Bipolar plate for fuel cells and method for manufacturing same

The method of mixing carbon nanotubes with thermoplastic polymers and subsequent compression molding addresses the integration challenges of single-walled carbon nanotubes in bipolar plates, achieving high conductivity and strength while maintaining low weight and stability, enhancing fuel cell performance.

WO2024225932A1PCT designated stage expired Publication Date: 2024-10-31MCD TECHNOLOGIES S A RL +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/RU2023/000131
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current methods for producing bipolar plates for fuel cells face challenges in achieving high electrical conductivity and mechanical strength while maintaining low weight and chemical stability, particularly due to the complexity of incorporating single-walled carbon nanotubes, which are essential for optimal performance but difficult to integrate effectively into composite materials.

Method used

A method involving mixing single-walled and/or double-walled carbon nanotube powder with thermoplastic polymer powder at a temperature below the polymer's glass transition temperature, followed by compression molding above the glass transition temperature, to create a composite material with non-uniform carbon nanotube distribution, enhancing electrical conductivity and mechanical strength without increasing weight.

Benefits of technology

This approach results in thin bipolar plates with high electrical conductivity, mechanical strength, and thermal stability, reducing the weight of fuel cell stacks and improving the efficiency of high-temperature fuel cells by achieving the desired properties with lower carbon nanotube concentrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure RU2023000131_31102024_PF_FP_ABST
    Figure RU2023000131_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to electrically conductive composite materials based on thermoplastic polymers containing carbon nanotubes, and to methods for manufacturing same. The invention further relates to electrically conductive thin plates for use as bipolar plates in fuel cells, inter alia, proton exchange membrane fuel cells. The present invention proposes a method for producing thin electrically conductive plates, and further proposes a thin bipolar plate with a thickness of less than 1 mm for a high-temperature fuel cell, said plate having gas transport channels on the surface thereof and containing a composite material comprised of a thermoplastic polymer and single-walled and / or double-walled carbon nanotubes, wherein the composite material contains connected regions having a carbon nanotube concentration of more than 1 wt%, and domains having a size of less than 200 μm and a local concentration of carbon nanotubes of less than 1 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] BIPOLAR PLATE FOR FUEL CELLS AND METHOD OF ITS MANUFACTURING

[0002] Field of technology.

[0003] The invention relates to electrically conductive composite materials based on thermoplastic polymers containing carbon nanotubes and methods for producing them. The invention also relates to electrically conductive thin plates used as bipolar plates in fuel cells, including those with proton exchange membranes.

[0004] Prior art.

[0005] Bipolar plates are one of the key components of PEM (Proton Exchange Membrane or Polymer Electrolyte Membrane) fuel cells and contribute the most to their weight and cost. Bipolar plates must have high electrical conductivity, mechanical strength, corrosion resistance, and low gas permeability. To achieve these properties in highly conductive thin plates, various composite bipolar plates have been developed. Most of them are made by compression molding polymers (thermoplastic or thermosetting resins) filled with conductive particles such as graphite powders or carbon fibers.

[0006] To impart conductivity to polymers, conductive fillers must be included in their composition, which usually leads to a decrease in mechanical strength, since it is quite difficult to simultaneously obtain high conductivity and good mechanical properties using such hard and brittle fillers as graphite and carbon fibers. Thus, there are certain difficulties in the manufacture of very thin plates, which are most important for reducing the weight of the fuel cell. In addition, the highly acidic environment required for the operation of the bipolar plate, especially at elevated temperatures, significantly narrows the class of thermoplastic polymers that can be used. Currently, there is a significant increase in interest in the proton exchange membrane, which operates at elevated temperatures due to the greater efficiency and stability of catalysts that can operate with hydrogen and other fuels of limited quality.

[0007] In the article [T.M. Besmann, J.W. Klett, J.J. Henry, E. Lara-Curzio, Carbon / Carbon Composite Bipolar Plate for Proton Exchange Membrane Fuel Cells J. Electrochem. Soc. (2000) Vol. 147, pp. 4083-4086] polymers are used only at the initial stage of plate formation and are subsequently carbonized. Carbon-containing composite bipolar plates were developed, fabricated in several steps, including the production of carbon fiber / phenolic resin preforms followed by compression molding, subsequent pyrolysis, and surface densification by chemical vapor infiltration. The plates have high electrical conductivity, about 200-300 S / cm. However, the plate fabrication process is too complex, and the resulting material is 2 mm thick and has limited strength (36.5 MPa tensile strength is reported).Meanwhile, it is desirable that the tensile strength and bending strength of the plate material be at least 60 MPa, and the plate thickness be less than 1 mm.

[0008] Composite materials of polymers with carbon nanotubes have been proposed in some sources. US Patent No. 7,056,452B2 [IPC: H01B1 / 24, C08J3 / 21, C08K7 / 24] discloses a polymer composite material comprising polyvinylidene fluoride (PVDF) or a copolymer of polyvinylidene fluoride and another monomer; and carbon nanotubes in an amount of from about 0.01 to 30% by weight of said composite material, wherein said carbon nanotubes have a diameter of less than about 100 nm, and wherein said polymer composite material has a specific volume resistance of less than about 10 ohm cm.The present patent also claims a method for producing an electrically conductive composite material, which includes the steps of: (a) dissolving a polymer selected from the group consisting of polyvinylidene fluoride and a copolymer of vinylidene fluoride and another monomer in a solvent to form a solution; (b) dispersing nanotubes in said solution; and (c) adding a precipitating component to said solution to precipitate a composite material containing the polymer and nanotubes, wherein the composite material has a volume resistivity of less than 10 Ohm cm.

