Method for producing fiber article
The method enhances the strength and compactness of textile articles by forming secondary fibers within the composite, addressing the challenge of uniform filter performance and fiber diameter disparities, resulting in improved filter efficiency and reduced weight.
Patent Information
- Application Number
- PCT/JP2023/017155
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-07
AI Technical Summary
Existing textile articles used as filters in air conditioners face challenges in achieving optimal strength and compactness while maintaining uniform filter performance, particularly when incorporating fibers with smaller outer diameters.
A method involving the impregnation of resin granules and a position stabilizing agent onto fibers, followed by application of external forces to reduce fiber gaps and form thinner secondary fibers, resulting in a fiber composite with enhanced strength and compactness.
The method improves the strength and compactness of textile articles, ensuring uniform filter performance by dispersing secondary fibers throughout the article, thereby enhancing the expression of each fiber's function and reducing production costs.
Smart Images

Figure JP2023017155_07112024_PF_FP_ABST
Abstract
Description
Method for manufacturing textile articles
[0001] The present disclosure relates to a method for manufacturing a textile article.
[0002] In this document, the following defined terms are used: TD: Total denier, which refers to the fiber density (grams per 9000 m) of the tow band or multiple filaments in a bundle.
[0003] FD: Filament denier, which refers to the fiber density (grams per 9000 m) of a single fiber (one fiber). Also called single fiber denier.
[0004] Tow band: A yarn, which is an aggregate of filaments (single fibers) discharged from each spinneret of a plurality of spinning tubes, is combined, and a plurality of yarns are combined and the TD is set to a predetermined value to form an end. This end is crimped. This crimped end (aggregate of filaments) is called a tow band. That is, the tow band has a TD and a crimp number.
[0005] As a fiber article used for applications such as air conditioner filters, for example, as disclosed in Patent Document 1, a method for manufacturing a fiber article including first fibers and second fibers having an outer diameter smaller than that of the first fibers is known.
[0006] International Publication No. 2021 / 039980
[0007] In the fiber article described in Patent Document 1, the second fibers are supported by the first fibers, and the functions of the first fibers and the second fibers are exerted, thereby improving the performance of the fiber article. Here, it would be more preferable if the fiber article could be manufactured so that the strength of the fiber article could be improved and the fiber article could be made more compact.
[0008] Therefore, the present disclosure aims to improve the strength and compactness of a fibrous article when manufacturing the fibrous article including a first fiber and a second fiber having an outer diameter smaller than that of the first fiber, while also achieving uniform filtering performance of the fibrous article.
[0009] In order to solve the above problem, a method for manufacturing a fiber article according to one embodiment of the present disclosure includes a first step of applying an application liquid containing a plurality of resin granules containing a polymer capable of being fiberized and a position stabilizer that stabilizes the positions of the plurality of resin granules relative to the plurality of first fibers to a fiber sheet that includes a plurality of first fibers and is transported in a predetermined transport direction, and then drying the application liquid; a second step of applying a first external force to the transported fiber sheet after the first step so as to reduce the fiber gaps between the first fibers; and a third step of forming a fiber composite containing the plurality of first fibers and the plurality of second fibers from the plurality of resin granules that have been applied to the plurality of first fibers by relaxing the first external force applied to the fiber sheet after the second step.
[0010] According to one aspect of the present disclosure, when manufacturing a fiber article including a first fiber and a second fiber having an outer diameter smaller than that of the first fiber, the strength and compactness of the fiber article can be improved, and uniform filtering performance of the fiber article can be obtained.
[0011] Fig. 1 is a schematic diagram of a fibrous sheet manufacturing apparatus according to an embodiment. Fig. 2 is a schematic diagram of a fibrous article manufacturing apparatus according to an embodiment. Fig. 3 is an enlarged photograph of the surface of a fibrous sheet according to Comparative Example 1 after the application of the adhering liquid and before the application of a first external force. Fig. 4 is an enlarged photograph of the interior of a fibrous sheet according to Comparative Example 1 after the application of the adhering liquid and before the application of a first external force. Fig. 5 is an enlarged photograph of the surface of a fibrous sheet according to Example 1 after the application of the adhering liquid and before the application of a first external force. Fig. 6 is an enlarged photograph of the interior of a fibrous sheet according to Example 1 after the application of the adhering liquid and before the application of a first external force.
[0012] An embodiment of the present disclosure will be described below with reference to the drawings. (Embodiment) A method for manufacturing a fiber article according to this embodiment includes the following first to third steps. In the first step, a fiber sheet containing a plurality of first fibers and transported in a predetermined transport direction is impregnated with an impregnation liquid containing a plurality of resin granules containing a fiberizable polymer and a position-stabilizing agent for stabilizing the positions of the resin granules relative to the plurality of first fibers, and then dried. In the second step, the impregnation liquid is dried, and a first external force is applied to the plurality of first fibers and the plurality of resin granules impregnated with the plurality of first fibers of the fiber sheet being transported, so as to reduce the inter-fiber spaces between the first fibers. In the third step, the first external force applied to the fiber sheet is relaxed, thereby forming a plurality of second fibers thinner than the first fibers from the plurality of resin granules, thereby forming a fiber composite containing the plurality of first fibers and the plurality of second fibers. In the first step of this embodiment, a nonwoven fabric is used as the fiber sheet. In this embodiment, in addition to the manufacturing method, a fiber sheet manufacturing apparatus 1 and a fiber article manufacturing apparatus 2 used in the manufacturing method will also be described.
[0013] [Fiber Sheet Manufacturing Apparatus] FIG. 1 is a schematic diagram of a fiber sheet manufacturing apparatus 1 (hereinafter also referred to as manufacturing apparatus 1) according to an embodiment. As shown in FIG. 1 , a packaging box B containing a bale-shaped raw web 50 folded and compressed and packed is supplied to the manufacturing apparatus 1. The raw web 50 includes first fibers 51, which are a plurality of long fibers. The manufacturing apparatus 1 continuously pays out the raw web 50 from the packaging box B. The manufacturing apparatus 1 manufactures a fiber sheet 60 from a plurality of short fibers 52 formed from the plurality of first fibers 51. The manufacturing apparatus 1 of this embodiment also functions as a nonwoven fabric manufacturing apparatus. The fiber sheet 60 of this embodiment is a nonwoven fabric. The term "nonwoven fabric" used herein refers to a nonwoven fabric conforming to JIS L 0222:2001. As an example, in this embodiment, the fiber sheet 60, which is a nonwoven fabric, is manufactured using a needle punching method. The method for manufacturing the nonwoven fabric is not limited to the needle punching method and may be other known methods such as a spunlace method. The fiber sheet 60 is transported in a predetermined transport direction P. The fiber sheet 60 is long, with the transport direction P as its longitudinal direction and a direction perpendicular to the thickness direction and orthogonal to the transport direction P as its width direction. The transport direction P is also referred to as the MD direction. The direction orthogonal to the transport direction P is also referred to as the TD direction.
[0014] The material of the first fibers 51 can be selected appropriately. For example, the first fibers 51 include at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate. For example, the first fibers 51 are crimped. This provides the raw web 50 with stretchability. The raw web 50 immediately after being unwound from the packaging box B has multiple first fibers 51 entangled. The raw web 50 of this embodiment is a tow band containing crimped cellulose acetate fibers (hereinafter also referred to as CA fibers) as the first fibers 51. For example, the CA fibers are spun by a dry spinning method. The spinning method is not limited to the dry spinning method. The CA fibers are crimped by a primary crimp, which is the smallest crimp unit, and by a secondary crimp, which is a crimp unit larger than the primary crimp. The CA fibers may be further crimped by a higher-order crimp, which is a crimp unit larger than the secondary crimp. The cross-sectional shape of the first fibers 51 can be appropriately set. For example, the cross-sectional shape of the first fibers 51 can be set to any of a circular shape, a Y-shape, and an irregular shape.
