Deposition material for semimetal nitride film, method for forming semimetal nitride film, and semiconductor substrate and semiconductor device manufactured therefrom

By employing halogen-free alkyl halides to modify metalloid precursor compounds, the deposition method addresses thermal decomposition and impurity issues, resulting in improved film properties and corrosion resistance for semiconductor applications.

WO2024225831A1PCT designated stage expired Publication Date: 2024-10-31SOULBRAIN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005719
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing deposition methods for metalloid nitride films face challenges in achieving high density, refractive index, and uniformity due to thermal decomposition and impurity issues, leading to insufficient corrosion resistance and step-coverage limitations in semiconductor device formation.

Method used

A halogen-free alkyl halide is used to substitute ligands in metalloid precursor compounds, enhancing the reactivity and adsorption process during atomic layer deposition, improving film growth rate, density, and refractive index, and reducing impurities.

Benefits of technology

The method significantly improves the thickness uniformity, density, and refractive index of metalloid nitride films, providing enhanced corrosion resistance and step coverage, suitable for complex semiconductor substrate structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005719_31102024_PF_FP_ABST
    Figure KR2024005719_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a deposition material for a semimetal nitride film, a method for forming a semimetal nitride film, and a semiconductor substrate and a semiconductor device manufactured therefrom, wherein low-temperature deposition materials are injected sequentially or simultaneously into a semimetal precursor compound that does not include a halogen as a ligand (halogen-free precursor), whereupon the ligand of the halogen-free precursor and the low-temperature deposition materials switch places and become implanted in the substrate, after which the reactivity with a reactant injected later in the deposition process improves, and therefore the thin film growth rate is improved and the density and refractive index of the deposited film are significantly enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Deposition material for a semi-metal nitride film, method for forming a semi-metal nitride film, semiconductor substrate and semiconductor device manufactured therefrom

[0001] The present invention relates to a deposition material for a semi-metal nitride film, a method for forming a semi-metal nitride film, a semiconductor substrate and a semiconductor device manufactured therefrom, and more particularly, to a deposition material for a semi-metal nitride film, a method for forming a semi-metal nitride film, and a semiconductor substrate and a semiconductor device manufactured therefrom, in which a low-temperature deposition material is sequentially or simultaneously injected into a semi-metal precursor compound (halogen-free precursor) that does not contain a halogen as a ligand, so that the ligand of the halogen-free precursor and the low-temperature deposition material exchange positions to be adsorbed onto the substrate and then the reactivity with a reactant subsequently injected in the deposition process is improved, thereby improving the thin film growth rate and greatly improving the density and refractive index of the deposited film.

[0002] The ideal ALD (atomic layer deposition) process is based on a self-limiting reaction, where the ligands of the precursors adsorbed on the substrate first inhibit the adsorption of the subsequently injected precursors.

[0003] However, in actual processes, the precursor may undergo thermal decomposition, which causes the ligand to detach from the central metal due to its thermal history. This process has the characteristics of a type of CVD (chemical vapor deposition), and the greater this characteristic, the lower the step coverage, density, and thickness uniformity of the deposited film may be. In addition, if the detached ligand species are easily adsorbed to the surface or easily form fluoride or chloride, there is a problem that they may remain as impurities in the deposited film (see J. Phys. Chem. B. 13491-8, “Surface chemistry in the atomic layer deposition of TiN films from TiCl4 and ammonia” (2006)).

[0004] The density and thickness uniformity of the above-mentioned deposition film are factors that affect the chemical properties, and by-products derived from the leaving group may be absorbed to contaminate the deposition film or disrupt the crystal arrangement of the deposition film, which may further lower the density.

[0005] Therefore, it is important to reduce the thermal history of the precursor so that the desired process can be achieved within the atomic layer deposition (ALD) window.

[0006] Meanwhile, the semi-metal nitride film is a deposition film manufactured using representative semi-metals such as silicon and germanium. For example, when depositing a silicon nitride film using precursors such as Si2Cl6 or SiCl2H2, which are represented by chlorosilane, and nitrogen-based reactants such as NH3 or N2H2, it is usually thermally deposited at a high temperature of 600˚C or higher to form a silicon nitride film (SiN x , wherein x is an integer from 0.8 to 1.2).

[0007] However, there are limitations in applying the high-temperature process due to problems such as the thermal budget mentioned above.

[0008] To solve this problem, a deposition process utilizing plasma at 400°C was reported, but the silicon nitride thin film formed at low temperature is not dense and thus does not have corrosion resistance, and as a result, there is a limitation in that it cannot form a structure for composing a semiconductor device.

[0009] There is a method of using a low-temperature process silicon precursor represented by precursors such as BTBAS (Bis(tertiarybutylamino)silane), TDMAS (Tris(dimethylamino)silane), DIPAS (Diisoprophylamino silane), BDEAS (Bis-Diethylamino Silane), and DIS (Diiodosilane), but the silicon nitride thin film formed from this has a low density and refractive index, which leads to insufficient corrosion resistance.

[0010] Therefore, there is a need for a method for manufacturing a deposition film that is based on a self-limiting reaction on a substrate, and that can form a complex structured deposition film by changing the ligand of the adsorbed precursor to a second ligand with higher reactivity and reacting it with a reactant, and that not only improves the thickness uniformity and film growth rate of the deposition film, but also reduces the amount of residual impurities and greatly improves the density and refractive index, and for the development of a semiconductor substrate and semiconductor device manufactured from the method.

[0011] [Prior Art Literature]

[0012] [Patent Document]

[0013] Korean Patent Publication No. 2017-0089422

[0014] In order to solve the problems of the prior art as described above, the present invention provides a deposition material for a semi-metal nitride film, a method for forming a semi-metal nitride film, a semiconductor substrate and a semiconductor device manufactured therefrom, which significantly improve the thin film growth rate, the thickness uniformity and density of the deposited film, and the refractive index by changing the ligand of the semi-metal precursor compound by providing a compound of a predetermined structure as a second ligand before, during, or after the precursor injection.

[0015] The above and other objects of the present invention can all be achieved by the present invention described below.

[0016] To achieve the above object, the present invention provides a deposition material for a metalloid nitride film comprising an alkyl-free halide for substituting part or all of the ligands of a Group 14 metalloid precursor compound.

[0017] The halogen constituting the above alkyl-free halide may be at least one selected from iodine and bromine.

[0018] The above group 14 metalloid may be at least one selected from silicon (Si), germanium (Ge), and tin (Sn).

[0019] The above alkyl-free halide may be an alkyl-free iodine, hydrogen iodide, hydrogen bromide, an iodine ion-containing substance or an iodine radical-containing substance.

[0020]

[0021] Additionally, the present invention may undergo a process of changing some or all of the ligands of the metalloid precursor compound using some or all of the deposition material for the metalloid nitride film on the substrate.

[0022] The above metalloid precursor compound may be a precursor compound having a Group 14 metalloid as a central metal.

[0023] The above Group 14 metalloid may be at least one selected from silicon (Si), germanium (Ge), and tin (Sn).

[0024] The ligand (L) is -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 can independently be -CH3, -CH2CH3, -iPr, -tBu, or -H.

