Biodegradable polymer dispersion and method for producing same
The method of warming a biodegradable polymer emulsion at lower temperatures and adding additives enhances bacterial resistance and stability in biodegradable polymer dispersions, addressing their vulnerability to bacteria and maintaining physical properties, thus extending shelf life and usability as a coating solution.
Patent Information
- Application Number
- PCT/KR2024/005617
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Biodegradable polymer dispersions, such as polyhydroxyalkanoate (PHA), are vulnerable to bacteria due to their large specific surface area and moisture content, leading to low resistance and stability, and existing methods like antibacterial agent introduction or high-temperature sterilization either limit bacterial resistance or degrade the polymer's physical properties.
A method involving the preparation of an emulsion by mixing a biodegradable polymer with an emulsifier, warming it at a lower temperature (50°C to 80°C) to minimize molecular weight reduction, and adding additives like thickeners, waxes, and antibacterial agents in stages to enhance bacterial resistance while maintaining the polymer's physical properties.
The approach results in a biodegradable polymer dispersion with significantly improved bacterial resistance and long-term storage stability, allowing for extended shelf life and effective use as a coating solution for various products without compromising the polymer's physical properties.
Smart Images

Figure KR2024005617_31102024_PF_FP_ABST
Abstract
Description
Biodegradable polymer dispersion and method for producing the same
[0001] The present invention relates to a biodegradable polymer dispersion and a method for producing the same.
[0002] As environmental problems become more serious due to the indiscriminate use of synthetic plastics, interest in biodegradable polymers that have similar properties to synthetic plastics and can be naturally decomposed by microorganisms in the soil or ocean is increasing.
[0003] Polyhydroxyalkanoate (PHA), one of the above biodegradable polymers, has the advantages of excellent mechanical properties, oil resistance, water resistance, etc., and complete biodegradability. Due to these advantages, polyhydroxyalkanoate (PHA) dispersions containing dispersed polyhydroxyalkanoate (PHA) particles are used to form coating layers to increase the lifespan and recyclability of various products such as films, fibers, packaging materials, and bottles.
[0004] However, biodegradable polymer dispersions, such as the polyhydroxyalkanoate (PHA) dispersion, have the problem of being vulnerable to bacteria. That is, the biodegradable polymer particles present in the dispersion have a large specific surface area with a size of several micrometers or less, and the dispersion contains sufficient moisture for bacterial growth, so the biodegradable polymer dispersion has low resistance (stability) to bacteria.
[0005] Therefore, in order to increase the resistance of biodegradable polymer dispersions to bacteria, methods such as introducing antimicrobial agents into the dispersions or sterilizing the manufactured dispersions at high temperatures have been attempted. However, the method of introducing antimicrobial agents has limitations in increasing the resistance to bacteria to the required level due to the limitations on the amount of antimicrobial agents used. In addition, the high-temperature sterilization treatment is performed at a high temperature of 145°C or higher, which is applied to sterilize synthetic plastics. Although this can sterilize biodegradable polymer dispersions, it has the problem of lowering the physical properties of the biodegradable polymers by reducing the molecular weight of biodegradable polymers that are weak to heat.
[0006] In order to solve the above-mentioned conventional problems, the task of the present invention is to provide a biodegradable polymer dispersion having high resistance to bacteria even when using a small amount of antibacterial agent while maintaining the basic physical properties of a biodegradable polymer that is relatively weak to heat, and a method for producing the same.
[0007] To achieve the above object, the present invention provides a method for producing a biodegradable polymer dispersion, comprising: (1) a step of producing an emulsion by mixing a biodegradable polymer and an emulsifier; (2) a step of warming the emulsion; and (3) a step of mixing the warmed emulsion with an additive.
[0008] According to one embodiment of the present invention, the heating treatment in step (2) can be performed at 50°C to 80°C.
[0009] According to another embodiment of the present invention, the heating treatment in step (2) may be performed for 10 to 30 minutes.
[0010] According to another embodiment of the present invention, the method for producing the biodegradable polymer dispersion may further include a step of filtering the emulsion before the heating treatment in step (2).
[0011] According to another embodiment of the present invention, the additive of step (3) may include at least one selected from the group consisting of a thickener, a wax, an antifoaming agent, and an antibacterial agent.
[0012] According to another embodiment of the present invention, the step (3) may include: (3-1) adding and mixing a first additive including a thickener to the heated emulsion; (3-2) adding and mixing a second additive including a wax to the emulsion mixed with the first additive; and (3-3) adding and mixing a third additive including at least one selected from the group consisting of a defoaming agent and an antibacterial agent to the emulsion mixed with the second additive.
[0013] According to another embodiment of the present invention, the amount of the antibacterial agent added in step (3-3) may be 0.001 wt% to 0.5 wt% based on the total weight of the biodegradable polymer dispersion.
[0014] According to another embodiment of the present invention, the biodegradable polymer of step (1) has an average particle diameter (D 50 ) may have a particle shape of 0.5 ㎛ to 5.0 ㎛.