[0015] The TD and FD of the raw web 50 can be set as appropriate. As an example, the TD of the raw web 50 is a value in the millions, hundreds of thousands, tens of thousands, or thousands. In another example, the TD of the raw web 50 is preferably a value in the range of 3 million to 5 million, and more preferably a value in the range of 1 million to 2 million. In yet another example, the TD of the raw web 50 is preferably a value in the range of 100,000 to 700,000, and more preferably a value in the range of 100,000 to 300,000. In yet another example, the TD of the raw web 50 is preferably a value in the range of 5,000 to 100,000, and more preferably a value in the range of 10,000 to 50,000.
[0016] As an example, the FD of the raw web 50 is a value in the range of not more than 20. As another example, the FD of the raw web 50 is preferably a value in the range of 1 to 15, more preferably a value in the range of 1 to 10, and even more preferably a value in the range of 1 to 8. When the manufacturing apparatus 1 of this embodiment is driven, the raw web 50 is conveyed in the predetermined conveying direction P while being subjected to a relatively weak tension (load) in the range of 2 mgf to 50 mgf per denier.
[0017] As a specific example, the manufacturing apparatus 1 includes a feed roll pair 3 that guides the raw web 50 unwound from the packaging box B, multiple guide members G1 to G3, and a cutter 10 that forms multiple short fibers 52 from the multiple first fibers 51 of the raw web 50. The feed roll pair 3 includes a pair of feed rolls 4 and 5. The guide members G1 to G3 include, for example, multiple guide rolls. The manufacturing apparatus 1 also includes a conveying device 11 that conveys the multiple short fibers 52 discharged from the cutter 10, and a packaging device 12 that compresses and packages the multiple short fibers 52 conveyed by the conveying device 11. The packaging device 12 forms a fiber block 53 in which the multiple short fibers 52 are compressed and packaged into a predetermined shape. The fiber block 53 is used in the next process. The feed roll pair 3 is not essential and may be omitted.
[0018] The manufacturing apparatus 1 also includes a blowing machine 13 that removes impurities from the fiber block 53 and arranges the plurality of staple fibers 52, a blower BL that transports the plurality of staple fibers 52 that have passed through the blowing machine 13 in the transport direction P, a weighing feeder 14 that weighs the plurality of staple fibers 52 transported by the blower BL and supplies them in predetermined amounts to a carding machine 15, and at least one carding machine 15 that card the plurality of staple fibers 52. The carding machine 15 forms a nonwoven fabric intermediate 54 containing the plurality of staple fibers 52.
[0019] The length of the staple fibers 52 can be set as appropriate. For example, the length of the staple fibers 52 is a value in the range of 10 mm to 100 mm. In another example, the length of the staple fibers 52 is a value in the range of 30 mm to 100 mm. For example, when the length of the staple fibers 52 is 100 mm or less, unnecessary entanglement of the staple fibers 52 with respect to the carding machine 15 can be suppressed. Furthermore, when the length of the staple fibers 52 is 10 mm or more, crimped staple fibers 52 can be easily entangled with one another. This results in a fiber sheet 60 that is a bulky nonwoven fabric with abundant inter-fiber gaps. Furthermore, a fiber article 62 (see FIG. 2 ) with a reduced fiber density can be obtained compared to when a plurality of uncrimped staple fibers are used.
[0020] The manufacturing apparatus 1 also includes an entanglement machine 19 that entangles the plurality of short fibers 52 in the nonwoven fabric intermediate 54 discharged from the carding machine 15 to form a fiber sheet 60 that is a nonwoven fabric, a dryer 20 that dries the fiber sheet 60 discharged from the entanglement machine 19, and a winder 21 that winds up the fiber sheet 60 that has passed through the dryer 20. The entanglement machine 19 has, as an example, a plurality of needles that entangle the plurality of short fibers 52 in the nonwoven fabric intermediate 54 by reciprocating in a predetermined direction.
[0021] The manufacturing apparatus 1 also includes a supply device 18. The supply device 18 supplies a second intermediate 59, which is a nonwoven fabric intermediate containing a plurality of fibers, to a first intermediate 56, which is a nonwoven fabric intermediate 54 discharged from the carding machine 15. The second intermediate 59 contains short fibers 52 or fibers different from the short fibers 52. As an example, the second intermediate 59 contains pulp fibers or synthetic fibers. The second intermediate 59 is unwound from a supply roll R1 provided in the supply device 18 and arranged so as to be overlapped on the first intermediate 56. The intermediates 56 and 59 are transported in an overlapped state and introduced into the entanglement machine 19. The entanglement machine 19 entangles the plurality of fibers in the intermediates 56 and 59. As a result, a fiber sheet 60, which is a composite sheet and nonwoven fabric in which the intermediates 56 and 59 are arranged overlapping each other, is formed.
[0022] The fiber sheet 60 may include a plurality of first intermediates 56 and at least one second intermediate 59. In this case, the second intermediate 59 may be disposed between the plurality of first intermediates 56. The second intermediate 59 may be disposed on top of a laminate including the plurality of first intermediates 56. The plurality of first intermediates 56 and the at least one second intermediate 59 may be integrally entangled. The manufacturing apparatus 1 may also omit the supply device 18. In this case, the fiber sheet 60 is composed of only the first intermediates 56.
[0023] The fiber sheet 60 discharged from the interlacing machine 19 is dried by the dryer 20. The dried fiber sheet 60 is wound onto a winding roll R2 of a winding machine 21. The winding roll R2 is used in the next step.
[0024] [Textile article manufacturing apparatus] Fig. 2 is a schematic diagram of a fiber article manufacturing apparatus 2 (hereinafter also referred to as manufacturing apparatus 2) according to an embodiment. Fig. 2 also shows enlarged views of first fibers 51 (short fibers 52), resin granules 91, and second fibers 92 contained in a manufactured fiber composite 61 and a manufactured fiber article 62. A fiber sheet 60 containing a plurality of first fibers 51 (short fibers 52 in this case) is supplied to the manufacturing apparatus 2 from a winding roll R2.
[0025] As will be described in detail later, in the manufacturing apparatus 2 of this embodiment, a first external force is applied to a fiber sheet 60 having a plurality of resin granules 91 attached thereto and being transported, so as to reduce the interstices between the plurality of first fibers 51, and then the first external force is released, thereby forming second fibers 92 from the resin granules 91. Also, in this embodiment, as an example, a predetermined first external force and a predetermined second external force are applied to a fiber sheet 60 having a plurality of resin granules 91 attached thereto and being transported, thereby forming abundant second fibers 92 from the resin granules 91. In this way, a fiber composite 61 containing the first fibers 51 and the second fibers 92 is formed.
[0026] As a specific example, the manufacturing apparatus 2 includes a plurality of guide members G4 to G7 that guide the fiber sheet 60 in the conveying direction P, an applicator 25 that applies a predetermined applicator liquid 90 to the fiber sheet 60, and a dryer 26 that dries the fiber sheet 60 to which the applicator liquid 90 has been applied. As an example, the guide members G4 to G7 include a plurality of guide rolls. The applicator liquid 90 contains a plurality of resin granules 91 and a predetermined position stabilizer 93 that stabilizes the position of the resin granules 91 relative to the first fibers 51.
