Fiber article

The textile article achieves improved strength and reduced weight by configuring first and second fibers with specific diameter ratios and support structures, ensuring effective filter performance and resistance to external forces.

WO2024228360A1PCT designated stage expired Publication Date: 2024-11-07DAICEL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016295
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2024-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Textile articles with first fibers and second fibers of smaller outer diameter require improved strength and reduced weight, while maintaining filter performance, as existing solutions often compromise on either strength or weight.

Method used

A sheet-like fiber article with first fibers and second fibers of smaller outer diameter, supported by the first fibers in a dispersed state, achieving a basis weight of 60 g/m² or more and tensile strength of 0.8 N/10 mm or more in the minimum strength direction, while maintaining a thickness of less than 3.0 mm and efficient filter performance.

Benefits of technology

The solution enhances the tensile strength and reduces the weight of the textile article, maintaining stable filter performance and preventing damage from external forces, while allowing for efficient fluid flow and filter functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016295_07112024_PF_FP_ABST
    Figure JP2024016295_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The objective of the present invention is to reduce the weight and improve the strength of a fiber article including a first fiber and a second fiber having an outer diameter smaller than that of the first fiber. The fiber article according to the present invention is sheet-shaped and includes a plurality of first fibers and a plurality of second fibers having an outer diameter smaller than that of the first fibers and being supported in a dispersed state by the plurality of first fibers. The basis weight of the fiber article is in a range between 60 g / m2 and 300 g / m2 both inclusive. The fiber article has a tensile strength between 0.8 N / 10 mm and 100 N / 10 mm both inclusive, in a minimum strength direction in which the tensile strength is minimum among directions perpendicular to the thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Textile products

[0001] The present disclosure relates to a fibrous article that includes a first fiber and a second fiber having a smaller outer diameter than the first fiber.

[0002] As a fibrous article used for applications such as air conditioner filters, for example, as disclosed in Patent Document 1, a fibrous article including first fibers and second fibers having an outer diameter smaller than that of the first fibers is known.

[0003] International Publication No. 2021 / 039980

[0004] In the fiber article described in Patent Document 1, the second fibers are supported by the first fibers, and the functions of the first fibers and the second fibers are exerted, thereby improving the performance of the fiber article. Here, it would be more preferable if the fiber article could be made lighter and have improved strength, for example.

[0005] Therefore, an object of the present disclosure is to provide a fiber article including a first fiber and a second fiber having an outer diameter smaller than that of the first fiber, which can reduce the weight of the fiber article and improve its strength.

[0006] In order to solve the above problems, a fiber article according to one aspect of the present disclosure is a sheet-like fiber article including a plurality of first fibers and a plurality of second fibers having an outer diameter smaller than that of the first fibers and supported by the first fibers in a dispersed state, and having a basis weight of 60 g / m 2 More than 300g / m 2 The tensile strength in the minimum strength direction, in which the tensile strength is smallest among directions perpendicular to the thickness direction, is a value in the range of 0.8 N / 10 mm or more and 100 N / 10 mm or less.

[0007] According to one aspect of the present disclosure, in a fiber article including first fibers and second fibers having an outer diameter smaller than that of the first fibers, the fiber article can be made lighter and have improved strength.

[0008] 1 is a schematic diagram of a fiber article according to a first embodiment; FIG. 2 is a cross-sectional view of a fiber composite according to a second embodiment;

[0009] The present inventors have conducted extensive research into the above-mentioned problems and have found that, when manufacturing a textile article, focusing on the basis weight of the textile article to be manufactured and the tensile strength in the minimum strength direction where the tensile strength is minimized, and adjusting these values ​​so that they fall within a predetermined range, can reduce the weight of the textile article and improve its strength. The present disclosure solves the above-mentioned problems by configuring a textile article so that it has excellent tensile strength despite having a relatively low basis weight. Hereinafter, each embodiment of the present disclosure will be described with reference to the drawings.

[0010] (First embodiment) FIG. 1 is a schematic diagram of a fiber article 1 according to a first embodiment. FIG. 1 also illustrates an enlarged view that schematically shows the internal structure of the fiber article 1. The fiber article 1 shown in FIG. 1 is, for example, a filter member that is disposed in a flow path through which a predetermined fluid flows and filters out impurities mixed in the fluid. The fluid that passes through the interior of the fiber article 1 may be either a gas or a liquid. An example of the gas is air. The fiber article 1 is in a sheet form. The fiber article 1 includes a plurality of first fibers 2 and a plurality of second fibers 3 that have an outer diameter smaller than the first fibers 2 and are supported by the first fibers 2 in a dispersed state.

[0011] The fiber article 1 has a basis weight of 60 g / m 2 More than 300g / m 2 Values ​​in the following range (for example, 152 g / m 2 The basis weight is set to, for example, 60 g / m 2 More than 250g / m 2 Values ​​in the following range are preferred: 60 g / m 2 More than 200g / m 2 It is more preferable that the value is in the following range. In another example, the basis weight is, for example, 80 g / m 2 More than 200g / m 2 Values ​​in the following range are preferred: 2 More than 200g / m 2 More preferably, the value is in the range below.

[0012] The tensile strength of the fiber article 1 in a minimum strength direction (hereinafter also referred to as the "first direction"), in which the tensile strength is minimum among directions perpendicular to the thickness direction, is at least 0.8 N / 10 mm or more. The unit "N / 10 mm" indicates how many N of load can be withstood per 10 mm of measurement width. The "minimum strength direction" here refers to the width direction of a fiber sheet (hereinafter also simply referred to as the "fiber sheet"), which is an intermediate product of the fiber article 1 before cutting, in a production line that continuously produces the fiber article 1. In other words, the "minimum strength direction" corresponds to the width direction perpendicular to the conveyance direction of the fiber sheet.

[0013] Generally, for example, when a fiber sheet is continuously produced by a wet papermaking method, many of the short fibers contained in the dispersion liquid, which is the fiber sheet material, are oriented to extend in the conveying direction of the fiber sheet in the production line. Furthermore, for example, when multiple first fibers contained in the fiber sheet are continuously spun by a melt spinning method, an electrospinning method, a dry spinning method, or the like, the first fibers of the long fibers discharged from the spinning tube are oriented to extend in the conveying direction. Therefore, a typical fiber product has multiple fibers extending in a direction perpendicular to the thickness direction, which is perpendicular to the minimum strength direction (in other words, a direction corresponding to the conveying direction of the fiber sheet in the production line; hereinafter, also referred to as the "second direction"). In a typical fiber product, the entanglement of multiple fibers in the minimum strength direction is relatively small. Therefore, the strength of the fiber product is smallest in this direction among multiple directions perpendicular to the thickness direction.