[0009] The method proposed above is very complex and includes the stages of dissolving polyvinylidene fluoride, dispersing the nanotubes in the solution and subsequent precipitation. This method requires large volumes of solvent, dispersing carbon nanotubes in the solution requires high energy costs, the resulting dispersions have a high viscosity and their mixing with the precipitating component is a difficult task. After precipitation and filtration, it is necessary to remove the residual solvent from the sediment. The indicated technological difficulties are especially serious if single-wall carbon nanotubes are used. US Patent No. 7,056,452 B2 [IPC: HO 1 B 1 / 24, C08J3 / 21, C08K7 / 24] describes embodiments only with multi-wall carbon nanotubes. The use of single-wall carbon nanotubes in the method proposed in US Patent No. 7,056,452 B2 [IPC: H01B1 / 24, C08J3 / 21, C08K7 / 24] is impossible.

[0010] Meanwhile, it is known that single-wall carbon nanotubes provide high electrical conductivity and have the greatest effect on the mechanical properties of composite materials compared to multi-wall carbon nanotubes. Single-wall carbon nanotubes have high mechanical strength (tensile stress exceeding 50 GPa), high thermal and electrical conductivity. Nanotubes are characterized by ballistic electrical conductivity of electrons on the scale of one nanotube at submicrometer lengths. Electrical conductivity along bundles or threads reaches 1 MS / cm. Single-wall carbon nanotubes have a diameter in the range of 0.7-5 nm and are theoretically unlimited in length. For example, commercially available material from OCSiAl Tuball™ has a length of single-wall carbon nanotubes greater than 5 cm and a diameter in the range of 1.6 ± 0.4 nm. The aspect ratio (length, L, to diameter, D) of single-wall carbon nanotubes is very large and can exceed several thousand.As a result of the interaction of van der Waals forces (l-l interaction), single-wall carbon nanotubes tend to agglomerate to form ordered bundles, which in turn can have an even higher aspect ratio. High L / D values ​​of carbon nanotube bundles make it possible to effectively increase the electrical conductivity in a composite material at low concentrations of carbon nanotubes. Single-wall carbon nanotubes and their bundles, unlike multi-wall carbon nanotubes, are flexible and can take any shape when bent, which is certainly important for their use as an electrically conductive and reinforcing additive in composite materials for bipolar plates obtained by compression molding. The properties of double-wall carbon nanotubes (DWCNTs) are close to the properties of single-wall carbon nanotubes.

[0011] The bipolar plates should have a high electrical conductivity of at least 2 S / cm, preferably more than 10 S / cm. Such electrical conductivity is achieved at a high concentration of the conductive filler, for example, when using single-wall and / or double-wall carbon nanotubes with a concentration exceeding several mass%. Adding a filler to a polymer composite melt / solution in an amount from several mass% to several tens of mass% is not a difficult task for carbon black, graphite, short fibers and even for multi-wall carbon nanotubes. However, for single- / double-wall carbon nanotubes, the process of adding them to the composite melt / solution is complicated by their extremely high L / D ratio noted above. This is why some patent documents propose adding several different fillers: an insignificant amount of carbon nanotubes and up to 70 mass% of graphite and / or carbon fibers.This approach improves electrical conductivity, but the mechanical properties of the composite material deteriorate, for example, brittleness increases. At the same time, brittle material cannot be used for thin plates with a fine structure of gas channels on the surface.

[0012] US Patent No. 7,629,070B2 [IPC: H01M8 / 02, H01B1 / 24] describes bipolar plates for fuel cells with proton exchange membranes, which include at least a mixture of two mutually immiscible polymers, including from 15 to 65% by weight of carbon fillers, wherein the polymer mixture contains as carbon fillers electrically conductive carbon in an amount of from 1 to 30% by weight, carbon fiber in an amount of from 5 to 60% by weight, and carbon nanotubes in an amount of from 1 to 25% by weight, based on the total weight of the polymer mixture. In addition to using three different types of conductive fillers with different L / D ratios, this invention proposes to use a mixture thereof with at least two immiscible polymers, wherein the polymer mixture comprises at least one polyamide and at least one polyether ketone or polyether sulfone as miscible polymers.In this case, at least two mixed polymers form a joint continuous structure, and carbon fillers are in a higher concentration in one of the mixed polymers or in the phase between the polymer mixture, or where the polymer mixture in which the carbon fillers are in a higher concentration forms a continuously conducting matrix in which at least one mixed polymer is intercalated. This approach allows for increasing electrical conductivity and reducing the required concentration of fillers, including carbon nanotubes. However, this imposes serious restrictions on the polymer composition - it is necessary to use at least two immiscible polymers, which complicates the preparation process and inevitably reduces the chemical and / or thermal stability of the composite material.The immiscible nature of the polymers means that they are very different in chemical nature, and it is therefore unlikely that the two polymers will have comparable thermal and chemical stability. US Patent No. 7,629,070B2 [IPC: H01M8 / 02, HO 1 B 1 / 24] cites as an example a blend of polyether ketone (PEEK) and polyamide (PA), where the polyamide is the weakest link: it decomposes rapidly at temperatures above 280 °C and dissolves in strong acids, while polyether ketone is chemically more stable and melts at 343 °C. In essence, the polyether ketone in this blend acts as an inert powder rather than a second thermoplastic polymer.

