Thermoplastic resin composition and molded article manufactured from same
The thermoplastic resin composition, combining polycarbonate, mineral filler, polyolefin-maleic anhydride graft copolymer, and ethylene-methyl acrylate copolymer, addresses the stability and impact resistance issues of polycarbonate/polyethylene terephthalate alloy resin, achieving superior performance for automotive applications.
Patent Information
- Application Number
- PCT/KR2024/005128
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-31
AI Technical Summary
Polycarbonate/polyethylene terephthalate alloy resin lacks dimensional stability, and reinforcing with mineral fillers compromises impact resistance, while adding impact modifiers reduces stability again, necessitating a composition that balances both properties.
A thermoplastic resin composition comprising 50-70% polycarbonate resin, 10-30% mineral filler, 0.5-3% polyolefin-maleic anhydride graft copolymer, and 1-5% ethylene-methyl acrylate copolymer, with a specific weight ratio, which includes additives like flame retardants and glass fibers, to enhance impact resistance and dimensional stability.
The composition achieves excellent impact resistance and dimensional stability, suitable for applications like automobile exterior materials, with notched Izod impact strength of 8 kgf·cm/cm and total energy of 48 J in falling ball impact tests.
Smart Images

Figure KR2024005128_31102024_PF_FP_ABST
Abstract
Description
Thermoplastic resin composition and molded article manufactured therefrom
[0001] It relates to a thermoplastic resin composition and a molded article manufactured therefrom.
[0002] Polycarbonate resin is one of the engineering plastics and is widely used in the plastics industry.
[0003] Polycarbonate resin exhibits high heat resistance due to its bulky molecular structure, similar to bisphenol-A, which results in a glass transition temperature (Tg) of approximately 150°C. Furthermore, the carbonyl group in the carbonate group exhibits high rotational mobility, imparting flexibility and rigidity to polycarbonate resin. Furthermore, as an amorphous polymer, it boasts excellent transparency, impact resistance, and compatibility with other resins.
[0004] However, polycarbonate resins have a drawback of low fluidity, so they are often used in alloy form with various resins to improve workability and post-processing. Among these, polycarbonate / polyethylene terephthalate alloy resins boast excellent durability, formability, heat resistance, and impact resistance, and are widely applied in fields such as electrical / electronics, automotive, construction, and other daily life materials. In particular, they are attracting attention as a material that can replace metal parts when used as automotive exterior materials.
[0005] However, polycarbonate / polyethylene terephthalate alloy resins lack dimensional stability, making them difficult to completely replace metal parts used in automobiles. Consequently, attempts have been made to supplement dimensional stability by reinforcing polycarbonate / polyethylene terephthalate alloy resins with mineral fillers. However, this method suffers from the problem of reduced impact resistance due to the mineral filler reinforcement.
[0006] In order to solve the above problem, there have been attempts to add various impact modifiers to polycarbonate / polyethylene terephthalate alloy resins reinforced with mineral fillers. However, when impact modifiers are used, impact strength is improved, but there is a problem that dimensional stability is reduced again.
[0007] Therefore, in order to solve the above problems, there is a need to develop a thermoplastic resin composition having excellent impact resistance and dimensional stability.
[0008] The present invention provides a thermoplastic resin composition having excellent impact resistance and dimensional stability, and a molded product using the same.
[0009] According to one embodiment, a thermoplastic resin composition is provided, comprising 100 parts by weight of a base resin comprising (A) 50 to 70 parts by weight of a polycarbonate resin; and (B) 30 to 50 parts by weight of a polyethylene terephthalate resin; (C) 10 to 30 parts by weight of a mineral filler; (D) 0.5 to 3 parts by weight of a polyolefin-maleic anhydride graft copolymer; and (E) 1 to 5 parts by weight of an ethylene-methyl acrylate copolymer, wherein a weight ratio of the (D) polyolefin-maleic anhydride graft copolymer to the (E) ethylene-methyl acrylate copolymer is 1:1 to 1:2.
