Sheet for structure
The structural sheet with a functional, intermediate, and adhesive layer configuration addresses shear deformation and peeling issues, ensuring robust adhesion and water resistance across temperature extremes, enhancing roof repair efficacy.
Patent Information
- Application Number
- PCT/JP2024/016290
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-24
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing structural sheets used for roof repairs are prone to shear deformation and peeling off from the base, leading to water infiltration issues, especially when exposed to varying temperatures and weight loads.
A structural sheet with a layered configuration comprising a functional layer, an intermediate layer, and an adhesive layer, where the adhesive layer has a storage modulus of 1.0×10^2 Pa at 80°C and 1.0×10^7 Pa or less at -10°C, providing enhanced adhesion and resistance to shear deformation.
The sheet effectively suppresses shear deformation and peeling, ensuring reliable attachment to the roof surface across temperature variations, thereby preventing water infiltration and allowing for extensive coverage without compromising structural integrity.
Smart Images

Figure JP2024016290_31102024_PF_FP_ABST
Abstract
Description
Structural Sheets
[0001] The present specification discloses a sheet that is attached to a structure when in use.
[0002] When a slate roof of a house is exposed to wind and rain for a long period of time, it deteriorates. Leaks from deteriorated slate roofs are a concern. Paint is applied to slate roofs to prevent leaks. However, in cases where a slate roof is severely deteriorated, applying paint may not prevent leaks.
[0003] Japanese Patent Application Laid-Open No. 2022-101896 discloses a roof repair method using a sheet having a polymer cement layer and a resin layer. By attaching this sheet to the roof, it is possible to suppress roof leaks.
[0004] JP 2022-101896 A
[0005] When a roof is repaired using the sheet disclosed in JP 2022-101896 A, a worker may step on the sheet. The worker's weight may apply a shear force to the sheet. This shear force induces shear deformation (shift) of the sheet.
[0006] A multi-sheet repair can cover a large area of a roof. In this repair, a second sheet is partially overlapped on top of a first sheet, adjacent to the first sheet. At the overlap, the second sheet can delaminate from the underlying first sheet. This delamination can lead to water infiltration into the roof.
[0007] Similar problems arise when repairing roofs other than slate roofs, and when repairing or reinforcing structures other than roofs.
[0008] The present applicant intends to provide a structural sheet that is resistant to shear deformation and peeling from the substrate.
[0009] The structural sheet disclosed in the present specification has a functional layer and an adhesive layer. The storage modulus of the adhesive layer at 80°C is 1.0 × 10 2The storage modulus of this adhesive layer at −10° C. is 1.0×10 7 Pa or less.
[0010] This structural sheet is resistant to shear deformation even when applied in summer, and is also resistant to peeling from the substrate even in winter.
[0011] FIG. 1 is a perspective view showing a portion of a structural sheet according to one embodiment. FIG. 2 is a cross-sectional view taken along line II-II in FIG. 1. FIG. 3 is an enlarged view showing a portion designated by reference numeral III in FIG. 2. FIG. 4 is a front view showing the structural sheet of FIG. 1 together with a roof. FIG. 5 is an enlarged view showing a portion designated by reference numeral V in FIG. 4. FIG. 6 is an enlarged cross-sectional view taken along line VI-VI in FIG. 4. FIG. 7 is an enlarged cross-sectional view taken along line VII-VII in FIG. 5. FIG. 8 is a flowchart showing a method for repairing a roof using the structural sheet of FIG. 1. FIG. 9 is a cross-sectional view showing a portion of a structural sheet according to a second embodiment. FIG. 10 is a cross-sectional view showing a portion of a structural sheet according to a third embodiment. FIG. 11 is a perspective view showing a method for measuring the shear strength of a structural sheet according to an example. FIG. 12 is a cross-sectional view schematically showing a structural sheet according to a fourth embodiment. FIG. 13 is a cross-sectional view schematically showing a structural sheet according to a fifth embodiment. Fig. 14 is a cross-sectional view schematically showing a structure of a structural sheet according to a sixth embodiment. Fig. 15 is a schematic diagram showing the structure of a supply item containing a structural sheet according to the present disclosure.
[0012] Preferred embodiments will be described in detail below, with reference to the accompanying drawings as appropriate. <First Embodiment> [Layer Structure] Figures 1-3 show a structure sheet 2 (hereinafter also referred to as sheet 2). The planar shape of this sheet 2 is generally rectangular. As is clear from Figure 3, this sheet 2 includes a functional layer 4, an intermediate layer 6, and an adhesive layer 8, each of which includes at least one layer. As is clear from Figure 3, the sheet 2 includes, for example, a single functional layer 4, an intermediate layer 6, and an adhesive layer 8. This sheet 2 is attached to a structure. The sheet 2 may have a release paper or release film (see release film 9 in Figure 12). The release paper and release film are laminated with the adhesive layer 8. The release paper or release film may remain until a predetermined time, such as when the sheet 2 is used. As will be described later, at least one of the adhesive layer 8 and the functional layer 4 may contain a filler.
[0013] [Functional Layer] In this embodiment, the functional layer 4 is located at the top. In other words, when the sheet 2 is attached to a substrate (such as a structure), the functional layer 4 is located farthest from the substrate. In this embodiment, the functional layer 4 is located above the adhesive layer 8. The functional layer 4 contributes to the functions desired for the sheet 2. Examples of these functions include light resistance, weather resistance, heat resistance, abrasion resistance, chemical resistance, water impermeability, moisture impermeability, and moisture permeability. The functional layer 4 can contribute to one or more functions.
[0014] The material of the functional layer 4 is a polymer composition. This functional layer 4 is generally flexible. The sheet 2 having this functional layer 4 can conform to the unevenness of the substrate. The polymer composition includes a base polymer. Synthetic resin, synthetic rubber, and natural rubber can be included in the composition as the base polymer.
[0015] When weather resistance is desired for the functional layer 4, the weather resistance of the functional layer 4 can be controlled, for example, by adjusting the material of the functional layer 4 and the selection and content of the material in the functional layer 4. When weather resistance is desired for the functional layer 4, a base polymer that is resistant to degradation by ultraviolet light is preferred as the material for the functional layer 4. Specifically, examples of methods include disposing a material (such as a polymer) in the functional layer 4 that can form a large number of bonding structures having a bonding energy stronger than ultraviolet light (410 kJ / mol), or increasing the content of the material in the functional layer 4. Examples of polymers that can contribute to the weather resistance of the functional layer 4 and the flexibility of the sheet 2 include acrylic resin, acrylic urethane resin, acrylic silicone resin, fluororesin, flexible epoxy resin, and polybutadiene.
[0016] Furthermore, from the viewpoint of reducing the number of reactive sites in the functional layer 4 and chemically stabilizing the functional layer 4, the functional layer 4 may contain a material having a structure with few double bonds. The presence of a large amount of such a material in the functional layer 4 increases the chemical stability of the functional layer 4. An example of such a material is a non-diene rubber. Specific examples of such non-diene rubber include at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber). Examples of methods for forming a large amount of such bond structures in the functional layer 4 include unevenly distributing at least one of a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays, an additive such as HALS that absorbs UV rays and suppresses the generation of radicals, and an antioxidant such as a phenolic or thioether-based antioxidant.
[0017] From the viewpoint of weather resistance, an example of a resin particularly suitable for the base polymer of the functional layer 4 of this embodiment is an acrylic silicone resin. The acrylic silicone resin contains a siloxane bond. The acrylic silicone resin also has excellent heat resistance and cold resistance. Specific examples of compositions containing an acrylic silicone resin include "Cool Life SP Black (CB1) P5-0" manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., "Bell Earth Elastic Black" manufactured by Fujikura Kasei Co., Ltd., "Aronble Coat T-1000" manufactured by Toagosei Co., Ltd., and "Acryset EMN325E" and "U-Double EF008" manufactured by Nippon Shokubai Co., Ltd. The polymer composition of the functional layer 4 may contain additives such as pigments, fillers, reinforcing materials, and antifouling agents as needed. The functional layer 4 containing a pigment has excellent cosmetic properties. The polymer composition may contain organic and inorganic pigments. Examples of fillers include metal oxide particles such as silica, alumina, and titania. An example of a reinforcing material is cellulose nanofiber. The content of each additive is adjusted depending on the function.
[0018] In Figure 3, arrow T1 indicates the thickness of the functional layer 4. From the viewpoint of functionality, the thickness T1 is preferably 10 µm or more, more preferably 30 µm or more, and particularly preferably 40 µm or more. From the viewpoints of flexibility, productivity, and lightness of the sheet 2, the thickness T1 is preferably 500 µm or less, more preferably 300 µm or less, and particularly preferably 200 µm or less. The structural sheet 2 may have two or more functional layers 4. When the functional layer 4 contains a filler, it may contain the same filler as the filler contained in the intermediate layer 6 described below.
[0019] [Intermediate Layer] The intermediate layer 6 contributes to the rigidity of the sheet 2. The intermediate layer 6 is, for example, a layer that determines the shape of the sheet 2. The intermediate layer 6 has, for example, the function of maintaining the overall shape of the sheet 2. A preferred material for the intermediate layer 6 is a composite material of a polymer and a filler. This makes it easier to impart a predetermined rigidity to the structural sheet 2. Examples of polymers include acrylic resin, acrylic silicone resin, fluororesin, and silicone resin. Examples of fillers include cement, mortar, silica, alumina, titanium oxide, calcium carbonate, and carbon black. A preferred composite material contains acrylic resin and mortar. Polymer cement is particularly preferred. The materials exemplified above may be used alone or in combination.