[0015] According to another embodiment of the present invention, the biodegradable polymer of step (1) may include at least one selected from the group consisting of polyhydroxyalkanoate (PHA), polylactic acid (PLA), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), and polycaprolactone (PCL).
[0016] According to another embodiment of the present invention, the polyhydroxyalkanoate may be a poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer.
[0017] According to another embodiment of the present invention, the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer may contain 6 to 20 wt% of repeating units derived from 4-hydroxybutyrate, based on the total weight of the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer.
[0018] According to another embodiment of the present invention, the emulsifier of step (1) may include at least one selected from the group consisting of polyvinyl alcohol (PVA), sodium dodecyl sulfonate (SDS), coco-betaine, and lecithin.
[0019] Meanwhile, in order to achieve the above task, the present invention provides a biodegradable polymer dispersion prepared by the above preparation method.
[0020] According to one embodiment of the present invention, the biodegradable polymer dispersion may have a viscosity of 10 cP to 3,000 cP as measured by a Brookfield viscometer at 25°C.
[0021] The present invention manufactures a biodegradable polymer dispersion by emulsifying a biodegradable polymer, heating the obtained emulsion at a temperature much lower than the conventional high-temperature sterilization temperature, and then adding an additive. Therefore, it is possible to provide a biodegradable polymer dispersion with significantly improved resistance (stability) to bacteria while maintaining the properties of a biodegradable polymer that is weak to heat.
[0022] Therefore, the biodegradable polymer dispersion according to the present invention has high resistance (stability) to bacteria and thus excellent long-term storage stability, thereby extending the shelf life of the dispersion compared to the conventional one.
[0023] In addition, the biodegradable polymer dispersion according to the present invention can be usefully used as a coating solution to increase the lifespan and recyclability of various products such as films, fibers, packaging materials, bottles, etc., due to the excellent physical properties of the biodegradable polymer contained in the dispersion.
[0024] Figure 1 is a flow chart schematically showing a method for manufacturing a biodegradable polymer dispersion according to one embodiment of the present invention.
[0025] Figure 2 is an image showing the results of a bacterial contamination test in Test Example 1.
[0026] Hereinafter, the present invention will be described in detail. However, the present invention is not limited to the contents disclosed below, and may be modified in various forms as long as the gist of the invention is not changed.
[0027] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.
[0028] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification are to be understood as being modified by the term “about” in all cases unless otherwise specified.
[0029] The terms first, second, etc. described in this specification are used to describe various components, and the components are not limited by the terms, and the terms may be used only for the purpose of distinguishing one component from another.
[0030]
[0031] The present invention, unlike the conventional method of sterilizing a biodegradable polymer dispersion after it has been manufactured, performs a heating treatment at a relatively low temperature during the manufacturing process of the biodegradable polymer dispersion to complete the manufacturing of the biodegradable polymer dispersion, thereby providing a biodegradable polymer dispersion having significantly improved resistance (stability) to bacteria. The present invention will be described in detail as follows.
[0032]
[0033] Method for producing biodegradable polymer dispersion
[0034] The method for producing a biodegradable polymer dispersion according to the present invention comprises: (1) a step of producing an emulsion by mixing a biodegradable polymer and an emulsifier; (2) a step of heating the emulsion; and (3) a step of mixing the heated emulsion with an additive.
[0035] Below, each step is described with reference to Figure 1.
[0036]
[0037] Step (1): Preparation of emulsion
[0038] According to the present invention, step (1) is a step of preparing an emulsion by mixing a biodegradable polymer and an emulsifier. Specifically, step (1) is a step of emulsifying the biodegradable polymer.
[0039] The biodegradable polymer may not be particularly limited as long as it is a polymer that can be naturally decomposed by microorganisms in the soil or ocean. Specifically, the biodegradable polymer may include at least one selected from the group consisting of polyhydroxyalkanoate (PHA), polylactic acid (PLA), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), and polycaprolactone (PCL). Preferably, the biodegradable polymer may be polyhydroxyalkanoate (PHA) that has excellent mechanical properties, oil resistance, water resistance, etc., and is completely biodegradable.
[0040] The above polyhydroxyalkanoate (PHA) may be obtained through cell disruption of a microorganism using a mechanical or physical method, or may be obtained through cell disruption of a microorganism using a non-mechanical or chemical method.
[0041] The above polyhydroxyalkanoate may have a weight average molecular weight (Mw) of, but is not limited to, 100,000 g / mol to 800,000 g / mol, 125,000 g / mol to 775,000 g / mol, 150,000 g / mol to 750,000 g / mol, 175,000 g / mol to 725,000 g / mol, or 200,000 g / mol to 700,000 g / mol.
