Thermally conductive sheet
The thermally conductive sheet, composed of an ester-based phase change material and silicone resin with anisotropically oriented fillers, effectively reduces contact thermal resistance, addressing the limitations of conventional sheets and improving heat transfer efficiency in electronic devices.
Patent Information
- Application Number
- PCT/JP2024/016291
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional thermally conductive sheets fail to sufficiently lower contact thermal resistance, limiting the efficiency of heat transfer in electronic devices despite improved thermal conductivity.
A thermally conductive sheet is developed by blending an ester-based phase change material with a silicone resin and thermally conductive fillers, where the ester phase change material has a melting point between 25°C and 120°C, and the filler is anisotropically oriented to reduce contact thermal resistance.
The thermally conductive sheet achieves a contact thermal resistance value of 0.040 K cm²/W and a thermal resistance value of 0.160 K cm²/W, enhancing heat dissipation efficiency in electronic devices.
Smart Images

Figure JP2024016291_31102024_PF_FP_ABST
Abstract
Description
Thermally conductive sheet
[0001] The present invention relates to a thermally conductive sheet.
[0002] In electronic devices such as computers, automobile parts, and mobile phones, heat sinks and other heat dissipators are commonly used to dissipate heat generated from heat-generating elements such as semiconductor elements and mechanical parts. It is known that a thermally conductive sheet is placed between the heat-generating element and the heat dissipator to improve the efficiency of heat transfer to the heat dissipator.
[0003] Various types of thermally conductive sheets have been proposed to improve their thermal conductivity. For example, Patent Documents 1 to 3 disclose thermally conductive sheets containing a side-chain crystalline polyalphaolefin (CPAO) as the hydrocarbon compound (B). Patent Document 4 also discloses a thermally conductive sheet containing a binder resin and a thermally conductive filler, in which the contact thermal resistance of the thermally conductive sheet with respect to an adherend is 0.46°C cm. 2 Furthermore, Patent Document 5 discloses a thermally conductive sheet having a thermal conductivity of 1 / W or less. Furthermore, Patent Document 5 discloses that the sliced surface is polished to expose the anisotropic filler from the sheet surface, and the arithmetic mean curve (Spc) of the peaks is smoothed to a predetermined value or less, thereby increasing the adhesion to the contact surface and reducing the thermal resistance, thereby improving the thermal conductivity of the thermally conductive sheet in the thickness direction.
[0004] International Publication No. 2022 / 070568 International Publication No. 2022 / 137762 International Publication No. 2022 / 163192 Patent No. 7029503 Publication No. International Publication No. 2020 / 067141
[0005] In recent years, in the market centered on the electronic devices, the amount of heat generated has increased due to improvements in device performance, and there is an increasing need for thermally conductive sheets with lower thermal resistance in order to efficiently diffuse heat.
[0006] Here, for example, the thermal resistance in heat transfer of a laminate consisting of a heating element, a thermally conductive sheet, and a heat sink is the sum of the thermal resistance of the thermally conductive sheet itself, the contact thermal resistance at the interface between the heating element and the thermally conductive sheet, and the contact thermal resistance at the interface between the thermally conductive sheet and the heat sink. To reduce the thermal resistance, it is important to improve the thermal conductivity of the thermally conductive sheet itself and to make the thermally conductive sheet thin. However, the thermal resistance of a thin thermally conductive sheet is more influenced by the contact thermal resistance than by the thermal conductivity of the thermally conductive sheet itself. Therefore, there is a demand for a thermally conductive sheet with low contact thermal resistance.
[0007] However, conventional thermally conductive sheets such as those disclosed in Patent Documents 1 to 5 are unable to sufficiently reduce contact thermal resistance, and even if the thermal conductivity of the thermally conductive sheet itself is improved, there is a limit to how much thermal resistance can be reduced.
[0008] Therefore, an object of the present invention is to provide a thermally conductive sheet with low contact thermal resistance.
[0009] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by incorporating an ester-based phase-change material into a thermally conductive sheet together with a silicone resin and a thermally conductive filler. That is, the present invention provides the following [1] to
[14] .
[0010] [1] A thermally conductive sheet comprising a matrix containing a silicone resin and an ester-based phase-change material, and a thermally conductive filler. [2] The thermally conductive sheet according to [1], wherein the melting point of the ester-based phase-change material is greater than 25°C and less than or equal to 120°C. [3] The thermally conductive sheet according to [1] or [2], wherein the ester-based phase-change material has a hydrocarbon chain containing 14 to 44 carbon atoms. [4] The thermally conductive sheet according to any one of [1] to [3], wherein the ester-based phase-change material is an ester of a fatty acid and an alcohol, and at least one of the fatty acid and the alcohol has an alkyl group containing 14 to 22 carbon atoms. [5] The thermally conductive sheet according to any one of [1] to [4], wherein the content of the ester-based phase-change material is 1 to 20 parts by mass per 100 parts by mass of the silicone resin and the ester-based phase-change material combined. [6] The thermally conductive sheet according to any one of [1] to [5], wherein the thermally conductive filler contains an anisotropic filler. [7] The thermally conductive sheet according to [6], wherein the major axis of the anisotropic filler is oriented in the thickness direction of the thermally conductive sheet. [8] The thermally conductive sheet according to any one of [1] to [7], wherein the thickness of the thermally conductive sheet is 0.05 to 3.0 mm. [9] The thermal contact resistance value to nickel is 0.040 (K cm 2
[10] The thermal conductive sheet according to any one of [1] to [8], wherein the thermal resistance value when compressed under a load of 40 psi is 0.160 (K cm 2 / W) or less.
[11] The thermally conductive sheet according to any one of [1] to [9], wherein the ester-based phase-change material comprises at least one selected from stearyl stearate, nonadecyl nonadecylate, cetyl myristate, myristyl myristate, and behenyl behenylate.
[12] The thermally conductive sheet according to [6], wherein the thermally conductive filler further comprises a non-anisotropic filler.
[13] A laminate comprising the thermally conductive sheet according to any one of [1] to
[12] and a release film laminated on at least one surface of the thermally conductive sheet.
[14] A method of using the thermally conductive sheet according to any one of [1] to
[12] , wherein the thermally conductive sheet is interposed between two members and conducts heat from one member to the other member.
[0011] According to the present invention, it is possible to provide a thermally conductive sheet having low contact thermal resistance.
[0012] FIG. 2 is a diagram illustrating a measuring device for measuring thermal resistance.
[0013] [Thermal Conductive Sheet] The thermal conductive sheet of the present invention comprises a matrix containing a silicone resin and an ester-based phase change material, and a thermally conductive filler. Each component of the thermally conductive sheet will be described in detail below.
[0014] (Ester-Based Phase-Change Material) In the thermally conductive sheet of the present invention, the matrix may be made of a silicone resin and an ester-based phase-change material. The ester-based phase-change material may be dispersed in the silicone resin in the matrix.
[0015] In the present invention, the matrix contains an ester-based phase-change material, which reduces the contact thermal resistance of the thermally conductive sheet. While the underlying mechanism is unclear, it is presumed to be as follows: In the matrix of the thermally conductive sheet, the ester-based phase-change material is dispersed in silicone resin. However, due to its low compatibility with silicone resin, some of the material precipitates on the surface of the thermally conductive sheet, filling the gaps between the thermally conductive sheet and the adherend. Furthermore, the ester-based phase-change material that fills the gaps has a higher polarity than silicone resin, giving it a high affinity for the metal surface (mainly oxide layers, etc.) of the adherend. This allows it to conform to the minute irregularities on the adherend surface, thereby reducing the contact thermal resistance. Furthermore, during actual use of the thermally conductive sheet, the ester-based phase-change material melts due to heat from a heating element, further enhancing the above-mentioned effect.
[0016] The melting point of the ester-based phase-change material is preferably higher than 25° C. and lower than 120° C., more preferably higher than 30° C. and lower than 80° C., and even more preferably higher than 40° C. and lower than 75° C. When the melting point of the ester-based phase-change material is within the above range, the contact thermal resistance of the thermal conductive sheet can be easily reduced.
