and the conjugated diene polymer solution is continuously discharged.
[0080] In a continuous reactor system, when continuous tank reactors connected in series are used, new monomers, inert solvents, and polar substances are added to the piping connecting the reactors, or when tubular reactors are used, they are added to the middle of the reactors, thereby allowing a polymer segment different from that synthesized in the previous polymerization step to be introduced into the conjugated diene polymer. Furthermore, by changing the polymerization temperature in the reactor, the bonding form of the conjugated diene compound changes, allowing a different polymer segment to be introduced into the conjugated diene polymer.
[0081] In the method for producing a conjugated diene polymer according to this embodiment, a continuous system is preferred to obtain the conjugated diene polymer, since the polymer can be continuously discharged and subjected to the next reaction in a short time. More preferably, a reaction system in which continuous tank reactors are connected in series is used, thereby increasing the residence time distribution in the reactor and the molecular weight distribution of each polymer segment. Additionally, the randomization effect of the aromatic vinyl compound is enhanced. This suppresses microphase separation of the conjugated diene polymer when vulcanized, resulting in a single glass transition temperature, and also tends to result in excellent wet grip performance and low-temperature performance.
[0082] In the first polymerization step (P1) for producing the first polymer segment, a conjugated diene compound, a polymerization initiator, and a polar substance are added to a reactor and polymerized continuously. The conjugated diene polymer solution after the first polymerization step (P1) is continuously distilled from the reactor and sent to the next step. The liquid destination is preferably, for example, the second polymerization step (P2) for forming the second polymer segment.
[0083] In the second polymerization step (P2) of the second polymer segment, one or two or more connected reactors are used, as in the polymerization step (P1). An aromatic vinyl compound and an additional polar substance are added to the conjugated diene polymer of the first polymer segment obtained in the first polymerization step (P1), and polymerization is carried out continuously. The conjugated diene polymer solution after the second polymerization step (P2) is continuously distilled from the reactor and sent to the next step. The destination of the solution is preferably, for example, the coupling step (P3) described below.
[0084] The conjugated diene polymer of this embodiment can also be produced by the following method. That is, to form a first polymer segment and a second polymer segment in the conjugated diene polymer, two or more continuous polymerization methods are used, for example, in the first polymerization step (P1) for producing the first polymer segment, an aromatic vinyl compound, a conjugated diene compound, a polymerization initiator, and a polar substance are added to a first reactor and polymerized continuously, and in the second polymerization step (P2) for forming the second polymer segment, no additional aromatic vinyl compound is added to the second reactor and any subsequent reactors, and the conditions for the polymerization steps in the respective reactors are changed, thereby producing the conjugated diene polymer of this embodiment.
[0085] Specifically, as described below, the polymerization reaction rate in the first reactor in the first polymerization step (P1) is reduced, and the conjugated diene compound and aromatic vinyl compound unreacted in the first polymerization step (P1) are polymerized in the second polymerization step (P2) or later, thereby forming a first polymer segment and a second polymer segment in the conjugated diene polymer. More specifically, by setting the polymerization reaction rate in the first polymerization step (P1) to 60% or less, the above-mentioned production method becomes easier. Note that, according to the method described in WO 2018 / 128285, the molecular weight distribution in the conjugated diene polymer is reduced. When the molecular weight distribution of the conjugated diene polymer is 1.7 or more, the processability of the vulcanized product tends to be excellent.
[0086] In the method for producing a conjugated diene polymer of this embodiment, it is preferable that, in the second polymerization step (P2) following the first polymerization step (P1), an aromatic vinyl compound and an additional polar substance are added to the conjugated diene polymer of the first polymer segment obtained in the first polymerization step (P1) and polymerization is carried out continuously. Unlike a production method in which an aromatic vinyl compound is added to the first polymerization step (P1) and then the second polymerization step (P2) is carried out, this production method can improve the polymerization reaction rate in the first polymerization step, can make the molecular weight distribution of the conjugated diene polymer 1.7 or more, and tends to result in a vulcanizate having excellent processability.
[0087] In the method for producing a conjugated diene polymer of this embodiment, the polymerization reaction rate in the first polymerization step (P1) is preferably 75% or more and 95% or less, more preferably 80% or more and 94% or less, and even more preferably 85% or more and 93% or less. By performing continuous polymerization using two or more continuous reactors and achieving the above-mentioned polymerization reaction rate, the molecular weight distribution of the conjugated diene polymer tends to be increased, and the processability of the vulcanizate thereof tends to be improved.
[0088] In the method for producing a conjugated diene polymer of this embodiment, the mass ratio of the conjugated diene compound added in the first polymerization step (P1) relative to the total amount of the conjugated diene compound and the aromatic vinyl compound added is preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 40% by mass or more and 60% by mass or less. By carrying out the polymerization step within this range, the ratio of the first polymer segment to the conjugated diene polymer can be preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 40% by mass or more and 60% by mass or less. When the ratio of the first polymer segment satisfies this numerical range, the vulcanizate tends to have excellent abrasion resistance.
[0089] The polymerization reaction rate in the first polymerization step (P1) can be calculated using the following formula (7). For example, the polymerization reaction rate in the first polymerization step (P1) can be calculated from the solid amount of the conjugated diene polymer per hour after the first polymerization step (P1) relative to the total amount of the conjugated diene compound and aromatic vinyl compound added per hour in the first polymerization step (P1). The solid amount (m1) in the conjugated diene polymer solution is determined from the amount of nonvolatile components in the polymer solution flowing through the outlet of the first polymerization step (P1) per unit time. Specifically, the entire amount of the polymer solution flowing through the outlet of the first polymerization step (P1) is sampled for 3 minutes, and a polymerization terminator is immediately added. The solution is then transferred to a heat-resistant dish or the like and dried in an oven at 140°C for 30 minutes or more, after which the mass M1 of the remaining solid matter is measured. The solid amount (m1) can be determined by combining the following formulas (7) and (8):
[0090]
[0091]
[0092] As described above, it is preferable to add an aromatic vinyl compound in the second polymerization step (P2) to form the second polymer segment. By controlling the mass ratio of the aromatic vinyl compound to the conjugated diene compound added in the second polymerization step (P2), the proportion of aromatic vinyl monomer units in the second polymer segment can be controlled, which tends to maintain the elastic properties of the conjugated diene polymer at high temperatures. Specifically, the lower limit of this mass ratio is preferably 0.15 or more, more preferably 0.25 or more, and even more preferably 0.30 or more. Increasing the amount of aromatic vinyl compound added in the second polymerization step (P2) increases the amount of bound aromatic vinyl monomer units in the second polymer segment in the conjugated diene polymer, which tends to improve the wet grip performance of the resulting vulcanizate. The upper limit of the mass ratio of the aromatic vinyl compound to the conjugated diene compound added in the second polymerization step (P2) is preferably 0.70 or less, more preferably 0.65 or less, and even more preferably 0.60 or less. By adjusting the amount of the aromatic vinyl compound added in the second polymerization step (P2) to fall within a predetermined range, the amount of bound aromatic vinyl monomer units in the second polymer segment in the conjugated diene polymer can be adjusted to fall within a desired range, and the resulting vulcanizate tends to have excellent handling stability.
[0093] In the second polymerization step (P2), one or more polar substances may be added, which increases the vinyl bond amount Y2 in the bonded conjugated diene of the second polymer segment and tends to improve the wet grip performance of the vulcanizate.
[0094] The amount of polar substance added in the second polymerization step (P2) is not particularly limited and can be selected depending on the purpose, etc., but it is preferably 0.01 mol to 100 mol per mol of polymerization initiator, including the polar substance added in the first polymerization step (P1). Furthermore, from the viewpoint of not reacting the bound aromatic vinyl compound in the second polymerization step (P2) and forming the bound aromatic vinyl compound monomer into a block, it is preferable that the amount of polar substance added in the second polymerization step (P2) be greater than that in the first polymerization step (P1). While not particularly limited, it is preferably more than 1.0 times and less than 25 times, more preferably 1.5 times or more and less than 20 times.
[0095] In producing the conjugated diene-based polymer of this embodiment, a predetermined step may be included before or after the first polymerization step (P1) and before or after the second polymerization step (P2). For example, a polymerization step for forming a polymer segment different from the first polymer segment and the second polymer segment may be included.
[0096] From the viewpoint of the modification rate in the coupling step described below, the polymerization steps are preferably carried out in the order of the first polymerization step (P1) and the second polymerization step (P2), but are not limited thereto. For example, after carrying out the second polymerization step (P2), the first polymerization step (P1) is carried out at a high polymerization temperature without adding an aromatic vinyl compound, thereby obtaining a modified conjugated diene-based polymer in which the coupling step is carried out after the second polymer segment and the first polymer segment. From the viewpoint of reaction controllability, a high conversion rate in each polymerization step is preferred.
[0097] (Coupling Step (P3)) In the method for producing a conjugated diene polymer of this embodiment, a step of coupling the active terminals of the conjugated diene polymer obtained through the polymerization step described above using a coupling agent, for example, a tri- or higher functional reactive compound, and / or a step of modifying the active terminals using a modifying agent having a nitrogen atom-containing group (preferably, a coupling agent having a nitrogen atom-containing group) may be carried out. Hereinafter, the coupling step and / or the modification step will be referred to as the coupling step (P3). In the coupling step (P3), one active terminal of the conjugated diene polymer is modified with the coupling agent or the modifying agent having a nitrogen atom to obtain a modified conjugated diene polymer.
[0098] <Coupling Agent> In the method for producing a conjugated diene polymer of the present embodiment, the coupling agent used in the coupling step may be a reactive compound having any structure as long as it is a tri- or higher functional compound, but is preferably a tri- or higher functional compound having a silicon atom.
[0099] Examples of the tri- or higher functional reactive compound having a silicon atom include, but are not limited to, halogenated silane compounds, epoxylated silane compounds, vinylated silane compounds, alkoxysilane compounds, and alkoxysilane compounds containing a nitrogen-containing group, with aminoalkoxysilane compounds being preferred.
[0100] Examples of halogenated silane compounds that serve as coupling agents include, but are not limited to, methyltrichlorosilane, tetrachlorosilane, tris(trimethylsiloxy)chlorosilane, tris(dimethylamino)chlorosilane, hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,2-bis(methyldichlorosilyl)ethane, 1,4-bis(trichlorosilyl)butane, and 1,4-bis(methyldichlorosilyl)butane.
[0101] Examples of the epoxidized silane compound that serves as a coupling agent include, but are not limited to, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and epoxy-modified silicone.