[0014] In contrast, the tensile strength of the fiber article 1 of this embodiment in the minimum strength direction is set to a value in the range of at least 0.8 N / 10 mm or more, thereby improving the tensile strength in that direction. As will be described later, in the fiber article 1 of this embodiment, the abundant second fibers 3 are formed to extend in the width direction of the fiber sheet during production. This increases the entanglement of the first fibers 2 and the second fibers 3 in the minimum strength direction in the fiber article 1. As a result, the tensile strength of the fiber article 1 in the minimum strength direction is improved by the abundant first fibers 2 and second fibers 3.

[0015] Furthermore, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 100 N / 10 mm or less. This, for example, can prevent the tensile strength of the fiber article 1 from becoming excessively high, making it easier to manufacture the fiber article 1. The tensile strength of the fiber article 1 of this embodiment is a value in the range of 0.8 N / 10 mm or more and 100 N / 10 mm or less. The range of the tensile strength in the direction of minimum strength is preferably, for example, a value in the range of 1 N / 10 mm or more and 100 N / 10 mm or less, and more preferably a value in the range of 5 N / 10 mm or more and 100 N / 10 mm or less. In another example, the range of the tensile strength in the direction of minimum strength is preferably, for example, a value in the range of 8 N / 10 mm or more and 100 N / 10 mm or less, and more preferably a value in the range of 10 N / 10 mm or more and 100 N / 10 mm or less.

[0016] Furthermore, as an example, the tensile elongation of the fiber article 1 of this embodiment relative to the natural state in the direction of minimum strength is at least 5%. Furthermore, the tensile elongation of the fiber article 1 of this embodiment is a value in the range of 250% or less. That is, the tensile elongation of the fiber article 1 of this embodiment is a value in the range of 5% or more and 250% or less. This makes the fiber article 1 less likely to break even when an external force acts in the direction of minimum strength. The tensile elongation is preferably, for example, a value in the range of 10% or more and 250% or less, and more preferably a value in the range of 20% or more and 250% or less. As another example, the tensile elongation is preferably, for example, a value in the range of 30% or more and 250% or less, and more preferably a value in the range of 40% or more and 250% or less.

[0017] Here, the tensile strength is measured using, for example, a Tensilon universal testing machine, which is a tensile testing machine conforming to JIS B 7721:2018. In this case, a test piece molded to a width of 10 mm and a length of 60 mm is used. The tensile strength is measured under set conditions of a chuck distance of 40 mm and a tensile speed of 200 mm / min. The tensile elongation is calculated based on the following formula 1 under the same conditions as in the measurement of the tensile strength. [Formula 1] Tensile elongation (%) = elongation (mm) / chuck distance (mm) × 100

[0018] Furthermore, the thickness of the fiber article 1 of this embodiment is set to a value in the range of less than 3.0 mm (for example, 1.1 mm). The thickness of the fiber article 1 is, for example, a value in the range of 0.1 mm or more and less than 3.0 mm. This thickness is, for example, preferably a value in the range of 0.1 mm or more and 2.5 mm or less, and more preferably a value in the range of 0.1 mm or more and 2.0 mm or less. In another example, this thickness is, for example, preferably a value in the range of 0.5 mm or more and 2.5 mm or less, and more preferably a value in the range of 1.0 mm or more and 2.5 mm or less. Note that the "thickness" of the fiber article 1 referred to in this specification refers to the thickness of the fiber article 1 in its natural state.

[0019] Furthermore, the fiber article 1 of this embodiment has a PF value set to a value in the range of 16 to 84 (for example, 64). The PF value referred to here refers to a value calculated based on the following formulas 2, 3, and 4. When calculating the transmittance (%) in formula 2, NaCl particles having a particle diameter of 0.4 μm are used, which are generated in accordance with the method described in JIS B9928 Appendix 5 (Regulations) NaCl aerosol generation method (pressure spray method). Air containing these NaCl particles is passed through the fiber article 1 in the thickness direction at a flow rate of 5.3 cm / sec, and the number of NaCl particles before and after passing through the fiber article 1 is measured using a particle counter. The transmittance (%) is calculated based on these measurements. [Formula 2] Transmittance (%) = (CO / CI) × 100 where CO is the number of NaCl particles after passing through the fiber article 1, and CI is the number of NaCl particles before passing through the fiber article 1. [Formula 3] Collection efficiency (%) = 100 - transmittance (%) [Formula 4] PF value = {-log((100 - collection efficiency (%)) / 100} / (pressure loss (Pa) / 1000)

[0020] The PF value is preferably, for example, a value in the range of 16 to 70, and more preferably a value in the range of 16 to 60. In another example, a value in the range of 20 to 84 is preferable, and more preferably a value in the range of 25 to 84.

[0021] The fiber article 1 of this embodiment has a pressure loss set to a value in the range of 3 Pa to 35 Pa (for example, 6 Pa) when air is passed through it in the thickness direction at a flow rate of 5.3 cm / sec. This pressure loss is, for example, preferably in the range of 3 Pa to 25 Pa, and more preferably in the range of 3 Pa to 15 Pa. In another example, it is, for example, preferably in the range of 6 Pa to 35 Pa, and more preferably in the range of 9 Pa to 35 Pa.

[0022] This pressure loss is measured, for example, by the following procedure. A measurement sample is placed in a filter having an inner diameter of 113 mm (effective area as a filter medium: 100 cm 2 The measurement sample is set in a holder. The flow rate of the air flowing through the measurement sample is adjusted to 5.3 cm / sec using a flow meter. The pressure loss occurring between the upstream and downstream sides of the measurement sample in the air flow direction is measured using a manometer.

[0023] In the fiber article 1 of this embodiment, the collection efficiency calculated by Equation 3 is set to a value in the range of 35% to 95% (for example, 61%). This collection efficiency is preferably, for example, in the range of 35% to 85%, and more preferably in the range of 35% to 75%. In another example, it is preferably, for example, in the range of 40% to 90%, and more preferably in the range of 45% to 90%.