[0020] By controlling the ratio of the resin component and mortar, which are the materials of the intermediate layer 6, the rigidity of the structural sheet 2 can be easily controlled and the degree of freedom in material design can be improved. Furthermore, the thickness of the intermediate layer 6 can be obtained to an extent that makes it easy to handle. Furthermore, for example, by adjusting the particle shape of the filler, the rigidity of the structural sheet 2 can be controlled. Specific examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod-shaped. Furthermore, by adjusting the thickness of the intermediate layer 6, the rigidity of the structural sheet 2 can be controlled.
[0021] Specific examples of compositions containing a polymer suitable for the intermediate layer 6 include "Spring Coat Brush Mixture" manufactured by Kikusui Chemical Industry Co., Ltd. and "Aronble Coat A450 Base" manufactured by Toagosei Co., Ltd. Specific examples of compositions containing cement suitable for the intermediate layer 6 include "Spring Coat Brush Powder" manufactured by Kikusui Chemical Industry Co., Ltd. and "Aronble Coat A450 Setter" manufactured by Toagosei Co., Ltd.
[0022] When the intermediate layer 6 contains a resin and mortar, the ratio of the resin to the total of the resin and mortar is preferably 10% by mass or more and 90% by mass or less. An intermediate layer 6 having this ratio of 10% by mass or more has excellent adhesion to other layers (functional layer 4). From this viewpoint, this ratio is more preferably 30% by mass or more, and particularly preferably 40% by mass or more. An intermediate layer 6 having this ratio of 90% by mass or less has excellent rigidity. From this viewpoint, this ratio is more preferably 70% by mass or less, and particularly preferably 60% by mass or less.
[0023] In Figure 3, arrow T2 indicates the thickness of the intermediate layer 6. From the viewpoint of the rigidity of the sheet 2, the thickness T2 is preferably 100 µm or more, more preferably 200 µm or more, and particularly preferably 300 µm or more. From the viewpoint of the productivity and lightness of the sheet 2, the thickness T2 is preferably 1500 µm or less, more preferably 1000 µm or less, and particularly preferably 700 µm or less. The structure sheet 2 may have two or more intermediate layers 6. The structure sheet 2 may have a layer structure that does not include an intermediate layer 6.
[0024] The structural sheet 2 may include one or more intermediate layers 6. The number of intermediate layers 6 included in the structural sheet 2 is set in consideration of, for example, the overall thickness of the structural sheet 2, the function to be imparted to the intermediate layers 6, the length of the factory production line, or the production cost of the structural sheet 2. For example, if a single intermediate layer 6 having a predetermined thickness cannot be obtained due to the short length of the factory production line, a laminated structure of multiple intermediate layers 6 having a predetermined overall thickness can be formed by applying multiple layers of material for the intermediate layer 6.
[0025] [Adhesive Layer] The adhesive layer 8 abuts against the base. The sheet 2 is attached to the structure due to the adhesive force of the adhesive layer 8. The adhesiveness of the adhesive layer 8 can be controlled, for example, by adjusting the thickness and surface properties of the adhesive layer 8, and the material of the adhesive layer 8. When controlling the surface properties of the adhesive layer 8, for example, a microstructure, as described below, can be employed. Furthermore, setting the thickness of the adhesive layer 8 to an appropriate value that is neither too thick nor too thin is also effective in controlling the adhesiveness of the adhesive layer 8. Furthermore, from the viewpoint of easily controlling the adhesive force of the adhesive layer 8 within a predetermined range, it is also preferable to adjust the adhesive material and the thickness of the adhesive layer 8 in combination.
[0026] More specifically, examples of materials for the adhesive layer 8 include adhesives that have a low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone having a siloxane bond, rubber, urethane-based materials, and polyester-based materials. The adhesive strength of the adhesive layer 8 can be controlled by adjusting the thickness of the adhesive layer 8 or the degree of crosslinking of the adhesive layer 8. The attachment surface of the adhesive layer 8 may also be configured with a microstructure (a structure with a large surface area and capable of utilizing intermolecular forces) similar to the limbs of a gecko. Furthermore, the adhesive and the microstructure may be used in combination.
[0027] The material of the adhesive layer 8 in this embodiment is, for example, a pressure-sensitive adhesive composition based on a polymer. Examples of polymers suitable for pressure-sensitive adhesive compositions include acrylic resin, silicone, polyurethane, polyester, natural rubber, and synthetic rubber. Acrylic resin is a particularly preferred polymer for the base material because of its excellent weather resistance and heat resistance and the wide variety of raw materials available. Acrylic resin has the advantage that the molecular weight can be adjusted by polymerization, and by forming a copolymer, cohesive components and / or functional group components can be incorporated into the skeleton of the base polymer.
[0028] Specific examples of acrylic pressure-sensitive adhesive compositions include those manufactured by Toyochem Co., Ltd. under the trade names "Olivine BPS6574," "Olivine BPS6554," and "Olivine BPS5565K." Specific examples of urethane pressure-sensitive adhesive compositions include those manufactured by Sanyo Chemical Industries, Ltd. under the trade names "Polysic UPK-2" and "Polysic UPS-2A." Specific examples of polyester pressure-sensitive adhesive compositions include those manufactured by Mitsubishi Chemical Corporation under the trade names "LP-050S50TO," "SNT," "NP-120S45EO," "NP-110S50EO," "S-0091S55EO," and "S-0097S55EO." Specific examples of rubber pressure-sensitive adhesive compositions include those manufactured by Big Technos Corporation under the trade names "GR-1139," "GR-1045M-1," "GR-1025M-1," and "GRN-13B." Specific examples of silicone-based pressure-sensitive adhesive compositions include those available under the trade names "X-40-3237," "X-40-3240," and "X-40-3291-1" manufactured by Shin-Etsu Chemical Co., Ltd. For the reasons described above, an acrylic pressure-sensitive adhesive composition is preferably used for the structural sheet of the present disclosure.
[0029] The pressure-sensitive adhesive composition may contain a curing agent. The type of curing agent is not particularly limited, and an appropriate curing agent can be selected and used depending on the type of polymer. Examples of curing agents include isocyanate curing agents, epoxy curing agents, and metal chelate curing agents. If necessary, irradiation crosslinking using ultraviolet (UV) or electron beam (EB) may be used in combination. The amount of curing agent is not particularly limited, and can be adjusted depending on the type of polymer and curing agent. For example, the amount of curing agent relative to 100 parts by mass of the base polymer of the pressure-sensitive adhesive composition may be 0.5 parts by mass or more, 1.0 parts by mass or more, 2.0 parts by mass or more, or 3.0 parts by mass or more, or 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less.
[0030] When the substrate is an acrylic resin, a preferred curing agent is an isocyanate curing agent. This is because isocyanates are highly reactive and readily undergo curing reactions with compounds containing active hydrogen, such as amines, alcohols, carboxylic acids, mercaptans, urethanes, and carboxylic acid amides. The ratio of isocyanate curing agent to 100 parts by mass of acrylic resin is preferably 1.0 parts by mass or more, more preferably 2.0 parts by mass or more, and particularly preferably 2.5 parts by mass or more. This ratio is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 7 parts by mass or less. By incorporating an appropriate amount of curing agent, an appropriate storage modulus (described in detail below) of the adhesive layer 8 can be achieved.
[0031] The pressure-sensitive adhesive composition may contain a tackifier. Generally, the resin or elastomer used as the base material of a pressure-sensitive adhesive composition has adhesive strength due to its high molecular weight, but may have poor wettability to the object to be adhered and may also have low cohesive strength due to its softness. The tackifier has the function of improving the wettability to the object to be adhered. Therefore, a pressure-sensitive adhesive composition containing a tackifier quickly wets and spreads on the object, thereby fully exerting its adhesive strength.
[0032] Examples of tackifiers include rosin resin-based tackifiers, rosin derivative resin-based tackifiers, terpene resin-based tackifiers, petroleum resin-based tackifiers such as C5 resin, C5 / C9 resin, and C9 resin, phenol resin-based tackifiers, terpene phenol resin-based tackifiers, and chroman-styrene resin-based tackifiers. The ratio of the tackifier to 100 parts by mass of the base polymer is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and particularly preferably 1.5 parts by mass or more. This ratio is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and particularly preferably 7 parts by mass or less. The type and amount of tackifier are selected so as to achieve the storage modulus value described below. By incorporating an appropriate amount of a tackifier having an appropriate softening point, an excellent storage modulus of the adhesive layer 8 can be achieved.
[0033] Specific examples of rosin resin-based tackifiers include the trade names "Ester Gum H," "Ester Gum AA-V," and "Ester Gum 105" manufactured by Arakawa Chemical Industries, Ltd. The hot softening points of these products are as follows: Ester Gum H: 68°C or higher and 75°C or lower Ester Gum AA-V: 82°C or higher and 95°C or lower Ester Gum 105: 100°C or higher and 110°C or lower
[0034] In Figure 3, arrow T3 indicates the thickness of the adhesive layer 8. From the viewpoint of adhesiveness, the thickness T3 is preferably 30 µm or more, and more preferably 50 µm or more. From the viewpoint of suppressing shear deformation of the sheet 2 and from the viewpoint of productivity and light weight of the sheet 2, the thickness T3 is preferably 300 µm or less, more preferably 200 µm or less, and particularly preferably 150 µm or less. From the viewpoint of easily obtaining an adhesive layer that is resistant to shear deformation and has excellent adhesive strength, the preferred thickness of the adhesive layer is 50 µm or more and 200 µm or less, and more preferably 100 µm or more and 150 µm or less. The structural sheet 2 may have two or more adhesive layers 8.