[0017] The ester-based phase-change material is a compound having an ester group, and may be a monoester having one ester group, or a diester or other compound having two or more ester groups. However, a monoester or diester is preferred, and a monoester is even more preferred. The number of carbon atoms in the ester-based phase-change material is not particularly limited as long as the ester-based phase-change material is solid at 25°C, but is, for example, 15 or more, preferably 20 or more, more preferably 25 or more, and even more preferably 28 or more. It is also preferably 150 or less, more preferably 100 or less, even more preferably 50 or less, and even more preferably 40 or less. The number of carbon atoms in the ester-based phase-change material is, for example, preferably 15 to 150, more preferably 20 to 100, even more preferably 25 to 50, and even more preferably 28 to 40.
[0018] The ester-based phase-change material preferably has a hydrocarbon chain containing 10 to 45 carbon atoms, more preferably 14 to 44 carbon atoms, even more preferably 14 to 22 carbon atoms, and even more preferably 14 to 18 carbon atoms. The hydrocarbon chain may be linear or branched, but is preferably linear. The ester-based phase-change material is preferably an ester of a fatty acid and an alcohol, and more preferably an ester of a higher fatty acid and a higher alcohol. At least one of the fatty acids and alcohols constituting the ester-based phase-change material preferably has an alkyl group containing 10 to 45 carbon atoms, more preferably 14 to 44 carbon atoms, even more preferably 14 to 22 carbon atoms, and even more preferably 14 to 18 carbon atoms. The alkyl groups in the fatty acids and alcohols may be linear or branched, but are preferably linear. When the carbon number of the hydrocarbon chain or alkyl group in the ester-based phase change material is equal to or greater than the lower limit, the low-polarity hydrocarbon group or alkyl group ensures a certain level of compatibility with the silicone resin, allowing the ester-based phase change material to be uniformly dispersed in the silicone resin, thereby facilitating a low contact thermal resistance value of the thermal conductive sheet. On the other hand, when the carbon number of the hydrocarbon chain or alkyl group in the ester-based phase change material is equal to or less than the upper limit, a certain level of compatibility with the silicone resin is ensured, allowing the ester-based phase change material to be uniformly dispersed in the silicone resin, thereby facilitating a low contact thermal resistance value of the thermal conductive sheet. Furthermore, when the carbon number is equal to or less than a certain level, the melting point of the ester-based phase change material is equal to or less than a certain level, which also facilitates a low contact thermal resistance value of the thermal conductive sheet. The carbon number of the hydrocarbon chain and alkyl group in the ester-based phase change material does not include the carbonyl carbon of the carboxy group.
[0019] The carbon number of the fatty acid is preferably 2 to 46, more preferably 5 to 41, even more preferably 10 to 22, and even more preferably 12 to 18. The carbon number of the fatty acid refers to the total number of carbon atoms, including the carbonyl carbon of the carboxy group. The alcohol may be an alcohol having one hydroxyl group, or an alcohol having two or more hydroxyl groups. The carbon number of the alcohol is preferably 2 to 45, more preferably 5 to 40, even more preferably 10 to 22, and even more preferably 12 to 18. Examples of ester-based phase-change materials that can be used include stearyl stearate, cetyl myristate, pentaerythritol distearate, myristyl myristate, myristyl stearate, nonadecyl nonadecylate, behenyl behenate, glycerin monostearyl ester, and ethylene glycol distearyl ester. Among these, at least one selected from stearyl stearate, nonadecyl nonadecylate, cetyl myristate, myristyl myristate, and behenyl behenylate is preferred, at least one selected from stearyl stearate, cetyl myristate, and myristyl myristate is more preferred, and myristyl myristate, myristyl stearate, and nonadecyl nonadecylate are even more preferred. One type of ester-based phase-change material may be used alone, or two or more types may be used in combination.
[0020] The content of the ester-based phase-change material in the thermally conductive sheet of the present invention is preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 3 to 12 parts by mass, per 100 parts by mass of the total of the silicone resin and the ester-based phase-change material. When the content of the ester-based phase-change material is equal to or greater than the above-mentioned lower limit, the contact thermal resistance of the thermally conductive sheet is easily reduced. Furthermore, when the content of the ester-based phase-change material is equal to or less than the above-mentioned upper limit, the ester-based phase-change material does not precipitate excessively from the thermally conductive sheet, preventing contamination of the heat-generating element and the heat-dissipating element.
[0021] (Silicone resin) The silicone used in the silicone resin may be either condensation reaction type or addition reaction type, but addition reaction type is preferred because it is easy to highly fill the thermally conductive filler and the curing temperature can be easily adjusted by catalyst etc. Silicone resin can be obtained, for example, by curing a curable silicone composition. The curable silicone composition may be, for example, composed of a base agent and a curing agent.
[0022] In the case of an addition reaction type curable silicone composition, it is preferable that the curable silicone composition contains an alkenyl group-containing organopolysiloxane as a base component and a hydrogen organopolysiloxane as a curing agent, from the viewpoint of facilitating high loading of a thermally conductive filler. It is preferable that the curable silicone composition is liquid before curing. Being liquid before curing makes it easy to load a thermally conductive filler highly, and furthermore, makes it easy to disperse an ester-based phase change material in the curable silicone composition. In this specification, "liquid" refers to a composition that is liquid at room temperature (23°C) and under 1 atmosphere.
[0023] The silicone resin in the matrix (or the silicone resin after curing in the case of a curable material) preferably has no fluidity at either room temperature (23°C) or at high temperatures (80°C). Because the silicone resin has no fluidity, the shape retention of the thermally conductive sheet can be ensured at both room temperature and high temperatures. Furthermore, silicone rubber, for example, may be used as the silicone resin of the present invention. The use of silicone rubber facilitates compressive deformation, making it easier to assemble between the heat generating element and the heat sink. Furthermore, the thermally conductive sheet can be given certain compression characteristics, thereby improving reliability.
[0024] Furthermore, in order to ensure the shape retention of the thermally conductive sheet, it is preferable to use a three-dimensionally crosslinked silicone matrix as the silicone resin. To achieve this, for example, in the case of an addition reaction type, it is sufficient to cure a curable silicone composition containing an alkenyl group-containing organopolysiloxane having at least three alkenyl groups per molecule, or a hydrogenorganopolysiloxane having at least three hydrogen atoms attached to silicon atoms.
[0025] The content of the silicone resin may be, for example, about 5 to 45% by volume, preferably 15 to 40% by volume, and more preferably 20 to 38% by volume, based on the total volume of the thermally conductive sheet.
[0026] (Thermal Conductive Filler) The thermally conductive sheet of the present invention further includes a thermally conductive filler. The thermally conductive filler is preferably dispersed in a matrix containing a silicone resin and an ester-based phase change material and held in the matrix. The thermally conductive filler preferably contains an anisotropic filler. The anisotropic filler preferably has its major axis oriented in the thickness direction of the thermally conductive sheet. This facilitates increasing the thermal conductivity of the thermally conductive sheet. When an anisotropic filler is oriented in the thickness direction, its major axis does not need to be strictly parallel to the thickness direction; even if the major axis is slightly tilted relative to the thickness direction, it is still considered to be oriented in the thickness direction. Specifically, an anisotropic filler whose major axis is tilted by less than 20° is also considered to be oriented in the thickness direction. If such anisotropic fillers constitute the majority of the thermally conductive sheet (e.g., more than 60%, preferably more than 80% of the total number of anisotropic fillers), they are considered to be oriented in the thickness direction.
[0027] The content of the thermally conductive filler is preferably 150 to 3,000 parts by mass, more preferably 200 to 2,000 parts by mass, and even more preferably 300 to 1,000 parts by mass, per 100 parts by mass of the total of the silicone resin and the ester-based phase change material. By using 150 parts by mass or more of the thermally conductive filler, a certain level of thermal conductivity can be imparted to the thermally conductive sheet. Furthermore, by using 1,500 parts by mass or less, the thermally conductive filler can be properly dispersed in the matrix. Furthermore, it is possible to prevent the viscosity of the mixed composition described below from becoming unnecessarily high. Furthermore, the volume filling rate of the thermally conductive filler relative to the total amount of the thermally conductive sheet is preferably 50 to 90% by volume, more preferably 55 to 80% by volume, and even more preferably 60 to 75% by volume. By using a volume filling rate above the above lower limit, a certain level of thermal conductivity can be imparted to the thermally conductive sheet. Furthermore, by using a volume filling rate below the upper limit, the thermally conductive sheet can be easily manufactured.