[0102] <Modifying Agent Having Nitrogen Atom-Containing Group> Examples of the modifying agent having a nitrogen atom include, but are not limited to, an isocyanate compound, an isothiocyanate compound, an isocyanuric acid derivative, a nitrogen atom group-containing carbonyl compound, a nitrogen atom group-containing vinyl compound, and a nitrogen atom group-containing epoxy compound.
[0103] In the modifying agent having a nitrogen atom-containing group, the nitrogen atom-containing group is preferably an amine compound having no active hydrogen, and examples thereof include tertiary amine compounds, protected amine compounds in which the active hydrogen is substituted with a protecting group, imine compounds represented by the general formula -N=C, and alkoxysilane compounds bonded to the nitrogen atom-containing group.
[0104] Examples of the isocyanate compound that is a modifying agent having a nitrogen atom-containing group include, but are not limited to, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate (C-MDI), phenyl isocyanate, isophorone diisocyanate, hexamethylene diisocyanate, butyl isocyanate, and 1,3,5-benzene triisocyanate.
[0105] Examples of isocyanuric acid derivatives that are modifying agents having a nitrogen atom-containing group include, but are not limited to, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-tris(3-triethoxysilylpropyl)isocyanurate, 1,3,5-tri(oxiran-2-yl)-1,3,5-triazinane-2,4,6-trione, 1,3,5-tris(isocyanatomethyl)-1,3,5-triazinane-2,4,6-trione, and 1,3,5-trivinyl-1,3,5-triazinane-2,4,6-trione.
[0106] Examples of carbonyl compounds that are modifying agents having a nitrogen atom-containing group include, but are not limited to, 1,3-dimethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 1-methyl-3-(2-methoxyethyl)-2-imidazolidinone, N-methyl-2-pyrrolidone, N-methyl-2-piperidone, N-methyl-2-quinolone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, methyl methyl-4-pyridyl ketone, propyl-2-pyridyl ketone, di-4-pyridyl ketone, 2-benzoylpyridine, N,N,N',N'-tetramethylurea, N,N-dimethyl-N',N'-diphenylurea, N,N-methyl diethylcarbamate, N,N-diethylacetamide, N,N-dimethyl-N',N'-dimethylaminoacetamide, N,N-dimethylpicolinic acid amide, and N,N-dimethylisonicotinic acid amide.
[0107] Examples of vinyl compounds that are modifying agents having a nitrogen atom-containing group include, but are not limited to, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methylmaleimide, N-methylphthalimide, N,N-bistrimethylsilyl acrylamide, morpholinoacrylamide, 3-(2-dimethylaminoethyl)styrene, (dimethylamino)dimethyl-4-vinylphenylsilane, 4,4'-vinylidenebis(N,N-dimethylaniline), 4,4'-vinylidenebis(N,N-diethylaniline), 1,1-bis(4-morpholinophenyl)ethylene, and 1-phenyl-1-(4-N,N-dimethylaminophenyl)ethylene.
[0108] Examples of epoxy compounds that are modifiers having a nitrogen atom-containing group include, but are not limited to, hydrocarbon compounds containing an epoxy group bonded to an amino group, and may further include an epoxy group bonded to an ether group. Examples of such epoxy compounds include, but are not limited to, epoxy compounds represented by general formula (a):
[0109]
[0110] In the formula (a), R is a divalent or higher organic group having at least one polar group selected from a divalent or higher hydrocarbon group, or a polar group having oxygen such as an ether, epoxy, or ketone, a polar group having sulfur such as a thioether or thioketone, or a polar group having nitrogen such as a tertiary amino group or an imino group.
[0111] The divalent or higher valent hydrocarbon group is a saturated or unsaturated hydrocarbon group which may be linear, branched, or cyclic, and includes an alkylene group, an alkenylene group, a phenylene group, etc. Preferably, it is a hydrocarbon group having 1 to 20 carbon atoms. Examples include methylene, ethylene, butylene, cyclohexylene, 1,3-bis(methylene)-cyclohexane, 1,3-bis(ethylene)-cyclohexane, o-, m-, and p-phenylene, m- and p-xylene, and bis(phenylene)-methane groups.
[0112] In the formula (a), R 1 , R 4 is a hydrocarbon group having 1 to 10 carbon atoms, and R 1 , R 4 may be the same or different. 2 , R 5 is hydrogen or a hydrocarbon group having 1 to 10 carbon atoms, and R 2 , R 5 may be the same or different. 3 R is a hydrocarbon group having 1 to 10 carbon atoms or a structure of the following formula (a1): 1 , R 2 , R 3 may be bonded to each other to form a cyclic structure. 3 When R is a hydrocarbon group, it may be bonded to R to form a cyclic structure. 3 In the formula (a), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.
[0113]
[0114] In the formula (a1), R 1 , R2 is R in the formula (a). 1 , R 2 is defined similarly to R 1 , R 2 may be the same or different from each other.
[0115] The epoxy compound, which is a modifying agent having a nitrogen atom-containing group, is preferably one having an epoxy group-containing hydrocarbon group, more preferably one having a glycidyl group-containing hydrocarbon group.
[0116] The epoxy group-containing hydrocarbon group bonded to the amino group or ether group is not particularly limited, but examples thereof include a glycidylamino group, a diglycidylamino group, and a glycidoxy group. More preferred epoxy compounds as the modifying agent are epoxy group-containing compounds having a glycidylamino group or a diglycidylamino group, and a glycidoxy group, respectively, and examples thereof include compounds represented by the following general formula (a2):
[0117]
[0118] In the formula (a2), R is defined as R in the formula (a), 6 is a hydrocarbon group having 1 to 10 carbon atoms or a structure of the following formula (a3): 6 When R is a hydrocarbon group, it may be bonded to R to form a cyclic structure. In this case, R 6 In formula (a2), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.
[0119]
[0120] As the epoxy compound which is a modifying agent having a nitrogen atom-containing group, a compound having one or more diglycidylamino groups and one or more glycidoxy groups in the molecule is particularly preferred.
[0121] The epoxy compound used as the modifying agent having a nitrogen atom-containing group is not limited to the following, but examples thereof include N,N-diglycidyl-4-glycidoxyaniline, 1-N,N-diglycidylaminomethyl-4-glycidoxy-cyclohexane, 4-(4-glycidoxyphenyl)-(N,N-diglycidyl)aniline, 4-(4-glycidoxyphenoxy)-(N,N-diglycidyl)aniline, 4-(4-glycidoxybenzyl)-(N,N-diglycidyl)aniline, 4-(N,N'-diglycidyl-2-piperazinyl)-glycidoxybenzene, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m- Examples thereof include xylylenediamine, 4,4-methylene-bis(N,N-diglycidylaniline), 1,4-bis(N,N-diglycidylamino)cyclohexane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, 4,4'-bis(diglycidylamino)benzophenone, 4-(4-glycidylpiperazinyl)-(N,N-diglycidyl)aniline, 2-[2-(N,N-diglycidylamino)ethyl]-1-glycidylpyrrolidine, N,N-diglycidylaniline, 4,4'-diglycidyl-dibenzylmethylamine, N,N-diglycidylaniline, N,N-diglycidylorthotoluidine, and N,N-diglycidylaminomethylcyclohexane. Of these, particularly preferred are N,N-diglycidyl-4-glycidoxyaniline and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.
[0122] In order to effectively and reliably achieve the effects of this embodiment, the modifying agent is preferably an alkoxysilane compound having a nitrogen atom-containing group.Examples of such modifiers include, but are not limited to, 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-diethylaminopropyltriethoxysilane, 3-morpholinopropyltrimethoxysilane, 3-piperidinopropyltriethoxysilane, 3-hexamethyleneiminopropylmethyldiethoxysilane, 3-(4-methyl-1-piperazino)propyltriethoxysilane, 1-[3-(triethoxysilyl)propyl]-3-methylhexahydropyrimidine, 3-(4-trimethylsilyl)propyl bis(3-triethoxysilylpropyl)methylamine, bis(3-trimethylsilyl-1-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 3-dimethylamino-2-(dimethylaminomethyl)propyltrimethoxysilane, bis(3-dimethoxymethylsilylpropyl)-N-methylamine, bis(3-trimethoxysilylpropyl)-N-methylamine, bis(3-triethoxysilylpropyl)methylamine, tris(trimethoxysilyl)amine, Tris(3-trimethoxysilylpropyl)amine, N,N,N',N'-tetra(3-trimethoxysilylpropyl)ethylenediamine, 3-isocyanatopropyltrimethoxysilane, 3-cyanopropyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(4-trimethoxysilylpropyl ... 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-8-(4-methylpiperazinyl)methyl-1,6-dioxa-2-silacyclooctane, 2,2-dimethoxy-8-(N,N-diethylamino)methyl-1,6-dioxa-2-silacyclooctane, and the like.
[0123] Particularly preferred examples of the alkoxysilane compound having a nitrogen atom-containing group include the following: tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-tripropoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (also known as "N,N,N',N'-tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine"). . ), tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-to trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, pentakis(3-trimethoxysilylpropyl) -diethylenetriamine, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]silane, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane, 1-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexane, 1-[3-(2,2- Examples of such bis(3-trimethoxysilylpropyl)-cyclohexane include 3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexyl-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]ether, (3-trimethoxysilylpropyl)phosphate, and bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate.
[0124] Also, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)phosphate, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate, N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, N-(1,3-dimethylbutylidene)-3-(trimethoxysilyl)-1-propanamine, N-benzylidene-3-(triethoxysilyl)propan-1-amine, N- benzylidene-3-(trimethoxysilyl)propan-1-amine, 1,1-(1,4-phenylene)bis(N-(3(triethoxysilyl)propyl)methanamine), 1,1-(1,4-phenylene)bis(N-(3(trimethoxysilyl)propyl)methanamine), 2-methoxy-2-methyl-1-(benzylideneaminoethyl)-1-aza-2-silacyclopentane, and 2-methoxy-2-methyl-1-(4-methoxybenzylideneaminoethyl)-1-aza-2-silacyclopentane.
[0125] Further, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(methyldimethoxysilyl)propyl]piperazine, 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), and 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine).
[0126] Further, 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine) dimethylmethane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethane-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethyl 1,3-bis(3-(1H-imidazol-1-yl)propyl)1,1,3,3-tetramethoxydisiloxane, 1,3-bis(3-(1H-imidazol-1-yl)propyl)1,1,3,3-tetraethoxydisiloxane, and 1,3-bis(3-(1H-imidazol-1-yl)propyl)1,1,3,3-tetrapropoxydisiloxane.
[0127] Among coupling modifiers having a group containing a nitrogen atom, protected amine compounds in which active hydrogen is substituted with a protecting group include alkoxysilanes and compounds having a protected amine in the molecule. Examples of such compounds include, but are not limited to, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane, N,N-bis(triethylsilyl)aminopropylmethyldiethoxysilane, 3-(4-trimethylsilyl-1-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane silane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, and 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane.