[0010] The above (A) polycarbonate resin may have a melt flow index of 5 to 30 g / 10 min as measured under conditions of 300°C and 1.2 kg weight according to ASTM D1238.
[0011] The above (B) polyethylene terephthalate resin may have an intrinsic viscosity of 0.7 to 1.5 dl / g as measured according to ASTM D4603.
[0012] The above (C) mineral filler may be in the form of fine particles or flakes.
[0013] The above (C) mineral filler may be any one of talc, mica, or a combination thereof.
[0014] The average particle diameter (D50) of the above (C) mineral filler may be 1 ㎛ or more and 10 ㎛ or less.
[0015] The above (D) polyolefin-maleic anhydride graft copolymer may include 95 to 99 wt% of a substituted or unsubstituted polyolefin-derived component and 1 to 5 wt% of a maleic anhydride-derived component based on the total weight of the above (D) polyolefin-maleic anhydride graft copolymer.
[0016] The above (E) ethylene-methyl acrylate copolymer may include 50 to 80 wt% of an ethylene-derived component and 20 to 50 wt% of a methyl acrylate-derived component based on the total weight of the above (E) ethylene-methyl acrylate copolymer.
[0017] The thermoplastic resin composition may further include at least one additive selected from among a flame retardant, a nucleating agent, a coupling agent, glass fiber, a plasticizer, a lubricant, an antibacterial agent, a release agent, a heat stabilizer, an antioxidant, an ultraviolet stabilizer, an antistatic agent, a pigment, and a dye.
[0018] Meanwhile, a molded product using a thermoplastic resin composition according to one embodiment can be provided.
[0019] The above molded article may have a notched Izod impact strength of 8 kgf·cm / cm or more at 1 / 8 inch thickness as measured in accordance with ASTM D256.
[0020] The above molded product may have a total energy of 48 J or more in a drop impact strength evaluation measured by dropping a 5 kg weight from a height of 1 m onto a 3.2 mm thick flat specimen according to ASTM D1709.
[0021] A thermoplastic resin composition according to one embodiment and a molded article using the same have excellent impact resistance and dimensional stability, and thus can be widely applied to various purposes, and in particular, can be usefully applied to purposes such as automobile exterior materials.
[0022] Figure 1 shows specific criteria for judging the degree of impact resistance according to the fracture shape of a specimen in the evaluation of impact strength from falling balls.
[0023] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and the present invention is not limited thereto, and the present invention is defined solely by the appended claims.
[0024] According to one embodiment, a thermoplastic resin composition is provided, comprising 100 parts by weight of a base resin comprising (A) 50 to 70 parts by weight of a polycarbonate resin; and (B) 30 to 50 parts by weight of a polyethylene terephthalate resin; (C) 10 to 30 parts by weight of a mineral filler; (D) 0.5 to 3 parts by weight of a polyolefin-maleic anhydride graft copolymer; and (E) 1 to 5 parts by weight of an ethylene-methyl acrylate copolymer, wherein a weight ratio of the (D) polyolefin-maleic anhydride graft copolymer to the (E) ethylene-methyl acrylate copolymer is 1:1 to 1:2.
[0025] Hereinafter, each component included in the thermoplastic resin composition will be described in detail.
[0026] (A) Polycarbonate resin
[0027] The above (A) polycarbonate resin is a polyester having a carbonate bond, and its type is not particularly limited, and any polycarbonate resin available in the field of resin compositions can be used.
[0028] For example, it can be produced by reacting a compound selected from the group consisting of diphenols represented by the following chemical formula 1 and phosgene, halogen acid esters, carbonic esters, and combinations thereof.
