Glycerogel stretchable electrode, glycerogel stretchable electrolyte, glycerogel stretchable supercapacitor comprising both, and manufacturing method therefor

Glycerogel-based stretchable electrodes and electrolytes address the mechanical and temperature stability issues in supercapacitors by providing strong adhesion and self-healing properties, ensuring stable performance from -20°C to 80°C, suitable for advanced energy storage applications.

WO2024228429A1PCT designated stage expired Publication Date: 2024-11-07IND FOUND OF CHONNAM NAT UNIV

Patent Information

Application Number
PCT/KR2023/013588
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2023-09-11
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current stretchable supercapacitors face issues with mechanical integrity between electrodes and electrolytes, leading to reduced cycle life, voltage drops, and short circuits due to poor interfacial connectivity and temperature instability, especially at extreme temperatures, which limits their performance in wearable and space exploration applications.

Method used

Development of glycerogel-based stretchable electrodes and electrolytes with excellent mechanical and electrical/ionic conductivity from -20°C to 80°C, fabricated through a method involving polymer and conductive polymer solutions, freeze-thaw cycles, and glycerol treatment, ensuring strong adhesion and self-healing properties.

Benefits of technology

The glycerogel stretchable supercapacitors demonstrate stable mechanical and electrochemical performance under extreme temperatures, preventing delamination and maintaining capacitance even after deformation, with high capacitance retention rates and long-term durability, making them suitable for next-generation energy storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023013588_07112024_PF_FP_ABST
    Figure KR2023013588_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a technology related to an electrode, an electrolyte and a supercapacitor that use a glycerogel, and, more specifically, relates to a glycerogel stretchable electrode, a glycerogel stretchable electrolyte, a glycerogel stretchable supercapacitor comprising both, and a manufacturing method therefor, the electrode, the electrolyte and the supercapacitor using a stretchable glycerogel newly developed so as to have excellent mechanical properties and electrical conductivity and / or ionic conductivity in temperature conditions from an ultra-low temperature of -20°C to a high temperature of 80°C.
Need to check novelty before this filing date? Find Prior Art

Description

Glycerogel stretchable electrode, glycerogel stretchable electrolyte, glycerogel stretchable supercapacitor including the same, and method for manufacturing the same

[0001] The present invention relates to technologies related to electrodes, electrolytes, and supercapacitors using glycerogel, and more specifically, to a glycerogel stretchable electrode, a glycerogel stretchable electrolyte, a glycerogel stretchable supercapacitor including these, and a method for manufacturing the same, using a newly developed stretchable glycerogel that has excellent mechanical properties as well as at least one of electrical conductivity and ionic conductivity under temperature conditions ranging from an ultra-low temperature of -20°C to a high temperature of 80°C.

[0002] The recent rapid growth of wearable and stretchable electronic devices necessitates the development of viable and durable energy storage devices. Among the various existing energy storage devices, supercapacitors have attracted considerable attention due to their superior power density, fast charging capability, excellent cycle stability, lightweight, and low cost. To meet the growing demand for stretchable electronic devices such as wearable health monitoring devices, electronic skin, electronic textiles, stretchable displays, and soft robots, the urgent need for stretchable supercapacitors (SSCs) has significantly increased.

[0003] Most SSCs consist of electrodes with pre-designed, stretchable configurations, such as spiral, cellular, wave, and bridge-island shapes, on polyimide, polyetherimide, and polydimethylsiloxane substrates. Unfortunately, the mechanical integrity of the electrodes and electrolyte in SSCs is compromised, resulting in reduced cycle life. To address this issue, fabricating supercapacitors based on inherently stretchable electrolytes and electrodes is essential. Much research has been conducted to develop hydrogel-based electrodes and electrolytes for SSC fabrication. However, in hydrogel-based SSCs, the electrodes and electrolyte are assembled separately in a sandwich configuration, making them prone to delamination and slippage under extreme strain. This structural imbalance results in poor interfacial connection between the electrodes and electrolyte, resulting in large voltage drops and device short-circuiting.

[0004] Furthermore, few studies have reported the inefficiency of hydrogel-based SSCs due to ion transport disruption at subzero temperatures. Similarly, these gels are unsuitable for SSCs because water evaporates from the gel, trapping ion transport within the device. Therefore, under extreme temperature conditions, hydrogel-based SSCs lose their mechanical stability (stretchability) and unique electrochemical properties.