[0035] [Release Film] The release film 9 is disposed (attached) on the surface of the adhesive layer 8 opposite to the intermediate layer 6. It is preferable that the release film 9 be attached to the sheet for structure 2 for the purpose of protecting the surface of the adhesive layer 8 before use. The release film 9 is peeled off when the sheet for structure 2 is attached. After the release film 9 is peeled off to expose the adhesive layer 8, the sheet for structure 2 is attached to a structure by bringing the adhesive layer 8 into contact with the surface of the structure.
[0036] The structure of the release film 9 is not particularly limited, and may be, for example, a sheet having a support layer and a peel layer. Examples of materials constituting the support layer include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, and synthetic resins such as polycarbonate. The support layer may also be formed primarily from paper. Furthermore, the support layer may be a laminate having two or more constituent layers.
[0037] Examples of materials constituting the release layer include silicone resins, melamine resins, and fluorinated polymers. The release layer can be formed, for example, by applying a coating liquid containing the material constituting the release layer and an organic solvent onto the support layer by a known coating method such as gravure coating, roll coating, comma coating, or lip coating, and then drying and curing the coating film formed by the application. In addition, when forming the release layer, the surface of the support layer on which the release layer is to be formed may be previously subjected to corona treatment or easy-adhesion treatment.
[0038] [Other Layers] The structural sheet 2 may have another layer located on the functional layer 4. A typical example of the other layer is a clear paint layer. The structural sheet 2 may have a layer located between the functional layer 4 and the intermediate layer 6. The structural sheet 2 may have a layer located between the intermediate layer 6 and the adhesive layer 8.
[0039] [Total Thickness] The total thickness of the structural sheet 2 is preferably 150 μm or more, more preferably 300 μm or more, and particularly preferably 400 μm or more. The total thickness is preferably 5.0 mm or less, more preferably 3.0 mm or less, and particularly preferably 1.0 mm or less.
[0040] [Flexibility of the Structure Sheet] The structure sheet 2 has the above-described rigidity while also having appropriate flexibility. For example, the structure sheet 2 has flexibility sufficient to allow it to be wound into a roll. "Rolling" here refers to winding the structure sheet 2 onto a roll core having a diameter of, for example, several centimeters to several tens of centimeters (specifically, for example, a diameter of 10 mm to 300 mm). Even with a thinner roll core, the structure sheet 2 can be wound up to several meters by hand winding or the like. Therefore, for example, the structure sheet 2 can be managed in roll form. Furthermore, the rolled structure sheet 2 can be unfolded at the construction site, and the structure sheet 2 cut to a predetermined size can be quickly prepared and applied. Therefore, the structure sheet 2 can be easily and simply applied to construction targets having a relatively large area.
[0041] Sheet 2 has a shear strength of 14.0 N / cm at 80°C. 2 This is all. This makes it possible to appropriately prevent the occurrence of so-called skidding, a phenomenon in which the structural sheet 2 becomes too flexible in the summer, causing the attachment position to shift when an external force acts on the surface. Furthermore, the adhesive strength of the sheet 2 at -10°C is 4.0 N / 25 mm or more. This allows the sheet to remain securely attached to the surface of a structure even in winter.
[0042] The shear strength of Sheet 2 at 80°C is 42.0 N / cm 2 If the adhesive strength of the sheet 2 at -10°C is 18.0 N / 25 mm or less, particularly 15.0 N / 25 mm or less, it is possible to easily maintain the strength of the sheet 2 within a range that allows easy processing of the sheet 2. Furthermore, if the adhesive strength of the sheet 2 at -10°C is 18.0 N / 25 mm or less, and particularly 15.0 N / 25 mm or less, it is possible to easily peel off the structural sheet 2 from the surface of the structure and re-apply it while preventing damage, even if it becomes necessary to re-apply the structural sheet 2. The shear strength of the sheet 2 at 80°C is, for example, 14.0 N / cm 2 Preferably, it is 20 N / cm or more. 2 More preferably, it is 25 N / cm or more. 2 The adhesive strength of the sheet 2 at −10° C. is, for example, preferably 4.0 N / 25 mm or more, more preferably 6.0 N / 25 mm or more, and even more preferably 9.0 N / 25 mm or more.
[0043] [Manufacturing Method] An example of a manufacturing method for this structural sheet 2 will be described below. In this manufacturing method, the polymer composition of the functional layer 4 is mixed with a solvent to obtain a first coating material. This first coating material is applied to a base film (see base film 39 in Figure 14) to obtain a first coating film. This first coating film is heated, and the solvent volatilizes from the first coating material. This heating hardens the base polymer in the first coating film, and the functional layer 4 is obtained. The base film is a shape-imparting film (sheet) that imparts a shape to the first coating film.
[0044] Next, the composite material of the intermediate layer 6 is mixed with a solvent to obtain a second coating material. This second coating material is applied onto the functional layer 4 to obtain a second coating film. This second coating film is heated to volatilize the solvent from the second coating material. This heating hardens the polymer, and the intermediate layer 6 is obtained.
[0045] Next, the adhesive composition of the adhesive layer 8 is mixed with a solvent to obtain a third coating material. This third coating material is applied onto a release paper or film to obtain a third coating film. This third coating film is heated to volatilize the solvent from the third coating material, thereby obtaining the adhesive layer 8.
[0046] This adhesive layer 8 is overlaid on the intermediate layer 6. Furthermore, the base film is peeled off from the functional layer 4, and the release film is peeled off from the adhesive layer 8, to obtain the structural sheet 2. Note that at least one of the release paper or release film and the base film may be peeled off and removed before use.
[0047] Specific examples of the base film will now be described. The base film is used as a substrate when manufacturing the structural sheet 2. The base film may include resin-laminated paper, which is a process paper used in the manufacturing process of the structural sheet 2, or a resin film. The resin-laminated paper referred to here may have an olefin resin layer such as polypropylene or polyethylene. Specifically, a PP laminate sheet (manufactured by, for example, Lintec Corporation) can be used as the base film. The thickness of this PP laminate sheet is, for example, 50 μm or more and 200 μm or less.
[0048] [Roof Repair] A typical use of this structural sheet 2 is roof repair. Figures 4 and 5 show a repaired roof 10. These figures show two sheets 2 (a first sheet 2a and a second sheet 2b) along with the roof 10. The specifications of the second sheet 2b are the same as those of the first sheet 2a. Examples of roofs 10 include slate roofs, tile roofs, steel roofs (including folded-plate roofs), copper roofs, galvanized roofs, and concrete roofs.
[0049] In Figure 4, the position of the lower edge 12a of the first sheet 2a is generally aligned with the position of the lower edge 14 of the roof 10. The first sheet 2a is attached as a whole to the roof 10. The second sheet 2b overlaps the vicinity of the upper edge 16a of the first sheet 2a near its lower edge 12b (see Figure 5). This overlap forms a seam 18. The portion of the second sheet 2b other than the seam 18 is attached to the roof 10.
[0050] Figure 6 is an enlarged cross-sectional view taken along line VI-VI in Figure 4. Figure 6 shows the roof 10, the first sheet 2a, and the primer layer 20. Figure 6 also shows the functional layer 4a, intermediate layer 6a, and adhesive layer 8a of the first sheet 2a. The primer layer 20 covers the surface of the roof 10. The first sheet 2a is attached to the roof 10 via the primer layer 20. The adhesive force of the adhesive layer 8a causes the first sheet 2a to be attached to the base (roof 10 or primer layer 20). In this specification, the phrase "a sheet is attached to a roof" is used to refer to a case where the sheet 2 is attached to the roof 10 via the primer layer 20 or the like.
[0051] FIG. 7 is an enlarged cross-sectional view taken along line VII-VII in FIG. 5. FIG. 7 shows a cross section of the seam 18. FIG. 7 shows the roof 10, the primer layer 20, the first sheet 2a, and the second sheet 2b. FIG. 7 shows the functional layer 4b, the intermediate layer 6b, and the adhesive layer 8b of the second sheet 2b. As mentioned in FIG. 6, the first sheet 2a is attached to the substrate. The second sheet 2b is attached to the first sheet 2a at the seam 18. The adhesive force of the adhesive layer 8b of the second sheet 2b bonds the second sheet 2b to the functional layer 4a of the first sheet 2a. The portion of the second sheet 2b other than the seam 18 is attached to the roof 10 or the primer layer 20, similar to the first sheet 2a shown in FIG. 6.
[0052] [Repair Method] Figure 8 shows a method for repairing a roof 10 using this sheet 2. In this repair method, first, a primer is applied to the surface of the roof 10 (STEP 1). This primer dries to form a primer layer 20. Next, a plurality of sheets 2 are prepared (STEP 2). These sheets 2 have the same specifications. These sheets 2 include a first sheet 2a (see Figures 4 and 5) and a second sheet 2b.
[0053] This first sheet 2a is attached to the roof 10 (STEP 3). As described above, the position of the lower edge 12a of the first sheet 2a roughly coincides with the position of the lower edge 14 of the roof 10. The second sheet 2b is patched onto this first sheet 2a (STEP 4). By patching, a seam 18 is formed between the first sheet 2a and the second sheet 2b. The third sheet 2 is patched onto this second sheet 2b, and the fourth sheet 2 is patched onto this third sheet 2b. This patching process is repeated in the same manner. When the desired zones on the surface of the roof 10 are covered with sheets 2, the repair is complete.