[0128] Further, for example, N-(1,3-dimethylbutylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1,3-dimethylbutylidene)-3-methyl(diethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-(trimethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-methyl N-ethylidene-3-(diethoxysilyl)-1-propanamine, N-ethylidene-3-(triethoxysilyl)-1-propanamine, N-ethylidene-3-(trimethoxysilyl)-1-propanamine, N-ethylidene-3-methyl(dimethoxysilyl)-1-propanamine, N-ethylidene-3-methyl(diethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(trimethoxysilyl)-1-propanamine , N-(1-methylpropylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-methyl(diethoxysilyl)-1-propanamine, N-benzylidene-3-methyl(dimethoxysilyl)propan-1-amine, N-benzylidene-3-methyl(diethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-(triethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-(trimethoxysilyl)propan-1-amine, N- 4-methylbenzylidene-3-methyl(dimethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-methyl(diethoxysilyl)propan-1-amine, N-naphthylidene-3-(triethoxysilyl)propan-1-amine, N-naphthylidene-3-(trimethoxysilyl)propan-1-amine, N-naphthylidene-3-methyl(dimethoxysilyl)propan-1-amine, 1,1-(1,4-phenylene)bis(N-(3-methyl(dimethoxysilyl)propyl)methanamine), 1,1-(1,4-phenylene)bis(N-(3-methyl(diethoxysilyl)propyl)methanamine), 2-ethoxy-2-methyl-1-(benzylideneaminoethyl)-1-aza-2-silacyclopentane, and 2-methoxy-2-methyl-1-(methylisobutylideneaminoethyl)-1-aza-2-silacyclopentane, 1-trimethylsilyl-4-[3-(trimethoxysilyl)propyl]piperazine, and 1-trimethylsilyl-4-[3-(triethoxysilyl)propyl]piperazine.
[0129] When a coupling step is carried out in the method for producing a conjugated diene polymer of this embodiment, it is more preferable to use a modifier having a nitrogen atom-containing group represented by any one of the following formulas (A) to (D) in the coupling step. These may be used alone or in combination of two or more.
[0130]
[0131] Here, R 10 , R 11 are hydrocarbon groups having 1 to 12 carbon atoms, which may contain unsaturated bonds, and may be the same or different from each other; R 12 is a hydrocarbon group having 1 to 20 carbon atoms. 8 , R 9 are aliphatic hydrocarbon groups having 1 to 6 carbon atoms, which may contain unsaturated bonds, and may be the same or different. 7 is a hydrocarbon group containing Si, O, or N and having 1 to 20 carbon atoms, which may be substituted with an organic group having no active hydrogen, and which may have an unsaturated bond. a is an integer of 1 to 3.
[0132]
[0133] In the formula (B), A represents a hydrocarbon group having 1 to 20 carbon atoms or an organic group having at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a phosphorus atom, and having no active hydrogen. 13 , R 14 , and R 15R each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms. 16 , R 17 , R 18 , R 19 , and R 21 R each independently represents an alkyl group having 1 to 20 carbon atoms. 20 , and R 22 R each independently represents an alkylene group having 1 to 20 carbon atoms. 23 each independently represents an alkyl group or a trialkylsilyl group having 1 to 20 carbon atoms, each b independently represents an integer of 1 to 3, each c independently represents 1 or 2, i independently represents an integer of 0 to 6, j independently represents an integer of 0 to 6, k independently represents an integer of 0 to 6, and the sum of i, j, and k is an integer of 4 to 10.
[0134]
[0135] However, in formula (C), R 24 , R 25 , R 26 , R 27 , R 28 , and R 29 R each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms. 30 , R 31 , and R 32 each independently represents an alkylene group having 1 to 20 carbon atoms. s, t, and u each independently represent an integer of 1 to 3, and the sum of s, t, and u is an integer of 4 or greater.
[0136]
[0137] However, in formula (D), B 1 and B 2 are each independently a divalent hydrocarbon group having 1 to 20 carbon atoms which may or may not contain an oxygen atom. 33 ~R 36 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 ~L 4are each independently a divalent, trivalent, or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms; 1 and L 2 And L 3 and L 4 may be linked together to form a ring having 1 to 5 carbon atoms, and L 1 and L 2 And L 3 and L 4 When are linked together to form a ring, the ring formed may contain 1 to 3 heteroatoms of one or more types selected from the group consisting of N, O, and S.
[0138] Specifically, in the formula (D), B 1 and B 2 are each independently an alkylene group having 1 to 10 carbon atoms; R 33 ~R 36 are each independently an alkyl group having 1 to 10 carbon atoms, and L 1 ~L 4 are each independently a tetravalent alkylsilyl group substituted with an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or L 1 and L 2 And L 3 and L 4 may be linked together to form a ring having 1 to 3 carbon atoms, and L 1 and L 2 And L 3 and L 4 When are linked together to form a ring, the ring formed may contain 1 to 3 heteroatoms of one or more types selected from the group consisting of N, O and S.
[0139] Examples of the coupling modifier represented by formula (A) include, but are not limited to, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-propyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-propyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-trimethylsilyl-4-[3-(trimethoxysilyl)propyl]piperazine, and 1-trimethylsilyl-4-[3-(triethoxysilyl)propyl]piperazine.
[0140] Among these, from the viewpoint of enhancing the reactivity and interaction between the conjugated diene polymer of the present embodiment and the inorganic filler such as silica, and from the viewpoint of enhancing processability, those in which a in the formula (A) is 3 are preferred.
[0141] In the coupling step using the coupling modifier represented by formula (A), the reaction temperature and reaction time are not particularly limited, but the reaction is preferably carried out at a temperature of 0°C or higher and 120°C or lower, and for 30 seconds or longer.
[0142] The amount of the coupling modifier represented by formula (A) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (A) is 0.2 to 2.0 times, more preferably 0.3 to 1.5 times, and even more preferably 0.4 to 1.0 times, the number of moles of the polymerization initiator added. From the viewpoint of setting the molecular weight of the resulting modified conjugated diene polymer in a more preferable range, the amount is preferably 0.2 times or more, and from the viewpoint of storage stability during long-term storage, the amount is preferably 2.0 times or less.
[0143] More specifically, the amounts of the polymerization initiator and the coupling modifier represented by the formula (A) added may be adjusted so that the number of moles of the coupling modifier represented by the formula (A) is preferably 0.1 to 1.0 times the number of moles of the polymerization initiator.
[0144] In the formula (B), A is preferably represented by any one of the following formulas (I) to (IV).
[0145]
[0146] In the formula (I), D 1 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms, and h represents an integer of 1 to 10. 1 are each independent of each other.
[0147]
[0148] In the formula (II), D 2 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. 3 represents an alkyl group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When a plurality of D 2 and D 3 are each independent of each other.
[0149]
[0150] In the formula (III), D 4 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When there are multiple D 4 are each independent of each other.
[0151]
[0152] In the formula (IV), D 5 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When there are multiple D 5 are each independent of each other.
[0153] In the formula (B), when A is represented by formula (I), examples of the coupling modifier include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)amine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tris(3-ethoxysilylpropyl)amine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)amine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-propanediamine.
[0154] Further, for example, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl] tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-triethoxysilylpropyl)-1,3-propanediamine, and tris(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine.
[0155] Further, for example, bis(3-triethoxysilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, and tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane.
[0156] Furthermore, for example, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl) bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane.
[0157] Furthermore, for example, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-triethoxysilylpropyl)-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-triethoxysilylpropyl)-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilylpropyl) bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2- trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, and pentakis(3-trimethoxysilylpropyl)-diethylenetriamine.
[0158] In the formula (B), when A is represented by formula (II), examples of the coupling modifier include, but are not limited to, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl), bis(2-triethoxysilylpropyl)-methyl-1,3-propanediamine, tris(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, N 1 , N 1 '-(propane-1,3-diyl)bis(N 1 -methyl-N 3 , N 3 -bis(3-(trimethoxysilyl)propyl)-1,3-propanediamine), and N 1 -(3-(bis(3-(trimethoxysilyl)propyl)amino)propyl)-N 1 -methyl-N 3 -(3-(methyl(3-(trimethoxysilyl)propyl)amino)propyl)-N 3 -(3-(trimethoxysilyl)propyl)-1,3-propanediamine.
[0159] In the formula (B), when A is represented by formula (III), examples of the coupling modifier include, but are not limited to, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, ]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, (3-trimethoxysilyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane propyl]silane, bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila- 2-azacyclopentane)propyl]-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-bis(3-trimethoxysilylpropyl)silane, and bis(3-trimethoxysilylpropyl)-bis[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]silane.
[0160] In the formula (B), when A is represented by formula (IV), examples of the coupling modifier include, but are not limited to, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-(2,2-dimethoxy-1-aza-2-silacyclopentane)propane and 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane.
[0161] The amount of the modifier represented by formula (B) to be added is preferably determined based on the ratio of the number of moles of the polymerization initiator to the number of moles of the modifier represented by formula (B) to be added, which allows the conjugated diene polymer and the modifier to react in a desired stoichiometric ratio.
[0162] More specifically, the amounts of the polymerization initiator and the coupling modifier represented by formula (B) added may be adjusted so that the ratio of the moles of the coupling modifier represented by formula (B) to the moles of the polymerization initiator is preferably 0.012 to 1.0, more preferably 0.02 to 0.5. In this case, the number of functional groups of the modifier in formula (B) (for example, when i and j are 2 or more and multiple w and x are present, and when f and g are equal, then f × i + (g + 1) × j + k) is preferably an integer of 5 to 10, more preferably an integer of 6 to 10. From the viewpoint of achieving a preferred range for the molecular weight of the resulting modified conjugated diene polymer, the ratio is preferably 0.012 or more. From the viewpoint of storage stability during long-term storage, the ratio is preferably 0.2 or less.
[0163] Among these, from the viewpoint of enhancing the reactivity and interaction between the modified conjugated diene polymer and the inorganic filler such as silica, and from the viewpoint of enhancing processability, it is preferable that i, j, and k in the formula (B) are all 3.
[0164] Examples of the coupling modifier represented by formula (C) include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, tris(3-methyldimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-methyldiethoxysilylpropyl)amine, tris(trimethoxysilylmethyl)amine, tris(2-trimethoxysilylethyl)amine, and tris(4-trimethoxysilylbutyl)amine.
[0165] In the coupling step using the coupling modifier represented by formula (C), the reaction temperature and reaction time are not limited to the following, but are preferably from 0°C to 120°C, and the reaction is preferably carried out for 30 seconds or more.