[0005] Practical applications of stretchable materials require long-term stable performance and the ability to withstand deformation. New energy storage systems capable of withstanding extreme environmental temperatures, such as those experienced under diverse climatic conditions on Earth (e.g., the extreme cold experienced in Europe, North America, and some Asian countries) and human missions to the Moon and Mars for space exploration, require novel energy storage systems. Few attempts have been made to synthesize organo-hydrogel electrolytes to eliminate the temperature instability of pure hydrogel-based systems. Recently, ethylene glycol / dimethyl sulfoxide / aqueous organo-hydrogel electrolytes have been used in antifreeze SSCs because both DMSO and ethylene glycol disrupt the hydrogen bonding network, lowering the freezing point of pure water and inhibiting ice crystal growth. However, these gels cannot be used for extended periods at higher temperatures because the water dries out. The poor interfacial connection between the electrode and electrolyte at extreme temperatures remains unresolved due to asynchronous deformation and weak adhesion.

[0006] Based on numerous research results, the inventors of the present invention have developed a stretchable glycerogel (GG) having excellent mechanical properties as well as at least one of electrical conductivity and ionic conductivity under temperature conditions ranging from an ultra-low temperature of -20°C to a high temperature of 80°C, thereby completing the present invention.

[0007] Accordingly, the purpose of the present invention is to provide a glycerogel stretchable electrode and a glycerogel stretchable electrolyte having excellent mechanical properties and at least one of electrical conductivity and ionic conductivity under extreme temperature conditions such as an ultra-low temperature of -20°C as well as a high temperature of 80°C, and a method for manufacturing the same.

[0008] Another object of the present invention is to provide a glycerogel stretchable supercapacitor having strong electrochemical and mechanical behavior under extreme temperature conditions such as an ultra-low temperature of -20°C as well as a high temperature of 80°C, and a method for manufacturing the same, including a glycerogel stretchable electrode and a glycerogel stretchable electrolyte.

[0009] Another object of the present invention is to provide a glycerogel stretchable supercapacitor and a method for manufacturing the same, which can suppress drying and freezing problems associated with aqueous and polymer (hydrogel)-based electrolytes at high and sub-zero temperatures, has no delamination problems, and has mechanical robustness such that the capacitance does not change even after bending, twisting, and stretching.

[0010] Another object of the present invention is to provide various applications including next-generation extreme energy storage devices, soft robots, etc., in which glycerogel stretchable electrodes, electrolytes, and supercapacitors having excellent elasticity, electrical conductivity, and ionic conductivity are applied.

[0011] The purpose of the present invention is not limited to the purposes mentioned above, and even if not explicitly mentioned, the purpose of the invention that can be recognized by a person of ordinary skill in the art from the description of the detailed description of the invention described below may also be included.

[0012] In order to achieve the above-described object of the present invention, first, the present invention provides a method for manufacturing a glycerogel stretchable electrode, comprising the steps of: preparing a gel-forming polymer solution and a conductive polymer solution; mixing the gel-forming polymer solution and the conductive polymer solution and stirring them to prepare a mixed solution; filling the mixed solution into a mold of a desired shape; repeating at least one cycle of freezing and then thawing the mold filled with the mixed solution to form a gel; a first drying step of drying the formed gel in a vacuum; a first immersion step of immersing the dried gel in a glycerol-water solution; a second drying step of drying the gel in which glycerol and water have been absorbed at a temperature of less than 100°C; a second immersion step of immersing the gel that has undergone the second drying step in a metal salt-glycerol solution at a temperature lower than room temperature; and annealing the gel that has undergone the second immersion step and then cooling it to room temperature.

[0013] In a preferred embodiment, the gel-forming polymer solution is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), and the conductive polymer solution comprises at least one selected from the group consisting of polyacetylene, polypyrrole, polythiophene, poly(3,4-ethylene dioxythio-phene) (PEDOT), polyaniline, and poly(3,4-ethylenedioxythiophene:poly(styrenesulfonate) (PEDOT:PSS).

[0014] In a preferred embodiment, the mixed solution contains a gel-forming polymer:conductive polymer in a weight ratio of 2.5 to 4.5:0.5 to 2.

[0015] In a preferred embodiment, the gel-forming polymer included in the mixed solution is polyvinyl alcohol (PVA), the conductive polymer is PEDOT:PSS, and the solvent is a DMSO-water mixed solution.

[0016] In a preferred embodiment, in the freezing and thawing cycle, the freezing is performed by leaving the mold at -20°C or lower for 12 hours or longer, and the thawing is performed by leaving the frozen mold at 25°C or lower for 6 hours or shorter.

[0017] In a preferred embodiment, in the first immersion step, the glycerol-water solution contains glycerol:water in a weight ratio of 10 to 20: 80 to 90, and the immersion time is 12 hours or more.

[0018] In a preferred embodiment, in the second immersion step, the metal salt-glycerol solution contains metal salt:glycerol in a weight ratio of 15 to 25:75 to 85, and the immersion time is 12 hours or more.

[0019] In a preferred embodiment, the metal salt is any one selected from the group consisting of LiClO4, NaCl, and LiCl.