[0024] The fiber article 1 of this embodiment has a nonwoven structure. The first fibers 2 are, for example, short fibers. The first fibers 2 have a length in the range of 10 mm to 100 mm. The first fibers 2 have a higher strength (e.g., tensile strength) than the second fibers 3. The plurality of first fibers 2 constitute the main skeleton of the fiber article 1. The first fibers 2 of this embodiment are crimped. By using the plurality of crimped first fibers 2, the fiber density of the fiber article 1 is reduced compared to when the plurality of uncrimped first fibers 2 is used. In addition, for example, the first fibers 2 are longer than the second fibers 3. As a result, even if the number of first fibers 2 is relatively small, the abundant second fibers 3 can be stably supported by the first fibers 2.

[0025] The outer diameter D2 of the second fibers 3 is smaller than the outer diameter D1 of the first fibers 2. Therefore, the fiber article 1 has a composite structure of fibers with different diameters. The second fibers 3 are supported by the first fibers 2 in a dispersed state throughout the fiber article 1. The second fibers 3 are at least partially attached to the first fibers 2. As an example, the ratio D1 / D2 of the outer diameter D1 of the first fibers 2 to the outer diameter D2 of the second fibers 3 is set to a value in the range of 15.0 to 1666.7. As such, the fiber article 1 of this embodiment includes, as an example, first fibers 2 having a large outer diameter D1 and second fibers 3 having an outer diameter D2 that is significantly smaller than the outer diameter D1.

[0026] The ratio D1 / D2 is preferably, for example, in the range of 15.0 to 1300.0, more preferably in the range of 15.0 to 714.3, and even more preferably in the range of 15.0 to 300.0.

[0027] In another example, the ratio D1 / D2 is preferably, for example, a value in the range of 60.0 or more and 1666.7 or less, more preferably a value in the range of 60.0 or more and 1300.0 or less, even more preferably a value in the range of 60.0 or more and 714.3 or less, and even more preferably a value in the range of 60.0 or more and 300.0 or less.

[0028] If the ratio D1 / D2 is 15.0 or more, it is possible to easily achieve the respective functions of the first fibers 2 and the second fibers 3, which have different outer diameters, in the fiber article 1. Furthermore, if the value of the ratio D1 / D2 is 1666.7 or less, it is possible to easily string the second fibers 3 around the first fibers 2, while suppressing an increase in the outer diameter D1 of the first fibers 2. Furthermore, by maintaining the outer diameter D2 at a certain value, it is possible to easily form the second fibers 3. Furthermore, by setting the ratio D1 / D2 to a value in the range of 60.0 or more and 1666.7 or less, it is possible to improve the filter performance of the fiber article 1, while reducing the amount of the second fibers 3 used and thereby suppressing the production cost of the fiber article 1.

[0029] The outer diameter D1 is preferably, for example, in the range of 5.0 μm to 50.0 μm, and more preferably in the range of 20.0 μm to 30.0 μm. This configuration makes it easy to arrange a large number of second fibers 3 around the first fibers 2 while stably supporting the second fibers 3 with the first fibers 2.

[0030] The outer diameter D2 is preferably, for example, in the range of 30.0 nm to 1.0 μm, more preferably in the range of 30.0 nm to 800 nm, and even more preferably in the range of 30.0 nm to 166.7 nm. In another example, the outer diameter D2 is preferably, for example, in the range of 50.0 nm to 800.0 nm. This configuration can increase the ratio D1 / D2 while preventing the outer diameter D2 of the second fibers 3 from becoming excessively thin. As a result, a fiber article 1 containing a large number of second fibers 3 can be stably constructed.

[0031] In addition, in the fiber article 1, for example, the ratio V1 / V2 of the total volume V1 of the first fibers 2 to the total volume V2 of the second fibers 3 and the resin granules 4 is set to a value in the range of 1.9 to 124.0. The ratio V1 / V2 is further preferably set to a value in the range of 20.0 to 124.0. By setting the ratios D1 / D2 and V1 / V2 to values ​​in the above ranges, the outer diameter D1 of the first fibers 2 and the outer diameter D2 of the second fibers 3 can be made different, making it easier for the first fibers 2 and the second fibers 3 to exhibit their respective functions.

[0032] The textile article 1 has interstices between the plurality of crimped first fibers 2 and interstices between the plurality of second fibers 3. In other words, the textile article 1 has a mesh structure made up of the plurality of crimped first fibers 2 and the plurality of second fibers 3. In the textile article 1 of this embodiment, the second fibers 3 are fixed to the first fibers 2, so that the mesh structure is less likely to be destroyed even when an external force is applied to the textile article 1.

[0033] Furthermore, inside the fiber article 1, the second fibers 3 are entangled with and supported by the first fibers 2. Therefore, even if the outer diameter D2 of the second fibers 3 is smaller than the outer diameter D1 of the first fibers 2, the second fibers 3 can be supported by the first fibers 2 while preventing damage such as breakage of the second fibers 3. Therefore, the functions of the second fibers 3 can be maintained for a long period of time.

[0034] Furthermore, the plurality of second fibers 3 are dispersed and arranged over a wide region of the sheet-like fiber article 1 extending in the direction of extension of the plurality of first fibers 2. As a result, the fiber article 1 has abundant fiber gaps formed by the plurality of first fibers 2 and the plurality of second fibers 3. In other words, the fiber article 1 is prevented from having uneven fiber gaps between the plurality of first fibers 2 and the plurality of second fibers 3, for example, in a plane perpendicular to the thickness direction, in a first direction and a second direction extending perpendicular to each other. As a result, when the fiber article 1 is placed in the flow path and a fluid is circulated through the fiber article 1, the fluid can be brought into uniform contact with the first fibers 2 and the second fibers 3, making it easier for the first fibers 2 and the second fibers 3 to exhibit their respective functions. Furthermore, the formation of the network structure in the fiber article 1 allows the shape of the fiber article 1 to be maintained, and the filter performance of the fiber article 1 to be stably maintained.

[0035] In this embodiment, the second fibers 3 are formed, for example, from resin granules 4 attached to the first fibers 2 during the production of the fiber article 1. For example, the resin granules 4 are extrusion molded bodies produced by a paste extrusion molding method. The resin granules 4 contain a polymer that can be fiberized. In this embodiment, with the resin granules 4 attached to a plurality of first fibers 2, a first external force is applied to the resin granules 4 in a direction that compresses (reduces) the interstices between the first fibers 2, and then a second external force is applied in a direction that relieves the first external force, thereby forming the second fibers 3 from the resin granules 4.

[0036] The second fibers 3 can also be formed when the first external force applied to the resin granules 4 is relaxed, thereby expanding the inter-fiber spaces between the multiple first fibers 2. However, in this embodiment, abundant second fibers 3 are actively formed by applying a second external force to the resin granules 4. Furthermore, as shown in the enlarged view in Figure 1, for example, some resin granules 4 remain in the manufactured fiber article 1. Depending on the manufacturing method of the fiber article 1, no resin granules 4 may remain in the fiber article 1.