[0025] The above deposition may be atomic layer deposition (ALD), plasma enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), metalorganic chemical vapor deposition (MOCVD), or low pressure vapor deposition (LPCVD).

[0026]

[0027] In addition, the present invention provides a semiconductor substrate including the aforementioned metalloid nitride film on a substrate, wherein the metalloid nitride film has a precursor adsorption state before ligand exchange as substrate-M-Ln (where n=an integer from 1 to 3, M=Si, Ge, Sn, L=halogen-free ligand), and a precursor adsorption state after ligand exchange as substrate-M-LnXm (where L=halogen-free ligand, X=Br, I, n=an integer from 1 to 3, and m=an integer from 1 to 3, satisfying n+m=3).

[0028] In addition, the present invention provides a semiconductor substrate including the aforementioned metalloid nitride film on a substrate, wherein the metalloid nitride film satisfies n+m=4 when the precursor before ligand exchange moving onto the substrate is M-Ln (n=an integer of 1 to 4, M=Si, Ge, Sn, L=halogen-free ligand), and the precursor state after ligand exchange is M-LnXm (L=halogen-free ligand, X=Br, I, n=an integer of 1 to 3, m=an integer of 1 to 4).

[0029] The ligand (L) is guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 are each independently -CH3, -CH2CH3, -iPr, -tBu, or -H, and the change in the precursor state before and after the ligand exchange can be formed by the process of moving to the substrate and the reaction between the halogen of the deposition material on the substrate and the alkyl-free halide for replacing the ligand of the Group 14 metalloid precursor.

[0030] The above semiconductor substrate may have a multilayer structure of two or more layers.

[0031] The above semi-metal nitride film may have a thin film growth rate of 0.09 Å / cycle or more, which is calculated by dividing the thickness measured by an ellipsometer by the number of deposition cycles.

[0032] The above semi-metal nitride film may have a refractive index (@350 nm wavelength) of 2 or less as measured using an ellipsometer.

[0033]

[0034] In addition, the present invention provides a semiconductor device characterized by including the semiconductor substrate described above.

[0035] According to the present invention, there is an activation effect that improves the thin film growth rate by changing some or all of the ligands of the precursor adsorbed on the substrate to halogen, and appropriately increases the thickness uniformity and density of the deposited film, thereby improving the productivity of the deposited film.

[0036] In addition, the refractive index is improved along with the density improvement during the deposition film formation, which has the effect of providing etching corrosion resistance required for forming a semiconductor element structure.

[0037] In addition, it is possible to improve the thickness uniformity of a deposition film even with a complex structure, and further, it has the effect of providing a method for manufacturing a deposition film using the same and a semiconductor substrate and semiconductor element manufactured thereby.

[0038] Figure 1 is a drawing comparing the thin film growth rates of three types of deposition films of Examples 1 to 3 using deposition materials for semi-metal nitride films according to the present invention, according to deposition temperature.

[0039] FIG. 2 is a drawing confirming the linearity of the cycle while increasing the deposition cycle of Example 2 using a deposition material for a semi-metal nitride film according to the present invention from 100 cycles to 1000 cycles.

[0040] FIG. 3 is a drawing comparing the refractive index (@350 nm wavelength) of the deposition film of Example 1 using a deposition material for a semi-metal nitride film according to the present invention with the refractive index (@350 nm wavelength) of the deposition films obtained from Comparative Examples 4, 7, and 8.

[0041] FIG. 4 is a drawing comparing the XRR (X-Ray Reflectometer, X-ray diffraction) thin film density of the deposited films of Examples 1 to 3 using a deposition material for a semi-metal nitride film according to the present invention with the XRR thin film density of the deposited films of Comparative Examples 4 to 6 not using the same.

[0042]

[0043] Hereinafter, the deposition material for the semi-metal nitride film of the present invention, the method for forming the semi-metal nitride film, and the semiconductor substrate and semiconductor device manufactured therefrom are described in detail.

[0044] The metalloids used in this document, unless otherwise specified, refer to group 14 elements represented by silicon (Si) and germanium (Ge).

[0045] The present inventors have provided a predetermined compound (deposition material for a semi-metal nitride film) that can change the halogen-free ligand of a semi-metal precursor compound used to form a deposition film on the surface of a substrate loaded inside a chamber, thereby improving the thin film growth rate and ensuring the thickness uniformity of the deposition film, while significantly improving the density and refractive index of the deposition film, and reducing H, C, N, Cl, etc. remaining as process byproducts. Based on this, the inventors have devoted themselves to further research on deposition materials for semi-metal nitride films, thereby completing the present invention.

[0046]

[0047] Below, we will specifically examine a deposition material for a semi-metal nitride film, a semiconductor substrate including a deposition film manufactured using the same, and a semiconductor device.

[0048]

[0049] Deposition material for semi-metal nitride films

[0050] The deposition material for the above semi-metal nitride film may be a predetermined compound capable of changing a ligand to be released from a precursor as a deposition additive compound used to better form a deposition film on the surface of a substrate loaded inside a chamber in the present invention.

[0051] The above metalloid precursor compound may be, for example, a compound in which a ligand is bonded to a Group 14 metalloid, and the ligand bonded to the central metal thereof easily exchanges part or all of the ligand with a deposition material for a metalloid nitride film.

[0052] In the case where the deposition material for the semi-metal nitride film used in the present invention is an alkyl-free halide, it can appropriately perform the role of substitution through a position exchange with the halogen-free ligand of the precursor.

[0053] The term “alkyl free” above, unless otherwise specified, refers to not only not containing an alkyl group, but also not containing an alkene group or an alkyne group.

[0054] The halogen constituting the above alkyl-free halide may be selected from at least one of iodine and bromine.

[0055] The deposition material for the above semi-metal nitride film may preferably be a compound having a purity of 99.99% or more, a compound having a purity of 99.999% or more, or a compound having a purity of 99.9999% or more or a purity of 99.99999% or more. For reference, when using a compound having a purity of less than 99%, impurities may remain in the deposition film or cause a side reaction with a precursor or a reactant, so it is recommended to use a material having a purity of 99% or more if possible.

[0056]

[0057] The deposition material for the above semi-metal nitride film preferably has a density of 1.0 to 4.0 g / cm 3 or 2.0 to 3.4 g / cm 3 , and the vapor pressure can be 1 atm at 180 to 240K, and within this range, there is an excellent effect in improving step coverage, thickness uniformity of the deposited film, and film quality.

[0058] As a deposition material for the above metalloid nitride film, an alkyl-free halide can form an intermediate for providing a deposition film having a structure in which a reactant-derived material is bonded to the Group 14 metalloid.

[0059] Here, the intermediate may refer to a state in which a compound of a predetermined structure is provided as a second ligand to replace the ligand of the metalloid precursor compound.

[0060] Here, the reactant may be a gaseous compound containing H2O, H2O2, O2, O3, O radical, D2, H2, H radical, NH3, NO2, N2O, N2, N radical, H2S or S. Here, D means deuterium.