[0020] In a preferred embodiment, the annealing is performed at 100°C to 150°C for 10 hours or more.

[0021] In addition, the present invention provides a glycerogel stretchable electrode made of glycerogel containing 0.5 to 2 wt% of a conductive polymer.

[0022] In a preferred embodiment, the conductive polymer is at least one selected from the group consisting of polyacetylene, polypyrrole, polythiophene, poly(3,4-ethylene dioxythio -phene)(PEDOT), polyaniline, poly(3,4-ethylenedioxythiophene: poly(styrenesulfonate)(PEDOT:PSS), and the gel-forming polymer in the glycerogel is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), any one selected from the group consisting of cellulose.

[0023] In a preferred embodiment, the glycerogel comprises PEDOT:PSS as the electrically conductive polymer and polyvinyl alcohol (PVA) as the gel-forming polymer.

[0024] In a preferred embodiment, the Young's modulus is 0.78 ± 0.06 MPa, the tensile strength is 2.09 ± 0.35 MPa, and the strain at break is 232 ± 41%.

[0025] In a preferred embodiment, the electrical conductivity is 1089 ± 49 S m -1 am.

[0026] In a preferred embodiment, after exposure to temperature conditions of -20°C to 80°C for one week, the weight change is maintained within ±10 wt%.

[0027] In addition, the present invention provides a method for producing a glycerogel stretchable electrolyte, comprising the steps of: preparing a polymer solution for gel formation; filling a mold of a desired shape with the polymer solution for gel formation; freezing and then thawing the mold filled with the polymer solution for gel formation to form a gel; equilibrating the formed gel in water to obtain a hydrogel; sequentially immersing the hydrogel in glycerol aqueous solutions having different concentrations one or more times to obtain a glycerogel in which water molecules of the hydrogel are replaced with glycerol; and immersing the glycerogel in a metal salt-glycerol solution.

[0028] In a preferred embodiment, the gel-forming polymer solution is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), and comprises one selected from the group consisting of cellulose, and a mixed solution containing DMSO:water in a weight ratio of 50-90:10-50 as a solvent.

[0029] In a preferred embodiment, in the step of obtaining the glycerogel, when the hydrogel is immersed in a glycerol aqueous solution twice or more, the glycerol concentration of the subsequent glycerol aqueous solution is higher than that of the preceding glycerol aqueous solution.

[0030] In a preferred embodiment, the metal salt-glycerol solution contains metal salt:glycerol in a weight ratio of 15 to 25:75 to 85, and the metal salt is any one selected from the group consisting of LiClO4, NaCl, and LiCl.

[0031] In addition, the present invention provides a glycerogel stretchable electrolyte composed of glycerogel containing 15 to 25 wt% of an ion conductive material.

[0032] In a preferred embodiment, the ion conductive material is a metal salt selected from the group consisting of LiClO4, NaCl, and LiCl, and the gel-forming polymer in the glycerogel is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), any one selected from the group consisting of cellulose.

[0033] In a preferred embodiment, the ionic conductivity is 0.18 ± 0.021 S / m at 80°C, 0.034 ± 0.0029 S / m at room temperature, and 0.0032 ± 0.00013 S / m at -20°C.

[0034] In a preferred embodiment, the weight change is maintained within 10 wt% after exposure to temperature conditions of -20°C to 80°C for one week.

[0035] In a preferred embodiment, the mechanical properties remain similar to the initial room temperature behavior after exposure to temperature conditions of -20°C to 80°C for one week.

[0036] In addition, the present invention provides a method for manufacturing a glycerogel stretchable supercapacitor, comprising the steps of: preparing two glycerogel stretchable electrodes by any one of the methods described above; preparing a glycerogel stretchable electrolyte by any one of the methods described above; forming a laminate by laminating the prepared two glycerogel stretchable electrodes and the glycerogel stretchable electrolyte, wherein the electrolyte is disposed between the two electrodes; and a self-healing step in which the two electrodes forming the laminate and the electrolyte are bonded to each other to form a stable adhesive interface.

[0037] In a preferred embodiment, the self-healing step is performed by including a heating step of treating the laminate at 80°C to 120°C for 30 to 90 minutes and a cooling step of leaving the laminate subjected to the heating step at room temperature for 10 hours or more.

[0038] In addition, the present invention provides a glycerogel stretchable supercapacitor comprising: a glycerogel stretchable first electrode; a glycerogel stretchable electrolyte having an upper surface of the glycerogel stretchable first electrode and a lower surface thereof bonded thereto; and a glycerogel stretchable electrode having a lower surface thereof bonded to an upper surface of the glycerogel stretchable electrolyte; wherein a first adhesive interface formed between the upper surface of the first electrode and the lower surface of the electrolyte and a second adhesive interface formed between the upper surface of the electrolyte and the lower surface of the second electrode are formed by interpenetration of polymer chains included in the first electrode, the electrolyte, and the second electrode.