[0037] The resin granules 4 contain a lamellar structure. As used herein, the term "lamellar structure" refers to a structure in which the polymer chains that make up the resin of the resin granules 4 are connected and folded. Specifically, the lamellar structure contained in the resin granules 4 is composed of fine fibers formed by millions of these polymer chains connected in a ribbon-like shape. These fine fibers are folded and stored inside the resin granules 4. By sequentially applying a first external force and a second external force to the resin granules 4, the fine fibers extend from the inside of the resin granules 4 toward the outside.

[0038] For example, during the production of the fiber article 1, a first external force is applied to a plurality of resin granules 4 attached to a plurality of first fibers 2, and then a second external force is applied in the conveying direction and the width direction, thereby forming a plurality of second fibers 3 extending in the conveying direction and a plurality of second fibers 3 extending in the width direction. This suppresses deviation of the fiber gaps at least in the first direction and the second direction, and a fiber article 1 is obtained whose tensile strength in the minimum strength direction perpendicular to the thickness direction is in the range of 0.8 N / 10 mm to 100 N / 10 mm. Furthermore, by using the second external force, the fiber gaps are appropriately enlarged, and the basis weight is increased to 60 g / m. 2 More than 300g / m 2 A fiber article 1 having values ​​in the following ranges is obtained.

[0039] The material of the first fibers 2 can be selected as appropriate. During the production of the fiber article 1, for example, an aqueous dispersion containing the resin granules 4 (hereinafter simply referred to as aqueous dispersion) is applied to the first fibers 2, thereby attaching the resin granules 4 to the first fibers 2. In this case, in order to increase the affinity of the first fibers 2 for the aqueous dispersion, it is preferable that the material of the first fibers 2 has a relatively low water contact angle θ1 immediately after water droplets are dropped on the surfaces of the first fibers 2.

[0040] As an example, the first fibers 2 include at least one of rayon, polypropylene (PP), polyethylene terephthalate (PET), polyethylene (PE), and cellulose acetate. Such materials can suppress the water contact angle θ1 to a relatively low value. The first fibers 2 in this embodiment are cellulose acetate fibers. The textile article 1 includes a plurality of first fibers 2 obtained by crimping and opening a tow (tow band) containing cellulose acetate fibers. This configuration allows the textile article 1 to easily achieve a desired bulkiness.

[0041] Next, the second fibers 3 will be described in detail. The first fibers 2 and the second fibers 3 have good affinity with each other. In this embodiment, the second fibers 3 are attached to the first fibers 2 by, for example, van der Waals forces. As an example, the second fibers 3 include a polymer that can be fiberized. The second fibers 3 are attached to the first fibers 2 while crossing the first fibers 2, for example.

[0042] As the polymer that can be made into a fiber, the second fibers 3 preferably contain at least one of polytetrafluoroethylene (hereinafter also referred to as PTFE), polypropylene (PP), polyethylene (PE), and polyamide (PA). The second fibers 3 of this embodiment contain PTFE as a main component. In other words, the second fibers 3 contain more than 50 wt % of PTFE based on the total weight of the second fibers 3. The second fibers 3 of this embodiment are ultrafine fibers of PTFE.

[0043] The PTFE used as the material for the second fiber 3 is, for example, high-molecular-weight PTFE obtained by emulsion polymerization or suspension polymerization of TFE. The high-molecular-weight PTFE may be at least one of modified PTFE and homo-PTFE. The modified PTFE includes, for example, TFE and a monomer other than TFE, such as a modified monomer. Generally, modified PTFE is uniformly modified with a modified monomer or modified at the initial or final stage of the polymerization reaction, but is not particularly limited thereto. The modified PTFE includes TFE units derived from TFE and modified monomer units derived from the modified monomer. The "modified monomer unit" referred to herein is a part of the molecular structure of the modified PTFE, derived from the modified monomer. The modified monomer is not particularly limited as long as it can be copolymerized with TFE.

[0044] The "high molecular weight" of high-molecular-weight PTFE as used herein refers to a molecular weight that is easily fiberized during the production of the fiber article 1, yields long fibrils, has a standard specific gravity (SSG) of 2.130 or more and 2.230 or less, and has a high melt viscosity so that it does not substantially melt flow. For details about fiberizable PTFE, see, for example, International Publication No. 2013 / 157647.

[0045] When the aqueous dispersion is used in the production of the textile article 1, it is preferable that the water contact angle θ2 immediately after a water droplet is dropped onto the surface of the textile article 1 be a relatively low value in order to increase the affinity of the textile article 1 for the aqueous dispersion. In this case, it is preferable that the water contact angle θ2 be a value in the same range as the water contact angle θ1, for example.

[0046] The water contact angles θ1 and θ2 can be measured, for example, by observing the surface of an object onto which a water droplet has been dropped from the side of the water droplet using a microscope. The water contact angles θ1 and θ2 can be calculated as the average of the measured values ​​when a water droplet is dropped onto the object and the contact angle is measured at five points using, for example, a commercially available contact angle meter (contact angle meter "DMs-401" manufactured by Kyowa Interface Science Co., Ltd.).

[0047] In the present embodiment, an example has been shown in which the water contact angles θ1 and θ2 are set to relatively low values ​​in order to increase the affinity of the first fibers 2 for the aqueous dispersion, but the water contact angles θ1 and θ2 may also be set to relatively high values ​​in accordance with the characteristics of the dispersion in which the resin granules 4 are dispersed. Furthermore, the dispersion containing the resin granules 4 in a dispersed state may be adjusted, for example, so that the contact angle with the surface of the first fibers 2 is low in order to increase the affinity for the first fibers 2. Furthermore, when the fiber article 1 is produced without using a dispersion, for example, by attaching powdered resin granules 4 to the first fibers 2, the water contact angles θ1 and θ2 can be set to somewhat arbitrary values.

[0048] As described above, the fiber article 1 includes a plurality of first fibers 2 and a plurality of second fibers 3 having an outer diameter D2 smaller than that of the first fibers 2 and supported by the plurality of first fibers 2 in a dispersed state, and has a basis weight of 60 g / m 2 More than 300g / m 2 The value is set to the range below. As a result, the fiber article 1 has a relatively low basis weight and contains abundant fiber gaps formed by the first fibers 2 and the second fibers 3. This makes it easier to reduce the weight of the fiber article 1.

