Conjugated diene polymer and method for producing conjugated diene polymer

A conjugated diene polymer with controlled structural features addresses the challenge of achieving both wet grip and winter performance in tire rubber, enhancing abrasion resistance and tensile properties, and overcoming previous formulations' limitations in physical properties.

WO2024225452A1PCT designated stage expired Publication Date: 2024-10-31ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016507
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional rubber compositions containing conjugated diene polymers face challenges in achieving both excellent wet grip performance and winter performance on icy and snowy surfaces while maintaining sufficient wear resistance and tensile properties, as improvements in one property often deteriorate the other, and existing formulations have limitations in physical properties such as dispersibility and flexibility when used with inorganic fillers like silica.

Method used

A conjugated diene polymer with specific structural characteristics, including two or more polymer segments with controlled amounts of bonded aromatic vinyl monomer units and vinyl bonds, and a glass transition temperature within a predetermined range, is developed to enhance wet grip, winter performance, and abrasion resistance, along with a method for producing this polymer using continuous reactors and a coupling step with a nitrogen-containing modifying group.

Benefits of technology

The resulting rubber composition exhibits improved wet grip and winter performance, along with enhanced abrasion resistance and tensile properties, effectively balancing conflicting characteristics and overcoming limitations of previous formulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000007
    Figure JPOXMLDOC01-APPB-C000007
  • Figure JPOXMLDOC01-APPB-C000008
    Figure JPOXMLDOC01-APPB-C000008
  • Figure JPOXMLDOC01-APPB-C000009
    Figure JPOXMLDOC01-APPB-C000009
Patent Text Reader

Abstract

Provided is a conjugated diene polymer comprising two or more polymer segments, wherein: the absolute value (|X1-X2|) of the difference between the bonded aromatic vinyl monomer unit quantity X1 (mass%) of a first polymer segment and the bonded aromatic vinyl monomer unit quantity X2 (mass%) of a second polymer segment is not more than 5 mass%; the difference (Y2-Y1) between the vinyl bond amount Y1 (mol%) in a bonded conjugated diene of the first polymer segment and the vinyl bond amount Y2 (mol%) in a bonded conjugated diene of the second polymer segment is 15-50 mol%, and the estimated glass transition temperature (estimated Tg) of the conjugated diene polymer is -72 to -40°C.
Need to check novelty before this filing date? Find Prior Art

Description

Conjugated diene polymer and method for producing conjugated diene polymer

[0001] The present invention relates to a conjugated diene polymer and a method for producing a conjugated diene polymer.

[0002] One of the basic functions required of automobile tire treads is braking performance on road surfaces. With recent climate change, road surfaces can become wet due to sudden rainfall, or turn into icy snow due to sudden snowfall. In these environments, tires with excellent braking performance are required not only on dry roads, but also on icy, snowy, and wet roads. Furthermore, tires that meet these requirements are becoming increasingly popular with consumers, as they eliminate the need for seasonal tire changes.

[0003] Generally, wet grip performance, which is a characteristic required of tread rubber in terms of braking performance on wet roads, conflicts with winter performance, which is a characteristic required of rubber in terms of braking performance on icy and snowy surfaces. In other words, improving one of these characteristics tends to cause the other to deteriorate. Therefore, tire tread rubber is required to resolve this conflicting characteristic.

[0004] Furthermore, due to increasing fuel economy regulations for automobiles, there is an increasing demand for the use of resin for automobile components and for thinner tires in order to reduce the weight of automobiles. When attempting to thin tires, it is necessary to reduce the thickness of the tread portion, which makes up a large proportion of the entire tire and is in contact with the road surface, and this has led to a demand for rubber materials with even better abrasion resistance than before.

[0005] On the other hand, from the viewpoint of tire durability, rubber materials are also required to have good tensile properties. As described above, when multiple rubber types are used to improve both wet grip performance and winter performance, if the mutual affinity of these multiple rubber types is low, the mechanical strength of the rubber material tends to decrease, and therefore a rubber material that can satisfy these properties is required.

[0006] As a rubber material that meets the demands for improving various properties as described above, for example, a rubber composition containing a rubbery polymer and a reinforcing filler such as carbon black and silica is known. In such a rubber composition, attempts have been made to improve the dispersibility of the filler in the rubber composition and to improve various properties such as abrasion resistance by introducing a functional group having affinity or reactivity with the filler into the molecular terminal of the highly mobile rubbery polymer.

[0007] For example, Patent Documents 1 to 3 disclose rubber compositions containing silica and a modified conjugated diene polymer obtained by reacting an amino group-containing alkoxysilane with the active terminal of a conjugated diene polymer. Patent Document 4 discloses a rubber composition containing a low-vinyl modified conjugated diene polymer. Furthermore, Patent Document 5 discloses a rubber composition containing a conjugated diene polymer composition blended with multiple types of modified conjugated diene polymers.

[0008] Japanese Patent Application Laid-Open No. 2005-290355 Japanese Patent Application Laid-Open No. 11-189616 Japanese Patent Application Laid-Open No. 2003-171418 Japanese Patent No. 6512240 Japanese Patent Application Laid-Open No. 2021-143324

[0009] However, conventionally known rubber compositions, including those disclosed in Patent Documents 1 to 4, still have the problem that there is room for improvement in their physical properties. For example, rubber compositions containing conventional conjugated diene polymers have the problem that when wet grip performance is improved, winter performance is reduced and performance on icy and snowy surfaces is deteriorated, making it difficult to achieve both. Furthermore, when such rubber compositions are vulcanized, particularly when they are vulcanized with an inorganic filler such as silica, the dispersibility of the silica is reduced, flexibility is impaired, performance on icy and snowy surfaces is reduced, and abrasion resistance is also insufficient.

[0010] Furthermore, upon detailed investigation of the rubber composition described in Patent Document 5, it was found that the composition is suitable for designing tires that require wet grip performance, such as summer tires, but on the other hand, there is a problem in that there is still room for improvement in winter performance intended for use in lower temperature environments, such as all-season applications.

[0011] Therefore, an object of the present invention is to provide a conjugated diene polymer from which a rubber composition excellent in wet grip performance, winter performance, abrasion resistance and tensile properties can be obtained, and a method for producing a conjugated diene polymer.

[0012] As a result of intensive research conducted by the present inventors to solve the above problems, it was found that a rubber composition that achieves both wet grip performance and winter performance and is also excellent in abrasion resistance and tensile properties can be obtained by setting the absolute value of the difference in the amount of bound aromatic vinyl monomer units and the difference in the amount of vinyl bonds among multiple polymer segments constituting a conjugated diene-based polymer within a predetermined numerical range and setting the glass transition temperature (estimated Tg) estimated from the microstructure of the conjugated diene-based polymer within a predetermined numerical range, and thus the present invention was completed.

[0013] [1] A conjugated diene polymer having two or more polymer segments, wherein the amount of bound aromatic vinyl monomer units X of the first polymer segment is 1 (mass%) and the amount of bound aromatic vinyl monomer units X of the second polymer segment 2 (mass%) and the absolute value of the difference (|X 1 -X 2 |) is 5 mass% or less, and the vinyl bond amount Y in the bonded conjugated diene of the first polymer segment is 1 (mol%) and the vinyl bond amount Y in the bonded conjugated diene of the second polymer segment 2 (mol%) difference (Y 2 -Y 1) is 15 mol % or more and 50 mol % or less, and the conjugated diene polymer has an estimated glass transition temperature (estimated Tg) of -72°C or more and -40°C or less. [2] The conjugated diene polymer according to [1] above, wherein the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is 1.7 or more. [3] The conjugated diene polymer according to [1] above, wherein the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is 1.7 or more. 2 ) the mass ratio of the first polymer segment to the 1 ) ratio (R = r 1 / r 2 ) is 0.25 to 4. [4] The conjugated diene polymer according to any one of [1] to [3] above, having a weight average molecular weight Mw of 350,000 or more and 1,350,000 or less. [5] The conjugated diene polymer according to any one of [1] to [4] above, having a nitrogen-containing modifying group and a modification rate of 60% or more. [6] A method for producing a conjugated diene polymer according to any one of [1] to [5] above, comprising: a polymerization step (P1) of forming the first polymer segment in two or more continuous reactors; and a polymerization step (P2) of forming the second polymer segment at an end of the first polymer segment obtained in (P1), wherein a polar substance is additionally added in the polymerization step (P2). [7] A method for producing a conjugated diene polymer according to [6] above, wherein a conjugated diene compound is additionally added in the polymerization step (P2). [8] The method for producing a conjugated diene polymer according to [6] or [7] above, further comprising a coupling step of reacting the conjugated diene polymer with a coupling agent having a nitrogen atom-containing group after the polymerization step (P2). [9] The method for producing a conjugated diene polymer according to [7] or [8] above, further comprising the step of adjusting the amount of the conjugated diene compound added in the polymerization step (P2) to 15 mass % or more of the total amount of the conjugated diene compound added.

[0014] According to the present invention, a conjugated diene polymer can be provided from which a rubber composition can be obtained that exhibits excellent abrasion resistance and tensile properties, and that exhibits excellent wet grip performance and winter performance.

[0015] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0016] [Conjugated Diene Polymer] The conjugated diene polymer of the present embodiment contains conjugated diene monomer units, and preferably contains conjugated diene monomer units and aromatic vinyl monomer units.

[0017] The conjugated diene polymer of the present embodiment is a conjugated diene polymer having two or more polymer segments, and the amount of bound aromatic vinyl monomer units X of the first polymer segment is 1 (mass%) and the amount of bound aromatic vinyl monomer units X of the second polymer segment 2 (mass%) and the absolute value of the difference (|X 1 -X 2 The vinyl bond amount Y in the bonded conjugated diene of the first polymer segment is 5% by mass or less. 1 (mol %), and the vinyl bond amount Y in the bonded conjugated diene of the second polymer segment 2 (mol%) difference (Y 2 -Y 1 Furthermore, the conjugated diene polymer has an estimated glass transition temperature (estimated Tg) calculated from the microstructure of the conjugated diene polymer of -72°C or higher and -40°C or lower.

[0018] According to the above constitution, the conjugated diene polymer can be used to obtain a rubber composition that exhibits excellent abrasion resistance and tensile properties, and that exhibits excellent wet grip performance and winter performance.

[0019] (Conjugated Diene Compound) Examples of conjugated diene compounds that form conjugated diene monomer units include, but are not limited to, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-heptadiene. Among these, 1,3-butadiene and isoprene are preferred from the viewpoint of ease of industrial availability. These may be used alone or in combination of two or more. From the viewpoints of ease of availability and ease of structural control during polymer synthesis, the conjugated diene compound is preferably 1,3-butadiene or isoprene, and more preferably 1,3-butadiene.

[0020] (Aromatic Vinyl Compound) Examples of aromatic vinyl compounds that form aromatic vinyl monomer units include, but are not limited to, styrene, p-methylstyrene, α-methylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, and diphenylethylene. Among these, styrene is preferred from the viewpoint of ease of industrial availability. These compounds may be used alone or in combination of two or more. The aromatic vinyl compound is preferably styrene from the viewpoint of ease of availability and ease of structural control during polymer synthesis.

[0021] (Amount X of Bound Aromatic Vinyl Monomer Units) In this specification, the amount X (% by mass) of bound aromatic vinyl monomer units is the value of the mass fraction (% by mass) of bound aromatic vinyl monomer units relative to the total mass of the conjugated diene-based polymer or the polymer segment described below.

[0022] Here, the amount of bound aromatic vinyl monomer units can be calculated by measuring the ultraviolet absorption of the phenyl group possessed by the portion of the conjugated diene polymer derived from the aromatic vinyl compound (hereinafter referred to as "bound aromatic vinyl monomer units"). Furthermore, when the conjugated diene polymer is composed of bound aromatic vinyl monomer units and bound conjugated diene monomer units, the amount of bound conjugated diene monomer units can also be determined from the amount of bound aromatic vinyl monomer units obtained as described above. Specifically, it can be measured by the method described in the Examples below.

[0023] (Amount of vinyl bonds Y in bound conjugated diene) In this specification, the amount of vinyl bonds Y (mol %) in the bound conjugated diene is the molar fraction (mol %) of 1,2-bond units relative to the polymerization units derived from the conjugated diene contained in the conjugated diene-based polymer or the polymer segment described below.

[0024] When the conjugated diene polymer of the present embodiment is a copolymer of butadiene and styrene, the vinyl bond content in the bound conjugated diene can be obtained by determining the vinyl bond content (1,2-bond content) in the bound butadiene by the Hampton method (R.R. Hampton, Analytical Chemistry, 21, 923 (1949)). Specifically, it can be measured by the method described in the examples below.

[0025] (Microstructure) In this specification, the microstructure refers to a conjugated diene-based polymer comprising an aromatic vinyl compound and a conjugated diene compound, or a polymer composition including isomers in a polymer segment described later. In the conjugated diene-based polymer of this embodiment, the mass of the copolymer comprising styrene and butadiene is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more, based on the mass of the entire conjugated diene-based polymer.

[0026] (Content of Bound Aromatic Vinyl Monomer Unit Block) The conjugated diene polymer of this embodiment preferably has a small number of or no blocks in which four or more bound aromatic vinyl monomer units are linked (hereinafter, may be referred to as bound aromatic vinyl monomer unit blocks). When the conjugated diene polymer of this embodiment has a small number of or no bound aromatic vinyl monomer unit blocks, the conjugated diene polymer tends to be less likely to have two or more glass transition temperatures (Tg). When the conjugated diene polymer is a butadiene-styrene copolymer, the content of the bound aromatic vinyl monomer unit blocks in the conjugated diene polymer can be measured by a known method in which the conjugated diene polymer is decomposed by the Kolthoff method (the method described in I. M. KOLTHOFF, et al., J. Polym. Sci. 1, 429 (1946)) and the amount of polystyrene insoluble in methanol is analyzed. The content of the bound aromatic vinyl monomer unit block measured by such a method is preferably 1.0 mass% or less, more preferably 0.1 mass% or less, and even more preferably 0 mass% relative to the total amount of the conjugated diene polymer. By not including a bound aromatic vinyl monomer unit block in the conjugated diene copolymer or in the polymer segment described below, the conjugated diene polymer tends to exhibit continuous properties with temperature change. As a result, vulcanizates using the conjugated diene polymer tend to exhibit continuous changes over a wide temperature range and have excellent tensile strength.

[0027] (Method for Estimating Glass Transition Temperature of Polymer): Estimated Glass Transition Temperature (Estimated Tg) The glass transition temperature of the conjugated diene polymer of this embodiment can be estimated using the Gordon-Taylor equation (Gordon, M.; Taylor, J.S.J. Appl. Chem. 1952, 2, 493.), which is expanded to a system of two or more components according to the following formula (1):

[0028]

[0029] In the formula (1), the variable subscript i represents each component of the microstructure contained in the conjugated diene polymer, and Δα iis the difference in thermal expansion coefficient before and after the glass transition of the homopolymer of component i, w i is the mass ratio of component i in the conjugated diene polymer, Tg i is the glass transition temperature of the homopolymer of component i, ρ i is the density of the homopolymer of component i. Both literature values ​​and measured values ​​can be used. For example, when a conjugated diene polymer contains styrene, if one of the i's is a styrene component, Δα is calculated from the thermal expansion coefficient of polystyrene (J. BRANDRUP et al., Polymer Handbook, 3rd Group, (USA), John Wiley & Sons, Inc., 1966, VI-75). i = 3.6 x 10 -4 K -1 , Tg from the measured value of the glass transition temperature i = 105.3°C, and from the measured density value, ρ i = 1.02 g / cm 3 can be used.

[0030] For example, when the conjugated diene polymer is a butadiene-styrene copolymer, the amount of bound aromatic vinyl monomer units X all (mass%), and the vinyl bond amount Y in the bound conjugated diene all (mol%), and the thermal expansion coefficients (Δa i ), glass transition temperature (Tg i ), density (ρ i ) the estimated glass transition temperature (estimated Tg) can be calculated from the following formula (i):

[0031]

[0032] The amount of bound aromatic vinyl monomer units X relative to the denominator of the formula (i) all (mass%), vinyl bond amount Y in the bonded conjugated diene all Since the influence of the product value of (mol%) is very small, it can be approximated by the following formula (ii): Furthermore, the following formula (ii) can be approximated as the following formula (iii):

[0033]

[0034]

[0035] That is, when the conjugated diene polymer is a butadiene homopolymer or a butadiene-styrene copolymer, the glass transition temperature (estimated Tg) of the conjugated diene polymer can be estimated by the above formula (iii) from values ​​usually used in design.