[0061]

[0062] The above alkyl-free halide is characterized by being at least one selected from alkyl-free iodine, hydrogen iodide, hydrogen bromide, iodine ion or iodine radical, and in this case, by suppressing side reactions and controlling the growth rate of the deposition film, process byproducts in the deposition film are reduced, corrosion or deterioration is reduced, the crystallinity of the deposition film is improved, and a stoichiometric composition ratio is reached when forming a metal oxide film, and even when forming a deposition film on a substrate having a complex structure, there is an effect of significantly improving step coverage and thickness uniformity of the deposition film.

[0063] As a specific example, the deposition material for the semi-metal nitride film is a single hydrogen iodide having a purity of 3N to 15N, a gas mixture containing 0.01 to 99.99 wt% of hydrogen iodide having a purity of 3N to 15N and the remainder of an inert gas so that the total amount becomes 100 wt%, or an aqueous solution mixture containing 0.5 to 70 wt% of hydrogen iodide having a purity of 3N to 15N and the remainder of water so that the total amount becomes 100 wt%, wherein the inert gas is nitrogen, helium or argon having a purity of 4N to 9N, the effect of reducing process by-products is large, the step coverage is excellent, and the effect of improving the density of the deposition film can be more outstanding. Here, N represents normal concentration.

[0064] Preferably, the deposition material for the semi-metal nitride film is a gas mixture of hydrogen iodide alone of 3N to 7N, hydrogen iodide of 1 to 99 wt% and an inert gas balance so that the total amount becomes 100 wt%, or an aqueous solution mixture of hydrogen iodide of 0.5 to 70 wt% and an water balance so that the total amount becomes 100 wt%, wherein the inert gas may be nitrogen, helium or argon having a purity of 4N to 9N, and in this case, when forming a deposition film, a substitution region that does not remain in the deposition film is formed, thereby forming a relatively sparse deposition film while suppressing side reactions and controlling the deposition film growth rate, thereby reducing process byproducts in the deposition film, reducing corrosion or deterioration, improving the crystallinity of the deposition film, and significantly improving step coverage and thickness uniformity of the deposition film even when forming a deposition film on a substrate having a complex structure.

[0065] In the present invention, the deposition material or the metalloid precursor compound for the semi-metal nitride film may include a step of vaporizing and then injecting and then performing plasma post-treatment before and after deposition, in which case the growth rate of the deposition film can be improved while reducing process byproducts.

[0066] The above deposition may be atomic layer deposition (ALD), plasma enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), metalorganic chemical vapor deposition (MOCVD), or low pressure vapor deposition (LPCVD).

[0067]

[0068] metalloid precursor compounds

[0069] In the present invention, the metalloid precursor compound used to form a deposition film is a molecule having a group 14 metalloid as a central metal atom (M) and at least one ligand composed of C, N, O, H, etc., and in the case of a precursor having a vapor pressure of 1 mTorr to 100 Torr at 25°C, the effect of filling a leaving site with a deposition material for a metalloid nitride film described below can be maximized.

[0070] As the above metalloid precursor compound, for example, a compound having a structure in which one or more ligands (L) are bonded to a Group 14 metalloid can be used.

[0071] The ligand (L) is guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 can be independently -CH3, -CH2CH3, -iPr, -tBu, or -H, and in this case, the change in the precursor state before and after the ligand exchange can be formed by the process of moving to the substrate and the reaction between the halogen of the deposition material on the substrate and the alkyl-free halide for replacing the ligand of the Group 14 metalloid precursor.

[0072] As a specific example, taking silicon as an example, a compound represented by the following chemical formula 1-1 or 1-2 can be used.

[0073] In the chemical formula 1-1 below, silicon can be replaced with another group 14 element such as germanium (Ge), and in this case, the effect of reducing process by-products is large, the step coverage is excellent, and the deposition film density is excellent.

[0074] [Chemical Formula 1-1]

[0075]

[0076] [Chemical Formula 1-2]

[0077]

[0078] In the case of the following chemical formula 1-1 or 1-2, there are advantages such as a large effect of reducing process by-products, excellent step coverage, and an effect of improving the density of the deposited film.

[0079] In the above chemical formula 1-1, L1, L2, L3 and L4 may be the same or different.

[0080] For example, in the chemical formula 1-1, L1 is -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, or -OR1, and L2, L3, and L4 can each independently be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2, and R3 can each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0081] As another example, in the above chemical formula 1-1, L1 and L2 may each independently be -iPr, -tBu, -Cp, -Ph, or -OR1, and L3 and L4 may each independently be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2, and R3 may each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0082]

[0083] As another example, in the above chemical formula 1-1, L1, L2, and L3 may each independently be -iPr, -tBu, -Cp, -Ph, or -OR1, and L4 may be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2, and R3 may each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0084] As another example, in the chemical formula 1-1 above, L 1' , L 2' , L 3' , L 4' are each independently -iPr, -tBu, -Cp, -Ph, or -OR1, and R1 can be -H, -CH3, -CH2CH3, -iPr, or -tBu.

[0085] In the above chemical formula 1-1, the ligands can form a symmetrical or asymmetrical structure.

[0086] In the above chemical formula 1-2, L1', L2', L3' and L4' may be the same or different.

[0087] For example, in the chemical formula 1-2 above, L 1' is -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, or -OR1, and L 2' , L 3' , L 4' can each independently be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2 and R3 can each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0088] As another example, in the above chemical formula 1-2, L 1' , L 2' are each independently -iPr, -tBu, -Cp, -Ph, or -OR1, and L 3' , L 4'can each independently be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2 and R3 can each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0089] As another example, in the above chemical formula 1-2, L 1' , L 2' , L 3' are each independently -iPr, -tBu, -Cp, -Ph, or -OR1, and L4 can be -H, -CH3, -CH2CH3, -OH, -NR2R3, wherein R1, R2, and R3 can each independently be -CH3, -CH2CH3, -iPr, or -tBu.

[0090] As another example, in the above chemical formula 1-2, L 1' , L 2' , L 3' , L 4' are each independently -iPr, -tBu, -Cp, -Ph, or -OR1, and R1 can be -H, -CH3, -CH2CH3, -iPr, or -tBu.

[0091] Unless otherwise stated herein, Pr refers to a propyl group, Bu refers to a butyl group, and Ph refers to a phenyl group.

[0092] The structure represented by the above chemical formula 1-1 or 1-2 may be, for example, DPS (Diphenyl silane), DIS (Diiodo silane), HCDS (Hexachloro disilane), DCS (Dichloro silane), etc.

[0093]

[0094] In the present invention, the semi-metal precursor compound can be introduced into the chamber by mixing it with, for example, a non-polar solvent, and in this case, there is an advantage in that the viscosity or vapor pressure of the semi-metal precursor compound can be easily controlled.

[0095] The above non-polar solvent may preferably be at least one selected from the group consisting of alkanes and cycloalkanes, and in this case, there is an advantage in that the step coverage is improved even when the deposition temperature increases during the formation of the deposition film while containing an organic solvent that has low reactivity and is easy to manage moisture.

[0096] As a more preferred example, the non-polar solvent may include a C1 to C10 alkane or a C3 to C10 cycloalkane, preferably a C3 to C10 cycloalkane, in which case it has the advantage of low reactivity and easy moisture management.

[0097] In this description, C1, C3, etc. refer to the number of carbon atoms.

