Polycarbonate-based resin composition and molded article
Aromatic polycarbonate resin compositions with specific structural units and additives enhance scratch resistance and other properties, addressing the limitations of polycarbonate resins in surface hardness and environmental impact by integrating multiple performance improvements into the resin itself.
Patent Information
- Application Number
- PCT/JP2024/016335
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Polycarbonate resins exhibit low surface hardness and insufficient scratch resistance, which complicates manufacturing and increases environmental burden when surface coating is used to improve scratch resistance, and existing solutions do not adequately address both scratch resistance and other properties like weather resistance and flame retardance.
Aromatic polycarbonate resin compositions containing specific structural units, combined with ultraviolet absorbers, flame retardants, polystyrene resins, polyester resins, and inorganic fillers, enhance scratch resistance and other properties such as weather resistance, flame retardance, tensile properties, and chemical resistance without compromising appearance.
The aromatic polycarbonate resin compositions improve scratch resistance and other properties like weather resistance, flame retardance, and tensile properties, providing a balanced set of mechanical and chemical attributes without the need for additional surface coatings.
Smart Images

Figure JP2024016335_31102024_PF_FP_ABST
Abstract
Description
Polycarbonate resin composition and molded article
[0001] The present invention relates to a polycarbonate resin composition and a molded article.
[0002] Polycarbonate resins have excellent impact resistance, transparency, heat resistance, and self-extinguishing properties, and are widely used as engineering plastics in various fields, such as electrical and electronic equipment and automobiles. However, polycarbonate resins have low surface hardness and may have insufficient scratch resistance. Patent Document 1 discloses a polycarbonate copolymer having improved scratch resistance, which contains units derived from a hydroxy-terminated monocyclic, polycyclic, or fused cyclic compound having a (meth)acrylate group and carbonate units. Patent Document 2 discloses branched or crosslinked fire-resistant polycarbonate resins and intermediates thereof.
[0003] Korean Patent Publication No. 2016-0141268 Publication JP-A-2-219818
[0004] A known method for improving surface hardness is to coat the top layer of a structure made of a polycarbonate-based resin, but this requires a coating process, which complicates the manufacturing process and increases the environmental impact. Furthermore, the invention described in Patent Document 1 has insufficient surface hardness. Patent Document 2 does not describe any method for improving surface hardness. Thus, further investigation was needed to achieve both scratch resistance and other effects using a polycarbonate-based resin alone.
[0005] An object of the present invention is to provide a polycarbonate resin composition and a molded article thereof which have improved surface hardness and scratch resistance without impairing the appearance, and which also have improved weather resistance, flame retardancy, flowability and tensile properties, chemical resistance, and / or rigidity.
[0006] The present inventors have found that the above problems can be solved by an aromatic polycarbonate resin containing a specific structural unit. That is, the present invention encompasses the following 1 to 11. 1. A polycarbonate resin composition comprising an aromatic polycarbonate resin containing a structural unit represented by the following formula (II), and at least one member selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene resin, a polyester resin, and an inorganic filler.
[0007]
[0008] [In formula (II), R 11 and R 12 R each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. 13 represents a group selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an aryl group having 6 to 14 carbon atoms. 14 represents a saturated or unsaturated alicyclic group having 3 to 20 carbon atoms, or a saturated or unsaturated heterocyclic group having 3 to 20 members. c and d each independently represent an integer of 0 to 4. n represents an integer of 0 to 20. 2. R 14 3. The polycarbonate resin composition according to 1, wherein R represents a saturated or unsaturated alicyclic group having 3 to 12 carbon atoms or a saturated or unsaturated heterocyclic group having 3 to 12 members. 14is a cyclopentyl group or a cyclohexyl group. 4. The polycarbonate resin composition according to any one of 1 to 3, wherein n is an integer of 0 to 4. 5. The polycarbonate resin composition according to any one of 1 to 4, wherein the ultraviolet absorber comprises at least one selected from the group consisting of benzotriazole-based ultraviolet absorbers, benzoxazinone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, malonic acid ester-based ultraviolet absorbers, oxalyl alanide-based ultraviolet absorbers, triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers. 6. The polycarbonate resin composition according to any one of 1 to 4, wherein the flame retardant comprises at least one selected from the group consisting of phosphorus-based flame retardants and metal salt-based flame retardants. 7. 7. The polycarbonate-based resin composition according to any one of 1 to 4, wherein the polystyrene-based resin comprises at least one selected from the group consisting of high-impact polystyrene resin, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-styrene copolymer, methyl methacrylate-butadiene-styrene copolymer, acrylonitrile-methyl acrylate-styrene copolymer, and acrylonitrile-(ethylene / propylene / diene copolymer)-styrene copolymer. 8. The polycarbonate-based resin composition according to any one of 1 to 4, wherein the polyester-based resin comprises at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate. 9. The polycarbonate-based resin composition according to any one of 1 to 4, wherein the inorganic filler is a glass filler. 10. The polycarbonate-based resin composition according to any one of 1 to 9, further comprising a repeating unit represented by the following formula (I):
[0009]
[0010] [In formula (I), R 1 and R 2each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, -S-, -SO-, -SO 2 represents —, —O—, or —CO—, and a and b each independently represent an integer of 0 to 4. 11. A molded article made from the polycarbonate resin composition according to any one of 1 to 10.
[0011] According to the present invention, it is possible to provide a polycarbonate resin composition and a molded article having improved scratch resistance and improved at least one of weather resistance, flame retardancy, flowability and tensile properties, chemical resistance, and rigidity.
[0012] The polycarbonate resin composition and molded article of the present invention will be described in detail below. In this specification, any definition that is considered preferable can be adopted at will, and a combination of preferable definitions can be considered more preferable. In this specification, the expression "XX to YY" means "XX or more and YY or less."
[0013] 1. Aromatic Polycarbonate Resin The polycarbonate resin composition of the present invention contains an aromatic polycarbonate resin containing a structural unit represented by the following formula (II):
[0014]
[0015] [In formula (II), R 11 and R 12R each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. 13 represents a group selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an aryl group having 6 to 14 carbon atoms. 14 represents a saturated or unsaturated alicyclic group having 3 to 20 carbon atoms or a saturated or unsaturated heterocyclic group having 3 to 20 members. c and d each independently represent an integer of 0 to 4. n represents an integer of 0 to 20.]
[0016] In the above formula (II), R 11 and R 12 The halogen atoms independently represented by R include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 11 and R 12 Examples of alkyl groups that R each independently represent include methyl, ethyl, n-propyl, isopropyl, various butyl groups (the term "various" refers to both linear and branched groups, and the same applies hereinafter), various pentyl groups, and various hexyl groups. 11 and R 12 The alkoxy groups each independently represent include those in which the alkyl group moiety is the above-mentioned alkyl group. 11 and R 12 Examples of the cycloalkyl group that each independently represents include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group. 11 and R 12The cycloalkyl group represented by each independently includes a case where the cycloalkyl group moiety is the above-mentioned cycloalkyl group. 11 and R 12 Examples of the alkenyl group that each independently represents include an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, and a hexenyl group. 11 and R 12 Examples of the aryl group that each independently represents include a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group. 11 and R 12 The aryloxy groups each independently represent include those in which the aryl group moiety is the above-mentioned aryl group. 11 and R 12 Examples of the aralkyl group that each independently represents include a phenylmethyl group and a phenylethyl group. 11 and R 12 The aralkyloxy groups represented by each independently include those in which the aralkyl group moiety is the above-mentioned aralkyl group.
[0017] In the above formula (II), R 13 Examples of the alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, various butyl groups, and various pentyl groups. 13 Examples of the cycloalkyl group represented by R include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group. 13 The cycloalkoxy group represented by R is a group in which the cycloalkyl group moiety is the above-mentioned cycloalkyl group. 13 Examples of the alkenyl group represented by R include an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, and a hexenyl group. 13 Examples of the aryl group represented by the formula (I) include a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group.
[0018] In the above formula (II), R 14The saturated or unsaturated alicyclic group represented by R has 3 to 20 carbon atoms, preferably 3 to 12 carbon atoms, and more preferably 4 to 8 carbon atoms. Specific examples thereof include cycloalkyl groups, which are saturated alicyclic groups such as cyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, adamantyl group, and nobornyl group, and cycloalkenyl groups, which are unsaturated alicyclic groups such as cyclopropenyl group, cyclobutenyl group, cyclopentenyl group, cyclohexenyl group, and cycloheptenyl group. Note that unsaturated alicyclic groups do not include aromatic groups. R 14 The heterocyclic group represented by the formula (I) has 3 to 20 ring-membering atoms, preferably 3 to 12 carbon atoms, and more preferably 3 to 8 carbon atoms. The heterocyclic group is a cyclic group containing at least one heteroatom, for example, 1, 2, or 3, among the ring-forming atoms. Specific examples of the heteroatom include a nitrogen atom, an oxygen atom, a sulfur atom, a silicon atom, a phosphorus atom, and a boron atom. Examples of the heterocyclic group include a pyridinyl group, a pyrazinyl group, a pyrimidinyl group, a pyridazinyl group, a triazinyl group, an indolinyl group, a quinolinyl group, an acridinyl group, a pyrrolidinyl group, a dioxanyl group, a piperidinyl group, an oxiranyl group (an epoxy group), an oxetanyl group, a morpholidinyl group, a piperazinyl group, a carbazolyl group, a furanyl group, a thiophenyl group, an oxazolyl group, an oxadiazolyl group, a benzoxazolyl group, a thiazolyl group, a thiadiazolyl group, a benzothiazolyl group, a triazolyl group, an imidazolyl group, a benzimidazolyl group, and a puranyl group. 14 represents preferably a saturated or unsaturated alicyclic group having 3 to 12 carbon atoms or a saturated or unsaturated heterocyclic group having 3 to 12 members, more preferably a cycloalkyl group having 3 to 8 carbon atoms, and even more preferably a cyclopentyl group or a cyclohexyl group.
[0019] c and d each independently represent an integer of 0 to 4, preferably an integer of 0 to 2, and more preferably 0 or 1.
[0020] n represents an integer of 0 to 20, preferably an integer of 0 to 10, more preferably an integer of 0 to 4, even more preferably 0, 1, 2, 3, or 4, and still more preferably 2. In another embodiment, n is preferably an integer of 1 to 10, more preferably an integer of 1 to 4.
[0021] In a preferred embodiment of the formula (II), from the viewpoint of improving scratch resistance, R 14 represents a cyclopentyl group or a cyclohexyl group, n is preferably 0 to 2, more preferably 2. Furthermore, c and d are each preferably 0, and R 13 is preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group. In the aromatic polycarbonate resin, the structural unit represented by the above formula (II) may be of one type alone or a combination of two or more types.
[0022] The aromatic polycarbonate resin may further contain a repeating unit represented by the following formula (I).
[0023]
[0024] [In formula (I), R 1 and R 2 each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, -S-, -SO-, -SO 2 represents —, —O—, or —CO—; and a and b each independently represent an integer of 0 to 4.]