[0036] As described above, the amount of bound aromatic vinyl monomer units X in the conjugated diene polymer of this embodiment all (mass%), vinyl bond amount Y in the bonded conjugated diene all The mass ratio of each microstructure component can be determined from the microstructure such as (mol%), and the glass transition temperature (estimated Tg) of the conjugated diene polymer can be calculated from the formula (1). That is, the formula (1) is expressed as the amount of bound aromatic vinyl monomer units X all (mass%), vinyl bond amount Y in the bonded conjugated diene all It is a measure of the change in the glass transition temperature of a conjugated diene polymer relative to the change in the molecular weight (mol%) of the polymer.

[0037] When the value of the formula (1) is small, the glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is small, and when the value is large, the glass transition temperature (Tg) is high. For example, when the formula (1) is −70, the glass transition temperature of the conjugated diene polymer is estimated to be −70° C., and when the formula (1) is −40, the glass transition temperature is estimated to be −40° C.

[0038] As described above, the value of formula (1) calculated from the microstructure of a polymer is generally an index of the glass transition temperature of a conjugated diene polymer. However, the present inventors have found that when the relaxation temperature of a conjugated diene polymer is broad, the viscoelasticity of the actual vulcanizate does not necessarily coincide with the viscoelasticity calculated from the estimated value of the glass transition temperature (estimated Tg) calculated from the microstructure using formula (1). Specifically, when the difference in the value of formula (1) between polymer segments (described below) is 33 or more, or when the mass ratio of the polymer segments (described below) is in the range of 0.67 to 1.5, the discrepancy between the glass transition temperature estimated from formula (1) and the measured glass transition temperature tends to become significant. Therefore, from the perspective of controlling the performance of a vulcanizate affected by the glass transition temperature, they have found that adjusting the estimated glass transition temperature (estimated Tg) using formula (1) calculated from the microstructure is more effective than adjusting the measured glass transition temperature of the conjugated diene polymer to a specific value. This is thought to be because DSC (differential scanning calorimetry) picks up small energy changes, and so the entire glass transition temperature is pulled up at the start of relaxation in the low Tg portion of the conjugated diene polymer, making the actually measured glass transition temperature lower than the estimated glass transition temperature. For example, it has been experimentally confirmed that even for conjugated diene polymers with the same microstructure overall, the glass transition temperatures measured by DSC can differ by as much as 2 to 5°C depending on the differences in the microstructure of each polymer segment.

[0039] The conjugated diene polymer of the present embodiment has a glass transition temperature (estimated Tg) estimated by the formula (1) that falls within the range of −72° C. or higher and −40° C. or lower, so that the glass transition temperature of the vulcanized product becomes an optimum value, and the polymer tends to have an excellent balance of wet grip performance, winter performance, and abrasion resistance.

[0040] In the conjugated diene polymer of this embodiment, the lower limit of the formula (1) is −72 or more, preferably −70 or more, and more preferably −68 or more. When the lower limit of the formula (1) is within the above range, the wet grip performance of the vulcanizate of the conjugated diene polymer of this embodiment can be improved. Furthermore, the upper limit of the value of the formula (1) is −40 or less, preferably −44 or less, and more preferably −50 or less. When the upper limit of the formula (1) is within the above range, the winter performance and abrasion resistance of the vulcanizate of the conjugated diene polymer of this embodiment can be improved. The formula (1) can be controlled to fall within the above-mentioned numerical range by adjusting the microstructure of the conjugated diene polymer. For example, when the conjugated diene polymer of this embodiment is a butadiene-styrene polymer, the bound styrene amount X of the conjugated diene polymer can be calculated from the formula (iii) all (mass%), vinyl bond amount Y in butadiene all By adjusting the (mol %), it is possible to control the content within the above-mentioned range.

[0041] (Polymer Segment) The conjugated diene polymer of this embodiment has two or more polymer segments. A polymer segment refers to a portion of a conjugated diene polymer composed of conjugated diene monomer units and aromatic vinyl monomer units, or composed of conjugated diene monomer units. The polymer segment is preferably composed of conjugated diene monomer units and aromatic vinyl monomer units. Furthermore, the conjugated diene polymer of this embodiment preferably has a small number or no blocks in which four or more linked aromatic vinyl monomer units are chained. The multiple polymer segments contained in the conjugated diene polymer of this embodiment have different microstructures. Each polymer segment may differ, for example, in the amount of linked aromatic vinyl monomer units or the amount of vinyl bonds in the linked conjugated diene, and each polymer segment can be distinguished by the method described in the examples described below.

[0042] The conjugated diene polymer of this embodiment has two or more polymer segments. By having two or more polymer segments, one conjugated diene polymer undergoes glass transition in multiple temperature ranges. While setting the microstructure of the conjugated diene polymer of this embodiment within an appropriate range, the amount of bound aromatic vinyl monomer units (X 1 , X 2 ) and the vinyl bond amount (Y 1 , Y 2 By controlling the difference in estimated glass transition temperatures of the polymer segments calculated by applying the formula (1) to the vulcanizate, within a certain range, the vulcanizate tends to exhibit excellent wet grip performance and winter performance.

[0043] Of the two or more polymer segments contained in the conjugated diene-based polymer of this embodiment, a polymer segment having an estimated glass transition temperature calculated by the above formula (1) that is 5°C or more lower than the average estimated glass transition temperature of the conjugated diene-based polymer of this embodiment is referred to as a "first polymer segment," and a polymer segment having an estimated glass transition temperature that is 5°C or more higher than the average estimated glass transition temperature of the conjugated diene-based polymer of this embodiment is referred to as a "second polymer segment." Although the first polymer segment and the second polymer segment may each contain multiple polymer segments, from the viewpoint of ease of production, it is preferable that each be composed of a single polymer segment. Furthermore, from the viewpoint of the balance between the wet grip performance and winter performance of a vulcanizate using the conjugated diene-based polymer of this embodiment, the proportion of the sum of the masses of the first polymer segment and the second polymer segment to the total mass of the conjugated diene-based polymer is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more.

[0044] Conventionally known continuously polymerized conjugated diene polymers are composed of a single polymer segment with a uniform microstructure and exhibit sharp glass transition behavior within a narrow temperature range. Generally, when winter performance is important, conjugated diene polymers with low glass transition temperatures are used to sufficiently increase flexibility at temperatures around −30 to −10°C. However, glass transition does not occur near 0°C, making energy absorption difficult, and thus wet grip performance tends to be poor. On the other hand, the conjugated diene polymer of the present embodiment exhibits a gentle glass transition behavior due to the multiple polymer segments each having a different glass transition temperature. Therefore, the polymer softens sufficiently at temperatures between −30 to −10°C, exhibiting good winter performance while increasing energy absorption near 0°C, and thus tending to exhibit excellent wet grip performance. The greater the difference in glass transition temperature between the two polymer segments constituting the conjugated diene polymer of the present embodiment, the gentler the glass transition behavior, making the above-mentioned tendency more pronounced. This tends to achieve both winter performance and wet grip performance.

[0045] In the conjugated diene polymer of this embodiment, in order to widen the difference in glass transition temperature between the polymer segments, it is preferable to increase the difference in the amount of aromatic vinyl monomer units between the first polymer segment and the second polymer segment and the difference in the amount of vinyl bonds in the linked conjugated diene. On the other hand, if the difference in the amount of aromatic vinyl monomer units between the two polymer segments becomes large, the compatibility of the two polymer segments tends to deteriorate, and the tensile strength of the vulcanized product tends to deteriorate. From this perspective, in order to obtain a vulcanized product with excellent tensile strength, it is effective to set the difference in the amount of aromatic vinyl monomer units between the two polymer segments within an appropriate range and increase the difference in the amount of vinyl bonds in the linked conjugated diene.

[0046] Amount X of aromatic vinyl monomer units in the first polymer segment 1 (mass%), and the amount of aromatic vinyl monomer units X of the second polymer segment 2The lower limit of the content (mass%) in each polymer segment is preferably 5 mass% or more, more preferably 7 mass% or more, and even more preferably 9 mass% or more, and the upper limit is preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 23 mass% or less, in each polymer segment.

[0047] Amount of vinyl bonds in the bonded conjugated diene of the first polymer segment Y 1 The lower limit of (mol%) is preferably 14 mol% or more, more preferably 16 mol% or more, and even more preferably 17 mol% or more. The upper limit is preferably 40 mol% or less, more preferably 35 mol% or less, even more preferably 30 mol% or less, and even more preferably 23 mol% or less. On the other hand, the vinyl bond amount Y in the bonded conjugated diene of the second polymer segment 2 The lower limit of (mol%) is preferably 40 mol% or more, more preferably 45 mol% or more, even more preferably 50 mol% or more, and even more preferably 55 mol% or more. The upper limit is preferably 65 mol% or less, more preferably 62 mol% or less, and even more preferably 61 mol% or less. The vinyl bond amount Y in the bonded conjugated diene of the polymer segment 1 , Y 2 may be within a range that is any combination of the above upper and lower limits.

[0048] The vinyl bond amount Y in the bonded conjugated diene of the first polymer segment of the conjugated diene-based polymer of this embodiment 1 (mol%) and the vinyl bond amount Y in the bonded conjugated diene of the second polymer segment 2 (mol%) difference (Y 2 -Y 1 ) is 15 mol% or more and 50 mol% or less, preferably 20 mol% or more and 45 mol% or less, and more preferably 25 mol% or more and 45 mol% or less. (Y 2 -Y 1 When the (Y) is 15 mol% or more, the vulcanizate tends to have an excellent balance between wet grip performance and winter performance. 2 -Y 1When the (Y) is 50 mol % or less, phase separation of the conjugated diene polymer is suppressed, and the vulcanizate thereof tends to have excellent tensile strength. 2 -Y 1 The value of (P1) can be measured by the method described in the Examples below, and can be controlled to fall within the above-mentioned range by adjusting the amount of the polar substance added in the polymerization steps (P1 and P2) described below.

[0049] The amount of bound aromatic vinyl monomer X in the first polymer segment of the conjugated diene polymer of this embodiment 1 (mass%) and the amount of bound aromatic vinyl monomer X of the second polymer segment 2 The absolute value of the difference (mass%) (|X 1 -X 2 (|X) is 5% by mass or less, preferably 3% by mass or less, and more preferably 2% by mass or less. 1 -X 2 When the ratio |) is 5 mass% or less, the distribution of aromatic vinyl monomer units becomes uniform, microphase separation of the conjugated diene polymer is suppressed, and the vulcanizate thereof tends to have even better tensile properties. The absolute value of the difference in the amount of bound aromatic vinyl monomer between polymer segments can be measured by the method described in the Examples below, and can be controlled to fall within the above-mentioned numerical range by adjusting the amount of aromatic vinyl monomer added in the polymerization step of each polymer segment.

[0050] In the conjugated diene polymer of this embodiment, the second polymer segment has an estimated glass transition temperature that is 5° C. or more higher than the average estimated glass transition temperature of the conjugated diene polymer, and therefore, the vinyl bond amount Y 2 (mol %) is the vinyl bond amount Y of the first polymer segment. 1The basic design concept is to set the bonded aromatic vinyl monomer amount to be higher than (mol%) and to ensure that there is no difference between the two polymer segments in terms of the amount of the bound aromatic vinyl monomer. In this embodiment, the difference in the absolute values ​​of the bonded aromatic vinyl monomer amounts of the two segments is set to 5% by mass or less in order to allow for manufacturing errors. Since the content of aromatic vinyl monomer units is also a factor that affects the estimated glass transition temperature, it is possible to design each polymer segment to have a different amount of bound aromatic vinyl monomer units. However, by reducing the difference in the amount of bound aromatic vinyl monomer units of the two polymer segments, the distribution of aromatic vinyl monomer units can be made uniform, as described above, and microphase separation can be suppressed. The estimated glass transition temperature of the polymer segment can be calculated using formula (1) in the same manner as for the conjugated diene polymer.

[0051] To the conjugated diene polymer of the present embodiment, a conjugated diene monomer unit may be added before the coupling step in order to increase the reactivity of the conjugated diene polymer with the coupling agent.

[0052] In the conjugated diene polymer of this embodiment, the polymer segments may be bonded to each other directly or via a coupling agent.

[0053] (Ratio R of Mass Ratio of First Polymer Segment to Mass Ratio of Second Polymer Segment) In the conjugated diene polymer of this embodiment, the first and second polymer segments preferably have a predetermined mass ratio. The mass ratio of the polymer segments is the mass ratio (r) of each polymer segment to the entire conjugated diene polymer. The mass ratios of the first and second polymer segments in the conjugated diene polymer of this embodiment are defined as the mass ratios of the polymer segments obtained in steps P1 and P2, which are polymerization steps for each polymer segment, to the total mass of the conjugated diene polymer. The first polymer segment mass ratio (r 1 ), and the second polymer segment mass ratio (r 2 ) ratio (R = r 1 / r 2) is preferably 0.25 to 4, more preferably 0.33 to 3, and even more preferably 0.4 to 2.4. When the lower limit of R is 0.25 or more, the fuel-saving performance during vulcanization tends to be excellent. When the upper limit of R is 4 or less, the processability of the vulcanized product tends to be excellent. R can be measured by the method described in the examples below, and can be controlled to fall within the above-mentioned range by adjusting conditions such as the polymerization time, polymerization temperature, amount of monomer added, and amount of vinyl bond in the polymerization step of each polymer segment in the production process of the conjugated diene polymer of this embodiment.

[0054] The method of introducing multiple polymer segments into the molecule of a conjugated diene polymer is carried out by using a continuous solution polymerization method in which multiple reactors are arranged in series, as described below, and sequentially adding a conjugated diene compound, an aromatic vinyl compound, a polar substance, and a solvent to each reactor. The sequentially added substances may be the same or different between reactors.

[0055] (Glass Transition Temperature) The glass transition temperature (Tg) of the conjugated diene polymer of this embodiment is preferably −72° C. or higher, more preferably −67° C. or higher. The glass transition temperature of the conjugated diene polymer of this embodiment is −40° C. or lower, more preferably −45° C. or lower. When the glass transition temperature satisfies the above range, the fuel-saving performance of the vulcanizate of the conjugated diene polymer of this embodiment tends to be even better. Furthermore, the conjugated diene polymer of this embodiment, whose estimated Tg of formula (1) satisfies the numerical range of −72° C. or higher and −40° C. or lower, basically has an actually measured glass transition temperature (Tg) within the above range. The glass transition temperature (Tg) may be within a range that arbitrarily combines the above upper and lower limits. The glass transition temperature of the conjugated diene polymer can be measured in accordance with ISO 22768:2006. More specifically, the glass transition temperature is determined by recording a DSC curve by differential scanning calorimetry (DSC) while increasing the temperature within a predetermined temperature range, and the inflection point of the DSC curve is taken as the glass transition temperature. Specifically, the glass transition temperature can be determined by the method described in the Examples below. Note that the conjugated diene polymer of this embodiment may contain plasticizing components such as resins and process oils described below, but these components must be removed in the DSC measurement to determine the glass transition temperature of the conjugated diene copolymer of this embodiment.

[0056] The glass transition temperature of a conjugated diene polymer varies depending on the amount of bound aromatic vinyl monomer units in the conjugated diene polymer and the amount of vinyl bonds in the bound conjugated diene. Specifically, the glass transition temperature increases by increasing the amount of bound aromatic vinyl monomer units and the amount of vinyl bonds in the bound conjugated diene, while the glass transition temperature decreases by decreasing the amount of bound aromatic vinyl monomer units and the amount of vinyl bonds in the bound conjugated diene. In the conjugated diene polymer of this embodiment, the measured glass transition temperature can be within a preferred range by setting the estimated Tg calculated by the formula (1) to be −72° C. or higher and −40° C. or lower.

[0057] (Weight Average Molecular Weight) The weight average molecular weight (Mw) of the conjugated diene polymer of the present embodiment measured by GPC measurement method is preferably 35×10 4More preferably, 40×10 4 or more, and more preferably 45×10 4 When the lower limit of the weight average molecular weight measured by GPC measurement method is within the above range, the vulcanizate tends to have excellent abrasion resistance. In addition, the weight average molecular weight is preferably 135×10 4 or less, more preferably 95 × 10 4 More preferably, it is 75×10 4 When the upper limit of the weight-average molecular weight is within the above range, the vulcanizate tends to have better filler dispersibility and better processability. The weight-average molecular weight may be within a range that combines any of the above upper and lower limits. The weight-average molecular weight of the conjugated diene polymer can be measured by GPC measurement, specifically, by the method described in the examples below.

[0058] (Number Average Molecular Weight) The number average molecular weight of the conjugated diene polymer of the present embodiment measured by GPC measurement is preferably 10 × 10 4 More preferably, 15×10 4 More preferably, it is 20×10 4 When the lower limit of the number average molecular weight measured by GPC measurement method is within the above range, the vulcanizate tends to have excellent abrasion resistance. In addition, the number average molecular weight is preferably 100 × 10 4 or less, and more preferably 70×10 4 or less, and more preferably 50×10 4 or less. When the upper limit of the number average molecular weight satisfies the above range, the dispersibility of the filler in the vulcanizate tends to be even better and the processability tends to be excellent. The number average molecular weight may be within a range that combines the above upper and lower limits. The number average molecular weight of the conjugated diene polymer can be measured by GPC measurement, and can be measured by the method described in the examples below.