[0098] The above cycloalkane may preferably be a C3 to C10 monocycloalkane, and among the above monocycloalkanes, cyclopentane is liquid at room temperature and has the highest vapor pressure, so it is preferred in a vapor deposition process, but is not limited thereto.

[0099] The above nonpolar solvent has, for example, a solubility in water (25°C) of 200 mg / L or less, preferably 50 to 400 mg / L, more preferably 135 to 175 mg / L, and within this range has the advantage of low reactivity toward the metalloid precursor compound and easy moisture management.

[0100] In this description, solubility is not particularly limited if it is measured using a measurement method or standard commonly used in the technical field to which the present invention belongs, and for example, a saturated solution can be measured using the HPLC method.

[0101] The non-polar solvent may preferably comprise 5 to 95 wt%, more preferably 10 to 90 wt%, even more preferably 40 to 90 wt%, and most preferably 70 to 90 wt%, based on the total weight of the metalloid precursor compound and the non-polar solvent.

[0102] If the content of the non-polar solvent is added in excess of the upper limit, impurities are generated, increasing the impurity level in the deposition film. If the content of the organic solvent is added in excess of the lower limit, there is a disadvantage in that the effect of improving the step coverage due to the addition of the solvent and the effect of reducing the impurities are small.

[0103] Furthermore, the semi-metal precursor compound may be injected into the deposition chamber simultaneously with the aforementioned low-temperature deposition material, or the semi-metal precursor compound may be pre-injected into the deposition chamber and then the low-temperature deposition material may be post-injected.

[0104]

[0105] semi-metal nitride film

[0106] It includes a deposition film obtained using the deposition material for the aforementioned metalloid nitride film.

[0107] The above metalloid nitride film may have a precursor adsorption state before ligand exchange as substrate-M-Ln (n= integer from 1 to 3, M= Si, Ge, Sn, L=halogen-free ligand), and a precursor adsorption state after ligand exchange as substrate-M-LnXm (L=halogen-free ligand, X=Br, I, n=integer from 1 to 3, m=integer from 1 to 3, n+m=3), or when the precursor before ligand exchange moving onto the substrate is M-Ln (n=integer from 1 to 4, M= Si, Ge, Sn, L=halogen-free ligand), a precursor state after ligand exchange may be M-LnXm (L=halogen-free ligand, X=Br, I, n=integer from 1 to 3, m=integer from 1 to 4, n+m=4).

[0108] The ligand (L) may be -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 may independently be -CH3, -CH2CH3, -iPr, -tBu, or -H. In this case, the change in the precursor state before and after the ligand exchange may be formed by the process of moving to the substrate and the reaction between the halogen of the deposition material on the substrate and the alkyl-free halide to substitute the ligand of the Group 14 metalloid precursor.

[0109] The above semi-metal nitride film may include, for example, a structure represented by the following chemical formula 2.

[0110] [Chemical Formula 2]

[0111] M a A d

[0112] (In the above chemical formula 2, M is a group 14 metalloid, A is at least one of N and S, a is an integer greater than or equal to 1, and d is 0.8 to 2.2.)

[0113] The above deposition film may be a nitride film alone, or may include a sulfide film or chalcogenide in the nitride film, in which case the purpose of the present invention can be achieved.

[0114] The above deposition film may include the above-described film composition alone or as a selective area, but is not limited thereto, and also includes SiH and SiOH.

[0115] The above-mentioned deposition film can be used in semiconductor devices not only as a diffusion barrier film but also as an etching stop film, electrode film, dielectric film, gate insulating film, block oxide film, or charge trap.

[0116]

[0117] The above deposition film can be manufactured by various methods, and for example, can be manufactured by the following methods:

[0118] As a first step, a metalloid precursor compound including a Group 14 metalloid and a ligand can be injected onto a substrate loaded in a chamber.

[0119] The above ligands are, for example, L1, L2, L3, L4, L shown in the chemical formulas 1-1 and 1-2. 1' , L 2' , L 3' , L 4' It can be done, and duplicate descriptions are omitted here.

[0120] In the present invention, the method for delivering the metalloid precursor compound to the deposition chamber may include, for example, a method for delivering volatilized gas by using a mass flow controller (MFC) method, a method for controlling the flow rate of a liquid (Mass Flow Controller; MFC), including a liquid mass flow controller (LMFC), and a method for delivering a liquid (Liquid Delivery System; LDS).

[0121] At this time, as a carrier gas or dilution gas for moving the semi-metal precursor compound on the substrate, one or more mixed gases selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He) may be used, but is not limited thereto.

[0122] In the present invention, an inert gas may be used as the purge gas, for example, and preferably, the carrier gas or dilution gas may be used.

[0123] The chamber may be an atomic layer deposition (ALD) chamber, a plasma enhanced atomic layer deposition (PEALD) chamber, a vapor deposition (CVD) chamber, a plasma enhanced vapor deposition (PECVD) chamber, a metalorganic chemical vapor deposition (MOCVD) chamber, or a low pressure vapor deposition (LPCVD) chamber.

[0124] The above chamber can load a substrate and then perform a purging pretreatment.

[0125] In the present invention, purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the deposition film growth rate per cycle is appropriately controlled, and deposition is performed as or close to a single atomic mono-layer, which is advantageous in terms of film quality.

[0126] The substrate loaded into the chamber may include a semiconductor substrate such as a silicon substrate or silicon oxide.

[0127] The above substrate may further have a conductive layer or an insulating layer formed on top thereof.

[0128] The substrate may be maintained at a temperature of 50 to 500°C, or 80 to 500°C, within the chamber.

[0129] The above substrate can be heated to, for example, 50 to 500°C, specifically, 80 to 500°C, 100 to 800°C, or 200 to 500°C, and the semi-metal precursor compound as well as the deposition material for a semi-metal nitride film described below can be injected onto the substrate in an unheated or heated state, and depending on the deposition efficiency, the injection can be performed in an unheated state and then the heating conditions can be adjusted during the deposition process. For example, the injection can be performed on a substrate heated to 300 to 600°C for 1 to 30 seconds.

[0130] The amount (mg / cycle) of the semi-metal precursor compound injected into the chamber is, for example, a ratio of the amount (mg / cycle) of the semi-metal precursor compound injected into the chamber to the deposition material for the semi-metal nitride film used in the second step described later, of 1:1 to 1:20, preferably 1:1 to 1:15, more preferably 1:1 to 1:10, and within this range, the effect of improving the step coverage and reducing the process by-products is significant.

[0131]

[0132] The above first step may include one or more purging steps using an inert gas. The inert gas may be the carrier gas or dilution gas described above.

[0133] In the step of purging the non-absorbed metalloid precursor compound, the amount of purge gas injected into the chamber is not particularly limited as long as it is an amount sufficient to remove the non-absorbed metalloid precursor compound. For example, the amount may be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, based on the volume of the metalloid precursor compound injected into the chamber. Within this range, the non-absorbed metalloid precursor compound is sufficiently removed, so that the deposition film is formed evenly and deterioration of the film quality can be prevented. Here, the amounts of the purge gas and the metalloid precursor compound injected are each based on one cycle, and the volume of the metalloid precursor compound means the volume of the vaporized metalloid precursor compound vapor.