[0027] The manufacturing apparatus 2 also includes a pair of pressure rolls 27 that press the dried fiber sheet 60, and a stretching device 30 that stretches in a predetermined direction the plurality of first fibers 51 (short fibers 52) contained in the fiber sheet 60 that has passed through the pair of pressure rolls 27. The pair of pressure rolls 27 includes a pair of pressure rolls 28 and 29. The manufacturing apparatus 2 also includes a winder 31 that winds up the fiber composite 61 discharged from the stretching device 30.
[0028] As an example, the applicator 25 includes a storage section 32 that stores the impregnation liquid 90 and an impregnation roll 33 that applies the impregnation liquid 90 in the storage section 32 to the short fibers 52 (first fibers 51) of the fibrous sheet 60 via the peripheral surface thereof. The applicator 25 also includes a liquid collector 34 that collects the impregnation liquid 90 discharged from the storage section 32 and a pump 35 that circulates the collected impregnation liquid 90 back to the storage section 32. The configuration of the applicator 25 is not limited. For example, the applicator 25 may include one or more nozzles that spray the impregnation liquid 90 onto the fibrous sheet 60 and a housing that accommodates the nozzles. As an example, the impregnation liquid 90 is a water impregnation liquid. Using a water impregnation liquid allows the impregnation liquid 90 to be produced relatively inexpensively. Furthermore, the impregnation liquid 90 can be easily handled. The impregnation liquid 90 may contain a liquid other than water.
[0029] As an example, the resin granules 91 have a lamellar structure in which polymer chains are connected and folded. This lamellar structure is specifically composed of fine fibers formed by millions of polymer chains connected in a ribbon shape. These fine fibers are folded and housed inside the resin granules 91.
[0030] The resin granules 91 are primary particles. Secondary particles are formed when multiple resin granules 91 are bonded to each other. When an external force is applied to two bonded resin granules 91 in a direction that pulls them apart, fine fibers of the resin granules 91 are pulled outward, forming second fibers 92. When the impregnation liquid 90 is impregnated to the first fibers 51, multiple resin granules 91 are dispersed and impregnated on the surfaces of the multiple first fibers 51. As an example, multiple secondary particles of the resin granules 91 are impregnated on the surfaces of the first fibers 51.
[0031] The resin granules 91 may be, for example, any material that is produced by a polymerization reaction and contains a lamellar structure. For example, the resin granules 91 contain at least one of PTFE (polytetrafluoroethylene), polypropylene, polyethylene, and polyamide. The resin granules 91 of this embodiment contain PTFE.
[0032] The PTFE contained in the resin granules 91 is, for example, high-molecular-weight PTFE obtained by emulsion polymerization or suspension polymerization of TFE. The high-molecular-weight PTFE may be at least one of modified PTFE and homo-PTFE. The modified PTFE includes, for example, TFE and a monomer other than TFE, such as a modified monomer. Generally, modified PTFE is uniformly modified with a modified monomer or modified at the initial or final stage of the polymerization reaction, but is not particularly limited thereto. The modified PTFE includes TFE units derived from TFE and modified monomer units derived from the modified monomer. The "modified monomer unit" referred to herein is a part of the molecular structure of modified PTFE, derived from the modified monomer. The modified monomer is not particularly limited as long as it can be copolymerized with TFE.
[0033] Furthermore, the "high molecular weight" of high molecular weight PTFE as used herein refers to a molecular weight that is easily fiberized during the production of the fiber article 62, that gives rise to long fibrils, that has a standard specific gravity (SSG) of 2.130 or more and 2.230 or less, and that does not substantially melt flow due to a high melt viscosity. For details about fiberizable PTFE, see, for example, International Publication No. 2013 / 157647.
[0034] The resin granules 91 have an average particle size, for example, set to a value in the range of 100 nm to 100 μm. For example, the average particle size is preferably set to a value in the range of 200 nm to 700 nm, and even more preferably to a value in the range of 250 nm to 400 nm. In this specification, the average particle size refers to the median diameter (cumulative 50% diameter (D50)) calculated from the measurement results using dynamic light scattering. For example, the resin granules 91 are molded by paste extrusion molding.
[0035] The position stabilizer 93 of this embodiment is attached to the plurality of first fibers 51 together with the plurality of resin granules 91, thereby maintaining the relative position of each resin granule 91 with respect to the plurality of first fibers 51. Therefore, the resin granules 91 attached to the plurality of first fibers 51 are restricted from unnecessary relative movement with respect to the first fibers 51 during the manufacturing process. Therefore, the relative position of each resin granule 91 with respect to the plurality of first fibers 51 can be well maintained.
[0036] The positional stabilizer 93 is dispersed in the impregnating liquid 90 together with the plurality of resin particles 91. The positional stabilizer 93 is impregnated onto the entire surfaces of the plurality of first fibers 51 together with the plurality of resin particles 91. In other words, the entire surfaces of the first fibers 51 are coated with the positional stabilizer 93. For example, the positional stabilizer 93 impregnated onto the first fibers 51 hardens upon drying. As a result, the relative positions of the resin particles 91 with respect to the plurality of first fibers 51 are fixed. Furthermore, the plurality of first fibers 51 are reinforced by the positional stabilizer 93. In this embodiment, the positional stabilizer 93 contains at least one of carboxymethylcellulose sodium (CMC-Na) and hydroxyethylcellulose (HEC). As a result, the positional stabilizer 93 exhibits high affinity for the first fibers 51 when the first fibers 51 contain cellulose acetate.
[0037] The concentration of the positional stabilizer 93 in the impregnation liquid 90 can be appropriately set depending on, for example, the composition of the positional stabilizer 93 and its dispersibility in the solvent of the impregnation liquid 90. As an example, the positional stabilizer 93 remains in the fiber article 62. In this case, the concentration of the positional stabilizer 93 in the impregnation liquid 90 is adjusted, for example, so that the content of the positional stabilizer 93 in the fiber article 62 is in the range of 0.1 wt % to 3.0 wt %. The content is preferably, for example, in the range of 0.1 wt % to 1.0 wt %, more preferably in the range of 0.1 wt % to 0.7 wt %, and even more preferably in the range of 0.1 wt % to 0.5 wt %.
[0038] The bonding roll pair 27 applies a first external force to the plurality of first fibers 51 and the plurality of resin granules 91 in the fiber sheet 60 to which the plurality of resin granules 91 are attached and being conveyed, so as to reduce the interfiber gaps between the first fibers 51. The bonding roll pair 27 of this embodiment is, for example, a pair of thermocompression rolls that thermocompress the fiber sheet 60. The heating temperature at which the plurality of first fibers 51 and the plurality of resin granules 91 are heated by the thermocompression roll pair can be adjusted as appropriate. For example, the heating temperature can be set to a temperature in the range of more than 25°C and less than 200°C. The heating temperature is, for example, preferably in the range of 50°C to 200°C, more preferably in the range of 70°C to 200°C, and even more preferably in the range of 90°C to 200°C. In another example, the heating temperature is preferably in the range of 110°C to 200°C, and even more preferably in the range of 150°C to 200°C. This heating temperature may be, for example, lower than the melting point of each material of the first fibers 51 and the resin granules 91, or lower than the decomposition temperature of each material.