[0028] <Anisotropic Filler> An anisotropic filler is a filler that has an anisotropic shape and can be oriented. Examples of anisotropic fillers include fibrous materials and scaly materials. An anisotropic filler has a high aspect ratio, specifically, an aspect ratio of greater than 2, preferably 5 or greater. By increasing the aspect ratio to greater than 2, the anisotropic filler is more easily oriented in one direction, such as the thickness direction, and the thermal conductivity of the thermal conductive sheet in one direction, such as the thickness direction, is easily increased. The upper limit of the aspect ratio is not particularly limited, but is practically 100. The aspect ratio is the ratio of the major axis length to the minor axis length of the anisotropic filler. In the case of fibrous materials, it means the fiber length / fiber diameter, and in the case of scaly materials, it means the major axis length / thickness of the scaly material.
[0029] The content of the anisotropic filler in the thermally conductive sheet is preferably 10 to 500 parts by mass, more preferably 30 to 300 parts by mass, and even more preferably 50 to 250 parts by mass, per 100 parts by mass of the total of the silicone resin and the ester-based phase-change material. By making the content of the anisotropic filler 10 parts by mass or more, it becomes easier to increase thermal conductivity. Furthermore, by making the content 500 parts by mass or less, the viscosity of the mixed composition described below tends to be appropriate, resulting in good orientation of the anisotropic filler. Furthermore, the dispersibility of the anisotropic filler in the silicone resin also becomes good.
[0030] When the anisotropic filler is a fibrous material, its average fiber length is preferably 10 to 500 μm, more preferably 20 to 350 μm, and even more preferably 50 to 300 μm. An average fiber length of 10 μm or more ensures proper contact between the anisotropic fillers within the thermally conductive sheet, ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive sheet. On the other hand, an average fiber length of 500 μm or less reduces the bulk of the anisotropic filler, allowing it to be highly packed into the matrix. Furthermore, the average fiber length of the fibrous material is preferably shorter than the thickness of the thermally conductive sheet. Being shorter than the thickness prevents the fibrous material from protruding more than necessary from the surface of the thermally conductive sheet. The above average fiber length can be calculated by observing the anisotropic filler under a microscope. More specifically, the fiber lengths of 50 pieces of any anisotropic filler can be measured using, for example, an electron microscope or optical microscope, and the average (arithmetic mean) of the measurements can be used as the average fiber length.
[0031] Furthermore, when the anisotropic filler is a scaly material, its average particle size is preferably 10 to 400 μm, more preferably 15 to 300 μm, and even more preferably 20 to 200 μm. By setting the average particle size to 10 μm or more, the anisotropic fillers in the thermally conductive sheet can easily come into contact with each other, ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive sheet. On the other hand, setting the average particle size to 400 μm or less reduces the bulk of the thermally conductive sheet, allowing for a high loading of the anisotropic filler in the matrix. The average particle size of the scaly material can be calculated by observing the anisotropic filler under a microscope and using the longest diameter as the diameter. More specifically, the longest diameters of 50 pieces of any anisotropic filler can be measured using, for example, an electron microscope or optical microscope, and the average (arithmetic mean) of the measurements can be used as the average particle size.
[0032] The anisotropic filler may be a known material having thermal conductivity. However, when oriented by magnetic field orientation as described below, it is preferable for the filler to have diamagnetic properties. On the other hand, when oriented by flow orientation or when the anisotropic filler is not oriented, it does not need to have diamagnetic properties. Specific examples of anisotropic fillers include carbon-based materials such as carbon fiber or flake carbon powder, metal materials such as metal fiber, metal oxides, boron nitride, metal nitrides, metal carbides, metal hydroxides, and polyparaphenylene benzoxazole fibers. Among these, carbon-based materials are preferred due to their low specific gravity and good dispersibility in the matrix, and graphitized carbon materials with high thermal conductivity are more preferred. Graphitized carbon materials have diamagnetic properties due to the alignment of graphite planes in a specific direction. Boron nitride is also a preferred anisotropic filler. While not particularly limited, boron nitride is preferably used as a flake material. The flake-like boron nitride may be agglomerated or not, but it is preferable that it is not agglomerated in part or in whole. Note that boron nitride also has diamagnetic properties when its crystal planes are aligned in a specific direction.
[0033] Furthermore, the anisotropic filler is not particularly limited, but its thermal conductivity along the anisotropic direction (i.e., the long axis direction) is generally 30 W / m K or more, preferably 60 W / m K or more, more preferably 100 W / m K or more, and even more preferably 200 W / m K or more. The upper limit of the thermal conductivity of the anisotropic filler is not particularly limited, but is, for example, 2000 W / m K or less. The thermal conductivity can be measured by a laser flash method or the like.
[0034] The anisotropic filler may be used alone or in combination of two or more. For example, the anisotropic filler may be an anisotropic filler having at least two different average particle sizes or average fiber lengths. When anisotropic fillers of different sizes are used, the smaller anisotropic fillers are embedded between the relatively larger anisotropic fillers, which is thought to enable the anisotropic fillers to be densely packed in the matrix and to improve heat conduction efficiency.
[0035] The carbon fiber used as the anisotropic filler is preferably graphitized carbon fiber. Furthermore, the scaly carbon powder is preferably scaly graphite powder. It is also preferable to use a combination of graphitized carbon fiber and scaly graphite powder as the anisotropic filler. Graphitized carbon fiber has graphite crystal planes aligned in the fiber axis direction, providing high thermal conductivity in the fiber axis direction. Therefore, by aligning the fiber axis direction in a predetermined direction, thermal conductivity in a specific direction can be increased. Furthermore, scaly graphite powder has graphite crystal planes aligned in the in-plane direction of the scaly surfaces, providing high thermal conductivity in the in-plane direction. Therefore, by aligning the scaly surfaces in a predetermined direction, thermal conductivity in a specific direction can be increased. The graphitized carbon fiber and scaly graphite powder preferably have a high degree of graphitization.
[0036] The graphitized carbon materials, such as the graphitized carbon fiber and flake graphite powder, can be obtained by graphitizing the following raw materials. Examples include condensed polycyclic hydrocarbon compounds such as naphthalene, condensed heterocyclic compounds such as PAN (polyacrylonitrile), and pitch. However, it is particularly preferable to use graphitized mesophase pitch, polyimide, or polybenzazole, which have a high degree of graphitization. For example, by using mesophase pitch, the pitch is anisotropically oriented in the fiber axis direction during the spinning process described below, thereby producing graphitized carbon fibers with excellent thermal conductivity in the fiber axis direction. The use of mesophase pitch in graphitized carbon fibers is not particularly limited as long as it can be spun. Mesophase pitch may be used alone or in combination with other raw materials. However, using mesophase pitch alone, i.e., graphitized carbon fibers with a 100% mesophase pitch content, is most preferable in terms of high thermal conductivity, spinnability, and quality stability.
[0037] The graphitized carbon fiber can be one that has been subjected to spinning, infusibilization, and carbonization in sequence, and then pulverized or cut to a predetermined particle size before graphitization, or one that has been carbonized, pulverized, or cut and then graphitized. When pulverization or cutting is performed before graphitization, condensation polymerization reactions and cyclization reactions are more likely to proceed on the newly exposed surface during the graphitization treatment, thereby increasing the degree of graphitization and enabling the production of graphitized carbon fibers with even improved thermal conductivity. On the other hand, when spun carbon fiber is pulverized after graphitization, the graphitized carbon fiber is stiff and therefore easy to pulverize, and carbon fiber powder with a relatively narrow fiber length distribution can be obtained by pulverization for a short period of time.
