Poly(3-hydroxypropionic acid) polymer and method for preparing same

The synthesis of poly(3-hydroxypropionic acid) with a novel network structure through condensation polymerization addresses efficiency and molecular weight challenges, resulting in a polymer with enhanced properties and broad application potential.

WO2024225797A1PCT designated stage expired Publication Date: 2024-10-31LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005649
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-25
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current methods for producing poly(3-hydroxypropionic acid) face challenges in economic efficiency, high solvent usage, and difficulties in achieving high molecular weight due to by-products, while also requiring a novel structure for improved physical properties and broader application.

Method used

A poly(3-hydroxypropionic acid) polymer with a novel network structure is synthesized by condensation polymerization using 3-hydroxypropionic acid and a reactive monomer, forming a branched structure with specific terminal groups and alpha values, which enhances molecular weight and elasticity, allowing for various product applications.

Benefits of technology

The novel network structure of the poly(3-hydroxypropionic acid) polymer achieves appropriate molecular weight characteristics, high cross-linking, and elasticity, reducing brittleness, making it suitable for diverse product groups and maintaining foam shape during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005649_31102024_PF_FP_ABST
    Figure KR2024005649_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a poly(3-hydroxypropionic acid) polymer comprising a novel network structure and a method for preparing same.
Need to check novelty before this filing date? Find Prior Art

Description

Poly(3-hydroxypropionic acid) polymer and method for producing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0055419, filed April 27, 2023, and Korean Patent Application No. 10-2024-0055648, filed April 25, 2024, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a poly(3-hydroxypropionic acid) polymer comprising a novel network structure and a method for producing the same.

[0004]

[0005] Poly(3-hydroxypropionic acid) has biodegradable properties, and due to these environmentally friendly properties, research on its use has been actively conducted recently.

[0006]

[0007] There are two main methods for producing poly(3-hydroxypropionic acid): one is a petrochemical-based method using β-propiolactone (PL) for polymerization, and the other is a bio-based method using 3-hydroxypropinic acid (3HP).

[0008]

[0009] When using PL, multiple synthesis steps using ethylene oxide are required, so there is a disadvantage in terms of economic feasibility compared to when using 3HP.

[0010]

[0011] Polymerization using 3HP biosynthesis requires multiple steps, including freeze-drying, ultrasonication, and solvent extraction, to obtain poly(3-hydroxypropionic acid), necessitating the use of large quantities of solvent. While the bio-based polymerization yields 100% bio-based poly(3-hydroxypropionic acid), the residual residues after fermentation often result in a high organic nitrogen content and a high YI.

[0012]

[0013] To address this issue, attempts have been made to polycondense 3HP, but the formation of byproducts in the form of cyclic oligomers limits the ability to obtain high-molecular-weight poly(3-hydroxypropionic acid). Attempts have been made to increase molecular weight by ROP of low-molecular-weight cyclic oligomers, but separation and purification are difficult.

[0014]

[0015] In addition, there is a need for a technology to synthesize these poly(3-hydroxypropionic acid) polymers with a novel structure that exhibits excellent physical properties so that they can be applied to a wider range of product groups.

[0016]

[0017] Accordingly, there is a need for a method for producing poly(3-hydroxypropionic acid) by polycondensation from 3HP, which has excellent physical properties and a novel structure that is easy to apply to a product group.

[0018]

[0019] The present invention provides a poly(3-hydroxypropionic acid) polymer having a novel network structure.

[0020] In addition, the present invention provides a method for producing the poly(3-hydroxypropionic acid) polymer.

[0021]

[0022] poly(3-hydroxypropionic acid) polymer

[0023] In order to solve the above problem, according to one embodiment of the present invention, a poly(3-hydroxypropionic acid) polymer is provided, which comprises a plurality of 3-hydroxypropionic acid-derived repeating units represented by the following chemical formula 1, has a network structure formed by a terminal group of one of the repeating units being bonded to a terminal group of another repeating unit by a reactive monomer, and has an alpha value of 0.4 to 0.8 according to a multi-angle light scattering detector (MALS):

[0024] [Chemical Formula 1]

[0025] .