[0029] [Chemical Formula 1]
[0030]
[0031] In the above chemical formula 1,
[0032] A is a linking group selected from the group consisting of a single bond, a substituted or unsubstituted C1 to C30 alkylene group, a substituted or unsubstituted C2 to C5 alkenylene group, a substituted or unsubstituted C2 to C5 alkylidene group, a substituted or unsubstituted C1 to C30 haloalkylene group, a substituted or unsubstituted C5 to C6 cycloalkylene group, a substituted or unsubstituted C5 to C6 cycloalkenylene group, a substituted or unsubstituted C5 to C10 cycloalkylidene group, a substituted or unsubstituted C6 to C30 arylene group, a substituted or unsubstituted C1 to C20 alkoxylene group, a halogen acid ester group, a carbonic acid ester group, C=O, S and SO2, and R 1 and R 2 are each independently a substituted or unsubstituted C1 to C30 alkyl group or a substituted or unsubstituted C6 to C30 aryl group, and n1 and n2 are each independently an integer from 0 to 4.
[0033] Two or more diphenols represented by the above chemical formula 1 may be combined to form a repeating unit of a polycarbonate resin.
[0034] Specific examples of the above diphenols include hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, 2,2-bis(4-hydroxyphenyl)propane (also called 'bisphenol-A'), 2,4-bis(4-hydroxyphenyl)-2-methylbutane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, Examples thereof include bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, and bis(4-hydroxyphenyl)ether. Among the above diphenols, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, or 1,1-bis(4-hydroxyphenyl)cyclohexane is preferably used. 2,2-bis(4-hydroxyphenyl)propane is more preferably used.
[0035] The above (A) polycarbonate resin may be a mixture of copolymers prepared from two or more diphenols. In addition, the polycarbonate resin may be a linear polycarbonate resin, a branched polycarbonate resin, a polyester carbonate copolymer resin, or the like.
[0036] A specific example of the linear polycarbonate resin is a bisphenol-A polycarbonate resin. A specific example of the branched polycarbonate resin is a resin produced by reacting a polyfunctional aromatic compound, such as trimellitic anhydride or trimellitic acid, with a diphenol and a carbonate. The polyester carbonate copolymer resin can be produced by reacting a difunctional carboxylic acid with a diphenol and a carbonate, and the carbonate used here can be a diaryl carbonate, such as diphenyl carbonate, or ethylene carbonate.
[0037] The above (A) polycarbonate resin may have a weight average molecular weight of 10,000 to 200,000 g / mol, for example, 14,000 to 50,000 g / mol. When the weight average molecular weight of the above (A) polycarbonate resin is within the above range, excellent impact resistance and fluidity can be obtained.
[0038] The above (A) polycarbonate resin may be included in an amount of 50 to 70 wt%, for example, 50 to 60 wt%, for example, 60 to 70 wt%, based on 100 wt% of the base resin comprising (A) polycarbonate resin and (B) polyethylene terephthalate resin. In the above weight range, the thermoplastic resin composition may exhibit excellent appearance properties and mechanical strength.
[0039] The above (A) polycarbonate resin may have a melt flow index of 5 to 30 g / 10 min, for example, 5 to 25 g / 10 min, for example, 5 to 20 g / 10 min, as measured under conditions of 300°C and 1.2 kg weight according to ASTM D1238. When the melt flow index of the above (A) polycarbonate resin is within the above range, it may exhibit excellent formability and excellent impact resistance.
[0040] Meanwhile, the above (A) polycarbonate resin can be used by mixing two or more polycarbonate resins having different weight average molecular weights or melt flow indices. By mixing and using polycarbonate resins having different weight average molecular weights or melt flow indices, it is easy to control the thermoplastic resin composition to have the desired fluidity.
[0041] (B) Polyethylene terephthalate resin
[0042] The above (B) polyethylene terephthalate resin can provide excellent chemical resistance, fluidity, and moldability to a thermoplastic resin composition.
[0043] The above (B) polyethylene terephthalate resin may be a resin obtained by a polycondensation reaction from terephthalic acid or a derivative thereof and ethylene glycol or a derivative thereof, and may include polyethylene terephthalate (PET), glycol-modified polyethylene terephthalate (PETG), polytetramethylene glycol (PTMG), polypropylene glycol (PPG), a copolymer of aliphatic polyester or aliphatic polyamide and polyethylene terephthalate (PET), and combinations thereof.