[0134] In the present invention, purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the deposition film growth rate per cycle is appropriately controlled, and deposition is performed as or close to a single atomic mono-layer, which is advantageous in terms of film quality.

[0135]

[0136] In the second step, alkyl-free halides are injected as low-temperature deposition materials to replace the leaving sites of the ligands with halogens. This effectively removes the ligands of the precursor adsorbed on the substrate, improving the reaction rate and appropriately reducing the deposition film growth rate. This significantly improves step coverage and film thickness uniformity, even when forming a deposition film on a substrate with a complex structure.

[0137] The above halogen may be selected from, for example, one or more of iodine and bromine, and it is preferable to use iodine.

[0138] The feeding time (second) of the deposition material for the semi-metal nitride film on the substrate surface is preferably 0.001 to 30 seconds per cycle, more preferably 0.02 to 30 seconds, even more preferably 0.04 to 30 seconds, and even more preferably 0.05 to 30 seconds. Within this range, there are advantages of a high deposition film growth rate, excellent step coverage, and excellent economic efficiency.

[0139] In this description, the feeding time of the deposition material for the semi-metal nitride film is based on a flow rate of 1 to 500 sccm for a chamber volume of 15 to 20 L, and more specifically, based on a flow rate of 10 to 200 sccm for a chamber volume of 18 L.

[0140] In this invention, a method for delivering a deposition material for a semi-metal nitride film to a deposition chamber may be, for example, a method for transporting volatile gas by using a mass flow controller (MFC) method (Vapor Flow Control; VFC).

[0141] The second step may include one or more purging steps using an inert gas. In the present disclosure, the purge gas may be, for example, the carrier gas or dilution gas.

[0142]

[0143] In the present invention, purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the deposition film growth rate per cycle is appropriately controlled, and deposition is performed as or close to a single atomic mono-layer, which is advantageous in terms of film quality.

[0144] In the step of purging the deposition material for the non-adsorbed metalloid nitride film, the amount of the purge gas injected into the chamber is not particularly limited as long as it is an amount sufficient to remove the deposition material for the non-adsorbed metalloid nitride film, but may be, for example, 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, and within this range, the deposition material for the non-adsorbed metalloid nitride film can be sufficiently removed so that the deposition film is formed evenly and deterioration of the film quality can be prevented. Here, the amounts of the purge gas and the deposition material for the metalloid nitride film are each based on one cycle, and the volume of the deposition material for the metalloid nitride film means the volume of the vaporized deposition material for the metalloid nitride film.

[0145] As a specific example, when the deposition material for the semi-metal nitride film is injected at a flow rate of 100 sccm and an injection time of 0.5 sec (based on 1 cycle), and a purge gas is injected at a flow rate of 3000 sccm and an injection time of 5 sec (based on 1 cycle) in the step of purging the deposition material for the semi-metal nitride film without adsorption, the injection amount of the purge gas is 300 times the injection amount of the deposition material for the semi-metal nitride film.

[0146]

[0147] If necessary, steps 1 and 2 above can be combined or performed in reverse order.

[0148] That is, a semi-metal precursor compound and a low-temperature deposition material can be simultaneously injected into a deposition chamber and then purged, thereby replacing all or part of the ligand of the precursor with the low-temperature deposition material to enable more effective adsorption onto the substrate.

[0149] In addition, the low-temperature deposition material can be sequentially injected into the deposition chamber and purged, and then the semi-metal precursor compound can be injected into the deposition chamber and purged, thereby replacing all or part of the low-temperature deposition material with the ligand of the precursor to enable more effective adsorption onto the substrate.

[0150] The chemical structure of the ligand of the above metalloid precursor compound may be formed through a 'pre-injection process in which the alkyl-free halogen compound is injected prior to the precursor injection process (sequential injection)', a 'mid-injection process in which the alkyl-free halogen compound and the precursor are injected simultaneously (co-injection)', or a 'post-injection process in which the alkyl-free halogen compound is injected after the precursor injection process'. This may be formed through a reaction of some or all of the ligands of the metalloid precursor compound implanted on the substrate with an alkyl-free halide containing a halogen.

[0151] The ligand of the semi-metal precursor compound implanted on the substrate and substituted with an alkyl-free halogen ligand is removed by reacting with a hydrogen (H) atom derived from the reactant, and as a result, the Group 14 semi-metal adsorbed on the substrate can form a thin film by combining with nitrogen (N) derived from the reactant.

[0152]

[0153] Next, as a third step, a reactant can be injected into the substrate to form a deposition film derived from a group 14 semi-metal.

[0154] The above reactant may be a gaseous compound including, for example, H2O, H2O2, O2, O3, O radical, D2, H2, H radical, NH3, N2H2, N2O, N2, N radical, H2S or S.

[0155] The above-mentioned deposition film intermediate may include a structure in which a group 14 metalloid is combined with a reactant-derived substance and a halogen.

[0156] The above deposition film may include a structure in which a reactant-derived material is bonded to a Group 14 metalloid.

[0157] The above deposition film forming method can be carried out at a deposition temperature in the range of, for example, 50 to 800°C, preferably at a deposition temperature in the range of 100 to 700°C, more preferably at a deposition temperature in the range of 200 to 650°C, even more preferably at a deposition temperature in the range of 220 to 500°C, and even more preferably at a deposition temperature in the range of 220 to 450°C, and within this range, there is an effect of growing a deposition film of excellent film quality while implementing process characteristics.

[0158] The above deposition film formation method can be performed at a deposition pressure in the range of, for example, 0.01 to 20 Torr, preferably at a deposition pressure in the range of 0.1 to 20 Torr, more preferably at a deposition pressure in the range of 0.1 to 10 Torr, and has the effect of obtaining a deposition film of uniform thickness within this range.

[0159] In this description, the deposition temperature and deposition pressure can be measured as the temperature and pressure formed within the deposition chamber, or as the temperature and pressure applied to the substrate within the deposition chamber.

[0160] The second step may further include a step of raising the temperature inside the chamber to a deposition temperature before introducing the deposition material for the semi-metal nitride film into the chamber; and / or a step of purging the chamber by injecting an inert gas into the chamber before introducing the deposition material for the semi-metal nitride film into the chamber.

[0161] The third step may include a purging step using an inert gas.

[0162] In the purging step performed immediately after the reaction gas supply step, the amount of purge gas injected into the chamber may be, for example, 10 to 10,000 times the volume of the reaction gas injected into the chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, and the desired purpose can be achieved within this range. Here, the injection amounts of the purge gas and the reaction gas are each based on one cycle.

[0163] In the present invention, purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the deposition film growth rate per cycle is appropriately controlled, and deposition is performed as or close to a single atomic mono-layer, which is advantageous in terms of film quality.

[0164]

[0165] The above deposition film forming method can repeat the unit cycle 1 to 99,999 times as needed, preferably repeat the unit cycle 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within this range, the desired thickness of the deposition film can be obtained while achieving the purpose to be achieved in the present invention.

[0166]

[0167] As a specific example of the above deposition film manufacturing method, in order to deposit a deposition film on a substrate positioned in the chamber, the above-described deposition material for a semi-metal nitride film and a semi-metal precursor compound or a mixture thereof and a non-polar solvent are each prepared.