[0059] The weight average molecular weight and number average molecular weight of the conjugated diene polymer can be controlled within the above numerical range by adjusting the ratio between the amount of polymerization initiator used and the amount of monomer used, and the type and amount of coupling agent used.

[0060] (Molecular Weight Distribution) The molecular weight distribution of the conjugated diene polymer of this embodiment is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn). The conjugated diene polymer of this embodiment preferably has a molecular weight distribution of 1.7 or more. A conjugated diene polymer with a molecular weight distribution in this range tends to have better processability when vulcanized. The molecular weight distribution of the conjugated diene polymer of this embodiment is more preferably 1.75 or more, even more preferably 1.8 or more. It is also more preferably 2.4 or less, even more preferably 2.2 or less.

[0061] (Modification Ratio) The conjugated diene polymer of this embodiment preferably has a nitrogen-containing modifying group. In this specification, the term "modification ratio" refers to the mass content (in %) of a modified conjugated diene polymer component having a specific functional group in the polymer molecule that has affinity or binding reactivity with a filler relative to the total amount of the conjugated diene polymer mixture, when a conjugated diene polymer is modified with a nitrogen-containing modifying agent to obtain a mixture of a conjugated diene polymer and an unmodified conjugated diene polymer. Therefore, when the specific functional group contains a nitrogen atom, the modification ratio refers to the mass ratio (%) of the nitrogen-containing modified conjugated diene polymer relative to the total amount of the conjugated diene polymer mixture. In this specification, the term "modified conjugated diene polymer" refers to a modified conjugated diene polymer and a mixture of a modified conjugated diene polymer and an unmodified conjugated diene polymer. For example, in the case where a conjugated diene polymer containing a modified conjugated diene polymer is obtained by reacting a nitrogen atom-containing modifying agent with the terminal end of a conjugated diene polymer, the modification rate is the mass ratio of the modified conjugated diene polymer having a nitrogen atom-containing functional group resulting from the nitrogen atom-containing modifying agent to the total amount of the modified conjugated diene polymer.

[0062] The modification rate can be measured by chromatography, which can separate functional group-containing modified components from unmodified components. Examples of methods using chromatography include a method using a gel permeation chromatography column packed with a polar substance such as silica that adsorbs specific functional groups, and quantifying the unadsorbed components using an internal standard for comparison. More specifically, the modification rate can be obtained by measuring the amount of adsorption to the silica column from the difference between a chromatogram measured on a polystyrene-based gel column and a chromatogram measured on a silica-based column for a sample solution containing a sample and a low-molecular-weight internal standard polystyrene. More specifically, the modification rate can be measured by the method described in the Examples.

[0063] In the conjugated diene polymer of this embodiment, the modification rate can be controlled by adjusting the amount of modifier added and the reaction method. For example, the above modification rate can be achieved by combining a method of polymerization using an organolithium compound having at least one nitrogen atom in the molecule described below as a polymerization initiator, a method of copolymerizing a monomer having at least one nitrogen atom in the molecule, and a method of using a modifier having a structural formula described below, and controlling the polymerization conditions.

[0064] From the viewpoint of fuel-saving performance of the vulcanizate, the conjugated diene polymer of the present embodiment preferably has a modification rate of 60% or more, more preferably 65% ​​or more, and even more preferably 70% or more.

[0065] [Method for Producing Conjugated Diene Polymer] The method for producing a modified conjugated diene polymer of this embodiment includes: a polymerization step (P1) of forming a first polymer segment in two or more continuous reactors; and a polymerization step (P2) of forming the second polymer segment at an end of the first polymer segment obtained in the polymerization step (P1); and a step of additionally adding a polar substance in the polymerization step (P2).

[0066] (Polymerization Initiator) A polymerization initiator is preferably used in the polymerization step (P1). It is preferable not to use a polymerization initiator in the polymerization step (P2). At least an organic monolithium compound can be used as the polymerization initiator. Examples of organic monolithium compounds include, but are not limited to, low molecular weight compounds and solubilized oligomeric organic monolithium compounds. Examples of organic monolithium compounds include compounds having a carbon-lithium bond, a nitrogen-lithium bond, and a tin-lithium bond in the bonding mode between the organic group and the lithium. The amount of the organic monolithium compound used as the polymerization initiator is preferably determined based on the target molecular weight of the conjugated diene polymer or modified conjugated diene polymer. The amount of the monomer, such as a conjugated diene compound, used relative to the amount of the polymerization initiator is related to the degree of polymerization. That is, it tends to be related to the number-average molecular weight and the weight-average molecular weight. Therefore, to increase the molecular weight of the conjugated diene polymer, it is advisable to decrease the amount of the polymerization initiator used, while to decrease the molecular weight, it is advisable to increase the amount of the polymerization initiator used.

[0067] When introducing nitrogen atoms into a conjugated diene polymer using a polymerization initiator, the organic monolithium compound is preferably an alkyllithium compound having a substituted amino group or a dialkylaminolithium compound, from the viewpoint that it can be used as one method for introducing nitrogen atoms into a conjugated diene polymer. In this case, a conjugated diene polymer having a nitrogen atom consisting of an amino group at the polymerization initiation terminal is obtained. The substituted amino group is an amino group that does not have an active hydrogen or has a structure in which the active hydrogen is protected. Examples of alkyllithium compounds having an amino group without an active hydrogen include, but are not limited to, 3-dimethylaminopropyllithium, 3-diethylaminopropyllithium, 4-(methylpropylamino)butyllithium, and 4-hexamethyleneiminobutyllithium. Examples of alkyllithium compounds having an amino group with a structure in which the active hydrogen is protected include, but are not limited to, 3-bistrimethylsilylaminopropyllithium and 4-trimethylsilylmethylaminobutyllithium. Examples of dialkylaminolithiums include, but are not limited to, lithium dimethylamide, lithium diethylamide, lithium dipropylamide, lithium dibutylamide, lithium di-n-hexylamide, lithium diheptylamide, lithium diisopropylamide, lithium dioctylamide, lithium-di-2-ethylhexylamide, lithium didecylamide, lithium ethylpropylamide, lithium ethylbutylamide, lithium ethylbenzylamide, lithium methylphenethylamide, lithium hexamethyleneimide, lithium pyrrolidide, lithium piperidide, lithium heptamethyleneimide, lithium morpholide, 1-lithioazacyclooctane, 6-lithio-1,3,3-trimethyl-6-azabicyclo[3.2.1]octane, and 1-lithio-1,2,3,6-tetrahydropyridine. These organomonolithium compounds having a substituted amino group can also be used as solubilized oligomeric organomonolithium compounds by reacting them with a small amount of a polymerizable monomer, such as 1,3-butadiene, isoprene, or styrene.

[0068] The polymerization initiator may be produced by reacting an aromatic vinyl compound and / or a conjugated diene compound having a substituted amino group with an organomonolithium compound, or may be capable of introducing a functional group into one end of a polymer chain. The organomonolithium compound is preferably an alkyllithium compound from the viewpoints of industrial availability and ease of control of the polymerization reaction. In this case, a conjugated diene polymer having an alkyl group at the polymerization initiation end is obtained. Examples of the alkyllithium compound include, but are not limited to, n-butyllithium, sec-butyllithium, tert-butyllithium, n-hexyllithium, benzyllithium, phenyllithium, and stilbenelithium. Examples of the alkyllithium compound include n-butyllithium and sec-butyllithium from the viewpoints of industrial availability and ease of control of the polymerization reaction. These organomonolithium compounds may be used alone or in combination of two or more. Furthermore, they may be used in combination with other organometallic compounds. Examples of the other organometallic compounds include alkaline earth metal compounds, other alkali metal compounds, and other organometallic compounds. Examples of alkaline earth metal compounds include, but are not limited to, organomagnesium compounds, organocalcium compounds, and organostrontium compounds. Also included are alkaline earth metal alkoxides, sulfonates, carbonates, and amides. Examples of organomagnesium compounds include dibutylmagnesium and ethylbutylmagnesium. Other organometallic compounds include organoaluminum compounds.

[0069] In the method for producing a conjugated diene polymer of this embodiment, a coupling step described below may be carried out after the polymerization step described above. The weight-average molecular weight of the conjugated diene polymer before the coupling step is controlled by the amount of polymerization initiator used relative to the conjugated diene compound and aromatic vinyl compound, and the weight-average molecular weight of the conjugated diene polymer tends to decrease as the amount of polymerization initiator used decreases. The amount of polymerization initiator used is preferably 0.15 mol or more and 1.5 mol or less, assuming that the total mass of the conjugated diene compound and aromatic vinyl compound used is 100 kg.

[0070] (Polar Substance) In the method for producing a conjugated diene polymer of this embodiment, a polar substance is added in the polymerization step (P2) for forming the second polymer segment. The polar substance can randomly copolymerize an aromatic vinyl compound with a conjugated diene compound, and tends to be usable as a vinylating agent for controlling the microstructure of the conjugated diene portion. It also tends to be effective in accelerating the polymerization reaction.

[0071] Examples of polar substances include, but are not limited to, ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-oxolanyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidinoethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butylate, sodium tert-butylate, and sodium amylate; and phosphine compounds such as triphenylphosphine. These polar substances may be used alone or in combination of two or more.

[0072] The amount of polar substance used is not particularly limited and can be selected depending on the purpose, but is preferably 0.01 mol or more and 100 mol or less per mol of the polymerization initiator used in the polymerization step.

[0073] Such polar substances (vinylating agents) can be used in an appropriate amount depending on the desired vinyl bond content as an adjuster for the microstructure of the conjugated diene portion of the conjugated diene polymer. Many polar substances also exhibit an effective randomizing effect in the copolymerization of a conjugated diene compound and an aromatic vinyl compound, and tend to be able to adjust the randomness of the aromatic vinyl monomer units and the conjugated diene monomer units in each polymer segment. A method for randomizing the conjugated diene monomer units and the aromatic vinyl monomer units, as described in JP-A-59-140211, for example, may involve initiating a copolymerization reaction with all of the styrene and a portion of the 1,3-butadiene, and then intermittently adding the remaining 1,3-butadiene during the copolymerization reaction. The 1,3-butadiene added here is added to adjust the randomness and does not necessarily form a polymer segment.

[0074] (Polymerization Step) In the method for producing a conjugated diene polymer of this embodiment, the polymerization step is carried out in a continuous reactor in which two or more reactors are connected in series, and a polymerization step (P1) for obtaining a first polymer segment and a polymerization step (P2) for obtaining a second polymer segment are carried out. The polymerization steps (P1) and (P2) can each be carried out using one or two or more connected reactors. The reactor may be a tank type or a tubular type equipped with a stirrer. It is not essential that the polymerization steps (P1) and (P2) be assigned to each reactor; for example, the polymerization step (P2) may be set to start downstream of the first reactor. Each reactor may have a temperature control function.

[0075] (Solid Amount) In the method for producing a conjugated diene polymer according to the present embodiment, the target conjugated diene polymer can be recovered in a predetermined solid amount. In this specification, the solid amount refers to the mass of the conjugated diene polymer recovered per unit time at a measurement point. The mass of the conjugated diene polymer includes only the polymer that has reacted with the polymerization initiator and been polymerized, and does not include the masses of the unreacted conjugated diene compound, aromatic vinyl compound, solvent, etc.

[0076] (Conversion Rate) In the method for producing a conjugated diene polymer according to the present embodiment, the "conversion rate" is defined as the mass of the conjugated diene polymer resulting from the complete reaction at the time of measurement out of the total mass of the conjugated diene compound and the aromatic vinyl compound. That is, it is calculated by the following formula (2) using the solid content.

[0077]

[0078] Furthermore, the conversion rates of the conjugated diene compound and the aromatic vinyl compound can be calculated by the following formulas (3) and (4) using the amount of bound conjugated diene monomer units and the amount of bound aromatic vinyl monomer units in the solid content obtained by the solid content measurement.

[0079]

[0080] The denominator in the calculation of the conversion rate is the total mass of the monomers added throughout the polymerization steps (P1, P2). Therefore, the conversion rate at the end of P1 will not be 100% even if all the monomers added up to that point have reacted.

[0081] From the viewpoint of controlling the physical properties of the conjugated diene polymer of this embodiment, it is preferable that the conversion rate is 95% or more by the end of the polymerization step. That is, the conversion rate may be controlled to 95% or more at the end of the polymerization step (P2), and the conversion rate in the polymerization step (P1) may be less than this. When the conversion rate is in the above range, the amount of bound aromatic vinyl monomer units X of the conjugated diene polymer can be controlled. all can be controlled by the ratio of the total amount of the conjugated diene compound to the total amount of the aromatic vinyl compound added during the polymerization step, which makes it easy to control the structure.

[0082] In the conjugated diene-based production method of this embodiment, a first polymer segment is obtained in the polymerization step (P1), and in this polymerization step (P1), it is preferable that the reactor has a raw material supply section that continuously supplies a conjugated diene compound, an aromatic vinyl compound, an inert solvent, a polymerization initiator, and a polar substance from one end thereof, and a discharge section that continuously discharges a polymer solution from the end opposite to the raw material supply section.

[0083] The conjugated diene polymer solution after the polymerization step (P1) is continuously distilled from the reactor and sent to the next step, for example, in a preferred embodiment to the polymerization step (P2) of the second polymer segment described below.

[0084] The polymerization step (P2) for obtaining the second polymer segment uses one or two or more connected reactors, as in the polymerization step (P1). At this time, a conjugated diene compound, an aromatic vinyl compound, an inert solvent, a polar substance, etc. are newly added to the middle of the reactor or to the piping connecting this step with the previous step, thereby introducing a second polymer segment having a higher vinyl bond content in the bound conjugated diene than that synthesized in the previous polymerization step into the end of the first polymer segment. This allows the formation of a second polymer segment having a Tg higher than that of the first polymer segment.

[0085] The second polymer segment has a higher vinyl bond amount Y than the first polymer segment. 2 (mol %), conditions are set in the polymerization step (P2) for forming the second polymer segment so that the vinyl bond content of the polymer is increased. In the polymerization step (P2), one or more polar substances are additionally added. The addition of the polar substance increases the vinyl bond content in the bound conjugated diene of the second polymer segment compared to the first polymer segment, and increases the difference in the vinyl bond content in the bound diene of the first polymer segment and the second polymer segment.

[0086] The amount of polar substance added in the polymerization step, in total, of the polar substance added in the polymerization step (P1) and the polymerization step (P2) is preferably 0.01 mol to 100 mol per mol of polymerization initiator. Within the above range, the amount of each substance added can be selected to control the difference in the amount of vinyl bonds in the bonded conjugated diene of the first polymer segment and the second polymer segment. The distribution of the polar substance added in the polymerization steps (P1) and (P2) varies depending on various factors such as the type of polar substance, polymerization temperature, and reactor shape, and is not particularly limited. However, for example, it is preferred that the concentration of the polar substance in the polymerization step (P2) be 3 to 20 times that of the polymerization step (P1).

[0087] The conjugated diene polymer solution after the polymerization step (P2) is continuously distilled from the reactor and sent to the next step, which may be, for example, the coupling step described below.

[0088] In the conjugated diene polymer of this embodiment, the difference in the amount of bound aromatic vinyl monomer units between the first polymer segment and the second polymer segment (X 1 -X 2 In order to make the absolute value of the ratio (P1 / P2) of the aromatic vinyl compound to the total aromatic vinyl compound (AVC) of the first polymer segment smaller than that of the second polymer segment, the conjugated diene compound and the aromatic vinyl compound must react in similar ratios in the polymerization step (P1) and the polymerization step (P2). To achieve this, it is preferable to reduce the difference in the conversion rates of the conjugated diene compound and the aromatic vinyl compound in the polymerization step (P1). For example, if the conversion rate of the aromatic vinyl compound is lower than that of the conjugated diene compound, the amount of bound aromatic vinyl monomer units in the first polymer segment decreases, and instead, a large amount of aromatic vinyl compound flows into the polymerization step (P2), widening the difference in the amount of bound aromatic vinyl monomer units between the first polymer segment and the second polymer segment. On the other hand, if the absolute value of the difference in the conversion rates between the first polymer segment and the second polymer segment is small, the first polymer segment and the second polymer segment both contain aromatic vinyl monomer units in the same ratio, and therefore the difference in the amount of bound aromatic vinyl monomer units becomes small. The difference in conversion rate between the conjugated diene compound and the aromatic vinyl compound is preferably less than 10% by mass, more preferably less than 8% by mass, and even more preferably less than 6% by mass. Addition of a polar substance is expected to have the effect of increasing the reaction rate of the aromatic vinyl compound, so it is possible to reduce the difference in conversion rate between the conjugated diene compound and the aromatic vinyl compound by increasing the amount of polar substance added. Meanwhile, polar substances generally also act as vinylating agents, and increasing the amount added tends to increase the amount of vinyl bonds in the resulting segments. Therefore, although the amount of polar substance is one variable for controlling the conversion rate, it is difficult to select it when designing to control the amount of vinyl bonds. Rather than controlling the conversion rate by the amount of polar substance added, it is preferable to adjust the amount of monomer supplied to each segment after setting the amount of polar substance added and the polymerization temperature.