[0013] Thus, there is a technical problem of obtaining thin bipolar plates with high specific electrical conductivity of more than 2 S / cm and bending strength above 60 MPa, in which the above-mentioned disadvantages of the manufacturing process are eliminated. The most important and desirable characteristics of thin bipolar plates, in addition to high electrical conductivity and strength, are high thermal and chemical stability and low weight.

[0014] Disclosure of invention.

[0015] The present invention provides a method for producing thin conductive plates, which includes the steps of:

[0016] (1) mixing powder of single-wall and / or double-wall carbon nanotubes and powder of thermoplastic polymer at a temperature not exceeding the glass transition temperature of the thermoplastic polymer (T g) to obtain a mixture, the particles of which consist of a thermoplastic polymer core and a carbon nanotube shell; and (2) compression molding the mixture obtained in step (1) at a temperature exceeding the glass transition temperature of the thermoplastic polymer (T g ) by at least 100 K to obtain a thin plate of a given shape. The proposed method can be used to manufacture a bipolar plate less than 1 mm thick for high-temperature fuel cells with a proton exchange membrane containing a composite material: a thermoplastic polymer and single-wall and / or double-wall carbon nanotubes, and having gas transport channels on the surface. The composite material of the bipolar plate contains connected regions with a concentration of carbon nanotubes greater than 1% by weight, and domains whose size is less than 200 μm, with a local concentration of carbon nanotubes less than 1% by weight.

[0017] In such a composite material, single-wall and / or double-wall carbon nanotubes are mainly concentrated outside such polymer domains with a low content of single-wall and / or double-wall carbon nanotubes. A higher local concentration of single-wall and / or double-wall carbon nanotubes allows achieving higher electrical conductivity and mechanical strength. The manufacturing method is quite simple and allows forming thin plates with a thickness of less than 1 mm, preferably less than 0.5 mm, most preferably less than 0.2 mm and a size of surface elements (e.g. gas channels) less than 100 μm.

[0018] Single-walled and double-walled carbon nanotubes have diameters greater than 0.7 nm and less than 10 nm, preferably greater than 1.2 nm and less than 4 nm. They have a length greater than 100 nm and less than 50 μm, preferably greater than 500 nm and less than 20 μm. When there is a difference in the sizes of the two types of particles being mixed and when these particles tend to stick together (agglomerate) with each other, they naturally form core-shell particles with larger particles as the core and smaller particles forming the shell. In the case of single-walled and / or double-walled carbon nanotubes, their ability to bend and agglomerate into bundles results in the formation of a dense shell around the polymer core.

[0019] It is preferable that 90% by weight of the particles of the mixture obtained in step (1) have a size greater than 10 μm, most preferable that 90% by weight of the particles have a size less than 200 μm, even more preferable that 90% by weight of the particles of the powder obtained in step (1) have a size less than 150 μm. It is preferable that 99% by weight of the particles of the powder obtained in step (1) have a size less than 1 mm.

[0020] The mixing of the single-wall and / or double-wall carbon nanotube powder and the thermoplastic polymer powder can be carried out by any type of mixer for mixing powders, including paddle mixers, ribbon mixers, twin-shaft mixers, drum mixers, planetary mixers, or any other known mixer, not limited to the examples given.

[0021] It is important to mix powder of single-wall and / or double-wall carbon nanotubes and powder of thermoplastic polymer at a temperature not exceeding the glass transition temperature of the polymer (T g ) in order to prevent agglomeration of the polymer particles. Even more preferably, mixing is carried out at a temperature below the glass transition temperature of the polymer (T g ) by at least 20 K or at least 50 K, in order to avoid local heating of the powder to a temperature above the glass transition temperature during mixing of the single-walled and / or double-walled carbon nanotubes and the thermoplastic polymer powder. In some embodiments, it is preferable that the mixing temperature in step (1) does not exceed the Vogel temperature of the thermoplastic polymer.

[0022] The thermoplastic polymer may be any of the thermoplastic polymers or elastomers or biopolymers. However, for use in bipolar plates, it is preferable that the thermoplastic polymer is one of the thermally stable thermoplastic polymers selected from the group: polyvinylidene fluoride (PVDF), polyphenylene sulfide (PPS), polyethersulfone (PES), polysulfone (PSU), polyphenylene sulfone (PPSU) or polyetheretherketone (PEEK) or their copolymers or their derivatives, without being limited to the examples given.

[0023] In the step of compression molding the mixture, it is important that the molding temperature exceeds the glass transition temperature of the thermoplastic polymer (Tg) by at least 100 K in order to ensure the necessary mobility of the thermoplastic polymer for forming a shell of single-walled and / or double-walled carbon nanotubes and forming a homogeneous electrically conductive plate. For some embodiments, it is acceptable for the compression molding temperature of the mixture to exceed the glass transition temperature of the thermoplastic polymer (T g ) by at least 150 K. This allows for the compression molding process to be accelerated. For some embodiments, it is preferable for the compression molding temperature of the mixture to be higher than the glass transition temperature of the thermoplastic polymer (T g) by at least 250 K. For some embodiments, it is preferable that the compression molding temperature of the mixture exceeds the melting temperature of the thermoplastic polymer (T т ).

[0024] For some embodiments of the invention, the compression molding process is performed in an inert gas atmosphere.