[0049] Furthermore, the tensile strength of the fiber article 1 in the direction perpendicular to the thickness direction, in which the strength is smallest, is set to a value in the range of 0.8 N / 10 mm to 100 N / 10 mm. This improves the strength of the fiber article 1. Therefore, even if an external force acts on the fiber article 1 during use, the shape of the fiber article 1 can be maintained. Therefore, stable filtering performance of the fiber article 1 can be obtained.

[0050] Furthermore, when the fiber article 1 is manufactured so that the tensile strength in the minimum strength direction of the fiber article 1 is set to a value within the above range, the range of external forces that can be applied in the same direction to the fiber sheet during manufacturing of the fiber article 1 is improved. As a result, for example, by applying an external force to a plurality of first fibers 2, abundant fiber gaps can be formed in the fiber article 1. This makes it easier to reduce the weight of the fiber article 1. Furthermore, for example, when manufacturing the fiber article 1, if resin granules 4 containing a fiberizable polymer are attached to the first fibers 2 and an external force is applied to the resin granules 4 to form second fibers 3, it becomes easier to adjust the external force applied to the resin granules 4. This allows abundant second fibers 3 to be formed.

[0051] Furthermore, the fiber article 1 of this embodiment has a tensile elongation in the direction of minimum strength relative to its natural state in a range of 5% to 250%. This configuration can further improve the strength of the fiber article 1. Therefore, for example, even if an external force is applied to the fiber article 1 during use, the fibers 2 and 3 in the fiber article 1 can be prevented from breaking or being damaged. Furthermore, the fiber article 1 can be prevented from being destroyed.

[0052] Furthermore, the fiber article 1 of this embodiment has a thickness in the natural state of less than 3.0 mm, for example, which allows the fiber article 1 to be configured thinly, thereby enabling the fiber article 1 to be made even more compact.

[0053] Furthermore, since the fiber article 1 includes the first fibers 2 and the second fibers 3 having an outer diameter D2 smaller than that of the first fibers 2, the plurality of second fibers 3 can be supported by the plurality of first fibers 2 in a dispersed state. This prevents the second fibers 3 from being cut, and allows the plurality of second fibers 3 to be stably maintained by the plurality of first fibers 2. This improves the strength of the fiber article 1, and also improves filter performance by bringing the first fibers 2 and the second fibers 3 in the fiber article 1 into stable and efficient contact with a fluid during use.

[0054] Furthermore, by setting the outer diameter D1 of the first fibers 2, the outer diameter D2 of the second fibers 3, and the ratio D1 / D2 to the above values, it is possible to form an abundance of both relatively large fiber gaps formed by a plurality of first fibers 2 and relatively small fiber gaps formed by a plurality of second fibers 3 in the fiber article 1. This makes it possible to easily exhibit the respective functions of the first fibers 2 and the second fibers 3, which have a predetermined difference in outer diameter, with respect to the fluid flowing inside the fiber article 1, even when the thickness or basis weight of the fiber article 1 is relatively small, for example.

[0055] Furthermore, the second fibers 3, which are extremely thin and have an outer diameter D2 of 1.0 μm or less, are supported by the first fibers 2, which have a relatively large outer diameter D1. This allows the second fibers 3 to be stably supported while preventing breakage of the second fibers 3, even when the second fibers 3 are relatively long, to be supported by the first fibers 2. This makes it easier for the first fibers 2 and the second fibers 3 to exhibit their respective functions over a long period of time.

[0056] Furthermore, the outer diameter D1 of the fiber article 1 is set to a value in the range of 5.0 μm or more and 50.0 μm or less. This allows the first fibers 2 to be formed to have an appropriate thickness. The strength of the first fibers 2 can be further improved. Therefore, even if an external force acts on the fiber article 1 during use, the first fibers 2 and the second fibers 3 in the fiber article 1 can be prevented from being damaged. This allows the strength of the fiber article 1 to be improved so that the functions of the first fibers 2 and the second fibers 3 can be exerted over a long period of time, thereby achieving stable filter performance.

[0057] Furthermore, the outer diameter D1 of the fiber article 1 is set to a value in the range of 20.0 μm to 30.0 μm. By setting the outer diameter D1 of the first fibers 2 to such a value, the first fibers 2 can stably support the second fibers 3 while preventing the inter-fiber gaps of the fiber article 1 from becoming excessively large. Therefore, the strength of the fiber article 1 can be improved while excellent filtering performance can be obtained.

[0058] In addition, in the fiber article 1, as an example, the first fibers 2 are crimped. This makes the first fibers 2 bulkier than when they are uncrimped. This allows abundant fiber gaps formed by the multiple first fibers 2 to be arranged in the fiber article 1. This makes it easier to reduce the weight and compactness of the fiber article 1, and also makes it easier to bring the first fibers 2 and the second fibers 3 into contact with a fluid, thereby allowing the first fibers 2 and the second fibers 3 to more easily exhibit their respective functions.

[0059] Furthermore, the first fibers 2 of this embodiment contain at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate, which broadens the range of materials that can be selected for the first fibers 2. This allows for greater freedom in designing the fiber article 1.

[0060] Furthermore, in the fiber article 1 of this embodiment, the second fibers 3 contain a fiberizable polymer. By using such a polymer, the second fibers 3 can be efficiently produced, for example, by attaching a material containing the polymer to the first fibers 2 and fiberizing the polymer. Furthermore, the second fibers 3 of this embodiment contain at least one of polytetrafluoroethylene, polypropylene, polyethylene, and polyamide. This expands the range of materials that can be selected for the second fibers 3. This further improves the design freedom of the fiber article 1.

[0061] In addition, in the fiber article 1 of this embodiment, for example, the second fibers 3 contain polytetrafluoroethylene as a main component. The term "main component" as used herein refers to a component that accounts for more than 50% by weight of the second fibers 3. This allows the fiber article 1 to stably exhibit the functions of polytetrafluoroethylene.

[0062] The fiber article 1 of this embodiment also includes resin granules 4 attached to the first fibers 2 and having the same composition as the second fibers 3, and the ratio V1 / V2 of the total volume V1 of the first fibers 2 to the total volume V2 of the second fibers 3 and the resin granules 4 is set to a value in the range of 1.9 to 124.0. This allows the first fibers 2, which have a large outer diameter D1 and a large volume, to stably support the second fibers 3, which have a small outer diameter D2 and a small volume. This makes it easier for the second fibers 3 to perform their functions more stably. This allows the filter performance to be improved even in a fiber article 1 whose basis weight is set to a relatively small value.