[0038] As described above, the average fiber length of the graphitized carbon fiber is preferably 10 to 500 μm, more preferably 20 to 350 μm, and even more preferably 50 to 300 μm. As described above, the aspect ratio of the graphitized carbon fiber is greater than 2, and preferably equal to or greater than 5. The thermal conductivity of the graphitized carbon fiber is not particularly limited, but the thermal conductivity in the fiber axis direction is preferably 400 W / m K or greater, and more preferably 800 W / m K or greater.
[0039] When the thermally conductive sheet contains an anisotropic filler, the anisotropic filler may or may not be exposed on the sheet surface, but is preferably exposed. The sheet surface of the thermally conductive sheet can be made non-adhesive by exposing the anisotropic filler. The thermally conductive sheet is the main surface of the sheet, and the anisotropic filler may be exposed on only one of the two surfaces of the sheet, or on both surfaces. The non-adhesive sheet surface of the thermally conductive sheet allows sliding when assembled to an electronic device, etc., improving assembly ease.
[0040] <Non-anisotropic filler> The thermally conductive filler of the present invention may contain a non-anisotropic filler, or the above-mentioned anisotropic filler may be used in combination with a non-anisotropic filler. When the non-anisotropic filler is used in combination with an anisotropic filler oriented in one direction, the non-anisotropic filler is interposed in the gaps between the oriented anisotropic fillers, thereby further increasing thermal conductivity. The non-anisotropic filler is a filler that has substantially no anisotropy in shape, and is a filler that does not orient in a predetermined direction even under an environment in which the anisotropic filler orients in a predetermined direction, such as under the generation of magnetic field lines or under the action of shear force, as described below.
[0041] The aspect ratio of the non-anisotropic filler is 2 or less, and preferably 1.5 or less. When used in combination with an anisotropic filler, a non-anisotropic filler with such a low aspect ratio is more likely to be arranged in the gaps between the anisotropic filler, making it easier to improve thermal conductivity. Furthermore, by setting the aspect ratio to 2 or less, an increase in the viscosity of the mixed composition described below can be prevented, enabling high filling.
[0042] Specific examples of non-anisotropic fillers include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, and oxides, nitrides, and carbides other than metals. The shapes of the non-anisotropic fillers include spherical and irregular powders. Examples of metals in non-anisotropic fillers include aluminum, copper, and nickel. Examples of metal oxides include aluminum oxide (e.g., alumina), magnesium oxide, and zinc oxide. Examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Examples of carbon materials include spherical graphite. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, aluminum oxide and aluminum are preferred because of their high thermal conductivity and the ease of obtaining spherical fillers. The non-anisotropic fillers may be used alone or in combination of two or more of the above.
[0043] The average particle size of the non-anisotropic filler is, for example, 0.1 to 200 μm. For example, when used in combination with an anisotropic filler, the average particle size of the non-anisotropic filler is preferably 0.1 to 50 μm, more preferably 0.5 to 35 μm, and even more preferably 1 to 15 μm. By setting the average particle size to 50 μm or less, problems such as disturbance of the orientation of the anisotropic filler are less likely to occur even when used in combination with an anisotropic filler. Furthermore, by setting the average particle size to 0.1 μm or more, the specific surface area of the non-anisotropic filler does not become larger than necessary, and even when a large amount is blended, the viscosity of the mixed composition is less likely to increase, making it easier to pack the non-anisotropic filler at a high density. For example, the non-anisotropic filler may be, for example, at least two non-anisotropic fillers having different average particle sizes.
[0044] The average particle size of the non-anisotropic filler is preferably 0.1 to 200 μm, more preferably 0.5 to 100 μm, and even more preferably 1 to 70 μm. The average particle size of the non-anisotropic filler can be measured by observation with an electron microscope or the like. More specifically, for example, the particle sizes of 50 random non-anisotropic fillers can be measured using an electron microscope or optical microscope, and the average value (arithmetic mean value) can be used as the average particle size.
[0045] The content of the non-anisotropic filler is preferably 50 to 2500 parts by mass, more preferably 100 to 1500 parts by mass, and even more preferably 200 to 750 parts by mass, per 100 parts by mass of the total of the silicone resin and the ester-based phase-change material. By using a content of 50 parts by mass or more, the thermal conductivity of the thermal conductive sheet can be improved. On the other hand, by using a content of 1500 parts by mass or less, the non-anisotropic filler is appropriately dispersed in the matrix, thereby achieving the effect of increasing thermal conductivity according to the content. Furthermore, an unnecessary increase in the viscosity of the mixed composition can be prevented.
[0046] The mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler is not particularly limited, but is preferably 0.5 to 5, more preferably 1 to 3, and more preferably 1.1 to 2.5. By setting the mass ratio within the above range, the non-anisotropic filler is appropriately filled between the anisotropic fillers, forming efficient heat transfer paths, thereby further improving the thermal conductivity of the thermally conductive sheet.
[0047] (Additives) In the thermally conductive sheet, various additives may be further blended into the matrix to the extent that the functionality of the thermally conductive sheet is not impaired. Examples of additives include at least one selected from the group consisting of plasticizers, adhesives, flame retardants, antioxidants, colorants, and anti-settling agents. Furthermore, when curing a curable silicone composition as described above, a curing catalyst that accelerates curing may be blended as an additive. Examples of the curing catalyst include platinum-based catalysts. Furthermore, as described below, a compatible substance may be blended into the mixed composition. The compatible substance may volatilize during the process of producing the thermally conductive sheet and not remain in the thermally conductive sheet, or at least a portion of the blended compatible substance may remain.
[0048] (Thickness) The thickness of the thermally conductive sheet is not particularly limited and may be set appropriately depending on the shape and application of the electronic device in which the thermally conductive sheet is mounted, but is, for example, 0.05 to 3.0 mm, preferably 0.1 to 2.0 mm, and more preferably 0.15 to 1.0 mm.
[0049] (Contact Thermal Resistance Value) The thermal conductive sheet of the present invention has a contact thermal resistance value to nickel (hereinafter also simply referred to as "contact thermal resistance value") of 0.060 (K·cm 2 / W) or less, and 0.058 (K cm 2 / W) or less, and more preferably 0.045 (K cm 2 / W) or less, and more preferably 0.040 (K cm 2 When the contact thermal resistance is equal to or less than the upper limit, heat can be efficiently diffused. The lower the contact thermal resistance, the better, and the lower the contact thermal resistance is, and the better.2 / W) or more, but in practice, it is preferable to use a value of, for example, 0.010 (K cm 2 / W) or more, preferably 0.020 (K cm 2 / W) or more.
[0050] (Thermal Resistance Value) The thermal conductive sheet of the present invention has a thermal resistance value (hereinafter simply referred to as "thermal resistance value") of 0.160 (K cm) when compressed under a load of 40 psi. 2 / W) or less, and 0.120 (K cm 2 / W) or less, and more preferably 0.100 (K cm 2 / W) or less, and more preferably 0.080 (K cm 2 / W) or less. When the thermal resistance value is equal to or less than the upper limit, the thermal resistance of the thermal conductive sheet itself is small, and heat can be efficiently diffused. The lower the thermal resistance value, the better, and it is preferably 0 (K cm 2 / W) or more, but in practice, it is preferable to use a value of, for example, 0.030 (K cm 2 / W) or more, preferably 0.050 (K cm 2 It is preferable that the thermal resistance value is within the above range regardless of the thickness of the thermally conductive sheet. For example, when the thickness of the thermally conductive sheet is 0.05 to 0.5 mm, the thermal resistance value measured is 0.160 (K cm 2 / W) or less, and the thermal resistance measured when the thickness of the thermal conductive sheet is 0.5 mm is 0.160 (K cm 2 / W) or less. It is more preferable that the thermal resistance measured when the thickness of the thermal conductive sheet is 0.05 to 0.3 mm is 0.120 (K cm 2 / W) or less, and the thermal resistance measured when the thickness of the thermal conductive sheet is 0.05 to 0.2 mm is 0.100 (K cm 2 / W) or less. The above-mentioned contact thermal resistance value and thermal resistance value can be adjusted by the type and content of the ester-based phase-change material, the content of the silicone resin, etc., and specific methods for measuring these are as described in the Examples.