[0025] Due to the non-uniform distribution of single-wall and / or double-wall carbon nanotubes in the thin plate composite material, the required electrical conductivity is achieved at a lower concentration of carbon nanotubes than in the case of a uniform distribution. This is due to the fact that the electrical conductivity and strength of the composite material are provided by connected regions with a high concentration of single-wall and / or double-wall carbon nanotubes. Thus, the weight ratio of the content of single-wall and double-wall carbon nanotubes to the content of the thermoplastic polymer in the mixture obtained in step (1) of the method can be less than 0.1 or less than 0.03, or less than 0.02, or less than 0.01. However, it is most preferable that the weight ratio of the content of single-wall and double-wall carbon nanotubes to the content of the thermoplastic polymer in the mixture is more than 0.01 and less than 0.3.For some embodiments of the invention, it is most preferable that the weight ratio of the content of single-wall and double-wall carbon nanotubes to the content of thermoplastic polymer in the mixture is from 0.05 to 0.25 by weight.

[0026] The powder of single-wall and / or double-wall carbon nanotubes used in this invention can be used both in unprocessed form and can be chemically and / or thermally processed for the purpose of purification, or functionalization, or defunctionalization, or doping, or chemical modification before mixing them with the thermoplastic polymer powder. If it is necessary to achieve higher electrical conductivity values, single-wall and / or double-wall carbon nanotubes can be subjected to chemical doping. One of the chemical modifications includes purification from residual catalyst, which can slightly affect the amount of functional oxygen-containing functional groups on the walls of single-wall carbon nanotubes.Oxygen-containing functional groups on the surface of single-wall carbon nanotubes promote better adhesion of single-wall carbon nanotubes to a polymer matrix and can be added to the surface of single-wall carbon nanotubes by heating them in an oxygen-saturated atmosphere or, if necessary, removed by heating the carbon nanotubes in an inert atmosphere.

[0027] The single-wall and / or double-wall carbon nanotubes used in the present invention may be either closed-ended or open-ended. Chemical and / or thermal treatment of the single-wall and / or double-wall carbon nanotubes may be used to open or close the ends of the carbon nanotubes.

[0028] The powder of single-wall and / or double-wall carbon nanotubes used in this invention may include particles of metals of groups 8-11 of the Periodic Table, such as iron (Fe), or cobalt (Co), or nickel (Ni), or ruthenium (Ru), or rhodium (Ro), or palladium (Pd), or iridium (Ir), or platinum (Pt), or copper (Cu), or silver (Ag), or gold (Au), or their alloys, or their carbides, without limiting themselves to the listed examples, which are impurities caused by the method of producing single-wall and / or double-wall carbon nanotubes. The metal particles may be coated with graphite shells, which also originate from the method of producing carbon nanotubes.

[0029] The present invention proposes a thin bipolar plate with a thickness of less than 1 mm for a high-temperature fuel cell, having gas transport channels on the surface and containing a composite material of a thermoplastic polymer and single-walled and / or double-walled carbon nanotubes, characterized in that the composite material contains connected regions with a concentration of carbon nanotubes of more than 1% by weight, and domains whose size is less than 200 μm, with a local concentration of carbon nanotubes of less than 1% by weight.

[0030] For some embodiments, it is preferred that the size of the domains with a local concentration of carbon nanotubes of less than 1% by weight be less than 100 μm.

[0031] The bipolar plate obtained by the method of the present invention can be thinner than the bipolar plates known in the prior art, which leads to a significant reduction in the weight of the bipolar fuel cell battery. The lower density of the composite material also helps to reduce the weight of the bipolar battery. A bipolar plate about 2 mm thick can be obtained by numerous methods known in the prior art, including those described above. The advantage of the present invention becomes obvious for a bipolar plate less than 1 mm thick: thinner plates have less weight and a lower drop in electrical resistance across it. For some embodiments, it is preferable that the bipolar plate thickness is less than 0.5 mm. For other embodiments, it is most preferable that the bipolar plate thickness is less than 0.2 mm.

[0032] As shown by the examples below, the thin plates obtained by this method have a bulk electrical conductivity of more than 2 S / cm, and some have a bulk electrical conductivity of more than 10 S / cm. The high electrical conductivity results in a lower surface electrical resistance of the bipolar plate. It is preferable that the bipolar plate have a surface electrical resistance of 10 ohms / square or less. It is most preferable that the bipolar plate have a surface electrical resistance of 1 ohm / square or less.

[0033] The composite material of the bipolar plate, especially for a thin bipolar plate, must have high mechanical strength to withstand the stresses that occur during fuel cell operation. It is important that the material has a bending strength of more than 60 MPa. Preferably, the bipolar plate has a bending modulus of 5 GPa or more at 25 °C.

[0034] Additional features and advantages of the present invention are set forth in the detailed description of embodiments of the invention that follows.

[0035] It should be understood that the foregoing general description of the invention and the following description of embodiments of the invention are exemplary and are intended to further disclose the invention as claimed.

[0036] Brief description of the drawings.

[0037] FIG. 1. Transmission electron microscopy of single-walled carbon nanotubes used to produce thin bipolar plates in Examples 1-4.

[0038] FIG 2. Optical micrographs of core-shell particles with a polyphenylene sulfide (PPS) core coated with a single-wall carbon nanotube shell and obtained in step (1) in Example 1. The horizontal size of the image is 300 μm. FIG 3. Size distribution (μm) of core-shell particles with a polyphenylene sulfide (PPS) core coated with a single-wall carbon nanotube shell and obtained in step (1) in Example 1.