[0168] Afterwards, the prepared semi-metal precursor compound or a mixture thereof with a non-polar solvent is injected into a vaporizer, changed into a vapor phase, and transferred to a deposition chamber to be adsorbed on a substrate, and the ligand of the semi-metal precursor compound is replaced by a deposition material for a semi-metal nitride film that has been injected in advance, and the non-adsorbed semi-metal precursor compound is purged.

[0169] Next, the prepared deposition material for a semi-metal nitride film is injected into a vaporizer, then changed into a vapor phase and transferred to a deposition chamber to be adsorbed on a substrate, and purging is performed to remove the deposition material for a semi-metal nitride film that is not adsorbed.

[0170] In this description, the method for delivering the deposition material and the metalloid precursor compound for the metalloid nitride film to the deposition chamber may be, for example, a method for delivering volatilized gas using a mass flow controller (MFC) method (Vapor Flow Control; VFC) or a method for delivering liquid using a liquid mass flow controller (LMFC) method (Liquid Delivery System; LDS).

[0171] At this time, as a transport gas or dilution gas for moving the deposition material for the semi-metal nitride film and the semi-metal precursor compound onto the substrate, one or more mixed gases selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He) may be used, but is not limited thereto.

[0172] In the present invention, an inert gas may be used as the purge gas, for example, and preferably, the carrier gas or dilution gas may be used.

[0173] Next, supply the reactant.

[0174] The above-mentioned reactant is not particularly limited as long as it is a reaction gas commonly used in the technical field to which the present invention pertains, and may preferably include a nitriding agent. The nitriding agent reacts with a metalloid precursor compound adsorbed on the substrate to form a nitride film.

[0175] Preferably, the nitriding agent may be nitrogen gas (N2), hydrazine gas (N2H4), or a mixture of nitrogen gas and hydrogen gas.

[0176] Next, the unreacted residual reaction gas is purged using an inert gas. This removes not only the excess reaction gas but also any generated byproducts.

[0177] As described above, the method for forming a deposition film comprises, for example, a step of adsorbing a semi-metal precursor compound onto a substrate, a step of purging the non-adsorbed semi-metal precursor compound, a step of supplying a deposition material for a semi-metal nitride film onto a substrate, a step of purging the non-adsorbed deposition material for a semi-metal nitride film, a step of supplying a reaction gas, and a step of purging the residual reaction gas, and the unit cycle can be repeated to form a deposition film of a desired thickness.

[0178] As another example, the method for forming a deposition film comprises a step of transferring a metalloid precursor compound and a low-temperature deposition material to a substrate and reacting them to replace a ligand, a step of adsorbing the substituted precursor compound onto the substrate, a step of purging the non-adsorbed metalloid precursor compound, the substituted precursor compound, and the unreacted low-temperature deposition material, a step of supplying a reaction gas, and a step of purging the residual reaction gas, and the unit cycle can be repeated to form a deposition film of a desired thickness.

[0179] The above unit cycle may be repeated, for example, 1 to 99,999 times, preferably 10 to 1,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within this range, there is an effect of well expressing the desired deposition film characteristics.

[0180]

[0181] When the injection time and purge time of the metalloid precursor compound in the first step are a and b, respectively, the injection time and purge time of the alkyl-free halide in the second step are c and d, respectively, and the injection time and purge time of the reactant in the third step are e and f, respectively, 0.1≤a≤30, a≤b≤3a, 0.1≤c≤30, c≤d≤4c, 2≤e≤60, e≤f≤3e can be satisfied simultaneously.

[0182] When the injection and purge of the above metalloid precursor compound and alkyl-free halide, and the injection and purge of the reactant are considered as one cycle, the following four conditions are met: 1) The deposition thickness of the above metalloid nitride film measured by an ellipsometer is 500 2) The film growth rate is 0.09 Å / cycle or more, and 3) the density of the deposited film is 2 g / cm 3 Above, 4) The refractive index of the deposited film (@350 nm wavelength) can satisfy all of 2 or more.

[0183] The above semi-metal nitride film has a deposition thickness of 500 as measured by an ellipsometer. or less, or 2 to 300 It can be, more preferably, 5 to 250 It could be.

[0184] The density of the above deposition film is 2 to 5.5 g / cm 3 , or 2 to 5 g / cm 3 It could be.

[0185] The above semi-metal nitride film may have a refractive index (@350 nm wavelength) measured by an ellipsometer of 2 or less, or 1 to 2.

[0186] The above deposition film manufacturing method can be performed using a deposition film manufacturing apparatus including, for example, an ALD chamber, a first vaporizer for vaporizing a deposition material for a semi-metal nitride film, a first transport means for transporting the vaporized deposition material for a semi-metal nitride film into the ALD chamber, a second vaporizer for vaporizing a deposition film precursor, and a second transport means for transporting the vaporized deposition film precursor into the ALD chamber. Here, the vaporizer and the transport means are not particularly limited as long as they are vaporizers and transport means commonly used in the technical field to which the present invention pertains, and the vaporizer may be omitted when the gas mixture or vapor pressure is 0.1 Torr or higher at room temperature.

[0187]

[0188] semiconductor substrate

[0189] The present invention also provides a semiconductor substrate, characterized in that the semiconductor substrate is manufactured by the deposition film forming method of the present invention or includes the deposition film, in which case the step coverage of the deposition film and the thickness uniformity of the deposition film are significantly excellent, and the density of the deposition film, etc. are excellent.

[0190] As described above, the change in the adsorption state of the semi-metal precursor before and after ligand exchange can be formed by a reaction between the halogen-containing Group 14 semi-metal precursor compound on the substrate and an alkyl-free halide containing a halogen to fill the ligand leaving site of the semi-metal precursor compound described above.

[0191] For example, the semiconductor substrate may include a metalloid nitride film formed through a process in which a ligand bonded to a Group 14 metalloid is substituted with a halogen atom (Br or I) forming an alkyl-free halide, and then the position from which the halogen atom (Br or I) has been removed is replaced with nitrogen (N).

[0192]

[0193] For example, the semiconductor substrate may provide a semiconductor substrate in which, when the precursor adsorption state before ligand exchange on the substrate is substrate-M-Ln (n=an integer from 1 to 3, M=Si, Ge, Sn, L=halogen-free ligand), the precursor adsorption state after ligand exchange is substrate-M-LnXm (L=halogen-free ligand, X=Br, I, n=an integer from 1 to 3, and m=an integer from 1 to 3, satisfying n+m=3).

[0194] As another example, the semiconductor substrate may provide a semiconductor substrate in which, when the precursor before ligand exchange moving onto the substrate is M-Ln (n=an integer from 1 to 4, M=Si, Ge, Sn, L=halogen-free ligand), the precursor state after ligand exchange is M-LnXm (L=halogen-free ligand, X=Br, I, n=an integer from 1 to 3, m=an integer from 1 to 4, satisfying n+m=4).

[0195] The above-mentioned semi-metal nitride film may be, for example, a multilayer structure of two or more layers, a multilayer structure of three or more layers, or a multilayer structure of two or three layers, as needed. The multilayer film having a two-layer structure may be, for example, a lower layer film-middle layer film structure, and the multilayer film having a three-layer structure may be, for example, a lower layer film-middle layer film-upper layer film structure.