[0039] The stretching device 30 applies a second external force to the conveyed fiber sheet 60, after the first external force has been applied and the first external force is released, so as to expand the interfiber spaces between the first fibers 51 at least in the width direction W of the fiber sheet 60 (the direction perpendicular to the paper surface in FIG. 2 ). The stretching device 30 of this embodiment, for example, applies the second external force to the conveyed fiber sheet 60 in both the conveying direction P and the width direction W. For example, the stretching device 30 is a known simultaneous biaxial stretching device. For the configuration of a simultaneous biaxial stretching device, see, for example, Japanese Patent No. 4224241. The stretching device 30 is not limited to a simultaneous biaxial stretching device and may be a known sequential secondary stretching device. The stretching device 30 is not essential in this embodiment. Therefore, the stretching device 30 may be omitted. In this case, the second external force is not applied to the fiber sheet 60 in the third step. In this case, in the third step, the first external force applied to the fiber sheet 60 is relaxed, thereby expanding the fiber gaps between the first fibers 51 and forming multiple second fibers 92 from multiple resin granules 91.
[0040] When the manufacturing apparatus 2 is in operation, the fiber sheet 60 to which the impregnating liquid 90 has been applied by the applicator 25 is sent to the dryer 26. The solvent component of the impregnating liquid 90 applied to the fiber sheet 60 evaporates and the impregnating liquid 90 dries. As the impregnating liquid 90 dries, the fluidity of the impregnating liquid 90 disappears. As a result, the relative position of the plurality of resin granules 91 contained in the impregnating liquid 90 to the plurality of first fibers 51 becomes stable. The dried fiber sheet 60 is introduced into the pair of pressure rolls 27. When the fiber sheet 60 passes through the nip point of the pair of pressure rolls 27, a first external force is applied to the plurality of first fibers 51 and the plurality of resin granules 91 of the fiber sheet 60. In this embodiment, the plurality of first fibers 51 and the plurality of resin granules 91 are heated by the pair of pressure rolls 27 when the first external force is applied. The first fibers 51 are plasticized by being heated. As a result, the first external force tends to reduce the interfiber gaps. When the fiber sheet 60 passes through the nip point between the pair of pressure rolls 27, the first external force applied to the plurality of first fibers 51 and the plurality of resin granules 91 is alleviated.
[0041] The first external force may be applied to the plurality of first fibers 51 and the plurality of resin granules 91 by a configuration other than a pair of pressure rolls. Also, the first external force may be applied to the plurality of first fibers 51 and the plurality of resin granules 91 by a configuration other than a thermocompression roll. In this case, for example, the manufacturing apparatus 2 may be provided with a pair of pressure rolls that does not have a heating function.
[0042] The fiber sheet 60, from which the first external force has been relaxed, is introduced into the stretching device 30. In the stretching device 30, a second external force is applied to the fiber sheet 60 in the machine direction P and the width direction W so as to expand the inter-fiber spaces between the plurality of first fibers 51. At this time, the second external force is applied to the plurality of first fibers 51 and the plurality of resin granules 91 so as to separate the resin granules 91 that are adhered to each other between the plurality of first fibers 51. As a result, the fine fibers of the resin granules 91 are stretched outward, and second fibers 92 are formed so as to bridge different plurality of first fibers 51. As a result, a fiber composite 61 is formed that contains the plurality of first fibers 51 and the plurality of second fibers 92.
[0043] Here, if the resin granules 91 attached to the plurality of first fibers 51 are not sufficiently anchored to the first fibers 51, they may move relative to the first fibers 51. As a result, for example, even if the adhering liquid 90 is uniformly applied to the plurality of first fibers 51 of the fiber sheet 60, the resin granules 91 may be localized in a region such as the surface layer of the fiber sheet 60 relative to the first fibers 51. In this case, the plurality of second fibers 92 are formed so as to be biased toward the surface layer of the fiber article. As a result, the effect achieved by the second fibers 92 varies at different positions in the fiber article (for example, at different positions inside and on the surface layer of the fiber article).
[0044] In contrast, in the present embodiment, an impregnation liquid 90 containing a plurality of resin granules 91 and a positional stabilizer 93 is impregnated onto a plurality of first fibers 51. As a result, in the fiber sheet 60, the relative positions of the resin granules 91 with respect to the first fibers 51 at the time the impregnation liquid 90 is impregnated are maintained. Therefore, in the fiber sheet 60, the positional stabilizer 93 can maintain a state in which the plurality of resin granules 91 are dispersed and impregnated onto the plurality of first fibers 51. As a result, a plurality of second fibers 92 are formed throughout the fiber sheet 60 without being displaced. Therefore, the abundant second fibers 92 formed and dispersed within the fiber sheet 60 can improve strength and produce a fiber article 62 with uniform filter performance.
[0045] In addition, in the fiber sheet 60 of this embodiment, after the applied first external force is alleviated, the fiber gaps between the first fibers 51 in the thickness direction naturally expand due to a restoring force. This natural expansion due to the restoring force also allows the second fibers 92 to be formed throughout the entire fiber sheet 60 without being displaced.
[0046] In addition, in the fiber sheet 60 of this embodiment, as an example, the fiber gaps between the multiple first fibers 51 in both the conveying direction P and the width direction W are expanded by applying a second external force. As a result, in the fiber sheet 60, the fiber gaps in two directions that are perpendicular to the thickness direction and perpendicular to each other are formed wider than the gaps in the thickness direction. The "fiber gaps in two directions" referred to here correspond to the conveying direction P and the width direction W.
[0047] As another example, the second fibers 92 of this embodiment contain PTFE as a main component. In other words, the second fibers 92 contain PTFE in an amount greater than 50 wt % of the total weight of the second fibers 92. The second fibers 92 are fixed to the first fibers 51 in a dispersed state by a positional stabilizer 93. Therefore, according to this embodiment, the network structure formed by the first fibers 51 and the second fibers 92 is less likely to be destroyed, and a fiber article 62 with improved strength can be produced.
[0048] Furthermore, by reinforcing the plurality of first fibers 51 with the positional stabilizer 93, the skeletal strength of the fiber article 62 formed by the plurality of first fibers 51 is improved. Therefore, the plurality of first fibers 51 can stably support the plurality of second fibers 92. Furthermore, because the strength of the fiber article 62 is improved, the thickness of the fiber article 62 can be made thinner than fiber articles having the same strength. This allows the fiber article 62 to be made more compact. As a result, when manufacturing a fiber article 62 including the first fibers 51 and the second fibers 92 having a smaller outer diameter than the first fibers 51, the strength of the fiber article 62 can be improved and the fiber article 62 can be made more compact.
[0049] The fiber composite 61 is wound onto a winding roll R3 of the winding machine 31. The fiber composite 61 is cut to a predetermined size to produce a fiber article 62. This produces a fiber article 62 in which the occurrence of bias in the fiber gaps between the plurality of first fibers 51 and the plurality of second fibers 92 in the fiber gaps in the two directions is suppressed. The fiber article 62 of this embodiment includes an abundant plurality of second fibers 92 that are dispersedly arranged inside, with bias of the second fibers 92 prevented. Therefore, the effect provided by the second fibers 92 is obtained throughout the entire fiber article 62.
[0050] Furthermore, the fiber article 62 of this embodiment has a configuration in which the fiber gaps in the two directions are wider than the fiber gaps in the thickness direction, which results in a fiber article 62 with a relatively small basis weight, which can suppress an increase in pressure loss over time, and which has uniform and excellent filtering performance.
[0051] The fiber article 62 of this embodiment is, for example, a filter member that is disposed in a flow path through which a predetermined fluid flows and filters out impurities mixed in the fluid. The fluid that passes through the interior of the fiber article 62 may be either a gas or a liquid. An example of the gas is air. The fiber article 62 is in a sheet form. As shown in the enlarged view of FIG. 2 , for example, a small amount of resin granules 91 may remain in the manufactured fiber article 62.