[0026]

[0027] The term 'poly(3-hydroxypropionic acid)' used in the present invention refers to a polymer that includes a repeating unit derived from 3-hydroxypropionic acid, and specifically includes a repeating unit represented by the chemical formula 1.

[0028] Poly(3-hydroxypropionic acid) polymers possess biodegradable properties due to the molecular structure of their repeating units. Furthermore, the poly(3-hydroxypropionic acid) according to the present invention is characterized by a novel network structure formed by polymerizing 3-hydroxypropionic acid with a reactive monomer under specific conditions, as described below.

[0029]

[0030] The term “network structure” used in the present invention may mean a network structure including at least two branch structures formed by combining at least three or more repeating units, and this is distinguished from a branched structure or a hyperbranched structure of a branch structure of multiple branches.

[0031] The novel poly(3-hydroxypropionic acid) polymer having the above-described network structure can exhibit appropriate molecular weight characteristics, a high degree of crosslinking, and appropriate elasticity at the same time. Typically, polymers with a high degree of crosslinking exhibit brittle characteristics, but the polymer having the novel network structure according to the present invention has elasticity supplemented by the empty spaces within the network structure, thereby reducing brittle characteristics, making it easy to apply to various product groups.

[0032] Specifically, a poly(3-hydroxypropionic acid) polymer according to one embodiment of the invention forms a novel network structure by bonding a terminal group of any one of the repeating units represented by the above chemical formula 1 to a terminal group of another repeating unit by a reactive monomer.

[0033]

[0034] According to one embodiment of the invention, the poly(3-hydroxypropionic acid) polymer having the novel network structure comprises a plurality of repeating units represented by the chemical formula 1, wherein a terminal group of any one of the repeating units is bonded to a terminal group of another repeating unit by a reactive monomer, thereby forming a novel network structure.

[0035] Here, the “terminal group of the repeating unit” means a terminal group derived by the reaction of 3-hydroxypropionic acid, a monomer constituting the repeating unit, with a reactive monomer.

[0036]

[0037] The alpha value of the poly(3-hydroxypropionic acid) polymer according to the multi-angle light scattering detector (MALS) may be 0.4 to 0.8, preferably 0.5 to 0.8. By satisfying the above range, the desired network structure can be achieved. Accordingly, the present invention can be manufactured into various molded products, and in particular, when manufactured in the form of a foam, the network structure supports the foam so that the shape is maintained without collapsing even after final processing.

[0038] The alpha value obtained by a multi-angle light scattering detector (MALS) is an indicator that can be used to determine the structure of a polymer, and the alpha value refers to the constant value of the Mark-Houwink equation derived from the multi-angle light scattering detector (MALS). If the alpha value is outside the above range and approaches 1, it means that the structure of the polymer is approaching linearity, so it is not suitable. In addition, if the alpha value in the cross-linked structure is too low and outside the above range, gelation occurs, which reduces processability and mechanical properties, and accordingly, it is difficult to maintain the shape of the final polymer in a foam form, making it difficult to apply to various product groups. The specific measurement method will be described in more detail in the experimental examples described below.

[0039]

[0040] The above reactive monomer may include at least one terminal reactive substituent selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), an amino group (-NH2), a cyano group (-CN), a thiol group (-SH), and an isocyanate group (-N=C=O). Preferably, it may be a multifunctional monomer including multiple terminal reactive substituents, thereby facilitating the formation of a novel network structure.

[0041] The above reactive monomer is polyC 1-60 Alkylene polyol or C 1-60It may be one or more selected from alkyl dicarboxylic acids, and poly C 1-60 Alkylene polyols and C 1-60 Alkyl dicarboxylic acids may be used simultaneously.

[0042] Here, the poly C 1-60 Alkylene polyols include glycerol, 3-arm-poly(ethylene glycol) n=2~15 , 4-arm-poly(ethylene glycol) n=2~10 , erythritol, pentaerythritol, di(trierythritolpropane), xylitol, sorbitol, tripentaerythritol, inositol, and ß-cyclodextrin, but are not limited thereto.