[0196] The above-mentioned intermediate layer may be, for example, a TiN electrode for DRAM or a barrier film for NAND.

[0197] The above-mentioned lower layer film may be formed by including at least one selected from the group consisting of Si, SiO2, MgO, Al2O3, CaO, ZrSiO4, ZrO2, HfSiO4, Y2O3, HfO2, LaLuO2, Si3N4, SrO, La2O3, Ta2O5, BaO, and TiO2, for example, as a metal film, nitride film, or oxide film of a different composition from a semi-metallic nitride film.

[0198] The above upper layer film may be formed by including, for example, a metal film, nitride film, or oxide film of a different composition from a semi-metallic nitride film, and at least one selected from the group consisting of Si, SiO2, TiN, TiSiN, W, Mo, and MoN.

[0199]

[0200] semiconductor devices

[0201] According to the present invention, a semiconductor device including the above-described semiconductor substrate can be provided.

[0202] The semiconductor device may be, for example, a low resistive metal gate interconnect, a high aspect ratio 3D metal-insulator-metal (MIM) capacitor, a DRAM trench capacitor, a 3D Gate-All-Around (GAA), or a 3D NAND flash memory.

[0203]

[0204] Hereinafter, preferred embodiments and drawings are presented to help understand the present invention, but the following embodiments and drawings are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present invention, and it is also natural that such changes and modifications fall within the scope of the appended patent claims.

[0205]

[0206] [Example]

[0207] Diphenyl silane (DPS), Diiodo silane (DIS), Hexachloro disilane (HCDS), and Dichloro silane (DCS) were prepared as metalloid precursor compounds, respectively.

[0208] 6N HI was prepared as a deposition material for the semi-metal nitride film.

[0209] An ALD deposition process was performed using the above metalloid precursor compound and the deposition material for a metalloid nitride film, with the deposition process sequence according to the present invention being one cycle.

[0210] The specific experimental methods of Examples 1 to 6 and Comparative Examples 1 to 8 are as follows.

[0211]

[0212] Examples 1 to 3

[0213] The internal atmosphere of the deposition chamber was formed so that the working pressure was 1.2 Torr by injecting 3000 sccm of argon into the chamber through a mass flow controller (MFC).

[0214] Then, a silicon wafer was placed on the heating block to match the deposition temperature.

[0215] Next, the canister filled with the semi-metal precursors shown in Table 1 below was heated or cooled so that the vapor pressure at which the semi-metal precursors were injected into the chamber was 0.01 to 10 Torr, thereby introducing the semi-metal precursors into the chamber in a vapor state, while injecting 100 sccm of hydrogen iodide as a low-temperature deposition material into the chamber for 1 to 30 seconds. Thereafter, the chamber was purged for twice the time for which the semi-metal precursors and low-temperature deposition material were injected.

[0216] Afterwards, ammonia as a reactant was injected into the chamber at 500 sccm for 3 to 60 seconds using a 100 W plasma, and then purged for twice the ammonia injection time. The specific experimental conditions are as shown in Table 1 below.

[0217] This process was repeated 200 to 400 times to form three types of self-limiting atomic layer deposition films.

[0218]

[0219] Comparative Examples 1 to 3

[0220] The same process as in Examples 1 to 3 was repeated except that no low-temperature deposition material was used in Examples 1 to 3.

[0221]

[0222] Examples 4 to 6

[0223] The internal atmosphere of the deposition chamber was formed so that the working pressure was 1.2 Torr by injecting 3000 sccm of argon into the chamber through a mass flow controller (MFC).

[0224] Then, a silicon wafer was placed on the heating block to match the deposition temperature.

[0225] Next, the canister filled with the semi-metal precursors shown in Table 1 below was heated or cooled so that the vapor pressure at which the semi-metal precursors were injected into the chamber was 0.01 to 10 Torr, and the semi-metal precursors were injected into the chamber in a vapor state for 1 to 30 seconds. Afterwards, the canister was purged for twice the time of the semi-metal precursor injection.

[0226] Next, the canister filled with the low-temperature deposition material was heated or cooled, and 100 sccm of hydrogen iodide was injected into the chamber for 1 to 30 seconds. Afterwards, the chamber was purged for twice the time of the low-temperature deposition material injection.

[0227] Afterwards, ammonia as a reactant was injected into the chamber at 500 sccm for 3 to 60 seconds using a 100 W plasma, and then purged for twice the ammonia injection time. The specific experimental conditions are as shown in Table 1 below.

[0228] This process was repeated 200 to 400 times to form three additional types of self-limiting atomic layer deposition films.

[0229]

[0230] Comparative examples 4 to 6

[0231] The same process as in Examples 4 to 6 was repeated except that no low-temperature deposition material was used in Examples 4 to 6.

[0232]

[0233] Comparative examples 7 and 8

[0234] The same process as in Comparative Example 4 was repeated except that the semi-metal precursor in Comparative Example 4 was replaced with the material shown in Table 1 below and the deposition temperature was increased to 600°C.

[0235]

[0236] [Example Exam]

[0237] *Film growth rate: The thickness of a 1 to 30 nm thick film measured at room temperature and pressure using an ellipsometer is divided by the number of deposition cycles, expressed in Å / cycle. The measurement results are shown in Table 1 and Fig. 2.

[0238] *Cycle linearity: In Example 2 above, the film thickness was measured while increasing the deposition from 100 cycles to 1000 cycles, and the results are shown in Fig. 2.

[0239] *Refractive index: The refractive index (@350 nm wavelength) of the manufactured deposition film was measured using an ellipsometer, and the results are shown in Table 1, Fig. 2, and Fig. 3, respectively.

[0240] *Film density: The film density of the manufactured deposition film was measured using X-ray diffraction (XRR) equipment, and the results are shown in Table 1 and Fig. 4 below.

[0241] Classification Metalloid precursor Low temperature deposition material Reactant Deposition temperature Deposition rate (Å / chycle) [Figure 1] Refractive index (λ = 350 nm) [Figure 3] Thin film density (g / cm) 3 ) [Figure 4] Example 1 DPSHI (co-injection) NH3 (PE 100W) 300 ℃ 0.24 1.83 2.47 Example 2 DPSHI (co-injection) NH3 (PE 100W) 400 ℃ 0.2-2.70 Example 3 DPSHI (co-injection) NH3 (PE 100W) 500 ℃ 0.18-2.60 Example 4 DPSHI (post-injection) NH3 (PE 100W) 300 ℃ 0.13--Example 5 DPSHI (post-injection) NH3 (PE 100W) 300 ℃ 0.1--Example 6 DPSHI (post-injection) NH3 (PE 100W) 300 ℃ 0.09--Comparative Example 1 DPS-NH3 (PE 100W) 300 ℃N / A--Comparative Example 2 DPS-NH3 (PE 100W) 400 ℃N / A--Comparative Example 3 DPS-NH3 (PE 100W) 500 ℃N / A-Comparative Example 4 DIS-NH3 (PE 100W) 300 ℃1.021.752.41Comparative Example 5 DIS-NH3 (PE 100W) 400 ℃0.95-2.53Comparative Example 6 DIS-NH3 (PE 100W) 500 ℃0.87-2.48Comparative Example 7 HCDS-NH3 600 ℃0.61.94-Comparative Example 8 DCS-NH3 600 ℃0.451.95-

[0242] As shown in Table 1 above, it was confirmed that Examples 1 to 6 according to the present invention, which used a precursor ligand and a deposition material for a metalloid nitride film of a different type, showed significantly improved thin film growth rate, refractive index, and thin film density compared to Comparative Examples 1 to 8, which did not use a low-temperature deposition material.