[0025] In the above formula (I), R 1 and R 2The halogen atoms independently represented by R include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 1 and R 2 Examples of alkyl groups that R each independently represent include methyl, ethyl, n-propyl, isopropyl, various butyl groups, various pentyl groups, and various hexyl groups. 1 and R 2 The alkoxy groups each independently represent include those in which the alkyl group moiety is the above-mentioned alkyl group. 1 and R 2 Examples of the cycloalkyl group that each independently represents include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group. 1 and R 2 The cycloalkyl group represented by each independently includes a case where the cycloalkyl group moiety is the above-mentioned cycloalkyl group. 1 and R 2 Examples of the alkenyl group that each independently represents include an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, and a hexenyl group. 1 and R 2 Examples of the aryl group that each independently represents include a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group. 1 and R 2 The aryloxy groups each independently represent include those in which the aryl group moiety is the above-mentioned aryl group. 1 and R 2 Examples of the aralkyl group that each independently represents include a phenylmethyl group and a phenylethyl group. 1 and R 2 The aralkyloxy groups represented by each independently include those in which the aralkyl group moiety is the above-mentioned aralkyl group.
[0026] The alkylene group represented by X has 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms. Specific examples thereof include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, and a hexamethylene group. Examples of the alkylidene group represented by X include an ethylidene group and an isopropylidene group. The cycloalkylene group represented by X has 5 to 15 carbon atoms, preferably 5 to 10 carbon atoms. Specific examples thereof include a cyclopentanediyl group, a cyclohexanediyl group, and a cyclooctanediyl group. Examples of the arylene group represented by X include a phenylene group, a naphthylene group, a biphenylene group, and a tetraphenyl group. The cycloalkylidene group represented by X has 5 to 15 carbon atoms, preferably 5 to 10 carbon atoms. Specific examples thereof include a cyclohexylidene group, a 3,5,5-trimethylcyclohexylidene group, and a 2-adamantylidene group. Examples of the aryl moiety of the aralkyl group (aryl alkylene group) represented by X include aryl groups having 6 to 14 ring carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group. Of the above, X is preferably an isopropylidene group, a cyclohexylidene group, or a 3,5,5-trimethylcyclohexylidene group, from the viewpoint of improving the scratch resistance of molded articles of aromatic polycarbonate resins.
[0027] a and b each independently represent an integer of 0 to 4, preferably 0 to 2, and more preferably 0 or 1. Among these, a case where a and b are 0 and X represents a single bond or an alkylene group having 1 to 8 carbon atoms, or a and b are 0 and X represents an alkylidene group, particularly an isopropylidene group, is preferred. In another embodiment, a and b are 1 and X represents a single bond or an alkylene group having 1 to 8 carbon atoms, or a and b are 1 and X represents an alkylidene group, particularly an isopropylidene group, is preferred from the viewpoint of improving the scratch resistance of molded articles of aromatic polycarbonate resins.
[0028] Specific examples of the repeating unit represented by the above formula (I) include repeating units represented by the following general formulae (Ii) to (I-iv).
[0029]
[0030] In the aromatic polycarbonate resin, the repeating unit represented by formula (I) may be a single type or a combination of two or more types. Specific examples include an embodiment consisting solely of a repeating unit represented by general formula (Ii); and an embodiment consisting of a combination of a repeating unit represented by general formula (Ii) with one or more repeating units selected from the group consisting of repeating units represented by general formulas (I-ii) to (I-iv). Such aromatic polycarbonate resins can be easily produced by an interfacial polymerization method, described below, in which a polycarbonate oligomer is produced in advance.
[0031] When the aromatic polycarbonate resin contains a repeating unit represented by formula (I), the aromatic polycarbonate resin is an aromatic polycarbonate copolymer containing a repeating unit represented by formula (I) and a structural unit represented by formula (II).
[0032] In the aromatic polycarbonate resin, the molar ratio ((I):(II)) of the repeating unit represented by formula (I) to the structural unit represented by formula (II) is preferably 0:100 to 99.5:0.5, more preferably 0.5:99.5 to 99.5:0.5, even more preferably 0.5:99.5 to 99:1, still more preferably 0.5:99.5 to 94:6, and most preferably 0.5:99.5 to 92:8. In particular, the molar ratio ((I):(II)) of the repeating unit represented by formula (I) to the structural unit represented by formula (II) is preferably 60:40 to 99.5:0.5, more preferably 70:30 to 99:1, and even more preferably 80:20 to 98:2. The molar ratio of the repeating unit represented by the formula (I) to the structural unit represented by the formula (II) in the aromatic polycarbonate resin is calculated by nuclear magnetic resonance (NMR) measurement. 1 H NMR measurement is carried out, and the value is calculated from the integrated values of the peak derived from the repeating unit represented by formula (I) above and the peak derived from the structural unit represented by formula (II) above.
[0033] The aromatic polycarbonate resin of the present invention may contain structural units other than the repeating unit represented by formula (I) and the structural unit represented by formula (II), such as a terminal structure derived from a terminal terminator described below and a structural unit containing a silicon atom.
[0034] From the viewpoints of mechanical properties and moldability, the viscosity average molecular weight of the aromatic polycarbonate resin is preferably 10,000 to 100,000, more preferably 10,000 to 80,000, even more preferably 15,000 to 30,000, and even more preferably 17,000 to 25,000. In the present invention, the viscosity average molecular weight (Mv) is calculated by measuring the viscosity of a methylene chloride solution (concentration: g / L) at 20°C using an Ubbelohde viscometer, determining the intrinsic viscosity [η] from this, and then calculating the viscosity average molecular weight (Mv) using the following Schnell formula: [η]=1.23×10 -5 Mv 0.83
[0035] The aromatic polycarbonate resin of the present invention improves the scratch resistance of molded articles thereof. The scratch resistance can be evaluated by scratch hardness (pencil method). The aromatic polycarbonate resin preferably has a scratch hardness (pencil method) of HB or higher, as evaluated in accordance with JIS K5600-5-4:1999.
[0036] 2. Method for Producing Aromatic Polycarbonate Resin (Dihydric Phenol Compound) The aromatic polycarbonate resin can be preferably produced using a dihydric phenol compound (a) represented by the following formula (ii). The structural unit represented by formula (II) of the aromatic polycarbonate resin is derived from the dihydric phenol compound (a). Therefore, the present invention also provides use of the dihydric phenol compound (a) represented by formula (ii) for producing an aromatic polycarbonate resin.
[0037]
[0038] [In formula (ii), R 11 , R 12 , R 13 , R 14, c, d and n are as defined above, and the preferred values are also the same.]
[0039] Preferred specific examples of the dihydric phenol compound (a) include cyclohexyl diphenolate represented by the following formula (ii-1), cyclopentyl diphenolate represented by the following formula (ii-2), and cyclohexyl 2,2-bis(4-hydroxyphenyl)propanoate represented by the following formula (ii-3).
[0040]
[0041] The dihydric phenol compound (a) can be produced, for example, by reacting a carboxylic acid compound (ax) represented by the following formula (ii-x) with an alcohol compound (ay) represented by the following formula (ii-y) in the presence of an acid catalyst, if necessary.
[0042]
[0043] [In formula (ii-x), R 11 , R 12 , R 13 , c, d and n are as defined above, and the preferred values are also the same.]
[0044]
[0045] [In formula (ii-y), R 14 are as defined above, and the preferred definitions are also the same.]
[0046] (Method for producing aromatic polycarbonate resin) The aromatic polycarbonate resin can be produced by a known method for producing polycarbonate resins, as long as the dihydric phenol compound (a) is represented by the formula (ii) above. Examples of methods for producing polycarbonate resins include: (i) an interfacial polymerization method (phosgene method) in which a dihydric phenol compound and phosgene are reacted in the presence of an organic solvent inert to the reaction or an aqueous alkali solution, followed by polymerization by adding a polymerization catalyst such as a tertiary amine or a quaternary ammonium salt; (ii) a melt polymerization method (ester exchange method) in which a dihydric phenol compound and a carbonate diester are subjected to an ester exchange reaction in a molten state without using a solvent, by adding a basic catalyst; and (iii) a pyridine method in which a dihydric phenol compound is dissolved in pyridine or a mixed solution of pyridine and an inert solvent, and phosgene is introduced to directly produce the polycarbonate resin. During the above reaction, a molecular weight modifier (terminal capping agent), a branching agent, etc. may be used as needed.
[0047] Among these, the following production method is preferred: a production method for an aromatic polycarbonate resin, comprising a step of interfacially polycondensing a dihydric phenol compound and a polycarbonate oligomer in the presence of a water-insoluble organic solvent and an aqueous alkaline compound solution, wherein the dihydric phenol compound comprises a dihydric phenol compound (a) represented by the above formula (ii).
[0048] Specifically, in the case of the interfacial polymerization method, the aromatic polycarbonate resin can be produced by dissolving a pre-produced polycarbonate oligomer (described below) in a water-insoluble organic solvent (e.g., methylene chloride), adding an alkaline compound aqueous solution of a dihydric phenol compound (e.g., sodium hydroxide aqueous solution), and using a tertiary amine (e.g., triethylamine) or a quaternary ammonium salt (e.g., trimethylbenzylammonium chloride) as a polymerization catalyst, and optionally in the presence of a terminal terminator (a monohydric phenol such as p-tert-butylphenol). In addition, in the case of the interfacial polymerization method, the aromatic polycarbonate resin can be produced by copolymerizing a dihydric phenol with phosgene, a carbonate ester, or a chloroformate.
[0049] Polycarbonate oligomers can be produced by reacting a dihydric phenol compound with a carbonate precursor such as phosgene or triphosgene in an organic solvent such as methylene chloride, chlorobenzene, chloroform, etc. When producing a polycarbonate oligomer using the transesterification method, it can also be produced by reacting a dihydric phenol compound with a carbonate precursor such as diphenyl carbonate.
[0050] The dihydric phenol includes a dihydric phenol compound (a) represented by the following formula (ii) from which the structural unit represented by the above formula (II) is derived. The dihydric phenol preferably further includes a dihydric phenol compound (b) represented by the following formula (i) from which the repeating unit represented by the above formula (I) is derived.
[0051]
[0052] [In formula (ii), R 11 , R 12 , R 13 , R 14 , c, d and n are as defined above, and the preferred values are also the same.]
[0053]
[0054] [In formula (i), R 1 , R 2 , X, a, and b are as defined above, and the preferred values are also the same.]
[0055] Examples of the dihydric phenol compound (b) include bis(hydroxyphenyl)alkane compounds such as 2,2-bis(4-hydroxyphenyl)propane [bisphenol A (BPA)], bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, and 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane; 4,4'-dihydroxydiphenyl; bis(4-hydroxyphenyl)cycloalkane; bis(4-hydroxyphenyl)oxide; bis(4-hydroxyphenyl)sulfide; bis(4-hydroxyphenyl)sulfone; bis(4-hydroxyphenyl)sulfoxide; and bis(4-hydroxyphenyl)ketone. These dihydric phenol compounds may be used alone or in combination of two or more. Among these, bis(hydroxyphenyl)alkane dihydric phenols are preferred, and bisphenol A is more preferred.