[0039] In a preferred embodiment, the first electrode and the second electrode are glycerogel stretchable electrodes manufactured by any one of the methods described above or any one of the glycerogel stretchable electrodes described above, and the electrolyte is a glycerogel stretchable electrolyte manufactured by any one of the methods described above or any one of the glycerogel stretchable electrolytes described above.

[0040] In a preferred embodiment, 26.27 mF cm at room temperature and 0.1 mA. -2 It has a capacitance of .

[0041] In a preferred embodiment, when the current increases 20-fold from 0.1 mA to 2 mA, the retention rate of the capacitance is 85% or more.

[0042] In a preferred embodiment, when the current increases 50-fold from 0.1 mA to 5 mA, the retention rate of the capacitance is 50% or more.

[0043] In a preferred embodiment, the retention rate of electrostatic capacity after being left at 80°C and -20°C for 7 days is 90% or more, respectively.

[0044] In a preferred embodiment, the capacitance retention rate after 10,000 charge / discharge cycles is 80% or more at 1.2 V and 90% or more at 0.8 V.

[0045] In a preferred embodiment, it stretches and recovers intact at temperatures from -20 to 80°C.

[0046] The glycerogel stretchable electrode and glycerogel stretchable electrolyte of the present invention described above have excellent mechanical properties and at least one of electrical conductivity and ionic conductivity under extreme temperature conditions such as an ultra-low temperature of -20°C as well as a high temperature of 80°C.

[0047] In addition, the supercapacitor of the present invention has strong electrochemical and mechanical behavior under extreme temperature conditions such as ultra-low temperature of -20℃ as well as high temperature of 80℃ by including glycerogel stretchable electrode and glycerogel stretchable electrolyte, so that it can suppress drying and freezing problems associated with aqueous and polymer (hydrogel)-based electrolytes at high and sub-zero temperatures, does not cause peeling problems, and has mechanical robustness that the capacitance does not change even after bending, twisting, and stretching.

[0048] Therefore, the glycerogel stretchable electrode and glycerogel stretchable electrolyte of the present invention, as well as the glycerogel stretchable supercapacitor, can meet the extreme resistance required for stringent next-generation applications, and thus can be used to fabricate various extreme resistance, flexibility, and stretchable devices for bio, electric / electronic, and soft robotic applications.

[0049] These technical effects of the present invention are not limited to the scope mentioned above, and effects of the invention that can be recognized by a person having ordinary skill in the art from the description of specific contents for implementing the invention described below, even if not explicitly mentioned, are also naturally included.

[0050] FIG. 1a is a schematic diagram of a conventional manufacturing technique for a supercapacitor in which an electrode and an electrolyte are sealed under pressure to achieve a sandwich-type supercapacitor, and FIG. 1b illustrates a design strategy for a glycerogel stretchable supercapacitor, namely an all-glycerogel stretchable supercapacitor (AGG-SSC), by laminating a glycerogel stretchable electrode and a glycerogel stretchable electrolyte in a sandwich structure according to various embodiments of the present invention.

[0051] FIGS. 2A to 2E are graphs showing typical tensile stress-strain curves, Young's modulus, tensile strength, strain at break, and conductivity of PVA-PEDOT:PSS(xy) glycerogels prepared according to various embodiments of the present invention, respectively, and FIGS. 2F to 2K are graphs showing the results of measuring the characteristics of PVA-PEDOT:PSS GG electrodes prepared according to various embodiments of the present invention after leaving them at -20°C, 25°C, and 80°C for 7 days, where FIG. 2F shows the weight change ratio, FIG. 2G shows the conductivity, FIG. 2H shows the stress, and FIG. 2I shows the resistance change of the electrode as the strain increases at 25°C. FIG. 2j shows the results of measuring (a) Young's modulus, (b) tensile strength, (d) strain at break, and (c) conductivity of PVA-PEDOT:PSS(4-1.5) glycerogel prepared by leaving it at -20°C, 25°C, and 80°C for 7 days, and FIG. 2k shows the results of measuring the conductivity and strain at break of a PVA-PEDOT:PSS(4-1.5) glycerogel electrode according to an embodiment of the present invention and a recently reported conductive polymer-based hydrogel.