[0243] In particular, in Comparative Examples 1 to 3 that did not use the deposition material for a semi-metal nitride film according to the present invention, a thin film was not grown, whereas in Examples 1 to 3 that used the same, a significantly reduced thin film growth rate was realized in growing a thin film, as shown in FIG. 1 below. For reference, FIG. 1 below is a diagram comparing the thin film growth rates of three types of deposition films of Examples 1 to 3 that used the deposition material for a semi-metal nitride film according to the present invention, according to deposition temperature.

[0244] As shown in the following Figure 2, Example 2 using the deposition material for a semi-metal nitride film according to the present invention was able to confirm the linearity of the cycles by measuring the film thickness while increasing from 100 cycles to 1000 cycles.

[0245] In addition, it was confirmed through Fig. 3 that Example 1 using the deposition material for a semi-metal nitride film according to the present invention had a higher refractive index value than Comparative Examples 4, 7, and 8 that did not use the same. For reference, Fig. 3 is a diagram comparing the refractive index (@350 nm wavelength) of the deposition film of Example 1 using the deposition material for a semi-metal nitride film according to the present invention with the refractive index (@350 nm wavelength) of the deposition films obtained from Comparative Examples 4, 7, and 8.

[0246]

[0247] Furthermore, it was confirmed through Fig. 4 that Examples 1 to 3 using the deposition material for a semi-metal nitride film according to the present invention had a higher thin film density than Comparative Examples 4 to 6 not using the same. For reference, Fig. 4 is a diagram comparing the XRR (X-ray diffraction) thin film density for the deposited films of Examples 1 to 3 using the deposition material for a semi-metal nitride film according to the present invention with the XRR (X-ray diffraction) thin film density for the deposited films of Comparative Examples 4 to 6 not using the same.

[0248]

[0249] Therefore, according to the present invention, by sequentially or simultaneously injecting a low-temperature deposition material into a halogen-free precursor compound that does not contain a halogen as a ligand, the ligand of the halogen-free precursor and the low-temperature deposition material exchange positions, thereby improving the reactivity with a reactant subsequently injected in the deposition process after being implanted on the substrate, thereby improving the thin film growth rate and greatly improving the density and refractive index of the deposition film, and it was confirmed that the deposition film is uniformly formed even on a substrate with a complex pattern.

Claims

A deposition material for a metalloid nitride film comprising an alkyl-free halide for substituting part or all of the ligands of a group 1.14 metalloid precursor compound.

2. In paragraph 1, A deposition material for a semi-metal nitride film, characterized in that the halogen constituting the above alkyl-free halide is at least one selected from iodine and bromine.

3. In paragraph 1, A deposition material for a metalloid nitride film, characterized in that the above Group 14 metalloid is selected from at least one of silicon (Si), germanium (Ge), and tin (Sn).

4. In paragraph 1, A deposition material for a metalloid nitride film, characterized in that the above alkyl-free halide is an alkyl-free iodine, hydrogen iodide, hydrogen bromide, iodine ion or iodine radical.

5. A method for forming a semi-metal nitride film, characterized in that it comprises a process of changing some or all of the ligands of the semi-metal precursor compound by using some or all of a deposition material for a semi-metal nitride film including an alkyl-free halide of any one of claims 1 to 4 on a substrate.

6. In paragraph 5, A method for forming a metalloid nitride film, characterized in that the above metalloid precursor compound is a precursor compound centered on a Group 14 metalloid, and the Group 14 metalloid is at least one selected from silicon (Si), germanium (Ge), and tin (Sn).

7. In paragraph 5, A method for forming a semi-metal nitride film, characterized in that the ligand (L) is -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 are each independently -CH3, -CH2CH3, -iPr, -tBu, or -H.

8. In paragraph 5, A semi-metal nitride film characterized in that the above deposition is atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma-enhanced vapor deposition (PECVD), metalorganic chemical vapor deposition (MOCVD), or low-pressure vapor deposition (LPCVD).

9. A semiconductor substrate comprising a semi-metal nitride film manufactured according to the method for forming a semi-metal nitride film of claim 5 on a substrate, wherein the semi-metal nitride film has a precursor adsorption state before ligand exchange as substrate-M-Ln (n=integer of 1 to 3, M=Si, Ge, Sn, L=halogen-free ligand), and a precursor adsorption state after ligand exchange as substrate-M-LnXm (L=halogen-free ligand, X=Br, I, n=integer of 1 to 3, m=integer of 1 to 3, n+m=3).

10. A semiconductor substrate comprising a semi-metal nitride film manufactured according to the method for forming a semi-metal nitride film of claim 5 on a substrate, wherein the semi-metal nitride film is a semiconductor substrate in which, when a precursor before ligand exchange moving onto the substrate is M-Ln (n= an integer of 1 to 4, M= Si, Ge, Sn, L= a halogen-free ligand), the precursor state after ligand exchange is M-LnXm (L= a halogen-free ligand, X=Br, I, n= an integer of 1 to 3, m= an integer of 1 to 4, n+m=4 is satisfied).

11. In paragraph 9, A semiconductor substrate characterized in that the ligand (L) is -guanidiate, -amidinate, -triazenide, -iPr, -tBu, -Cp, -Ph, -OR1, -OH, -H, or -NR2R3, wherein R1, R2, and R3 are each independently -CH3, -CH2CH3, -iPr, -tBu, or -H, and the change in the precursor state before and after the ligand exchange is formed by a reaction between an alkyl-free halide for the halogen of the deposition material to replace the ligand of the Group 14 metalloid precursor on the substrate and the process of moving to the substrate.

12. In paragraph 9, A semiconductor substrate characterized in that the semiconductor substrate has a multilayer structure of two or more layers.

13. In paragraph 9, A semiconductor substrate characterized in that the above semi-metal nitride film has a thin film growth rate of 0.09 Å / cycle or more, which is calculated by dividing the thickness measured by an ellipsometer by the number of deposition cycles.

14. In paragraph 9, A semiconductor substrate characterized in that the above semi-metal nitride film has a refractive index (@350 nm wavelength) of 2 or less as measured using an ellipsometer.

15. A semiconductor device characterized by including a semiconductor substrate according to claim 9.

Citation Information

Patent Citations

  • Organometallic composition

    JP2007169785A

  • Apparatus and method for injection molding of high-density polyethylene-carbon composite

    KR1020230114511A

  • Hydraulic servo valve control device, hydraulic servo valve control method, hydraulic servo valve control program

    KR102510782B1

  • Forming improved metal nitrides

    US7276121B1

  • KR20230143549A