Infrared persistently luminescent oxysulfide phosphor and luminescent composition for determining authenticity

Oxysulfide phosphors with specific activators offer infrared persistence and distinct afterglow peaks, addressing the limitations of conventional phosphors by providing enhanced authentication capabilities through their unique light-emitting characteristics.

WO2024225460A1PCT designated stage expired Publication Date: 2024-10-31NEMOTO TOKUSHIYU KAGAKU KK
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016529
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional infrared-emitting phosphors used for authenticity determination exhibit afterglow, making it difficult to distinguish between genuine and counterfeit products, and there is a need for phosphors with different light-emitting characteristics to enhance authentication methods.

Method used

Development of oxysulfide phosphors activated with specific elements, such as Yb and R, which exhibit infrared persistence with afterglow peaks around 980 nm and 1020 nm for several seconds to tens of seconds, and a luminescent composition incorporating these phosphors for authenticity determination.

Benefits of technology

The oxysulfide phosphors provide distinct afterglow characteristics in the infrared region, enabling effective authentication by maintaining detectable emission for several seconds to tens of seconds, distinguishing them from conventional phosphors and enhancing counterfeiting prevention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016529_31102024_PF_FP_ABST
    Figure JP2024016529_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This infrared persistently luminescent oxysulfide phosphor is represented by Ln2O2S:Yb, R, where Ln is at least one element selected from Y, La, Gd, and Lu, and R is at least one element selected from Mg, Sr, Ba, Zn, Ga, Zr, Mo, Mn, Sc, Hf, Ta, and Nb. The phosphor has persistent luminescence in the infrared region for several seconds to several tens of seconds after excitation due to the activator Yb3+.
Need to check novelty before this filing date? Find Prior Art

Description

Infrared afterglow oxysulfide phosphor and luminescent composition for authenticity determination

[0001] The present disclosure relates to an infrared afterglow oxysulfide phosphor and a luminescent composition that have afterglow in the infrared region and are used for authenticity determination.

[0002] In recent years, methods for determining whether a product is genuine or counterfeit have become known to prevent the counterfeiting of securities, banknotes, prepaid cards, ID cards, various travel passes, credit cards, and the like, as well as brand-name goods. One such method involves printing a mark or the like with a fluorescent-containing ink that is invisible to the naked eye to form a latent mark. The latent mark is then irradiated with light suitable for the fluorescent material, such as ultraviolet light, visible light, or infrared light, to excite the fluorescent material. The latent mark can be detected with the naked eye if the light emitted from the fluorescent material is visible light, or by receiving the light with an optical reader or the like if the light is infrared. According to this method, since the latent mark used for authenticity determination is difficult to see with the naked eye, it is difficult for counterfeiters to print the latent mark, thereby enabling reliable detection of counterfeit or altered cards and goods. Furthermore, since the content recorded by the latent mark is known only to the genuine card manufacturer or product manufacturer, counterfeiting or altering cards or goods is extremely difficult.

[0003] Conventionally, one type of phosphor used for such applications is a phosphor that is excited by at least one of visible light and infrared light and emits light in the infrared region. For example, the following phosphors are known as such infrared-emitting phosphors: Na 5 (Yb, Nd) (MoO 4 ) 4 (See, for example, Japanese Patent Application Laid-Open No. 3-288984.) (Y,La,Lu)PO 4 : Yb, Nd (see, for example, Japanese Patent No. 3438188) (Y, Gd, La, Lu) VO 4 : Yb, Nd (see, for example, Japanese Patent No. 4020408) These infrared emitting phosphors have emission peak wavelengths in the infrared region around 980 nm and 1020 nm.

[0004] However, some infrared-emitting phosphors, when excited by at least one of ultraviolet and visible light, emit afterglow even after the excitation is stopped. For example, the following phosphors are known as such phosphors: Sr 2 SnO 4 :Nd (See, for example, Japanese Patent No. 6249476.) These infrared afterglow phosphors have an afterglow peak wavelength around 1100 nm. For further authentication purposes, there has been a demand for phosphors with different emission characteristics to those described above, which can be distinguished from or used in combination with the above phosphors.