[0044] In addition, the above (B) polyethylene terephthalate resin may be a recycled polyethylene terephthalate resin regenerated from waste polyethylene terephthalate resin. Here, the waste polyethylene terephthalate resin refers to a polyethylene terephthalate resin that has been used, such as waste PET bottles, and may be a waste polyethylene terephthalate resin that has been used one or more times.
[0045] The above (B) polyethylene terephthalate resin may have an intrinsic viscosity of 0.7 to 1.5 dl / g as measured according to ASTM D4603 in order to sufficiently secure impact resistance of a molded product using the thermoplastic resin composition.
[0046] According to one embodiment, the (B) polyethylene terephthalate resin may be included in an amount of 30 to 50 wt% based on 100 wt% of the base resin, for example, 30 to 40 wt%. By including the polyethylene terephthalate resin within the above range, the thermoplastic resin composition has excellent chemical resistance, fluidity, and moldability.
[0047] (C) Mineral filler
[0048] In one embodiment, (C) the mineral filler can improve the dimensional stability of the thermoplastic resin composition.
[0049] The above (C) mineral filler may be, for example, in the form of fine particles or flakes.
[0050] As the above (C) mineral filler, mica, quartz powder, titanium dioxide, silicate, aluminosilicate, chalk, wollastonite, mica, layered clay, montmorillonite (especially ion-exchange modified organo-philic form of montmorillonite), talc, kaolin, zeolite, vermiculite, aluminum oxide, silica, magnesium hydroxide, aluminum hydroxide, glass flakes, etc. can be used, and mixtures of different mineral fillers can also be used.
[0051] In one embodiment, the (C) mineral filler may be any one of talc, mica, and combinations thereof, preferably talc.
[0052] The average particle diameter of the above (C) mineral filler may be 1 ㎛ or more, for example, 2 ㎛ or more, for example, 3 ㎛ or more, for example, 5 ㎛ or more, for example, 7 ㎛ or more, as measured by a median value (D50) in a cumulative particle size distribution curve using a particle size analyzer using laser diffraction (for example, a particle size analyzer from Malvern Panalytical) according to ISO 13320-1, and may be 10 ㎛ or less, for example, 8 ㎛ or less, for example, 5 ㎛ or less, for example, 4 ㎛ or less, and may be, for example, 1 to 6 ㎛, for example, 2 to 5 ㎛. In the above average particle diameter range, the mechanical strength and appearance of a molded product using the thermoplastic resin composition may be excellent.
[0053] The above (C) mineral filler may be included in an amount of 10 to 30 parts by weight, for example, 10 to 20 parts by weight, based on 100 parts by weight of the base resin. Within the above weight range, a thermoplastic resin composition including the (C) mineral filler and a molded product using the same may have excellent dimensional stability, heat resistance, mechanical strength, and appearance.
[0054] (D) Polyolefin-maleic anhydride graft copolymer
[0055] In one embodiment, the (D) polyolefin-maleic anhydride graft copolymer is used together with the (E) ethylene-methyl acrylate copolymer described below to impart excellent impact resistance and appearance properties to the thermoplastic resin composition.
[0056] In one embodiment, the (D) polyolefin-maleic anhydride graft copolymer may be one in which maleic anhydride is grafted onto a substituted or unsubstituted polyolefin backbone.
[0057] Examples of the olefins constituting the substituted or unsubstituted polyolefin include ethylene, propylene, 1-butene, isobutylene, 2-butene, cyclobutene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 3-methyl-1-butene, 4-methyl-1-butene, cyclopentene, 1-hexene, cyclohexene, 1-octene, 1-decene, and 1-dodecene, or combinations thereof.
[0058] In one embodiment, the (D) polyolefin-maleic anhydride graft copolymer may include 95 to 99 wt% of a substituted or unsubstituted polyolefin-derived component and 1 to 5 wt% of a maleic anhydride-derived component, based on the total weight of the (D) polyolefin-maleic anhydride graft copolymer.