[0042] These polyhydroxyalkanoates are selected from at least one selected from the group consisting of 3-hydroxybutyrate (3-HB), 3-hydroxypropionate (3-HP), 3-hydroxyvalerate (3-HV), 3-hydroxyhexanoate (3-HH), 4-hydroxybutyrate (4-HB), 4-hydroxyvalerate (4-HV), 4-hydroxyhexanoate (4-HH), 5-hydroxyvalerate (5-HV) and 6-hydroxyhexanoate (6-HH) (from at least one monomer). It may be a copolymer containing a derived repeating unit, but is not limited thereto.
[0043] The above polyhydroxyalkanoate may be crystalline polyhydroxyalkanoate (cPHA), semi-crystalline polyhydroxyalkanoate (scPHA), or amorphous polyhydroxyalkanoate (aPHA) depending on the type of the monomer and the content of the repeating unit derived therefrom. For example, the polyhydroxyalkanoate may be classified as cPHA, scPHA, or aPHA by controlling its crystallinity depending on the content of the repeating unit derived from 4-hydroxybutyrate (4-HB).
[0044] Specifically, the polyhydroxyalkanoate may be a poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer comprising a repeating unit derived from the 3-hydroxybutyrate (3-HB) and a repeating unit derived from the 4-hydroxybutyrate (4-HB).
[0045] The poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer may contain, based on the total weight of the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer, a repeating unit derived from 4-hydroxybutyrate (4-HB) (4-HB repeating unit), in an amount of 6 wt% to 20 wt%, but is not limited thereto. Specifically, the content of the 4-HB repeating unit may be 6.5 wt% to 19 wt%, 7 wt% to 18 wt%, 7.5 wt% to 17 wt%, 8 wt% to 16 wt%, 8 wt% to 15 wt%, 8.5 wt% to 15 wt%, 9 wt% to 14 wt%, or 9.5 wt% to 13 wt%, based on the total weight of the copolymer. As the content of the above 4-HB repeating unit is within the above range, the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer may be a semi-crystalline PHA (scPHA) or an amorphous PHA (aPHA), and the dispersion of the present invention in which such PHA is dispersed as the biodegradable polymer can form a coating layer having excellent mechanical properties, oil resistance, water resistance, heat resistance, etc.
[0046] The biodegradable polymer may have a particle shape controlled to a predetermined size. Specifically, the biodegradable polymer is a biodegradable polymer particle, and has an average particle diameter (D 50 ) may be 0.5 ㎛ to 5.0 ㎛, but is not limited thereto. For example, the biodegradable polymer particles may have an average particle diameter (D 50 ) may be 0.6 ㎛ to 4.9 ㎛, 0.7 ㎛ to 4.8 ㎛, 0.8 ㎛ to 4.7 ㎛, 0.9 ㎛ to 4.6 ㎛, 1 ㎛ to 4.5 ㎛, 1.1 ㎛ to 4.4 ㎛, 1.2 ㎛ to 4.3 ㎛, or 1.2 ㎛ to 4.2 ㎛. The average particle diameter (D of the biodegradable polymer particles 50) is within the above range, a biodegradable polymer dispersion having excellent dispersibility can be obtained, and when a coating layer is formed on a substrate (e.g., film, etc.) using the dispersion, a coating layer having excellent mechanical properties, oil resistance, water resistance, heat resistance, etc. can be formed.
[0047] The biodegradable polymer may be mixed with the emulsifier in a crude liquid state containing the biodegradable polymer. At this time, the crude liquid containing the biodegradable polymer may contain 10 wt% to 70 wt% of the biodegradable polymer solid content based on the total weight of the crude liquid, but is not limited thereto. Specifically, the crude liquid containing the biodegradable polymer may be a crude liquid containing 20 wt% to 70 wt%, 20 wt% to 60 wt%, or 30 wt% to 50 wt% of the biodegradable polymer solid content. In addition, the crude liquid containing the biodegradable polymer may be a solution in which a biodegradable polymer (biodegradable polymer particles) is dispersed in an aqueous solvent (e.g., water).
[0048] The emulsifier may not be particularly limited as long as it is a substance capable of evenly dispersing the biodegradable polymer. Specifically, the emulsifier may include at least one selected from the group consisting of polyvinyl alcohol (PVA), sodium dodecyl sulfonate (SDS), coco betaine, and lecithin. More specifically, the emulsifier may be a PVA emulsifier in which the polyvinyl alcohol (PVA) is dispersed in an aqueous solvent (e.g., water). By applying the PVA emulsifier, an emulsion in which the biodegradable polymer is evenly and uniformly dispersed can be obtained.
[0049] The above PVA emulsifier may have a viscosity of, but is not limited to, 10 cPs to 1,000 cPs, 20 cPs to 700 cPs, 30 cPs to 500 cPs, or 40 cPs to 300 cPs.
[0050] The content of the polyvinyl alcohol (PVA) included in the PVA emulsifier may be 1 wt% to 50 wt%, 2 wt% to 40 wt%, 3 wt% to 30 wt%, or 4 wt% to 20 wt%, based on the total weight of the PVA emulsifier, but is not limited thereto.