[0056] In a preferred production method, the dihydric phenol compound (b) alone can be used as the dihydric phenol compound for producing the polycarbonate oligomer. In this case, the dihydric phenol compound (a) and the dihydric phenol compound (b) are used in combination, or the dihydric phenol compound (a) alone is used in the interfacial polycondensation reaction step.
[0057] A terminal terminator (molecular weight regulator) can be used to adjust the molecular weight of the resulting aromatic polycarbonate resin. Examples of terminal terminators include monohydric phenols such as phenol, p-cresol, p-tert-butylphenol, p-tert-octylphenol, p-cumylphenol, p-nonylphenol, m-pentadecylphenol, and p-tert-amylphenol. These monohydric phenols may be used alone or in combination of two or more.
[0058] 3. Polycarbonate Resin Composition The polycarbonate resin composition of the present invention contains the above-described aromatic polycarbonate resin and at least one selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene resin, a polyester resin, and an inorganic filler.
[0059] (Ultraviolet Absorber) When the polycarbonate resin composition of the present invention contains the aromatic polycarbonate resin and an ultraviolet absorber, the polycarbonate resin composition and molded articles thereof exhibit the effects of improved scratch resistance and improved weather resistance.
[0060] When the polycarbonate-based resin composition contains an ultraviolet absorber, the ultraviolet absorber is preferably contained in an amount of 0.01 to 3.0 parts by mass per 100 parts by mass of the aromatic polycarbonate-based resin. When the content of the ultraviolet absorber is 0.01 part by mass or more, the weather resistance of the resulting molded article can be further improved. When the content of the ultraviolet absorber is 3.0 parts by mass or less, adhesion to the mold during molding of the resin composition can be further suppressed. In the polycarbonate-based resin composition, the content of the ultraviolet absorber is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, even more preferably 0.15 parts by mass or more, even more preferably 0.20 parts by mass or more, and even more preferably 0.25 parts by mass or more, per 100 parts by mass of the aromatic polycarbonate-based resin, from the viewpoint of further improving weather resistance. However, from the viewpoint of further suppressing adhesion to the mold during molding of the resin composition, the content is preferably 2.0 parts by mass or less, more preferably 1.0 part by mass or less, even more preferably 0.50 parts by mass or less, and even more preferably 0.35 parts by mass or less. The content of the ultraviolet absorber in the polycarbonate resin composition is preferably 0.05 to 2.0 parts by mass, more preferably 0.10 to 1.0 part by mass, even more preferably 0.15 to 0.50 parts by mass, even more preferably 0.20 to 0.35 parts by mass, and still more preferably 0.25 to 0.35 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin. The polycarbonate resin composition according to the present invention can contain one or more ultraviolet absorbers.
[0061] Examples of ultraviolet absorbers include at least one selected from the group consisting of benzotriazole-based ultraviolet absorbers, benzoxazinone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, malonic acid ester-based ultraviolet absorbers, oxalyl alanide-based ultraviolet absorbers, triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers. These may be used alone or in combination of two or more. From the viewpoint of weather resistance, the ultraviolet absorber preferably includes at least one selected from the group consisting of benzotriazole-based ultraviolet absorbers and benzoxazinone-based ultraviolet absorbers, more preferably at least one selected from the group consisting of benzotriazole-based ultraviolet absorbers and benzoxazinone-based ultraviolet absorbers, and even more preferably a benzotriazole-based ultraviolet absorber.
[0062] Examples of benzotriazole-based ultraviolet absorbers include 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t tert-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-[2-hydroxy-3-(3,4,5,6-tetra-hydrophthalimidomethyl)-5-methylphenyl]benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], methyl-3-[3-tert-butyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate-polyethylene glycol (molecular weight approximately 300) condensate, and the like. Among these, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, or 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] is preferred, and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] is more preferred. These can be used alone or in combination of two or more.
[0063] The benzoxazinone compound may be, for example, a compound represented by the following general formula (1).
[0064] [In the formula, R 21R represents a residue obtained by removing s hydrogen atoms from a hydrocarbon compound having one or two aromatic rings in the molecule. 22 represents hydrogen, a halogen group, a nitro group, an alkyl group having 1 to 8 carbon atoms, an alkoxyl group having 1 to 8 carbon atoms, or an alkenyloxy group having 2 to 8 carbon atoms. s represents an integer of 2 or 3, and t represents an integer of 1 to 4.]
[0065] In general formula (1), R 21 R is a residue obtained by removing s hydrogen atoms from a hydrocarbon compound having one or two aromatic rings in the molecule, and examples of R include arylene groups such as a phenylene group, a biphenylene group, and a naphthylene group. 22 In the formula (I), examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, a propyl group, and a butyl group; examples of the alkoxy group having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group; and examples of the alkenyloxy group having 2 to 8 carbon atoms include an allyloxy group, a 2-propenyloxy group, a 2-butenyloxy group, and a 2-methyl-3-propenyloxy group.
[0066] Among the compounds represented by the general formula (1), 2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) [p-phenylenebis(1,3-benzoxazin-4-one)] is preferred. 2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) is a compound represented by the following formula:
[0067]
[0068] Examples of salicylate-based UV absorbers include phenyl salicylate, p-tert-butylphenyl salilethate, and p-octylphenyl salilethate. Examples of malonic acid ester-based UV absorbers include benzylidenebisdiethylmalonate, 4-methoxyphenylmethylenedimethylester, and tetraethyl-2,2'-(1,4-phenylenedimethylidene)bismalonate. Examples of oxalyl alanide-based UV absorbers include oxalyl alanide compounds having a hydrocarbon group having 1 to 12 carbon atoms. Examples of triazine-based UV absorbers include 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-s-triazine.
[0069] The total content of the aromatic polycarbonate resin and the ultraviolet absorber in the polycarbonate resin composition according to the present invention is, from the viewpoint of further improving the balance between tensile properties and weather resistance, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, when the entire polycarbonate resin composition is taken as 100% by mass. The upper limit of the total content of the aromatic polycarbonate resin and the ultraviolet absorber is not particularly limited, but from the viewpoint of obtaining a resin composition having desired properties, it is, for example, 100% by mass or less.
[0070] (Flame retardant) When the polycarbonate resin composition of the present invention contains the aromatic polycarbonate resin and a flame retardant, the polycarbonate resin composition and molded articles thereof exhibit the effects of improving scratch resistance and flame retardancy. The polycarbonate resin composition of the present invention can contain one or more flame retardants.
[0071] Examples of the flame retardant include at least one selected from the group consisting of phosphorus-based flame retardants, halogen-based flame retardants, and metal salt-based flame retardants. From the viewpoint of further improving flame retardancy, at least one selected from the group consisting of phosphorus-based flame retardants and metal salt-based flame retardants is preferred.
[0072] Examples of phosphorus-based flame retardants include red phosphorus and phosphate ester-based flame retardants. Phosphate ester-based flame retardants are preferably halogen-free, and examples include phosphate ester monomers, oligomers, polymers, and mixtures thereof. Examples include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, tri(2-ethylhexyl)phosphate, diisopropylphenyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, trinaphthyl phosphate, bisphenol A bisphosphate, hydroquinone bisphosphate, resorcinol bisphosphate, resorcinol-diphenyl phosphate, trioxybenzene triphosphate, and the like, as well as substitution products and condensates thereof. Among these, condensed phosphate ester-based flame retardants are preferred.
[0073] Commercially available phosphate ester compounds that can be used as phosphate ester flame retardants include, for example, TPP (triphenyl phosphate), TXP (trixylenyl phosphate), CR733S (resorcinol bis(diphenyl phosphate)), CR741 (bisphenol A bis(diphenyl phosphate)), PX200 (1,3-phenylene-tetrakis(2,6-dimethylphenyl)phosphate), PX201L (1,4-phenylene-tetrakis(2,6-dimethylphenyl)phosphate), and PX202 (4,4'-biphenylene-tetrakis(2,6-dimethylphenyl)phosphate), all manufactured by Daihachi Chemical Industry Co., Ltd. The phosphate ester flame retardants are obtained by reacting dihydric phenols and monohydric phenols represented by Ar·OH with phosphorus oxychloride. These phosphate ester flame retardants may be used alone or in combination of two or more. As the phosphate ester flame retardant, 1,3-phenylene-tetrakis(2,6-dimethylphenyl)phosphate is preferred.
[0074] When the polycarbonate resin composition according to the present invention contains a phosphorus-based flame retardant as a flame retardant, the content of the flame retardant is preferably 1.0 part by mass or more, more preferably 2.0 parts by mass or more, even more preferably 3.0 parts by mass or more, even more preferably 5.0 parts by mass or more, and still more preferably 7.0 parts by mass or more, relative to 100 parts by mass of the aromatic polycarbonate resin, from the viewpoint of further improving flame retardancy; and from the viewpoint of further suppressing adhesion to the mold during molding of the resin composition and a decrease in the heat resistance of the molded product, and from the viewpoint of improving impact resistance and flowability, the content of the flame retardant is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and still more preferably 12 parts by mass or less. Furthermore, when the polycarbonate resin composition according to the present invention contains a phosphorus-based flame retardant as a flame retardant, the content of the flame retardant is preferably 1.0 to 40 parts by mass, more preferably 2.0 to 30 parts by mass, even more preferably 3.0 to 20 parts by mass, even more preferably 5.0 to 15 parts by mass, and still more preferably 7.0 to 12 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin.
[0075] Examples of halogen-based flame retardants include tetrabromobisphenol A (TBA), halogenated polycarbonate, copolymers of halogenated polycarbonate, oligomers thereof (TBA carbonate oligomer), decabromodiphenyl ether, TBA epoxy oligomer, halogenated polystyrene, and halogenated polyolefin. The halogen-based flame retardants can be used alone or in combination of two or more.
[0076] Examples of metal salt flame retardants include organic alkali metal salts and organic alkaline earth metal salts.The metal salt flame retardant preferably includes at least one selected from organic alkali metal salts and organic alkaline earth metal salts, and more preferably at least one selected from organic alkali metal salts and organic alkaline earth metal salts.The organic sulfonate salts of the alkali metal or alkaline earth metal (hereinafter, both may be collectively referred to as "alkali (earth) metal") include metal salts of fluorine-substituted alkylsulfonic acid, such as metal salts of perfluoroalkanesulfonic acid and alkali metal or alkaline earth metal, and metal salts of aromatic sulfonic acid and alkali metal or alkaline earth metal.
[0077] Examples of alkali metals include lithium, sodium, potassium, rubidium, and cesium. Examples of alkaline earth metals include beryllium, magnesium, calcium, strontium, and barium. Alkali metals are more preferred. Among these alkali metals, potassium and sodium are preferred, with potassium being more preferred, from the viewpoints of flame retardancy and thermal stability. Potassium salts can also be used in combination with alkali metal sulfonates made from other alkali metals.