[0052] As described above, the method for manufacturing the fiber article 62 of this embodiment includes a first step of applying an application liquid 90 containing a plurality of resin granules 91 containing a fiberizable polymer and a position stabilizing agent 93 that stabilizes the positions of the plurality of resin granules 91 relative to the plurality of first fibers 51 to a fiber sheet 60 that includes a plurality of first fibers 51 and is being transported in the transport direction P, followed by drying the application liquid 90. After the first step, the method also includes a second step of applying a first external force to the transported fiber sheet 60 so as to reduce the inter-fiber spaces between the first fibers 51.
[0053] The manufacturing method also includes a third step in which, after the second step, the first external force applied to the fiber sheet 60 is relaxed to form a plurality of second fibers 92 thinner than the first fibers 51 from a plurality of resin granules 91 attached to a plurality of first fibers 51, thereby forming a fiber composite 61 containing a plurality of first fibers 51 and a plurality of second fibers 92.
[0054] In addition, as an example of the manufacturing method of this embodiment, in the first step, when the fiber sheet 60 after the first step and before the second step is divided into five parts in the thickness direction, the amount of resin granules 91 in the divided region located at the center of the thickness direction of the fiber sheet 60 is equal to or greater than the amount of resin granules 91 in a pair of divided regions located at the outermost sides in the thickness direction of the fiber sheet 60.
[0055] The amount of resin granules 91 in each divided region of the fiber sheet 60 can be calculated using the results of a known elemental analysis method, such as SEM-EDX (energy dispersive X-ray spectroscopy). This calculation method allows the proportion of resin granules present in each divided region of the fiber sheet 60 to be confirmed, for example, by the following procedure. (i) In the first step, a sample is prepared by solidifying the fiber sheet 60 with resin granules 91 in its natural state using resin. Based on SEM-EDX, primary rays are irradiated onto the multiple resin granules 91 on the cross section of the sample. As a result, fluorescent X-rays are generated from the multiple resin granules 91. A cross-sectional image is then captured in which the fluorescent X-ray emission appears as bright spots. (ii) The total cross-sectional area S0 of the first fibers 51 in each divided region in the cross-sectional image is measured. Furthermore, the total cross-sectional area S1 of the resin granules 91 indicated by the bright spots in each divided region in the cross-sectional image is measured. The ratio S1 / S0 is then calculated. Here, the ratio S1 / S0 is calculated, for example, by the following formula 1: [Formula 1] Ratio S1 / S0 (%) = (total cross-sectional area S1 of resin granules 91 / total cross-sectional area S0 of first fibers 51) × 100 (iii) Comparing the ratios S1 / S0 in each divided region. It is also possible to calculate the ratio V1 / V0 of the volume V0 of a divided region calculated from the area S0 to the total volume V1 of the multiple resin granules 91 calculated from the area S1, and compare the ratios V1 / V0 in each divided region.
[0056] In addition, in the third step of the manufacturing method of this embodiment, as an example, the first external force applied to the fiber sheet 60 is alleviated, and a second external force is applied to the fiber sheet 60 being transported in the transport direction P so as to expand the fiber gaps between the multiple first fibers 51 at least in the width direction W of the fiber sheet 60.
[0057] Furthermore, for example, by adjusting at least one of the strength of the second external force and the temperature when the second external force is applied, it is possible to adjust the fiber gaps between the plurality of first fibers 51 and the plurality of second fibers 92 of the fiber article 62, the number of second fibers 92, and the length of the second fibers 92. This allows the production of fiber articles 62 with different properties. Specifically, by increasing the second external force within a certain range, the basis weight and thickness of the fiber article 62 in its natural state decrease. By reducing the second external force within a certain range, the basis weight and thickness of the fiber article 62 in its natural state increase. By increasing the second external force within a certain range, it is possible to form abundant second fibers 92. For example, increasing the number of second fibers 92 reduces the tensile elongation of the fiber article 62 relative to its natural state. For example, increasing the number of second fibers 92 increases the tensile strength of the fiber article 62.
[0058] Furthermore, for example, the outer diameter D2 of the second fibers 92 can be adjusted by adjusting at least one of the strength of the second external force and the temperature at which the second external force is applied. By increasing the second external force within a certain range, the outer diameter D2 can be set to be small. By decreasing the second external force within a certain range, the outer diameter D2 can be set to be large.
[0059] In the manufacturing method of this embodiment, the outer diameter D2 of the second fibers 92 is set to be smaller than the outer diameter D1 of the first fibers 51. Therefore, the manufactured fiber article 62 has a composite structure of fibers with different diameters. As an example, by adjusting at least one of the strength of the second external force and the temperature when the second external force is applied, the ratio D1 / D2 of the outer diameter D1 to the outer diameter D2 can be set to a value in the range of 15.0 to 1666.7. For example, the ratio D1 / D2 is preferably a value in the range of 15.0 to 1300.0, more preferably a value in the range of 15.0 to 714.3, and even more preferably a value in the range of 15.0 to 300.0. In another example, the ratio D1 / D2 is preferably, for example, a value in the range of 60.0 or more and 1666.7 or less, more preferably a value in the range of 60.0 or more and 1300.0 or less, even more preferably a value in the range of 60.0 or more and 714.3 or less, and even more preferably a value in the range of 60.0 or more and 300.0 or less.
[0060] When the ratio D1 / D2 is 15.0 or more, it is possible to manufacture a fiber article 62 in which the functions of the first fibers 51 and the second fibers 92, which have different outer diameters, can be easily exerted. Furthermore, when the value of the ratio D1 / D2 is 1666.7 or less, it is possible to manufacture a fiber article 62 in which the second fibers 92 can be easily wound around the first fibers 51 while suppressing an increase in the outer diameter D1 of the first fibers 51. Furthermore, by maintaining the outer diameter D2 at a relatively large value, it is possible to easily form the second fibers 92. Furthermore, by setting the ratio D1 / D2 to a value in the range of 60.0 or more and 1666.7 or less, it is possible to improve the filter performance of the manufactured fiber article 62 while reducing the amount of the second fibers 92 used and thereby suppressing the production cost of the fiber article 62.
[0061] The outer diameter D1 is preferably, for example, in the range of 5.0 μm to 50.0 μm, and more preferably in the range of 20.0 μm to 30.0 μm, which allows the first fibers 51 to stably support the second fibers 92 and makes it easy to arrange a large number of second fibers 92 around the first fibers 51.
[0062] Furthermore, the outer diameter D2 is preferably, for example, in the range of 30.0 nm to 1.0 μm, more preferably in the range of 30.0 nm to 800 nm, and even more preferably in the range of 30.0 nm to 166.7 nm. In another example, the outer diameter D2 is preferably, for example, in the range of 50.0 nm to 800.0 nm. This allows the ratio D1 / D2 to be increased while preventing the outer diameter D2 of the second fibers 92 from becoming excessively thin. As a result, a fiber article 62 containing a large number of second fibers 92 can be stably manufactured.
[0063] Furthermore, in the fiber article 62 manufactured by the manufacturing method of this embodiment, for example, the ratio V1 / V2 of the total volume V1 of the first fibers 51 to the total volume V2 of the second fibers 92 and the resin granules 91 is set to a value in the range of 1.9 to 124.0. The ratio V1 / V2 is preferably set to a value in the range of 20.0 to 124.0. By setting the ratios D1 / D2 and V1 / V2 to values in the above ranges, the outer diameter D1 of the first fibers 51 and the outer diameter D2 of the second fibers 92 are made different, thereby making it possible to manufacture a fiber article 62 in which the functions of the first fibers 51 and the second fibers 92 can be easily exhibited.