[0054] [Storage Modulus] The storage modulus G'(1) of the adhesive layer 8 at 80°C is 1.0 × 10 2 After the sheet 2 is attached to the roof 10, a worker may step on the sheet 2. At this time, a shear force is applied to the sheet 2. When an object is placed on the sheet 2, a shear force may also be applied to the sheet 2. When the storage modulus G'(1) of the adhesive layer 8 is 1.0×10 2 In the sheet 2 having a storage modulus G'(1) of 3.1 x 10 Pa or more, shear deformation when a shear force is applied can be suppressed. This sheet 2 is less likely to slip. In this sheet 2, shear deformation can be suppressed even in a high temperature environment such as in summer. From the viewpoint of suppressing shear deformation, the storage modulus G'(1) is set to 3.1 x 10 3 Pa or more is more preferable, and 2.3 × 10 4 Pa or more is particularly preferred.
[0055] The storage modulus G'(2) of the adhesive layer 8 at −10° C. is 1.0×10 7As described above, the adhesive layer 8 contacts the base and the functional layer 4 of the other sheet 2. The storage modulus G'(2) of the adhesive layer 8 is preferably 1.0×10 Pa or less. 7 The sheet 2 having a modulus of elasticity of 1.5 Pa or less is unlikely to peel off from the base and the functional layer 4 of another sheet 2. This adhesive layer 8 can sufficiently prevent peeling even at the point where the adhesive layer 8 abuts on another sheet 2 without the primer layer 20 in between (i.e., at the seam 18). In a structure repaired with this sheet 2, the intrusion of water or the like due to peeling is unlikely to occur. With this sheet 2, peeling can be prevented even in low temperature environments such as winter. From the viewpoint of preventing peeling, the storage modulus G'(2) is 2.3 x 10 6 Pa or less is more preferable, and 8.7 × 10 5 Pa or less is particularly preferred.
[0056] The storage moduli G'(1) and G'(2) can be measured using a viscoelasticity measuring device. An example of a device suitable for the measurement is the "DMAQ850 Rheometer DHR-2" manufactured by TA Instruments Japan Co., Ltd. In this measurement, a 2.0 mm thick slab is prepared from the same composition as the adhesive layer 8. This slab is punched out to obtain a disk-shaped sample with a diameter of 5.0 mm. The measurement conditions are as follows: Frequency: 1.0 Hz Temperature range: -80°C to 80°C Heating rate: 5°C / min Mode: Shear
[0057] As mentioned above, desirable storage moduli G'(1) and G'(2) can be achieved by (1) selecting the type of curing agent, (2) adjusting the content of the curing agent, (3) selecting the type of tackifier, or (4) adjusting the amount of tackifier. Furthermore, desirable storage moduli G'(1) and G'(2) can also be achieved by means of (5) selecting the molecular weight of the base polymer, (6) selecting the type of filler, (7) adjusting the amount of filler, (8) selecting the type of reinforcing material, or (9) adjusting the amount of reinforcing material.
[0058] [Effects] As described above, this sheet 2 is less likely to allow water to seep in through the seams 18. By patching and pasting this sheet 2, the surface of the roof 10 can be covered with the sheet 2 over a wide area. Because the sheet 2 is flexible, it can conform to unevenness. Therefore, even if the roof 10 has unevenness on its surface, the surface of the roof 10 can be covered with the sheet 2 over a wide area. Because the adhesive layer 8 has excellent adhesiveness, the surface of the roof 10 can be covered with the sheet 2 over a wide area even if the surface of the roof 10 is made of a combination of materials. For example, even if the surface of the roof 10 includes both metal and slate, the surface of the roof 10 can be covered with the sheet 2 over a wide area.
[0059] The entire surface of the roof 10 may be covered with the sheet 2. In this specification, the surface of the roof 10 means the surface that can be seen when the roof 10 is viewed vertically from above. A repair method in which the entire surface of the roof 10 is covered with a single type of sheet 2 is not found in conventional construction methods.
[0060] This sheet 2 is lighter than steel plates, copper plates, galvanized iron plates, etc. Therefore, even if a wide area of the surface of the roof 10 is covered with the sheet 2, the adverse effect on the earthquake resistance of the building is small. When deterioration of the sheet 2 occurs over time, another sheet 2 may be laminated on this sheet 2. Even in this case, the adverse effect on the earthquake resistance of the building is small. From the viewpoint of earthquake resistance, the density of the sheet 2 is 4.0 g / cm 3 Preferably, 3.0 g / cm or less 3 More preferably, 2.5 g / cm 3 The following is particularly preferable: This density is much smaller than the density of aluminum-zinc alloy plated steel sheet (trade name "Galvalume Steel Sheet (registered trademark)") which is commonly used for repairing the roof 10.
[0061] [Other Uses] The sheet 2 can contribute to the repair or reinforcement of structures other than the roof 10. Examples of structures other than the roof 10 include residential walls, pillars, eaves, fences, gates, doors, parapets, and rows of trees. The sheet 2 may also be used in commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, and the like.
[0062] Second Embodiment [Layer Structure] Figure 9 shows a structure sheet 22 according to a second embodiment. This sheet 22 has a functional layer 24, an intermediate layer 26, and an adhesive layer 28. The material, thickness, and other configurations of the functional layer 24 are the same as those of the functional layer 4 of the sheet 2 shown in Figure 1-7. The material, thickness, and other configurations of the adhesive layer 28 are the same as those of the adhesive layer 8 of the sheet 2 shown in Figure 1-7. This sheet 22 is attached to a structure. The sheet 22 may have release paper or a release film. The release paper and release film are laminated with the adhesive layer 28.
[0063] [Intermediate Layer] The intermediate layer 26 is disposed between the functional layer 24 and the adhesive layer 28. The intermediate layer 26 includes a reinforcing material 30. The material of the intermediate layer 26, excluding the reinforcing material 30, is the same as the material of the intermediate layer 6 of the sheet 2 shown in Figures 1-7. In this embodiment, the reinforcing material 30 is, for example, a mesh.
[0064] Examples of materials for the reinforcing material 30 include synthetic resins and metals. Preferred examples of synthetic resins include vinylon, polyethylene terephthalate, polypropylene, polystyrene, and polyvinylidene fluoride. Preferred examples of metals include aluminum alloys, carbon steel, and alloy steels. The reinforcing material 30 can contribute to the rigidity of the sheet 22. The sheet 22 including the reinforcing material 30 has excellent handleability. The reinforcing material 30 may include a resin film or metal foil instead of a mesh. The resin film may be, for example, a biaxially stretched film. The reinforcing material 30 can be pressed against the coating film for the intermediate layer 26 before the coating film dries, thereby obtaining the intermediate layer 26 including the reinforcing material 30.
[0065] When the reinforcing material 30 is a mesh, the reinforcing material 30 has, for example, a biaxially woven structure in which warp and weft fibers are arranged in a lattice pattern. The shape of the reinforcing material 30 is not particularly limited. When the reinforcing material 30 is a mesh, the shape of the reinforcing material 30 can be any shape, such as a biaxially woven structure or a triaxially woven structure. As the reinforcing material 30, for example, a mesh material such as high-strength vinylon mesh (e.g., for civil engineering applications) or vinylon (e.g., for agricultural applications), cheesecloth made from polyester, polyvinyl alcohol, or the like is preferred. These reinforcing materials 30 can easily widen the elastic range of the structural sheet 22. They can also easily impart appropriate rigidity to the structural sheet 22. Furthermore, they can improve the handleability of the structural sheet 22.
[0066] For example, the line pitch of the reinforcing material 30 is preferably 50 mm or more and 1.2 mm or less. In other words, the line density of the reinforcing material 30 is preferably 0.2 lines / cm or more and 8.0 lines / cm or less. Such a reinforcing material 30 can easily impart rigidity to the structural sheet 22 while ensuring the tensile strength of the structural sheet 22.
[0067] For example, when the intermediate layer 26 is viewed in a plan view, the reinforcing material 30 may have a size that covers the entire surface of the intermediate layer 26, or may have a size that is smaller than the intermediate layer 26. In other words, the area of the reinforcing material 30 when viewed in a plan view may be equal to or smaller than the area of the intermediate layer 26 when viewed in a plan view.
[0068] The area of the reinforcing material 30 when viewed in a plane (plan view area) is preferably, for example, 60% to 95% of the plan view area of the intermediate layer 26. If the plan view area of the reinforcing material 30 is 60% or more, for example, it is easier to ensure the rigidity of the structural sheet 22 and to control the elongation rate of the structural sheet 22. It is also easier to suppress variations in rigidity in different regions of the structural sheet 22. If the plan view area of the reinforcing material 30 is 95% or less, for example, when the intermediate layer 26 is formed so as to sandwich the reinforcing material 30 in the thickness direction of the structural sheet 22, it is easier to ensure the adhesive strength of the reinforcing material 30 to the intermediate layer 26 throughout the entire intermediate layer 26. The plan view area of the reinforcing material 30 can be measured using a known method.