[0005] The present disclosure aims to provide an oxysulfide phosphor and a luminescent composition for authentication that have afterglow peaks in the infrared region around 980 nm and 1020 nm for several seconds to several tens of seconds after excitation.

[0006] As a result of examining various phosphors, the inventors have found that oxysulfide phosphors activated with specific elements have characteristic afterglow properties and are useful as the above-mentioned infrared afterglow oxysulfide phosphors and luminescent compositions for authenticity determination.

[0007] The present disclosure includes the following aspects. 2 O 2 <2> The infrared afterglow oxysulfide phosphor according to <1>, wherein the crystal has lattice defects. <3> Ln is at least one element selected from Y, La, Gd, and Lu, and R is at least one element selected from Mg, Sr, Ba, Zn, Ga, Zr, Mo, Mn, Sc, Hf, Ta, and Nb. 2-x-y O 2 S: Yb x , R yAn infrared afterglow oxysulfide phosphor represented by the formula (1), wherein Ln is at least one element selected from Y, La, Gd, and Lu, R is at least one element selected from Mg, Sr, Ba, Zn, Ga, Zr, Mo, Mn, Sc, Hf, Ta, and Nb, and x and y satisfy 0<x<0.4 and 0<y<1.0. <4> The infrared afterglow oxysulfide phosphor according to any one of <1> to <3>, wherein Ln is Y. <5> The infrared afterglow oxysulfide phosphor according to any one of <1> to <3>, wherein Ln is Gd. <6> The infrared afterglow oxysulfide phosphor according to any one of <1> to <5>, wherein R is at least one element selected from Mg and Ga. <7> A light-emitting composition for determining authenticity, comprising the infrared afterglow oxysulfide phosphor according to any one of <1> to <6>.

[0008] According to the infrared afterglow oxysulfide phosphor and luminescent composition for authentication determination of the present disclosure, it is possible to obtain an oxysulfide phosphor and a luminescent composition for authentication determination that have afterglow in the infrared region for several seconds to several tens of seconds after excitation.

[0009] FIG. 1 is a graph showing the spectrum of afterglow emission of the infrared afterglow oxysulfide phosphor in Example 2 according to the present disclosure, measured with a silicon photodiode detector. FIG. 2 is a graph showing the spectrum of afterglow emission of the infrared afterglow oxysulfide phosphor in Example 2 according to the present disclosure, measured with an InGaAs photodiode detector. FIG. 3 is a graph showing the spectrum of afterglow emission of the infrared afterglow oxysulfide phosphors in Examples 1 to 2 and Comparative Example 2 according to the present disclosure, measured with a silicon photodiode detector. FIG. 4 is a graph showing the spectrum of afterglow emission of the infrared afterglow oxysulfide phosphors in Examples 2, 10, and 13 and Comparative Example 2 according to the present disclosure, measured with a silicon photodiode detector. FIG. 5 is a graph showing glow curves obtained by thermoluminescence measurement of the infrared afterglow oxysulfide phosphor in Example 1 according to the present disclosure and the infrared oxysulfide phosphor in Comparative Example 1.

[0010] Next, as one embodiment of the present disclosure, an example of a process for producing the infrared afterglow oxysulfide phosphor of the present disclosure will be described.