[0078] Examples of alkali metal perfluoroalkanesulfonates include potassium perfluorobutanesulfonate, potassium trifluoromethanesulfonate, potassium perfluorohexanesulfonate, potassium perfluorooctane sulfonate, sodium pentafluoroethanesulfonate, sodium perfluorobutanesulfonate, sodium perfluorooctane sulfonate, lithium trifluoromethanesulfonate, lithium perfluorobutanesulfonate, lithium perfluoroheptanesulfonate, cesium trifluoromethanesulfonate, cesium perfluorobutanesulfonate, cesium perfluorooctane sulfonate, cesium perfluorohexanesulfonate, rubidium perfluorobutanesulfonate, and rubidium perfluorohexanesulfonate, and these can be used alone or in combination of two or more. Here, the number of carbon atoms in the perfluoroalkyl group is preferably 1 to 18, more preferably 1 to 10, and even more preferably 1 to 8. Among these, potassium perfluorobutanesulfonate is preferred.
[0079] Examples of aromatic sulfonic acid alkali (earth) metal salts include disodium diphenyl sulfide-4,4'-disulfonate, dipotassium diphenyl sulfide-4,4'-disulfonate, potassium 5-sulfoisophthalate, sodium 5-sulfoisophthalate, polysodium polyethylene terephthalate polysulfonate, calcium 1-methoxynaphthalene-4-sulfonate, disodium 4-dodecylphenyl ether disulfonate, polysodium poly(2,6-dimethylphenylene oxide) polysulfonate, polysodium poly(1,3-phenylene oxide) polysulfonate, polysodium poly(1,4-phenylene oxide) polysulfonate, polypotassium poly(2,6-diphenylphenylene oxide) polysulfonate, lithium poly(2-fluoro-6-butylphenylene oxide) polysulfonate, potassium benzenesulfonate, sodium benzenesulfonate, sodium p-toluenesulfonate, and strontium benzenesulfonate. , magnesium benzenesulfonate, dipotassium p-benzenedisulfonate, dipotassium naphthalene-2,6-disulfonate, calcium biphenyl-3,3'-disulfonate, sodium diphenylsulfone-3-sulfonate, potassium diphenylsulfone-3-sulfonate, dipotassium diphenylsulfone-3,3'-disulfonate, dipotassium diphenylsulfone-3,4'-disulfonate, sodium α,α,α-trifluoroacetophenone-4-sulfonate, benzof Examples of suitable aromatic sulfonic acid salts include dipotassium benzophenone-3,3'-disulfonate, disodium thiophene-2,5-disulfonate, dipotassium thiophene-2,5-disulfonate, calcium thiophene-2,5-disulfonate, sodium benzothiophenesulfonate, potassium diphenylsulfoxide-4-sulfonate, formalin condensates of sodium naphthalenesulfonate, and formalin condensates of sodium anthracenesulfonate, with potassium diphenylsulfone-3-sulfonate being preferred. Of these alkali (earth) metal salts of aromatic sulfonates, sodium and potassium salts are preferred.
[0080] These metal salt flame retardants may be used alone or in combination of two or more. When the polycarbonate resin composition according to the present invention contains a metal salt flame retardant as a flame retardant, the content of the flame retardant is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, even more preferably 0.03 parts by mass or more, still more preferably 0.04 parts by mass or more, relative to 100 parts by mass of the aromatic polycarbonate resin, from the viewpoint of further improving flame retardancy, and is preferably 1.0 part by mass or less, more preferably 0.8 parts by mass or less, even more preferably 0.6 parts by mass or less, still more preferably 0.4 parts by mass or less, from the viewpoint of further suppressing adhesion to the mold during molding of the resin composition and a decrease in the heat resistance of the molded product. Furthermore, when the polycarbonate resin composition according to the present invention contains a metal salt flame retardant as a flame retardant, the content of the flame retardant is preferably 0.01 to 1.0 part by mass, more preferably 0.02 to 0.8 parts by mass, even more preferably 0.03 to 0.6 parts by mass, and still more preferably 0.04 to 0.4 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin.
[0081] The total content of the aromatic polycarbonate resin and the flame retardant in the polycarbonate resin composition according to the present invention is, from the viewpoint of further improving the balance between tensile properties and flame retardancy, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, when the entire polycarbonate resin composition is taken as 100% by mass. The upper limit of the total content of the aromatic polycarbonate resin and the flame retardant is not particularly limited, but is, for example, 100% by mass or less, from the viewpoint of obtaining a resin composition having desired properties.
[0082] (Polystyrene-based resin) When the polycarbonate-based resin composition of the present invention contains the aromatic polycarbonate-based resin and the polystyrene-based resin, the fluidity of the polycarbonate-based resin composition is improved, and the molded article thereof has improved scratch resistance and tensile properties.
[0083] When the polycarbonate-based resin composition contains a polystyrene-based resin, it preferably contains 1% by mass or more and 30% by mass or less of the polystyrene-based resin relative to 100% by mass of the total of the aromatic polycarbonate-based resin and the polystyrene-based resin. When the polystyrene-based resin content is 1% by mass or more, the tensile properties and resin fluidity of the resulting molded article can be further improved. When the polystyrene-based resin content is 30% by mass or less, the mechanical strength and heat resistance can be further improved. The content of the polystyrene-based resin in the polycarbonate-based resin composition according to the present invention is preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 9% by mass or more, based on 100% by mass of the total of the aromatic polycarbonate-based resin and the polystyrene-based resin, from the viewpoint of further improving the tensile properties and resin fluidity of the resulting molded article. From the viewpoint of further improving the mechanical strength and heat resistance, the content is preferably 25% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and even more preferably 12% by mass or less. The content of the polystyrene resin in the polycarbonate resin composition according to the present invention is preferably 5 to 25 mass%, more preferably 7 to 20 mass%, even more preferably 9 to 15 mass%, and still more preferably 9 to 12 mass%, when the total of the aromatic polycarbonate resin and the polystyrene resin is taken as 100 mass%. The polycarbonate resin composition according to the present invention can contain one or more polystyrene resins.
[0084] From the viewpoint of further improving the tensile properties of the resulting molded article and the fluidity of the resin, the polystyrene resin preferably has a structural unit derived from acrylonitrile and a structural unit derived from styrene, and more preferably has a structural unit derived from butadiene, a structural unit derived from acrylonitrile, and a structural unit derived from styrene, and an amorphous polystyrene resin and a crystalline polystyrene resin can be used. In the present invention, as the polystyrene resin, one type of polystyrene resin may be used, or two or more types may be used in combination.
[0085] Examples of amorphous polystyrene resins include polymers without a crystalline structure obtained by polymerizing a monomer or a monomer mixture consisting of 20 to 100% by mass of a monovinyl aromatic monomer such as styrene or α-methylstyrene, 0 to 60% by mass of a vinyl cyanide monomer such as acrylonitrile or methacrylonitrile, and 0 to 50% by mass of other vinyl monomers copolymerizable therewith, such as maleimide or methyl (meth)acrylate. Examples of such polymers include general-purpose polystyrene (GPPS) and acrylonitrile-styrene copolymers (AS resins).
[0086] Furthermore, as the amorphous polystyrene resin, a rubber-modified polystyrene resin reinforced with a rubber-like polymer is preferably used. This rubber-modified polystyrene resin is preferably an acrylonitrile-butadiene-styrene copolymer, such as high impact polystyrene (HIPS) in which styrene is polymerized with a rubber such as polybutadiene, an acrylonitrile-butadiene-styrene copolymer (ABS resin) in which acrylonitrile and styrene are polymerized with polybutadiene, or a methyl methacrylate-butadiene-styrene copolymer (MBS resin) in which methyl methacrylate and styrene are polymerized with polybutadiene. Two or more types of rubber-modified polystyrene resins can be used in combination, and they can also be used as a mixture with the above-mentioned rubber-unmodified amorphous polystyrene resin.
[0087] The rubber content in the rubber-modified polystyrene resin is preferably 2 to 50% by mass, more preferably 5 to 30% by mass, and even more preferably 5 to 15% by mass. A rubber content of 2% by mass or more can improve impact resistance, while a rubber content of 50% by mass or less can suppress deterioration in thermal stability, deterioration in melt fluidity, gel formation, coloration, and the like. Specific examples of the rubber include polybutadiene, rubbery polymers containing acrylate and / or methacrylate, styrene-butadiene-styrene rubber (SBS), styrene-butadiene rubber (SBR), butadiene-acrylic rubber, isoprene rubber, isoprene-styrene rubber, isoprene-acrylic rubber, and ethylene-propylene rubber. Of these, polybutadiene is preferred. The polybutadiene used here may be either a polybutadiene with a low 1,4-cis bond content (e.g., one containing 1 to 30 mol % of 1,2-vinyl bonds and 30 to 42 mol % of 1,4-cis bonds) or a polybutadiene with a high 1,4-cis bond content (e.g., one containing 20 mol % or less of 1,2-vinyl bonds and 78 mol % or more of 1,4-cis bonds), or a mixture thereof.
[0088] Furthermore, examples of crystalline polystyrene-based resins include styrene-based (co)polymers having a syndiotactic structure or an isotactic structure. However, in the present invention, amorphous polystyrene-based resins are preferably used for the purpose of further improving fluidity. Furthermore, among amorphous polystyrene-based resins, those having a melt flow rate (MFR) at 200°C and a 5 kg load of preferably 0.5 g / 10 min to 100 g / 10 min, more preferably 2 g / 10 min to 80 g / 10 min, and even more preferably 2 g / 10 min to 50 g / 10 min are used. A melt flow rate (MFR) of 5 g / 10 min or more provides sufficient fluidity, and a melt flow rate (MFR) of 100 g / 10 min or less provides good impact resistance to the polycarbonate-based resin composition.
[0089] As the polystyrene resin, among amorphous polystyrene resins, from the viewpoint of further improving the tensile properties and resin fluidity of the obtained molded article, high impact polystyrene resin (HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), methyl methacrylate-styrene copolymer (MS resin), methyl methacrylate-butadiene-styrene copolymer (MBS resin), acrylonitrile-methyl acrylate-styrene copolymer (AAS resin), and acrylonitrile-(ethylene / propylene copolymer) At least one selected from the group consisting of acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), and methyl methacrylate-butadiene-styrene copolymer (MBS resin) is preferred, and at least one selected from the group consisting of acrylonitrile-butadiene-styrene copolymer (ABS resin) and acrylonitrile-styrene copolymer (AS resin) is even more preferred.
[0090] The total content of the aromatic polycarbonate resin and the polystyrene resin in the polycarbonate resin composition according to the present invention is, when the entire polycarbonate resin composition is taken as 100% by mass, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, from the viewpoint of further improving the tensile properties of the obtained molded article and the fluidity of the resin. The upper limit of the total content of the aromatic polycarbonate resin and the polystyrene resin is not particularly limited, but is, for example, 100% by mass or less, from the viewpoint of obtaining a resin composition having desired properties.