[0043] Also, the above C 1-60 The alkyl dicarboxylic acid may include, but is not limited to, at least one selected from the group consisting of malonic acid, succinic acid, adipic acid, 1,3,5-benzenetricarboxylic acid, 1,3,5-triazine-2,4,6-tricarboxylic acid, citric acid, and 2,2-bis(hydroxymethyl)butyric acid.

[0044]

[0045] According to one embodiment of the invention, the poly(3-hydroxypropionic acid) polymer may have the following structure, but is not limited thereto:

[0046]

[0047] In the above structure, R1 and R2 may mean a structure derived from a reactive monomer.

[0048] n can be from 1 to 100.

[0049]

[0050] The melting temperature (Tm) of the above poly(3-hydroxypropionic acid) polymer is 50 to 70°C. More preferably, it is 51°C or higher, 52°C or higher, 68°C or lower, 67°C or lower, or 51 to 68°C or 52 to 67°C. By satisfying the above thermal characteristics, it is advantageous to achieve the desired effect.

[0051] Additionally, the melting temperature (Tm) of the poly(3-hydroxypropionic acid) polymer may be 50 to 70°C, and the total sum of enthalpies (ΔH) in that region may be less than 50 J / g.

[0052]

[0053] Preferably, the polydispersity index (PDI) of the poly(3-hydroxypropionic acid) weight body is 3.0 to 20.0. More preferably, it is 3.1 or more, 3.3 or more, 3.5 or more, 4.0 or more, or 5.0 or more, and 19.5 or less, 19.4 or less, 19.0 or less, 18.0 or less, or 16.0 or less.

[0054]

[0055] Preferably, the weight average molecular weight (Mw) of the poly(3-hydroxypropionic acid) polymer is 2,000 to 100,000. More preferably, it is 3,000 or more, 4,000 or more, 5,000 or more, 5,100 or more, 5,500 or more, 7,000 or more, or 9,000 or more, and 90,000 or less, 70,000 or less, 50,000 or less, 30,000 or less, 25,000 or less, 23,000 or less, 20,000 or less, 17,000 or less, 15,000 or less, or 13,000 or less.

[0056]

[0057] Preferably, the number average molecular weight (Mn) of the poly(3-hydroxypropionic acid) polymer is 500 to 50,000. More preferably, it is 700 or more, 900 or more, 1,000 or more, 1,500 or more, or 3,000 or more, and 30,000 or less, 15,000 or less, 10,000 or less, 9,000 or less, 7,000 or less, 5,000 or less, or 4,500 or less.

[0058]

[0059] Method for producing poly(3-hydroxypropionic acid) polymer

[0060] Meanwhile, according to one embodiment of the present invention, a method for producing the above-described poly(3-hydroxypropionic acid) polymer is provided, which can be produced from 3-hydroxypropionic acid, and 3-hydroxypropionic acid can be produced through biosynthesis.

[0061] Therefore, preferably, the poly(3-hydroxypropionic acid) may have a bio-content of 90% or more. The bio-content can be determined by analyzing the content of the radioactive isotope 14C (bio-derived) after graphitizing the sample to be measured using the ASTM D6866-22 method.

[0062]

[0063] More specifically, the method for producing a poly(3-hydroxypropionic acid) polymer comprises a first step of polymerizing 3-hydroxypropionic acid and a reactive monomer to form an oligomer; and a second step of polymerizing the oligomer to produce a poly(3-hydroxypropionic acid) polymer having a network structure.

[0064] At this time, by controlling the manufacturing conditions of steps 1 and 2, a poly(3-hydroxypropionate) polymer having the novel network structure described above can be manufactured. Here, the description of the 3-hydroxypropionic acid and reactive monomer used can be equally applied to all of the above.