[0059] The above (D) polyolefin-maleic anhydride graft copolymer may be included in an amount of 0.5 to 3 parts by weight, for example, 1 to 3 parts by weight, for example, 1 to 2 parts by weight, for example, 2 to 3 parts by weight, based on 100 parts by weight of the base resin. When the content of the (D) polyolefin-maleic anhydride graft copolymer satisfies the above-mentioned range, the thermoplastic resin composition and the molded article manufactured therefrom may exhibit excellent impact resistance and compatibility.
[0060] (E) ethylene-methyl acrylate copolymer
[0061] In one embodiment, the (E) ethylene-methyl acrylate copolymer is used together with the (D) polyolefin-maleic anhydride graft copolymer to impart excellent impact resistance and appearance properties to the thermoplastic resin composition.
[0062] The above (E) ethylene-methyl acrylate copolymer may include 50 to 80 wt% of an ethylene-derived component and 20 to 50 wt% of a methyl acrylate-derived component based on the total weight of the above (E) ethylene-methyl acrylate copolymer.
[0063] According to one embodiment, the (E) ethylene-methyl acrylate copolymer may be included in an amount of 1 to 5 parts by weight, for example, 2 to 3 parts by weight, based on 100 parts by weight of the base resin. Within the above range of parts by weight, the impact resistance of the thermoplastic resin composition may be further improved.
[0064] In one embodiment, the weight ratio of the (D) polyolefin-maleic anhydride graft copolymer to the (E) ethylene-methyl acrylate copolymer may be 1:1 to 1:2. When the components are included in the above weight ratio range, the impact resistance of the thermoplastic resin composition and the molded article manufactured therefrom may be further improved.
[0065] (F) Other additives
[0066] In addition to the components (A) to (E) described above, a thermoplastic resin composition according to one embodiment may further include one or more additives necessary to balance the properties under conditions of maintaining excellent impact resistance, dimensional stability, etc., or depending on the final use of the thermoplastic resin composition.
[0067] Specifically, the additives may include flame retardants, nucleating agents, coupling agents, glass fibers, plasticizers, lubricants, antibacterial agents, release agents, heat stabilizers, antioxidants, ultraviolet stabilizers, antistatic agents, pigments, dyes, etc., and these may be used alone or in combination of two or more.
[0068] These additives may be appropriately included within a range that does not impair the physical properties of the thermoplastic resin composition, and may be included in an amount of 20 parts by weight or less per 100 parts by weight of the base resin, but are not limited thereto.
[0069] The thermoplastic resin composition according to the present invention can be manufactured by a known method for manufacturing a thermoplastic resin composition.
[0070] For example, the thermoplastic resin composition according to the present invention can be manufactured in the form of pellets by mixing the components of the present invention and other additives and then melting / mixing them with an extruder.
[0071] A molded article according to one embodiment of the present invention can be manufactured from the thermoplastic resin composition described above.
[0072] The above molded article may have a notched Izod impact strength of 8 kgf·cm / cm or more at 1 / 8 inch thickness as measured in accordance with ASTM D256.
[0073] The above molded product may have a total energy of 48 J or more in a drop impact strength evaluation measured by dropping a 5 kg weight from a height of 1 m onto a 3.2 mm thick flat specimen according to ASTM D1709.
[0074] Hereinafter, the present invention will be described in more detail through examples and comparative examples. However, the following examples and comparative examples are for the purpose of explanation and are not intended to limit the present invention.
[0075] Examples 1 to 4 and Comparative Examples 1 to 4
[0076] The thermoplastic resin compositions of Examples 1 to 4 and Comparative Examples 1 to 4 were prepared according to the component content ratios described in Table 1 below.
[0077] The components listed in Table 1 were dry-mixed and quantitatively and continuously fed into the feed section of a twin-screw extruder (L / D = 29, diameter = 45 mm) to be melted / kneaded. At this time, the barrel temperature of the twin-screw extruder was set to about 250°C. Subsequently, the pelletized thermoplastic resin composition was dried at about 100°C for about 2 hours through the twin-screw extruder, and then a specimen for measuring physical properties was injection-molded using a 6 oz injection molding machine with a cylinder temperature of about 270°C and a mold temperature of about 60°C.