[0051] The above polyvinyl alcohol (PVA) may have a saponification value of, but is not limited to, 1 mol% to 99 mol%, 2 mol% to 97 mol%, 3 mol% to 95 mol%, or 4 mol% to 93 mol%.
[0052] When mixing the biodegradable polymer (a) and the emulsifier (b), the mixing ratio (a:b) (based on solid content) thereof may be a weight ratio of 1:99 to 10:90, a weight ratio of 2:98 to 9:91, or a weight ratio of 3:97 to 8:92, but is not limited thereto.
[0053] The mixing of the biodegradable polymer and the emulsifier can be performed using a commonly known mixer (e.g., a homomixer, etc.). When mixing (stirring) the biodegradable polymer and the emulsifier using the mixer, the rotation speed of the mixer may be, but is not limited to, 4,000 rpm to 10,000 rpm, 5,000 rpm to 8,500 rpm, 5,300 rpm to 8,300 rpm, or 5,500 rpm to 8,200 rpm. In addition, the mixing (stirring) time using the mixer may be, but is not limited to, 15 minutes to 60 minutes, 20 minutes to 50 minutes, 20 minutes to 40 minutes, or 25 minutes to 35 minutes.
[0054]
[0055] Meanwhile, the method for producing a biodegradable polymer dispersion according to the present invention may further include a step of filtering the emulsion obtained by mixing the biodegradable polymer and the emulsifier before the heating treatment described below. By performing the step of filtering the emulsion, biodegradable polymers having a large particle size that were not dispersed during the mixing process with the emulsifier can be removed, thereby obtaining an emulsion in which biodegradable polymers having a fine particle size are uniformly dispersed.
[0056] The filtering of the above emulsion can be performed using a commonly known filter. Specifically, the filtering step can be performed by performing primary filtering or secondary or more filtering. More specifically, the filtering step includes a step of primary filtering the emulsion using a filter having a particle size of 100 μm to 150 μm (e.g., 120 μm to 145 μm, 125 μm to 140 μm, or 125 μm to 135 μm) (e.g., a filter capable of filtering biodegradable polymers having an average particle size of 120 μm to 150 μm); And it may include a step of secondarily filtering the first-filtered emulsion with a filter (e.g., a filter capable of filtering biodegradable polymers having an average particle size of 90 ㎛ to less than 120 ㎛) of 90 ㎛ to less than 300 ㎛ (e.g., 95 ㎛ to 280 ㎛, 100 ㎛ to 270 ㎛, or 100 ㎛ to 250 ㎛).
[0057]
[0058] Step (2): Emulsion heating treatment
[0059] According to the present invention, step (2) is a step of heating the emulsion (e.g., the emulsion that has optionally undergone the filtering described above). Specifically, step (2) is a step of sterilizing the emulsion by heating the emulsion at a temperature significantly lower than a conventional high-temperature sterilization temperature (e.g., 145°C or higher).
[0060] The temperature at which the emulsion is heated may be, but is not limited to, 50°C to 80°C. Specifically, the temperature at which the emulsion is heated may be 51°C to 78°C, 52°C to 78°C, 53°C to 75°C, 54°C to 75°C, 55°C to 73°C, 56°C to 73°C, 57°C to 70°C, 58°C to 70°C, 59°C to 68°C, or 60°C to 65°C.
[0061] In addition, the time for heating the emulsion may be 10 to 30 minutes, but is not limited thereto. Specifically, the time for heating the emulsion may be 11 to 30 minutes, 12 to 29 minutes, 13 to 29 minutes, 14 to 28 minutes, 15 to 28 minutes, 16 to 27 minutes, 17 to 27 minutes, 18 to 26 minutes, 18 to 25 minutes, 19 to 23 minutes, 19 to 22 minutes, or 20 to 21 minutes.
[0062] By heating the emulsion solution in the above temperature range for the above time, sterilization can be efficiently performed while minimizing changes in the physical properties of the biodegradable polymer contained in the emulsion solution (e.g., reduction in molecular weight). Therefore, by manufacturing the dispersion solution of the present invention using the emulsion solution subjected to the heating treatment, a biodegradable polymer dispersion solution having excellent resistance (stability) to bacteria and containing a biodegradable polymer with maintained physical properties can be provided.
[0063] In addition, the heating treatment of the emulsion may be performed until the viscosity of the emulsion becomes 100 cPs to 3,000 cPs. Specifically, the viscosity of the emulsion heated through the step (2) may be, but is not limited to, 200 cPs to 2,000 cPs, 300 cPs to 1,500 cPs, or 350 cPs to 1,200 cPs.
[0064]
[0065] Step (3): Mixing the emulsion and additives
[0066] According to the present invention, step (3) is a step of mixing the heated emulsion with an additive. Specifically, step (3) is a step of formulating an emulsion by mixing the heated emulsion with two or more additives.
[0067] The above additive may not be particularly limited as long as it is a commonly known additive. Specifically, the additive may include at least one selected from the group consisting of a thickener, a wax, an anti-foaming agent, and an antibacterial agent. More specifically, the additive may include at least two selected from the group consisting of a thickener, a wax, an anti-foaming agent, and an antibacterial agent.