[0064] In the third step of this embodiment, as an example, the basis weight is 60 g / m 2 More than 300g / m 2 A second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a tensile strength in the minimum strength direction, which is a direction perpendicular to the thickness direction, within the range below, and a value in the minimum strength direction, in which the tensile strength is smallest, within the range of 0.8 N / 10 mm to 100 N / 10 mm. The unit "N / 10 mm" indicates how many N of load can be withstood per 10 mm of measurement width. The "minimum strength direction" referred to here corresponds to the width direction W of the fiber sheet 60. The tensile strength in the minimum strength direction can be adjusted, for example, by applying a second external force in the width direction W to the fiber sheet 60 being conveyed. This allows the production of a fiber article 62 whose basis weight and tensile strength in the minimum strength direction are set to values within the above ranges. Therefore, a fiber article 62 can be produced that is lightweight and has improved strength.
[0065] Generally, for example, when a fiber sheet is continuously produced by a wet papermaking process, a large number of short fibers contained in the impregnation solution, which is the fiber sheet material, are oriented to extend in the conveying direction of the fiber sheet in the production line. Also, for example, when a plurality of first fibers contained in the fiber sheet are continuously spun by a dry spinning process, the first long fibers discharged from the spinning tube are oriented to extend in the conveying direction. Therefore, a typical fiber article has a configuration in which a plurality of fibers extend in a direction perpendicular to the thickness direction, which is perpendicular to the minimum strength direction (in other words, a direction corresponding to the conveying direction of the fiber sheet in the production line; hereinafter, also referred to as the "second direction"). In a typical fiber article, the entanglement of the plurality of fibers in the minimum strength direction is relatively small. Therefore, the strength of the fiber article is smallest in this direction among multiple directions perpendicular to the thickness direction.
[0066] In contrast, the fibrous article 62 of the present embodiment is formed during manufacturing so that the abundant second fibers 92 extend in the width direction W of the fibrous sheet. This increases the entanglement of the first fibers 51 and the second fibers 92 in the minimum strength direction of the fibrous article 62. As a result, the tensile strength of the fibrous article 62 in the minimum strength direction is set to a value in the range of 0.8 N / 10 mm to 100 N / 10 mm by the abundant first fibers 51 and second fibers 92.
[0067] The basis weight value set in the third step is, for example, 60 g / m 2 More than 300g / m 2 Values in the following range are preferred: 60 g / m 2 More than 250g / m 2 More preferably, the basis weight is in the range of 60 g / m. 2 More than 200g / m 2 Values in the following range are preferred: 2 More than 200g / m 2 It is more preferable that the value is in the range of 100 g / m 2 More than 200g / m 2 It is more preferable that the value is in the following range: This makes it easier to reduce the weight of the fiber article 62.
[0068] In the third step of this embodiment, for example, a second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a tensile elongation of 5% to 250% relative to the natural state when the external force is applied in the minimum strength direction. This allows the production of a fiber article 62 having a tensile elongation set to a value within this range. The tensile elongation is preferably, for example, in the range of 10% to 250%, and more preferably in the range of 20% to 250%. In another example, the tensile elongation is preferably, for example, in the range of 30% to 250%, and more preferably in the range of 40% to 250%.
[0069] Here, the tensile strength is measured using, for example, a Tensilon universal testing machine, which is a tensile testing machine conforming to JIS B 7721:2018. In this case, a test piece molded to a width of 10 mm and a length of 60 mm is used. The tensile strength is measured under set conditions of a chuck distance of 40 mm and a tensile speed of 200 mm / min. The tensile elongation is calculated based on the following formula 2 under the same conditions as in the measurement of the tensile strength. [Formula 2] Tensile elongation (%) = elongation (mm) / chuck distance (mm) × 100
[0070] In the third step of this embodiment, a second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a PF value in the range of 16 to 84, for example. The PF value referred to herein refers to a value calculated based on the following formulas 3, 4, and 5. When calculating the transmittance (%) in formula 3, NaCl particles having a particle diameter of 0.4 μm are used, which are generated in accordance with the method described in JIS B9928:1998, Annex 5 (Regulations) NaCl Aerosol Generation Method (Pressure Spray Method). Air containing these NaCl particles is passed through the fiber article 62 in the thickness direction at a flow rate of 5.3 cm / sec. The number of NaCl particles before and after passing through the fiber article 62 is measured using a particle counter. The transmittance (%) is calculated based on these measurements. [Formula 3] Transmittance (%) = (CO / CI) × 100, where CO is the number of NaCl particles after passing through the fiber article 62. CI is the number of NaCl particles before passing through the fiber article 62. [Formula 4] Collection efficiency (%)=100−Transmittance (%) [Formula 5] PF value={−log(100−Collection efficiency (%)) / 100} / (Pressure loss (Pa) / 1000)
[0071] The PF value is preferably, for example, a value in the range of 16 to 70, and more preferably a value in the range of 16 to 60. In another example, a value in the range of 20 to 84 is preferable, and more preferably a value in the range of 25 to 84.
[0072] In the third step of this embodiment, for example, a second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a thickness in the natural state that is less than 3.0 mm. This produces a fiber article 62 having a thickness in the natural state that is set to a value less than 3.0 mm. This allows for the production of a fiber article 62 that is easy to compact. The thickness in the natural state of the fiber composite 61 set in the third step is preferably, for example, 0.1 mm or more and less than 3.0 mm, more preferably 0.1 mm or more and 2.5 mm or less, and even more preferably 0.1 mm or more and 2.0 mm or less. In another example, the thickness is preferably, for example, 0.5 mm or more and 2.5 mm or less, and even more preferably 1.0 mm or more and 2.5 mm or less.
[0073] Furthermore, in the third step of this embodiment, as one example, a second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a pressure loss in the range of 3 Pa to 35 Pa when air is passed through the fiber composite 61 in the thickness direction at a flow rate of 5.3 cm / sec. This allows the production of a fiber article 62 having a pressure loss set to a value within this range. The pressure loss of the fiber composite 61 set in the third step is, for example, preferably in the range of 3 Pa to 25 Pa, and more preferably in the range of 3 Pa to 15 Pa. In another example, the pressure loss is, for example, preferably in the range of 6 Pa to 35 Pa, and more preferably in the range of 9 Pa to 35 Pa.
[0074] The pressure loss is measured, for example, by the following procedure. A measurement sample is placed in a filter having an inner diameter of 113 mm (effective area as a filter medium: 100 cm 2 The measurement sample is set in a holder. The flow rate of the air flowing through the measurement sample is adjusted to 5.3 cm / sec using a flow meter. The pressure loss occurring between the upstream and downstream sides of the measurement sample in the air flow direction is measured using a manometer.
[0075] Furthermore, in the third step of this embodiment, as one example, a second external force is applied to the fiber sheet 60 so as to form a fiber composite 61 having a collection efficiency in the range of 35% to 95%. This collection efficiency is calculated using the above-mentioned formula 4. This allows the production of a fiber article 62 having a collection efficiency set within this range. The collection efficiency of the fiber composite 61 set in the third step is preferably, for example, a value in the range of 35% to 85%, and more preferably a value in the range of 35% to 75%. In another example, the collection efficiency is preferably, for example, a value in the range of 40% to 90%, and more preferably a value in the range of 45% to 90%.