[0089] In order to reduce the difference in conversion rate between the conjugated diene compound and the aromatic vinyl compound, it is effective to add the conjugated diene compound and aromatic vinyl compound to be added in the polymerization step in portions in the polymerization step (P1) and the polymerization step (P2). By reducing the amount of either monomer with a large reaction rate constant in the polymerization step (P1), a decrease in the reaction rate due to raw material depletion can be induced, and the conversion rate at the end of the polymerization step (P1) can be made uniform. In order to control the conversion rate, if there is any compound whose amount added in the polymerization step (P1) is insufficient compared to the total amount that should be added due to the divided addition of the monomer, the shortfall is added in the polymerization step (P2). As mentioned above, the conversion rate at the end of the polymerization step is preferably 95% or more, so that the amount of bound aromatic vinyl monomer units X of the conjugated diene polymer naturally increases. all is approximately equal to the ratio of (aromatic vinyl compound) to (conjugated diene compound + aromatic vinyl compound). This value is the amount of bound aromatic vinyl monomer units X of the first polymer segment synthesized in the polymerization step (P1). 1 is roughly equal to. For example, when a typical copolymerization reaction is carried out using normal hexane as a solvent and 1,3-butadiene and styrene as the polymerization monomers of a conjugated diene compound and an aromatic vinyl compound, respectively, the polymerization reaction rate of the conjugated diene compound is higher than that of the aromatic vinyl compound. Therefore, the conversion rate of the conjugated diene compound tends to be higher than that of the aromatic vinyl compound. In order to reduce the difference in conversion rate between the two compounds, when the conversion rates of the conjugated diene compound and the aromatic vinyl compound expected when polymerization is completed in step P1 alone are A and B, respectively, the conjugated diene compound is added in step P1 in accordance with the ratio obtained by dividing B by A, and the remaining amount is added additionally in step P2, thereby reducing the difference in conversion rate between the conjugated diene compound and the aromatic vinyl compound.

[0090] The amount of the conjugated diene compound added in the polymerization step (P2) is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, of the total amount of the conjugated diene compound added. When the amount added in the polymerization step (P2) is 15% by mass or more of the total amount of the conjugated diene compound added, the amount of bound aromatic vinyl monomer units X 1 (mass%) and the amount of bound aromatic vinyl monomer units X of the second polymer segment 2 (mass%) and the difference (X 1 -X 2 ) is 5 mass% or less, and the mass ratio (r 2 ) the mass ratio of the first polymer segment (r 1 ) ratio (R = r 1 / r 2 ) tends to be in the range of 0.25 to 4.00.

[0091] In the conjugated diene polymer of this embodiment, the mass ratio of the first polymer segment (r 1 ) and the mass ratio of the second polymer segment (r 2 ) and the ratio (R = r 1 / r 2 ), can be controlled by the ratio of the conjugated diene compound and the aromatic vinyl compound added in the polymerization step (P2). By reducing the ratio of the conjugated diene compound and the aromatic vinyl compound added in the polymerization step (P2), the conversion rates of the components in the polymerization step (P1) increase, and R increases. At this time, it is preferable to control so that the difference between the conversion rate of the conjugated diene compound and the conversion rate of the aromatic vinyl compound is small.

[0092] From the viewpoint of reaction controllability, it is preferable that the conversion rate is high in each polymerization step. However, the R may be controlled by supplying the unreacted conjugated diene compound and / or aromatic vinyl compound in the previous polymerization step to the next step.

[0093] The production of the conjugated diene-based polymer of the present embodiment may include a predetermined step before or after the polymerization step (P1) or before or after the polymerization step (P2). For example, a step of synthesizing a polymer different from the first polymer segment or the second polymer segment may be included.

[0094] The polymerization temperature in the polymerization step of the conjugated diene polymer of this embodiment is preferably a temperature at which living anionic polymerization proceeds, and from the viewpoint of productivity, is more preferably 0°C or higher, and even more preferably 120°C or lower. By keeping the temperature in this range, it tends to be possible to ensure a sufficient amount of the modifying agent reacting with the active terminals after the polymerization is completed. Even more preferably, it is 50°C or higher and 100°C or lower.

[0095] In the production of the conjugated diene polymer of this embodiment, a high molecular weight distribution can be obtained by reducing the height (L) / diameter (D) of the tank reactor. A smaller L / D ratio increases the residence time distribution in the reactor, which increases the variation in reaction time for each polymerization initiator molecule and widens the molecular weight distribution.

[0096] (Coupling Step) In the method for producing a conjugated diene polymer of this embodiment, a step of coupling the active terminals of the conjugated diene polymer obtained through the polymer segment polymerization step using a coupling agent, for example, a trifunctional or higher functional reactive compound, and / or a step of modifying the active terminals using a modifying agent having a nitrogen atom-containing group (preferably, a coupling agent having a nitrogen atom-containing group) may be carried out. Hereinafter, the coupling step and / or the modification step are referred to as the coupling step. In the coupling step, one active terminal of the conjugated diene polymer is modified with the coupling agent or the modifying agent having a nitrogen atom to obtain a modified conjugated diene polymer.

[0097] <Coupling Agent> In the method for producing a conjugated diene polymer of the present embodiment, the coupling agent used in the coupling step may be a reactive compound having any structure as long as it is a tri- or higher functional compound, but is preferably a tri- or higher functional compound having a silicon atom.

[0098] Examples of the tri- or higher functional reactive compound having a silicon atom include, but are not limited to, halogenated silane compounds, epoxy silane compounds, vinylated silane compounds, alkoxy silane compounds, and alkoxy silane compounds containing a nitrogen-containing group.

[0099] Examples of halogenated silane compounds that serve as coupling agents include, but are not limited to, methyltrichlorosilane, tetrachlorosilane, tris(trimethylsiloxy)chlorosilane, tris(dimethylamino)chlorosilane, hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,2-bis(methyldichlorosilyl)ethane, 1,4-bis(trichlorosilyl)butane, and 1,4-bis(methyldichlorosilyl)butane.

[0100] Examples of the epoxidized silane compound that serves as a coupling agent include, but are not limited to, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and epoxy-modified silicone.

[0101] <Modifying Agent Having Nitrogen Atom-Containing Group> Examples of the modifying agent having a nitrogen atom include, but are not limited to, an isocyanate compound, an isothiocyanate compound, an isocyanuric acid derivative, a nitrogen atom group-containing carbonyl compound, a nitrogen atom group-containing vinyl compound, and a nitrogen atom group-containing epoxy compound.

[0102] The modifying agent having a nitrogen atom-containing group is preferably an amine compound having no active hydrogen, and examples thereof include tertiary amine compounds, protected amine compounds in which the active hydrogen is substituted with a protecting group, imine compounds represented by the general formula -N=C, and alkoxysilane compounds bonded to the nitrogen atom-containing group.

[0103] Examples of the isocyanate compound that is a modifying agent having a nitrogen atom-containing group include, but are not limited to, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate (C-MDI), phenyl isocyanate, isophorone diisocyanate, hexamethylene diisocyanate, butyl isocyanate, and 1,3,5-benzene triisocyanate.

[0104] Examples of isocyanuric acid derivatives that are modifying agents having a nitrogen atom-containing group include, but are not limited to, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-tris(3-triethoxysilylpropyl)isocyanurate, 1,3,5-tri(oxiran-2-yl)-1,3,5-triazinane-2,4,6-trione, 1,3,5-tris(isocyanatomethyl)-1,3,5-triazinane-2,4,6-trione, and 1,3,5-trivinyl-1,3,5-triazinane-2,4,6-trione.

[0105] Examples of carbonyl compounds that are modifying agents having a nitrogen atom-containing group include, but are not limited to, 1,3-dimethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 1-methyl-3-(2-methoxyethyl)-2-imidazolidinone, N-methyl-2-pyrrolidone, N-methyl-2-piperidone, N-methyl-2-quinolone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, methyl methyl-4-pyridyl ketone, propyl-2-pyridyl ketone, di-4-pyridyl ketone, 2-benzoylpyridine, N,N,N',N'-tetramethylurea, N,N-dimethyl-N',N'-diphenylurea, N,N-methyl diethylcarbamate, N,N-diethylacetamide, N,N-dimethyl-N',N'-dimethylaminoacetamide, N,N-dimethylpicolinic acid amide, and N,N-dimethylisonicotinic acid amide.

[0106] Examples of vinyl compounds that are modifying agents having a nitrogen atom-containing group include, but are not limited to, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methylmaleimide, N-methylphthalimide, N,N-bistrimethylsilyl acrylamide, morpholinoacrylamide, 3-(2-dimethylaminoethyl)styrene, (dimethylamino)dimethyl-4-vinylphenylsilane, 4,4'-vinylidenebis(N,N-dimethylaniline), 4,4'-vinylidenebis(N,N-diethylaniline), 1,1-bis(4-morpholinophenyl)ethylene, and 1-phenyl-1-(4-N,N-dimethylaminophenyl)ethylene.

[0107] Examples of epoxy compounds that are modifiers having a nitrogen atom-containing group include, but are not limited to, hydrocarbon compounds containing an epoxy group bonded to an amino group, and may further include an epoxy group bonded to an ether group. Examples of such epoxy compounds include, but are not limited to, epoxy compounds represented by the following general formula (a):

[0108]

[0109] In the formula (a), R is a divalent or higher organic group having at least one polar group selected from a divalent or higher hydrocarbon group, or a polar group having oxygen such as an ether, epoxy, or ketone, a polar group having sulfur such as a thioether or thioketone, or a polar group having nitrogen such as a tertiary amino group or an imino group.

[0110] The divalent or higher valent hydrocarbon group is a saturated or unsaturated hydrocarbon group which may be linear, branched, or cyclic, and includes an alkylene group, an alkenylene group, a phenylene group, etc. Preferably, it is a hydrocarbon group having 1 to 20 carbon atoms. Examples include methylene, ethylene, butylene, cyclohexylene, 1,3-bis(methylene)-cyclohexane, 1,3-bis(ethylene)-cyclohexane, o-, m-, and p-phenylene, m- and p-xylene, and bis(phenylene)-methane groups.

[0111] In the formula (a), R 1 , R 4is a hydrocarbon group having 1 to 10 carbon atoms, and R 1 , R 4 may be the same or different. 2 , R 5 is hydrogen or a hydrocarbon group having 1 to 10 carbon atoms, and R 2 , R 5 may be the same or different. 3 R is a hydrocarbon group having 1 to 10 carbon atoms or a structure of the following formula (a1): 1 , R 2 , R 3 may be bonded to each other to form a cyclic structure. 3 When R is a hydrocarbon group, it may be bonded to R to form a cyclic structure. 3 In the formula (a), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.

[0112]

[0113] In the formula (a1), R 1 , R 2 is R in the formula (a). 1 , R 2 is defined similarly to R 1 , R 2 may be the same or different from each other.

[0114] The epoxy compound, which is a modifying agent having a nitrogen atom-containing group, is preferably one having an epoxy group-containing hydrocarbon group, more preferably one having a glycidyl group-containing hydrocarbon group.

[0115] The epoxy group-containing hydrocarbon group bonded to an amino group or an ether group is not particularly limited, but examples thereof include a glycidylamino group, a diglycidylamino group, and a glycidoxy group. A more preferred molecular structure is an epoxy group-containing compound having a glycidylamino group or a diglycidylamino group, and a glycidoxy group, respectively, and examples thereof include compounds represented by the following general formula (a2):

[0116]

[0117] In the formula (a2), R is defined as R in the formula (a), 6 is a hydrocarbon group having 1 to 10 carbon atoms or a structure of the following formula (a3): 6 When R is a hydrocarbon group, it may be bonded to R to form a cyclic structure. In this case, R 6 In formula (a2), n is an integer of 1 or more, and m is 0 or an integer of 1 or more.

[0118]

[0119] As the epoxy compound which is a modifying agent having a nitrogen atom-containing group, a compound having one or more diglycidylamino groups and one or more glycidoxy groups in the molecule is particularly preferred.

[0120] The epoxy compound used as the modifying agent having a nitrogen atom-containing group is not limited to the following, but examples thereof include N,N-diglycidyl-4-glycidoxyaniline, 1-N,N-diglycidylaminomethyl-4-glycidoxy-cyclohexane, 4-(4-glycidoxyphenyl)-(N,N-diglycidyl)aniline, 4-(4-glycidoxyphenoxy)-(N,N-diglycidyl)aniline, 4-(4-glycidoxybenzyl)-(N,N-diglycidyl)aniline, 4-(N,N'-diglycidyl-2-piperazinyl)-glycidoxybenzene, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m- Examples thereof include xylylenediamine, 4,4-methylene-bis(N,N-diglycidylaniline), 1,4-bis(N,N-diglycidylamino)cyclohexane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, 4,4'-bis(diglycidylamino)benzophenone, 4-(4-glycidylpiperazinyl)-(N,N-diglycidyl)aniline, 2-[2-(N,N-diglycidylamino)ethyl]-1-glycidylpyrrolidine, N,N-diglycidylaniline, 4,4'-diglycidyl-dibenzylmethylamine, N,N-diglycidylaniline, N,N-diglycidylorthotoluidine, and N,N-diglycidylaminomethylcyclohexane. Of these, particularly preferred are N,N-diglycidyl-4-glycidoxyaniline and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0121] From the viewpoint of effectively and reliably achieving the effects of this embodiment, the modifying agent is preferably an alkoxysilane compound having a nitrogen atom-containing group.Such modifiers include, but are not limited to, 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-diethylaminopropyltriethoxysilane, 3-morpholinopropyltrimethoxysilane, 3-piperidinopropyltriethoxysilane, 3-hexamethyleneiminopropylmethyldiethoxysilane, 3-(4-methyl-1-piperazino)propyltriethoxysilane, 1-[3-(triethoxysilyl)propyl]-3-methylhexahydropyrimidine, 3-(4-trimethylsilyl) 3-(3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyl)trimethoxysilane, 3-(3-(3-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 3-dimethylamino-2-(dimethylaminomethyl)propyltrimethoxysilane, bis(3-dimethoxymethylsilylpropyl)-N-methylamine, bis(3-trimethoxysilylpropyl)-N-methylamine, bis(3-triethoxysilylpropyl)methylamine, tris(trimethoxysilyl)amine, Tris(3-trimethoxysilylpropyl)amine, N,N,N',N'-tetra(3-trimethoxysilylpropyl)ethylenediamine, 3-isocyanatopropyltrimethoxysilane, 3-cyanopropyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(4-trimethoxysilylpropyl ... 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-8-(4-methylpiperazinyl)methyl-1,6-dioxa-2-silacyclooctane, 2,2-dimethoxy-8-(N,N-diethylamino)methyl-1,6-dioxa-2-silacyclooctane, and the like.

[0122] Particularly preferred examples of the alkoxysilane compound having a nitrogen atom-containing group include the following: tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-tripropoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (also known as "N,N,N',N'-tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine"). . ), tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-to trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, pentakis(3-trimethoxysilylpropyl) -diethylenetriamine, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]silane, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane, 1-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-3,4,5-tris(3-tri 1-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexane, 1-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexane, 3,4,5-tris(3-trimethoxysilylpropyl)-cyclohexyl-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]ether, (3-trimethoxysilylpropyl)phosphate.

[0123] Further, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)phosphate, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]phosphate, N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, N-(1,3-dimethylbutylidene)-3-(trimethoxysilyl)-1-propanamine, N-benzylsilyl N-benzylidene-3-(triethoxysilyl)propan-1-amine, N-benzylidene-3-(trimethoxysilyl)propan-1-amine, 1,1-(1,4-phenylene)bis(N-(3(triethoxysilyl)propyl)methanamine), 1,1-(1,4-phenylene)bis(N-(3(trimethoxysilyl)propyl)methanamine), 2-methoxy-2-methyl-1-(benzylideneaminoethyl)-1-aza-2-silacyclopentane, and 2-methoxy-2-methyl-1-(4-methoxybenzylideneaminoethyl)-1-aza-2-silacyclopentane.