[0052] FIG. 3a shows the change in properties of the PVA GG electrolyte according to various concentrations of PVA, namely (a) Young's modulus, (b) tensile strength, (c) fracture strain, (d) and ionic conductivity, and FIG. 3b shows the change in properties of the PVA GG electrolyte according to various concentrations of salt (LiClO4), namely (a) Young's modulus, (b) tensile strength, (c) fracture strain, (d) and ionic conductivity, and FIGS. 3c to 3f show the results of measuring the properties of the PVA GG electrolyte prepared according to various embodiments of the present invention after leaving it at -20°C, 25°C and 80°C for 7 days, where FIG. 3c shows the weight change ratio, FIG. 3d shows the conductivity, FIG. 3e shows the stress, and FIG. 3f shows the results of measuring the resistance change of the electrolyte as the strain increases at 25°C. Figure 3g shows the results of comparing (a) Young's modulus, (b) tensile strength, and (c) strain at break of PVA GG electrolyte before and after exposure to -20°C, 25°C, and 80°C for 7 days, and Figure 3h shows the Nyquist EIS plot of PVA GG electrolyte at various temperatures. Figures 3i and 3j show the Nyquist EIS plot and tensile stress-strain curve, respectively, of PVA GG electrolyte prepared by direct equilibration hydrogel in 100% glycerol containing 20% ​​LiClO4 (w / w).

[0053] FIG. 4a is a schematic diagram showing the thermally mediated self-healing mechanism and healing properties between a PVA-PEDOT:PSS electrode and a PVA electrolyte prepared according to various embodiments of the present invention, FIG. 4b is a lap shear test to determine the bonding strength, and FIG. 4c is a microscope and SEM image of the self-healing interface of a PVA GG electrolyte and a PVA-PEDOT:PSS GG electrode.

[0054] FIGS. 5A to 5D illustrate the electrical characteristics of an AGG-SSC (All-glycerogel stretchable supercapacitor) prepared according to various embodiments of the present invention, measured at 25°C. FIG. 5A is a cyclic voltammetry curve from 1 mV / s to 100 mV / s, FIG. 5B is a galvanostatic charge-discharge curve from 0.1 mA to 5 mA at 25°C and a Nyquist plot at 25°C, FIG. 5C shows the cycle performance up to 10,000 cycles at 1.2 V and 0.8 V, and FIG. 5D shows an area Ragone plot of the AGG-SSC compared to other reported supercapacitors. FIG. 5E shows (a) the capacitance contribution at different scan rates of the AGG-SSC and (b) the areal capacitance variation as a function of current.

[0055] FIGS. 6A to 6G are results of measuring the performance of AGG-SSC prepared according to various embodiments of the present invention under various conditions, wherein FIG. 6A shows a CV curve in a state of being stretched up to 100%, FIG. 6B shows a CV curve in a state of being bent and twisted, FIGS. 6C and 6D are CV curves at a scan rate of 10 mV / s and GCD at a current of 1 mA of the AGG-SSC at -20°C, 25°C, and 80°C, respectively, and FIG. 6E shows the retention of capacitance after being left for 7 days at -20°C, 25°C, and 80°C, and FIG. 6F shows LED lighting using the AGG-SSC under stretching and relaxation conditions at -20°C and 80°C, and FIG. 6G shows CV and GCD curves of parallel and series connections.

[0056] FIG. 7 is a GCD profile measured for a 1 mA current at room temperature in a mechanically deformed state of an AGG-SSC prepared according to various embodiments of the present invention, where a is a 100% elongated state and b is a bent and twisted state.

[0057] FIGS. 8A to 8F are CV and GCD plots measured after AGG-SSC prepared according to various embodiments of the present invention was left at -20°C, 25°C, and 80°C for 7 days. FIGS. 8A and B show the results after leaving at 25°C, FIGS. 8C and D show the results after leaving at 80°C, and FIGS. 8E and F show the results after leaving at -20°C.

[0058] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, it should be understood that the terms "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the description of the invention, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0059] While terms like "first" and "second" may be used to describe various components, these components should not be limited by these terms. These terms are used solely to distinguish one component from another. For example, without departing from the scope of the present invention, a first component could be referred to as a "second component," and similarly, a second component could also be referred to as a "first component."

[0060] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and shall not be interpreted in an idealized or overly formal sense unless explicitly defined herein.

[0061] When interpreting components, even if there is no explicit description, they are interpreted as including the tolerance range. In particular, when terms such as "about" or "substantially" are used, they may be interpreted as meaning at or near that value when manufacturing and material tolerances inherent to the meaning stated are provided.

[0062] When describing a temporal relationship, for example, when the temporal continuity is described as ‘after’, ‘following’, ‘next to’, ‘before’, etc., it also includes cases where it is not continuous, unless ‘right away’ or ‘directly’ is used.

[0063] Hereinafter, the technical configuration of the present invention will be described in detail with reference to the attached drawings and preferred embodiments.

[0064] However, the present invention is not limited to the embodiments described herein and may be embodied in other forms. The same reference numbers used to describe the present invention throughout the specification represent the same components.