[0076] Furthermore, when setting at least one of the tensile strength, tensile elongation, PF value, thickness in natural state, pressure loss, and collection efficiency of the fiber composite 61, it is possible to easily set them to the desired set value by using, for example, only the first intermediate 56.
[0077] As described above, according to the method for manufacturing the fiber article 62 of this embodiment, the fluidity of the impregnation liquid 90 disappears as the impregnation liquid 90 impregnated on the fiber sheet 60 dries. At this time, the relative positions of the plurality of resin granules 91 with respect to the plurality of first fibers 51 are stabilized by the position stabilizing agent 93. This prevents the resin granules 91 from moving relative to the first fibers 51 after being impregnated on the first fibers 51. This allows the plurality of resin granules 91 to be dispersed and maintained in an impregnated state throughout the fiber sheet 60. This allows the formation of a plurality of second fibers 92 dispersed throughout the fiber article 62. This allows the manufacture of a fiber article 62 with uniform filtering performance and improves the strength of the fiber article 62.
[0078] Furthermore, by applying the positional stabilizer 93 to the fiber sheet 60 together with the impregnation liquid 90, for example, the entire surface of the first fibers 51 is coated with the positional stabilizer 93. As a result, the first fibers 51 are reinforced by the positional stabilizer 93. This improves the skeletal strength of the fiber article 62 formed by a plurality of first fibers 51. This further improves the strength of the fiber article 62. Furthermore, the improved strength of the fiber article 62 allows the thickness of the fiber article 62 to be thinner than fiber articles having the same strength. This allows the fiber article 62 to be made more compact.
[0079] The positional stabilizer 93 of this embodiment includes, for example, at least one of sodium carboxymethyl cellulose and hydroxyethyl cellulose. This improves the affinity of the positional stabilizer 93 to the first fibers 51, for example, when the first fibers 51 include cellulose acetate. Therefore, the positional stabilizer 93 and the resin particles 91 can be effectively attached to the entire surfaces of the first fibers 51.
[0080] In the first step of this embodiment, as an example, when the fiber sheet 60 is divided into five thicknesswise portions after the first step and before the second step, the adhesive liquid 90 is applied to the fiber sheet 60 so that the amount of resin granules 91 in the divided region located at the center of the thickness direction of the fiber sheet 60 is equal to or greater than the amount of resin granules 91 in a pair of divided regions located at the outermost sides of the thickness direction of the fiber sheet 60. This manufacturing method makes it easy to ensure a plentiful amount of resin granules 91 in the divided region located at the center of the thickness direction of the fiber sheet 60. This makes it easy to form an abundant amount of second fibers 92 in and around the center of the thickness direction of the fiber article 62. This therefore further improves the strength of the fiber article 62.
[0081] In addition, in the third step of this embodiment, as an example, the first external force applied to the fiber sheet 60 is alleviated, and a second external force is applied to the fiber sheet 60 being transported in the transport direction P so as to expand the fiber gaps between the multiple first fibers 51 at least in the width direction W of the fiber sheet 60.
[0082] According to the above-described manufacturing method, the interstices between the plurality of first fibers 51 can be actively enlarged in the direction in which the second external force is applied. As a result, the second external force is applied to the resin granules 91 attached to the plurality of first fibers 51, and abundant second fibers 92 can be formed from the plurality of resin granules 91 so that the second fibers 92 extend in the direction in which the second external force is applied. This increases the degree of entanglement between the first fibers 51 and the second fibers 92 in the direction in which the second external force is applied. This facilitates improving the strength of the fiber article 62. Furthermore, the fiber sheet 60 conveyed in the conveying direction P has wide interstices at least in the direction in which the second external force is applied. This allows for the manufacture of a fiber article 62 with a reduced basis weight and thus a lighter weight.
[0083] In the third step of this embodiment, for example, a second external force is applied to the fiber sheet 60 while the fiber sheet 60 is heated. According to this manufacturing method, the fine fibers folded and contained within the heated resin granules 91 can be easily pulled out to the outside by the second external force. This makes it easy to form abundant second fibers 92.
[0084] In the third step of this embodiment, as an example, a second external force is also applied to the fiber sheet 60 in the conveying direction P of the fiber sheet 60. According to this manufacturing method, by additionally applying a second external force to the plurality of resin granules 91 in the conveying direction P in the third step, it is possible to pull out fine fibers from the resin granules 91 to the outside, for example, and to easily form a more abundant second fiber 92.
[0085] In the first step of this embodiment, as an example, a nonwoven fabric is used as the fiber sheet 60. This manufacturing method, when manufacturing a fiber article 62 that includes first fibers 51 and second fibers 92 having a smaller outer diameter than the first fibers 51 and has a nonwoven fabric structure, can effectively improve the strength and compactness of the fiber article 62. Furthermore, by forming wide interstices between the multiple first fibers 51, the weight of the fiber article 62 can be reduced.
[0086] In addition, in the first step of this embodiment, as an example, a plurality of resin granules 91 having a lamellar structure are used. According to this manufacturing method, the second fibers 92 can be efficiently formed from the resin granules 91 in the third step.
[0087] In addition, in the first step of this embodiment, as an example, a plurality of crimped first fibers 51 are used. According to this manufacturing method, the first fibers 51 can be configured to be bulkier than those in an uncrimped state. This allows abundant fiber gaps formed by the plurality of first fibers 51 to be arranged in the fiber article 62. This makes it easier to reduce the weight and compactness of the fiber article 62.
[0088] In the first step of this embodiment, for example, a plurality of first fibers 51 containing at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate are used. This manufacturing method allows for a wider range of choices for the material of the first fibers 51. This improves the design freedom of the fiber article 62.
[0089] In addition, the fiberizable polymer in this embodiment includes, for example, at least one of polytetrafluoroethylene, polypropylene, polyethylene, and polyamide. This manufacturing method can expand the range of materials that can be selected for the second fibers 92. Therefore, this manufacturing method can also further improve the design freedom of the fiber article 62.
[0090] (Confirmation Tests) Next, confirmation tests and their results for the present disclosure are described below. The present disclosure is not limited to the following examples. [Test 1] A fiber sheet 60 was prepared, including a plurality of first fibers 51 (short fibers 52) that were crimped CA fibers. A plurality of resin granules 91 containing PTFE was also prepared. An impregnation liquid 90 containing a plurality of resin granules 91 and a positional stabilizer 93 (CMC) was also prepared. A fiber article 62 according to Example 1 was produced by sequentially performing steps 1 to 3. For comparison with Example 1, a fiber article according to Comparative Example 1 was produced in the same manner as Example 1, except that the impregnation liquid did not contain a positional stabilizer.
[0091] Fig. 3 is an enlarged photograph of the surface of the fibrous sheet according to Comparative Example 1 after the impregnation liquid has dried and before the first external force has been applied. Fig. 4 is an enlarged photograph of the interior of the fibrous sheet according to Comparative Example 1 after the impregnation liquid has dried and before the first external force has been applied. As shown in Figs. 3 and 4, in Comparative Example 1, it was confirmed that the resin granules attached to the first fibers in the interior of the fibrous sheet migrated to the surface layer of the fibrous sheet over time and decreased in the interior of the fibrous sheet. This revealed that in Comparative Example 1, the second fibers were biased toward the surface layer relative to the interior.