[0039] FIG. 4. Optical micrograph of a 0.2 mm thick bipolar plate obtained in reflective mode for Example 1. The horizontal dimension of the image is 1 mm. The central groove is intentionally produced with a copper wire of ~85 μm diameter, to illustrate the ability to produce very fine details in the sample.

[0040] FIG. 5. Optical micrograph of a 0.2 mm thick bipolar plate in reflective mode with polarizers for Example 1. The horizontal size of the image is 600 µm.

[0041] FIG. 6. Bending strength of the bipolar plate (MPa, squares, left axis) and specific volume conductivity (S / cm, circles, right axis) depending on the mass fraction of single-walled carbon nanotubes in the composite material of the plate at a temperature of 25 °C, for Examples 1-4. Filled marks for Examples 1-3 and empty marks for Example 4, where doped carbon nanotubes were used.

[0042] FIG 7. Dependence of the ultimate bending strength (MPa) on the temperature (°C) for bipolar plates with a thickness of 0.2 mm for Example 1 (squares) and Example 2 (circles).

[0043] FIG. 8. Transmission electron microscopy images of the mixture of single-walled and double-walled carbon nanotubes used to produce thin bipolar plates in Example 5.

[0044] FIG 9. Specific volume conductivity (S / cm) of the bipolar plate according to Examples 1-3 (empty squares) and Examples 6-7 (filled diamonds) depending on the mass fraction of single-wall carbon nanotubes in the composite material of the plate.

[0045] Table 1. Mechanical and electrically conductive properties of thin plates with a thickness of 0.2 mm according to Examples 1-5. PPS - polyphenylene sulfide, SWCNT - single-wall carbon nanotubes, DWCNT - double-wall carbon nanotubes, R s - surface electrical resistance (Ohm / square), sc - specific volume conductivity, S / cm. Table 2. Mechanical and electrically conductive properties of thin plates according to examples 8-13. PSU - polysulfone, PPSU - polyphenylene sulfone, PEEK - polyetheretherketone, o v - specific volume conductivity, S / cm.

[0046]

[0047]

[0048] Embodiments of the invention.

[0049] The following describes in detail preferred embodiments of the present invention, examples of which are illustrated in the accompanying drawings.

[0050] Transmission electron microscopy studies were performed using a JEM-2010 (JEOL). Optical micrographs were taken using a Leica DM 2700 P microscope. Particle size distributions were obtained in aqueous dispersion using a Malvern Mastersizer 3000. The bulk conductivity of the plate (sc) was calculated from the bipolar plate resistivity (Rs) as

[0051] Cv = l / (R s d), where d is the thickness of the plate. The surface electrical resistance of the bipolar plate (R s) was measured using the inductive method on EddyCus® TF lab 2020 Series devices from Suragus. Flexural strength and flexural modulus measurements were performed on dried specimens using a Shimadzu AGS-5-20KNXD universal testing machine with a 20 kN load cell according to ASTM D790. The strength and flexural modulus values ​​were averaged over 3 specimens.

[0052] For convenience, information on the thin plates given in the examples is also given in Tables 1 and 2.

[0053] Example 1.

[0054] A thin plate with a thickness of 0.2 mm was prepared as follows: 8.5 g of polyphenylene sulfide (PPS) powder, a polymer with a glass transition temperature of T g= 115 °C and 1.5 g of single-wall carbon nanotubes (OCSiAl, Tuball™) with a diameter of 1.6 ± 0.2 nm and a length of more than 5 μm were mixed in a grinding mixer LM-201 (OOO Plaun, Russia) for 30 seconds at room temperature. Transmission electron microscopy images of the used single-wall carbon nanotubes are shown in FIG. 1. The resulting mixture consists of particles with a polymer core covered with a shell of single-wall carbon nanotubes. A micrograph of the resulting powder is shown in FIG.

[0055] The particle size distribution of the powder of the mixture of thermoplastic polymer and single-wall carbon nanotubes was determined in aqueous dispersion using a Malvern Mastersizer 3000. The distribution is shown in FIG. 3. The D10 of the powder was 12.5 μm, the D50 of the powder was 72 μm, and the D90 of the powder was 145 μm. That is, 90% by weight of the powder has a size greater than 12.5 μm and more than 90% by weight of the powder has a size less than 145 μm.

[0056] The resulting black mixture with a mass ratio of single-wall carbon nanotubes to polymer content equal to 0.176 (or 15 mass %) was placed in a compression mold defining the desired shape of a bipolar plate, 0.2 mm deep, and compression molding was performed at a temperature of 290 °C under a pressure of 10 MPa for 30 seconds. Optical micrographs of the resulting bipolar plate are shown in FIG.

[0057] FIG. 5 is a photograph showing the non-uniform distribution of single-wall carbon nanotubes in a polyphenylene sulfide / single-wall carbon nanotube bipolar plate composite material.

[0058] Connected regions with a high content of single-wall carbon nanotubes appear dark, and domains with a low content of single-wall carbon nanotubes appear as lighter areas. The concentration of single-wall carbon nanotubes can be estimated from the degree of darkness of the region by comparison with reference samples of well-homogenized polyphenylene sulfide / single-wall carbon nanotube mixtures with a known concentration of single-wall carbon nanotubes. The concentration of single-wall carbon nanotubes in the light domains is less than 1 wt.%, in the lightest regions - less than 0.1 wt.%. Domains with a content of single-wall and / or double-wall carbon nanotubes less than 1 wt.% are limited to a size of 200 μm or less.