[0166] The amount of coupling modifier represented by formula (C) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (C) is 0.1 to 2.0 times the number of moles of polymerization initiator added, more preferably 0.2 to 1.0 times, and even more preferably 0.3 to 0.5 times. From the viewpoint of the molecular weight of the resulting modified conjugated diene polymer, it is preferably 0.1 times or more. Furthermore, from the viewpoint of storage stability during long-term storage, it is preferably 2.0 times or less.
[0167] Examples of the coupling modifier represented by formula (D) include 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(N,N-dimethyl ... methoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine).
[0168] In the coupling step using the coupling modifier represented by formula (D), the reaction temperature and reaction time are not particularly limited, but the reaction is preferably carried out at a temperature of 0°C or higher and 120°C or lower, and for 30 seconds or longer.
[0169] The amount of the coupling modifier represented by formula (D) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (D) is 0.25 to 2.0 times the number of moles of the polymerization initiator added, more preferably 0.3 to 1 time, and even more preferably 0.35 to 0.5 times. From the viewpoints of the molecular weight of the resulting modified conjugated diene polymer and storage stability during long-term storage, it is preferably 2.0 times or less.
[0170] The method for producing a conjugated diene polymer of the present embodiment may include a condensation reaction step in which a condensation promoter is added to cause a condensation reaction after and / or before the coupling step.
[0171] In the method for producing a conjugated diene polymer of this embodiment, after the coupling step, a deactivator and / or a neutralizing agent may be added to the polymer solution as needed. Examples of deactivators include, but are not limited to, water, and alcohols such as methanol, ethanol, and isopropanol. Examples of neutralizing agents include, but are not limited to, aqueous solutions of carboxylic acids such as stearic acid, oleic acid, and versatic acid (a mixture of highly branched carboxylic acids having 9 to 11 carbon atoms and mainly containing 10 carbon atoms), inorganic acids, and carbon dioxide.
[0172] It is preferable to add a rubber stabilizer to the conjugated diene polymer of this embodiment from the viewpoint of preventing gel formation after polymerization and improving stability during processing. The rubber stabilizer is not limited to the following and any known stabilizer can be used, but preferred examples include antioxidants such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenol)propionate, and 2-methyl-4,6-bis[(octylthio)methyl]phenol.
[0173] (Step of Obtaining from Polymer Solution) The method for producing a conjugated diene polymer of this embodiment may include a step of obtaining the obtained conjugated diene polymer from the polymer solution. As a method for obtaining the conjugated diene polymer from the polymer solution, known methods can be used, and for example, the following methods may be used. Examples include a method in which the solvent is separated by steam stripping or the like, and the conjugated diene polymer is then filtered off, and then dehydrated and dried to obtain a conjugated diene polymer; a method in which the conjugated diene polymer is obtained by concentrating the polymer in a flashing tank and then devolatilizing it using a vent extruder or the like; and a method in which the conjugated diene polymer is obtained by directly devolatilizing it using a drum dryer or the like.
[0174] (Step of Obtaining Extended Conjugated Diene Polymer) In the method for producing a conjugated diene polymer of this embodiment, at least one selected from the group consisting of extended oil, liquid rubber, and resin may be added to the produced conjugated diene polymer to obtain an extended conjugated diene polymer. The extended conjugated diene polymer includes not only oil-extended conjugated diene polymers containing oil, but also those containing liquid polybutadiene or various resins other than oil. This can further improve the processability of the conjugated diene polymer.
[0175] The method for adding an extender oil to a conjugated diene polymer is not limited to the following methods, but a preferred method involves adding an extender oil to a conjugated diene polymer solution, mixing, and then desolvating the resulting extended polymer solution. Examples of extender oils include aroma oils, naphthenic oils, paraffin oils, and vegetable oils. The vegetable oil can be made from an oil selected from the group consisting of linseed oil, safflower oil, soybean oil, corn oil, cottonseed oil, castor oil, tung oil, pine oil, sunflower oil, palm oil, olive oil, coconut oil, peanut oil, and grapeseed oil. Among these, from the standpoints of environmental safety, oil bleed prevention, and wet grip performance, aroma substitute oils having a polycyclic aromatic (PCA) content of 3% by mass or less according to the IP346 method are preferred. Examples of aroma substitute oils include TDAE (Treated Distillate Aromatic Extracts) and MES (Mild Extraction Solvate) as shown in Kautschuk Gummi Kunststoffe 52(12)799(1999), as well as RAE (Residual Aromatic Extracts).
[0176] Examples of liquid rubbers include, but are not limited to, liquid polybutadiene and liquid styrene-butadiene rubber. Examples of resins include, but are not limited to, aromatic petroleum resins, coumarone-indene resins, terpene resins, rosin derivatives (including tung oil resins), tall oil, tall oil derivatives, rosin ester resins, natural and synthetic terpene resins, aliphatic hydrocarbon resins, aromatic hydrocarbon resins, mixed aliphatic-aromatic hydrocarbon resins, coumarin-indene resins, phenolic resins, p-tert-butylphenol-acetylene resins, phenol-formaldehyde resins, xylene-formaldehyde resins, monoolefin oligomers, diolefin oligomers, hydrogenated aromatic hydrocarbon resins, cyclic aliphatic hydrocarbon resins, hydrogenated hydrocarbon resins, hydrogenated tung oil resins, hydrogenated oil resins, and esters of hydrogenated oil resins with monofunctional or polyfunctional alcohols. These resins may be used alone or in combination. In the case of hydrogenation, all of the unsaturated groups may be hydrogenated, or some of them may remain. The amount of at least one selected from the group consisting of extender oil, liquid rubber, and resin to be added is not particularly limited, but is preferably 1 to 60 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 15 to 37.5 parts by mass, relative to 100 parts by mass of the conjugated diene-based polymer of the present embodiment.
[0177] [Rubber Composition] The conjugated diene polymer of this embodiment can be added with a filler to form a rubber composition (hereinafter, sometimes referred to as the rubber composition of this embodiment). The rubber composition of this embodiment includes a rubber component containing the conjugated diene polymer of this embodiment and 5.0 parts by mass to 150 parts by mass of a filler per 100 parts by mass of the rubber component. Preferably, the rubber component contains 10 parts by mass or more of the conjugated diene polymer of this embodiment per 100 parts by mass of the total rubber component. By dispersing a filler in the rubber component containing the conjugated diene polymer of this embodiment, a rubber composition can be obtained that has better processability during vulcanization and that provides a vulcanizate with better low hysteresis loss, fracture properties, and abrasion resistance. Furthermore, by including the conjugated diene polymer of this embodiment in a predetermined proportion in the rubber component, the low hysteresis loss, processability, and abrasion resistance tend to be further improved.
[0178] Examples of fillers include, but are not limited to, silica-based inorganic fillers, carbon black, metal oxides, and metal hydroxides. Among these, silica-based inorganic fillers are preferred. In particular, when the rubber composition of this embodiment is used for vulcanized rubber applications such as tires, automobile parts such as anti-vibration rubber, and shoes, it is preferred that the rubber composition contain a silica-based inorganic filler. Such fillers may be used alone or in combination of two or more.
[0179] The silica-based inorganic filler is not particularly limited, and known fillers can be used. 2 or Si 3 Solid particles containing Al as a constituent unit are preferred, and SiO 2 or Si 3 Solid particles containing Al as the main component of the structural units are more preferred. Here, the main component refers to a component contained in the silica-based inorganic filler in an amount of more than 50% by mass, preferably 70% by mass or more, and more preferably 80% by mass or more.
[0180] Examples of silica-based inorganic fillers include, but are not limited to, inorganic fibrous materials such as silica, clay, talc, mica, diatomaceous earth, wollastonite, montmorillonite, zeolite, and glass fiber. Surface-hydrophobized silica-based inorganic fillers and mixtures of silica-based inorganic fillers with non-silica-based inorganic fillers may also be used. Among these, silica or glass fiber is preferred, and silica is more preferred, from the viewpoint of further improving the strength and abrasion resistance of the rubber composition of this embodiment. Examples of silica include, but are not limited to, dry silica, wet silica, and synthetic silicate silica. Among these silicas, wet silica is preferred from the viewpoint of further improving the breaking strength of the rubber composition.
[0181] From the viewpoint of more reliably obtaining a rubber composition having practically good abrasion resistance and breaking strength, the nitrogen adsorption specific surface area of the silica-based inorganic filler determined by the BET adsorption method is 100 m 2 / g or more 300m 2 / g or less, and 2 / g or more 250m 2 / g or less. If necessary, a relatively small specific surface area (for example, a specific surface area of 200 m 2 / g) silica-based inorganic filler and a relatively large specific surface area (e.g., 200 m 2 In particular, silica-based inorganic fillers having a relatively large specific area (for example, 200 m / g or more) may be used in combination. 2 When a silica-based inorganic filler (at least 1000 saturates / g) is used, the dispersibility of the silica in the rubber composition of the present embodiment is further improved, and as a result, the rubber composition tends to have even better abrasion resistance, fracture strength, and low hysteresis loss.
[0182] Examples of carbon black include, but are not limited to, carbon blacks of various classes such as SRF, FEF, HAF, ISAF, and SAF. Among these, carbon blacks having a nitrogen adsorption specific surface area of 50 m or more as determined by the BET adsorption method are preferred. 2 Carbon black having a carbon absorption of 80 mL / 100 g or more and a dibutyl phthalate (DBP) oil absorption of 80 mL / 100 g or less is preferred.
[0183] The metal oxides include those represented by the chemical formula M x O y (M represents a metal atom, and x and y each independently represent an integer of 1 to 6.) As long as the solid particles have as a main component a structural unit, there is no particular limitation, but examples thereof include alumina, titanium oxide, magnesium oxide, and zinc oxide.
[0184] Examples of metal hydroxides include, but are not limited to, aluminum hydroxide, magnesium hydroxide, and zirconium hydroxide.
[0185] The content of the filler in the rubber composition of this embodiment is preferably 5.0 parts by mass to 150 parts by mass, more preferably 20 parts by mass to 100 parts by mass, and even more preferably 30 parts by mass to 90 parts by mass, per 100 parts by mass of the rubber component. When the filler satisfies the above range, the rubber composition tends to have even more excellent processability during vulcanization, and the vulcanizate thereof tends to have even more excellent low hysteresis loss, fracture properties, and abrasion resistance.