[0065] The technical features of the present invention are a glycerogel stretchable electrode made of glycerogel having excellent mechanical properties and at least one of electrical conductivity and ionic conductivity under extreme temperature conditions such as an ultra-low temperature of -20°C as well as a high temperature of 80°C, a glycerogel stretchable electrolyte, and a glycerogel stretchable supercapacitor including these, which has strong electrochemical and mechanical behavior under extreme temperature conditions such as an ultra-low temperature of -20°C as well as a high temperature of 80°C, and thus does not cause drying and freezing problems as well as peeling problems at high temperatures and sub-zero temperatures, and has mechanical robustness in which the capacitance does not change even after bending, twisting, and stretching, and a method for manufacturing the same.

[0066] As is well known, in order to realize stretchable supercapacitors (SSCs) under all kinds of environmental conditions (low temperature, room temperature, and high temperature), the electrodes and electrolytes must be stretchable at different temperatures, have strong adhesion and shape recovery properties at the electrode / electrolyte interface to prevent slippage and peeling during stretching, and the electrodes and electrolytes must have anti-freezing and anti-drying properties to provide stable electrical energy at low and high temperatures. However, the problem of poor interfacial connection between electrodes and electrolytes at extreme temperatures remains unresolved due to asynchronous deformation and weak adhesion.

[0067] Accordingly, the method for manufacturing a glycerogel stretchable electrode of the present invention comprises the steps of: preparing a gel-forming polymer solution and a conductive polymer solution; mixing the gel-forming polymer solution and the conductive polymer solution and stirring them to prepare a mixed solution; filling the mixed solution into a mold of a desired shape; repeating a cycle of freezing and then thawing the mold filled with the mixed solution at least once to form a gel; a first drying step of drying the formed gel in a vacuum; a first immersion step of immersing the dried gel in a glycerol-water solution; a second drying step of drying the gel in which glycerol and water have been absorbed at a temperature of less than 100°C; a second immersion step of immersing the gel that has undergone the second drying step in a metal salt-glycerol solution at a temperature lower than room temperature; and annealing the gel that has undergone the second immersion step and then cooling it to room temperature.

[0068] Here, the polymer solution for gel formation can be formed by dissolving a polymer capable of forming a hydrogel in water or a mixed solvent of water and an organic solvent. As an example, the solvent can be Dimethyl sulfoxide (DMSO) or a mixed solvent in which an organic solvent having properties similar to DMSO and water are mixed at a certain ratio, and the polymer can be polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), which may be any one selected from the group consisting of cellulose.

[0069] The conductive polymer solution can be formed by dissolving one or more conductive polymers in water or a mixed solvent of water and an organic solvent. As an example, the solvent can be Dimethyl sulfoxide (DMSO) or a mixed solvent in which an organic solvent having properties similar to DMSO and water are mixed at a certain ratio, and the conductive polymer can be a substance having high electrical conductivity and dissolving in water or a mixed solvent of water and an organic solvent. As an example, the conductive polymer solution can be any one or more selected from the group consisting of polyacetylene, polypyrrole, polythiophene, poly(3,4-ethylene dioxythiophene) (PEDOT), polyaniline, and poly(3,4-ethylenedioxy thiophene:poly(styrenesulfonate)(PEDOT:PSS).

[0070] Since the mixed solution is formed by mixing and stirring the gel-forming polymer solution and the conductive polymer solution, the solvent of the gel-forming polymer solution and the solvent of the conductive polymer solution may be the same for uniform mixing, and the gel-forming polymer: conductive polymer may be included in a weight ratio of 2.5 to 4.5: 0.5 to 2, and of course, a solvent may be added to adjust the concentration if necessary. The concentration ratio of the gel-forming polymer: conductive polymer in the mixed solution was determined through experiments as described below. When the concentration of the gel-forming polymer was fixed at 2.5 to 4.5 wt%, the electrical conductivity increased as the concentration of the conductive polymer increased, and when the concentration of the conductive polymer was fixed, the mechanical properties tended to increase as the concentration of the gel-forming polymer increased.

[0071] As an example of implementation, the gel-forming polymer included in the mixed solution may be polyvinyl alcohol (PVA), the conductive polymer may be PEDOT:PSS, and the solvent may be a DMSO-water mixed solution, as in the examples described below. In this case, DMSO:water may be included in a ratio of 50:50 to 75:25.

[0072] In the freezing and thawing cycle in the gel forming step, freezing may be performed by leaving the mold at -20°C or lower for 12 hours or longer, and thawing may be performed by leaving the frozen mold at 25°C or lower for 6 hours or shorter. The freezing temperature is not limited as long as it is -20°C or lower, but may be performed up to -50°C considering the freezing time and gel properties, and thawing may be performed at 25°C or lower considering the thawing time.