[0059] The surface electrical resistance of the 0.2 mm thick bipolar plate was 1.43 Ohm / square, which corresponds to a specific volume conductivity of 35 S / cm. The measured bending strength was 112 MPa. The obtained mechanical and electrical conductive properties of the bipolar plate are shown in Table 1 and in FIG. 6 (filled marks for the mass fraction of SWCNT = 0.15). The temperature dependence of the bending strength of the bipolar plate is shown in FIG. 7 (square marks).

[0060] The bipolar plate can be made in different thicknesses by varying the depth of the mold or the thickness of the insert in the mold. According to the method of the present invention, bipolar plates with a thickness of several mm to less than 0.1 mm can be made.

[0061] Example 2.

[0062] A thin plate with a thickness of 0.2 mm was prepared similarly to Example 1, but using 9.0 g of polyphenylene sulfide (PPS) powder and 1.0 g of single-wall carbon nanotubes. The mass ratio of the content of single-wall carbon nanotubes to the content of polymer in the mixture prepared in step (1) was 1:9 = 0.11. The particle size distribution of the powder of the mixture of thermoplastic polymer and single-wall carbon nanotubes, determined in an aqueous dispersion using a Malvern Mastersizer 3000, is characterized by D10 of the powder was 12 μm, D50 of the powder was 67 μm, D90 of the powder was 135 μm.

[0063] The surface electrical resistance of the 0.2 mm thick bipolar plate was 3.1 Ohm / square, which corresponds to a bulk conductivity of 16 S / cm. The measured flexural strength was 80 MPa. The obtained mechanical and electrical conductive properties of the bipolar plate are shown in Table 1 and in FIG. 6 (labels for the mass fraction of SWCNT = 0.1). The temperature dependence of the flexural strength of the bipolar plate is shown in FIG. 7 (round labels).

[0064] Example 3.

[0065] A thin bipolar plate with a thickness of 0.2 mm was prepared similarly to Example 1, but using 9.5 g of polyphenylene sulfide (PPS) powder and 0.5 g of single-wall carbon nanotubes. The mass ratio of the content of single-wall carbon nanotubes to the content of polymer in the mixture prepared in step (1) was 0.053. The particle size distribution of the powder mixture was characterized by the values ​​of D10 of the powder of 11 μm, D50 of the powder of 64 μm, and D90 of the powder of 130 μm. The surface electrical resistance of the bipolar plate with a thickness of 0.2 mm was 15.2 Ohm / square, which corresponds to a specific volume conductivity of 3.3 S / cm. The measured bending strength was 60 MPa. The obtained mechanical and electrical conductive properties of the bipolar plate are shown in Table 1 and in FIG. 6. (labels for the mass fraction of SWCNT = 0.05).

[0066] Example 4. A thin bipolar plate with a thickness of 0.2 mm was prepared similarly to Example 1, but using chemically treated (copied) single-wall carbon nanotubes. Single-wall carbon nanotubes (OCSiAl, Tuball™) were mixed with an aqueous solution of a dopant (H3PO4), kept in the solution for 1 day, the water was evaporated and dried. The mass ratio of the dopant content to the single-wall carbon nanotube content in the doped nanotubes was 1:4. The mixing stage was carried out using 8.13 g of polyphenylene sulfide powder and 1.87 g of single-wall carbon nanotubes doped with H3PO4. The mass ratio of the doped single-wall carbon nanotube content to the polymer content in the mixture prepared in stage (1) was 0.185 (15 wt. % SWCNT).The use of doped single-wall carbon nanotubes made it possible to further reduce the surface electrical resistance of the 0.2 mm thick bipolar plate to 0.49 Ohm / square and increase the specific volume conductivity to 103 S / cm, which is almost three times higher than that of the plate with 15 wt. % undoped single-wall carbon nanotubes (Example 1). The use of doped single-wall carbon nanotubes also led to a decrease in the bending strength to 80 MPa, which is still a very high value. The resulting mechanical and electrically conductive properties of the bipolar plate are shown in Table 1 and in FIG. 6 (empty dots).

[0067] Example 5.

[0068] A thin bipolar plate with a thickness of 0.2 mm was manufactured similarly to Example 1, but using a mixture of single-wall and double-wall carbon nanotubes. The powder of single-wall and double-wall carbon nanotubes used contained 9.8 wt. % of metallic iron nanoparticles coated with graphite shells (impurity), which is due to the method of obtaining carbon nanotubes. Transmission electron micrographs of a mixture of single-wall and double-wall carbon nanotubes are shown in FIG. 8. The amount of double-wall carbon nanotubes is about 80 wt. % of the total mass of carbon nanotubes.

[0069] The mixture is characterized by a mass ratio of single-wall and double-wall carbon nanotubes to the polymer content equal to 0.176. The particle size distribution of the powder mixture is characterized by the values ​​of D10 powder 16 μm, D50 powder 90 μm and D90 powder 160 μm. The resulting mixture was placed in a compression mold defining the desired shape of a bipolar plate, 0.2 mm deep, and compression molding was performed at a temperature of 290 °C under a pressure of 10 MPa for 30 seconds.