[0068] The mixing of the above additives can be performed in steps, thereby producing a biodegradable polymer dispersion that is efficiently formulated from an emulsion. Specifically, the step of mixing the additives can include: (3-1) adding a first additive including a thickener to the heated emulsion and mixing; (3-2) adding a second additive including a wax to the emulsion in which the first additive is mixed and mixing; and (3-3) adding a third additive including at least one selected from the group consisting of an antifoaming agent and an antibacterial agent to the emulsion in which the second additive is mixed and mixing.
[0069] The above step (3-1) is a step of adding and mixing a first additive including a thickener into the emulsion, thereby controlling the viscosity of the biodegradable polymer dispersion to a required level. The thickener may not be particularly limited as long as it is a substance capable of controlling the viscosity of the emulsion. Specifically, the thickener may include at least one selected from the group consisting of starch, xanthan gum, guar gum, carboxymethyl cellulose (CMC), and carrageenan.
[0070] The mixing of the above emulsion and the first additive including the thickener can be performed using a commonly known mixer (e.g., a homomixer, etc.). When mixing (stirring) the above emulsion and the first additive using the mixer, the rotation speed of the mixer may be, but is not limited to, 4,500 rpm to 9,000 rpm, 5,000 rpm to 8,500 rpm, 5,300 rpm to 8,300 rpm, or 5,500 rpm to 8,200 rpm. In addition, the mixing (stirring) time using the mixer may be, but is not limited to, 10 minutes to 30 minutes, 15 minutes to 30 minutes, or 20 minutes to 25 minutes.
[0071] The above step (3-2) is a step of adding and mixing a second additive including wax into the emulsion mixed with the first additive, thereby improving the water resistance, coatability, etc. of the biodegradable polymer dispersion. The wax may not be particularly limited as long as it is a commonly known material. Specifically, the wax may include at least one selected from the group consisting of beeswax, soy wax, and carnauba wax.
[0072] The mixing of the emulsion containing the first additive and the second additive containing the wax can be performed using a commonly known mixer (e.g., a homomixer, etc.). When mixing (stirring) the emulsion and the second additive using the mixer, the rotation speed of the mixer may be, but is not limited to, 4,500 rpm to 9,000 rpm, 5,000 rpm to 8,500 rpm, 5,300 rpm to 8,300 rpm, or 5,500 rpm to 8,200 rpm. In addition, the mixing (stirring) time using the mixer may be, but is not limited to, 10 minutes to 30 minutes, 15 minutes to 30 minutes, or 20 minutes to 25 minutes.
[0073] The above step (3-3) is a step of adding and mixing a third additive including at least one selected from the group consisting of a defoaming agent and an antibacterial agent into the emulsion mixed with the second additive, thereby improving the antibacterial properties, coating properties, etc. of the biodegradable polymer dispersion. The defoaming agent may not be particularly limited as long as it is a commonly known substance. Specifically, the defoaming agent may include at least one selected from the group consisting of a silicone defoaming agent, a mineral oil defoaming agent, and a polymer defoaming agent. In addition, the antibacterial agent may not be particularly limited as long as it is a commonly known substance. Specifically, the antibacterial agent may include at least one selected from the group consisting of alcohol, salicylic acid, benzoic acid, licorice extract, yucca extract, chitooligosaccharide, chitosan, 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (DCOIT), octylisothiazolone (OIT), and benzisothiazolone (BIT).
[0074] Meanwhile, in the step (3-3), the amount of the antimicrobial agent added to the emulsion may be, but is not limited to, 0.001 wt% to 0.5 wt% based on the total weight of the biodegradable polymer dispersion. Specifically, the amount of the antimicrobial agent added may be 0.005 wt% to 0.5 wt%, 0.005 wt% to 0.4 wt%, 0.01 wt% to 0.4 wt%, 0.01 wt% to 0.3 wt%, 0.02 wt% to 0.3 wt%, or 0.03 wt% to 0.2 wt% based on the total weight of the biodegradable polymer dispersion. As the amount of the antimicrobial agent added is within the above range, a biodegradable polymer dispersion having excellent antimicrobial properties can be provided while applying an amount suitable for international regulations (e.g., the U.S. FDA).
[0075]
[0076] In this way, the present invention manufactures a biodegradable polymer dispersion by subjecting a biodegradable polymer-containing emulsion obtained through emulsification of a biodegradable polymer to a heating treatment at a relatively low temperature of 50°C to 80°C and then mixing additives in stages to form a formulation. Therefore, it is possible to provide a biodegradable polymer dispersion having excellent resistance (stability) to bacteria while minimizing changes in the physical properties of a biodegradable polymer that is weak to heat.
[0077]
[0078] Biodegradable polymer dispersion
[0079] The present invention provides a biodegradable polymer dispersion prepared by the above-described preparation method. The biodegradable polymer dispersion according to the present invention may include the above-described biodegradable polymer (biodegradable polymer particles); the above-described emulsifier; the above-described additive; and a dispersion solvent (e.g., water, etc.).