[0011] (Synthesis of Infrared Afterglow Oxysulfide Phosphor) First, an example of a method for synthesizing an infrared afterglow oxysulfide phosphor will be described. The raw material of the infrared afterglow oxysulfide phosphor is, for example, yttrium oxide (Y 2 O 3 ), elemental sulfur (S) as a raw material for sulfur (S), and ytterbium oxide (Yb) as a raw material for ytterbium (Yb) used as an activator. 2 O 3 ), and magnesium carbonate (MgCO ) as a raw material for magnesium (Mg) used as a coactivator. 3 ), and as a raw material for gallium (Ga), for example, gallium oxide (Ga 2 O 3 ) is prepared. These raw materials for the phosphor and the flux are weighed out in predetermined amounts and mixed to produce a mixed powder of raw materials. Here, oxides are used as examples of raw materials, but other compounds that change into oxides when fired, such as carbonates, may also be selected. For example, sodium carbonate (Na 2 CO 3 ) and sodium bicarbonate (NaHCO 3 ) and lithium phosphate (Li 3 P.O. 4 ) and potassium phosphate (K 3 P.O. 4 ) and potassium hydrogen phosphate (K 2 HPO 4 ), phosphates such as boric acid (H 3 BO 3 ), boron compounds such as potassium sulfate (K 2 SO 4Alkali metal sulfates such as ammonium hydroxide, ammonium hydroxide, and ammonium hydroxide are preferably used. In this mixing process, the raw material powders are placed in a pot containing alumina balls and mixed using a ball mill to create a uniform mixture. This mixed powder is then filled into a heat-resistant container such as an alumina crucible. This may be further placed in a larger quartz crucible to create a double crucible. The resulting mixture is placed in an electric furnace and fired at a temperature ranging from 900°C to 1300°C, preferably from 950°C to 1250°C, for 1 hour to 8 hours, preferably from 2 hours to 6 hours. After this firing process, the resulting material is subjected to appropriate steps such as crushing, washing, drying, and sieving to obtain a phosphor of the desired particle size.

[0012] (Preparation of Light-Emitting Composition) Next, a light-emitting composition for determining authenticity containing the infrared afterglow oxysulfide phosphor will be described. In order to actually provide the infrared afterglow oxysulfide phosphor on an object to be authenticated, for example, the following light-emitting composition is prepared. For example, a transparent ink is mixed with an infrared afterglow oxysulfide phosphor to prepare an ink-like light-emitting composition. This ink-like light-emitting composition can be applied to an authentic product for marking. Alternatively, a transparent resin is mixed with an infrared afterglow oxysulfide phosphor to prepare a resin-like composition. For example, this can be molded into a film and used as a part of a card, etc. Furthermore, the film-like composition can be cut into strips and mixed with paper or resin film to be used for banknotes or securities. In addition, a light-emitting composition for determining authenticity can be obtained by mixing a translucent medium with an infrared afterglow oxysulfide phosphor.

[0013] Furthermore, the infrared afterglow oxysulfide phosphor according to this embodiment may be one in which the crystals contained in the infrared afterglow oxysulfide phosphor have lattice defects.

[0014] The lattice defects may be caused by substitutional solid solution of Yb or R, or may be caused by interstitial solid solution.

[0015] Furthermore, by making lattice defects exist in the crystal structure of the crystalline body, it is possible to obtain an infrared afterglow oxysulfide phosphor that exhibits even better afterglow properties than when lattice defects are not present.

[0016] In particular, in the infrared afterglow oxysulfide phosphor according to this embodiment, Yb 3+ is at least a part of the Ln, possibly a solid solution of Yb 3+ Most of these exist in the crystal in a state substituting for Ln, and they exhibit excellent afterglow characteristics, which will be described later.

[0017] Next, as examples of the above-described embodiment, the infrared afterglow oxysulfide phosphor of the present disclosure and its characteristics will be described, although the present disclosure is not limited to these examples.

[0018] Example 1 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 7.7 g of ytterbium oxide (Yb 2 O 3 ), 4.8 g of magnesium carbonate (MgCO 3 ) and 55.1 g of elemental sulfur (S), 52.5 g of sodium carbonate (Na 2 CO 3 ), 32.7 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and flux are weighed, and the above raw materials are thoroughly mixed using a ball mill. This mixture is filled into an alumina crucible and fired in air at 1200°C for 4 hours using an electric furnace. After that, it is cooled to room temperature, recovered from the crucible, washed with water, and milled using glass beads with a diameter of 2 mm. Further, it is washed with hydrochloric acid and water five times, and then passed through a drying process and a sieving process to obtain Y 1.805 O 2 S: Yb 0.08 , Mg 0.115 The compound represented by the formula:

[0019] Example 2: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.88 O 2 S: Yb 0.005, Mg 0.115 The compound represented by the formula:

[0020] Example 3: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.8849 O 2 S: Yb 0.0001 , Mg 0.115 The compound represented by the formula:

[0021] Example 4: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.685 O 2 S: Yb 0.2 , Mg 0.115 The compound represented by the formula:

[0022] Example 5: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.9199 O 2 S: Yb 0.08 , Mg 0.0001 The compound represented by the formula:

[0023] Example 6: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.905 O 2 S: Yb 0.08 , Mg 0.015 The compound represented by the formula:

[0024] Example 7 Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.72 O 2 S: Yb 0.08 , Mg 0.2 The compound represented by the formula:

[0025] Example 8: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.52 O 2 S: Yb 0.08 , Mg 0.4 The compound represented by the formula:

[0026] Example 9: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.12 O 2 S: Yb0.08 , Mg 0.8 The compound represented by the formula:

[0027] Comparative Example 1: Y was prepared in the same manner as in Example 1, except that the elements and their molar ratios were changed as shown in Table 1. 1.92 O 2 S: Yb 0.08 The compound represented by the formula:

[0028]

[0029] Example 10: 100 g of gadolinium oxide (Gd 2 O 3 ), 0.29 g of ytterbium oxide (Yb 2 O 3 ), 2.84 g of magnesium carbonate (MgCO 3 ) and 32.9 g of elemental sulfur (S), 31.1 g of sodium carbonate (Na 2 CO 3 ), 19.5 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 O) was weighed out, and the raw materials and the flux were thoroughly mixed using a ball mill. This mixture was treated in the same manner as in Example 1 to obtain Gd 1.88 O 2 S: Yb 0.005 , Mg 0.115 The compound represented by the formula:

[0030] Example 11 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 8.1 g of lanthanum oxide (La 2 O 3 ), 0.49 g of ytterbium oxide (Yb 2 O 3 ), 4.8 g of magnesium carbonate (MgCO 3 ) and 55.9 g of elemental sulfur (S), 52.8 g of sodium carbonate (Na 2 CO 3 ), 33.1 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.78 La 0.1 O 2 S: Yb 0.005 , Mg 0.115 The compound represented by the formula:

[0031] Example 12 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 9.9 g of lutetium oxide (Lu 2 O 3 ), 0.49 g of ytterbium oxide (Yb 2 O 3 ), 4.8 g of magnesium carbonate (MgCO 3 ) and 55.9 g of elemental sulfur (S), 52.8 g of sodium carbonate (Na 2 CO 3 ), 33.1 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.78 Lu 0.1 O 2 S: Yb 0.005 , Mg 0.115 The compound represented by the formula:

[0032] Example 13 Next, 100 g of yttrium oxide (Y 2 O 3 ), 0.46 g of ytterbium oxide (Yb 2 O 3 ), 4.6 g of magnesium carbonate (MgCO 3 ), 0.044 g of gallium oxide (Ga 2 O 3 ) and 52.9 g of elemental sulfur (S), 49.9 g of sodium carbonate (Na 2 CO 3 ), 31.4 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.879 O 2 S: Yb 0.005 , Mg 0.115 , Ga 0.001 These compounds are shown in Table 2.

[0033]

[0034] Comparative Example 2: As an existing infrared afterglow phosphor, Sr 1.98 SnO 4 : Nd 0.02 A compound represented by the following formula was prepared.

[0035] Example 14 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 1.7 g of strontium carbonate (SrCO 3 ) and 50.5 g of elemental sulfur (S), 47.7 g of sodium carbonate (Na 2 CO 3 ), 32.2 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.97 O 2 S: Yb 0.005 , Sr 0.025 The compound represented by the formula:

[0036] Example 15 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.46 g of ytterbium oxide (Yb 2 O 3 ), 10.7 g of barium carbonate (BaCO 3 ) and 52.9 g of elemental sulfur (S), 49.9 g of sodium carbonate (Na 2 CO3 ), 33.8 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.88 O 2 S: Yb 0.005 , Ba 0.115 The compound represented by the formula:

[0037] Example 16: As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.91 g of zinc oxide (ZnO) and 50.5 g of elemental sulfur (S), 47.7 g of sodium carbonate (Na 2 CO 3 ), 32.2 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.97 O 2 S: Yb 0.005 , Zn 0.025 The compound represented by the formula:

[0038] Example 17 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.46 g of ytterbium oxide (Yb 2 O 3 ), 5.1 g of gallium oxide (Ga 2 O 3 ) and 52.9 g of elemental sulfur (S), 49.9 g of sodium carbonate (Na 2 CO 3 ), 33.8 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y1.88 O 2 S: Yb 0.005 , Ga 0.115 The compound represented by the formula:

[0039] Example 18 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.27 g of zirconium oxide (ZrO 2 ) and 49.9 g of elemental sulfur (S), 47.2 g of sodium carbonate (Na 2 CO 3 ), 21.9 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.99 O 2 S: Yb 0.005 , Zr 0.005 The compound represented by the formula:

[0040] Example 19 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.32 g of molybdenum oxide (MoO 3 ) and 49.9 g of elemental sulfur (S), 47.2 g of sodium carbonate (Na 2 CO 3 ), 31.9 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.99 O 2 S: Yb 0.005 , Mo 0.005 The compound represented by the formula:

[0041] Example 20: As a raw material, 100 g of yttrium oxide (Y 2O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.26 g of manganese carbonate (MnCO 3 ) and 49.9 g of elemental sulfur (S), 47.2 g of sodium carbonate (Na 2 CO 3 ), 31.9 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.99 O 2 S: Yb 0.005 , Mn 0.005 The compound represented by the formula:

[0042] Example 21 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.08 g of scandium oxide (Sc 2 O 3 ) and 49.9 g of elemental sulfur (S), 47.1 g of sodium carbonate (Na 2 CO 3 ), 31.9 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.9925 O 2 S: Yb 0.005 , Sc 0.0025 The compound represented by the formula:

[0043] Example 22 As a raw material, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.94 g of hafnium oxide (HfO 2) and 50.1 g of elemental sulfur (S), 47.3 g of sodium carbonate (Na 2 CO 3 ), 32.0 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.985 O 2 S: Yb 0.005 , Hf 0.01 The compound represented by the formula:

[0044] Example 23 Next, 100 g of yttrium oxide (Y 2 O 3 ), 0.44 g of ytterbium oxide (Yb 2 O 3 ), 0.25 g of tantalum pentoxide (Ta 2 O 5 ) and 50.0 g of elemental sulfur (S), 47.1 g of sodium carbonate (Na 2 CO 3 ), 31.9 g of potassium phosphate trihydrate (K 3 P.O. 4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.9925 O 2 S: Yb 0.005 , Ta 0.0025 The compound represented by the formula:

[0045] Example 24 Next, 100 g of yttrium oxide (Y 2 O 3 ), 8.1 g of ytterbium oxide (Yb 2 O 3 ), 13.7 g of niobium pentoxide (Nb 2 O 5 ) and 52.9 g of elemental sulfur (S), 52.5 g of sodium carbonate (Na 2 CO 3 ), 32.7 g of potassium phosphate trihydrate (K 3 P.O.4 ・3H 2 The raw materials and the flux are thoroughly mixed using a ball mill. This mixture is treated in the same manner as in Example 1 to obtain Y 1.72 O 2 S: Yb 0.08 , Nb 0.2 These compounds are shown in Table 3.

[0046]

[0047] [Afterglow Spectrum Measurement] First, for Example 2, the afterglow spectrum was measured from 800 nm to 1100 nm using a multichannel spectrometer (model: PMA-12 silicon photodiode detector, manufactured by Hamamatsu Photonics). After irradiating ultraviolet light for 1 minute using an ultraviolet lamp (peak emission wavelength 365 nm) to create an excited state, the afterglow spectrum was measured using the multichannel spectrometer based on the count integrated value for 10 seconds immediately after the end of irradiation. The results are shown in Figure 1. From the obtained afterglow spectrum, Yb 3+ It can be seen that the afterglow in the infrared region with peaks around 980 nm and 1010 nm, which are characteristic of Yb ions, is observed. The afterglow spectrum from 900 nm to 1600 nm, measured by a multichannel spectrometer (model: NIRQuest InGaAs photodiode detector, manufactured by Ocean Insight), is shown in Figure 2. The obtained afterglow spectrum reveals the presence of Yb ions similar to those shown in Figure 1. 3+ It can be seen that the afterglow in the infrared region has peaks near 980 nm and 1010 nm, which are characteristic of the compound, and has no peak after 1100 nm.