[0070] The surface electrical resistance of the obtained bipolar plate with a thickness of 0.2 mm was 2.3 Ohm / square, which corresponds to a bulk conductivity of 22 S / cm. The measured bending strength was 103 MPa. The elastic modulus in transverse bending was 8.5 MPa. The obtained mechanical and electrically conductive properties of the bipolar plate are shown in Table 1. The surface electrical resistance and bending strength of the bipolar plate prepared using a mixture of single-wall and double-wall carbon nanotubes are close to the values ​​obtained for the thin bipolar plate in Example 1 (with single-wall carbon nanotubes only).

[0071] Example 6.

[0072] A thin bipolar plate of 0.2 mm thickness was prepared similarly to Example 1, but using 9.0 g of polyvinylidene fluoride powder (PVDF, Solef 5130 from Solvay) and 1.0 g of single-wall carbon nanotubes (OCSiAl, Tuball™). The mixture obtained after step (1) (black powder) contained particles with a PVDF core and a single-wall carbon nanotube shell, the mass ratio of the content of single-wall carbon nanotubes to the content of PVDF was 0.11.

[0073] The particle size distribution of the mixture was determined in aqueous dispersion using a Malvern Mastersizer 3000. The D10 of the mixture was 14 µm, the D50 of the mixture was 70 µm, and the D90 of this powder was 155 µm.

[0074] The mixture of polymer and single-wall carbon nanotubes obtained in step (1) was placed in a mold defining the desired shape of a bipolar plate, 0.2 mm deep, and compression molding was performed at a temperature of 230 °C under a pressure of 10 MPa for 30 seconds. Using the molds, plates with different thicknesses were obtained, from several mm to less than 0.1 mm.

[0075] The surface electrical resistance of the 0.2 mm thick bipolar plate was 3.3 Ohm / square, which corresponds to a specific volume conductivity of 15 S / cm. The resulting conductive properties of the bipolar plate are shown in FIG. 9. Example 7.

[0076] A thin bipolar plate of 0.2 mm thickness was prepared similarly to Example 6, however, the mass ratio of the content of single-walled carbon nanotubes to the content of polymer in the mixture was 0.25. The particle size distribution of the mixture was determined in an aqueous dispersion using a Malvern Mastersizer 3000. D10 of the mixture was 17 μm, D50 of the mixture was 70 μm, and D90 of this powder was 140 μm.

[0077] The surface electrical resistance of the 0.2 mm thick bipolar plate was 0.83 Ohm / square, which corresponds to a specific volume conductivity of 60 S / cm. The resulting conductive properties of the bipolar plate are shown in FIG. 9.

[0078] Example 8.

[0079] A thin bipolar plate was prepared as follows: 15 g of polysulfone (PSU, Udel® P-3500 LCD MVZ, T g = 185 °C, T m= 330 °C) was ground into powder in a grinding mixer LM-201 (OOO Plaun, Russia) for 60 seconds, the fraction 14 - 200 μm was screened; 1.5 g of single-wall carbon nanotubes were then added to 10 g of the PSU fraction and mixed in LM-201 for 30 seconds at room temperature. The particle size distribution of the powder of the resulting mixture is characterized by the values ​​of D10 powder 11 μm, D50 powder 85 μm and D90 powder 190 μm. The obtained black mixture with a mass ratio of single-wall carbon nanotubes to polymer content equal to 0.15 (13 mass % of single-wall carbon nanotubes) was placed in a mold defining the desired shape of a bipolar plate, 0.18 mm deep, and compression molding was performed at a temperature of 340 °C under a pressure of 10 MPa for 30 seconds (IMC-1811 machine, from ImoNet). The obtained mechanical and electrically conductive properties of the bipolar plate are presented in Table 2.

[0080] Example 9.

[0081] A thin bipolar plate was made similar to Example 8, but the mass ratio of the single-wall carbon nanotube content to the polymer content was 0.075. The bipolar plate was produced by hot pressing using a 0.12 mm deep mold. The resulting mechanical and electrically conductive properties of the bipolar plate are presented in Table 2. Example 10.

[0082] A thin bipolar plate was prepared as follows: 15 g of polyphenylene sulfone (PPSU, Radel® R-5800, T g = 220 °C, T m= 370 °C) were ground into powder in a grinding mixer LM-201 (OOO Plaun, Russia) for 60 seconds, the fraction 14 - 200 μm was screened; 1.7 g of single-wall carbon nanotubes were added to 7.3 g of the PPSU fraction and mixed in the LM-201 for 30 seconds at room temperature. The particle size distribution of the powder of the resulting mixture is characterized by the values ​​of D10 powder 13 μm, D50 powder 80 μm and D90 powder 180 μm. The obtained black mixture with a mass ratio of single-wall carbon nanotubes to polymer content equal to 0.205 (17 mass % of single-wall carbon nanotubes) was placed in a mold defining the desired shape of a bipolar plate, with a depth of 0.2 to 5 mm, and compression molding was performed at a temperature of 380 °C under a pressure of 10 MPa for 30 seconds (IMC-1811 machine, from ImoNet). The obtained mechanical and electrically conductive properties of the bipolar plate are presented in Table 2.

[0083] Example 11.

[0084] A thin bipolar plate was fabricated similarly to Example 10, but the mass ratio of single-wall carbon nanotubes to polyphenylene sulfone (PPSU) polymer was 0.28. The bipolar plate was produced by hot pressing using a 0.11 mm deep mold. The mechanical and electrical conductivity properties of the bipolar plate are presented in Table 2.

[0085] Example 12.