[0080] The biodegradable polymer dispersion according to the present invention has high resistance (stability) to bacteria and thus can have excellent long-term storage stability.
[0081] In addition, the biodegradable polymer dispersion according to the present invention may have a viscosity that can secure coatability, workability, etc. Specifically, the biodegradable polymer dispersion according to the present invention may have a viscosity measured at 25°C using a Brookfield viscometer of 10 cP to 3,000 cP, and more specifically, may be 20 cP to 2,500 cP, 30 cP to 2,000 cP, 40 cP to 1,500 cP, or 50 cP to 1,000 cP, but is not limited thereto.
[0082] The biodegradable polymer dispersion according to the present invention may have a pH that ensures long-term storage stability (storage stability), etc. Specifically, the biodegradable polymer dispersion according to the present invention may have a pH of 5 to 9, and more specifically, 5.5 to 8.8, but is not limited thereto.
[0083] The biodegradable polymer dispersion according to the present invention has excellent long-term storage stability and coating properties for substrates, and thus can be usefully used as a coating solution for increasing the lifespan and recyclability of various products such as films, fibers, packaging materials, bottles, etc.
[0084] The present invention is described in more detail through the following examples. However, the scope of the present invention is not limited to these examples.
[0085]
[0086] [Example 1]
[0087] Distilled water was added to dry particles (powder) of polyhydroxyalkanoate (PHA) (Mw: 340,000 g / mol, 4-HB repeating unit content: 10 wt%, manufacturer: CJ CheilJedang) to obtain a crude solution having a solid concentration of 40 wt%. Next, the crude solution and a 10% concentration PVA emulsifier were added to a disper (product name: homogenizing disper, manufacturer: PRIMIX) at a solid concentration of 1.5 parts by weight relative to the crude solution, and mixed and stirred at 1,000 to 2,000 rpm for 5 minutes to obtain a suspension. Then, the obtained suspension was emulsified using a homogenizing mixer (product name: homogenizing mixer, manufacturer: PRIMIX) at 6,000 to 8,000 rpm for 30 minutes to prepare a PHA emulsion.
[0088] The PHA emulsion obtained by completing the above emulsification process was first filtered with a 130 μm filter and then second filtered with a 110 μm filter to remove large particles that were not emulsified.
[0089] The PHA emulsion obtained through the above first and second filtering was sterilized by heating at 60°C for 20 minutes.
[0090] The first formulation was performed by adding 0.3 wt% (based on the total weight of the PHA dispersion) of a thickener to the PHA emulsion sterilized through the above heat treatment and stirring the mixture in a homomixer at 6,000 to 8,000 rpm for 20 minutes. Next, the second formulation was performed by adding 0.9 wt% (based on the total weight of the PHA dispersion) of wax to the PHA obtained through the first formulation and stirring the mixture in a homomixer at 6,000 to 8,000 rpm for 20 minutes. Next, 0.05 wt% of a defoaming agent (based on the total weight of the PHA dispersion) and 0.05 wt% of an antimicrobial agent (based on the total weight of the PHA dispersion) were added to the PHA obtained through the second formulation, and the mixture was stirred at 6,000 to 8,000 rpm in a homomixer for 20 minutes to produce the third formulation. Thereafter, the PHA obtained through the third formulation was finally filtered through a 245 μm filter to produce a PHA dispersion.
[0091]
[0092] [Example 2]
[0093] A PHA dispersion was prepared through the same process as in Example 1, except that the PHA emulsion obtained through primary and secondary filtering in Example 1 was heated for 30 minutes.
[0094]
[0095] [Example 3]
[0096] A PHA dispersion was prepared by following the same procedure as in Example 1, except that polyhydroxyalkanoate (PHA) (Mw): 450,000 g / mol, 4-HB repeat unit content: 12.6 wt%, manufacturer: CJ CheilJedang) dry particles (powder) were used instead of the polyhydroxyalkanoate dry particles (powder) used in Example 1.
[0097]
[0098] [Comparative Example 1]
[0099] Distilled water was added to dry particles (powder) of polyhydroxyalkanoate (PHA) (Mw: 340,000 g / mol, 4-HB repeating unit content: 10 wt%, manufacturer: CJ CheilJedang) to obtain a crude solution having a solid concentration of 40 wt%. Next, the crude solution and a 10% concentration PVA emulsifier were added to a disper (product name: homogenizing disper, manufacturer: PRIMIX) at a solid concentration of 1.5 parts by weight relative to the crude solution, and mixed and stirred at 1,000 to 2,000 rpm for 5 minutes to obtain a suspension. Then, the obtained suspension was emulsified using a homogenizing mixer (product name: homogenizing mixer, manufacturer: PRIMIX) at 6,000 to 8,000 rpm for 30 minutes to prepare a PHA emulsion.