[0051] (E Hardness) The thermally conductive sheet of the present invention preferably has a Type E hardness (hereinafter also referred to as "E hardness") as defined in JIS K6253 of 10 to 80, more preferably 20 to 75, and even more preferably 30 to 70. When the E hardness is equal to or greater than the above lower limit, a certain degree of elasticity is imparted to the thermally conductive sheet even when it is extremely thin, and excellent shape retention is also easily achieved. On the other hand, when the E hardness is equal to or less than the above upper limit, a certain degree of flexibility is imparted to the thermally conductive sheet.
[0052] [Method for producing thermally conductive sheet] The thermally conductive sheet of the present invention can be produced, for example, by a production method including the following steps X and Y. Step X: A step of mixing at least a curable silicone composition, an ester-based phase-change material, a thermally conductive filler, and a compatible substance to obtain a mixed composition. Step Y: A step of heating and curing the mixed composition obtained in step X. Each step will be described in detail below.
[0053] (Step X) In step X, a compatible substance is mixed with the curable silicone composition, ester-based phase change material, and thermally conductive filler to obtain a mixed composition. The compatible substance is a substance that is compatible with or dissolves in the ester-based phase change material and the curable silicone composition. By using the compatible substance, the ester-based phase change material can be uniformly mixed into the curable silicone composition. Therefore, the ester-based phase change material is uniformly dispersed in the silicone resin obtained by curing the curable silicone composition. Generally, ester compounds have low compatibility with silicone resins due to the high polarity of the carbonyl group, and it can be difficult to use them with silicone. However, by using the ester-based phase change material together with the compatible substance, it becomes easier to obtain a mixed composition in which the ester-based phase change material is uniformly dispersed in the silicone resin.
[0054] In step X, the mixing method and mixing order are not particularly limited as long as the above components can be mixed to obtain a mixed composition, and the curable silicone composition, ester-based phase-change material, thermally conductive filler, compatible substance, and other components that are optionally added as needed may be mixed appropriately in any order to obtain a mixed composition. Also, as described above, the curable silicone composition consists of, for example, a base agent and a curing agent, but in such cases, the base agent, curing agent, ester-based phase-change material, thermally conductive filler, compatible substance, and other components that are optionally added as needed may be mixed in any order to obtain a mixed composition.
[0055] Furthermore, it is preferable that the ester-based phase-change material be dissolved in a compatible substance and then mixed with the curable silicone composition and other components. In this case, the mixture of the ester-based phase-change material and the compatible substance, the curable silicone composition (or the base and curing agent), the thermally conductive filler, and other components optionally added as needed may be mixed in any order to obtain a mixed composition. In this way, by dissolving the ester-based phase-change material in a compatible substance in step X, the ester-based phase-change material can be mixed more uniformly in the silicone resin, making it easier to prevent residual ester-based phase-change material from remaining undissolved.
[0056] When dissolving the ester-based phase-change material in the compatible substance, heating is preferred. Heating makes it easier to obtain a mixed composition in which the ester-based phase-change material is uniformly dispersed in the silicone resin. The heating temperature is preferably higher than the melting point of the compatible substance, and may be, for example, 60°C or higher to dissolve the ester-based phase-change material. Furthermore, when mixing the base material and the curing agent, the upper limit of the heating temperature can be set to a temperature at which the thermally conductive silicone does not substantially harden during the mixing process. On the other hand, when a compatible substance is mixed with each of the base material and the curing agent, the temperature can be set to a temperature at which the compatible substance is unlikely to volatilize. The heating temperature is not particularly limited, but may be, for example, 120°C or lower, preferably 80°C or lower, for dissolution. The silicone resin and ester-based phase-change material are mixed in a transparent or slightly opaque homogeneous mixture due to the presence of the compatible substance. On the other hand, when the compatible substance is not included, the mixture will be in a state in which the solid ester-based phase-change material is dispersed or a two-phase state in which the liquid ester-based phase-change material is separated.
[0057] (Compatible Substance) The compatible substance used in the present invention is preferably a substance that dissolves in the ester-based phase-change material and is compatible with the curable silicone composition. The compatible substance is preferably a substance that is liquid at room temperature (23°C) and 1 atmosphere. As described below, the compatible substance is preferably a component that volatilizes upon heating at approximately 50 to 180°C in step Y. The compatible substance volatilizes upon heating during curing, thereby increasing the content of the thermally conductive filler in the thermally conductive sheet. Furthermore, the inclusion of the compatible substance reduces the viscosity of the mixed composition. This makes it easier to increase the amount of thermally conductive filler incorporated, and further, facilitates orienting the anisotropic filler in a predetermined direction by magnetic field orientation, as described below. The compatible substance volatilizes upon heating after the start of curing, thereby curing the matrix, thereby maintaining the ester-based phase-change material dispersed in the matrix.
[0058] Examples of compatible substances include alkoxysilane compounds, hydrocarbon solvents, alkoxysiloxane compounds, and ester compounds that are liquid at 25°C. These compounds have high solubility or compatibility with ester-based phase-change materials and curable silicone compositions, and therefore can improve the dispersibility of the ester-based phase-change material in the curable silicone composition in the mixed composition. This makes it easier for the ester-based phase-change material to be properly dispersed in the thermally conductive sheet. The compatible substances may be used alone or in combination of two or more.
[0059] As the compatible substance, an alkoxysilane compound or a hydrocarbon solvent is preferred due to its ease of volatilization in step Y, with the use of an alkoxysilane compound being particularly preferred. The use of an alkoxysilane compound results in a good appearance without bubbles on the surface of the thermally conductive sheet obtained by curing. The alkoxysilane compound used as the compatible substance is a compound having a structure in which one to three of the four bonds possessed by a silicon atom (Si) are bonded to alkoxy groups, and the remaining bond is bonded to an organic substituent. The alkoxysilane compound, by having an alkoxy group and an organic substituent, can improve the dispersibility of the ester-based phase change material in the curable silicone composition. Examples of alkoxy groups possessed by alkoxysilane compounds include methoxy, ethoxy, protoxy, butoxy, pentoxy, and hexatoxy. The alkoxysilane compound may be contained in the curable silicone composition as a dimer.
[0060] Among alkoxysilane compounds, from the viewpoint of easy availability, alkoxysilane compounds having at least one of a methoxy group and an ethoxy group are preferred. From the viewpoint of compatibility and solubility with the curable silicone composition and the ester-based phase change material, the number of alkoxy groups in the alkoxysilane compound is preferably 2 or 3, and more preferably 3. Specifically, the alkoxysilane compound is preferably at least one selected from a trimethoxysilane compound, a triethoxysilane compound, a dimethoxysilane compound, and a diethoxysilane compound.
[0061] Examples of functional groups contained in the organic substituents of alkoxysilane compounds include acryloyl groups, alkyl groups, carboxy groups, vinyl groups, methacrylic groups, aromatic groups, amino groups, isocyanate groups, isocyanurate groups, epoxy groups, hydroxyl groups, and mercapto groups. When a platinum catalyst is used as a curing catalyst for the curable silicone composition, it is preferable to select and use an alkoxysilane compound that is less likely to affect the curing reaction of the organopolysiloxane. Specifically, when an addition reaction-type organopolysiloxane using a platinum catalyst is used, it is preferable that the organic substituents of the alkoxysilane compound do not contain amino groups, isocyanate groups, isocyanurate groups, hydroxyl groups, or mercapto groups.
[0062] From the viewpoint of enhancing the dispersibility of the ester-based phase-change material in the silicone resin, the alkoxysilane compound preferably includes an alkylalkoxysilane compound having an alkyl group bonded to the silicon atom, i.e., an alkoxysilane compound having an alkyl group as an organic substituent. Therefore, dialkyldialkoxysilane compounds and alkyltrialkoxysilane compounds are preferred, with alkyltrialkoxysilane compounds being particularly preferred. The number of carbon atoms in the alkyl group bonded to the silicon atom may be, for example, 1 to 16. Furthermore, in trialkoxysilane compounds such as trimethoxysilane compounds and triethoxysilane compounds, from the viewpoint of enhancing the dispersibility of the ester-based phase-change material, the number of carbon atoms in the alkyl group is preferably 6 or more, more preferably 8 or more, and preferably 12 or less, more preferably 10 or less. On the other hand, in dialkoxysilane compounds such as dimethoxysilane compounds and diethoxysilane compounds, from the viewpoint of enhancing the dispersibility of the ester-based phase-change material, the number of carbon atoms in the alkyl group may be 1 or more, and preferably 10 or less, more preferably 6 or less, even more preferably 4 or less.