[0186] From the viewpoint of reliably imparting the performance required for applications such as tires, such as dry grip performance and conductivity, the rubber composition of this embodiment preferably contains carbon black in an amount of 0.5 parts by mass to 100 parts by mass per 100 parts by mass of the rubber component containing the conjugated diene polymer of this embodiment. From the same viewpoint, the rubber composition preferably contains carbon black in an amount of 3.0 parts by mass to 100 parts by mass, and even more preferably 5.0 parts by mass to 50 parts by mass, per 100 parts by mass of the rubber component containing the conjugated diene polymer of this embodiment.
[0187] The rubber composition of this embodiment may further contain a silane coupling agent. By including a silane coupling agent in the rubber composition, the interaction between the rubber component and the filler can be further improved. Examples of silane coupling agents include, but are not limited to, compounds having a sulfur bond moiety and an alkoxysilyl group or silanol group moiety in one molecule. Examples of such compounds include, but are not limited to, bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, and bis-[2-(triethoxysilyl)-ethyl]-tetrasulfide.
[0188] In the rubber composition of this embodiment, the content of the silane coupling agent is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, and even more preferably 1.0 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the filler. When the content of the silane coupling agent is within the above range, the interaction between the rubber component and the filler tends to be further improved.
[0189] The rubber composition of the present embodiment may contain, as a rubber component, a rubbery polymer other than the conjugated diene polymer of the present embodiment (hereinafter simply referred to as a "rubbery polymer"). Examples of the rubbery polymer include, but are not limited to, conjugated diene polymers and hydrogenated products thereof, random copolymers of conjugated diene compounds and vinyl aromatic compounds and hydrogenated products thereof, block copolymers of conjugated diene compounds and vinyl aromatic compounds and hydrogenated products thereof, non-diene polymers, and natural rubber. Examples of the rubbery polymer include, but are not limited to, styrene-based elastomers such as butadiene rubber and hydrogenated products thereof, isoprene rubber and hydrogenated products thereof, styrene-butadiene rubber and hydrogenated products thereof, styrene-butadiene block copolymers and hydrogenated products thereof, and styrene-isoprene block copolymers and hydrogenated products thereof, as well as acrylonitrile-butadiene rubber and hydrogenated products thereof. Non-diene polymers include, but are not limited to, olefin elastomers such as ethylene-propylene rubber, ethylene-propylene-diene rubber, ethylene-butene-diene rubber, ethylene-butene rubber, ethylene-hexene rubber, and ethylene-octene rubber, butyl rubber, brominated butyl rubber, acrylic rubber, fluororubber, silicone rubber, chlorinated polyethylene rubber, epichlorohydrin rubber, α,β-unsaturated nitrile-acrylate-conjugated diene copolymer rubber, urethane rubber, and polysulfide rubber. Natural rubber includes, but is not limited to, smoked sheets RSS3 to 5, SMR, and epoxidized natural rubber.
[0190] The rubbery polymer may be a modified rubber to which a polar functional group such as a hydroxyl group, an amino group, etc. When the rubber composition of the present embodiment is used for a tire, the rubbery polymer is preferably at least one selected from the group consisting of butadiene rubber, isoprene rubber, styrene-butadiene rubber, natural rubber, and butyl rubber.
[0191] From the viewpoint of the balance between the abrasion resistance, breaking strength, low hysteresis loss, and processability of the rubber composition, the weight average molecular weight of the rubber polymer is preferably 2,000 to 2,000,000, and more preferably 5,000 to 1,500,000. Furthermore, a low molecular weight rubber polymer, so-called liquid rubber, can also be used as the rubber polymer. These rubber polymers may be used alone or in combination of two or more.
[0192] When the rubber composition of this embodiment contains the above-mentioned rubbery polymer in addition to the conjugated diene polymer of this embodiment, the content ratio (mass ratio) of the conjugated diene polymer to the rubbery polymer (conjugated diene polymer / rubbery polymer) is preferably 10 / 90 to 100 / 0, more preferably 20 / 80 to 99 / 1, and even more preferably 30 / 70 to 95 / 5. That is, the rubber component contains preferably 10 to 100 parts by mass, more preferably 20 to 90 parts by mass, and even more preferably 30 to 80 parts by mass of the conjugated diene polymer of this embodiment per 100 parts by mass of the total rubber component. When the proportion of the conjugated diene polymer of this embodiment in the rubber component is within the above range, the vulcanizate of the rubber composition tends to have even better wear resistance and low hysteresis loss.
[0193] To further improve its processability, the rubber composition of this embodiment may contain a rubber softener in addition to the rubber component. The rubber softener may be the same as those exemplified for the conjugated diene polymer described above, but mineral oil or a liquid or low-molecular-weight synthetic softener is preferred. Mineral oil-based rubber softeners, known as process oils or extender oils, are used to soften the rubber component, increase its volume, and improve its processability. They are mixtures of aromatic rings, naphthenic rings, and paraffin chains. Among these, those in which 50% or more of the total carbon atoms belong to paraffin chains are called paraffinic; those in which 30% to 45% of the total carbon atoms belong to naphthenic rings are called naphthenic; and those in which more than 30% of the total carbon atoms belong to aromatic carbons are called aromatic. The rubber composition of this embodiment preferably contains a rubber softener with an appropriate aromatic content. The inclusion of such a rubber softener further improves compatibility with the conjugated diene polymer. The content of the rubber softener in the rubber composition of this embodiment is represented by the total amount of the rubber softener added in advance to the conjugated diene polymer or rubbery polymer and the rubber softener added when preparing the rubber composition. In the rubber composition of this embodiment, the content of the rubber softener is preferably 0 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 90 parts by mass or less, and even more preferably 30 parts by mass or more and 90 parts by mass or less, per 100 parts by mass of the rubber component. By having the content of the rubber softener be 100 parts by mass or less per 100 parts by mass of the rubber component, bleed-out can be suppressed, and stickiness of the surface of the rubber composition can be further suppressed.
[0194] The rubber composition can be produced by mixing a conjugated diene polymer, a rubbery polymer, a filler, a silane coupling agent, a rubber softener, and the like. The mixing method is not particularly limited, but examples include a melt-kneading method using a general mixer such as an open roll, a Banbury mixer, a kneader, a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, and a method in which the components are dissolved and mixed and then the solvent is removed by heating. Among these, the melt-kneading method using a roll, a Banbury mixer, a kneader, or an extruder is preferred from the viewpoints of productivity and good kneading ability. The rubber component, the filler, the silane coupling agent, and the additives may be kneaded all at once, or may be mixed in multiple batches.
[0195] The rubber composition of the present embodiment may be vulcanized with a vulcanizing agent to form a vulcanizate. The vulcanizing agent is not particularly limited, but examples thereof include radical generators such as organic peroxides and azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, and sulfur compounds. Examples of sulfur compounds include sulfur monochloride, sulfur dichloride, disulfide compounds, and polymeric polysulfur compounds.
[0196] In the rubber composition of this embodiment, the content of the vulcanizing agent is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the rubber component. A conventionally known method can be used as the vulcanization method. The vulcanization temperature is preferably 120°C or more and 200°C or less, and more preferably 140°C or more and 180°C or less.
[0197] When vulcanizing the rubber composition, a vulcanization accelerator and / or vulcanization aid may be used as necessary. As the vulcanization accelerator, conventionally known materials can be used, and examples thereof include, but are not limited to, sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, and dithiocarbamate-based vulcanization accelerators. Furthermore, examples of the vulcanization aid include, but are not limited to, zinc oxide and stearic acid. The content of each of the vulcanization accelerator and vulcanization aid is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the rubber component.
[0198] The rubber composition of this embodiment may contain various additives such as softeners other than those described above, other fillers, heat stabilizers, antistatic agents, weather stabilizers, antioxidants, colorants, and lubricants, as long as the effects of this embodiment are not impaired. Known softeners can be used as softeners. Examples of other fillers include, but are not limited to, calcium carbonate, magnesium carbonate, aluminum sulfate, and barium sulfate. Known materials can be used as heat stabilizers, antistatic agents, weather stabilizers, antioxidants, colorants, and lubricants.
[0199] The rubber composition of the present embodiment is suitably used as a rubber composition for tires. The rubber composition of the present embodiment is not particularly limited, but can be suitably used for various tire parts such as fuel-efficient tires, all-season tires, high-performance tires, and studless tires, including treads, carcasses, sidewalls, and bead portions.
[0200] In addition, the numerical ranges described above as preferred ranges, etc., may be replaced with numerical ranges that arbitrarily combine the values described as upper limits and the values described as lower limits, unless otherwise specified.
[0201] Hereinafter, the present embodiment will be described in more detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples and comparative examples.
[0202] Various physical properties in the examples and comparative examples were measured by the methods shown below.
[0203] [(Property 1) Amount of bound aromatic vinyl monomer units (amount of bound styrene)] (amount of bound styrene in conjugated diene polymer X all A conjugated diene polymer containing no rubber softener was used as a sample, and 100 mg of the sample was dissolved in chloroform to prepare a measurement sample. The amount of bound styrene (mass%) relative to 100 mass% of the conjugated diene polymer sample was measured based on the amount of absorption of ultraviolet light by the phenyl group of styrene (near 254 nm) (measuring device: Shimadzu Corporation's spectrophotometer "UV-2450").
[0204] (Amount of bound styrene in the first polymer segment X 1 The bound styrene amount was calculated in the same manner as for the bound styrene amount in the conjugated diene polymer segment, except that the sample was changed from the conjugated diene polymer to the first polymer segment.
[0205] (Amount of bound styrene in the second polymer segment X 2 The segment ratio (r1) of the first polymer segment and the segment ratio (r2) of the second polymer segment were determined by the method described below. 2 ) is calculated, and the amount of bound styrene in the conjugated diene polymer X calculated from the measurement all and the bound styrene amount X1 in the first polymer segment, the bound styrene amount (X 2 ) was calculated.
[0206]
[0207] [(Property 2) Amount of vinyl bonds in bound conjugated diene (amount of 1,2-vinyl bonds in bound butadiene)] (amount of vinyl bonds in conjugated diene polymer Y all A conjugated diene polymer containing no rubber softener was used as a sample, and 50 mg of the sample was dissolved in 10 mL of carbon disulfide to prepare a measurement sample. The infrared spectrum of each sample was measured from 600 to 1000 cm -1The absorbance at a predetermined wave number was measured using a Fourier transform infrared spectrophotometer (trade name "FT-IR230" manufactured by JASCO Corporation). The amount of 1,2-vinyl bonds (mol %) in the bound butadiene was determined from the absorbance at a predetermined wave number according to the Hampton method (described in R.R. Hampton, Analytical Chemistry 21, 923 (1949)).