[0100] A first formulation was performed by adding 0.3 wt% (based on the total weight of the PHA dispersion) of a thickener to the above PHA emulsion and stirring the mixture in a homomixer at 6,000 to 8,000 rpm for 20 minutes. Next, a second formulation was performed by adding 0.9 wt% (based on the total weight of the PHA dispersion) of wax to the PHA obtained through the first formulation and stirring the mixture in a homomixer at 6,000 to 8,000 rpm for 20 minutes. Next, 0.05 wt% of a defoaming agent (based on the total weight of the PHA dispersion) and 0.05 wt% of an antimicrobial agent (based on the total weight of the PHA dispersion) were added to the PHA obtained through the second formulation, and the mixture was stirred at 6,000 to 8,000 rpm in a homomixer for 20 minutes to produce the third formulation. Thereafter, the PHA obtained through the third formulation was first filtered with a 130 μm filter, and then secondarily filtered with a 110 μm filter, thereby producing a PHA dispersion.
[0101]
[0102] [Comparative Example 2]
[0103] The PHA dispersion prepared in Comparative Example 1 was heated at 70°C for 10 minutes.
[0104]
[0105] [Comparative Example 3]
[0106] A PHA dispersion was prepared through the same process as in Comparative Example 1, except that an antibacterial agent was added at 0.1 wt% (based on the total weight of the PHA dispersion) during the second formulation in Comparative Example 1.
[0107]
[0108] The following evaluation was conducted on each of the PHA dispersions of the above examples and comparative examples.
[0109]
[0110] [Test Example 1] Bacterial Contamination Test
[0111] Three types of dry media (MC-Media Pad, JNC CORPORATION) were prepared, each for general bacteria, fungi, and E. coli. 1 ml of PHA dispersion was diluted 10-fold in 9 ml of sterilized water to prepare a dilution, which was vortexed for 1 minute and 1 ml was evenly dispensed onto each dry media. Next, the dry media for general bacteria was incubated at 35°C for 48 hours, the dry media for fungi was incubated at 25°C for 48 hours, and the dry media for E. coli was incubated at 35°C for 24 hours. After incubation, the number of colonies was counted. If the measured number of colonies was less than 10, it was evaluated as no bacterial contamination (pass), and if it was 10 or more, it was evaluated as bacterial contamination (contamination).
[0112] Figure 1 shows the results of a bacterial contamination test. It was confirmed that Examples 1 and 2, which are PHA dispersions according to the present invention, had excellent stability (resistance) against bacteria as they were manufactured by mixing additives after heating the emulsion. In particular, it was confirmed that when an antibacterial agent was added after heating for 20 to 30 minutes at a temperature of about 60°C, general bacteria, Escherichia coli, and fungi were all sterilized, preventing bacterial contamination.
[0113] On the other hand, Comparative Example 1, in which heating treatment was not performed, showed serious bacterial contamination, and Comparative Example 2, in which heating treatment was performed after the production of the PHA dispersion, was found to be stable against E. coli and fungi, but showed bacterial contamination against general bacteria. This may imply that the heating treatment process is preferably performed between the PHA emulsion production process and the additive addition process.
[0114] Meanwhile, Comparative Example 3, which contained a higher amount of antimicrobial agent than Comparative Example 1, showed a decrease in the number of bacteria compared to Comparative Example 1, but was unable to prevent bacterial contamination. This may indicate that, without a heating treatment process, even if the antimicrobial agent content is increased, bacterial contamination cannot be effectively prevented. In contrast, the present invention can prevent bacterial contamination even with a relatively small amount of antimicrobial agent used by using a heating treatment process.
[0115]
[0116] [Test Example 2] Viscosity
[0117] Measurements were made using spindle #63 at 12 rpm using DV-1 VISCOMETER (BROOKFIELD Co.), and the results are shown in Table 1 below.
[0118]
[0119] [Experimental Example 3] Particle size (average particle diameter, D 50 )
[0120] The measurement was performed using a particle size analyzer (LS13 320 Laser Paricle size Analyzer), and the results are shown in Table 1 below. At this time, a PHA dispersion diluted 100 times using ultrapure water was used as the measurement sample.
[0121]
[0122] Classification Example 1 Example 2 Comparative Example 1 Comparative Example 2 PHA particle concentration (weight %) 39.9 40.1 40.0 40.0 Viscosity (cP) 450 560 350 420 pH 4.9 4.9 4.9 4.8 Particle size (㎛) 2.9 2.9 3.1 3.1
[0123] Referring to Table 1 above, it was confirmed that Examples 1 and 2 and Comparative Examples 1 and 2 had the same or similar pH and particle size, and thus, even if heating treatment was performed, the pH of the PHA dispersion and the particle size of the PHA particles did not change much. On the other hand, in the case of Example 2, where the heating treatment time was 10 minutes longer than that of Example 1, it was confirmed that the viscosity of the PHA dispersion increased, and it was also found that it was necessary to control the heating treatment time when considering the coating properties of the PHA dispersion.