[0065]

[0066] (Step 1)

[0067] Step 1 above is a step of producing an oligomer by melt polymerizing 3-hydroxypropionic acid and a reactive polymer. The melt polymerization above means that the reactants, 3-hydroxypropionic acid and the reactive polymer, and the product, the oligomer, remain in a liquid state.

[0068]

[0069] The above reactive monomer functions to link multiple repeating units formed by 3-hydroxypropionic acid so that the polymer can form a new network.

[0070] The reactive monomer may include at least one terminal reactive substituent selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), an amino group (-NH2), a cyano group (-CN), a thiol group (-SH), and an isocyanate group (-N=C=O). Preferably, the reactive monomer may be a multifunctional monomer including multiple terminal reactive substituents, thereby facilitating the formation of a novel network structure. The specific types of the reactive monomer may all be equally applied to the above-mentioned contents.

[0071] Preferably, the reactive monomer is polyC 1-60 Alkylene polyol or C 1-60 It may contain at least one type of alkyl dicarboxylic acid, preferably poly C. 1-60 Alkylene polyols and C 1-60 It may simultaneously contain alkyl dicarboxylic acid. The poly C 1-60 Alkylene polyols and C 1-60 The specific types of alkyl dicarboxylic acids can all be applied equally to the above-mentioned contents.

[0072] The above poly C 1-60The alkylene polyol may be included in an amount of 0.1 to 15 mol%, preferably 0.5 to 10 mol%, based on 100 mol of 3-hydroxypropionic acid. In addition, the C 1-60 The alkyldicarboxylic acid may be included in an amount of 0.01 to 10 mol%, preferably 0.25 to 5 mol%, based on 100 mol of 3-hydroxypropionic acid. By using each reactive monomer in the above content range, it is easy to form a new network structure.

[0073]

[0074] The above step 1 can be performed by controlling the reaction temperature to a temperature of 80°C to 100°C. Preferably, the reaction temperature of the above step 1 is 81°C or higher, 82°C or higher, 83°C or higher, 84°C or higher, or 85°C or higher, and 99°C or lower, 98°C or lower, 97°C or lower, 96°C or lower, or 95°C or lower.

[0075] Additionally, step 1 may be performed at a pressure of 5 torr to 20 torr. Preferably, step 1 is at least 6 torr, at least 7 torr, at least 8 torr, or at least 9 torr, and at most 19 torr, at most 18 torr, at most 17 torr, at most 16 torr, or at most 15 torr.

[0076] In addition, the reaction time of the above step 1 can be appropriately considered in consideration of the molecular weight, yield, etc. of the oligomer produced, and it is preferable to perform it for 1 to 3 hours.

[0077]

[0078] Preferably, step 1 is performed in the presence of a sulfonic acid catalyst. Preferably, the sulfonic acid catalyst is p-toluenesulfonic acid, m-xylene-4-sulfonic acid, 2-mesitylenesulfonic acid, or p-xylene-2-sulfonic acid. The catalyst is used in an amount of 0.1 to 0.5 mol% relative to 3-hydroxypropionic acid.

[0079]

[0080] (Step 2)

[0081] Step 2 of the present invention is a step of further polymerizing the oligomer of step 1 to produce a poly(3-hydroxypropionate) polymer having a novel network structure.

[0082]

[0083] Step 2 above can be performed at a lower pressure than step 1 because the reactant is an oligomer.

[0084] Preferably, the reaction temperature of step 2 can be controlled to be 75°C to 95°C. More preferably, the reaction temperature of step 2 is 80°C or higher, or 85°C or higher, and 94°C or lower, 93°C or lower, 92°C or lower, or 91°C or lower.

[0085] Preferably, the reaction pressure of step 2 can be performed at 5 torr or less. More preferably, the pressure of step 2 is 4 torr or less, 3 torr or less, 2 torr or less, 1 torr or less, 0.5 torr or less, 0.4 torr or less, or 0.3 torr or less, and 0.01 torr or more, 0.02 torr or more, 0.03 torr or more, 0.04 torr or more, 0.05 torr or more, 0.06 torr or more, 0.07 torr or more, 0.08 torr or more, 0.09 torr or more, or 0.1 torr or more.