[0092] Fig. 5 is an enlarged photograph of the surface of the fibrous sheet 60 according to Example 1 after the impregnation liquid 90 has dried and before the first external force has been applied. Fig. 6 is an enlarged photograph of the interior of the fibrous sheet 60 according to Example 1 after the impregnation liquid 90 has dried and before the first external force has been applied. As shown in Figs. 5 and 6 , in Example 1, as opposed to Comparative Example 1, it was confirmed that the relative positions of the resin particles 91 attached to the first fibers 51 inside the fibrous sheet 60 were stably maintained relative to the first fibers 51 by the position stabilizing agent 93 even after a certain period of time. This demonstrates that Example 1 produced a fibrous article 62 in which an abundant number of second fibers 92 were dispersed.
[0093] [Test 2] Based on the above-described steps (i) to (iii), the S1 / S0 ratios of each of the divided regions of the fiber sheet in Example 1 and Comparative Example 1 were calculated at a timing corresponding to after the first step and before the second step. As a result, the S1 / S0 (%) of the divided region located at the center in the thickness direction of the fiber sheet in Comparative Example 1 was 10%, and the S1 / S0 (%) of the pair of divided regions located at the outermost positions in the thickness direction of the fiber sheet in Example 1 was 350% and 180%. In contrast, the S1 / S0 (%) of the divided region located at the center in the thickness direction of the fiber sheet 60 in Example 1 was 340%, and the S1 / S0 (%) of the pair of divided regions located at the outermost positions in the thickness direction of the fiber sheet in Example 1 was 890% and 530%.
[0094] These test results also confirmed that in Example 1, compared to Comparative Example 1, the resin particles 91 attached to the multiple first fibers 51 inside the fiber sheet 60 were able to stably maintain their relative position to the first fibers 51 due to the position stabilizer 93 even after a certain period of time had passed.
[0095] [Test 3] Fiber articles 62 of Examples 2 to 5 were manufactured in which the amounts of resin granules 91 attached to the plurality of first fibers 51 and the amount of positional stabilizer 93 attached to the plurality of first fibers were different. Furthermore, fiber articles of Comparative Examples 2 to 7 were manufactured in which no positional stabilizer was attached to the plurality of first fibers and the amounts of resin granules attached to the plurality of first fibers were different. Resin granules containing PTFE were used as the resin granules 91. Carboxymethyl cellulose sodium was used as the positional stabilizer 93.
[0096] In producing each fiber article, a first external force was applied to the fiber sheet under the following production conditions: a pressure of 5 MPa, a heating temperature of 170°C during application of the external force, and an external force application time of 90 seconds. In producing each fiber article, a second external force was applied to the fiber sheet in the width direction W of the fiber sheet under the following production conditions: a heating temperature of 60°C during application of the external force, an elongation of 30%, and a stretching speed of 1 mm / s. The basis weight, thickness, thickness change rate, pressure loss, collection efficiency, and PF value of each produced fiber article were measured. Furthermore, the tensile strength (N / 10 mm) in the machine direction P, the elongation (%) in the machine direction P, the tensile strength (N / 10 mm) in the width direction W, and the elongation (%) in the width direction W were measured for the fiber articles of Examples 3 and 4 and Comparative Examples 4 and 5. The measurement results are shown in Tables 1 and 2. The elongation is expressed based on the following formula 6. In Table 1, "wt%" indicates mass fraction. [Formula 6] Elongation (%) = (length after elongation L / natural length L0) x 100-100
[0097]
[0098]
[0099] As shown in Table 1, it was confirmed that Examples 2 to 5 tended to have higher values for at least the collection efficiency (%) and PF value compared to Comparative Examples 2 to 7. Furthermore, as shown in Table 2, it was confirmed that Examples 3 and 4 tended to have higher tensile strength in the conveying direction and width direction compared to Comparative Examples 4 and 5. Furthermore, the tensile strength in Example 4 in the conveying direction and width direction was equal to or higher than those of Comparative Examples 4 and 5.
[0100] Each configuration and combination thereof in the embodiments are examples. Addition, omission, substitution, and other modifications of configurations are possible as appropriate without departing from the spirit of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the claims. Furthermore, each aspect disclosed herein can be combined with any other feature disclosed herein.
[0101] In the first step, the number of times the adhering liquid 90 is applied to the fiber sheet 60 is not limited to one, and may be two or more times. In this case, for example, after the adhering liquid 90 that has been applied once to the fiber sheet 60 is dried, new adhering liquid 90 may be applied to the fiber sheet 60. Furthermore, when the adhering liquid 90 is applied multiple times, the position at which the adhering liquid 90 is applied to the fiber sheet 60 may be changed. The size of the fiber article 62 to be manufactured is not limited. Furthermore, the fiber article 62 may be used in a state where a plurality of fiber articles 62 or other configurations are combined.
[0102] 51 First fiber 60 Fiber sheet 61 Fiber composite 62 Fiber article 90 Impregnation liquid 91 Resin granules 92 Second fiber 93 Position stabilizer
Claims
1. A method for manufacturing a fiber article, comprising: a first step of applying an application liquid containing a plurality of resin granules containing a polymer capable of being fiberized and a position stabilizing agent for stabilizing the positions of the plurality of resin granules relative to the plurality of first fibers to a fiber sheet which contains a plurality of first fibers and is transported in a predetermined transport direction, and then drying the applied liquid; a second step of applying a first external force to the transported fiber sheet after the first step so as to reduce the fiber gaps between the first fibers; and a third step of forming a fiber composite containing the plurality of first fibers and the plurality of second fibers from the plurality of resin granules applied to the plurality of first fibers by relaxing the first external force applied to the fiber sheet after the second step.
2. The method for producing a fiber article according to claim 1, wherein the position stabilizer comprises at least one of sodium carboxymethylcellulose or hydroxyethylcellulose.
3. A method for manufacturing a fiber article as described in claim 1 or 2, wherein in the first step, the adhesive liquid is applied to the fiber sheet so that when the fiber sheet is divided into five parts in the thickness direction after the first step and before the second step, the amount of resin granules in a divided area located at the center of the thickness direction of the fiber sheet is equal to or greater than the amount of resin granules in a pair of divided areas located at the outermost sides in the thickness direction of the fiber sheet.
4. A method for manufacturing a fiber article described in any one of claims 1 to 3, wherein in the third step, the first external force applied to the fiber sheet is alleviated and a second external force is applied to the fiber sheet transported in the transport direction so as to expand the fiber gaps between the multiple first fibers at least in the width direction of the fiber sheet.
5. A method for producing a fiber article as described in claim 4, wherein in the third step, the second external force is applied to the fiber sheet while the fiber sheet is in a heated state.
6. A method for manufacturing a fiber article as described in claim 4 or 5, wherein in the third step, the second external force is also applied to the fiber sheet in the conveying direction of the fiber sheet.
7. A method for producing a fiber article according to any one of claims 1 to 6, wherein in the first step, a nonwoven fabric is used as the fiber sheet.
8. A method for producing a fiber article according to any one of claims 1 to 7, wherein the first step uses a plurality of resin particles having a lamellar structure.
9. A method for producing a fiber article according to any one of claims 1 to 8, wherein the first step uses the plurality of first fibers that have been crimped.
10. A method for producing a fiber article according to any one of claims 1 to 9, wherein the first step uses the plurality of first fibers containing at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate.
11. The method for producing a fiber article according to any one of claims 1 to 10, wherein the fiberizable polymer comprises at least one of polytetrafluoroethylene, polypropylene, polyethylene, and polyamide.
Citation Information
Patent Citations
Skin-contacting articles
WO1998031868A1
Method for producing fiber articles
WO2021039979A1