[0091] (Polyester-Based Resin) When the polycarbonate-based resin composition of the present invention contains the aromatic polycarbonate-based resin and the polyester-based resin, the polycarbonate-based resin composition and molded articles thereof exhibit the effects of improved scratch resistance and improved chemical resistance.
[0092] When the polycarbonate-based resin composition contains a polyester-based resin, it preferably contains 1 to 50% by mass of the polyester-based resin relative to 100% by mass of the total of the aromatic polycarbonate-based resin and the polyester-based resin. When the content of the polyester-based resin is 1% by mass or more, the balance between the tensile properties and chemical resistance of the resulting molded article can be further improved. When the content of the polyester-based resin is 50% by mass or less, the balance between the tensile properties and chemical resistance can be further improved. From the viewpoint of further improving the balance between the tensile properties and chemical resistance, the content of the polyester-based resin in the polycarbonate-based resin composition according to the present invention is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and even more preferably 18% by mass or more, relative to 100% by mass of the total of the aromatic polycarbonate-based resin and the polyester-based resin. From the viewpoint of further improving the balance between the tensile properties and chemical resistance, the content of the polyester-based resin is preferably 40% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. The content of the polyester resin in the polycarbonate resin composition according to the present invention is preferably 5 to 40% by mass, more preferably 10 to 35% by mass, even more preferably 15 to 30% by mass, and still more preferably 18 to 25% by mass, when the total of the aromatic polycarbonate resin and the polyester resin is taken as 100% by mass. The polycarbonate resin composition according to the present invention can contain one or more polyester resins.
[0093] The polyester resin is a polymer or copolymer of a polycarboxylic acid and a polyhydric alcohol. The polyester resin is preferably a polymer or copolymer of an aromatic dicarboxylic acid and a diol, and more preferably a polymer or copolymer obtained by a condensation reaction of an aromatic dicarboxylic acid or its reactive derivative with a diol or its ester derivative as the main components.
[0094] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-biphenyletherdicarboxylic acid, 4,4'-biphenylmethanedicarboxylic acid, 4,4'-biphenylsulfonedicarboxylic acid, 4,4'-biphenylisopropylidenedicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 2,5-anthracenedicarboxylic acid, 2,6-anthracenedicarboxylic acid, 4,4'-p-terphenylenedicarboxylic acid, and 2,5-pyridinedicarboxylic acid. Substituted products thereof (e.g., alkyl group substituted products such as 5-methylisophthalic acid) and reactive derivatives thereof (e.g., alkyl ester derivatives such as dimethyl terephthalate and diethyl terephthalate) can also be used. Among these, terephthalic acid, 2,6-naphthalenedicarboxylic acid, and alkyl ester derivatives thereof are more preferred, and terephthalic acid and alkyl ester derivatives thereof are even more preferred. These aromatic dicarboxylic acids may be used alone or in combination of two or more, and the aromatic dicarboxylic acids may also be used in combination with one or more aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and dodecanedioic acid, and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid.
[0095] Examples of diols that are components of polyester resins include aliphatic diols such as ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propanediol, triethylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, decamethylene glycol, and 2,2-dimethyl-1,3-propanediol; alicyclic diols such as 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, cyclohexanediol, trans- or cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol; and aromatic diols such as p-xylenediol, bisphenol A, tetrabromobisphenol A, and tetrabromobisphenol A-bis(2-hydroxyethyl ether). Substituted versions of these may also be used. Among these, from the viewpoints of heat resistance, dimensional stability, etc., aliphatic diols are preferred, with ethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol being more preferred, and ethylene glycol being even more preferred. The diols may be used alone or in combination of two or more. Furthermore, as the diol component, one or more long-chain diols having a molecular weight of 400 to 6,000, such as polyethylene glycol, poly-1,3-propylene glycol, and polytetramethylene glycol, may be copolymerized in combination with the above diols.
[0096] Polyester-based resins can be copolymerized with hydroxycarboxylic acids such as parahydroxybenzoic acid, other carboxylic acids, and alcohols other than the above diols, and such copolymer resins can also be used in this embodiment. However, it is preferable that such copolymerization components are present in small amounts, and it is preferable that 80% by mass or more, and even 90% by mass or more, of the polyester-based resin are components derived from aromatic dicarboxylic acids and aliphatic diols. Furthermore, it is preferable that 80 mol% or more, and even 90 mol% or more of the aromatic dicarboxylic acids and aliphatic diols are each composed of one type of compound. The polyester-based resin can be branched by introducing a small amount of a branching agent. The type of branching agent is not limited, but examples include trimesic acid, trimellitic acid, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0097] Examples of polyester resins include polyethylene terephthalate (PET), polypropylene terephthalate, polybutylene terephthalate (PBT), polyhexylene terephthalate, polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate, and copolymer polyester resins such as polyethylene isophthalate / terephthalate and polybutylene terephthalate / isophthalate. Of these, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, and mixtures thereof, which have a good balance of mechanical properties, can be preferably used. From the viewpoint of further improving the balance between tensile properties and chemical resistance, the polyester-based resin preferably contains at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate, more preferably at least one selected from the group consisting of polyethylene terephthalate and polybutylene terephthalate, and even more preferably at least one selected from the group consisting of polyethylene terephthalate and polybutylene terephthalate. Furthermore, from the viewpoint of further improving tensile properties, the polyester-based resin preferably contains polyethylene terephthalate, more preferably polyethylene terephthalate. When used in combination, the ratio between PET and PBT is preferably, for example, 1:1 to 1:8 (mass ratio).
[0098] The total content of the aromatic polycarbonate resin and polyester resin in the polycarbonate resin composition according to the present invention is, from the viewpoint of further improving the balance between tensile properties and chemical resistance, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, when the entire polycarbonate resin composition is taken as 100% by mass. The upper limit of the total content of the aromatic polycarbonate resin and polyester resin is not particularly limited, but from the viewpoint of obtaining a resin composition having desired properties, it is, for example, 100% by mass or less.
[0099] (Inorganic Filler) When the polycarbonate resin composition of the present invention contains the aromatic polycarbonate resin and an inorganic filler, the polycarbonate resin composition and molded articles thereof exhibit the effects of improving scratch resistance and rigidity.
[0100] When the polycarbonate-based resin composition contains an inorganic filler, the inorganic filler is preferably contained in an amount of 0.1 to 100 parts by mass per 100 parts by mass of the aromatic polycarbonate-based resin. When the content of the inorganic filler is 0.1 parts by mass or more, the balance between tensile properties and rigidity can be further improved. When the content of the inorganic filler is 100 parts by mass or less, for example, the moldability and impact resistance can be further improved. From the viewpoint of further improving the balance between tensile properties and rigidity, the content of the inorganic filler in the polycarbonate-based resin composition according to the present invention is more preferably 0.5 parts by mass or more, even more preferably 1.0 parts by mass or more, even more preferably 2.0 parts by mass or more, even more preferably 3.0 parts by mass or more, and even more preferably 4.0 parts by mass or more per 100 parts by mass of the aromatic polycarbonate-based resin. From the viewpoint of further improving the balance between tensile properties and rigidity, the content is more preferably 50 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and even more preferably 12 parts by mass or less. The content of the inorganic filler in the polycarbonate resin composition according to the present invention is more preferably 0.5 to 50 parts by mass, even more preferably 1.0 to 20 parts by mass, even more preferably 2.0 to 15 parts by mass, even more preferably 3.0 to 12 parts by mass, and even more preferably 4.0 to 12 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin. The polycarbonate resin composition according to the present invention can contain one or more types of inorganic fillers.
[0101] Examples of the inorganic filler include at least one selected from the group consisting of glass fillers (e.g., glass fibers, glass beads, glass flakes, glass powder, etc.), carbon fibers, aluminum fibers, calcium carbonate, magnesium carbonate, dolomite, silica, diatomaceous earth, alumina, titanium oxide, iron oxide, zinc oxide, magnesium oxide, calcium sulfate, magnesium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, carbon black, graphite, iron powder, lead powder, aluminum powder, and white pigments. From the viewpoint of further improving the balance between tensile properties and rigidity, glass fillers are preferred, and glass fibers are more preferred.
[0102] The white pigment is not particularly limited, but is preferably at least one selected from the group consisting of titanium oxide, zinc oxide, and zinc sulfide. Among these white pigments, titanium oxide is preferred from the viewpoint of making the color tone whiter.
[0103] Titanium oxide whose surface is coated with a polyol is preferred. Such a coating improves the dispersibility of titanium oxide in polycarbonate resin compositions and prevents a decrease in the molecular weight of the polycarbonate. Examples of surface treatments of titanium oxide with organic compounds include surface coating with polyols, as well as organic silicon compounds, alkanolamines, higher fatty acids, etc. Furthermore, for example, before coating the surface with a polyol, the titanium oxide surface may be coated with a hydrous oxide and / or oxide of at least one element, including elements such as aluminum, silicon, magnesium, zirconia titanium, and tin.
[0104] Examples of polyols used to coat titanium oxide with polyols include trimethylolpropane, trimethylolethane, ditrimethylolpropane, trimethylolpropane ethoxylate, and pentaerythritol. Among these, trimethylolpropane and trimethylolethane are preferred. Methods for coating the surface with polyol include wet and dry methods. The wet method involves adding titanium oxide to a mixture of polyol and a low-boiling solvent, stirring, and then removing the low-boiling solvent. The dry method involves mixing the polyol and titanium oxide in a mixer such as a Henschel mixer or tumbler, or dissolving or dispersing the polyol in a solvent and spraying the resulting mixed solution onto the titanium oxide. Coating the surface with such polyols can prevent deterioration of the physical properties of the polycarbonate resin composition, improve the dispersibility of titanium oxide in the resin composition, and prevent molding defects such as silver. Titanium oxide produced by either the chlorine method or the sulfuric acid method can be used. The crystalline structure of titanium oxide may be either rutile or anatase, but the rutile type is more preferred from the viewpoint of the thermal stability, light resistance, etc. of the polycarbonate resin composition.
[0105] Any talc commercially available as an additive for thermoplastic resins can be used. Talc is a hydrous magnesium silicate, and in addition to the main components of silicic acid and magnesium oxide, it may contain trace amounts of aluminum oxide, calcium oxide, or iron oxide, or these may be included. The average particle size is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 50 μm or less, more preferably 20 μm or less. The average particle size is preferably 0.5 to 50 μm, more preferably 1 to 20 μm. The aspect ratio is, for example, 2 to 20. These average particle size and aspect ratio are determined by comprehensively considering the flowability during molding, the impact resistance and rigidity required of the molded product, and other ingredients. Talc that has been surface-treated with a fatty acid or the like, or pulverized in the presence of a fatty acid or the like, can also be used.
[0106] When glass fibers are blended as an inorganic filler in the polycarbonate-based resin composition according to the present invention, the rigidity of the molded article can be further improved. The glass fibers are preferably produced using alkali-containing glass, low-alkali glass, or alkali-free glass as the raw material, and the fiber form may be any of roving, milled fiber, chopped strand, etc. The cross section of the glass fibers may also be flat. The diameter of the glass fibers is preferably 3 to 30 μm, and the length is preferably 1 to 6 mm. When the diameter of the glass fibers is 3 μm or more, the rigidity of the polycarbonate-based resin composition can be further increased, and when it is 30 μm or less, the appearance of the molded article becomes good.