[0048] [Afterglow Characteristics] Next, the afterglow characteristics were examined for Examples 1 to 9 and Comparative Examples 1 and 2. The target phosphor samples were filled into aluminum sample containers and then left in a dark place for 1 hour to remove afterglow. An ultraviolet lamp (peak emission wavelength 365 nm) was used as the excitation light source, and the ultraviolet intensity was 90 μW / m 2The sample from which the afterglow had been removed was irradiated for one minute at a position where the afterglow intensity was measured. The afterglow intensity was measured using a multichannel spectrometer similar to that shown in FIG. 1 as the integrated count value from 900 nm to 1050 nm 8 to 10 seconds after the end of irradiation. The results of Examples 1 to 2 and Comparative Example 2 are shown in FIG. 3. Furthermore, the afterglow intensities of Examples 1 to 9 and Comparative Example 2 are shown in Table 4 as relative afterglow intensities, with Comparative Example 2 being set at 100.

[0049]

[0050] From the results shown in FIG. 3 and Table 4, it can be seen that the infrared afterglow oxysulfide phosphors of Examples 1 to 9 according to the present disclosure all exhibit higher afterglow intensity than Comparative Example 2. Furthermore, Comparative Example 1 did not exhibit clear afterglow. Therefore, the afterglow intensity is based on Comparative Example 2. Thus, unlike conventional infrared afterglow phosphors, the infrared afterglow oxysulfide phosphors according to the present disclosure emit Yb in the infrared region within several seconds to several tens of seconds after excitation. 3+ It can be seen that the phosphor exhibits detectable strong afterglow with peaks near 980 nm and 1010 nm, which are characteristic of the phosphor.

[0051] The afterglow characteristics were examined for Examples 10 to 13 and Example 2. The results are shown in Fig. 4, and the relative afterglow intensity is shown in Table 5, with Comparative Example 2 set as 100.

[0052]

[0053] As shown in FIG. 4 and Table 5, the infrared afterglow oxysulfide phosphors of Examples 10 to 13 according to the present disclosure all emit Yb in the infrared region. 3+ It can be seen that the infrared afterglow oxysulfide phosphor according to the present disclosure has peaks at around 980 nm and 1010 nm, which are characteristic of the infrared afterglow phosphor, and exhibits a afterglow intensity similar to that of Example 2. Thus, unlike conventional infrared afterglow phosphors, the infrared afterglow oxysulfide phosphor according to the present disclosure emits Yb in the infrared region for several seconds to several tens of seconds after excitation. 3+ It can be seen that the phosphor exhibits detectable strong afterglow with peaks near 980 nm and 1010 nm, which are characteristic of the phosphor.

[0054] The afterglow characteristics were examined for Examples 14 to 24. The relative afterglow intensities obtained are shown in Table 6, with Comparative Example 2 set as 100.

[0055]

[0056] The results shown in Table 6 show that the infrared afterglow oxysulfide phosphors of Examples 14 to 24 according to the present disclosure all exhibit stronger afterglow intensities than Comparative Example 2.

[0057] [Thermoluminescence Measurement] Next, the afterglow characteristics and lattice defect properties of Example 1 and Comparative Example 1 were evaluated by thermoluminescence measurement. Thermoluminescence intensity was measured at a constant temperature increase rate, and the plot as a function of temperature is called a glow curve. This thermoluminescence intensity depends on the density of carriers (electrons or holes) trapped in lattice defects. Furthermore, since the lattice defect concentration and the trapped carrier density are proportional to each other, the thermoluminescence intensity also increases as the lattice defect concentration increases. Figure 5 compares the glow curves of each sample at a temperature increase rate of 20 K / s.

[0058] 5, it was revealed that the infrared afterglow oxysulfide phosphor containing Mg of Example 1 at 280 K had an increased intensity of the glow curve at 280 K compared to the infrared oxysulfide phosphor containing no Mg of Comparative Example 1. In other words, it was shown that the presence of Mg increases the concentration of lattice defects in the material, resulting in an infrared afterglow oxysulfide phosphor with strong phosphorescent properties.