[0208] (Amount of vinyl bond in the first polymer segment Y 1 The vinyl bond amount was calculated in the same manner as for the bound vinyl amount of the conjugated diene polymer, except that the sample was changed from the conjugated diene polymer to the first polymer segment. In the table, if the numerical range of formula (2) was satisfied, it was indicated as "○", and if it was not satisfied, it was indicated as "×".
[0209] (Amount of vinyl bond in the second polymer segment Y 2 The segment ratio (r1) of the first polymer segment and the segment ratio (r2) of the second polymer segment were determined by the method described below. 2 ) is calculated, and the amount of bound styrene in the conjugated diene polymer X calculated from the measurement all , the amount of bound styrene in the first polymer segment X1, the amount of bound styrene in the second polymer segment X 2 and the vinyl bond amount Y in the conjugated diene polymer all Using the vinyl bond amount Y1 in the first polymer segment and the vinyl bond amount Y2 in the second polymer segment, the vinyl bond amount Y2 in the second polymer segment was calculated from the following formula (10).
[0210]
[0211] [(Property 3) Ratio of Polymer Segments] (First polymer segment ratio r 1) The first polymer segment ratio was calculated using the following formula (11). The ratio of the polymer segment in the first polymerization step (P1) for preparing the first polymer segment was calculated from the solid amount of the conjugated diene polymer per hour after the first polymerization step (P1) relative to the total amount of the conjugated diene compound and the aromatic vinyl compound added per hour in polymerizing the conjugated diene polymer. The solid amount in the conjugated diene polymer solution was determined from the amount of nonvolatile components in the polymer solution flowing through the outlet of the first polymerization step (P1) per unit time. The entire amount of the polymer solution flowing through the outlet of the first polymerization step (P1) was collected for 3 minutes, and a polymerization terminator was immediately added. Thereafter, the solution was transferred to a heat-resistant dish or the like, and dried in an oven at 140°C for 30 minutes or more, and the mass M1 of the remaining solid matter was measured. Here, the solid amount m1 and the first polymer segment ratio (r 1 ) was calculated using equation (11).
[0212]
[0213] (second polymer segment ratio r 2 ) Second polymer segment ratio (r 2 ) was calculated using the following formula (12). The second polymer segment ratio in the second polymerization step (P2) for forming the second polymer segment was calculated from the difference between the solid amount of the conjugated diene polymer per hour after the second polymerization step (P2) and the solid amount of the conjugated diene polymer per hour after the first polymerization step (P1), relative to the total amount of the conjugated diene compound and the aromatic vinyl compound added per hour in polymerizing the conjugated diene polymer. The solid amount in the conjugated diene polymer solution was determined from the amount of nonvolatile components in the polymer solution flowing through the outlet of the second polymerization step (P2) per unit time. The entire amount of the polymer solution flowing through the outlet of the second polymerization step (P2) was sampled for 3 minutes, and a polymerization terminator was immediately added. Thereafter, the solution was transferred to a heat-resistant dish or the like and dried in an oven at 140°C for 30 minutes or more, and the mass M2 of the remaining solid matter was measured. The second polymer segment ratio r 2 was calculated using equation (12).
[0214]
[0215] (Physical Property 4) Estimated Glass Transition Temperature The estimated glass transition temperature of the conjugated diene polymer was determined using the above formula (iii).
[0216] [(Property 5) Molecular Weight] Using a conjugated diene polymer as a sample, a GPC measurement apparatus (manufactured by Tosoh Corporation under the trade name "HLC-8320GPC") equipped with three columns packed with polystyrene gel was used. A chromatogram was measured using an RI detector (manufactured by Tosoh Corporation under the trade name "HLC8020"), and the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) were determined based on a calibration curve obtained using standard polystyrene. The eluent used was tetrahydrofuran (THF) containing 5 mmol / L triethylamine. Three columns (manufactured by Tosoh Corporation under the trade name "TSKgel SuperMultiporeHZ-H") were connected, and a guard column (manufactured by Tosoh Corporation under the trade name "TSKguardcolumn SuperMP(HZ)-H") was connected in front of the columns. 10 mg of the sample to be measured was dissolved in 10 mL of THF to prepare a measurement solution, and 10 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 0.35 mL / min.
[0217] [Physical Property 6] Mooney Viscosity of Polymer] Using a conjugated diene polymer as a sample, Mooney viscosity was measured using a Mooney viscometer (trade name "VR1132" manufactured by Ueshima Seisakusho Co., Ltd.) with an L-shaped rotor at a measurement temperature of 100°C in accordance with ISO 289. First, the sample was preheated at the test temperature for 1 minute, and then the rotor was rotated at 2 rpm. After 4 minutes, the torque was measured to determine the Mooney viscosity (ML (1+4) )
[0218] [(Property 7) Glass Transition Temperature (Tg)] When the conjugated diene polymer is an oil-extended product, the conjugated diene polymer after extraction of the extended oil was used as a sample, and a DSC temperature rise curve was recorded in accordance with ISO 22768:2006 using a differential scanning calorimeter "DSC3200S" manufactured by Mac Science, Inc., by lowering the temperature from 20°C at 20°C / min to -120°C under a helium flow of 50 mL / min, and then raising the temperature from -120°C at 10°C / min, and the only inflection point observed between -100°C and -20°C on the DSC temperature rise curve was taken as the glass transition temperature.
[0219] The extrapolated glass transition onset temperature was determined as the temperature at the intersection of a straight line extending from the low-temperature baseline toward the high-temperature side and a tangent drawn at the point where the gradient of the step-like change in the glass transition curve is maximum.
[0220] The extrapolated glass transition end temperature was determined as the temperature at the intersection of a straight line extending from the high-temperature baseline to the low-temperature side and a tangent drawn at the point where the gradient of the step-like change in the glass transition curve is maximum.
[0221] [(Property 8) Modification Ratio] The modification ratio of the conjugated diene polymers of the Examples and Comparative Examples was measured by the column adsorption GPC method as follows. Using the conjugated diene polymer as a sample, the measurement was carried out by applying the property of the modified basic polymer component being adsorbed to a GPC column packed with silica gel. The amount of adsorption to the silica column was measured by subtracting the chromatogram of a sample solution containing the sample and low-molecular-weight internal standard polystyrene measured on a polystyrene column from that measured on a silica column, and the modification ratio was determined. <Preparation of Sample Solution>: 10 mg of sample and 5 mg of standard polystyrene were dissolved in 20 mL of THF (tetrahydrofuran) to prepare a sample solution. <GPC measurement conditions using a polystyrene-based column>: Using a Tosoh Corporation product name "HLC-8320GPC", 10 μL of the sample solution was injected into the apparatus using 5 mmol / L triethylamine-containing THF as the eluent, and a chromatogram was obtained using an RI detector under the conditions of a column oven temperature of 40 ° C. and a THF flow rate of 0.35 mL / min. Three Tosoh Corporation product name "TSKgel SuperMultiporeHZ-H" columns were connected, and a Tosoh Corporation product name "TSKguardcolumn SuperMP(HZ)-H" was connected to the preceding stage as a guard column. <GPC measurement conditions using a silica-based column> GPC measurements were performed using a Tosoh Corporation product name "HLC-8320GPC" and an RI detector (Tosoh Corporation product name "HLC8020"). THF was used as the eluent, and 50 μL of the sample solution was injected into the device. A chromatogram was obtained under the conditions of a column oven temperature of 40 ° C. and a THF flow rate of 0.5 ml / min. The columns were connected in this order: Agilent Zorbax PSM-1000S, PSM-300S, and PSM-60S. A guard column, DIOL 4.6 × 12.5 mm 5 micron, was connected in front of the columns.<Method of calculating modification rate>: The total peak area of the chromatogram using a polystyrene-based column was set to 100, the peak area of the sample was set to p1, the peak area of the standard polystyrene was set to p2, the total peak area of the chromatogram using a silica-based column was set to 100, the peak area of the sample was set to p3, and the peak area of the standard polystyrene was set to p4, and the modification rate (%) was calculated using the following formula: Modification rate (%) = [1 - (p2 × p3) / (p1 × p4)] × 100 (where p1 + p2 = p3 + p4 = 100).
[0222] [Production of Conjugated Diene Polymer] (Example 1) Two tank-type pressure vessels each having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom, an outlet at the top, and a jacket for temperature control, were connected as polymerization reactors. 1,3-Butadiene, from which moisture had been removed in advance, and normal hexane were mixed at 18.8 g / min and 163.4 g / min to obtain a mixed solution. In a static mixer installed midway through the piping supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating remaining impurities was added at a rate of 0.104 mmol / min, and after mixing, the mixture was continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.027 mmol / min and n-butyllithium as a polymerization initiator at a rate of 0.239 mmol / min were supplied to the bottom of the first reactor, which was being vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 78°C. Thereafter, when the polymerization reaction became stable, a small amount of conjugated diene polymer was extracted from the top of the reactor, and an antioxidant (BHT) was added so that the amount was 0.2 g per 100 g of polymer. Thereafter, the solvent was removed, and the amount of vinyl bonds (Y 1 ) was measured.
[0223] Next, the polymer solution was continuously supplied from the top of the first reactor to the bottom of the second reactor, and further, to the second reactor, 1,3-butadiene was added at a rate of 10.6 g / min, styrene at 4.5 g / min, normal hexane at 41.9 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.415 mmol / min with stirring, and the reaction was continued at 78°C.
[0224] Next, to the polymer solution flowing out from the top of the second reactor, coupling agents 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "Coupling Agent A" in the table) were continuously added at a rate of 0.097 mmol / min and tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "Coupling Agent B" in the table) were continuously added at a rate of 0.010 mmol / min, and the mixture was mixed using a static mixer to carry out a coupling reaction. At this time, it took 4.8 minutes for the coupling agent to be added to the polymer solution flowing out from the reactor outlet, the temperature was 68°C, and the difference between the temperature during the polymerization process and the temperature before the addition of the coupling agent was 2°C. After the coupling reaction, a small amount of the conjugated diene polymer solution was withdrawn, and an antioxidant (BHT) was added in an amount of 0.2 g per 100 g of the polymer. After that, the solvent was removed, and the bound styrene amount (X), vinyl bond amount (Y), glass transition temperature, extrapolated glass transition onset temperature, and end temperature were identified.
[0225] Next, an antioxidant (BHT) was continuously added to the coupled polymer solution at a rate of 0.055 g / min (n-hexane solution) to give 0.2 g per 100 g of polymer, and the coupling reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener to give 5.0 g per 100 g of polymer, and the mixture was mixed in a static mixer. The solvent was removed by steam stripping to obtain a conjugated diene polymer (A1). The molecular weight, Mooney viscosity, and modification rate were determined.