[0069] The thickness of the reinforcing material 30 is, for example, 10% or more of the thickness of the intermediate layer 26. The thickness of the reinforcing material 30 is, for example, preferably 20% or more of the thickness of the intermediate layer 26, more preferably 30% or more, particularly preferably 40% or more, and most preferably 50% or more. On the other hand, the thickness of the reinforcing material 30 is, for example, 80% or less of the thickness of the intermediate layer 26. The thickness of the reinforcing material 30 is, for example, preferably 70% or less of the thickness of the intermediate layer 26, more preferably 60% or less, and particularly preferably 55% or less. Setting the thickness of the intermediate layer 26 in this manner makes it easier to impart appropriate rigidity to the structural sheet 22.
[0070] Furthermore, by setting the thickness of the reinforcing material 30 and the thickness of the intermediate layer 26 to satisfy the above-mentioned relationship, the structural sheet 22 of the present disclosure can be configured to have excellent adhesion between the adhesive layer 28 and the intermediate layer 26 and appropriate rigidity. Therefore, excellent handleability is obtained when attaching the structural sheet 22 to the roof of a structure or the like, and the structure can be protected for a long period of time by the structural sheet 22 without causing wrinkles or gaps between the structural sheet 22 and the roof of the structure. For example, the lower limit of the thickness of the reinforcing material 30 relative to the thickness of the intermediate layer 26 is preferably 45%, and the upper limit of this thickness is preferably 55%.
[0071] In Figure 9, arrow T2 indicates the thickness of the intermediate layer 26. From the viewpoint of the rigidity of the sheet 22, the thickness T2 is preferably 100 µm or more, more preferably 200 µm or more, and particularly preferably 300 µm or more. From the viewpoint of the productivity and light weight of the sheet 22, the thickness T2 is preferably 1500 µm or less, more preferably 1000 µm or less, and particularly preferably 700 µm or less. The structure sheet 22 may have two or more intermediate layers 26. The structure sheet 22 may have a layer structure that does not include an intermediate layer 26.
[0072] [Uses] This sheet 22 is suitable for roof repair, similar to the sheet 2 shown in Figures 1 to 7. This sheet 22 can also be used for residential walls, pillars, eaves, fences, gates, doors, parapets, tree-lined streets, etc. This sheet 22 may also be used for commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, etc.
[0073] [Storage Modulus] As described above, the material of the adhesive layer 28 is the same as the material of the adhesive layer 8 of the sheet 2 shown in Figures 1-7. Therefore, the storage moduli G'(1) and G'(2) of this adhesive layer 28 are the same as those of the adhesive layer 8. Shear deformation can be suppressed in this sheet 22. Furthermore, this sheet 22 is difficult to peel off from the base and the functional layer 24 of another sheet 22.
[0074] [Density] The density of the sheet 22 is 4.0 g / cm 3 Preferably, 3.0 g / cm or less 3 More preferably, 2.5 g / cm 3 The following are particularly preferred:
[0075] <Third Embodiment> [Layer Structure] Figure 10 shows a structural sheet 32 according to a third embodiment. This sheet 32 has a functional layer 34 and an adhesive layer 36. The material of the functional layer 34 is the same as the material of the functional layer 4 of the sheet 2 shown in Figure 1-7. The material, thickness, and other configurations of the adhesive layer 36 are the same as those of the adhesive layer 8 of the sheet 2 shown in Figure 1-7. This sheet 32 is attached to a structure. The sheet 32 may have release paper or a release film. The release paper and release film are laminated with the adhesive layer 36.
[0076] [Uses] This sheet 32 is suitable for roof repair, similar to the sheet 2 shown in Figures 1 to 7. This sheet 32 can also be used for residential walls, pillars, eaves, fences, gates, doors, parapets, row of trees, etc. This sheet 32 may also be used for commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, etc.
[0077] [Storage Modulus] As described above, the material of the adhesive layer 36 is the same as the material of the adhesive layer 8 of the sheet 2 shown in Figures 1-7. Therefore, the storage moduli G'(1) and G'(2) of this adhesive layer 36 are the same as those of the adhesive layer 8. Shear deformation can be suppressed in this sheet 32. Furthermore, this sheet 32 is difficult to peel off from the base and the functional layer 34 of another sheet 32.
[0078] [Density] The density of the sheet 32 is 4.0 g / cm 3 Preferably, 3.0 g / cm or less 3 More preferably, 2.5 g / cm 3 The following are particularly preferred:
[0079] <Other Supplementary Notes> [Regarding the Rigidity of the Structural Sheet] The structural sheet 2 preferably has a rigidity that can withstand bending, for example, from the viewpoint of ensuring ease of handling when attached to a structure. Therefore, for example, the structural sheet 2 may be configured so that at least one of the first layer disposed on the attachment surface side and the second layer disposed on the opposite side from the attachment surface has a predetermined rigidity. Alternatively, the structural sheet 2 may include a first layer disposed on the attachment surface side, a second layer disposed on the opposite side from the attachment surface, and a third layer disposed between the first and second layers, and the third layer may be configured so as to have a predetermined rigidity. Specific details are described below.
[0080] An example of the first layer disposed on the adhesive surface of the structural sheet 2 is the adhesive layer 8. One method for imparting rigidity to the adhesive layer 8 is to configure the adhesive layer 8 to contain an adhesive and a filler. In this case, the adhesive layer 8 contains an adhesive that has a relatively low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone with a siloxane bond, rubber, or urethane, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the adhesive layer 8 can be controlled by adjusting at least one of the amount of filler added to the adhesive layer 8 and the particle shape of the filler. Specific examples of filler particle shapes include spherical, acicular, amorphous, and tetrapod-shaped. The rigidity of the structural sheet 2 can also be controlled by adjusting the thickness of the functional layer 4. The rigidity of the structural sheet 2 can also be controlled by adjusting the Tg of the adhesive in the functional layer 4.
[0081] An example of the layer disposed on the surface side of the structure sheet 2, i.e., the second layer disposed on the opposite side of the adhesive surface of the structure sheet 2, is the functional layer 4. One example of a method for imparting rigidity to the functional layer 4 is to configure the functional layer 4 to contain a main material and a filler. In this case, the functional layer 4 contains, for example, a main material such as acrylic silicone, fluororesin, silicone resin, or non-diene rubber, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the functional layer 4 can be controlled by adjusting at least one of the amount of filler added to the functional layer 4 and the particle shape of the filler. Specific examples of filler particle shapes include spherical, acicular, amorphous, and tetrapod-shaped. Furthermore, the rigidity of the structure sheet 2 can be controlled by adjusting at least one of the thickness of the functional layer 4 and the Tg of the main material of the functional layer 4. In this way, in the structure sheet 2, at least one of the adhesive layer 8 and the functional layer 4 may contain a filler.
[0082] In a structural sheet 2 that comprises a first layer (e.g., adhesive layer 8) arranged on the side of the application surface, a second layer (e.g., functional layer 4) arranged on the opposite side of the application surface, and a third layer arranged between the first and second layers, and that is configured so that the third layer has a predetermined rigidity, one method of imparting rigidity to the third layer is, for example, to configure the third layer as an intermediate layer 6 described below and impart rigidity to the intermediate layer 6.
[0083] Furthermore, the rigidity of the structural sheet 2 can be controlled by adjusting the Tg of the resin component contained in the intermediate layer 6. The rigidity of the structural sheet 2 can also be controlled by adjusting the amount and diameter of voids in the intermediate layer 6. Furthermore, when the structural sheet 2 includes multiple intermediate layers 6, it may include, for example, a first intermediate layer 6 including a resin component having a Tg of a predetermined value, and a second intermediate layer 6 including a resin component having a Tg lower than that of the resin component contained in the first intermediate layer 6.
[0084] From the viewpoint of ensuring the rigidity of the structural sheet 2, the thickness of the intermediate layer 6 is, for example, 100 μm or more. The thickness of the intermediate layer 6 is, for example, preferably 200 μm or more, more preferably 300 μm or more, and most preferably 350 μm or more. On the other hand, taking into consideration productivity and the like, the thickness of the intermediate layer 6 is, for example, 1500 μm or less. The thickness of the intermediate layer 6 is preferably 1200 μm or less, more preferably 1000 μm or less, and most preferably 750 μm or less. In this way, by appropriately adjusting the thickness of the intermediate layer 6, appropriate rigidity of the structural sheet 2 can be obtained.
[0085] When a resin component, a mortar component, and a reinforcing material 30 are used as materials for the intermediate layer 6, as a specific example, a Spring Coat (Brush) admixture manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the resin component. Also, a Spring Coat (Brush) powder manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the mortar component. Also, a vinylon mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Ltd. can be used as the reinforcing material 30 (mesh component).
[0086] [Details of Reinforcing Material] In order to control the internal structure of the structural sheet 2, it is preferable to place the reinforcing material 30 inside the intermediate layer 6, as described above. In this case, the internal structure of the structural sheet 2 can be controlled by changing the content of the reinforcing material 30 in the intermediate layer 6. Furthermore, when the structural sheet 2 has multiple layers, the structural sheet 2 may have a layered reinforcing material 30 placed inside. In this case, the layered reinforcing material 30 imparts a predetermined rigidity to the structural sheet 2, thereby controlling the internal structure of the structural sheet 2.
[0087] When the sheet for structure 2 contains a filler for adjusting strength, specific methods for imparting rigidity to the sheet for structure 2 include, for example, controlling at least one of the filler material, the amount of filler added to the sheet for structure 2, and the size and shape of the filler particles. In this case, the filler material may be either an inorganic material or an organic material, or a mixture of inorganic and organic materials.