[0063] Furthermore, the pressure loss of the fiber article 1 when air is passed through it in the thickness direction at a flow rate of 5.3 cm / sec is set to a value in the range of 3 Pa to 35 Pa. This prevents clogging of the fiber article 1 during use and allows fluid to circulate efficiently inside the fiber article 1. This prevents performance degradation associated with use of the fiber article 1. Furthermore, by suppressing the pressure loss of the fiber article 1 to a value in the above range, fluid can be brought into contact with the first fibers 2 and the second fibers 3 in the fiber gaps in the fiber article 1, making it easier for the first fibers 2 and the second fibers 3 to exhibit their respective functions.

[0064] Furthermore, the PF value of the fiber article 1 is set to, for example, a value in the range of 16 to 84. This allows the fiber article 1 to be lighter in weight and stronger while favorably adjusting the balance between collection efficiency and pressure loss. This allows the fiber article 1 to achieve excellent filtering performance. Below, other embodiments will be described, focusing on the differences from the first embodiment.

[0065] Second Embodiment Fig. 2 is a cross-sectional view of a fiber composite 10 according to a second embodiment. As shown in Fig. 2, the fiber composite 10 includes a first sheet 6, a second sheet 7, and a third sheet 8. The first sheet 6 and the second sheet 7 are the fiber article 1 of the first embodiment. The first sheet 6 and the second sheet 7 are disposed on top of each other. As an example, the first sheet 6 and the second sheet 7 have the same thickness, but may have different thicknesses.

[0066] The third sheet 8 is disposed between the first sheet 6 and the second sheet 7, overlapping the first sheet 6 and the second sheet 7. The third sheet 8 includes, for example, a nonwoven fabric. The third sheet 8 includes the same or a different material as the fiber article 1. The third sheet 8 of this embodiment may include at least one of resin fiber and pulp fiber. The fiber composite 10 has improved strength and bulkiness compared to the fiber article 1 alone, due to the overlapping arrangement of multiple sheets 6 to 8.

[0067] According to the above configuration, by using the first sheet 6 and the second sheet 7, which are the fiber article 1 of the first embodiment, a fiber composite 10 with improved strength can be obtained. Furthermore, by reducing the basis weight of the first sheet 6 and the second sheet 7, the fiber composite 10 can be made lighter. Furthermore, for example, by adjusting the thickness of at least one of the multiple sheets 6 to 8, the total thickness of the fiber composite 10 can be easily adjusted. This allows the fiber composite 10 to be made more compact.

[0068] The configuration of the fiber composite using the fiber article 1 is not limited to that of the second embodiment. For example, the fiber composite may have a configuration in which a third sheet is disposed on at least one of both thickness-wise sides of the first sheet 6. Furthermore, the fiber composite may have a configuration in which a plurality of first sheets and a plurality of third sheets are alternately disposed.

[0069] (Confirmation Test) Next, a confirmation test of the present disclosure will be described, but the present disclosure is not limited to the examples shown below. Example 1 of a fiber article 1 was produced under the following set conditions. Cellulose acetate fibers, which are multiple crimped short fibers with an outer diameter D1 of 20 μm, were used as the first fibers 2. PTFE fibers with an outer diameter D2 of 70 nm were used as the second fibers 3. The fiber articles 1 of Examples 1 to 7 were produced by varying various parameters, including basis weight and thickness. Furthermore, fiber articles of Comparative Examples 1 to 6 were produced for comparison with Examples 1 to 7. In the production of Examples 1 to 7, the second external force was applied to a fiber sheet, which was a production intermediate, whereas in the production of Comparative Examples 1 to 6, the second external force was not applied to the fiber sheet.

[0070] The basis weight and thickness of the fiber articles of Examples 1 to 7 and Comparative Examples 1 to 6 were measured. Furthermore, the pressure loss, collection efficiency (using NaCl particles with a particle diameter of 0.4 μm), and PF value of the fiber articles were measured based on the methods described in the embodiments. Furthermore, the tensile strength and elongation of the fiber articles in the direction of minimum strength (first direction) were measured based on the methods described in the embodiments. Furthermore, the tensile strength and elongation of the fiber articles in the orthogonal direction (second direction) perpendicular to the direction of minimum strength were measured. Furthermore, when manufacturing the fiber articles of Examples 1 to 7 and Comparative Examples 1 to 6, testers evaluated the ease of handling of the fiber articles during manufacturing. In this test, fiber articles with good handling performance, taking into consideration the transportation of the fiber articles during manufacturing, were rated as "A," and fiber articles with handling performance worse than "A" were rated as "B."

[0071] Furthermore, for the fiber articles of Examples 1 to 7 and Comparative Examples 1 to 6, the J-ePM1 filtering efficiency (%) was measured based on a method conforming to Item 7.2 "Calculation of particulate matter filtering efficiency (J-eMPx)" of the General Ventilation Filter Test (JIS B 9908-1:2019). For this measurement, particulate matter (PM1) used for testing was at least one of solid and liquid particles suspended in the atmosphere, with a 50% cutoff at an aerodynamic particle size of 1 μm using a classification device. The measurement results and evaluation results are shown in Tables 1 and 2. In Table 2, the calculated J-ePM1 filtering efficiency (%) is denoted as "ePM1 (%)."

[0072]

[0073]

[0074] In an example based on the test results shown in Tables 1 and 2, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 1.5 N / 10 mm or more and 100 N / 10 mm or less. In another example, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 9.9 N / 10 mm or more and 100 N / 10 mm or less. In yet another example, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 10.5 N / 10 mm or more and 100 N / 10 mm or less. In yet another example, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 10.8 N / 10 mm or more and 100 N / 10 mm or less. According to another embodiment, the tensile strength of the fiber article 1 in the direction of minimum strength is a value in the range of 0.8 N / 10 mm or more and 100 N / 10 mm or less.

[0075] Furthermore, according to an example based on the embodiment and the test results, it can be said that the elongation percentage of the fiber article 1 in the minimum strength direction is, for example, a value in the range of 24.1% or more and 250% or less. In another example, the elongation percentage of the fiber article 1 in the minimum strength direction is a value in the range of 28.4% or more and 250% or less. In yet another example, the elongation percentage of the fiber article 1 in the minimum strength direction is a value in the range of 99.7% or more and 250% or less. In yet another example, the elongation percentage of the fiber article 1 in the minimum strength direction is a value in the range of 120.7% or more and 250% or less. In yet another example, the elongation percentage of the fiber article 1 in the minimum strength direction is a value in the range of 171.8% or more and 250% or less.