[0086] In addition, the reaction time of the above step 2 can be appropriately considered in consideration of the molecular weight, yield, etc. of the poly(3-hydroxypropionate) polymer produced, and is preferably performed for 5 to 30 hours.

[0087] Preferably, steps 1 and 2 are performed for a total of 7 to 30 hours, more preferably 7 to 24 hours.

[0088]

[0089] Meanwhile, since step 2 is performed subsequent to step 1, the catalyst added in step 1 also participates in the reaction in step 2. Therefore, the catalyst described in step 1 can also be applied in step 2.

[0090] Additionally, according to one embodiment of the invention, the second step may be performed by additionally introducing a tin-based catalyst. Preferably, the tin-based catalyst is SnCl2 or Sn(oct)2. The catalyst is used in an amount of 0.001 to 0.5 mol% relative to 3-hydroxypropionic acid.

[0091]

[0092] Meanwhile, if necessary, before performing steps 1 and 2, the 3-hydroxypropionic acid and the reactive monomer may be independently pretreated at 30°C to 100°C and 30 mbar to 150 mbar, respectively. Through the pretreatment step, moisture present in the 3-hydroxypropionic acid and the reactive monomer can be removed.

[0093]

[0094] The novel poly(3-hydroxypropionic acid) polymer having a network structure manufactured according to the above-described method can exhibit appropriate molecular weight characteristics, a high degree of crosslinking, and appropriate elasticity at the same time. Typically, polymers with a high degree of crosslinking exhibit brittle characteristics, but the polymer having a novel network structure according to the present invention has elasticity supplemented by empty spaces within the network structure, thereby reducing brittle characteristics, and thus is easily applicable to various product groups.

[0095]

[0096] As described above, the present invention can provide a poly(3-hydroxypropionic acid) polymer having a novel network structure by polymerizing 3-hydroxypropionic acid with a reactive monomer under specific conditions.

[0097]

[0098] Figure 1 is a photograph evaluating the shape over time when the polymers of the examples and comparative examples were manufactured into molded products.

[0099]

[0100] Hereinafter, embodiments of the present invention will be described in more detail in the following examples. However, the following examples are merely illustrative of embodiments of the present invention, and the content of the present invention is not limited by the following examples.

[0101]

[0102] [Examples and Comparative Examples]

[0103] Example 1

[0104] (Step 1)

[0105] 3-Hydroxypropionic acid (70 g) from which moisture had been removed, 7.156 g of the reactive monomer glycerol (A: 10 mol% compared to 3-HP), and 4.59 g of succinic acid (B: 5 mol% compared to 3-HP) were placed in a reactor, and 295.6 mg of p-TSA (p-Toluenesulfonic acid) (0.2 mol% compared to 3-HP) as a catalyst was added. The temperature and pressure inside the reactor were maintained at 90°C and 10 mbar (7.5 torr), respectively, and the reaction was carried out for 2 hours to produce an oligomer.

[0106] (Step 2)

[0107] Next, the temperature and pressure in the reactor were adjusted to 80°C and 0.1 torr, respectively, and SnOct2157.4mg (0.05 mol% compared to 3-HP) was added as an additional catalyst, and the reaction was further performed for 5 hours to produce a poly(3-hydroxypropionic acid) polymer having a network structure.

[0108]

[0109] Examples 2 to 11

[0110] A poly(3-hydroxypropionic acid) polymer having a network structure was manufactured using the same method as in Example 1, but the reaction conditions were changed as shown in Table 1 below.

[0111]

[0112] Comparative Example 1

[0113] (Step 1)

[0114] 3-Hydroxypropionic acid (60 g) from which moisture had been removed was placed in a reactor, and 253.4 mg (0.2 mol% relative to 3-HP) of p-TSA (p-Toluenesulfonic acid) was added as a catalyst. The temperature and pressure inside the reactor were maintained at 90°C and 10 mbar (7.5 torr), respectively, and the reaction was conducted for 2 hours to produce a 3-hydroxypropionic acid oligomer.