[0063] Examples of alkyl group-containing alkoxysilane compounds include methyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, di-n-propyldimethoxysilane, di-n-propyldiethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, and n-decyltriethoxysilane. Among alkyl group-containing alkoxysilane compounds, n-decyltrimethoxysilane, dimethyldimethoxysilane, and n-octyltriethoxysilane are more preferred from the viewpoint of improving the dispersibility of the ester-based phase-change material, and n-decyltrimethoxysilane and n-octyltriethoxysilane are even more preferred from the viewpoint of solubility with the ester-based phase-change material.
[0064] The alkoxysiloxane compound used as the compatible material has two or more siloxane bonds and a structure in which an alkoxy group is bonded to at least one silicon atom. The alkoxysiloxane compound has a structure in which an organic substituent is bonded to at least one of the silicon atoms constituting the siloxane bond. The alkoxysiloxane compound can improve the dispersibility of the ester-based phase-change material by having an alkoxy group and an organic substituent. Examples of the alkoxy group and organic substituent possessed by the alkoxysiloxane compound include those exemplified in the description of the alkoxysilane compound above. From the viewpoint of improving the dispersibility of the ester-based phase-change material, it is preferable that the alkoxysiloxane compound have at least an alkyl group.
[0065] Examples of the alkoxysiloxane compound include methyl methoxy siloxane oligomer, methyl phenyl methoxy siloxane oligomer, methyl epoxy methoxy siloxane oligomer, methyl mercapto methoxy siloxane oligomer, and methyl acryloyl methoxy siloxane oligomer, etc. One or more types of alkoxy siloxane compounds can be used.
[0066] Examples of hydrocarbon solvents used as compatible substances include aromatic hydrocarbon solvents. Of these, aromatic hydrocarbon solvents are preferred from the standpoint of compatibility with the curable silicone composition. Examples of aromatic hydrocarbon solvents include aromatic hydrocarbon solvents with approximately 6 to 10 carbon atoms, such as toluene, xylene, mesitylene, ethylbenzene, propylbenzene, butylbenzene, and t-butylbenzene, with toluene and xylene being preferred.
[0067] The ester compound that is liquid at 25°C and used as a compatible substance may be either a monoester or a diester, but is preferably a monoester. The ester compound used as a compatible substance may be, for example, an ester of a fatty acid such as a saturated aliphatic acid with an alcohol such as an alkanol, and examples thereof include octyl laurate, 1-methylheptyl laurate, isopropyl myristate, 1-methylheptyl myristate, and isopropyl palmitate.
[0068] In the mixed composition, the content of the compatible substance is preferably 6 to 60 parts by mass per 100 parts by mass of the total of the curable silicone composition and the ester-based phase-change material. At 6 parts by mass or more, the uniformity of the mixing of the ester-based phase-change material with the curable silicone composition can be sufficiently enhanced. Furthermore, by setting the content to 60 parts by mass or less, an effect commensurate with the amount of compatible substance used can be obtained. From these viewpoints, the content of the compatible substance is more preferably 10 to 50 parts by mass, and even more preferably 15 to 45 parts by mass. In this case, if the ester-based phase-change material is mixed uniformly, the ester-based phase-change material is sufficiently dissolved, thereby preventing, for example, the solid ester-based phase-change material from becoming dispersed. Therefore, in the mixed composition, the remaining solid ester-based phase-change material is prevented from exhibiting filler properties and increasing the viscosity, making it easier to incorporate a larger amount of thermally conductive filler. Furthermore, from the viewpoint of improving the dispersibility of the ester-based phase-change material in the mixed composition, the content of the compatible substance is preferably greater than the content of the ester-based phase-change material. It is preferable that the compatible substance is partially or completely volatilized by the heating in step Y. Therefore, the compatible substance does not need to be contained in the thermally conductive sheet, but may be contained in the thermally conductive sheet in an amount less than the content in the mixed composition.
[0069] The detailed description of the components other than the compatible substance in the mixed composition (i.e., the curable silicone composition, the ester-based phase-change material, the thermally conductive filler, other additives, etc.) is as described above. The contents of the ester-based phase-change material and the thermally conductive filler in the mixed composition are also as described above. However, while the contents of each component are shown above as amounts based on a total of 100 parts by mass of the silicone resin and the ester-based phase-change material, in the mixed composition, the amounts are based on a total of 100 parts by mass of the curable silicone composition and the ester-based phase-change material.
[0070] (Step Y) Step Y is a step of curing the mixed composition by heating. The temperature at which the mixed composition is heated is not particularly limited as long as the curable silicone composition can be cured by heating. It is sufficient that the temperature is higher than room temperature (23°C), but it is preferably 50°C or higher. The heating temperature is also not particularly limited, but it is sufficient that the thermally conductive sheet and the mixed composition do not thermally deteriorate, and is, for example, 180°C or lower, preferably 150°C or lower. The mixed composition may be heated in one stage or in two or more stages. When heating in two or more stages, it is sufficient that the heating temperature is within the above range in at least one stage, but it is preferable that the heating temperature is within the above range in all stages. The total heating time is, for example, about 10 minutes to 14 hours. When heating in two or more stages, it is preferable that the mixed composition is partially cured in the first stage and then fully cured by heating in the second or subsequent stages.
[0071] In step Y, the mixed composition may be formed into a predetermined shape such as a block or a sheet, and then heated to harden. Furthermore, in step Y, if the mixed composition contains an anisotropic filler as the thermally conductive filler, the anisotropic filler may be oriented in one direction and then hardened by heating. The anisotropic filler can be oriented by a magnetic field orientation method or a flow orientation method, but magnetic field orientation is preferred.
[0072] In the magnetic field orientation method, the mixed composition is poured into a mold or the like and placed in a magnetic field, and the anisotropic filler is oriented along the magnetic field. The curable silicone composition is then cured to obtain an oriented molded body. The mixed composition is preferably cured under the heating conditions described above. The oriented molded body is preferably in the form of a block, but may also be in the form of a sheet. By making it in the form of a sheet, the oriented molded body can be used as a thermally conductive sheet as is without slicing. On the other hand, by making it in the form of a block, the orientation of the anisotropic filler is enhanced.
[0073] In the magnetic field orientation method, a release film may be placed inside the mold in the portion that comes into contact with the mixed composition. For example, a resin film with good releasability or a resin film whose one side has been treated with a release agent or the like is used as the release film. By using the release film, the oriented molded body can be easily released from the mold.
[0074] The viscosity of the mixed composition used in the magnetic field orientation method is preferably 10 to 300 Pa·s in order to achieve magnetic field orientation. By setting the viscosity at 10 Pa·s or higher, the thermally conductive filler is less likely to settle. Furthermore, by setting the viscosity at 300 Pa·s or less, the fluidity is improved, the anisotropic filler is properly oriented in the magnetic field, and problems such as excessive time required for orientation do not occur. The viscosity is measured using a rotational viscometer (Brookfield viscometer DV-E, spindle SC4-14) at 25°C and a rotation speed of 10 rpm. However, when using a thermally conductive filler that is less likely to settle or when combining with additives such as anti-settling agents, the viscosity of the mixed composition may be less than 10 Pa·s.
[0075] In the magnetic field orientation method, magnetic field line generating sources for applying magnetic field lines include superconducting magnets, permanent magnets, electromagnets, etc., but superconducting magnets are preferred because they can generate a magnetic field with a high magnetic flux density. The magnetic flux density of the magnetic field generated from these magnetic field line generating sources is preferably 1 to 30 T (tesla). If the magnetic flux density is 1 T or higher, it becomes possible to easily orient the above-mentioned anisotropic filler made of a carbon material, etc. Furthermore, if the magnetic flux density is 30 T or less, practical production becomes possible.