[0226] Example 2 To the first reactor, 1,3-butadiene was added at 15.8 g / min and normal hexane at 156.0 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance was added at a rate of 0.072 mmol / min. To the second reactor, 1,3-butadiene was added at 14.0 g / min, styrene at 4.4 g / min, normal hexane at 49.9 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance was added at a rate of 0.370 mmol / min. The other conditions were the same as in Example 1, and a conjugated diene polymer (A2) was obtained.
[0227] Example 3 To the first reactor, 1,3-butadiene was added at a rate of 19.8 g / min and normal hexane at a rate of 165.6 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance was added at a rate of 0.145 mmol / min, and to the second reactor, 1,3-butadiene was added at a rate of 7.2 g / min, styrene at a rate of 4.2 g / min, normal hexane at a rate of 33.2 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.253 mmol / min, and the internal temperature of the second reactor was set to 78° C. Other conditions were the same as in Example 1, and a conjugated diene polymer (A3) was obtained.
[0228] Example 4 To the first reactor, 1,3-butadiene was added at a rate of 18.8 g / min and normal hexane at a rate of 163.4 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance was added at a rate of 0.023 mmol / min, and the temperature inside the first reactor was raised to 82°C. Further, to the second reactor, 1,3-butadiene was added at a rate of 11.2 g / min, styrene at a rate of 5.3 g / min, normal hexane at a rate of 44.8 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.153 mmol / min. Other conditions were the same as in Example 1, and a conjugated diene polymer (A4) was obtained.
[0229] (Example 5) As coupling agents, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "coupling agent A" in the table) was continuously added at a rate of 0.110 mmol / min, and tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent B" in the table) was continuously added at a rate of 0.007 mmol / min. Other conditions were the same as in Example 1, and a conjugated diene polymer (A5) was obtained.
[0230] Example 6 The polymerization initiator added to the first reactor was n-butyllithium at 0.193 mmol / min, and the polar substance added to the second reactor was 2,2-bis(2-oxolanyl)propane at 0.019 mmol / min, and the coupling agent added to the second reactor was 2,2-bis(2-oxolanyl)propane at 0.298 mmol / min. The other conditions were the same as in Example 1, and a conjugated diene polymer (A6) was obtained.
[0231] Example 7 To the first reactor, n-butyllithium was added as a polymerization initiator at a rate of 0.343 mmol / min, 2,2-bis(2-oxolanyl)propane was added as a polar substance at a rate of 0.033 mmol / min, and to the second reactor, 2,2-bis(2-oxolanyl)propane was added at a rate of 0.596 mmol / min, and 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "coupling agent A" in the table) was added as a coupling agent at a rate of 0.173 mmol / min. Other conditions were the same as in Example 1, and a conjugated diene polymer (A7) was obtained.
[0232] Example 8 To the first reactor, n-butyllithium was added as a polymerization initiator at a rate of 0.198 mmol / min, 2,2-bis(2-oxolanyl)propane was added as a polar substance at a rate of 0.019 mmol / min, and to the second reactor, 2,2-bis(2-oxolanyl)propane was added at a rate of 0.298 mmol / min, and 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (referred to as "coupling agent C" in the table) was added as a coupling agent at a rate of 0.052 mmol / min. The other conditions were the same as in Example 1, and a conjugated diene polymer (A8) was obtained.
[0233] Example 9 To the first reactor, n-butyllithium was added as the polymerization initiator at a rate of 0.130 mmol / min, 2,2-bis(2-oxolanyl)propane was added as the polar substance at a rate of 0.015 mmol / min, and to the second reactor, 2,2-bis(2-oxolanyl)propane was added at a rate of 0.235 mmol / min. Tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent B" in the table) was continuously added as a coupling agent at a rate of 0.017 mmol / min. SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that 25.0 g was added per 100 g of polymer. The other conditions were the same as in Example 1, and a conjugated diene polymer (A9) was obtained.
[0234] Example 10 1,3-butadiene and styrene were continuously added to the second reactor at a rate of 13.8 g / min, 2.7 g / min, and normal hexane was continuously added to the second reactor at a rate of 46.6 g / min. Other conditions were the same as in Example 4, to obtain a conjugated diene polymer (A10).
[0235] Example 11 As a polar substance to be added to the first reactor, 2,2-bis(2-oxolanyl)propane was continuously added at a rate of 0.266 mmol / min, and to the second reactor, 2,2-bis(2-oxolanyl)propane was continuously added at a rate of 0.176 mmol / min. Other conditions were the same as in Example 1, and a conjugated diene polymer (A11) was obtained.
[0236] Example 12 To the first reactor, 1,3-butadiene and styrene were added at 13.8 g / min and 4.4 g / min simultaneously, normal hexane was added at 104.8 g / min, and 2,2-bis(2-oxolanyl)propane was added as a polar substance at a rate of 0.003 mmol / min, and the internal temperature of the first reactor was set to 65°C. Furthermore, to the second reactor, 1,3-butadiene was added at 2.9 g / min, no additional styrene was added, normal hexane was added at 9.5 g / min, and 2,2-bis(2-oxolanyl)propane as an additional polar substance was added at a rate of 0.020 mmol / min, the internal temperature of the second reactor was raised to 65°C, and as a coupling agent, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "coupling agent A" in the table) was added at a rate of 0.087 mmol / min, and tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent B" in the table) was added continuously at 0.009 mmol / min. Other conditions were the same as in Example 1, and a conjugated diene-based polymer (A12) was obtained.
[0237] Example 13 The polymerization initiator n-butyllithium was added to the first reactor at a rate of 0.370 mmol / min, and the polar substance 2,2-bis(2-oxolanyl)propane was added to the second reactor at a rate of 0.036 mmol / min, and the other conditions were the same as in Example 7, to obtain a conjugated diene polymer (A13).
[0238] Example 14 To the first reactor, n-butyllithium was added as the polymerization initiator at a rate of 0.062 mmol / min, 2,2-bis(2-oxolanyl)propane was added as the polar substance at a rate of 0.007 mmol / min, and to the second reactor, 2,2-bis(2-oxolanyl)propane was added at a rate of 0.094 mmol / min. Tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent B" in the table) was continuously added as a coupling agent at a rate of 0.008 mmol / min. SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that 37.5 g was added per 100 g of polymer. The other conditions were the same as in Example 9, and a conjugated diene polymer (A14) was obtained.
[0239] Example 15 To the first reactor, 1,3-butadiene was added at 21.4 g / min, normal hexane at 170.3 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance was added at 0.054 mmol / min, and to the second reactor, 1,3-butadiene was added at 9.2 g / min, styrene at 3.5 g / min, normal hexane at 36.8 g / min, and 2,2-bis(2-oxolanyl)propane at 0.394 mmol / min. The other conditions were the same as in Example 1, and a conjugated diene polymer (A15) was obtained.
[0240] Example 16 To the first reactor, 1,3-butadiene was added at 15.4 g / min, normal hexane at 166.0 g / min, and 2,2-bis(2-oxolanyl)propane as a polar substance at 0.072 mmol / min, and to the second reactor, 1,3-butadiene was added at 12.6 g / min, styrene at 5.3 g / min, normal hexane at 48.2 g / min, and 2,2-bis(2-oxolanyl)propane at 0.340 mmol / min, and the polymerization temperature of the second reactor was 80° C. The other conditions were the same as in Example 1, and a conjugated diene polymer (A16) was obtained.
[0241] Reference Example 1 To the first reactor, 1,3-butadiene was added at 22.3 g / min and styrene at 4.2 g / min simultaneously, normal hexane was added at 178.8 g / min, 2,2-bis(2-oxolanyl)propane was added as a polar substance at a rate of 0.101 mmol / min, the internal temperature of the first reactor was set to 68° C. Further, to the second reactor, 1,3-butadiene was added at 7.4 g / min, no additional styrene was added, normal hexane was added at 26.7 g / min, no additional polar substance was added, and the internal temperature of the second reactor was set to 73° C. Other conditions were the same as in Example 1, and a conjugated diene polymer (B1) was obtained.
[0242] Comparative Example 1 A conjugated diene polymer (B2) was obtained in the same manner as in Example 1, except that 2,2-bis(2-oxolanyl)propane was added as a polar substance to the first reactor at a rate of 0.266 mmol / min, and 1,3-butadiene was added at 9.7 g / min, additional styrene at 5.4 g / min, normal hexane at 41.3 g / min, and 2,2-bis(2-oxolanyl)propane as an additional polar substance at a rate of 0.156 mmol / min to the second reactor.
[0243] Comparative Example 2 A conjugated diene polymer (B3) was obtained under the same conditions as in Reference Example 1, except that the step of adding a coupling agent was not carried out.
[0244] Comparative Example 3 A conjugated diene polymer (B4) was obtained in the same manner as in Reference Example 1, except that n-butyllithium was continuously added to the first reactor at a rate of 0.343 mmol / min as a polymerization initiator, 2,2-bis(2-oxolanyl)propane at a rate of 0.124 mmol / min and normal hexane at a rate of 109.2 g / min as polar substances, and 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "coupling agent A" in the table) as a coupling agent at a rate of 0.173 mmol / min.
[0245] Comparative Example 4 A conjugated diene polymer (B5) was obtained in the same manner as in Reference Example 1, except that to the first reactor, n-butyllithium was added at a rate of 0.198 mmol / min as a polymerization initiator, 2,2-bis(2-oxolanyl)propane was added at a rate of 0.070 mmol / min as a polar substance, and 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (referred to as "coupling agent C" in the table) was added at a rate of 0.052 mmol / min as a coupling agent, and then SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was added continuously as a rubber softener so that 25.0 g was added per 100 g of the polymer.
[0246] Comparative Example 5 A conjugated diene polymer (B6) was obtained in the same manner as in Reference Example 1, except that to the first reactor, n-butyllithium was added at a rate of 0.130 mmol / min as a polymerization initiator, 2,2-bis(2-oxolanyl)propane at a rate of 0.055 mmol / min as a polar substance, and tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent B" in the table) at a rate of 0.017 mmol / min as a coupling agent, and then SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 37.5 g per 100 g of the polymer.