[0115] (Step 2)

[0116] Next, the temperature and pressure inside the reactor were adjusted to 80°C and 0.1 torr, respectively, and the reaction was performed for 5 hours to produce a poly(3-hydroxypropionate) polymer.

[0117]

[0118] Comparative examples 2 and 3

[0119] A poly(3-hydroxypropionic acid) polymer was manufactured using the same method as in Comparative Example 1, but the reaction conditions were changed as shown in Table 1 below.

[0120]

[0121] Comparative Example 4

[0122] (Step 1) 70 g of dried 3-hydroxypropionic acid (3HP) and 7.156 g of glycerol (10 mol% relative to 3HP) were added to the reactor, and 295.6 mg of p-TSA (0.2 mol% relative to 3HP) was used as a catalyst to perform an oligomerization reaction at 90°C and 10 mbar (7.5 torr) for 2 hours.

[0123] (Step 2) An additional polymerization reaction was performed for 5 hours while adding 157.4 mg of Sn(Oct)2 (0.05 mol% compared to 3HP) as a cocatalyst at a vacuum of 0.1 torr, thereby producing a branched polymer.

[0124]

[0125] [Experimental Example 1 - Polymer Properties Evaluation]

[0126] The physical properties of the polymers manufactured in the above examples and comparative examples were evaluated using the following methods.

[0127] 1) Weight average molecular weight and molecular weight distribution

[0128] For the polymers manufactured in the above examples and comparative examples, the weight average molecular weight, number average molecular weight, and polydispersity index were measured by gel permeation chromatography (GPC: gel permeation chromatography, Waters Alliance e2695), and the results are shown in Table 1 below.

[0129] - Solvent: chloroform (eluent)

[0130] - Flow rate: 1.0 ml / min

[0131] - Column temperature: 40℃

[0132] - Standard: Polystyrene

[0133]

[0134] 2) Alpha value measurement using a light scattering detector (MALS)

[0135] For the polymers manufactured in the above examples and comparative examples, the Alpha value was measured using a light scattering detector (MALS), and the results are shown in Table 1 below.

[0136] First, the polymer was dissolved in chloroform (Stabilized with ETOH) at a concentration of 5 mg / mL to prepare a sample, and the mobile phase was prepared by filtering 1000 mL of chloroform (Stabilized with ETOH) using a solvent clarification system. The radius of gyration (Rg) of the solvated chain of the polymer was measured using a mass air dispersion detector (MALS), and a plot of intrinsic viscosity (η) and absolute molecular weight (M; Absolute MW) was derived from this. The constant Alpha (α) value was calculated using the Mark-Houwink equation of the following mathematical equation 1, and the results are shown in Table 1 below.

[0137] - RI (Refractive Index) Measurement: DAWN8 (Manufacturer: Wyatt)

[0138] - Visocmeter (viscosity) measurement: Viscostar III (Manufacturer: Wyatt)

[0139] - Light scattering measurement: Optilab T-rEX (Manufacturer: Wyatt)

[0140] - Stationary phase: 2x Agilent PLgel MIXED-B and C, 7.5 x 300 mm, 5 μm

[0141] - Mobile phase: Chloroform (stablized with ETOH) = 100(v / v, %)

[0142] - Flow rate: 1.0 mL / min

[0143] - Fixed temperature: 40 ℃

[0144] - Injection volume: 100 ㎕ (0.45 μm filtered)

[0145] - Analysis time: 35 minutes

[0146] - System calibration: Polystyrene (Mp:135700))

[0147] - Chloroform refractive index: 1.45

[0148] [Mathematical Formula 1]

[0149] log[η] = αlogM + logK

[0150] In the above mathematical formula 1,

[0151] [η] is the intrinsic viscosity (㎗ / g) of the polymer,

[0152] M is the absolute molecular weight (Absolute MW) of the polymer,

[0153] K is a constant.