[0078] In Table 1, (A) and (B) represent the weight % of each component among 100 weight % of the base resin, and (C) to (E) represent the weight parts based on 100 weight parts of the base resin ((A) + (B)).
[0079] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 (A) 65656565656565 (B) 35353535353535 (C) 2020201020202040 (D) 12112121 (E) 221.52-312
[0080] A description of each component listed in Table 1 above is as follows.
[0081] (A) Polycarbonate resin
[0082] Bisphenol-A polycarbonate resin (Lotte Chemical Co.) with a melt flow index of approximately 18 g / 10 min measured at 300°C and 1.2 kg weight according to ASTM D1238
[0083] (B) Polyethylene terephthalate resin
[0084] Polyethylene terephthalate resin (Lotte Chemical Co., Ltd.) with an intrinsic viscosity of approximately 1.2 dl / g as measured according to ASTM D4603
[0085] (C) Mineral filler
[0086] Talc (IMERYS, JETFINE 3CA) with a median value (D50) of approximately 4.4 μm on the cumulative particle size distribution curve measured according to ISO 13320-1
[0087] (D) Polyolefin-maleic anhydride graft copolymer
[0088] Polyethylene-maleic anhydride graft copolymer containing approximately 1.3 wt% of maleic anhydride-derived components (Lotte Chemical Co., Ltd., EM-101)
[0089] (E) ethylene-methyl acrylate copolymer
[0090] Ethylene-methyl acrylate copolymer containing approximately 24 wt% methyl acrylate (DOW, AC 12024)
[0091]
[0092] Experimental example
[0093] The experimental results are shown in Table 2 below.
[0094] (1) Impact resistance (unit: kgf·cm / cm): The notched Izod impact strength was measured at room temperature (approximately 23℃) for a 1 / 8 inch thick specimen according to ASTM D256.
[0095] (2) Dimensional stability (unit: μm / m·℃): According to ASTM E831, a specimen measuring 6 mm x 12 mm x 10 mm in length x width x height was subjected to stress relief at temperatures ranging from -50°C to 130°C in the direction of resin flow (transverse direction) using a thermomechanical analyzer (TA Instruments, Q400). The linear expansion coefficient of the specimen in the direction of resin flow was measured at temperatures ranging from -30°C to 30°C. A lower linear expansion coefficient was considered to indicate better dimensional stability.
[0096] (3) Practical impact resistance (unit: J): According to ASTM D1709, the total energy at the time of specimen fracture was measured through the falling dart impact (FDI) evaluation in which a 5 kg weight (dart) was dropped from a height of 1 m on a 3.2 mm thick flat specimen. After the evaluation, the fracture shape of the specimen was visually observed to determine the degree of impact resistance. The specific judgment criteria for determining the degree of impact resistance according to the fracture shape of the specimen in the falling dart impact strength evaluation are shown in Fig. 1. As shown in Fig. 1, if the specimen was not broken but only deformed after the weight was dropped, it was evaluated as O, if it was slightly broken, it was evaluated as △, and if it was completely broken and fragmented, it was evaluated as ×.
[0097] Unit Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Izod impact strength kgf·cm / cm 9 10 8 20 5 9 6 3 Coefficient of linear expansion μm / m·℃ 4 3 4 4 4 1 5 2 4 0 4 6 4 2 3 5 Degree of impact resistance in the city due to falling ball impact - OOOO△O△ × Total energy in the city due to falling ball impact J 4 8 4 8 4 8 4 8 3 8 4 8 4 0 2 0
[0098] From the above Tables 1 and 2, it can be seen that by using polycarbonate resin, polyethylene terephthalate resin, mineral filler, polyolefin-maleic anhydride graft copolymer, and ethylene-methyl acrylate copolymer in optimal amounts, a thermoplastic resin composition having excellent impact resistance and dimensional stability and a molded article using the same can be produced.