[0076] In the flow orientation method, a primary sheet is produced in which the anisotropic filler is oriented in the plane direction by applying a shear force to the mixed composition. More specifically, in the flow orientation method, the mixed composition prepared in step X is first flattened and stretched while applying a shear force to form a sheet (primary sheet). By applying a shear force, the anisotropic filler can be oriented in the shear direction. Examples of sheet-forming methods include applying the mixed composition to a substrate film using a coating applicator such as a bar coater or doctor blade, or by extrusion molding or nozzle discharge, and then drying, semi-curing, or fully curing the mixed composition as needed. The thickness of the primary sheet is preferably approximately 50 to 5,000 μm. In the primary sheet, the anisotropic filler is oriented in one direction along the plane direction of the sheet. The mixed composition used in the flow orientation method has a relatively high viscosity so that a shear force is applied when stretched into a sheet. Specifically, the viscosity of the mixed composition is preferably 3 to 500 Pa·s.
[0077] The primary sheet may be used as a thermally conductive sheet without being formed into a block, as described below. Alternatively, a laminated block (a block-shaped oriented molded product) may be formed by stacking multiple primary sheets so that they are oriented in the same direction, and then bonding the primary sheets together using a heat press or the like while curing them by heating as needed. To form a laminated block, at least one of the surfaces of the primary sheets to be stacked may be irradiated with vacuum ultraviolet light, and then the primary sheets may be stacked. By stacking the primary sheets via the surface irradiated with vacuum ultraviolet light, the primary sheets can be firmly bonded to each other. When irradiating with vacuum ultraviolet light, the mixed composition may be fully cured when preparing the primary sheet; curing by heating or the like is not necessary when stacking the primary sheets to form the laminated block. Even in the flow orientation method, the mixed composition may be cured under the heating conditions described above.
[0078] As described above, when forming a block-shaped oriented molded body, the obtained oriented molded body may be cut perpendicular to the orientation direction of the anisotropic filler by slicing or the like to form a sheet-shaped molded body. Slicing may be performed, for example, with a shear blade. By slicing or cutting the sheet-shaped molded body, the tips of the anisotropic filler are exposed from the matrix on each surface, which is the cut surface. The sheet-shaped molded body obtained by cutting may be used as a thermally conductive sheet as is, or may be further processed. For example, each surface, which is the cut surface, may be polished. Polishing the surface smoothes the surface of the thermally conductive sheet, making it easier to further reduce contact resistance. The surface may be polished using, for example, abrasive paper, abrasive film, abrasive cloth, abrasive belt, etc., and abrasive paper is preferably used.
[0079] The properties of the abrasive paper are preferably such that the average particle size (D50) of the abrasive grains contained therein is 0.1 to 100 μm, more preferably 1 to 60 μm. The grain size of the abrasive grains in the abrasive paper is preferably #120 to 20,000, more preferably #300 to 15,000, and more preferably #320 to 4,000.
[0080] The polishing method can be, for example, polishing the surface of the sheet-like molded body by continuously contacting abrasive paper in the same linear direction, or by polishing by reciprocating a fixed distance, by polishing by rotating in the same direction, or by polishing by contacting in various directions. The degree of polishing can be determined, for example, while observing the surface condition. For example, in the case of reciprocating polishing, 1 to 300 reciprocating cycles is preferred, 2 to 200 cycles is more preferred, and 3 to 80 cycles is even more preferred. The surface of the sheet-like molded body may be polished in two separate polishing steps. For example, after the first polishing using abrasive paper with a larger average particle size of abrasive grains, the second polishing using abrasive paper with a smaller average particle size of abrasive grains than that used in the first polishing may be performed.
[0081] [Laminate] The present invention also provides a laminate comprising the thermally conductive sheet described above and a release film laminated on at least one surface of the thermally conductive sheet. In the laminate, the release film can protect the surface of the thermally conductive sheet. Therefore, by providing the thermally conductive sheet to the user in the form of a laminate, it is possible to prevent the thermally conductive sheet from being scratched or damaged during transportation, etc. Furthermore, the release film is preferably peeled from the thermally conductive sheet before use. The release film may be laminated on only one side of the thermally conductive sheet, but to adequately protect the thermally conductive sheet, it is preferable to laminate it on both sides of the thermally conductive sheet. The release film can be any of the above-mentioned films, as appropriate. Specifically, for example, a resin film with good release properties or a resin film whose one side has been treated with a release agent or the like can be used. Release films other than these may also be used. For example, the release film may be attached to the thermally conductive sheet produced as described above, and then laminated to the thermally conductive sheet.
[0082] [Method of Use of Thermally Conductive Sheet] The thermally conductive sheet of the present invention is used inside electronic devices, etc. Specifically, the thermally conductive sheet is interposed between two components and used to conduct heat from one component to the other. Specifically, the thermally conductive sheet is interposed between a heat generating element and a heat dissipating element, thermally conducting the heat generated by the heat generating element to the heat dissipating element, and dissipating the heat from the heat dissipating element. Here, examples of the heat generating element include various electronic components used inside electronic devices, such as CPUs, power amplifiers, and power supplies. Examples of the heat dissipating element include heat sinks, heat pumps, heat spreaders, and metal housings for electronic devices. The thermally conductive sheet is preferably used with both surfaces in close contact with the heat generating element and the heat dissipating element, respectively, and compressed.
[0083] The thermally conductive sheet may be heated to a certain temperature or higher during use. When the thermally conductive sheet is heated during use, at least a portion of the ester-based phase-change material melts, making it easier to fill voids on the sheet surface and reducing contact thermal resistance. The thermally conductive sheet may be heated, for example, by the heating element described above. From a similar perspective, the thermally conductive sheet may be heated before use and then assembled between two components in a heated state. The heating temperature is not particularly limited, but is, for example, 40 to 130°C, preferably 45 to 100°C, and more preferably 50 to 90°C. Furthermore, the thermally conductive sheet is used by being placed between two components, and in this case, it is preferable that at least a portion of the component that the thermally conductive sheet comes into contact with is metal. Placing a metal in a position that contacts the thermally conductive sheet further reduces contact thermal resistance. Examples of metals include, but are not limited to, iron, aluminum, nickel, copper, gold, silver, titanium, and alloys containing at least one of these.
[0084] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0085] The thermally conductive sheets obtained in the present examples and comparative examples were evaluated by the following methods.
[0086] [E Hardness] The Type E hardness of the thermally conductive sheet was measured based on Japanese Industrial Standard JIS K 6253. Specifically, a 2 mm thick sample was cut out from the oriented molded body produced in each Example and Comparative Example, and six of the samples were stacked together and measured using a Type E durometer in an environment of 25°C.
[0087] [Thermal Resistance Value] The thermal resistance value was measured using a thermal resistance measuring instrument as shown in FIG. 1 by the following method. Specifically, for each sample, a test piece S measuring 30 mm × 30 mm was prepared for this test. Each test piece S was then attached to a copper block 22 with a measurement surface of 25.4 mm × 25.4 mm and sides covered with a heat insulating material 21, and sandwiched between upper copper blocks 23. A load of 40 psi (0.276 MPa) was applied by a load cell 26. Here, the lower copper block 22 was in contact with a heater 24. The upper copper block 23 was also covered with a heat insulating material 21 and connected to a heat sink 25 equipped with a fan. Next, the heater 24 was activated, and after 10 minutes when the temperature reached a substantially steady state, the temperature (θ j0 ), the temperature of the lower copper block 22 (θ j1 The heat resistance value of each sample was calculated from the following formula (1). The heat resistance value was adjusted so that the temperature of the thermal conductive sheet was 80°C. Heat resistance value = (θ j1 -θ j0 ) / Q Formula (1) In formula (1), θ j1 is the temperature of the lower copper block 22, θ j0 is the temperature of the upper copper block 23, and Q is the amount of heat generated. When measuring the amount of heat generated, the thickness of the test piece was also recorded.
[0088] [Contact Thermal Resistance Value] Test pieces S were sliced from the molded body blocks produced in each Example and Comparative Example to thicknesses of 0.2 mm, 0.3 mm, and 0.5 mm, and the thermal resistance and thickness at the time of measurement were measured using the method described above. Next, a graph was created with the thickness at the time of thermal resistance measurement on the horizontal axis and the thermal resistance value on the vertical axis, and an approximate line was obtained using the least squares method for the thermal resistance values at three different thicknesses. The value on the vertical axis of this approximate line when the thickness was 0 mm was taken as the contact thermal resistance value.