[0124] Furthermore, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(methyldimethoxysilyl)propyl]piperazine, 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), )bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), and 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine).

[0125] Furthermore, 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine), 3,3'-(1 ,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylmethane-1-amine) Disiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethane-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethane-1-amine) Examples of suitable siloxanes include 1,3-bis(3-(1H-imidazol-1-yl)propyl)bis(N,N-dipropylmethane-1-amine), 1,3-bis(3-(1H-imidazol-1-yl)propyl)-1,1,3,3-tetramethoxydisiloxane, 1,3-bis(3-(1H-imidazol-1-yl)propyl)-1,1,3,3-tetraethoxydisiloxane, and 1,3-bis(3-(1H-imidazol-1-yl)propyl)-1,1,3,3-tetrapropoxydisiloxane.

[0126] Among coupling modifiers having a group containing a nitrogen atom, protected amine compounds in which active hydrogen is substituted with a protecting group include alkoxysilanes and compounds having a protected amine in the molecule. Examples of such compounds include, but are not limited to, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane, N,N-bis(triethylsilyl)aminopropylmethyldiethoxysilane, 3-(4-trimethylsilyl-1-piperazino)propyltriethoxysilane, 3-(3-triethylsilyl-1-imidazolidinyl)propylmethyldiethoxysilane silane, 3-(3-trimethylsilyl-1-hexahydropyrimidinyl)propyltrimethoxysilane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, and 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane.

[0127] Further, for example, N-(1,3-dimethylbutylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1,3-dimethylbutylidene)-3-methyl(diethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-(trimethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1-methylethylidene)-3-methyl N-ethylidene-3-(diethoxysilyl)-1-propanamine, N-ethylidene-3-(triethoxysilyl)-1-propanamine, N-ethylidene-3-(trimethoxysilyl)-1-propanamine, N-ethylidene-3-methyl(dimethoxysilyl)-1-propanamine, N-ethylidene-3-methyl(diethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(triethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-(trimethoxysilyl)-1-propanamine , N-(1-methylpropylidene)-3-methyl(dimethoxysilyl)-1-propanamine, N-(1-methylpropylidene)-3-methyl(diethoxysilyl)-1-propanamine, N-benzylidene-3-methyl(dimethoxysilyl)propan-1-amine, N-benzylidene-3-methyl(diethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-(triethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-(trimethoxysilyl)propan-1-amine, N- 4-methylbenzylidene-3-methyl(dimethoxysilyl)propan-1-amine, N-4-methylbenzylidene-3-methyl(diethoxysilyl)propan-1-amine, N-naphthylidene-3-(triethoxysilyl)propan-1-amine, N-naphthylidene-3-(trimethoxysilyl)propan-1-amine, N-naphthylidene-3-methyl(dimethoxysilyl)propan-1-amine, 1,1-(1,4-phenylene)bis(N-(3-methyl(dimethoxysilyl)propyl)methanamine), 1,1-(1,4-phenylene)bis(N-(3-methyl(diethoxysilyl)propyl)methanamine), 2-ethoxy-2-methyl-1-(benzylideneaminoethyl)-1-aza-2-silacyclopentane, and 2-methoxy-2-methyl-1-(methylisobutylideneaminoethyl)-1-aza-2-silacyclopentane, 1-trimethylsilyl-4-[3-(trimethoxysilyl)propyl]piperazine, and 1-trimethylsilyl-4-[3-(triethoxysilyl)propyl]piperazine.

[0128] When a coupling step is carried out in the process for producing the conjugated diene polymer of this embodiment, it is more preferable to use a modifier having a nitrogen atom-containing group represented by any one of the following formulas (A) to (D) in the coupling step. These may be used alone or in combination of two or more.

[0129]

[0130] Here, R 10 , R 11 are hydrocarbon groups having 1 to 12 carbon atoms, which may contain unsaturated bonds, and may be the same or different. 12 is a hydrocarbon group having 1 to 20 carbon atoms. 8 , R 9 are aliphatic hydrocarbon groups having 1 to 6 carbon atoms, which may contain unsaturated bonds, and may be the same or different. 7 is a hydrocarbon group containing Si, O, or N and having 1 to 20 carbon atoms which may be substituted with an organic group having no active hydrogen, and which may have an unsaturated bond. a is an integer of 1 to 3.

[0131]

[0132] In the formula (B), A represents a hydrocarbon group having 1 to 20 carbon atoms or an organic group having at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a phosphorus atom, and having no active hydrogen. 13 , R 14 , and R 15R each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms. 16 , R 17 , R 18 , R 19 , and R 21 R each independently represents an alkyl group having 1 to 20 carbon atoms. 20 , and R 22 R each independently represents an alkylene group having 1 to 20 carbon atoms. 23 each independently represents an alkyl group or a trialkylsilyl group having 1 to 20 carbon atoms, each b independently represents an integer of 1 to 3, each c independently represents 1 or 2, i independently represents an integer of 0 to 6, j independently represents an integer of 0 to 6, k independently represents an integer of 0 to 6, and the sum of i, j, and k is an integer of 4 to 10.

[0133]

[0134] However, in formula (C), R 24 , R 25 , R 26 , R 27 , R 28 , and R 29 R each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms. 30 , R 31 , and R 32 each independently represents an alkylene group having 1 to 20 carbon atoms. s, t, and u each independently represent an integer of 1 to 3, and the sum of s, t, and u is an integer of 4 or greater.

[0135]

[0136] However, in formula (D), B 1 and B 2 are each independently a divalent hydrocarbon group having 1 to 20 carbon atoms which may or may not contain an oxygen atom. 33 ~R 36 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 ~L 4 are each independently a divalent, trivalent, or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, or a monovalent hydrocarbon group having 1 to 20 carbon atoms;1 and L 2 And, L 3 and L 4 may be linked together to form a ring having 1 to 5 carbon atoms, and L 1 and L 2 And, L 3 and L 4 When are linked together to form a ring, the ring formed may contain 1 to 3 heteroatoms of one or more types selected from the group consisting of N, O, and S.

[0137] Specifically, in the formula (D), B 1 and B 2 are each independently an alkylene group having 1 to 10 carbon atoms; R 33 ~R 36 are each independently an alkyl group having 1 to 10 carbon atoms, and L 1 ~L 4 are each independently a tetravalent alkylsilyl group substituted with an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or L 1 and L 2 And, L 3 and L 4 may be linked together to form a ring having 1 to 3 carbon atoms, and L 1 and L 2 And, L 3 and L 4 When are linked together to form a ring, the ring formed may contain 1 to 3 heteroatoms of one or more types selected from the group consisting of N, O and S.

[0138] Examples of the coupling modifier represented by formula (A) include, but are not limited to, 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-methyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-propyl-4-[3-(trimethoxysilyl)propyl]piperazine, 1-propyl-4-[3-(triethoxysilyl)propyl]piperazine, 1-trimethylsilyl-4-[3-(trimethoxysilyl)propyl]piperazine, and 1-trimethylsilyl-4-[3-(triethoxysilyl)propyl]piperazine.

[0139] Among these, from the viewpoint of enhancing the reactivity and interaction between the conjugated diene polymer of the present embodiment and the inorganic filler such as silica, and from the viewpoint of enhancing processability, those in which a in the formula (A) is 3 are preferred.

[0140] In the coupling step using the coupling modifier represented by formula (A), the reaction temperature and reaction time are not particularly limited, but the reaction is preferably carried out at a temperature of 0°C or higher and 120°C or lower, and for 30 seconds or longer.

[0141] The amount of the coupling modifier represented by formula (A) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (A) is 0.2 to 2.0 times, more preferably 0.3 to 1.5 times, and even more preferably 0.4 to 1.0 times, the number of moles of the polymerization initiator added. From the viewpoint of setting the molecular weight of the resulting modified conjugated diene polymer in a more preferred range, the amount is preferably 0.2 times or more, and from the viewpoint of storage stability during long-term storage, the amount is preferably 2.0 times or less.

[0142] More specifically, the amounts of the polymerization initiator and the coupling modifier represented by formula (A) added may be adjusted so that the number of moles of the coupling modifier represented by formula (A) is preferably 0.1 to 1.0 times the number of moles of the polymerization initiator.

[0143] In the formula (B), A is preferably represented by any one of the following formulae (I) to (IV).

[0144]

[0145] In the formula (Chemical Formula I), D 1 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When there are multiple D 1 are each independent of each other.

[0146]

[0147] In the formula (Chemical Formula II), D 2 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms.3 represents an alkyl group having 1 to 20 carbon atoms, and h represents an integer of 1 to 10. When a plurality of D 2 and D 3 are each independent of each other.

[0148]

[0149] In the formula (III), D 4 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When there are multiple D 4 are each independent of each other.

[0150]

[0151] In the formula (Chemical Formula IV), D 5 represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. h represents an integer of 1 to 10. When there are multiple D 5 are each independent of each other.

[0152] In the formula (B), when A is represented by formula (Chemical Formula I), examples of the coupling modifier include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)amine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tris(3-ethoxysilylpropyl)amine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, bis[3-(2,2-diethoxy-1 -aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)amine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]amine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-propanediamine.

[0153] Further, for example, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl] tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tetrakis(3-triethoxysilylpropyl)-1,3-propanediamine, and tris(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine.

[0154] Further, for example, bis(3-triethoxysilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-propanediamine, and tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane.

[0155] Furthermore, for example, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-trimethoxysilylpropyl) bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane.

[0156] Furthermore, for example, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-triethoxysilylpropyl)-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis(3-triethoxysilylpropyl)-1,3-propanediamine, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilylpropyl)-bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-1,3-propanediamine, tetrakis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tris(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilylpropyl) bis(3-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-[3-(1-ethoxy-2- trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tris[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-[3-(1-ethoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-1,3-bisaminomethylcyclohexane, tetrakis(3-trimethoxysilylpropyl)-1,6-hexamethylenediamine, and pentakis(3-trimethoxysilylpropyl)-diethylenetriamine.

[0157] In the formula (B), when A is represented by formula (II), examples of the coupling modifier include, but are not limited to, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl), bis(2-triethoxysilylpropyl)-methyl-1,3-propanediamine, tris(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, bis(2-triethoxysilylpropyl)-[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-methyl-1,3-propanediamine, bis[3-(2,2-diethoxy-1-aza-2-silacyclopentane)propyl]-(3-triethoxysilylpropyl)-methyl-1,3-propanediamine, N 1 , N 1 '-(propane-1,3-diyl)bis(N 1 -methyl-N 3 , N 3 -bis(3-(trimethoxysilyl)propyl)-1,3-propanediamine), and N 1 -(3-(bis(3-(trimethoxysilyl)propyl)amino)propyl)-N 1 -methyl-N 3 -(3-(methyl(3-(trimethoxysilyl)propyl)amino)propyl)-N 3 -(3-(trimethoxysilyl)propyl)-1,3-propanediamine.

[0158] In the formula (B), when A is represented by formula (III), examples of the coupling modifier include, but are not limited to, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, tris[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)silane, silane, bis(3-trimethoxysilylpropyl)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, (3-trimethoxysilyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, propyl]silane, bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)-bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis(3-trimethoxysilylpropyl)-[3-(1-methoxy-2-trimethylsilyl-1-sila- 2-azacyclopentane)propyl]-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]silane, bis[3-(1-methoxy-2-trimethylsilyl-1-sila-2-azacyclopentane)propyl]-bis(3-trimethoxysilylpropyl)silane, and bis(3-trimethoxysilylpropyl)-bis[3-(1-methoxy-2-methyl-1-sila-2-azacyclopentane)propyl]silane.

[0159] In the formula (B), when A is represented by formula (chemical formula IV), examples of the coupling modifier include, but are not limited to, 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-(2,2-dimethoxy-1-aza-2-silacyclopentane)propane and 3-tris[2-(2,2-dimethoxy-1-aza-2-silacyclopentane)ethoxy]silyl-1-trimethoxysilylpropane.

[0160] The amount of the modifier represented by formula (B) to be added is preferably determined based on the ratio of the number of moles of the polymerization initiator to the number of moles of the modifier represented by formula (B) to be added, which allows the conjugated diene polymer and the modifier to react in a desired stoichiometric ratio.

[0161] More specifically, the amounts of the polymerization initiator and the coupling modifier represented by formula (B) added may be adjusted so that the ratio of the number of moles of the coupling modifier represented by formula (B) to the number of moles of the polymerization initiator is preferably 0.012 to 1.0, more preferably 0.02 to 0.5. In this case, the number of functional groups of the modifier in formula (B) (for example, when i and j are 2 or more and multiple w and x are present, and when f and g are equal, then f × i + (g + 1) × j + k) is preferably an integer of 5 to 10, more preferably an integer of 6 to 10. From the viewpoint of achieving a molecular weight in a preferred range for the resulting modified conjugated diene polymer, the ratio is preferably 0.012 or more. From the viewpoint of storage stability during long-term storage, the ratio is preferably 0.2 or less.

[0162] Among these, from the viewpoint of enhancing the reactivity and interaction between the modified conjugated diene polymer and the inorganic filler such as silica, and from the viewpoint of enhancing processability, it is preferable that i, j, and k in the formula (B) are all 3.

[0163] Examples of the coupling modifier represented by formula (C) include, but are not limited to, tris(3-trimethoxysilylpropyl)amine, tris(3-methyldimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-methyldiethoxysilylpropyl)amine, tris(trimethoxysilylmethyl)amine, tris(2-trimethoxysilylethyl)amine, and tris(4-trimethoxysilylbutyl)amine.

[0164] The reaction temperature and reaction time in the coupling step using the coupling modifier represented by formula (C) are not limited to the following, but are preferably 0°C or higher and 120°C or lower, and the reaction is preferably carried out for 30 seconds or longer.

[0165] The amount of the coupling modifier represented by formula (C) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (C) is 0.1 to 2.0 times the number of moles of the polymerization initiator added, more preferably 0.2 to 1.0 times, and even more preferably 0.3 to 0.5 times. From the viewpoint of the molecular weight of the resulting modified conjugated diene polymer, it is preferably 0.1 times or more. Furthermore, from the viewpoint of storage stability during long-term storage, it is preferably 2.0 times or less.

[0166] Examples of the coupling modifier represented by formula (D) include 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(N,N-dimethyl ...dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(N,N-dimethylpropan-1-amine), 3,3'-(1,1,3,3-tetramethyldisiloxane- methoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), and the like.

[0167] In the coupling step using the coupling modifier represented by formula (D), the reaction temperature and reaction time are not particularly limited, but the reaction is preferably carried out at a temperature of 0°C or higher and 120°C or lower, and for 30 seconds or longer.

[0168] The amount of the coupling modifier represented by formula (D) added is preferably in a range such that the total number of moles of alkoxy groups bonded to silyl groups in the compound represented by formula (D) is 0.25 to 2.0 times the number of moles of the polymerization initiator added, more preferably 0.3 to 1 time, and even more preferably 0.35 to 0.5 times. From the viewpoint of the molecular weight of the resulting modified conjugated diene polymer and from the viewpoint of storage stability during long-term storage, it is preferably 2.0 times or less.

[0169] The method for producing a conjugated diene polymer of the present embodiment may include a condensation reaction step in which a condensation promoter is added to cause a condensation reaction after and / or before the coupling step.

[0170] In the method for producing a conjugated diene polymer of this embodiment, after the coupling step, a deactivator and / or a neutralizing agent may be added to the polymer solution as needed. Examples of deactivators include, but are not limited to, water, and alcohols such as methanol, ethanol, and isopropanol. Examples of neutralizing agents include, but are not limited to, aqueous solutions of carboxylic acids such as stearic acid, oleic acid, and versatic acid (a mixture of highly branched carboxylic acids having 9 to 11 carbon atoms and mainly containing 10 carbon atoms), inorganic acids, and carbon dioxide gas.

[0171] It is preferable to add a rubber stabilizer to the conjugated diene polymer of this embodiment from the viewpoint of preventing gel formation after polymerization and improving stability during processing. The rubber stabilizer is not limited to the following and any known stabilizer can be used, but preferred examples include antioxidants such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenol)propionate, and 2-methyl-4,6-bis[(octylthio)methyl]phenol.

[0172] (Step of Obtaining from Polymer Solution) The method for producing a conjugated diene polymer of this embodiment may include a step of obtaining the obtained conjugated diene polymer from the polymer solution. As a method for obtaining the conjugated diene polymer from the polymer solution, known methods can be used, and for example, the following methods may be used. Examples include a method in which the solvent is separated by steam stripping or the like, and the conjugated diene polymer is then filtered off, and then dehydrated and dried to obtain a conjugated diene polymer; a method in which the conjugated diene polymer is obtained by concentrating the polymer in a flashing tank and then devolatilizing it using a vent extruder or the like; and a method in which the conjugated diene polymer is obtained by directly devolatilizing it using a drum dryer or the like.