[0107] The fiber length of the glass fiber is, for example, 0.01 to 8 mm, preferably 0.1 to 6 mm. The fiber diameter is, for example, approximately 0.1 to 30 μm, preferably 0.5 to 25 μm. These glass fibers may be used singly or in combination of two or more. To enhance their affinity with resins, glass fibers may be surface-treated with silane coupling agents such as aminosilanes, epoxysilanes, vinylsilanes, and methacrylsilanes, chromium complex compounds, or boron compounds, or may be further subjected to a sizing treatment using a sizing agent. Suitable examples of such glass fibers include MA-409C (average fiber diameter: 13 μm) and TA-409C (average fiber diameter: 23 μm) manufactured by Asahi Fiberglass Co., Ltd., and T-511 (average fiber diameter: 12 to 14 μm) manufactured by Nippon Electric Glass Co., Ltd.
[0108] When the polycarbonate resin composition according to the present invention contains titanium oxide as an inorganic filler, the content of the inorganic filler is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, and even more preferably 2.0 parts by mass or more, per 100 parts by mass of the aromatic polycarbonate resin, from the viewpoint of further improving the balance between tensile properties and rigidity and from the viewpoint of improving the degree of whiteness, and is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, from the viewpoint of further improving moldability and impact resistance. Furthermore, when the polycarbonate resin composition according to the present invention contains titanium oxide as an inorganic filler, the content of the inorganic filler is preferably 0.5 to 50 parts by mass, more preferably 1.0 to 40 parts by mass, and even more preferably 2.0 to 40 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin.
[0109] When the polycarbonate resin composition according to the present invention contains talc as an inorganic filler, the content of the inorganic filler is, from the viewpoint of further improving the balance between tensile properties and rigidity and from the viewpoint of improving dimensional stability, preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, even more preferably 2.0 parts by mass or more, even more preferably 3.0 parts by mass or more, and still more preferably 4.0 parts by mass or more, relative to 100 parts by mass of the aromatic polycarbonate resin; and, from the viewpoint of further improving moldability and impact resistance, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, even more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, and still more preferably 8.0 parts by mass or less. When the polycarbonate resin composition according to the present invention contains talc as an inorganic filler, the content of the inorganic filler is preferably 0.5 to 100 parts by mass, more preferably 1.0 to 50 parts by mass, even more preferably 2.0 to 20 parts by mass, even more preferably 3.0 to 15 parts by mass, even more preferably 3.0 to 12 parts by mass, even more preferably 4.0 to 10 parts by mass, and even more preferably 4.0 to 8.0 parts by mass, relative to 100 parts by mass of the aromatic polycarbonate resin.
[0110] When the polycarbonate-based resin composition according to the present invention contains glass fiber as an inorganic filler, the content of the inorganic filler is, from the viewpoint of further improving the balance between tensile properties and rigidity and from the viewpoint of improving dimensional stability, preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, even more preferably 2.0 parts by mass or more, even more preferably 3.0 parts by mass or more, even more preferably 4.0 parts by mass or more, even more preferably 6.0 parts by mass or more, and still more preferably 8.0 parts by mass or more, relative to 100 parts by mass of the aromatic polycarbonate-based resin; and from the viewpoint of further improving moldability and impact resistance and from the viewpoint of further improving appearance, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and still more preferably 12 parts by mass or less. Furthermore, when the polycarbonate resin composition according to the present invention contains glass fiber as an inorganic filler, the content of the inorganic filler is preferably 0.5 to 100 parts by mass, more preferably 1.0 to 50 parts by mass, even more preferably 2.0 to 20 parts by mass, even more preferably 3.0 to 15 parts by mass, even more preferably 4.0 to 15 parts by mass, even more preferably 6.0 to 12 parts by mass, and even more preferably 8.0 to 12 parts by mass, relative to 100 parts by mass of the aromatic polycarbonate resin.
[0111] The total content of the aromatic polycarbonate resin and inorganic filler in the polycarbonate resin composition according to the present invention is, from the viewpoint of further improving the balance between tensile properties and rigidity, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, when the entire polycarbonate resin composition is taken as 100% by mass. The upper limit of the total content of the aromatic polycarbonate resin and inorganic filler is not particularly limited, but is, for example, 100% by mass or less, from the viewpoint of obtaining a resin composition having desired properties.
[0112] When the polycarbonate-based resin composition of the present invention contains at least two or more components selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene-based resin, a polyester-based resin, and an inorganic filler, the polycarbonate-based resin composition can exhibit the respective effects derived from each component.
[0113] The content of the aromatic polycarbonate resin in the polycarbonate resin composition of the present invention varies depending on whether the polycarbonate resin composition contains an ultraviolet absorber, a flame retardant, a polystyrene resin, a polyester resin, or an inorganic filler, but is preferably 60% by mass or more, more preferably 65% by mass or more, and even more preferably 70% by mass or more, and is preferably 99.99% by mass or less, more preferably 99.97% by mass or less, and even more preferably 99.96% by mass or less. The content of the aromatic polycarbonate resin in the polycarbonate resin composition of the present invention is preferably 60 to 99.99% by mass, more preferably 65 to 99.97% by mass, and even more preferably 70 to 99.96% by mass.
[0114] The polycarbonate resin composition of the present invention may contain, in addition to the aromatic polycarbonate resin, ultraviolet absorber, flame retardant, polystyrene resin, polyester resin, and inorganic filler, additives such as hydrolysis stabilizers, antioxidants, flame retardant aids, pigments, and dyes.
[0115] For example, the polycarbonate resin composition may contain an antioxidant from the viewpoint of preventing oxidative degradation during melting and preventing coloration due to oxidative degradation. The content of the antioxidant is preferably 0.001 to 0.5 parts by mass, more preferably 0.01 to 0.3 parts by mass, and even more preferably 0.02 to 0.2 parts by mass, per 100 parts by mass of the aromatic polycarbonate resin. When the content of the antioxidant is within the above range, a sufficient antioxidant effect can be obtained and mold contamination during molding can be suppressed.
[0116] The method for producing the polycarbonate resin composition of the present invention is not particularly limited as long as it includes a step of mixing the aromatic polycarbonate resin with at least one selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene resin, a polyester resin, and an inorganic filler. For example, the polycarbonate resin composition can be produced by mixing the aromatic polycarbonate resin with at least one selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene resin, a polyester resin, and an inorganic filler using a mixer or the like, followed by melt-kneading. Melt-kneading can be carried out by a commonly used method, such as a method using a ribbon blender, a Henschel mixer, a Banbury mixer, a drum tumbler, a single-screw extruder, a twin-screw extruder, a co-kneader, or a multi-screw extruder. The heating temperature during melt-kneading is appropriately selected, for example, from 150°C to 300°C, preferably from about 220°C to 300°C.
[0117] 2. Molded Articles The molded article of the present invention contains the polycarbonate resin composition. The molded article can be produced by injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum molding, foam molding, or the like, using a melt-kneaded product of the polycarbonate resin composition or pellets obtained by melt-kneading as a raw material. It is particularly preferable to produce a molded article by injection molding or injection compression molding using pellets obtained by melt-kneading. The thickness of the molded article can be set as desired depending on the application. When transparency is particularly required, the thickness is preferably 0.2 to 4.0 mm, more preferably 0.3 to 3.0 mm, and even more preferably 0.3 to 2.0 mm. A molded article having a thickness of 0.2 mm or more will not warp and will have good mechanical strength. Furthermore, a molded article having a thickness of 4.0 mm or less will have high transparency.
[0118] The polycarbonate resin composition of the present invention can improve the scratch resistance of molded articles, and therefore can be suitably used in scratch-resistant applications. Examples of scratch-resistant applications include structures whose outer surfaces are formed from the polycarbonate resin composition, and more specifically, plastic windows, touch panels, interior and exterior products, vehicle interior and exterior parts, housings, electrical appliance parts, building materials, and office automation equipment parts. The polycarbonate resin composition of the present invention can be suitably used to produce the above-mentioned articles.
[0119] Molded articles made from the polycarbonate resin composition of the present invention can be suitably used, for example, as plastic windows, touch panels, interior and exterior products, vehicle interior and exterior parts, housings, electrical appliance parts, or building materials.
[0120] The present invention will be further described with reference to examples. However, the present invention is not limited to these examples. Measurements and evaluations in each example were carried out by the methods shown below.
[0121] 1. Measurement of Viscosity Average Molecular Weight (Mv) The viscosity average molecular weight (Mv) was determined by measuring the viscosity of a methylene chloride solution (concentration: g / L) at 20°C using an Ubbelohde viscometer, determining the intrinsic viscosity [η] from the viscosity, and calculating the viscosity average molecular weight (Mv) using the following formula (Schnell's formula): [η] = 1.23 × 10 -5 Mv 0.83
[0122] 2. 1 H-NMR measurement conditions Nuclear magnetic resonance (NMR) apparatus: "ECA-500" manufactured by JEOL RESONANCE Co., Ltd. Probe: 50TH5AT / FG2 Measurement nucleus: 1 H Observation width: -5 to 15 ppm Observation center: 5 ppm Pulse repetition time: 9 seconds Pulse width: 45° NMR sample tube: 5 mmφ Sample amount: 30 to 40 mg Solvent: deuterated chloroform Solvent amount: 0.4 mL Measurement temperature: 25°C Number of accumulations: 256 Chemical shift correction: The peak of the methyl group derived from bisphenol A in the sample was set as the reference at 1.68 ppm
[0123] 3. Quantitative determination of the composition ratio of aromatic polycarbonate resins. Using the "ECA-500" manufactured by JEOL RESONANCE Co., Ltd., the sample dissolved in deuterated chloroform was 1 H-NMR was measured under the same conditions as above, and the structure of the aromatic polycarbonate resin was assigned.
[0124] Synthesis Example 1 (Synthesis of Cyclohexyl Diphenolate) 620 mL of cyclohexanol, 111 g (388 mmol) of diphenolic acid, and 5.69 g (58.0 mmol) of sulfuric acid were charged into a 1 L flask to obtain a reaction solution, and a stirrer tip, thermometer, and reflux condenser were attached. The reaction solution was heated to 80°C using an oil bath and stirred for 19 hours using a magnetic stirrer. After confirming the disappearance of diphenolic acid by thin layer chromatography (TLC), the reaction solution was returned to room temperature. 600 mL of toluene was added to the reaction solution, and the solution was washed twice with 800 mL of aqueous sodium bicarbonate (saturated aqueous sodium bicarbonate solution) and once with 800 mL of brine (saturated saline solution). The organic phase was dried over anhydrous sodium sulfate and then concentrated under reduced pressure to obtain 316 g of a pale brown liquid as a crude product. The obtained crude product was purified using a silica gel column (1.05 kg of neutral silica gel, solvent: heptane / ethyl acetate = 4 / 1) to obtain 263 g of a pale yellow liquid. The resulting pale yellow liquid was azeotropically distilled eight times with a 2:1 acetonitrile / water (300 g) mixed solvent. The precipitated solid was collected by vacuum filtration and washed twice with 500 mL of hexane. The resulting solid was dried under reduced pressure at 40°C for 12 hours to obtain 113 g of a white solid of cyclohexyl diphenolate.