[0076] As shown in Table 2, in Examples 1 to 7, the tensile strength of the fiber article 1 in the minimum strength direction was at least 0.8 N / 10 mm. Furthermore, in Examples 1 to 7, the elongation of the fiber article 1 in the minimum strength direction was at least 24.1%. In contrast, as shown in Table 1, the tensile strength and elongation in the minimum strength direction were unmeasurable in all of Comparative Examples 1 to 6. The tensile strength in the orthogonal direction of Comparative Examples 1 to 6 was 14.2 N / 10 mm, which was higher than the tensile strength in the orthogonal direction of Examples 1 to 4. However, the tensile strength in the minimum strength direction of Comparative Examples 1 to 6 was so small that it was unmeasurable. Therefore, it is considered that the overall strength of the fiber articles of Comparative Examples 1 to 6 was inferior to that of Examples 1 to 7. From the above results, it was confirmed that Examples 1 to 7 had improved strength compared to Comparative Examples 1 to 6.

[0077] According to the embodiment and the test results, the basis weight of the fiber article 1 is, for example, 60 g / m 2 More than 92g / m 2 In another example, the basis weight of the fiber article 1 is 60 g / m 2 More than 82g / m 2 In another example, the basis weight of the fiber article 1 is 60 g / m 2 70g / m or more 2 The values ​​are in the following ranges. As can be seen from Tables 1 and 2, in Examples 1 to 7, the basis weight is adjusted to a wider range of values ​​than in Comparative Examples 1 to 6, and the thickness is reduced compared to Comparative Examples 1 to 6. This confirms that in Examples 1 to 7, it is easier to achieve weight reduction and compactness compared to Comparative Examples 1 to 6.

[0078] Furthermore, as shown in Table 2, it was confirmed that in Examples 1 to 7, the fiber sheets transported through the fiber article manufacturing apparatus were less likely to become entangled in the apparatus and less likely to lose their shape, making them easy to handle during production. As a result, Examples 1 to 7 were rated "A" for ease of handling during production. As shown in Table 1, in contrast, in Comparative Examples 1 to 6, the fiber sheets were more likely to become entangled in the fiber article manufacturing apparatus and lose their shape compared to Examples 1 to 7, so they were not rated as easy to handle. As a result, Comparative Examples 1 to 6 were rated "B" for ease of handling during production. The above evaluation results also confirmed that Examples 1 to 7 had improved strength compared to Comparative Examples 1 to 6.

[0079] Furthermore, as shown in Table 2, all of Examples 1 to 7 had a J-ePM1 filtering efficiency (%) of 50% or more. Therefore, it was confirmed that Examples 1 to 7 correspond to the filter group classified as "JIS-ePM1" in Item 7.3 "Classification" of JIS B 9908-1:2019. This indicates that the fiber articles of the present disclosure are filters having high-quality filtering functions classified as "JIS-ePM1." Note that Comparative Examples 1 to 6 also had a J-ePM1 filtering efficiency (%) of 50% or more. However, as described above, it was confirmed that Comparative Examples 1 to 6 had lower performance than Examples 1 to 7 in other respects.

[0080] (Disclosure Items) Each of the following items is a disclosure of a preferred embodiment. [Item 1] A sheet of paper comprising a plurality of first fibers and a plurality of second fibers having an outer diameter smaller than that of the first fibers and supported by the plurality of first fibers in a dispersed state, the sheet of paper having a basis weight of 60 g / m 2 More than 300g / m 2 and the tensile strength in a strength minimum direction, in which the tensile strength is minimum, among directions perpendicular to the thickness direction, is a value in the range of 0.8 N / 10 mm or more and 100 N / 10 mm or less.

[0081] According to the above configuration, the fiber article has a relatively low basis weight and contains abundant fiber gaps formed by the first fibers and the second fibers. This facilitates weight reduction of the fiber article. Furthermore, the strength of the fiber article can be improved by setting the tensile strength in the minimum strength direction, which is perpendicular to the thickness direction, to a value within the above range. Therefore, for example, even if an external force acts on the fiber article during use, the shape of the fiber article can be maintained. Therefore, stable filtering performance of the fiber article can be obtained.

[0082] [Item 2] The fiber article according to item 1, wherein the tensile elongation in the direction of minimum strength relative to the natural state is a value in the range of 5% to 250%.

[0083] According to the above configuration, the strength of the fiber article can be further improved. Therefore, for example, even if an external force is applied to the fiber article during use, the first fibers and the second fibers in the fiber article can be prevented from being broken or damaged. Furthermore, the fiber article can be prevented from being destroyed.

[0084] [Item 3] The fiber article according to item 1 or 2, which has a thickness in its natural state of less than 3.0 mm.

[0085] According to the above configuration, the fiber article can be made thinner, which makes it possible to further reduce the size of the fiber article.

[0086] [Item 4] The fiber article according to any one of Items 1 to 3, wherein a ratio D1 / D2 of an outer diameter D1 of the first fibers to an outer diameter D2 of the second fibers is set to a value in the range of 15.0 to 1666.7, the outer diameter D1 is set to a value in the range of 5.0 μm to 50.0 μm, and the outer diameter D2 is set to a value in the range of 30.0 nm to 1.0 μm.

[0087] According to the above configuration, the ratio D1 / D2 can be increased while preventing the outer diameter D2 of the second fibers from becoming excessively small, thereby enabling a fibrous article containing a large number of second fibers to be stably produced.

[0088] [Item 5] The fiber article according to Item 4, wherein the outer diameter D1 is set to a value in the range of 20.0 μm or more and 30.0 μm or less.

[0089] According to the above configuration, the second fibers are stably supported by the first fibers, and a plurality of second fibers can be easily arranged abundantly around the first fibers.

[0090] [Item 6] The fiber article according to any one of Items 1 to 5, wherein the plurality of first fibers are crimped.

[0091] According to the above configuration, the first fibers are bulkier than in an uncrimped state, which allows for abundant fiber gaps formed by the plurality of first fibers to be arranged in the fiber article, thereby facilitating a reduction in the weight and size of the fiber article and allowing the first fibers and the second fibers to come into contact with a fluid, thereby further enhancing the functions of the first fibers and the second fibers.

[0092] [Item 7] The fiber article according to any one of Items 1 to 6, wherein the plurality of first fibers comprise at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate.