[0173] (Step of Obtaining Extended Conjugated Diene Polymer) In the method for producing a conjugated diene polymer of this embodiment, at least one selected from the group consisting of extended oil, liquid rubber, and resin may be added to the produced conjugated diene polymer to obtain an extended conjugated diene polymer. The extended conjugated diene polymer includes not only oil-extended conjugated diene polymers containing oil, but also those containing liquid polybutadiene or various resins other than oil. This can further improve the processability of the conjugated diene polymer.

[0174] The method for adding an extender oil to a conjugated diene polymer is not limited to the following methods, but a preferred method involves adding an extender oil to a conjugated diene polymer solution, mixing, and then desolvating the resulting extended polymer solution. Examples of extender oils include aroma oils, naphthenic oils, paraffin oils, and vegetable oils. The vegetable oil can be made from an oil selected from the group consisting of linseed oil, safflower oil, soybean oil, corn oil, cottonseed oil, castor oil, tung oil, pine oil, sunflower oil, palm oil, olive oil, coconut oil, peanut oil, and grapeseed oil. Among these, from the viewpoints of environmental safety, oil bleed prevention, and wet grip properties, aroma substitute oils having a polycyclic aromatic (PCA) content of 3% by mass or less according to the IP346 method are preferred. Examples of aroma substitute oils include TDAE (Treated Distillate Aromatic Extracts) and MES (Mild Extraction Solvate) as shown in Kautschuk Gummi Kunststoffe 52(12)799(1999), as well as RAE (Residual Aromatic Extracts).

[0175] Examples of liquid rubbers include, but are not limited to, liquid polybutadiene and liquid styrene-butadiene rubber. Examples of resins include, but are not limited to, aromatic petroleum resins, coumarone-indene resins, terpene resins, rosin derivatives (including tung oil resins), tall oil, tall oil derivatives, rosin ester resins, natural and synthetic terpene resins, aliphatic hydrocarbon resins, aromatic hydrocarbon resins, mixed aliphatic-aromatic hydrocarbon resins, coumarin-indene resins, phenolic resins, p-tert-butylphenol-acetylene resins, phenol-formaldehyde resins, xylene-formaldehyde resins, monoolefin oligomers, diolefin oligomers, hydrogenated aromatic hydrocarbon resins, cyclic aliphatic hydrocarbon resins, hydrogenated hydrocarbon resins, hydrogenated tung oil resins, hydrogenated oil resins, and esters of hydrogenated oil resins with monofunctional or polyfunctional alcohols. These resins may be used alone or in combination. In the case of hydrogenation, all of the unsaturated groups may be hydrogenated, or some of them may remain. The amount of at least one selected from the group consisting of extender oil, liquid rubber, and resin to be added is not particularly limited, but is preferably 1 to 60 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 15 to 37.5 parts by mass, relative to 100 parts by mass of the conjugated diene-based polymer of the present embodiment.

[0176] [Rubber Composition] The conjugated diene polymer of this embodiment can be added with a filler to form a rubber composition (hereinafter, sometimes referred to as the rubber composition of this embodiment). The rubber composition of this embodiment includes a rubber component containing the conjugated diene polymer of this embodiment described above and 5.0 parts by mass to 150 parts by mass of a filler per 100 parts by mass of the rubber component. Preferably, the rubber component contains 10 parts by mass or more of the conjugated diene polymer of this embodiment per 100 parts by mass of the total rubber component. By dispersing a filler in the rubber component containing the conjugated diene polymer of this embodiment, a rubber composition can be obtained that has even better processability during vulcanization and that produces a vulcanizate with even better low hysteresis loss, fracture properties, and abrasion resistance. Furthermore, by including the conjugated diene polymer of this embodiment in a predetermined proportion in the rubber component, processability and abrasion resistance are further improved.

[0177] Examples of fillers include, but are not limited to, silica-based inorganic fillers, carbon black, metal oxides, and metal hydroxides. Among these, silica-based inorganic fillers are preferred. In particular, when the rubber composition is used for vulcanized rubber applications such as tires, automobile parts such as anti-vibration rubber, and shoes, it is particularly preferred to contain a silica-based inorganic filler. Such fillers may be used alone or in combination of two or more.

[0178] The silica-based inorganic filler is not particularly limited, and known fillers can be used. 2 or Si 3 Solid particles containing Al as a constituent unit are preferred, and SiO 2 or Si 3 Solid particles containing Al as the main component of the structural units are more preferred. Here, the main component refers to a component contained in the silica-based inorganic filler in an amount of more than 50% by mass, preferably 70% by mass or more, and more preferably 80% by mass or more.

[0179] Examples of silica-based inorganic fillers include, but are not limited to, inorganic fibrous materials such as silica, clay, talc, mica, diatomaceous earth, wollastonite, montmorillonite, zeolite, and glass fiber. Surface-hydrophobized silica-based inorganic fillers and mixtures of silica-based inorganic fillers with non-silica-based inorganic fillers may also be used. Among these, silica or glass fiber is preferred, and silica is more preferred, from the viewpoint of further improving the strength and abrasion resistance of the rubber composition of this embodiment. Examples of silica include, but are not limited to, dry silica, wet silica, and synthetic silicate silica. Among these silicas, wet silica is preferred from the viewpoint of further improving the breaking strength of the rubber composition.

[0180] From the viewpoint of more reliably obtaining a rubber composition having practically good abrasion resistance and breaking strength, the nitrogen adsorption specific surface area of ​​the silica-based inorganic filler determined by the BET adsorption method is 100 m 2 / g or more 300m 2 / g or less, and 2 / g or more 250m 2 / g or less. If necessary, a relatively small specific surface area (for example, a specific surface area of ​​200 m 2 / g) silica-based inorganic filler and a relatively large specific surface area (e.g., 200 m 2 In particular, silica-based inorganic fillers having a relatively large specific area (for example, 200 m / g or more) may be used in combination. 2 When a silica-based inorganic filler (at least 1000 saturates / g) is used, the rubber composition of the present embodiment further improves the dispersibility of silica, which tends to result in a rubber composition having even better abrasion resistance, fracture strength, and low hysteresis loss.

[0181] Examples of carbon black include, but are not limited to, carbon blacks of various classes such as SRF, FEF, HAF, ISAF, and SAF. Among these, carbon blacks having a nitrogen adsorption specific surface area of ​​50 m or more as determined by the BET adsorption method are preferred. 2 Carbon black having a carbon absorption of 80 mL / 100 g or more and a dibutyl phthalate (DBP) oil absorption of 80 mL / 100 g or less is preferred.

[0182] The metal oxides include those represented by the chemical formula M x O y (M represents a metal atom, and x and y each independently represent an integer of 1 to 6.) As long as the solid particles have as a main component a structural unit, there is no particular limitation, but examples thereof include alumina, titanium oxide, magnesium oxide, and zinc oxide.

[0183] The metal hydroxide is not particularly limited, but examples thereof include aluminum hydroxide, magnesium hydroxide, and zirconium hydroxide.

[0184] The content of the filler in the rubber composition of this embodiment is preferably 5.0 parts by mass to 150 parts by mass, more preferably 20 parts by mass to 100 parts by mass, and even more preferably 30 parts by mass to 90 parts by mass, per 100 parts by mass of the rubber component. When the filler satisfies the above range, the rubber composition tends to have even more excellent processability during vulcanization, and the vulcanizate thereof tends to have even more excellent low hysteresis loss, fracture properties, and abrasion resistance.

[0185] From the viewpoint of reliably imparting the performance required for applications such as tires, such as dry grip performance and conductivity, the rubber composition of this embodiment preferably contains carbon black in an amount of 0.5 parts by mass to 100 parts by mass per 100 parts by mass of the rubber component containing the conjugated diene polymer of this embodiment. From the same viewpoint, the rubber composition preferably contains carbon black in an amount of 3.0 parts by mass to 100 parts by mass, and even more preferably 5.0 parts by mass to 50 parts by mass, per 100 parts by mass of the rubber component containing the conjugated diene polymer of this embodiment.

[0186] The rubber composition of this embodiment may further contain a silane coupling agent. By including a silane coupling agent in the rubber composition, the interaction between the rubber component and the filler can be further improved. Examples of silane coupling agents include, but are not limited to, compounds having a sulfur bond moiety and an alkoxysilyl group or silanol group moiety in one molecule. Examples of such compounds include, but are not limited to, bis-[3-(triethoxysilyl)-propyl]-tetrasulfide, bis-[3-(triethoxysilyl)-propyl]-disulfide, and bis-[2-(triethoxysilyl)-ethyl]-tetrasulfide.

[0187] In the rubber composition of this embodiment, the content of the silane coupling agent is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, and even more preferably 1.0 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the filler. When the content of the silane coupling agent is within the above range, the interaction between the rubber component and the filler tends to be further improved.

[0188] The rubber composition of the present embodiment may contain, as a rubber component, a rubbery polymer other than the conjugated diene polymer of the present embodiment (hereinafter simply referred to as a "rubbery polymer"). Examples of the rubbery polymer include, but are not limited to, conjugated diene polymers and hydrogenated products thereof, random copolymers of conjugated diene compounds and vinyl aromatic compounds and hydrogenated products thereof, block copolymers of conjugated diene compounds and vinyl aromatic compounds and hydrogenated products thereof, non-diene polymers, and natural rubber. Examples of the rubbery polymer include, but are not limited to, styrene-based elastomers such as butadiene rubber and hydrogenated products thereof, isoprene rubber and hydrogenated products thereof, styrene-butadiene rubber and hydrogenated products thereof, styrene-butadiene block copolymers and hydrogenated products thereof, and styrene-isoprene block copolymers and hydrogenated products thereof, as well as acrylonitrile-butadiene rubber and hydrogenated products thereof. Non-diene polymers include, but are not limited to, olefin elastomers such as ethylene-propylene rubber, ethylene-propylene-diene rubber, ethylene-butene-diene rubber, ethylene-butene rubber, ethylene-hexene rubber, and ethylene-octene rubber, butyl rubber, brominated butyl rubber, acrylic rubber, fluororubber, silicone rubber, chlorinated polyethylene rubber, epichlorohydrin rubber, α,β-unsaturated nitrile-acrylate-conjugated diene copolymer rubber, urethane rubber, and polysulfide rubber. Natural rubber includes, but is not limited to, smoked sheets RSS3 to 5, SMR, and epoxidized natural rubber.

[0189] The rubbery polymer may be a modified rubber to which a polar functional group such as a hydroxyl group, an amino group, etc. When the rubber composition of the present embodiment is used for a tire, the rubbery polymer is preferably at least one selected from the group consisting of butadiene rubber, isoprene rubber, styrene-butadiene rubber, natural rubber, and butyl rubber.

[0190] From the viewpoint of the balance between the abrasion resistance, breaking strength, low hysteresis loss, and processability of the rubber composition, the mass average molecular weight of the rubber polymer is preferably 2,000 to 2,000,000, and more preferably 5,000 to 1,500,000. Furthermore, a low molecular weight rubber polymer, so-called liquid rubber, can also be used as the rubber polymer. These rubber polymers may be used alone or in combination of two or more.

[0191] When the rubber composition of this embodiment further contains the above-described rubbery polymer in addition to the conjugated diene polymer of this embodiment, the content ratio (mass ratio) of the conjugated diene polymer to the rubbery polymer (conjugated diene polymer / rubbery polymer) is preferably 10 / 90 to 100 / 0, more preferably 20 / 80 to 90 / 10, and even more preferably 30 / 70 to 80 / 20. That is, the rubber component contains preferably 10 to 100 parts by mass, more preferably 20 to 90 parts by mass, and even more preferably 30 to 80 parts by mass of the conjugated diene polymer of this embodiment per 100 parts by mass of the total rubber component. When the proportion of the conjugated diene polymer of this embodiment in the rubber component is within the above range, the vulcanizate of the rubber composition tends to have even better wear resistance and low hysteresis loss.

[0192] To further improve its processability, the rubber composition of this embodiment may contain a rubber softener in addition to the rubber component. The rubber softener may be the same as those exemplified for the conjugated diene polymer described above, but mineral oil or a liquid or low-molecular-weight synthetic softener is preferred. Mineral oil-based rubber softeners, known as process oils or extender oils, are used to soften the rubber component, increase its volume, and improve its processability. They are mixtures of aromatic rings, naphthenic rings, and paraffin chains. Among these, those in which 50% or more of the total carbon atoms belong to paraffin chains are called paraffinic; those in which 30% to 45% of the total carbon atoms belong to naphthenic rings are called naphthenic; and those in which more than 30% of the total carbon atoms belong to aromatic carbons are called aromatic. The rubber composition of this embodiment preferably contains a rubber softener with an appropriate aromatic content. The inclusion of such a rubber softener further improves compatibility with the conjugated diene polymer. The content of the rubber softener in the rubber composition of this embodiment is represented by the total amount of the rubber softener added in advance to the conjugated diene polymer or rubbery polymer and the rubber softener added when preparing the rubber composition. In the rubber composition of this embodiment, the content of the rubber softener is preferably 0 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 90 parts by mass or less, and even more preferably 30 parts by mass or more and 90 parts by mass or less, per 100 parts by mass of the rubber component. By having the content of the rubber softener be 100 parts by mass or less per 100 parts by mass of the rubber component, bleed-out can be suppressed, and stickiness of the surface of the rubber composition can be further suppressed.

[0193] The rubber composition can be produced by mixing a conjugated diene polymer, a rubbery polymer, a filler, a silane coupling agent, a rubber softener, and the like. The mixing method is not particularly limited, but examples include a melt-kneading method using a general mixer such as an open roll, a Banbury mixer, a kneader, a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, and a method in which the components are dissolved and mixed and then the solvent is removed by heating. Among these, the melt-kneading method using a roll, a Banbury mixer, a kneader, or an extruder is preferred from the viewpoints of productivity and good kneading ability. The rubber component, the filler, the silane coupling agent, and the additives may be kneaded all at once, or may be mixed in multiple batches.

[0194] The rubber composition of the present embodiment may be vulcanized with a vulcanizing agent to form a vulcanizate. The vulcanizing agent is not particularly limited, but examples thereof include radical generators such as organic peroxides and azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, and sulfur compounds. Examples of sulfur compounds include sulfur monochloride, sulfur dichloride, disulfide compounds, and polymeric polysulfur compounds.

[0195] In the rubber composition of this embodiment, the content of the vulcanizing agent is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the rubber component. A conventionally known method can be used as the vulcanization method. The vulcanization temperature is preferably 120°C or more and 200°C or less, and more preferably 140°C or more and 180°C or less.

[0196] When vulcanizing the rubber composition, a vulcanization accelerator and / or vulcanization aid may be used as necessary. As the vulcanization accelerator, conventionally known materials can be used, and examples thereof include, but are not limited to, sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, and dithiocarbamate-based vulcanization accelerators. Furthermore, examples of the vulcanization aid include, but are not limited to, zinc oxide and stearic acid. The content of each of the vulcanization accelerator and vulcanization aid is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the rubber component.

[0197] The rubber composition of this embodiment may contain various additives such as softeners other than those described above, other fillers, heat stabilizers, antistatic agents, weather stabilizers, antioxidants, colorants, and lubricants, as long as the effects of this embodiment are not impaired. Known softeners can be used as softeners. Examples of other fillers include, but are not limited to, calcium carbonate, magnesium carbonate, aluminum sulfate, and barium sulfate. Known materials can be used as heat stabilizers, antistatic agents, weather stabilizers, antioxidants, colorants, and lubricants.

[0198] The rubber composition of the present embodiment is suitably used as a rubber composition for tires. The rubber composition of the present embodiment is not particularly limited, but can be suitably used for various tire parts such as fuel-efficient tires, all-season tires, high-performance tires, and studless tires, including treads, carcasses, sidewalls, and bead portions.

[0199] In addition, the numerical ranges described above as preferred ranges, etc., may be replaced with numerical ranges that arbitrarily combine the values ​​described as upper limits and the values ​​described as lower limits, unless otherwise specified.

[0200] The present embodiment will be described in more detail below with reference to specific examples and comparative examples, but the present invention is not limited to these examples and comparative examples. Various physical properties in the examples and comparative examples were measured by the methods shown below.

[0201] ((Property 1) Polymer Segment Ratio) <Solid Amount> The solid amount in the conjugated diene polymer solution was determined from the amount of nonvolatile components in the conjugated diene polymer solution flowing through the measurement point per unit time. The entire amount of the conjugated diene polymer solution flowing through the measurement point was sampled for 3 minutes, and a polymerization terminator was immediately added. The solution was then transferred to a heat-resistant dish and dried in an oven at 140°C for 30 minutes or more, after which the mass (M) of the remaining solid matter was measured. Here, the solid amount (m) was determined using the following formula (I):

[0202]

[0203] The measurement points were the discharge part of the polymerization step (P1) for synthesizing the first polymer segment and the discharge part of the polymerization step (P2) for forming the second polymer segment, and the solid amount at each point was measured by m 1 , m 2 It was decided.