[0088] Nonwoven fabric can also be used as the reinforcing material 30. In this case, the nonwoven fabric is not particularly limited as long as it is formed into a sheet shape without weaving fibers. Examples of fibers constituting the nonwoven fabric include at least one of natural fibers and chemical fibers. Examples of chemical fibers include fibers made of polyolefin resins such as polypropylene and polyethylene, polyester resins, polyacrylic resins, and polyamide resins such as nylon, as well as copolymers and modified products of these resins and synthetic fibers made of combinations of these. Among these, polyester fibers are preferred as they have excellent water resistance, heat resistance, dimensional stability, weather resistance, and the like.
[0089] As a specific method for imparting rigidity to the structural sheet 2, the thickness of the structural sheet 2 may be controlled. In the case of a structural sheet 2 that includes an intermediate layer 6, the rigidity of the structural sheet 2 can also be controlled by adjusting the viscoelasticity of the intermediate layer 6. In this case, the viscoelasticity of the intermediate layer 6 may be adjusted by adjusting the glass transition temperature (Tg, hereinafter also simply referred to as Tg) of the resin contained in the intermediate layer 6 or by changing the degree of crosslinking of the resin. In this way, various methods can be used to control the rigidity of the structural sheet 2.
[0090] <Other Embodiments> Further configurations of the structure sheet 2 are exemplified below. Fig. 12 is a cross-sectional configuration diagram that schematically shows a structure sheet for a structure according to a fourth embodiment. When the release film 9 described above is the first release film 9, the structure sheet 2 of this embodiment includes a second release film 17 that is arranged on the side of the functional layer 44 opposite to the adhesive layer 48 side. As an example, the structure sheet 2 has the first release film 9, adhesive layer 48, intermediate layer 46, functional layer 44, and second release film 17 arranged in this order in the thickness direction.
[0091] The second release film 17 is configured so that when the surface 17a exposed to the outside comes into contact with the surface 9a exposed to the outside of the first release film 9, the surfaces 17a and 9a are unlikely to stick to each other. Therefore, when the structural sheet 2 is unwound from a roll 51 (see FIG. 15 ) around which the sheet 2 described below is wound, the first release film 9 can be easily separated from the second release film 17, and the structural sheet 2 can be easily unwound.
[0092] Furthermore, the second release film 17 has a predetermined rigidity. This improves the rigidity of the structural sheet 2 remaining after the first release film 9 has been peeled off. Therefore, even if the structural sheet 2 remaining after the first release film 9 and the second release film 17 have been peeled off has low rigidity, the handling of the sheet 2 during application can be improved, and the structural sheet 2 can be easily applied to the surface of the structure. Furthermore, the structural sheet 2 remaining after the first release film 9 and the second release film 17 have been peeled off can be designed to have a relatively low rigidity. Therefore, for example, even if the surface of the structure to which the structural sheet 2 is to be applied is not flat due to unevenness or differences in elevation caused by defects, the structural sheet 2 can be applied by conforming well to the surface. Furthermore, for example, the anchoring effect on the surface can be improved, and the adhesive strength of the structural sheet 2 can be sufficiently improved within an acceptable range.
[0093] The structure of the second release film 17 can be set as appropriate. For example, as shown in Fig. 12, the second release film 17 has a contact layer 11 that comes into contact with the first release film 9 when the structural sheet 2 is wound into a roll, and a weak adhesive layer 13 that is disposed on the first release film 9 side of the contact layer 11 when the structural sheet 2 is placed flat.
[0094] The contact layer 11 may be composed of a single layer or multiple layers. The contact layer 11 may also contain a resin. In other words, the contact layer 11 may be a resin layer. Examples of resins that may be contained in the contact layer 11 include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6 and aramid, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, synthetic resins such as polycarbonate, and urethane.
[0095] Alternatively, the contact layer 11 may be a fiber layer containing a fiber component and a binder component that binds the fiber component. Alternatively, the contact layer 11 may contain paper. In this case, the contact layer 11 may contain paper as a main component, or may contain paper in addition to a predetermined main component. When the contact layer 11 contains paper, the contact layer 11 preferably contains paper that has a strength sufficient to prevent the contact layer 11 from being accidentally torn when the structural sheet 2 is attached to the target. Furthermore, when the contact layer 11 contains paper, the contact layer 11 preferably contains, for example, silicone having a siloxane bond in addition to paper. The contact layer 11 has higher rigidity than, for example, the remaining portion of the structural sheet 2 from which the release film 9 and the second release film 17 and the contact layer 11 and the weak adhesive layer 13 are omitted.
[0096] The thickness of the contact layer 11 can be set appropriately, but is, for example, 20 μm to 500 μm. When the contact layer 11 contains polyethylene terephthalate (PET), the thickness of the contact layer 11 is preferably, for example, 20 μm to 50 μm.
[0097] The weak adhesive layer 13 has a relatively low adhesive strength. For example, the adhesive strength of the weak adhesive layer 13 to the functional layer 44 is lower than the adhesive strength of the adhesive layer 48 to the intermediate layer 46. Also, for example, the adhesive strength of the weak adhesive layer 13 to the contact layer 11 is higher than the adhesive strength of the weak adhesive layer 13 to the functional layer 44. The weak adhesive layer 13 may be attached to the functional layer 44 by, for example, static electricity. The weak adhesive layer 13 may contain a main component whose Tg is substantially 0. The weak adhesive layer 13 may contain, for example, ethylene vinyl acetate (EVA), urethane, silicone having a siloxane bond, acrylic, etc. Note that the second release film 17 is not limited to the above-described configuration and may be, for example, a base film 39 described below.
[0098] 13 is a cross-sectional view schematically illustrating a structure of a structural sheet 2 according to a fifth embodiment. The structural sheet 2 of this embodiment includes a release sheet 29 disposed on the side of the functional layer 44 opposite the adhesive layer 48. As an example, the structural sheet 2 has the adhesive layer 48, intermediate layer 46, functional layer 44, and release sheet 29 disposed in this order in the thickness direction. The structural sheet 2 of this embodiment does not include the release film 9.
[0099] The release sheet 29 contains a surface 29a exposed to the outside and a release agent disposed in the vicinity thereof. An example of the release agent is silicone having a siloxane bond. This structure makes it difficult for the surface 29a and the adhesive surface 48a of the release sheet 29 exposed to the outside of the roll 51 to adhere to each other when the surface 29a comes into contact with the adhesive surface 48a of the adhesive layer 48. Therefore, when the structural sheet 2 is unwound from the roll 51, the adhesive layer 48 can be easily peeled from the release sheet 29, allowing the structural sheet 2 to be unwound easily.
[0100] As described above, in the present disclosure, when unwinding the structural sheet 2 from the roll 51, the structural sheet 2 may be made easier to unwind from the roll 51 in advance so that, for example, the portion of the structural sheet 2 provided with the adhesive component does not adhere to other portions of the structural sheet 2, making it difficult to remove. Furthermore, the release sheet 29 has a predetermined rigidity. Therefore, in this embodiment, even if the release film 9 is omitted, the rigidity of the structural sheet 2 can be improved. Therefore, the handleability of the structural sheet 2 is improved, and the structural sheet 2 can be easily attached to the target of the structure. In this case, the release sheet 29 has a higher rigidity than the remaining structural sheet 2 from which the release sheet 29 has been peeled off.
[0101] The structure of the release sheet 29 can be set as appropriate. For example, as shown in Figure 13, the release sheet 29 has a release intermediate layer 15 having a surface 29a that contacts the attachment surface 48a of the adhesive layer 48 when the structural sheet 2 is wound into a roll, and a weak adhesive layer 13 that is disposed on the adhesive layer 48 side of the release intermediate layer 15 when the structural sheet 2 is placed flat. The release intermediate layer 15 may have a configuration similar to that of the contact layer 11, except that it contains, for example, a release agent. The release sheet 29 may also have a release agent layer disposed over the surface 29a.
[0102] 14 is a cross-sectional view schematically illustrating a structural sheet 2 according to a sixth embodiment. The structural sheet 2 of this embodiment includes a base film 39 that is disposed on the side of the functional layer 44 opposite the adhesive layer 48 when laid flat. The base film 39 is the base film used when forming the functional layer 4 described above. The structural sheet 2 of this embodiment includes the base film 39, which remains attached even after the functional layer 44 is formed.
[0103] As an example, the structural sheet 2 has a release film 9, an adhesive layer 48, an intermediate layer 46, a functional layer 44, and a base film 39 arranged in this order in the thickness direction. The surface 39a exposed to the outside of the base film 39 and the surface 9a exposed to the outside of the release film 9 are configured to be less likely to adhere to each other when they come into contact with each other. Therefore, the structural sheet 2 can be easily unwound from the roll 51. The base film 39 also has a predetermined rigidity. In this case, the base film 39 has a higher rigidity than the remaining structural sheet 2 from which the release film 9 and the base film 39 have been peeled off. Therefore, the rigidity of the structural sheet 2 can be improved by the base film 39 in the remaining structural sheet 2 from which the release film 9 has been peeled off. Therefore, even if the rigidity of the remaining structural sheet 2 after the first release film 9 and the base film 39 have been peeled off is low, the handleability of the structural sheet 2 can be improved and the structural sheet 2 can be easily attached to the target structure.
[0104] The base film 39 may contain resin-laminated paper having pseudo-adhesion, which means that two components attached to each other cannot be re-adhered once they are peeled off. In this case, for example, the base film 39 may contain resin-laminated paper in which a resin layer and paper are laminated, and the resin layer and the paper are bonded to each other by pseudo-adhesion within the resin-laminated paper. With this configuration, when the paper in the resin-laminated paper is peeled off from the resin layer while the resin layer is attached to the functional layer 44, only the paper is peeled off and removed, and the resin layer remains attached to the functional layer 44 of the structural sheet 2.