[0073] In the first immersion step, the glycerol-water solution contains glycerol:water in a weight ratio of 10 to 20: 80 to 90, and the immersion time may be 12 hours or more. In one embodiment, when glycerol:water is contained in a weight ratio of 15:85, the immersion time may be performed for 24 hours.

[0074] In the second immersion step, the metal salt-glycerol solution contains metal salt:glycerol in a weight ratio of 15 to 25:75 to 85, and the immersion time may be 12 hours or more. In one embodiment, when the metal salt:glycerol is contained in a weight ratio of 20:80, the immersion time may be performed at 25°C or lower for 24 hours.

[0075] The metal salt may be a substance having high ionic conductivity and soluble in water or a mixture of water and an organic solvent, and as an example, may be any one selected from the group consisting of LiClO4, NaCl, and LiCl.

[0076] Annealing can be performed at 100°C to 150°C for more than 10 hours. If it is less than 100°C, the material still has conductive properties, but there is a problem that mechanical properties decrease when stored for a long period of time. If it is more than 150°C, the material may dry out during long-term annealing, and the mechanical properties of the material may decrease.

[0077] Next, the glycerogel stretchable electrode of the present invention is made of glycerogel containing 0.5 to 2 wt% of a conductive polymer.

[0078] Here, the conductive polymer may be a material having high electrical conductivity and soluble in water or a mixture of water and an organic solvent, and examples thereof include polyacrylamide (PAAm), polyvinyl alcohol (PVA), and poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe). 3+ ), may be at least one selected from the group consisting of cellulose. The gel-forming polymer included in the glycerogel is a polymer that can form a hydrogel by dissolving in water or a mixed solvent of water and an organic solvent, and may be polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), which may be any one selected from the group consisting of cellulose.

[0079] In particular, a glycerogel stretchable electrode composed of glycerogel containing PEDOT:PSS as an electrically conductive polymer and polyvinyl alcohol (PVA) as a gel-forming polymer has excellent mechanical properties such as Young's modulus of 0.78 ± 0.06 MPa, tensile strength of 2.09 ± 0.35 MPa, and strain at break of 232 ± 41%, and electrical conductivity of 1089 ± 49 S m -1 It has excellent electrochemical properties as well as extreme resistance in which the weight change is maintained within ±10 wt% after exposure to temperature conditions of -20 ℃ to 80 ℃ for one week.

[0080] The glycerogel stretchable electrode of the present invention having these characteristics can be obtained in a simple manner by the above-described method for manufacturing a glycerogel stretchable electrode.

[0081] Next, the method for manufacturing a glycerogel stretchable electrolyte of the present invention comprises the steps of: preparing a polymer solution for gel formation; filling a mold of a desired shape with the polymer solution for gel formation; freezing and then thawing the mold filled with the polymer solution for gel formation to form a gel; equilibrating the formed gel in water to obtain a hydrogel; sequentially immersing the hydrogel in glycerol aqueous solutions having different concentrations one or more times to obtain a glycerogel in which water molecules of the hydrogel are replaced with glycerol; and immersing the glycerogel in a metal salt-glycerol solution.

[0082] Here, the polymer solution for gel formation can be formed by dissolving a polymer capable of forming a hydrogel in water or a mixed solvent of water and an organic solvent. As an example, the solvent can be a mixed solvent in which an organic solvent having properties similar to DMSO and water are mixed at a certain ratio, and a mixed solution containing DMSO:water in a weight ratio of 50 to 90:10-50, preferably 75:25, can be used, and the polymer for gel formation is a polymer capable of forming a hydrogel by dissolving in water or a mixed solvent of water and an organic solvent, such as polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), which may be any one selected from the group consisting of cellulose.

[0083] In the step of obtaining a glycerogel, if the hydrogel is immersed in a glycerol aqueous solution more than twice, the glycerol concentration of the subsequent glycerol aqueous solution may be higher than that of the preceding glycerol aqueous solution. The immersion time may be 10 hours or more.

[0084] The metal salt-glycerol solution contains metal salt:glycerol in a weight ratio of 15 to 25:75 to 85, and the immersion time can be 12 hours or more. In one embodiment, when the metal salt:glycerol is contained in a weight ratio of 20:80, the immersion time can be performed for 24 hours.

[0085] The metal salt may be a substance having high ionic conductivity and soluble in water or a mixture of water and an organic solvent, and as an example, may be any one selected from the group consisting of LiClO4, NaCl, and LiCl.

[0086] Next, the glycerogel stretchable electrolyte of the present invention may be composed of glycerogel containing 15 to 25 wt% of an ion conductive material.

[0087] Here, the ionic conductive material may be a material having high ionic conductivity and soluble in water or a mixture of water and an organic solvent, and may be a metal salt as an example. In addition, the metal salt may be any one selected from the group consisting of LiClO4, NaCl, and LiCl.