[0204] <mass ratio r of the first polymer segment to the second polymer segment 1 , r 2 The mass ratio r of each of the first polymer segment and the second polymer segment is expressed as the ratio m of the solid mass at each discharge point of the polymerization step (P1) for synthesizing the first polymer segment and the polymerization step (P2) for forming the second polymer segment to the sum of the mass (U) of the conjugated diene compound and the mass (V) of the aromatic vinyl compound added per unit time throughout the entire polymerization step, as shown in the following formula (II) and formula (III): 1 , m 2 In this example, U is the total amount of 1,3-butadiene added in the first unit and 1,3-butadiene added in the second unit per unit time, and V is the total amount of styrene added in the first unit and styrene added in the second unit per unit time.

[0205]

[0206] <Ratio of polymer segment ratio: R> The ratio of the mass ratio of the first polymer segment to the mass ratio of the second polymer segment: R (= r 1 / r 2 ) was calculated using the following formula (IV).

[0207]

[0208] ((Property 2) Amount of bound aromatic vinyl monomer units (amount of bound styrene)) <Amount of bound styrene in conjugated diene polymer X all A conjugated diene polymer sampled from the discharge port of the polymerization step (P2) for forming a second polymer segment, which did not contain a rubber softener, was used as a sample. 100 mg of the sample was diluted to 100 mL with chloroform and dissolved to prepare a measurement sample. The amount of bound styrene (mass %) relative to 100 mass % of the coupled conjugated diene polymer sample was measured based on the amount of absorption of ultraviolet light by the phenyl group of styrene (near 254 nm) (measuring device: Shimadzu Corporation's spectrophotometer "UV-2450").

[0209] <Amount of bound styrene in the first polymer segment X 1 The sample was changed from the conjugated diene polymer to the solid content of the polymer solution discharged from the polymerization step (P1) for synthesizing the first polymer segment. The bound styrene amount was calculated in the same manner as for the bound styrene amount in the conjugated diene polymer segment, with the other conditions being the same.

[0210] <Amount of bound styrene in the second polymer segment X 2 > The amount of solids m in each of the polymerization step (P1) for synthesizing the first polymer segment and the polymerization step (P2) for forming the second polymer segment 1 , m 2 , bound styrene amount X 1 , X all From the above, the bound styrene amount (X 2 ) was calculated.

[0211]

[0212] <Difference |ΔX| Between Bound Styrene Amounts Between First Polymer Segment and Second Polymer Segment> The difference |ΔX| between the bound styrene amounts between the first polymer segment and the second polymer segment was calculated by the following formula (IX).

[0213]

[0214] ((Property 3) Amount of vinyl bonds in bound conjugated diene (amount of 1,2-vinyl bonds in bound butadiene)) <Amount of vinyl bonds in conjugated diene polymer Y all A conjugated diene polymer not containing a rubber softener was collected from the discharge section of the polymerization step (P2) for forming the second polymer segment, and 50 mg of the sample was dissolved in 10 mL of carbon disulfide to prepare a measurement sample. The infrared spectrum of each sample was measured from 600 to 1000 cm -1 The absorbance at a predetermined wave number was measured using a Fourier transform infrared spectrophotometer (trade name "FT-IR230" manufactured by JASCO Corporation). The amount of 1,2-vinyl bonds (mol %) in the bound butadiene was determined from the absorbance at a predetermined wave number according to the Hampton method (described in R.R. Hampton, Analytical Chemistry 21, 923 (1949)).

[0215] <Amount of vinyl bond in first polymer segment Y 1 The sample was changed from the conjugated diene polymer to the solid content of the polymer solution discharged from the polymerization step (P1) for synthesizing the first polymer segment. Regarding other conditions, the vinyl bond content was calculated in the same manner as for the vinyl bond content of the conjugated diene polymer.

[0216] <Amount of vinyl bond in second polymer segment Y 2 > The solid amount m in each of the polymerization step (P1) for synthesizing the first polymer segment and the polymerization step (P2) for forming the second polymer segment 1 , m 2 , the amount of vinyl bonds in the bonded conjugated diene Y 1 , Y all From the above, the amount of vinyl bonds in the second polymer segment was calculated from the following formula (X).

[0217]

[0218] <Difference ΔY in Vinyl Bond Amount Between First Polymer Segment and Second Polymer Segment> The difference ΔY in the vinyl bond amount in the bonded conjugated diene between the first polymer segment and the second polymer segment was calculated by the following formula (XI).

[0219]

[0220] (Physical Property 4) Conversion Rate, Difference in Polymerization Conversion Rate The conversion rate c of the conjugated diene compound in the polymerization step (P1) for synthesizing the first polymer segment bd , and the conversion rate of the aromatic vinyl compound c st were calculated using the following formulas (V) and (VI), respectively.

[0221]

[0222] The difference between the conversion rate of the conjugated diene compound and the conversion rate of the aromatic vinyl compound is the polymerization conversion rate difference c dif was calculated using the following formula (VII).

[0223]

[0224] (Physical Property 5) Estimated Glass Transition Temperature The estimated glass transition temperature of the conjugated diene polymer was determined using the above formula (iii).

[0225] (Physical Property 6) Molecular Weight) Using the conjugated diene polymers of the Examples and Comparative Examples as samples, a GPC measurement apparatus (trade name "HLC-8320GPC" manufactured by Tosoh Corporation) in which three columns packed with polystyrene gel were connected was used, and a chromatogram was measured using an RI detector (trade name "HLC8020" manufactured by Tosoh Corporation). The weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) were determined based on a calibration curve obtained using standard polystyrene. THF (tetrahydrofuran) containing 5 mmol / L triethylamine was used as the eluent. Three columns, trade name "TSKgel SuperMultiporeHZ-H" manufactured by Tosoh Corporation, were connected, and a guard column, trade name "TSKguardcolumn SuperMP(HZ)-H" manufactured by Tosoh Corporation, was connected in front of them. 10 mg of the sample to be measured was dissolved in 10 mL of THF to prepare a measurement solution, and 10 μL of the measurement solution was injected into a GPC measurement device and measured under conditions of an oven temperature of 40° C. and a THF flow rate of 0.35 mL / min.

[0226] (Physical Property 7) Mooney Viscosity of Polymers The conjugated diene polymers of the Examples and Comparative Examples were used as samples, and Mooney viscosities were measured using a Mooney viscometer (trade name "VR1132" manufactured by Ueshima Seisakusho Co., Ltd.) in accordance with ISO 289 using an L-shaped rotor at a measurement temperature of 100°C. First, the samples were preheated at the test temperature for 1 minute, and then the rotor was rotated at 2 rpm. After 4 minutes, the torque was measured to determine the Mooney viscosity (ML (1+4) )

[0227] (Physical Property 8) Glass Transition Temperature (Tg) When the conjugated diene polymers of the Examples and Comparative Examples were oil-extended products, the conjugated diene polymers after extraction of the extended oil were used as samples, and a DSC curve was recorded in accordance with ISO 22768:2006 using a differential scanning calorimeter "DSC3200S" manufactured by Mac Science, while heating from -120°C to 40°C at a rate of 10°C / min under a helium flow of 50 mL / min, and the inflection point of the DSC observed in the range of -100°C to 20°C was taken as the glass transition temperature.

[0228] The extrapolated glass transition onset temperature was determined as the temperature at the intersection of a line drawn by extending the low-temperature baseline toward the high temperature and a tangent drawn at the maximum slope of the step-like change in the glass transition curve.The extrapolated glass transition finish temperature was determined as the temperature at the intersection of a line drawn by extending the high-temperature baseline toward the low temperature and a tangent drawn at the maximum slope of the step-like change in the glass transition curve.

[0229] (Physical Property 9) Modification Ratio The modification ratio of the conjugated diene polymers of the Examples and Comparative Examples was measured by the column adsorption GPC method as follows. The conjugated diene polymer was used as a sample, and the measurement was carried out by applying the property of the modified basic polymer component being adsorbed to a GPC column filled with silica gel. The amount of adsorption to the silica column was measured from the difference between the chromatogram measured on a polystyrene column and the chromatogram measured on a silica column for a sample solution containing the sample and low-molecular-weight internal standard polystyrene, and the modification ratio was calculated. <Preparation of Sample Solution>: 10 mg of sample and 5 mg of standard polystyrene were dissolved in 20 mL of THF (tetrahydrofuran) to prepare a sample solution. <GPC measurement conditions using a polystyrene-based column>: Using a Tosoh Corporation product name "HLC-8320GPC", 10 μL of the sample solution was injected into the apparatus using 5 mmol / L triethylamine-containing THF as the eluent, and a chromatogram was obtained using an RI detector under the conditions of a column oven temperature of 40 ° C. and a THF flow rate of 0.35 mL / min. Three Tosoh Corporation product name "TSKgel SuperMultiporeHZ-H" columns were connected, and a Tosoh Corporation product name "TSKguardcolumn SuperMP(HZ)-H" was connected to the preceding stage as a guard column. <GPC measurement conditions using a silica-based column> GPC measurements were performed using a Tosoh Corporation product name "HLC-8320GPC" and an RI detector (Tosoh Corporation product name "HLC8020"). THF was used as the eluent, and 50 μL of the sample solution was injected into the device. A chromatogram was obtained under the conditions of a column oven temperature of 40 ° C. and a THF flow rate of 0.5 ml / min. The columns were connected in this order: Agilent Zorbax PSM-1000S, PSM-300S, and PSM-60S. A guard column, DIOL 4.6 × 12.5 mm 5 micron, was connected in front of the columns.<Method of calculating modification rate>: The total peak area of ​​the chromatogram using a polystyrene-based column was set to 100, the peak area of ​​the sample was set to p1, the peak area of ​​the standard polystyrene was set to p2, the total peak area of ​​the chromatogram using a silica-based column was set to 100, the peak area of ​​the sample was set to p3, and the peak area of ​​the standard polystyrene was set to p4, and the modification rate (%) was calculated using the following formula: Modification rate (%) = [1 - (p2 × p3) / (p1 × p4)] × 100 (where p1 + p2 = p3 + p4 = 100).

[0230] [Production of Conjugated Diene Polymer] (Example 1) Two tank-type pressure vessels, each having an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom, an outlet at the top, and a jacket for temperature control, were connected as polymerization reactors. The polymerization step (P1) for synthesizing a first polymer segment was carried out using the first polymerization reactor. 1,3-butadiene, from which moisture had been removed in advance, was mixed at 20.3 g / min, styrene at 4.31 g / min, and normal hexane at 173 g / min. n-Butyllithium, used for inactivating residual impurities, was added at 0.104 mmol / min in a static mixer installed in the middle of the pipe supplying this mixed solution to the inlet of the reactor, and the mixture was then continuously fed to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.0235 mmol / min and n-butyllithium as a polymerization initiator at a rate of 0.239 mmol / min were supplied to the bottom of the first reactor, which was being vigorously mixed with a stirrer, and the temperature inside the reactor was maintained at 78°C. Thereafter, when the polymerization reaction became stable, the entire amount of the conjugated diene polymer was extracted from the top of the reactor, and an antioxidant (BHT) was added in an amount of 0.2 g per 100 g of the conjugated diene polymer, followed by removal of the solvent. Thereafter, the amount of bound aromatic vinyl monomer units (X 1 ) and the vinyl bond content in the bonded conjugated diene (Y 1 ), solid concentration (m 1 ) was measured.

[0231] Next, a step (P2) of forming a second polymer segment was carried out using a second polymerization reactor. The conjugated diene polymer solution was continuously supplied from the top of the first reactor to the bottom of the second reactor, and the reaction was continued at 78°C while stirring the mixture, adding 1,3-butadiene, normal hexane, and 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 8.71 g / min, 32.1 g / min, and 0.450 mmol / min to the second reactor.

[0232] Next, in the modification step, coupling agents, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine (referred to as "coupling agent A" in the table below) at a rate of 0.0103 mmol / min and 1-methyl-4-[3-(trimethoxysilyl)propyl]piperazine (referred to as "coupling agent B" in the table below) at a rate of 0.0965 mmol / min, were continuously added to the conjugated diene polymer solution flowing out from the top of the second reactor, and the mixture was mixed using a static mixer to carry out a coupling reaction. At this time, it took 4.8 minutes for the coupling agent to be added to the polymer solution flowing out from the outlet of the reactor, and the temperature was 68°C. After the coupling reaction, the entire conjugated diene polymer solution was withdrawn, and an antioxidant (BHT) was added in an amount of 0.2 g per 100 g of polymer, followed by removal of the solvent, and various measurements of molecular weight, bound aromatic vinyl content (X all ) and the amount of vinyl bonds in the bonded conjugated diene (Y all ), solid content concentration (m 2 ) and the glass transition temperature was measured.

[0233] Next, an antioxidant (BHT) was continuously added to the conjugated diene polymer solution after the coupling reaction at a rate of 0.055 g / min (n-hexane solution) so that the amount was 0.2 g per 100 g of polymer, and the coupling reaction was terminated. Simultaneously with the antioxidant, SRAE oil (JOMO Process NC140, manufactured by JX Nippon Oil & Energy Corporation) was continuously added as a rubber softener so that the amount was 5.0 g per 100 g of polymer, and the mixture was mixed in a static mixer. The solvent was removed by steam stripping, yielding the modified conjugated diene polymer of Example 1.

[0234] Example 2 A modified conjugated diene polymer of Example 2 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene supplied to the first reactor were changed to 18.7 g / min and 6.67 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 8.00 g / min.

[0235] (Example 3) A modified conjugated diene polymer of Example 3 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene supplied to the first reactor were changed to 17.3 g / min and 8.67 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 7.40 g / min.

[0236] Example 4 A modified conjugated diene polymer of Example 4 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene supplied to the first reactor were changed to 21.0 g / min and 3.33 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 9.00 g / min.

[0237] Example 5 A modified conjugated diene polymer of Example 5 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene supplied to the first reactor were changed to 21.9 g / min and 2.00 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 9.40 g / min.

[0238] Example 6 A modified conjugated diene polymer of Example 6 was obtained in the same manner as in Example 1, except that the L / D of the first reactor was changed to 6.0, the rates of styrene supplied to the first reactor were 3.88 g / min, 2,2-bis(2-oxolanyl)propane as a polar substance was 0.0208 mmol / min, and n-butyllithium as a polymerization initiator was 0.208 mmol / min, and the rate of 2,2-bis(2-oxolanyl)propane supplied to the second reactor was 0.396 mmol / min, the rates of coupling agent A added in the modification step were changed to 0.00917 mmol / min and coupling agent B to 0.0856 mmol / min, and styrene was newly added to the second reactor at 0.43 g / min.

[0239] Example 7 A modified conjugated diene polymer of Example 7 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene supplied to the first reactor were changed to 24.9 g / min and 4.35 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 4.35 g / min.

[0240] Example 8 A modified conjugated diene polymer of Example 8 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene were supplied to the first reactor at 4.64 g / min and 0.46 g / min, respectively, the internal temperature of the first reactor was changed to 80°C, the 1,3-butadiene added to the second reactor at 26.3 g / min, and the temperature of the second polymerization reactor was changed to 82°C, and styrene was newly added to the second reactor at 1.98 g / min.

[0241] Example 9 A modified conjugated diene polymer of Example 9 was obtained in the same manner as in Example 1, except that the rates of 1,3-butadiene and styrene supplied to the first reactor were changed to 19.5 g / min and 2.66 g / min, respectively, and the rate of 1,3-butadiene added to the second reactor was changed to 10.5 g / min, and 2,2-bis(2-oxolanyl)propane was added as a polar substance at 0.0177 mmol / min, and styrene was newly added to the second reactor at 0.67 g / min.

[0242] Example 10 A modified conjugated diene polymer of Example 10 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane supplied to the first reactor were 0.0408 mmol / min, n-butyllithium as a polymerization initiator was 0.442 mmol / min, the rate of 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.776 mmol / min, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.018 mmol / min and 0.168 mmol / min, respectively.

[0243] Example 11 A modified conjugated diene-based polymer of Example 11 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane supplied to the first reactor were 0.0271 mmol / min, n-butyllithium as a polymerization initiator was 0.297 mmol / min, the rate of 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.461 mmol / min, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.0125 mmol / min and 0.117 mmol / min, respectively.

[0244] Example 12 A modified conjugated diene-based polymer of Example 12 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane supplied to the first reactor were 0.0190 mmol / min, n-butyllithium as a polymerization initiator was 0.187 mmol / min, the rate of 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.362 mmol / min, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.0084 mmol / min and 0.0783 mmol / min, respectively.