[0105] Next, fourth to sixth embodiments illustrate an installation method for reinforcing or repairing a structure by attaching a structural sheet 2 to the structure. In this installation method, a worker unrolls the required length of the structural sheet 2 from the roll 51. Next, in the fourth and sixth embodiments, the worker peels off the release film 9 from the structural sheet 2 and attaches the exposed attachment surface 48a of the adhesive layer 48 to the surface of the structure to which the structural sheet is to be attached. At this time, the worker may peel off the release film 9 from the structural sheet 2 little by little, and attach the exposed attachment surface 48a of the adhesive layer 48 to the surface of the structure to which the structural sheet is to be attached. On the other hand, in the fifth embodiment, the worker attaches the attachment surface 48a of the adhesive layer 48 of the structural sheet 2 to the surface of the structure to which the structural sheet is to be attached.
[0106] Then, in the fourth to sixth embodiments, the worker applies the structural sheet 2 to the target, and then peels off and removes the corresponding second release film 17, release sheet 29, or base film 39 from the structural sheet 2.
[0107] That is, the construction methods according to the fourth to sixth embodiments include a preparation step of preparing a roll 51 in which the structural sheet 2 is wound into a roll, a payout step of paying out the structural sheet 2 from the roll 51, and an attachment step of peeling the first release film 9 from the paid-out structural sheet 2 and attaching the exposed attachment surface to the surface of the structure. Here, in the preparation step of the fourth and sixth embodiments, the roll 51 is prepared using the structural sheet 2 whose attachment surface 48a is covered with the first release film 9.
[0108] In this construction method, the structural sheet 2 in the roll body 51 prepared in the preparation step has a laminated structure including a functional layer 44 and an adhesive layer 48, and a cover sheet is disposed on the side of the functional layer 44 opposite to the adhesive layer 48. The structural sheet 2 including this cover sheet is wound in a roll shape in the roll body 51, and the cover sheet may be peeled off and removed during or after the attachment step. This cover sheet may be any of the second release film 17, the release sheet 29, and the base film 39.
[0109] Furthermore, in the construction method of the fourth embodiment, the structural sheet 2 in the roll body 51 prepared in the preparation step has a laminated structure including a functional layer 44 and an adhesive layer 48, and has a release sheet 29 that is arranged on the opposite side of the adhesive layer 48 of the functional layer 44 and is separate from the release film 9, and in the preparation step, a roll body 51 in which the structural sheet 2 is wound into a roll shape may be prepared so that the release sheet 29 comes into contact with the adhesive layer 48.
[0110] When using the structural sheet 2 of the present disclosure, for example, the following supply item 45 can be used. FIG. 15 is a schematic diagram showing the structure of a supply item 45 containing the structural sheet 2 of the present disclosure. FIG. 15 shows, as an example, a structural sheet 2 provided with a release film 9. The supply item 45 shown in FIG. 15 includes a roll 51 around which a strip-shaped structural sheet 2 is wound, and a container 50 having a storage space 50a for storing the roll 51. The container 50 has a supply port 50b that can unwind and supply the structural sheet 2 from the roll 51 stored in the storage space 50a to the outside. The supply port 50b has a width dimension that is equal to or greater than the width dimension of the structural sheet 2 in the axial direction of the roll 51.
[0111] For example, a worker can carry the supply item 45 to a construction site, unwind the required length of the structural sheet 2 from the supply item 45, and use the structural sheet 2 for construction. Therefore, the supply item 45 allows the structural sheet 2 to be stored in the form of a roll 51 suitable for storage. Furthermore, when using the structural sheet 2, only the required amount can be unwound from the supply item 45. This improves work efficiency.
[0112] Furthermore, when unwinding the structural sheet 2 from the supply port 50b, the worker can unwind the structural sheet 2 while applying uniform tension to the entire widthwise area of the structural sheet 2, for example, by pressing the entire widthwise area of the structural sheet 2 against the periphery of the opening of the supply port 50b. This allows the structural sheet 2 to be applied to the surface of the structure with uniform tension. Therefore, it is possible to prevent unexpected contraction or expansion of the structural sheet 2 after application due to uneven tension acting on the structural sheet 2 after application. Note that in order to apply uniform tension to the entire widthwise area of the structural sheet 2, a separate member such as a long member that extends in the widthwise direction of the structural sheet 2 and comes into contact with the structural sheet 2 may be placed, for example, around the periphery of the opening of the supply port 50b.
[0113] Furthermore, the structural sheet provided in the supply item 45 may be any structural sheet disclosed herein, and may be, for example, the structural sheet 2 of any of the fourth to sixth embodiments, or the structural sheet 2 of any other embodiment.
[0114] <Examples> The effects of the structural sheet according to the examples will be explained below. The scope of the disclosure in this specification should not be construed as being limited based on the description of these examples. [Example 1] A pressure-sensitive adhesive composition A was obtained by adding 2.0 parts by mass of a tackifier (the above-mentioned product name "Ester Gum AAV") to 100 parts by mass of an acrylic resin (the above-mentioned product name "Oribain BPS5565K"), and further adding 6.0 parts by mass of an isocyanate curing agent (the above-mentioned product name "BHS8515" manufactured by Toyochem Co., Ltd.). This pressure-sensitive adhesive composition A was used to form a 2.0 mm thick adhesive layer, and the storage modulus was measured. The storage modulus G'(1) at 80°C of the adhesive layer according to Example 1 was 8.4 x 10 4 Pa, and the storage modulus G'(2) at -10°C is 5.8 × 10 5 It was Pa.
[0115] A 130 μm-thick base film, a PP laminate sheet manufactured by Lintec Corporation, was prepared. A functional layer-forming composition containing an acrylic resin (a 50:50 mixture of "Cool Life SP Black (CB1) P5-0" manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. and FC Coat Water-Based Silicone Elastic Black manufactured by Fujikura Kasei Co., Ltd.) was applied to the base film. The resulting coating was dried to form a single-layer functional layer with a thickness of 110 μm.
[0116] Next, a mixture of cement and a liquid mixture of a composition for forming an intermediate layer (manufactured by Kikusui Chemical Industry Co., Ltd., product name "Spring Coat (trowel)") in a ratio of 60:40 was prepared. This mixture was applied to the functional layer. A vinylon-based mesh material (manufactured by Kuraray Co., Ltd., product name "Cremona", #600 (600 grit, thickness 230 μm) was placed so as to be pressed against the surface of the coating film of this mixture. This cured the coating, and an intermediate layer with a thickness of 450 μm after curing was formed on the functional layer. Thereafter, an adhesive layer was combined with the functional layer and intermediate layer to produce the structural sheet shown in Figure 1-3 as the structural sheet of Example 1.
[0117] [Examples 2-5 and Comparative Examples 1-3] Structural sheets of Examples 2-5 and Comparative Examples 1-3 were produced in the same manner as Example 1, except that the type and amount of tackifier were changed as shown in the following Table 1. The storage modulus G'(1) at 80°C and the storage modulus G'(2) at -10°C of the adhesive layers provided in the structural sheets of Examples 2-5 and Comparative Examples 1-3 are shown in Table 1 below.
[0118] Example 6: 2-Ethylhexyl acrylate (2-EHA) and acrylic acid (AA) were mixed in ethyl acetate at a molar ratio (2-EHA / AA) of 97 / 3, and then azobisisobutyronitrile (AIBN) was added as a crosslinking agent to carry out solution polymerization, thereby synthesizing an acrylic polymer. The resulting acrylic polymer was measured by gel permeation chromatography (GPC), and the results were a weight-average molecular weight Mw of 412,000, a number-average molecular weight Mn of 42,000, and a molecular weight distribution Mw / Mn of 9.8. The GPC measurement was carried out using tetrahydrofuran as the eluent at 40°C.
[0119] To 100 parts by mass of the obtained acrylic polymer, 1.0 part by mass of a tackifier (polymerized rosin manufactured by Arakawa Chemical Industries, Ltd., trade name "Aradigm R-95") and 1.0 part by mass of a curing agent (trade name "Tetrad C" manufactured by Mitsubishi Gas Chemical Trading Co., Ltd.) were added, thereby obtaining a pressure-sensitive adhesive composition M. Except for using this pressure-sensitive adhesive composition M, a pressure-sensitive adhesive layer and a sheet for structures for measuring the storage modulus were prepared as Example 6 in the same manner as in Example 1. The storage modulus G'(1) at 80°C of the pressure-sensitive adhesive layer of the sheet for structures in Example 6 was 1.4 × 10 2 Pa, and the storage modulus G'(2) at -10°C is 2.6 × 10 4 It was Pa.