[0093] According to the above configuration, the range of materials that can be selected for the first fibers is widened, thereby improving the degree of freedom in designing fiber articles.

[0094] [Item 8] The fiber article according to any one of Items 1 to 7, wherein the plurality of second fibers include a fiberizable polymer.

[0095] According to the above configuration, for example, by attaching a material containing the polymer to the first fibers and fiberizing the polymer, the second fibers can be efficiently produced.

[0096] [Item 9] The fibrous article according to item 8, wherein the second fibers comprise at least one of polytetrafluoroethylene, polypropylene, polyethylene, and polyamide.

[0097] According to the above configuration, the range of materials that can be selected for the second fibers is expanded, thereby further improving the degree of freedom in designing fiber articles.

[0098] [Item 10] The fiber article according to any one of Items 1 to 9, further comprising resin granules attached to the first fibers and having the same composition as the second fibers, wherein a ratio V1 / V2 of a total volume V1 of the first fibers to a total volume V2 of the second fibers and the resin granules is set to a value in the range of 1.9 to 124.0.

[0099] According to the above configuration, the first fibers having a large outer diameter D1 and a large volume can stably support the second fibers having a small outer diameter D2 and a small volume, which allows the second fibers to more stably perform their functions, thereby improving the filtering performance even in a fibrous article having a relatively small basis weight.

[0100] [Item 11] The fiber article according to any one of Items 1 to 10, wherein the pressure loss when air is passed through the fiber in the thickness direction at a flow rate of 5.3 cm / sec is set to a value in the range of 3 Pa to 35 Pa.

[0101] According to the above configuration, clogging of the fiber article during use can be prevented, and fluid can be efficiently circulated inside the fiber article. Therefore, deterioration of performance due to use of the fiber article can be prevented. Furthermore, by suppressing the pressure loss of the fiber article to a value within the above range, fluid can be brought into contact with the first fibers and the second fibers in the fiber gaps in the fiber article, making it easier for the first fibers and the second fibers to exhibit their respective functions.

[0102] [Item 12] The fiber article according to any one of Items 1 to 11, which is classified into the JIS-ePM1 filter group in the classification described in Item 7.3 of JIS B 9908-1:2019.

[0103] According to the above configuration, the fiber article of the present disclosure can be used as a high-quality filter classified into the "JIS-ePM1" filter group.

[0104] [Item 13] The fiber article according to any one of Items 1 to 12, comprising: a first sheet and a second sheet disposed so as to overlap each other; and a third sheet disposed between the first sheet and the second sheet and so as to overlap the first sheet and the second sheet.

[0105] According to the above configuration, by using the first sheet and the second sheet, a fiber composite with improved strength can be obtained. Furthermore, since the basis weight of the first sheet and the second sheet is reduced, the weight of the fiber composite can be reduced. Furthermore, for example, by adjusting the thickness of at least one of the first to third sheets, the total thickness of the fiber composite can be easily adjusted. This allows the fiber composite to be made more compact.

[0106] Each configuration and their combinations in each embodiment are examples. Addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but only by the claims. Furthermore, each aspect disclosed herein can be combined with any other feature disclosed herein. The size of the fiber article 1 is not limited. Furthermore, the fiber article 1 may be used in a combination of multiple fiber articles 1.

[0107] REFERENCE SIGNS LIST 1 Fiber article 2 First fiber 3 Second fiber 4 Resin granules 6 First sheet 7 Second sheet 8 Third sheet 10 Fiber composite

Claims

1. A fabric comprising a plurality of first fibers and a plurality of second fibers having an outer diameter smaller than that of the first fibers and supported by the plurality of first fibers in a dispersed state, the fabric having a basis weight of 60 g / m 2 More than 300g / m 2 The tensile strength in a strength minimum direction, in which the tensile strength is smallest, among directions perpendicular to the thickness direction, is in the range of 0.8 N / 10 mm or more and 100 N / 10 mm or less.

2. The fiber article according to claim 1, wherein the tensile elongation in the direction of minimum strength relative to the natural state is in the range of 5% or more and 250% or less.

3. The fiber article according to claim 1, having a thickness in its natural state of less than 3.0 mm.

4. The fiber article according to claim 1, wherein the ratio D1 / D2 of the outer diameter D1 of the first fiber to the outer diameter D2 of the second fiber is set to a value in the range of 15.0 to 1666.7, the outer diameter D1 is set to a value in the range of 5.0 μm to 50.0 μm, and the outer diameter D2 is set to a value in the range of 30.0 nm to 1.0 μm.

5. The fiber article according to claim 4, wherein the outer diameter D1 is set to a value in the range of 20.0 μm or more and 30.0 μm or less.

6. The fiber article according to any one of claims 1 to 5, wherein the plurality of first fibers are crimped.

7. The fibrous article according to any one of claims 1 to 5, wherein the plurality of first fibers comprises at least one of rayon, polypropylene, polyethylene terephthalate, polyethylene, and cellulose acetate.

8. The fiber article according to any one of claims 1 to 5, wherein the plurality of second fibers comprises a fiberizable polymer.

9. The fibrous article of claim 8, wherein said second fibers comprise at least one of polytetrafluoroethylene, polypropylene, polyethylene, and polyamide.

10. A fiber article as described in any one of claims 1 to 5, further comprising resin granules attached to the first fibers and having a similar composition to the second fibers, wherein the ratio V1 / V2 of the total volume V1 of the first fibers to the total volume V2 of the second fibers and the resin granules combined is set to a value in the range of 1.9 or more and 124.0 or less.

11. A fiber article according to any one of claims 1 to 5, in which the pressure loss when air is passed through the fiber in the thickness direction at a flow rate of 5.3 cm / sec is set to a value in the range of 3 Pa or more and 35 Pa or less.

12. The textile article according to any one of claims 1 to 5, which is classified into the JIS-ePM1 filter group in the classification described in item 7.3 of JIS B 9908-1:2019.

13. A fiber composite, comprising the fiber article according to any one of claims 1 to 5, a first sheet and a second sheet arranged to overlap each other, and a third sheet arranged between the first sheet and the second sheet and overlapping the first sheet and the second sheet.

Citation Information

Patent Citations

  • Composition mainly composed of ptfe, mixed powder, molding material, filtering medium for filter, air filter unit, and porous membrane manufacturing method

    WO2013157647A1

  • Fiber article

    WO2021039980A1

  • Nonwoven fabric and method for manufacturing nonwoven fabric

    JP2012188774A

  • Method for producing fiber articles

    WO2021039979A1