[0124]
[0125] [Test Example 4] Storage Stability
[0126] The storage stability of the PHA dispersion prepared in Example 3 was evaluated while storing it in a constant temperature and humidity device at 35°C and 80% humidity for 12 weeks, and the results are shown in Table 2 below. Specifically, the PHA dispersion according to each order was redispersed by vortexing for 1 minute, and the degree of agglomeration of particles contained in the PHA dispersion was checked using a spoon. If there was no agglomeration after the redispersion, it was evaluated that the storage stability was secured.
[0127] Meanwhile, the PHA dispersion prepared in Example 3 was also evaluated in Test Examples 1 and 3, and the results are shown in Table 2 below.
[0128]
[0129] Classification particle size (㎛) Escherichia coli fungi general bacteria (mold fungi) storage stability 0 Week 3.1 Passed Passed Passed -1 Week 2.8 Passed Passed Passed Verified 2 Week 3.2 Passed Passed Passed Verified 3 Week 3.2 Passed Passed Passed Verified 4 Week 3.2 Passed Passed Passed Verified 8 Week 3.2 Passed Passed Passed Verified 12 Week 3.2 Passed Passed Passed Verified
[0130] Referring to Table 2 above, Example 3, a PHA dispersion according to the present invention, was manufactured by mixing additives after heating the emulsion, so it was possible to redisperse for up to 12 weeks, and it was confirmed that it had excellent storage stability and excellent stability (resistance) against bacteria as no bacterial contamination occurred.
Claims
1. (1) A step of preparing an emulsion by mixing a biodegradable polymer and an emulsifier; (2) a step of heating the emulsion; and (3) A method for producing a biodegradable polymer dispersion, comprising a step of mixing the heated emulsion and an additive.
2. In paragraph 1, A method for producing a biodegradable polymer dispersion, wherein the heating treatment of the above step (2) is performed at 50°C to 80°C.
3. In paragraph 1, A method for producing a biodegradable polymer dispersion, wherein the heating treatment of the above step (2) is performed for 10 to 30 minutes.
4. In paragraph 1, A method for producing a biodegradable polymer dispersion, further comprising a step of filtering the emulsion before the heating treatment of the above step (2).
5. In paragraph 1, A method for producing a biodegradable polymer dispersion, wherein the additive of the above step (3) comprises at least one selected from the group consisting of a thickener, a wax, an antifoaming agent, and an antibacterial agent.
6. In paragraph 1, The above step (3) is, (3-1) A step of adding and mixing a first additive including a thickener into the heated emulsion; (3-2) A step of adding and mixing a second additive including wax into the emulsion mixed with the first additive; and (3-3) A method for producing a biodegradable polymer dispersion, comprising a step of adding and mixing a third additive including at least one selected from the group consisting of a defoaming agent and an antibacterial agent into an emulsion mixed with the second additive.
7. In paragraph 6, A method for producing a biodegradable polymer dispersion, wherein the amount of the antibacterial agent added in the above step (3-3) is 0.001 wt% to 0.5 wt% based on the total weight of the biodegradable polymer dispersion.
8. In paragraph 1, The biodegradable polymer of the above step (1) has an average particle diameter (D 50 ) A method for producing a biodegradable polymer dispersion having a particle shape of 0.5 ㎛ to 5.0 ㎛.
9. In paragraph 1, A method for producing a biodegradable polymer dispersion, wherein the biodegradable polymer of step (1) comprises at least one selected from the group consisting of polyhydroxyalkanoate (PHA), polylactic acid (PLA), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), and polycaprolactone (PCL).
10. In paragraph 9, A method for producing a biodegradable polymer dispersion, wherein the above polyhydroxyalkanoate is a poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer.
11. In paragraph 10, A method for producing a biodegradable polymer dispersion, wherein the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer contains 6 to 20 wt% of repeating units derived from 4-hydroxybutyrate based on the total weight of the poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer.
12. In paragraph 1, A method for producing a biodegradable polymer dispersion, wherein the emulsifier of the above step (1) comprises at least one selected from the group consisting of polyvinyl alcohol (PVA), sodium dodecyl sulfonate (SDS), cocobetaine, and lecithin.
13. A biodegradable polymer dispersion prepared by a method according to any one of claims 1 to 12.
14. In paragraph 13, A biodegradable polymer dispersion having a viscosity of 10 cP to 3,000 cP as measured by a Brookfield viscometer at 25°C.
Citation Information
Patent Citations
Method for producing water dispersion of biodegradable polyester resin
JP2002173535A
Method for producing polylactic acid resin aqueous dispersion
JP2006089687A
Process for preparing Sperical fine particle ofantimicrobial polybuthylenesuccinate and Antimicrobialfine particle produced by the Process
KR1020050060471A
New Method for preparing Edoxaban intermediate, and the method for preparing Edoxaban using thereof
KR1020230158354A
Biodegradable coating composition, preparation method thereof, and biodegradable articles using same
KR102399861B1