[0154]

[0155] Classification Reaction time (hr) Reactive monomer (content (relative to 3-HP)) MnMwPDIAlpha1 Step 2 Step A (mol%) B (mol%) Example 1 25 10 5 12 6 25 10 4 4.0 5 0.5 Example 2 28 10 5 12 10 5 6 20 4.6 5 0.5 Example 3 25 5 2.5 9 3 17 0 6 0 5.9 0.5 Example 4 28 5 2.5 10 2 4 9 6 8 3 9.4 9 0.5 Example 5 25 10.5 10 3 27 4 6 9 7.2 4 0.8 Example 6 28 10.5 12 8 3 12 17 5 9.4 9 0.8 Example 7 21 8 10.5 12 17 23 6 8 4 19.4 7 0.8 Example 822210.517642841416.110.8Experimental 9250.50.253461123043.550.8Experimental Example 10280.50.254144161223.890.8Experimental Example 112220.50.54363208934.790.8Comparative Example 125--500080001.60.9Comparative Example 228--100008000020.9Comparative Example 3222--12000320002.50.9Comparative Example 42510-112926992.390.3Reactive Monomer Type A: Glycerol B: Succinic Acid

[0156] 3) DSC (differential scanning calorimetry) thermal property evaluation

[0157] For the polymers manufactured in the above examples and comparative examples, thermal properties (Tg, Tm, cold crystallization (2nd heating result), Tc (1st cooling result), total enthalpy (ΔH)) were measured under nitrogen gas flow using a TA DSC250 model equipment, and the results are shown in Table 2 below.

[0158] Heat up from 40℃ to 190℃ at 5℃ / min (1st heating) / maintain temperature at 190℃ for 10 minutes

[0159] Cooling from 190℃ to -60℃ at 5℃ / min (1st cooling) / Temperature maintained at -60℃ for 10 minutes

[0160] -Heat increase from -60℃ to 190℃ at 5℃ / min (2 nd heating)

[0161]

[0162] Classification TcTgCold crystallizationTmTemperature ( o C)ΔH (J / g)Temperature ( o C)Temperature ( o C)ΔH (J / g)Temperature ( o C)ΔH (J / g)Example 2N.DN.D-33.15N.DN.DN.DN.DExample 4N.DN.D-22.5728.2914.0152.1313.99Example 834.949.1-25.61N.DN.D66.5549.72Comparative Example 33265.2-20N.DN.D71.969.4

[0163] In general, a faster crystallization rate will result in a larger enthalpy of Tc and less or no cold crystallization, while a higher crystallinity will result in a larger enthalpy of Tm.

[0164] In addition, when the degree of crystallinity is high, the strength of the material increases, but it is brittle and inelastic. However, in the case of a novel network structure such as the present invention, it can be confirmed that the brittle characteristic can be reduced by lowering the degree of crystallinity.

[0165]

[0166] [Experimental Example 2 - Polymer Shape Evaluation]

[0167] The polymers manufactured in the above examples and comparative examples were used to manufacture final products using the following method, and their shapes were evaluated.

[0168] First, samples were prepared by dissolving each of the polymers of Example 1 and Comparative Example 4 in chloroform at 10 wt%. The samples were placed in a distillation device, and the pressure was changed to vacuum conditions to remove the excess chloroform.

[0169] Next, the sample was injected into a Teflon mold up to 1 / 3 of the way, formed into a foam under vacuum conditions, and dried at 25°C for 18 hours.

[0170] In the case of Example 1, the foam shape was maintained even after 24 hours of drying (see (b) of Fig. 1), but in the case of Comparative Example 4, it was confirmed that the foam shape was not maintained after 1 hour of drying and changed into a film shape (see (a) of Fig. 1).

Claims

1. Contains multiple 3-hydroxypropionic acid-derived repeating units represented by the following chemical formula 1, It has a network structure formed by the terminal group of one of the above repeating units being bonded to the terminal group of another repeating unit by a reactive monomer, Alpha value of 0.4 to 0.8 according to multi-angle light scattering detector (MALS), Poly(3-hydroxypropionic acid) polymer: [Chemical Formula 1] .