[0125] Synthesis Example 2 (Synthesis of Cyclopentyl Diphenolate) A 1-L flask was charged with 694 mL of cyclopentanol, 124 g (434 mmol) of diphenolic acid, and 6.37 g (65.0 mmol) of sulfuric acid to obtain a reaction solution. A stirrer tip, a thermometer, and a reflux condenser were then installed. The reaction solution was heated to 80°C using an oil bath and stirred for 19 hours using a magnetic stirrer. After confirming the disappearance of diphenolic acid by thin-layer chromatography (TLC), the reaction solution was returned to room temperature. 600 mL of toluene was added to the reaction solution, which was then washed twice with 600 mL of aqueous sodium bicarbonate (saturated aqueous sodium bicarbonate solution) and once with 600 mL of brine (saturated saline solution). The organic phase was dried over anhydrous sodium sulfate and then concentrated under reduced pressure to obtain 172 g of a light brown liquid as a crude product. The resulting crude product was dissolved in hexane / ethyl acetate = 9 / 1 (350 g) and left at room temperature overnight. The precipitated solid was collected by vacuum filtration and dried under reduced pressure at 40°C for 12 hours to give a white solid of cyclopentyl diphenolate (55.3 g). The filtrate was allowed to stand overnight at 4°C, and the precipitated solid was collected by vacuum filtration and dried under reduced pressure at 40°C for 12 hours to give a white solid of cyclopentyl diphenolate (38.5 g). The filtrate was concentrated under reduced pressure, and the resulting liquid was dissolved in chloroform (100 g), to which toluene (180 g) was added, and the mixture was left overnight at 4°C. The precipitated solid was collected by vacuum filtration and suspended and washed twice with hexane. The washed solid was dried under reduced pressure at 50°C for 12 hours to give a white solid of cyclopentyl diphenolate (14.4 g). A total of 108.2 g of cyclopentyl diphenolate was obtained.
[0126] Synthesis Example 3 (Synthesis of cyclohexyl 2,2-bis(4-hydroxyphenyl)propanoate) Phenol (131 g, 1.39 mol), pyruvic acid (60.3 g, 0.68 mol), and ion-exchanged water (45.6 g) were placed in a 1 L four-neck flask, and a stirrer tip and thermometer were attached. The flask was ice-cooled, and 95% sulfuric acid (112 g, 1.14 mol) was added dropwise over 50 minutes. The reaction solution was then warmed to room temperature and stirred for 14 hours. Diethyl ether (1 L) was added to the reaction solution, and the mixture was washed once with ion-exchanged water (1 L). The organic layer was extracted twice with 0.1 M aqueous sodium hydroxide solution (1 L). The extract was adjusted to pH 2 with 1 M hydrochloric acid and extracted twice with diethyl ether (1 L). The extract was dried over sodium sulfate and then dried under reduced pressure to obtain a light brown solid (139 g). A 5-L four-neck flask was charged with this light brown solid (130 g), cyclohexanol (2.01 L), and 95% sulfuric acid (27.7 g, 0.28 mol), and a stirring blade, thermometer, and reflux condenser were installed. The reaction solution was then heated to 100°C and stirred for 15 days. The reaction solution was diluted two-fold with diethyl ether and washed twice with aqueous sodium bicarbonate, once with water, and once with brine. The organic layer was dried over magnesium sulfate and concentrated under reduced pressure to obtain a crude product (815 g). The crude product was purified three times with silica gel (neutral silica gel: 5.0 kg, solvent: chloroform / ethyl acetate = 1 / 0 → 0 / 1). The crude product was then dissolved in a chloroform / ethyl acetate = 1 / 1 solution and recrystallized to obtain a white solid (52.9 g) of cyclohexyl 2,2-bis(4-hydroxyphenyl)propanoate.
[0127] Synthesis Example 4 (Synthesis of Methyl Diphenolate) A 1-L flask was charged with 500 mL of methanol, 50 g (175 mmol) of diphenolic acid, and 2.5 mL of sulfuric acid, and a stirrer tip, thermometer, and reflux condenser were attached. The reaction solution was heated to 70°C using an oil bath and stirred for 5 hours using a magnetic stirrer. The reaction solution was returned to room temperature and then concentrated under reduced pressure. Ethyl acetate was added to the reaction solution, which was then washed three times with 100 mL of aqueous sodium bicarbonate and twice with 100 mL of water. The solution was concentrated under reduced pressure to obtain 55.3 g of a colorless solid as a crude product. The resulting crude product and 100 mL of toluene were added to a 200-mL flask, and a stirrer tip, thermometer, and reflux condenser were attached. The reaction solution was heated using an oil bath until the toluene refluxed, and the crude product was completely dissolved in the toluene. The mixture was then allowed to cool to room temperature, and the precipitated solid was collected by vacuum filtration. The recovered solid was dissolved again in 100 mL of toluene, and the same procedure was repeated to obtain 32.7 g of a white solid of methyl diphenolate.
[0128] Synthesis Example 5 (Synthesis of Polycarbonate Oligomer) Sodium dithionite (Na 2 S 2 O 4 ) was added to the bisphenol A (BPA) to be dissolved later to a concentration of 2000 ppm. BPA was dissolved in this to a BPA concentration of 13.5% by mass, preparing an aqueous sodium hydroxide solution of BPA. This aqueous sodium hydroxide solution of BPA was continuously passed through a tubular reactor with an inner diameter of 6 mm and a tube length of 30 m at flow rates of 40 L / hr, methylene chloride at 13 L / hr, and phosgene at 4.5 kg / hr. The tubular reactor had a jacket, and cooling water was passed through the jacket to maintain the temperature of the reaction solution below 40°C. The reaction solution was continuously withdrawn from the tubular reactor and allowed to stand, allowing the aqueous phase to be separated and removed, and the methylene chloride phase to be collected. The methylene chloride solution of polycarbonate oligomer (PCO) thus obtained (PCO solution (a)) had a concentration of 301 g / L and a chloroformate group concentration of 1.03 mol / L.
[0129] Production Example 1 (Synthesis of aromatic polycarbonate resin (PC-1) [BPA-cyclohexyl diphenolate copolymer]) A 1 L separable flask equipped with a baffle was charged with 255 mL of the polycarbonate oligomer solution produced in Synthesis Example 5, 495 mL of methylene chloride, 21.2 g of cyclohexyl diphenolate produced in Synthesis Example 1 above, and 178 μL of triethylamine (TEA), and an aqueous sodium hydroxide solution (3.3 g of sodium hydroxide dissolved in 38.1 mL of pure water) was added thereto with stirring, and the reaction was carried out for 20 minutes to obtain a polymerization liquid. To this polymerization solution, a methylene chloride solution of p-tert-butylphenol (PTBP) (1.84 g of PTBP dissolved in 13 mL of methylene chloride) and an aqueous sodium hydroxide solution of BPA (17.9 g of BPA dissolved in an aqueous solution of 9.9 g of sodium hydroxide and 36 mg of sodium dithionite dissolved in 145 mL of pure water) were added, and the polymerization reaction was carried out for 40 minutes. After adding 100 mL of methylene chloride for dilution and stirring for 10 minutes, the mixture was separated into an organic phase containing the aromatic polycarbonate resin (PC-1) and an aqueous phase containing excess BPA and sodium hydroxide, and the organic phase was isolated. The methylene chloride solution of the aromatic polycarbonate resin (PC-1) thus obtained was washed successively with a 15% by volume 0.03 mol / L aqueous sodium hydroxide solution and 0.2 mol / L hydrochloric acid, and then repeatedly washed with pure water until the electrical conductivity of the aqueous phase after washing was 5 μS / cm or less. The washed organic phase was flaked by distilling off the solvent using an evaporator to obtain an aromatic polycarbonate resin (PC-1) as a white product. The content of the structural unit represented by formula (II) in the aromatic polycarbonate resin (PC-1) was 21.3 mass %, and the viscosity average molecular weight (Mv) was 22,100.
[0130] Production Example 2 (Synthesis of aromatic polycarbonate resin (PC-2) [BPA-cyclohexyl 2,2-bis(4-hydroxyphenyl)propanoate copolymer]) A 300 mL separable flask equipped with a baffle was charged with 58 mL of the polycarbonate oligomer solution produced in Synthesis Example 5, 19 mL of methylene chloride, 4.15 g of cyclohexyl 2,2-bis(4-hydroxyphenyl)propanoate produced in Synthesis Example 3 above, and 41 μL of triethylamine (TEA), and an aqueous sodium hydroxide solution (0.9 g of sodium hydroxide dissolved in 9.8 mL of pure water) was added thereto with stirring, and the reaction was carried out for 20 minutes to obtain a polymerization liquid. To this polymerization solution, a methylene chloride solution of p-tert-butylphenol (PTBP) (0.34 g of PTBP dissolved in 2.4 mL of methylene chloride) and an aqueous sodium hydroxide solution of BPA (4.5 g of BPA dissolved in an aqueous solution of 2.2 g of sodium hydroxide and 9 mg of sodium dithionite dissolved in 32 mL of pure water) were added, and the polymerization reaction was carried out for 40 minutes. 105 mL of methylene chloride was added for dilution and the mixture was stirred for 10 minutes, after which the mixture was separated into an organic phase containing the aromatic polycarbonate resin (PC-2) and an aqueous phase containing excess BPA and sodium hydroxide, and the organic phase was isolated. The methylene chloride solution of the aromatic polycarbonate resin (PC-2) thus obtained was washed successively with a 15% by volume 0.03 mol / L aqueous sodium hydroxide solution and 0.2 mol / L hydrochloric acid, and then repeatedly washed with pure water until the electrical conductivity of the aqueous phase after washing was 5 μS / cm or less. The washed organic phase was flaked by distilling off the solvent using an evaporator, yielding an aromatic polycarbonate resin (PC-2) as a white product. The content of the structural unit represented by formula (II) in the aromatic polycarbonate resin (PC-2) was 23.0 mass %, and the viscosity average molecular weight (Mv) was 22,300.