[0086] A thin bipolar plate was prepared as follows: 15 g of polyetheretherketone (PEEK, VESTAKEEP 2000 FP, T g = 143 °C, T m= 343 °C) was ground into powder in a grinding mixer LM-201 (OOO Plaun, Russia) for 60 seconds, the fraction of 14 - 200 μm was screened; 1.5 g of single-wall carbon nanotubes were then added to 8.5 g of the PEEK fraction and mixed in the LM-201 for 30 seconds at room temperature. The obtained black mixture with a mass ratio of single-wall carbon nanotubes to PEEK content equal to 0.165 (15 mass % of single-wall carbon nanotubes) was placed in a press mold defining the desired shape of a bipolar plate, 0.3 mm thick, and compression molding was performed at a temperature of 345 °C under a pressure of 10 MPa for 30 seconds (IMC-1811 machine, from ImoNet). The obtained mechanical and electrically conductive properties of the bipolar plate are presented in Table 2.

[0087] Example 13.

[0088] A thin bipolar plate was made similarly to Example 12, but the mass ratio of the content of single-wall carbon nanotubes to the content of PEEK polymer was 0.30. The bipolar plate was obtained by hot pressing using a mold with a depth of 0.18 mm. The obtained mechanical and electrically conductive properties of the bipolar plate are presented in Table 2.

[0089] Industrial applicability.

[0090] The present invention relates to electrically conductive composite materials based on thermoplastic polymers containing single-walled and / or double-walled carbon nanotubes and methods for producing them. The invention also relates to electrically conductive thin plates used as bipolar plates in fuel cells, including those with proton exchange membranes.

[0091] Patent literature.

[0092] Patent literature 1: US7056452B2, 09.06.2004, IPC: HO 1 B 1 / 24, C08J3 / 21, C08K7 / 24.

[0093] Patent Literature 2: US7629070B2, dated 09 / 22 / 2003, MPC: H01M8 / 02, H01B1 / 24.

[0094] Non-patent literature.

[0095] T.M. Besmann, JW Klett, JJ Henry, E. Lara-Curzio, Carbon / Carbon Composite Bipolar Plate for Proton Exchange Membrane Fuel Cells, J. Electrochem. Soc. (2000) Vol. 147, p. 4083- 4086.

Claims

23 Invention formula 1. A method for producing a thin conductive plate, comprising the steps of: (1) mixing powder of single-walled and / or double-walled carbon nanotubes and powder of a thermoplastic polymer at a temperature not exceeding the glass transition temperature of the thermoplastic polymer (T g ) to obtain a mixture, the particles of which consist of a thermoplastic polymer core and a carbon nanotube shell; and (2) compression molding the mixture obtained in step (1) at a temperature exceeding the glass transition temperature of the thermoplastic polymer (T g ) by at least 100 K to obtain a thin plate of a given shape.

2. The method according to claim 1, characterized in that 90% of the mass of the particles of the mixture have a size greater than 10 μm.

3. The method according to claim 1, characterized in that the thermoplastic polymer powder is selected from a series of thermally stable polymers: polyvinylidene fluoride, polyphenylene sulfide, polyethersulfone, polysulfone, polyphenylene sulfone or polyetheretherketone or their copolymers or their derivatives.

4. The method according to claim 1, characterized in that the temperature of mixing the powder of single-wall and / or double-wall carbon nanotubes and the powder of the thermoplastic polymer does not exceed the Vogel temperature of the thermoplastic polymer.

5. The method according to claim 1, characterized in that the compression molding temperature exceeds the glass transition temperature of the thermoplastic polymer (T g ) by at least 150 K.

6. The method according to claim 1, characterized in that the compression molding temperature exceeds the melting temperature of the thermoplastic polymer (T т ).

7. The method according to claim 1, characterized in that the compression molding is performed in an inert gas atmosphere.

8. The method according to claim 1, characterized in that the mass ratio of the content of carbon nanotubes to the content of thermoplastic polymer in the mixture is from 0.01 to 0.

3.

9. The method according to claim 1, characterized in that the mass ratio of the content of carbon nanotubes to the content of thermoplastic polymer in the mixture is from 0.05 to 0.

25.

10. A thin bipolar plate for a high-temperature fuel cell with a thickness of less than 1 mm, having gas transport channels on the surface and containing a composite material made of a thermoplastic polymer and single-wall and / or double-wall carbon nanotubes, characterized in that the composite material contains connected regions with a concentration of carbon nanotubes of more than 1% by weight, and domains whose size is less than 200 μm, with a local concentration of carbon nanotubes of less than 1% by weight.

11. A bipolar plate according to claim 10, characterized in that the domains with a local concentration of carbon nanotubes of less than 1% by weight have a size of less than 100 µm.

12. A bipolar plate according to claim 10, characterized in that the plate has a thickness of less than 0.2 mm.

13. A bipolar plate according to claim 10, characterized in that its surface electrical resistance is 10 ohms / square or less.

14. The bipolar plate of claim 10, wherein its surface electrical resistance is 1 ohm / square or less.

15. The bipolar plate of claim 10, wherein the flexural modulus of elasticity is 5 GPa or more at 25 °C.

Citation Information

Patent Citations

  • Polyvinylidene fluoride composites and methods for preparing same

    US7056452B2

  • Production method of carbon-based composite molded bipolar plate

    CN115332484A

  • Preparing method of polymer hybrid composite forbipolar plate of fuel cell and resin composition forbipolar plate

    KR100764008B1

  • Bipolar plate for PEM fuel cells

    US7629070B2