[0089] Example 1 Myristyl myristate (melting point: 46°C) as an ester-based phase-change material and n-decyltrimethoxysilane as a compatible substance were mixed at 23°C according to the blending amounts in Table 1, and the mixture was heated to 60°C to obtain a mixture in which the ester-based phase-change material was dissolved in the compatible substance. The obtained mixture was uniformly mixed with a silicone base (alkenyl group-containing organopolysiloxane), a silicone curing agent (hydrogenorganopolysiloxane), and a catalyst (platinum-based catalyst) as a curable silicone composition, and then a thermally conductive filler was mixed according to the blending amounts in Table 1 to obtain a mixed composition.
[0090] The thermally conductive fillers used were aluminum powder (spherical, average particle size 3 μm, aspect ratio 1-1.5, thermal conductivity 236 W / m·K) and aluminum oxide (polyhedral, average particle size 0.5 μm, aspect ratio 1, thermal conductivity 30 W / m·K) as non-anisotropic fillers. The anisotropic fillers used were flake graphite powder (average particle size 15 μm, aspect ratio 10, thermal conductivity 550 W / m·K) and graphitized carbon fiber 1 (average fiber length 80 μm, aspect ratio 8, thermal conductivity 1200 W / m·K). The melting point of the ester-based phase change material was measured by weighing 20 mg into an aluminum cell and then heating from 25°C to 90°C at a rate of 10°C / min using a Shimadzu DSC-60 under nitrogen flow.
[0091] Next, the mixed composition was poured into a mold set to a thickness sufficiently greater than that of the thermally conductive sheet, and an 8 T magnetic field was applied in the thickness direction to orient the anisotropic filler in the thickness direction. The curable silicone composition was then semi-cured by heating at 80°C for 8 hours, resulting in a block-shaped oriented molded product. Next, the block-shaped oriented molded product was sliced into sheets using a shear blade, resulting in a sheet-shaped molded product with the anisotropic filler exposed. The sheet-shaped molded product was then further heated at 150°C for 6 hours to fully cure the curable silicone composition. Note that the heating during curing volatilized some of the compatible substances.
[0092] Then, both surfaces of the sheet-like molded body were polished 50 times with coarse abrasive paper (grain size #800) with an average abrasive grain size (D50) of 20 μm, and then polished 10 times with coarse abrasive paper (grain size #4000) with an average abrasive grain size (D50) of 3 μm. Three types of thermally conductive sheets were prepared: one with a thickness of 0.2 mm, one with a thickness of 0.3 mm, and one with a thickness of 0.5 mm. For each thermally conductive sheet, the thermal resistance value measured under a load of 40 psi and the thickness at the time of measurement were measured as described above. The results are shown in Table 1.
[0093] Examples 2 to 4 Thermally conductive sheets were obtained in the same manner as in Example 1, except that the blending amounts of each component were changed to the amounts shown in Table 1.
[0094] [Example 5] A thermally conductive sheet was obtained in the same manner as in Example 1, except that the phase change material was changed to stearyl stearate (melting point: 59°C) and the amounts of each component were changed to those shown in Table 1.
[0095] [Example 6] A thermally conductive sheet was obtained in the same manner as in Example 1, except that the phase change material was changed to cetyl myristate (melting point: 56°C) and the amounts of each component were changed to those shown in Table 1.
[0096] [Example 7] A thermally conductive sheet was obtained in the same manner as in Example 1, except that the phase change material was changed to behenyl behenylate (melting point: 75°C) and the amounts of each component were changed to those shown in Table 1.
[0097] Comparative Example 1 The same procedure as in Example 1 was carried out except that no ester-based phase-change material was used, and graphitized carbon fiber 2 (average fiber length 100 μm, aspect ratio 10, thermal conductivity 1200 W / m·K) was further used as the anisotropic filler, and the components were mixed according to the formulation in Table 2 to obtain a mixed composition, from which a thermally conductive sheet was produced.
[0098] Comparative Example 2 The same procedure as in Example 1 was carried out except that side-chain crystalline polyalphaolefin (CPAO) (melting point: 40°C) was used instead of the ester-based phase-change material, and the amounts of each component were changed to those shown in Table 2.
[0099] Comparative Examples 3 and 4 were carried out in the same manner as in Example 1, except that paraffin (melting point: 48° C.) was used instead of the ester-based phase-change material and the amounts of each component were changed to those shown in Table 2.
[0100] Comparative Examples 5 and 6 were carried out in the same manner as in Example 1, except that distearyltetramethyldisiloxane (melting point: 45°C) was used instead of the ester-based phase-change material, and the amounts of each component were changed to those shown in Table 2.
[0101]
[0102]
[0103] As is clear from the above examples, thermally conductive sheets that satisfy the requirements of the present invention resulted in low contact thermal resistance. In contrast, the thermally conductive sheet produced in Comparative Example 1 did not contain an ester-based phase-change material, resulting in high contact thermal resistance. Furthermore, the thermally conductive sheets produced in Comparative Examples 2 to 6 contained non-ester-based phase-change materials, and these thermally conductive sheets also resulted in high contact thermal resistance.
[0104] 21 Heat insulating material 22 Lower copper block 23 Upper copper block 24 Heater 25 Heat sink 26 Load cell S Test piece θ j0 Temperature of the upper copper block θ j1 Temperature of the lower copper block
Claims
1. A thermally conductive sheet comprising a matrix containing a silicone resin and an ester-based phase change material, and a thermally conductive filler.
2. The thermally conductive sheet according to claim 1, wherein the melting point of the ester-based phase change material is greater than 25°C and less than or equal to 120°C.
3. The thermally conductive sheet according to claim 1 or 2, wherein the ester-based phase change material has a hydrocarbon chain having 14 to 44 carbon atoms.
4. A thermally conductive sheet according to claim 1 or 2, wherein the ester-based phase change material is an ester of a fatty acid and an alcohol, and at least one of the fatty acid and the alcohol has an alkyl group having 14 to 22 carbon atoms.
5. A thermally conductive sheet according to claim 1 or 2, wherein the content of the ester-based phase-change material is 1 to 20 parts by mass per 100 parts by mass of the silicone resin and the ester-based phase-change material combined.
6. The thermally conductive sheet according to claim 1 or 2, wherein the thermally conductive filler comprises an anisotropic filler.
7. The thermally conductive sheet according to claim 6, wherein the major axis of said anisotropic filler is oriented in the thickness direction of the thermally conductive sheet.
8. The thermally conductive sheet according to claim 1 or 2, wherein the thermally conductive sheet has a thickness of 0.05 to 3.0 mm.
9. The contact thermal resistance to nickel is 0.040 (K cm 2 The thermal conductive sheet according to claim 1 or 2, wherein the thermal conductivity is less than or equal to 1 / W.
10. The thermal resistance when compressed with a load of 40 psi is 0.160 (K cm 2 The thermal conductive sheet according to claim 1 or 2, wherein the thermal conductivity is less than or equal to 1 / W.
11. The thermally conductive sheet according to claim 1 or 2, wherein the ester-based phase change material comprises at least one selected from stearyl stearate, nonadecylate, cetyl myristate, myristyl myristate, and behenyl behenylate.
12. The thermally conductive sheet of claim 6, wherein the thermally conductive filler further comprises a non-anisotropic filler.
13. A laminate comprising the thermally conductive sheet according to claim 1 or 2 and a release film laminated on at least one surface of the thermally conductive sheet.
14. A method of using the thermally conductive sheet according to claim 1 or 2, wherein the thermally conductive sheet is interposed between two members and conducts heat from one member to the other member.
Citation Information
Patent Citations
LED street lamp
CN104019436A
Phase change heat transfer material
JP2001089756A
Tablet for heat sink, heat sink obtained from the same, and method for preparation of the same
JP2004182983A
Thermally conductive sheet and production method thereof
JP2021136454A
Cited By
Thermally conductive sheet
WO2026205586A1