[0131] Production Example 3 (Synthesis of aromatic polycarbonate resin (PC-3) [BPA-cyclopentyl diphenolate copolymer]) A 300 mL separable flask equipped with a baffle was charged with 58 mL of the polycarbonate oligomer solution produced in Synthesis Example 5, 19 mL of methylene chloride, 4.1 g of cyclopentyl diphenolate produced in Synthesis Example 2 above, and 41 μL of triethylamine (TEA), and an aqueous sodium hydroxide solution (0.8 g of sodium hydroxide dissolved in 8.7 mL of pure water) was added thereto with stirring, and the mixture was allowed to react for 20 minutes to obtain a polymerization solution. To this polymerization solution, a methylene chloride solution of p-tert-butylphenol (PTBP) (0.34 g of PTBP dissolved in 2.4 mL of methylene chloride) and an aqueous sodium hydroxide solution of BPA (4.3 g of BPA dissolved in an aqueous solution of 2.3 g of sodium hydroxide and 9 mg of sodium dithionite dissolved in 33 mL of pure water) were added, and the polymerization reaction was carried out for 40 minutes. After adding 100 mL of methylene chloride for dilution and stirring for 10 minutes, the mixture was separated into an organic phase containing the aromatic polycarbonate resin (PC-3) and an aqueous phase containing excess BPA and sodium hydroxide, and the organic phase was isolated. The methylene chloride solution of the aromatic polycarbonate resin (PC-3) thus obtained was washed successively with a 15% by volume 0.03 mol / L aqueous sodium hydroxide solution and 0.2 mol / L hydrochloric acid, and then repeatedly washed with pure water until the electrical conductivity of the aqueous phase after washing was 5 μS / cm or less. The washed organic phase was flaked by distilling off the solvent using an evaporator, yielding an aromatic polycarbonate resin (PC-3) as a white product. The content of the structural unit represented by formula (II) in the aromatic polycarbonate resin (PC-3) was 21.8 mass %, and the viscosity average molecular weight (Mv) was 24,500.
[0132] Production Example 4 (Synthesis of aromatic polycarbonate resin (PC-4) [BPA-methyl diphenolate]) A 300 mL separable flask equipped with a baffle was charged with 42 mL of the polycarbonate oligomer solution produced in Synthesis Example 5, 58 mL of methylene chloride, 0.24 g of p-tert-butylphenol (PTBP), 2.9 g of methyl diphenolate produced in Synthesis Example 4 above, and 29 μL of triethylamine (TEA), and an aqueous sodium hydroxide solution (0.5 g of sodium hydroxide dissolved in 6.2 mL of pure water) was added thereto with stirring, and the reaction was carried out for 20 minutes to obtain a polymerization solution. To this polymerization solution, an aqueous sodium hydroxide solution of BPA (3.1 g of BPA dissolved in an aqueous solution of 1.6 g of sodium hydroxide and 6 mg of sodium dithionite dissolved in 24 mL of pure water) was added, and the polymerization reaction was carried out for 40 minutes. After adding 50 mL of methylene chloride for dilution and stirring for 10 minutes, the mixture was separated into an organic phase containing aromatic polycarbonate-based resin (PC-4) and an aqueous phase containing excess BPA and sodium hydroxide, and the organic phase was isolated. The methylene chloride solution of aromatic polycarbonate-based resin (PC-4) thus obtained was washed successively with a 15% by volume 0.03 mol / L aqueous sodium hydroxide solution and 0.2 mol / L hydrochloric acid, and then repeatedly washed with pure water until the electrical conductivity of the aqueous phase after washing was 5 μS / cm or less. The washed organic phase was flaked by distilling off the solvent using an evaporator, yielding aromatic polycarbonate-based resin (PC-4) as a white product. The content of the structural unit represented by formula (II) in aromatic polycarbonate-based resin (PC-4) was 19.4% by mass, and the viscosity average molecular weight (Mv) was 21,400.
[0133] Examples 1 to 10 and Comparative Examples 1 to 9 As shown in Table 1, aromatic polycarbonate resins (PC-1) to (PC-4) and aromatic polycarbonate resin "Taflon FN2200" (trade name, manufactured by Idemitsu Kosan Co., Ltd., aromatic polycarbonate resin composed of BPA, viscosity average molecular weight Mv 21,700), as well as any of ultraviolet absorbers, flame retardants, polystyrene resins, polyester resins, and inorganic fillers were mixed and supplied to a vented twin-screw extruder (manufactured by DSM Xplore, Micro 15cc Twin Screw Compounder), and melt-kneaded at a screw rotation speed of 50 to 60 rpm, a discharge rate of 20 kg / hr, and a resin temperature of 270 to 295°C to obtain evaluation pellet samples of polycarbonate resin compositions 1 to 10 and 21 to 29.
[0134] (Evaluation of Scratch Hardness (Pencil Method)) The polycarbonate resin compositions 1 to 10 and 21 to 29 obtained above were injection molded using an injection molding machine ("Mini Jet Pro" manufactured by Thermo Fisher Scientific) under conditions of a cylinder temperature of 275 to 300°C and a mold temperature of 110 to 120°C to produce disc-shaped molded products (diameter 30 mm, thickness 1.5 mm). In accordance with JIS K 5600-5-4:1999, a line was drawn with a pencil held at a 45-degree angle and a load of 750 g applied, and the presence or absence of scratches on the surface was inspected with the naked eye to evaluate the scratch hardness (pencil method). The pencil hardness determined by the scratch hardness (pencil method) was rated on a 14-level scale of 6B to B, HB, F, and H to 6H. The results are shown in Table 1.
[0135] *1: FN refers to Idemitsu Kosan Co., Ltd.'s "Toughlon FN2200" (aromatic polycarbonate resin composed of BPA, viscosity average molecular weight Mv 21,700). *2: LA-31 refers to ADEKA Corporation's "ADEKA STAB™ LA-31RG" (2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol]). *3: KFBS refers to Mitsubishi Materials Corporation's "EFTOP KFBS" (potassium perfluorobutanesulfonate). *4: PX-200 refers to Daihachi Chemical Industry Co., Ltd.'s "PX-200" (1,3-phenylene-tetrakis(2,6-dimethylphenyl)phosphate). *5: AT-05 refers to Nippon A&L Co., Ltd.'s "Santac AT-05" (acrylonitrile-butadiene-styrene copolymer). *6: S101N means "S101N" (acrylonitrile-styrene binary copolymer) manufactured by Techno UMG Co., Ltd. *7: J055 means "Mitsui Pet (trademark) J055" (polyethylene terephthalate) manufactured by Mitsui Chemicals, Inc. *8: J125 means "Mitsui Pet (trademark) J125" (polyethylene terephthalate) manufactured by Mitsui Chemicals, Inc. *9: GF means "T511" (glass fiber) manufactured by Nippon Electric Glass Co., Ltd.
[0136] As shown in Table 1, the polycarbonate-based resin compositions 1 to 10 of the examples exhibited superior scratch hardness and improved scratch resistance compared to the polycarbonate-based resin compositions 21 to 29 of the comparative examples, which correspond to the ultraviolet absorber, flame retardant, polystyrene-based resin, polyester-based resin, and inorganic filler contained therein. Furthermore, the scratch hardness of the polycarbonate-based resin compositions 23 and 25 to 28 of the comparative examples 3 and 5 to 9 was HB or F, which was a good result, but the scratch hardness of the polycarbonate-based resin compositions 3 and 5 to 8 of the corresponding examples 3 and 5 to 8 was F or 2H, which suggests that the scratch hardness of the polycarbonate-based resin compositions 23 and 25 to 28 is due to the flame retardant, polystyrene-based resin, polyester-based resin, and inorganic filler rather than the aromatic polycarbonate-based resin. It was found that the polycarbonate-based resin composition 1 of Example 1 exhibited scratch hardness equivalent to or superior to that of the polycarbonate-based resin composition 29 of Comparative Example 9 containing the same amount of ultraviolet absorber, and thus had improved scratch resistance. 14 By including an aromatic polycarbonate-based resin containing a structural unit represented by formula (II) in which R is a group having a cyclic structure, the scratch resistance of the polycarbonate-based resin composition can be improved. 14 It is believed that the scratch resistance of the polycarbonate resin composition containing an aromatic polycarbonate resin containing a structural unit represented by formula (II) in which R is a group having a chain structure is improved compared to that of the polycarbonate resin composition containing an aromatic polycarbonate resin containing a structural unit represented by formula (II) in which R is a group having a chain structure.
Claims
1. A polycarbonate-based resin composition comprising an aromatic polycarbonate-based resin containing a structural unit represented by the following formula (II), and at least one selected from the group consisting of an ultraviolet absorber, a flame retardant, a polystyrene-based resin, a polyester-based resin, and an inorganic filler. [In formula (II), R 11 and R 12 R each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. 13 R represents a group selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, and an aryl group having 6 to 14 carbon atoms. 14 represents a saturated or unsaturated alicyclic group having 3 to 20 carbon atoms, or a saturated or unsaturated heterocyclic group having 3 to 20 members. c and d each independently represent an integer of 0 to 4. n represents an integer of 0 to 20.] 2. R 14 2. The polycarbonate resin composition according to claim 1, wherein represents a saturated or unsaturated alicyclic group having 3 to 12 carbon atoms, or a saturated or unsaturated heterocyclic group having 3 to 12 members.
3. R 14 The polycarbonate resin composition according to claim 2, wherein is a cyclopentyl group or a cyclohexyl group.
4. The polycarbonate resin composition according to any one of claims 1 to 3, wherein n is an integer of 0 to 4.
5. The polycarbonate resin composition according to any one of claims 1 to 4, wherein the ultraviolet absorber comprises at least one member selected from the group consisting of benzotriazole-based ultraviolet absorbers, benzoxazinone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, malonic acid ester-based ultraviolet absorbers, oxalyl alanide-based ultraviolet absorbers, triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers.
6. The polycarbonate resin composition according to any one of claims 1 to 4, wherein the flame retardant comprises at least one selected from the group consisting of phosphorus-based flame retardants and metal salt-based flame retardants.
7. The polycarbonate resin composition according to any one of claims 1 to 4, wherein the polystyrene resin comprises at least one selected from the group consisting of impact resistant polystyrene resin, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-styrene copolymer, methyl methacrylate-butadiene-styrene copolymer, acrylonitrile-methyl acrylate-styrene copolymer, and acrylonitrile-(ethylene / propylene / diene copolymer)-styrene copolymer.
8. The polycarbonate resin composition according to any one of claims 1 to 4, wherein the polyester resin comprises at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate.
9. The polycarbonate resin composition according to any one of claims 1 to 4, wherein the inorganic filler is a glass filler.
10. The polycarbonate resin composition according to any one of claims 1 to 9, further comprising a repeating unit represented by the following formula (I): [In formula (I), R 1 and R 2each independently represents a group selected from the group consisting of a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a cycloalkoxy group having 3 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxyl group. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, -S-, -SO-, -SO 2 represents -, -O-, or -CO-; a and b each independently represent an integer of 0 to 4.
11. A molded article made from the polycarbonate resin composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Novel copolycarbonate resin and its production
JP1989065125A
T-alkyl ester bisphenol, process for producing same and use thereof
JP1992226942A
Polycarbonate resin, electrophotographic photoreceptor and image-forming device
JP2005139339A
Soakable blocks with rain storage which upstep permeability
KR1020210031875A
Aromatic polycarbonate resin, polycarbonate resin composition and molded article
WO2023074830A1