2. In paragraph 1, The above network structure includes at least two branch structures formed by combining at least three or more repeating units. Poly(3-hydroxypropionic acid) polymer.

3. In paragraph 1, The reactive monomer comprises at least one terminal reactive substituent selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), an amino group (-NH2), a cyano group (-CN), a thiol group (-SH), and an isocyanate group (-N=C=O). Poly(3-hydroxypropionic acid) polymer.

4. In paragraph 1, The above reactive monomer is polyC 1-60 Alkylene polyol or C 1-60 At least one selected from among alkyl dicarboxylic acids, Poly(3-hydroxypropionic acid) polymer.

5. In paragraph 4, The above poly C 1-60 Alkylene polyols include glycerol, 3-arm-poly(ethylene glycol) n=2~15 , 4-arm-poly(ethylene glycol) n=2~10 , at least one selected from the group consisting of erythritol, pentaerythritol, di(trierythritolpropane), xylitol, sorbitol, tripentaerythritol, inositol and ß-cyclodextrin, Poly(3-hydroxypropionic acid) polymer.

6. In paragraph 4, C above 1-60 The alkyl dicarboxylic acid is at least one selected from the group consisting of malonic acid, succinic acid, adipic acid, 1,3,5-benzenetricarboxylic acid, 1,3,5-triazine-2,4,6-tricarboxylic acid, citric acid, and 2,2-bis(hydroxymethyl)butyric acid. Poly(3-hydroxypropionic acid) polymer.

7. In paragraph 1, The weight average molecular weight (Mw) of the above poly(3-hydroxypropionic acid) polymer is 2,000 to 100,000, Poly(3-hydroxypropionic acid) polymer.

8. In paragraph 1, The number average molecular weight (Mn) of the above poly(3-hydroxypropionic acid) polymer is 500 to 50,000, Poly(3-hydroxypropionic acid) polymer.

9. In paragraph 1, The polydispersity index (PDI) of the above poly(3-hydroxypropionic acid) polymer is 3.0 to 20.

0. Poly(3-hydroxypropionic acid) polymer.

10. In paragraph 1, The melting temperature (Tm) of the poly(3-hydroxypropionic acid) polymer is 50 to 70°C, and the total sum of enthalpies (ΔH) in the corresponding region is less than 50 J / g. Poly(3-hydroxypropionic acid) polymer. A first step of polymerizing 11.3-hydroxypropionic acid and a reactive monomer to form an oligomer; A second step of producing a poly(3-hydroxypropionic acid) polymer having a network structure by polymerizing the above oligomer; comprising; A method for producing a poly(3-hydroxypropionic acid) polymer according to claim 1.

12. In paragraph 11, The reactive monomer comprises at least one terminal reactive substituent selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), an amino group (-NH2), a cyano group (-CN), a thiol group (-SH), and an isocyanate group (-N=C=O). A method for producing a poly(3-hydroxypropionic acid) polymer.

13. In paragraph 11, The above reactive monomer is polyC 1-60 Alkylene polyol or C 1-60 At least one selected from alkyl dicarboxylic acids, A method for producing a poly(3-hydroxypropionic acid) polymer.

14. In paragraph 13, The above poly C 1-60 Alkylene polyol is contained in an amount of 0.1 to 15 mol% with respect to 100 mol of 3-hydroxypropionic acid, C above 1-60 Alkyl dicarboxylic acid is included in an amount of 0.01 to 5 mol% per 100 mol of -hydroxypropionic acid. A method for producing a poly(3-hydroxypropionic acid) polymer.

Citation Information

Patent Citations

  • Quantum dot, producing method of quantum dot and electronic device

    KR1020240127773A

  • Din rail and stopper for fixing terminal block mounted thereto

    KR102577083B1

  • Branched poly (hydroxy acid) and production process thereof

    US20120027973A1

  • Method for manufacturing a branched poly(hydroxyl acid)

    WO2016173640A1

  • Branched poly(3-hydroxypropionic acid) polymer, and method for preparation thereof

    WO2022235112A1