[0099] In particular, in the present example, when evaluating the impact strength of a falling ball, ductile failure occurs in which the specimen is not broken but only deformed, whereas brittle failure occurs in which the specimen is broken or fragmented in Comparative Examples 1, 3, and 4. These results indicate that the impact resistance of a thermoplastic resin composition and a molded article manufactured therefrom can be particularly improved by including the above components within a specific range, and particularly by including a weight ratio of a polyolefin-maleic anhydride graft copolymer and an ethylene-methyl acrylate copolymer of 1:1 to 1:2.
[0100] Although the present invention has been described above through preferred embodiments as described above, the present invention is not limited thereto, and those engaged in the technical field to which the present invention pertains will readily understand that various modifications and variations are possible without departing from the concept and scope of the patent claims described below.
Claims
1. (A) 50 to 70 wt% of polycarbonate resin; and (B) 30 to 50 wt% of polyethylene terephthalate resin For 100 parts by weight of base resin containing (C) 10 to 30 parts by weight of mineral filler; (D) 0.5 to 3 parts by weight of polyolefin-maleic anhydride graft copolymer; and (E) Containing 1 to 5 parts by weight of ethylene-methyl acrylate copolymer, A thermoplastic resin composition wherein the weight ratio of the above (D) polyolefin-maleic anhydride graft copolymer to the (E) ethylene-methyl acrylate copolymer is 1:1 to 1:
2.
2. In paragraph 1, The above (A) polycarbonate resin is a thermoplastic resin composition having a melt flow index of 5 to 30 g / 10 min, measured under conditions of 300°C and 1.2 kg weight according to ASTM D1238.
3. In paragraph 1 or 2, The above (B) polyethylene terephthalate resin is a thermoplastic resin composition having an intrinsic viscosity of 0.7 to 1.5 dl / g as measured according to ASTM D4603.
4. In any one of paragraphs 1 to 3, The above (C) mineral filler is a thermoplastic resin composition in the form of fine particles or flakes.
5. In any one of paragraphs 1 to 4, A thermoplastic resin composition wherein the above (C) mineral filler is any one of talc, mica, and a combination thereof.
6. In any one of paragraphs 1 to 5, A thermoplastic resin composition, wherein the average particle diameter (D50) of the above (C) mineral filler is 1 ㎛ or more and 10 ㎛ or less.
7. In any one of paragraphs 1 to 6, The above (D) polyolefin-maleic anhydride graft copolymer is a thermoplastic resin composition comprising 95 to 99 wt% of a substituted or unsubstituted polyolefin-derived component and 1 to 5 wt% of a maleic anhydride-derived component based on the total weight of the polyolefin-maleic anhydride graft copolymer.
8. In any one of paragraphs 1 to 7, The above (E) ethylene-methyl acrylate copolymer is a thermoplastic resin composition comprising 50 to 80 wt% of an ethylene-derived component and 20 to 50 wt% of a methyl acrylate-derived component based on the total weight of the ethylene-methyl acrylate copolymer.
9. In any one of paragraphs 1 to 8, A thermoplastic resin composition further comprising at least one additive selected from among flame retardants, nucleating agents, coupling agents, glass fibers, plasticizers, lubricants, antibacterial agents, release agents, heat stabilizers, antioxidants, ultraviolet stabilizers, antistatic agents, pigments, and dyes.
10. A molded product using a thermoplastic resin composition according to any one of claims 1 to 9.
11. In paragraph 10, The above molded product is a molded product having a notched Izod impact strength of 8 kgf·cm / cm or more measured according to ASTM D256 at a thickness of 1 / 8 inch.
12. In paragraph 10 or 11, The above molded product is a molded product having a total energy of 48 J or more in a drop impact strength evaluation measured by dropping a 5 kg weight from a height of 1 m onto a 3.2 mm thick flat specimen according to ASTM D1709.
Citation Information
Patent Citations
Modification of engineering plastics using olefin-maleic anhydride copolymers
KR1020170054382A
Polycarbonate resin composition having excellent thermal decomposition resistance
US20180155543A1
Thermoplastic Resin Composition and Molded Article Formed Therefrom
US20220033650A1
Thermoplastic polyester compositions having improved impact properties
US7119152B1
Polycarbonate resin composition and molded product comprising same
WO2016108539A1