[0247]
[0248]
[0249]
[0250] [Examples 17 to 32], [Reference Example 2], [Comparative Examples 6 to 10] Using the conjugated diene polymers A1 to A16 and B1 to B6 shown in Tables 1 to 3 as raw rubbers, rubber compositions containing each raw rubber were obtained according to the formulation shown below. Conjugated diene polymers (A1 to A16, B1 to B6): 100 parts by mass (oil excluded) Silica (trade name "Ultrasil 7000GR" manufactured by Evonik Degussa, nitrogen adsorption specific surface area 170 m 2 / g): 85.0 parts by mass Carbon black (trade name "SEAST 7HM (N234)" manufactured by Tokai Carbon Co., Ltd.): 2.0 parts by mass Silane coupling agent (trade name "Si69" manufactured by Evonik Degussa, bis(triethoxysilylpropyl)tetrasulfide): 6.8 parts by mass S-RAE oil (trade name "Process NC140" manufactured by JX Nippon Oil & Energy Corporation): 40 parts by mass Zinc oxide: 2.4 parts by mass Stearic acid: 1.25 parts by mass Antioxidant (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine): 3.5 parts by mass Sulfur: 1.0 part by mass Vulcanization accelerator 1 Tetrabenzyl thiuram disulfide: 0.5 parts by mass Vulcanization accelerator 2 N-(tert-butyl)-2-benzothiazole sulfenamide: 2.5 parts by mass Total: 246.95 parts by mass
[0251] The above materials were kneaded by the following method to obtain rubber compositions. Using an internal kneader (0.3 L capacity) equipped with a temperature control device, the raw rubbers (A1 to A16, B1 to B6), fillers (silica, carbon black), silane coupling agent, process oil, zinc oxide, and stearic acid were kneaded in the first stage at a filling rate of 65% and a rotor rotation speed of 30 to 50 rpm. The temperature of the internal mixer was controlled, and each rubber composition (compound) was obtained at a discharge temperature of 145 to 150°C.
[0252] Next, in the second stage of mixing, the compound obtained above was cooled to room temperature, and then an antioxidant was added. The compound was then mixed again to improve the dispersion of the silica. Again, the temperature of the mixer was controlled to 120°C to discharge the compound. After cooling, in the third stage of mixing, sulfur and vulcanization accelerators 1 and 2 were added and mixed using an open roll set at 70°C. The mixture was then molded and vulcanized in a vulcanization press at 160°C for 20 minutes. The rubber compositions before and after vulcanization were evaluated. Specifically, the evaluations were performed using the following methods. The evaluation results are shown in Tables 4 to 6.
[0253] [Evaluation 1 to 3: Viscoelastic parameters] Viscoelastic parameters were measured in torsion mode using a viscoelasticity tester "ARES" manufactured by Rheometrics Scientific Co. Each measured value was indexed, with the result for the rubber composition of Reference Example 2 being set at 100.
[0254] ([Evaluation 1] Low hysteresis loss) Tan δ measured at 50° C., a frequency of 10 Hz, and a strain of 3% was used as an index of low hysteresis loss. The larger the index, the better the low hysteresis loss, and an index value of 85 or more was determined to have sufficient low hysteresis loss.
[0255] ([Evaluation 2] Wet Grip Performance) Tan δ measured at 0°C, a frequency of 10 Hz, and a strain of 1% was used as an index of wet grip performance. A larger index value indicates better wet grip performance. An index value of 130 or more was determined to have sufficient wet grip performance.
[0256] ([Evaluation 3] Low-temperature performance) The storage modulus G' measured at -20°C, a frequency of 10 Hz, and a strain of 1% was used as an index of low-temperature performance. A larger index indicates better low-temperature properties. An index value of 65 or more was determined to have sufficient low-temperature properties.
[0257] [Evaluation 4] Abrasion Resistance Using an Acron Abrasion Tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.), the amount of abrasion was measured at a load of 44.4 N and 1,000 revolutions in accordance with JIS K6264-2, and the result of Reference Example 2 was indexed as 100. The larger the index, the better the abrasion resistance. A value of 70 or higher was determined to have sufficient abrasion resistance.
[0258] [Evaluation 5: Processability] With regard to the unvulcanized conjugated diene polymers produced by the methods shown in the Examples and Comparative Examples, the polymers were formed into a sheet using a roll immediately after being discharged from the pressure kneader (immediately after discharge following completion of kneading by the pressure kneader in the first stage of kneading), and the sheet was visually observed for its cohesion (shape). Each panelist was given a perfect score of 5 based on the following criteria. Cohesion is an index of the processability of the vulcanized product. A higher index indicates better processability. A score of 4 or higher was considered to have sufficient processability. <Evaluation Criteria> 1: The edge portions of the sheet are 50% or less smooth, resulting in very poor processability. 2: The edge portions of the sheet are more than 50% but not more than 60% smooth, resulting in poor processability. 3: The edge portions of the sheet are more than 60% but not more than 80% smooth, resulting in good processability. 4: The edge portions of the sheet are more than 80% but not more than 90% smooth, resulting in excellent processability. 5: The edge portions of the sheet are more than 90% smooth, resulting in excellent processability.
[0259] [Evaluation 6] Wet grip performance and low temperature properties The index of wet grip performance and low temperature properties was determined by adding up the indices calculated in Evaluations 2 and 3. The larger the index, the better the wet grip performance and low temperature properties.
[0260]
[0261]
[0262]
[0263] As shown in Tables 4 to 6, the rubber compositions of conjugated diene polymers of Examples 17 to 32, which used conjugated diene polymers A1 to A16 satisfying the estimated Tg, were found to have excellent low-temperature properties when vulcanized, compared to the rubber composition of Comparative Example 6, which used conjugated diene polymer B2.
[0264] As shown in Tables 4 to 6, the rubber compositions of conjugated diene polymers of Examples 17 to 21, 23, 27 to 29, 31 and 32, which used conjugated diene polymers A1 to A5, A7, A11 to A13, A15 and A16, in which the difference between the extrapolated glass transition end temperature and the onset temperature satisfies the range of 15°C or more and 35°C or less, were found to have an excellent balance of wet grip performance and low temperature properties when vulcanized, compared to the rubber composition of Reference Example 2, which used conjugated diene polymer B1.
[0265] As shown in Tables 4 to 6, the rubber composition of Example 22 using the conjugated diene polymer A6 was found to have an excellent balance between wet grip performance and low-temperature properties when vulcanized, compared to the rubber composition of Comparative Example 7 using the conjugated diene polymer B3.
[0266] When the rubber compositions of Example 23 and Comparative Example 8, Example 24 and Comparative Example 9, and Example 25 and Comparative Example 10 were compared, it was found that the rubber compositions of Example 23 and Comparative Example 8, Example 24 and Comparative Example 9, and Example 25 and Comparative Example 10, respectively, exhibited an excellent balance between wet grip performance and low temperature properties when vulcanized.
[0267] Furthermore, as shown in Tables 4 to 6, it was found that the rubber compositions of Examples 17 to 24, 26, 27, 29, 31, and 32, which used the conjugated diene polymers A1 to A8, A10, A11, A13, A15, and A16, each of which had a molecular weight distribution of 1.7 or more and 2.5 or less, had excellent processability when vulcanized.
[0268] Furthermore, as shown in Tables 4 to 6, the rubber compositions of Examples 17 to 21 and Examples 23 to 32, which used conjugated diene polymers A1 to A5 and A7 to A16, were found to have excellent low hysteresis loss properties when vulcanized, compared to the rubber composition of Comparative Example 7, which used conjugated diene polymer B3.
[0269] This application is based on a Japanese patent application (Patent Application No. 2023-072838) filed with the Japan Patent Office on April 27, 2023, the contents of which are incorporated herein by reference.
[0270] The conjugated diene polymer of the present invention has industrial applicability as a material in fields such as tire treads, interior and exterior parts of automobiles, vibration-proof rubber, belts, footwear, foams, and various industrial goods.
Claims
1. A conjugated diene polymer, the conjugated diene polymer having an estimated glass transition temperature (estimated Tg) derived from a microstructure in the conjugated diene polymer, of -72°C or more and -45°C or less, the conjugated diene polymer having only one glass transition temperature (Tg) measured by differential scanning calorimetry (DSC), and the difference between the extrapolated glass transition onset temperature and the extrapolated glass transition end temperature of the glass transition temperature (Tg) being 15°C or more and 35°C or less.
2. The conjugated diene polymer according to claim 1, comprising a first polymer segment not containing an aromatic vinyl monomer unit and a second polymer segment containing an aromatic vinyl monomer unit, wherein the amount of vinyl bonds Y1 (mol %) in the bound conjugated diene in the first polymer segment satisfies the following formula (2): 10≦Y1≦45... (2) The estimated glass transition temperature (estimated Tg) derived from the microstructure of the second polymer segment is higher than -45°C and lower than -5°C.
3. The conjugated diene polymer according to claim 1, wherein the molecular weight distribution, which is the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn, is 1.7 or more and 2.5 or less.
4. The conjugated diene polymer according to claim 2, wherein the first polymer segment has a segment ratio of 20% by mass or more and 80% by mass or less.
5. The conjugated diene polymer according to claim 1, having a weight average molecular weight of 300,000 or more and 1,350,000 or less.
6. The conjugated diene polymer according to claim 1, which contains a nitrogen atom.
7. The conjugated diene polymer according to claim 6, wherein the modification rate of the conjugated diene copolymer is 70% or more.
8. A method for producing a conjugated diene polymer according to claim 2, comprising: using two or more continuous reactors; a first polymerization step (P1) of adding a conjugated diene compound, a polymerization initiator and a polar substance to the continuous reactors to continuously form a first polymer segment of a conjugated diene polymer; and a second polymerization step (P2) of adding an aromatic vinyl compound and a polar substance to the continuous reactors to form a second polymer segment at an end of the first polymer segment.
9. The method for producing a conjugated diene polymer according to claim 8, further comprising a coupling step (P3) of reacting the conjugated diene polymer with a coupling agent after the second polymer step (P2).
10. The method for producing a conjugated diene polymer according to claim 8, wherein the mass ratio of the conjugated diene compound added in the first polymerization step (P1) to the total amount of the conjugated diene compound and the aromatic vinyl compound added is 20 mass% or more and 80 mass% or less.
11. The method for producing a conjugated diene polymer according to claim 8, wherein the polymerization reaction rate in the first polymerization step (P1) is 75% or more and 95% or less.
12. The method for producing a conjugated diene polymer according to claim 8, wherein the mass ratio of the aromatic vinyl compound added in the second polymerization step (P2) to the amount of the conjugated diene compound added is 0.15 or more and 0.70 or less.
13. The method for producing a conjugated diene-based polymer according to claim 8, wherein a polar substance is added in the second polymerization step (P2) in an amount greater than the amount of polar substance added in the first polymerization step (P1).
14. The method for producing a conjugated diene polymer according to claim 9, wherein the coupling agent is an aminoalkoxysilane compound.
Citation Information
Patent Citations
Organic compound and organic light-emitting element
JP2023072838A
Boiling cooler
JP2024140211A
Rubber composition for tire treads
JP3438317B2
Method for preparing modified conjugated diene-based polymer
WO2018128285A1
Rubber composition for a tyre tread
WO2021005295A1