[0059] As described above, the infrared afterglow oxysulfide phosphor according to the light-emitting composition for authentication of the present disclosure emits Yb in the infrared region within several seconds to several tens of seconds after excitation. 3+ This phosphor exhibits detectable afterglow with peaks around 980 nm and 1010 nm, which are characteristic of infrared afterglow phosphors. Therefore, it exhibits characteristics different from conventional infrared afterglow phosphors, and for example, Yb 3+By detecting the afterglow having peaks around 980 nm and 1010 nm, which are characteristic of the fluorescent material, the fluorescent material can be clearly distinguished from existing fluorescent materials for authenticity determination. The fluorescent material may also be used in combination with existing fluorescent materials for authenticity determination.

[0060] The disclosure of Japanese Patent Application No. 2023-073810, filed on April 27, 2023, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.

[0061] The infrared afterglow oxysulfide phosphor and the light-emitting composition for authentication of the present disclosure exhibit excellent afterglow characteristics different from those of conventional infrared afterglow phosphors, and therefore can be suitably used for forming latent image marks for authentication to prevent counterfeiting. In particular, the infrared afterglow oxysulfide phosphor and the light-emitting composition for authentication of the present disclosure, unlike conventional infrared afterglow phosphors, exhibit detectable afterglow in the infrared region for several seconds to several tens of seconds after excitation, and contain Yb 3+ Because the phosphor has peaks near 980 nm and 1010 nm, which are characteristic of existing phosphors for authenticity determination, it can be differentiated from existing phosphors for authenticity determination. Furthermore, by combining the phosphors with existing phosphors for authenticity determination, it is possible to form latent image marks with even higher security. In addition, by combining the phosphors with technologies such as ink-making, resin-making, film-making, sheet-making, and lamination, they can be suitably used to prevent counterfeiting of securities, banknotes, prepaid cards, ID cards, various travel passes, and credit cards, as well as to prevent counterfeiting of brand-name goods and genuine products. Furthermore, since the infrared-afterglow oxysulfide phosphor and the luminescent composition for authenticity determination of the present disclosure emit excellent infrared afterglow, they serve as markers when attached to a subject, making them suitable for tracing applications, enabling the subject to be identified and tracked in the dark using a night vision scope or the like. Furthermore, since the infrared-afterglow oxysulfide phosphor and the luminescent composition for authenticity determination of the present disclosure continue to emit afterglow in the infrared region, they are also expected to be used for in vivo optical imaging.

Claims

1. Ln 2 O 2 The infrared afterglow oxysulfide phosphor contains a crystal represented by S in which Yb and R are dissolved in a solid solution, wherein Ln is at least one element selected from Y, La, Gd and Lu, and R is at least one element selected from Mg, Sr, Ba, Zn, Ga, Zr, Mo, Mn, Sc, Hf, Ta and Nb.

2. The infrared afterglow oxysulfide phosphor according to claim 1, wherein the crystal has lattice defects.

3. Ln 2-x-y O 2 S: Yb x , R y wherein Ln is at least one element selected from Y, La, Gd and Lu, R is at least one element selected from Mg, Sr, Ba, Zn, Ga, Zr, Mo, Mn, Sc, Hf, Ta and Nb, and x and y satisfy 0<x<0.4 and 0<y<1.

0.

4. The infrared afterglow oxysulfide phosphor according to any one of claims 1 to 3, wherein Ln is Y.

5. The infrared afterglow oxysulfide phosphor according to any one of claims 1 to 3, wherein Ln is Gd.

6. The infrared afterglow oxysulfide phosphor according to any one of claims 1 to 3, wherein R is at least one element selected from the group consisting of Mg and Ga.

7. A luminescent composition for determining authenticity, comprising the infrared afterglow oxysulfide phosphor according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Sulfur oxide high-efficiency infrared up-conversion fluorescent powder and preparation method thereof

    CN102703080A

  • Mn-reinforced rare-earth oxysulfide upconversion luminescent material and preparation method thereof

    CN105018090A

  • Zn reinforced rare earth sulfur oxide up-conversion luminescent material and preparation method thereof

    CN105602564A

  • Up-conversion long afterglow fluorescence materials, and preparation method and application thereof

    CN106566547A

  • Fluorescent substance of rare earth element oxysulfide and x-ray detector using the same