[0245] Example 13 A modified conjugated diene-based polymer of Example 13 was obtained in the same manner as in Example 1, except that the 2,2-bis(2-oxolanyl)propane supplied to the first reactor was 0.0084 mmol / min, n-butyllithium as a polymerization initiator was 0.065 mmol / min, 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.168 mmol / min, coupling agent A added in the modification step was 0.0130 mmol / min, coupling agent B was not added, and the amount of SRAE oil added was changed to 25 g per 100 g of polymer.

[0246] (Example 14) A modified conjugated diene polymer of Example 14 was obtained in the same manner as in Example 1, except that the coupling agent A added in the modification step was changed to 0.0067 mmol / min and the coupling agent B was changed to 0.0627 mmol / min.

[0247] Example 15 A modified conjugated diene polymer of Example 15 was obtained in the same manner as in Example 1, except that the coupling agent added in the modification step was changed to 0.0895 mmol / min of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (coupling agent C) instead of coupling agent A and coupling agent B.

[0248] Example 16 A conjugated diene-based polymer of Example 16 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane and n-butyllithium as a polymerization initiator supplied to the first reactor were changed to 0.0200 mmol / min and 0.198 mmol / min, respectively, the rate of 2,2-bis(2-oxolanyl)propane added to the second reactor was changed to 0.379 mmol / min, and both of the coupling agent A and the coupling agent B added in the modification step were changed to 0.

[0249] Example 17 A conjugated diene-based polymer of Example 17 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane supplied to the first reactor were 0.013 mmol / min, n-butyllithium as a polymerization initiator was 0.12 mmol / min, the rate of 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.253 mmol / min, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.0059 mmol / min and 0.0546 mmol / min, respectively.

[0250] Example 18 A conjugated diene-based polymer of Example 18 was obtained in the same manner as in Example 1, except that the 2,2-bis(2-oxolanyl)propane supplied to the first reactor was 0.012 mmol / min, n-butyllithium as a polymerization initiator was 0.213 mmol / min, 2,2-bis(2-oxolanyl)propane added to the second reactor was 0.405 mmol / min, coupling agent A added in the modification step was 0.0312 mmol / min, coupling agent B was not added, and the amount of SRAE oil added was changed to 25 g per 100 g of polymer.

[0251] Example 19 A modified conjugated diene polymer of Example 19 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane to be supplied to the first reactor were 0.0209 mmol / min, n-butyllithium as a polymerization initiator was 0.208 mmol / min, n-butyllithium for residual impurity inactivation treatment was 0.114 mmol / min, 1,3-butadiene was 21.6 g / min, styrene was 4.57 g / min, and normal hexane was 153 g / min, and the rates of 2,2-bis(2-oxolanyl)propane to be added to the second reactor were 0.396 mmol / min, normal hexane was 35.5 g / min, and 1,3-butadiene was 7.16 g / min, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.00917 mmol / min and 0.0856 mmol / min.

[0252] Reference Example 1 A modified conjugated diene polymer of Reference Example 1 was obtained in the same manner as in Example 1, except that the rate of 2,2-bis(2-oxolanyl)propane supplied to the first reactor was 0.136 mmol / min, no 2,2-bis(2-oxolanyl)propane was added to the second reactor, and the temperatures of the first and second reactors were 68°C and 73°C, respectively.

[0253] Comparative Example 1 A modified conjugated diene polymer of Comparative Example 1 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene were supplied to the first reactor at 16.8 g / min and 9.33 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 7.20 g / min.

[0254] Comparative Example 2 A modified conjugated diene polymer of Comparative Example 2 was obtained in the same manner as in Example 1, except that the 1,3-butadiene and styrene were supplied to the first reactor at 23.3 g / min and 1.00 g / min, respectively, and the 1,3-butadiene added to the second reactor was changed to 9.70 g / min.

[0255] Comparative Example 3 A modified conjugated diene-based polymer of Comparative Example 3 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane and n-butyllithium as a polymerization initiator supplied to the first reactor were changed to 0.168 mmol / min and 0.297 mmol / min, respectively, no 2,2-bis(2-oxolanyl)propane was added to the second reactor, and the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.0125 mmol / min and 0.117 mmol / min, respectively.

[0256] Comparative Example 4 A modified conjugated diene polymer of Comparative Example 4 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane and n-butyllithium as a polymerization initiator supplied to the first reactor were changed to 0.106 mmol / min and 0.187 mmol / min, respectively, and that no 2,2-bis(2-oxolanyl)propane was added to the second reactor, and that the rates of coupling agent A and coupling agent B added in the modification step were changed to 0.0084 mmol / min and 0.0783 mmol / min, respectively.

[0257] Comparative Example 5 A conjugated diene-based polymer of Comparative Example 5 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane and n-butyllithium as a polymerization initiator to be supplied to the first reactor were set to 0.115 mmol / min and 0.198 mmol / min, respectively, and no 2,2-bis(2-oxolanyl)propane was added to the second reactor, the temperatures of the first and second reactors were set to 68°C and 73°C, respectively, and the amounts of coupling agent A and coupling agent B added in the modification step were both changed to 0.

[0258] Comparative Example 6 A conjugated diene polymer of Comparative Example 6 was obtained in the same manner as in Example 1, except that the rates of 2,2-bis(2-oxolanyl)propane, n-butyllithium as a polymerization initiator, and the addition rates of 1,3-butadiene, styrene, and n-hexane to be supplied to the first reactor were changed to 0.145 mmol / min, 0.239 mmol / min, 21.0 g / min, 2.01 g / min, and 172 g / min, respectively, and the rates of 1,3-butadiene, styrene, and n-hexane to be added to the second reactor were changed to 8.99 g / min, 2.01 g / min, and 32.9 g / min, respectively, and no 2,2-bis(2-oxolanyl)propane was added to the second reactor.

[0259] Comparative Example 7 Four tank-type pressure vessels with an internal volume of 10 L, an internal height (L) to diameter (D) ratio (L / D) of 4.0, an inlet at the bottom, an outlet at the top, and a temperature-controlling jacket were connected as polymerization reactors. The polymerization step (P1) for synthesizing a first polymer segment was carried out using the first to third polymerization reactors. Pre-dehydrated 1,3-butadiene, styrene, and normal hexane were mixed at 21.3 g / min, 6.70 g / min, and 205 g / min, respectively. In a static mixer installed midway through the piping supplying this mixed solution to the inlet of the reactor, n-butyllithium for inactivating residual impurities was added at 0.104 mmol / min, mixed, and then continuously supplied to the bottom of the reactor. Furthermore, 2,2-bis(2-oxolanyl)propane as a polar substance at a rate of 0.120 mmol / min and n-butyllithium as a polymerization initiator at a rate of 0.205 mmol / min were supplied to the bottom of the first reactor, which was being vigorously mixed with a stirrer, and the internal temperatures of the three reactors were maintained at 45 to 55°C. Thereafter, when the polymerization reaction stabilized, the entire amount of the conjugated diene polymer was extracted from the top of the reactor, and an antioxidant (BHT) was added in an amount of 0.2 g per 100 g of the conjugated diene polymer, followed by removal of the solvent. Thereafter, the amount of bound aromatic vinyl monomer units (X 1 ) and the vinyl bond content in the bonded conjugated diene (Y 1 ), solid concentration (m 1 ) was measured.

[0260] Next, a step (P2) of forming a second polymer segment was carried out using a fourth polymerization reactor. The conjugated diene polymer solution was continuously supplied from the top of the first reactor to the bottom of the second reactor, and 1,3-butadiene, normal hexane, and 2,2-bis(2-oxolanyl)propane as a polar substance were added to the second reactor at rates of 5.30 g / min, 36.0 g / min, and 2.230 mmol / min, respectively, with stirring, and the reaction was continued at 60°C.

[0261] After the modification step, the conjugated diene polymer of Comparative Example 7 was obtained in the same manner as in Example 1, except that "coupling agent B" was added at a rate of 0.1200 mmol / min.

[0262]

[0263]

[0264]

[0265] [Examples 20 to 38], [Reference Example 2], [Comparative Examples 8 to 14] Using Samples 1 to 27 shown in Tables 1 to 3 as raw rubbers, rubber compositions containing each raw rubber were obtained according to the formulations shown below. Conjugated diene polymer (Samples 1 to 27): 100 parts by mass (oil excluded) Silica (trade name "Ultrasil 7000GR" manufactured by Evonik Degussa, nitrogen adsorption specific surface area 170 m 2 / g): 85.0 parts by mass Carbon black (trade name "SEAST 7HM (N234)" manufactured by Tokai Carbon Co., Ltd.): 2.0 parts by mass Silane coupling agent (trade name "Si69" manufactured by Evonik Degussa, bis(triethoxysilylpropyl)tetrasulfide): 6.8 parts by mass S-RAE oil (trade name "Process NC140" manufactured by JX Nippon Oil & Energy Corporation): 40 parts by mass Zinc oxide: 2.4 parts by mass Stearic acid: 1.25 parts by mass Antioxidant (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine): 3.5 parts by mass Sulfur: 1.0 part by mass Vulcanization accelerator 1 Tetrabenzyl thiuram disulfide: 0.5 parts by mass Vulcanization accelerator 2 N-(tert-butyl)-2-benzothiazole sulfenamide: 2.5 parts by mass Total: 246.95 parts by mass

[0266] The above materials were kneaded by the following method to obtain rubber compositions. Using an internal kneader (0.3 L capacity) equipped with a temperature control device, the raw rubber (samples 1 to 26), filler (silica, carbon black), silane coupling agent, process oil, zinc oxide, and stearic acid were kneaded in the first stage at a filling rate of 65% and a rotor rotation speed of 30 to 50 rpm. The temperature of the internal mixer was controlled, and each rubber composition (compound) was obtained at a discharge temperature of 145 to 150°C.

[0267] Next, in the second stage of mixing, the compound obtained above was cooled to room temperature, and then an antioxidant was added and mixed again to improve the dispersion of silica. In this case, the discharge temperature of the compound was adjusted to 120°C by temperature control of the mixer. After cooling, in the third stage of mixing, sulfur and vulcanization accelerators 1 and 2 were added and mixed using an open roll set at 70°C. The mixture was then molded and vulcanized in a vulcanization press at 160°C for 20 minutes. The rubber composition before vulcanization and the rubber composition after vulcanization were evaluated. Specifically, the evaluation was performed using the following methods.

[0268] [Evaluation 1 and Evaluation 2: Viscoelastic Parameters] Viscoelastic parameters were measured in torsion mode using a viscoelasticity tester "ARES" manufactured by Rheometrics Scientific Inc. Each measurement value was indexed, with the result for the rubber composition of Reference Example 2 being set at 100.

[0269] (Evaluation 1) Tan δ measured at 0°C, a frequency of 10 Hz, and a strain of 1% was used as an index of wet grip performance. A larger index indicates better wet grip performance. An index value of 80 or more was determined to have sufficient wet grip performance as a vulcanizate.

[0270] (Evaluation 2) The storage modulus G' measured at -20°C, a frequency of 10 Hz, and a strain of 1% was used as an index of low-temperature properties. A higher index indicates better winter properties. An index value of 50 or more was determined to have sufficient winter performance as a vulcanizate.

[0271] [Evaluation 3: Abrasion Resistance] Using an Acron abrasion tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.), the amount of abrasion was measured at a load of 44.4 N and 1,000 revolutions in accordance with JIS K6264-2, and the result of Reference Example 2 was indexed as 100. A larger index indicates better abrasion resistance.

[0272] [Evaluation 4: Processability] The unvulcanized modified conjugated diene polymers or conjugated diene polymers produced by the methods shown in the Examples, Reference Examples, and Comparative Examples were visually observed for cohesion (shape) immediately after being discharged from the pressure kneader (immediately after discharge following completion of kneading by the pressure kneader in the first stage of kneading), and evaluated by each panelist based on the following criteria, with 5 being the maximum score. Cohesion is an index of the processability of the vulcanized product. A higher index indicates better processability. <Evaluation Criteria> 1: The edge portions of the sheet are 50% or less smooth, resulting in very poor processability. 2: The edge portions of the sheet are more than 50% but not more than 60% smooth, resulting in poor processability. 3: The edge portions of the sheet are more than 60% but not more than 80% smooth, resulting in good processability. 4: The edge portions of the sheet are more than 80% but not more than 90% smooth, resulting in excellent processability. 5: The edge portions of the sheet are more than 90% smooth, resulting in excellent processability.

[0273] [Evaluation 5: Tensile Properties] Tensile strength and tensile elongation were measured in accordance with the tensile testing method of JIS K6251, and the product of these values ​​was indexed, with the result of Reference Example 2 being set at 100. A larger index indicates better tensile strength and tensile elongation (breaking strength). An index value of 80 or more was determined to have sufficient tensile properties as a vulcanizate.

[0274]

[0275]

[0276]

[0277] As shown in Tables 4 to 6, when compared with the rubber compositions of Examples 20 to 38 using Samples 1 to 19 in which the difference in bound styrene amount, the difference in vinyl bond amount, and the estimated glass transition temperature were all within the preferred ranges, and the rubber compositions of Reference Example 2 and Comparative Examples 8 to 14 in which Samples 20 to 27 were used, it was confirmed that the rubber compositions had an excellent balance of wet grip performance and winter performance when vulcanized, and had sufficient abrasion resistance and tensile properties.

[0278] Furthermore, when Example 30 and Comparative Example 10, and Example 31 and Comparative Example 11, which use modified conjugated diene polymers with equivalent molecular weights and estimated glass transition temperatures, were compared, it was confirmed that the Examples had an excellent balance of wet grip performance and winter performance, and had sufficient abrasion resistance and tensile properties.

[0279] Furthermore, when Example 35 and Comparative Example 12 were compared, it was confirmed that even when conjugated diene-based polymers that were not modified with each other were used, the Example had an excellent balance of wet grip performance and winter performance, abrasion resistance, and tensile properties.

[0280] This application is based on a Japanese patent application (Patent Application No. 2023-072878) filed with the Japan Patent Office on April 27, 2023, the contents of which are incorporated herein by reference.

[0281] The conjugated diene polymer of the present invention has industrial applicability as a material in fields such as tire treads, interior and exterior parts of automobiles, vibration-proof rubber, belts, footwear, foams, and various industrial goods.

Claims

1. A conjugated diene polymer having two or more polymer segments, wherein the first polymer segment has a bound aromatic vinyl monomer unit amount X 1 (mass%) and the amount of bound aromatic vinyl monomer units X of the second polymer segment 2 (mass%) and the absolute value of the difference (|X 1 -X 2 |) is 5 mass% or less, and the vinyl bond amount Y in the bonded conjugated diene of the first polymer segment is 1 (mol%) and the vinyl bond amount Y in the bonded conjugated diene of the second polymer segment 2 (mol%) difference (Y 2 -Y 1 % or more and 50 mol % or less of the conjugated diene-based polymer, and the conjugated diene-based polymer has an estimated glass transition temperature (estimated Tg) of -72°C or more and -40°C or less.

2. The conjugated diene polymer according to claim 1, wherein the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is 1.7 or more.

3. The mass ratio of the second polymer segment (r 2 The mass ratio (r 1 ) ratio (R = r 1 / r 2 2. The conjugated diene polymer according to claim 1 , wherein 4. The conjugated diene polymer according to claim 1, having a weight average molecular weight Mw of 350,000 or more and 1,350,000 or less.

5. The conjugated diene polymer according to claim 1, which has a nitrogen-containing modifying group and has a modification rate of 60% or more.

6. A method for producing a conjugated diene polymer according to claim 1, comprising: a polymerization step (P1) for forming the first polymer segment in two or more continuous reactors; and a polymerization step (P2) for forming the second polymer segment at an end of the first polymer segment obtained in (P1), wherein a polar substance is additionally added in the polymerization step (P2).

7. The method for producing a conjugated diene polymer according to claim 6, wherein a conjugated diene compound is additionally added in the polymerization step (P2).

8. The method for producing a conjugated diene polymer according to claim 6, further comprising, after the polymerization step (P2), a coupling step of reacting the conjugated diene polymer with a coupling agent having a nitrogen atom-containing group.

9. The method for producing a conjugated diene polymer according to claim 7, wherein the amount of the conjugated diene compound added in the polymerization step (P2) is 15 mass % or more of the total amount of the conjugated diene compound added.

Citation Information

Patent Citations

  • Production of polymer, polymer obtained thereby, and rubber composition containing the same

    JP1999189616A

  • Conjugated diolefin (Co)Polymer rubber, method for producing the (Co)Polymer rubber, rubber composition and tire

    JP2003171418A

  • Modified diene polymer rubber and its production method

    JP2005290355A

  • Conjugated diene polymer composition and tire

    JP2021143324A