[0120] [Shear Test] A plate 38 shown in Fig. 11 was prepared. The material of this plate 38 was steel. This plate 38 had a width of 30 mm and a length of 50 mm. Meanwhile, a test piece 40 having a width of 15 mm and a length of 50 mm was cut out from a structural sheet. This plate 38 and test piece 40 were placed in a thermostatic chamber at a temperature of 80°C and left to stand for 30 minutes. As shown in Fig. 11, the test piece 40 was overlapped on the plate 38 so that the overlap length was 15 mm. The adhesive layer was in contact with the plate 38. The contact area between the plate 38 and the adhesive layer was 2.25 cm 2The test specimen 40 was firmly attached to the plate 38 by rolling a roller having a mass of 2 kg back and forth on the test specimen 40 once. The plate 38 and the test specimen 40 were placed in a thermostatic chamber at 80°C and left to stand for 30 minutes. The plate 38 and the test specimen 40 were set in a tensile tester equipped with a temperature controller, and a tensile test was performed. In this test, the test specimen 40 was pulled relative to the plate 38 in the direction indicated by arrow A1. The test conditions were as follows: Temperature controller: "THC1 WF-200T-X" manufactured by Shimadzu Corporation Tensile tester: "AGX-V" manufactured by Shimadzu Corporation Test temperature: 80°C Chuck distance: 50 mm Tensile speed: 50 mm / min The measurement was stopped when the rate of decrease in the test force reached 1% / s, and the maximum test force (N) was determined. This maximum test force is applied to the contact area (2.25 cm 2 ) to obtain the shear force (N / cm 2 The results are shown in Table 1 below.
[0121] [Peel Test] Using test pieces prepared in accordance with the provisions of "JIS Z0237:2022 10.1," a 180° peel test was performed in accordance with the provisions of "JIS Z0237:2022 11.5" to measure adhesive strength (N / 25 mm). The test conditions were as follows: Testing machine: "Autograph AGX-V" manufactured by Shimadzu Corporation Testing temperature: -10°C Testing speed: 300 mm / min The results are shown in Table 1 below.
[0122]
[0123] [Examples 7-12]
[0124] Structural sheets of Examples 7-12 were prepared in the same manner as in Example 1, except that the thickness of the adhesive layer was changed to the values shown in Table 2 below. The storage modulus G'(1) at 80°C and the storage modulus G'(2) at -10°C of the adhesive layer provided in the structural sheets of Examples 1-12 are shown in Table 2 below. In addition, the structural sheets of Examples 7-12 were each subjected to the above-mentioned [shear test] and [peel test] to measure the shear force (N / cm 2The adhesive strength (N / 25 mm) and the adhesive strength (N / 25 mm) were measured. The results are shown in Table 2 below. For comparison, the results of Example 1, in which the adhesive layer had a thickness of 100 μm, are also shown in Table 2.
[0125]
[0126] As is clear from Table 1, the structural sheets of each Example exhibit a sufficiently large shear force in an environment of 80°C. These sheets also exhibit a sufficiently large adhesive force in an environment of -10°C. Furthermore, as is clear from Table 2, the structural sheets of each Example can control the shear force and adhesive force by changing the thickness of the adhesive layer. These evaluation results clearly demonstrate the superiority of the structural sheets according to the present disclosure.
[0127] [Disclosure items]
[0128] Each of the following sections discloses a preferred embodiment.
[0129] [Item 1] A sheet-like adhesive having a functional layer and an adhesive layer, wherein the adhesive layer has a storage modulus of 1.0 × 10 at 80°C. 2 Pa or more, and the storage modulus at -10°C is 1.0 × 10 7 A structural sheet having a compressive strength of 0.2 Pa or less.
[0130] [Item 2] The structural sheet according to Item 1, wherein the adhesive layer is made of an adhesive composition, and the base material of this composition is an acrylic resin.
[0131] [Item 3] The structural sheet according to Item 2, wherein the pressure-sensitive adhesive composition contains an isocyanate curing agent.
[0132] [Item 4] The structural sheet according to item 2 or 3, wherein the pressure-sensitive adhesive composition contains a tackifier.
[0133] [Item 5] The structural sheet according to any one of Items 1 to 4, wherein the adhesive layer has a thickness of 30 μm or more and 300 μm or less.
[0134] [Item 6]
[0135] Shear force at 80°C is 14.0 N / cm 26. The structural sheet according to any one of items 1 to 5, wherein the adhesive strength at -10°C is 4.0 N / 25 mm or more.
[0136] [Item 7]
[0137] 7. The structural sheet according to any one of items 1 to 6, further comprising an intermediate layer disposed between the functional layer and the adhesive layer.
[0138] [Item 8]
[0139] 8. The structural sheet according to claim 7, wherein the intermediate layer includes a reinforcing material.
[0140] [Item 9] The structural sheet according to item 7 or 8, wherein at least one of the functional layer and the adhesive layer contains a filler.
[0141] [Item 10]
[0142] 10. The structural sheet according to any one of items 1 to 9, further comprising a release film disposed on the surface of the adhesive layer opposite to the functional layer side.
[0143] [Item 11] A method for repairing or reinforcing a structure, comprising: (1) a functional layer and a film having a storage modulus of 1.0 × 10 at 80 °C; 2 Pa or more, and the storage modulus at -10°C is 1.0 × 10 7 (2) preparing a first sheet having a functional layer and an adhesive layer having a storage modulus at 80°C of 1.0 x 10 2 Pa or more, and the storage modulus at -10°C is 1.0 × 10 7 (3) a step of attaching the first sheet to the surface of the structure by the adhesive force of the adhesive layer of the first sheet; and (4) a step of attaching the second sheet to the surface of the first sheet and the surface of the structure by the adhesive force of the adhesive layer of the second sheet, while overlapping a portion of the second sheet near the edge of the first sheet.
[0144] [Item 12] A method for repairing a roof, comprising: (1) forming a functional layer and a laminated laminated laminated laminated with a storage modulus at 80°C of 1.0 x 10 2Pa or more, and the storage modulus at -10°C is 1.0 × 10 7 (1) preparing a plurality of sheets each having an adhesive layer with a modulus of elasticity of 100 Pa or less; and (2) attaching the sheets to the surface of the roof by the adhesive strength of the adhesive layer of each sheet, thereby covering the entire surface of the roof with the plurality of sheets.
[0145] The configurations of the present disclosure are not limited to the above-described embodiments and examples, and the configurations and methods can be changed, added, or deleted without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. For example, part of the configuration described in one embodiment or example can be applied to the configuration described in any other embodiment or example.
[0146] The structural sheet described above can be used by being attached to various objects.
[0147] DESCRIPTION OF SYMBOLS 2: Structural sheet 2a: First sheet 2b: Second sheet 4: Functional layer 4a: Functional layer of first sheet 4b: Functional layer of second sheet 6: Intermediate layer 6a: Intermediate layer of first sheet 6b: Intermediate layer of second sheet 8: Adhesive layer 8a: Adhesive layer of first sheet 8b: Adhesive layer of second sheet 10: Roof 18: Seam 20: Primer layer 22: Structural sheet 24: Functional layer 26: Intermediate layer 28: Adhesive layer 30: Reinforcing material 32: Structural sheet 34: Functional layer 36: Adhesive layer 38: Plate 40: Test piece 44: Functional layer 46: Intermediate layer 48: Adhesive layer
Claims
1. A film having a functional layer and an adhesive layer, wherein the adhesive layer has a storage modulus of 1.0×10 at 80° C. 2 Pa or more, and the storage modulus at −10° C. is 1.0×10 7 A structural sheet having a compressive strength of 100 Pa or less.
2. The structural sheet according to claim 1, wherein the adhesive layer is made of an adhesive composition, and the base material of this composition is an acrylic resin.
3. The structural sheet according to claim 2, wherein the pressure-sensitive adhesive composition contains an isocyanate curing agent.
4. The structural sheet according to claim 2 or 3, wherein the pressure-sensitive adhesive composition contains a tackifier.
5. The structural sheet according to claim 1 or 2, wherein the thickness of the adhesive layer is 30 μm or more and 300 μm or less.
6. Shear force at 80°C is 14.0 N / cm 2 3. The structure sheet according to claim 1 or 2, wherein the adhesive strength at -10°C is 4.0 N / 25 mm or more.
7. The structural sheet according to claim 1 or 2, further comprising an intermediate layer disposed between the functional layer and the adhesive layer.
8. The structural sheet according to claim 7, wherein the intermediate layer includes a reinforcing material.
9. The structural sheet according to claim 7, wherein at least one of the functional layer and the adhesive layer contains a filler.
10. The structural sheet according to claim 1 or 2, further comprising a release film disposed on the surface of the adhesive layer opposite the functional layer.
11. A method for repairing or reinforcing a structure, comprising: (1) a functional layer and a material having a storage modulus of 1.0 x 10 at 80°C 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 (2) preparing a first sheet having a functional layer and an adhesive layer having a storage modulus at 80° C. of 1.0×10 Pa or less; 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 (3) a step of attaching the first sheet to the surface of the structure by the adhesive force of the adhesive layer of the first sheet; and (4) a step of attaching the second sheet to the surface of the first sheet and the surface of the structure by the adhesive force of the adhesive layer of the second sheet, while overlapping a portion of the second sheet near an edge of the first sheet.
12. A method for repairing a roof, comprising: (1) forming a functional layer and a layer having a storage modulus of 1.0 x 10 at 80°C; 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 and (2) a step of attaching each sheet to the surface of the roof by the adhesive strength of the adhesive layer of each sheet, thereby covering the entire surface of the roof with the multiple sheets.
Citation Information
Patent Citations
Adhesive composition, adhesive sheet, and moisture-permeable waterproof adhesive sheet
JP2015040280A
Adhesive composition, adhesive sheet and image display device
JP2017095659A
Adhesive composition, adhesive and adhesive sheet
JP2021075651A
Adhesive and adhesive sheet for repeated-bendable device, repeated-bendable laminate, and repeated-bendable device
JP2022117307A
Acrylic adhesive composition, acrylic adhesive, adhesive film, and flexible device