[0088] In the above glycerogel, the gel-forming polymer is a polymer that can be dissolved in water or a mixed solvent of water and an organic solvent to form a hydrogel, and as an exemplary embodiment, polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), which may be any one selected from the group consisting of cellulose.

[0089] In particular, a glycerogel stretchable electrolyte composed of glycerogel containing LiClO4 as an ion-conducting material and polyvinyl alcohol (PVA) as a gel-forming polymer has ionic conductivities of 0.18 ± 0.021 S / m at 80°C, 0.034 ± 0.0029 S / m at room temperature, and 0.0032 ± 0.00013 S / m at -20°C, mechanical properties that are maintained similar to the initial room temperature behavior even after exposure to temperature conditions of -20°C to 80°C for one week, and extreme resistance in which a weight change is maintained within 10 wt% after exposure to temperature conditions of -20°C to 80°C for one week.

[0090] The glycerogel stretchable electrolyte of the present invention having these characteristics can be obtained in a simple manner by the above-described method for producing a glycerogel stretchable electrolyte.

[0091] Next, the method for manufacturing a glycerogel stretchable supercapacitor of the present invention may include the steps of: preparing two glycerogel stretchable electrodes by the method of any one of claims 1 to 9; preparing a glycerogel stretchable electrolyte by the method of any one of claims 16 to 19; forming a laminate by laminating the prepared two glycerogel stretchable electrodes and the glycerogel stretchable electrolyte, wherein the electrolyte is disposed between the two electrodes; and a self-healing step in which the two electrodes forming the laminate and the electrolyte are bonded to each other to form a stable adhesive interface.

[0092] Here, since the detailed description for the preparation of the glycerogel stretchable electrode and the glycerogel stretchable electrolyte has been described above, only the non-overlapping parts will be reviewed.

[0093] The glycerogel stretchable electrodes and glycerogel stretchable electrolytes prepared as described above can be prepared with the same size and the same or different thicknesses, as needed. They can be cut to a desired size from the outset and used. However, as described below, they can also be cut to the required size after completing the glycerogel stretchable supercapacitor.

[0094] The step of forming a laminate can be formed by placing one of the two prepared glycerogel stretchable electrodes parallel to the ground and then placing it so that the glycerogel stretchable electrolyte is in contact with its upper surface, and placing the remaining glycerogel stretchable electrode so that it is in contact with the upper surface of the glycerogel stretchable electrolyte.

[0095] The self-healing step can be performed by including a heating step in which the laminate is treated at 80°C to 120°C for 30 to 90 minutes, and a cooling step in which the laminate subjected to the heating step is left at room temperature for 10 hours or more. As illustrated in Fig. 4a, in the heating step, due to the presence of metal salt (e.g., LiClO4) ions, physical cross-linking within the polymer chains is weakened at high temperatures, softening the gel, resulting in polymer chain interpenetration at the electrode and electrolyte interface. In the cooling step, gel-forming polymer chains (e.g., PVA chains) reorganize and reassemble while exchanging H bonds at the electrode and electrolyte interface, thereby inducing strong self-healing, so that two elastic glycerogels and a glycerogel elastic electrolyte disposed therebetween can be bonded to each other with strong adhesive strength.

[0096] If necessary, a further step of cutting the obtained glycerogel stretchable supercapacitor into a desired size can be performed.

[0097] Therefore, according to the method for manufacturing a glycerogel stretchable supercapacitor of the present invention, the inherent elasticity of the electrode and electrolyte can reduce additional costs and inconveniences associated with manufacturing. That is, the interfacial adhesion between the electrode and electrolyte was not damaged due to efficient self-healing, and the manufactured glycerogel stretchable supercapacitor exhibited stable electrochemical behavior under extreme and strain conditions.

[0098] Next, the glycerogel stretchable supercapacitor of the present invention comprises: a glycerogel stretchable first electrode; a glycerogel stretchable electrolyte having an upper surface and a lower surface of the glycerogel stretchable first electrode bonded to each other; and a glycerogel stretchable electrode having a lower surface bonded to the upper surface of the glycerogel stretchable electrolyte; wherein a first adhesive interface formed between the upper surface of the first electrode and the lower surface of the electrolyte and a second adhesive interface formed between the upper surface of the electrolyte and the lower surface of the second electrode may be formed by interpenetration of polymer chains included in the first electrode, the electrolyte, and the second electrode.

[0099] Here, the first electrode and the second electrode may be a glycerogel stretchable electrode manufactured by the method of any one of claims 1 to 9 or a glycerogel stretchable electrode manufactured by any one of claims 10 to 15, and the electrolyte may be a glycerogel stretchable electrolyte manufactured by the method of any one of claims 16 to 19 or a glycerogel stretchable electrolyte manufactured by any one of claims 20 to 24.

[0100] As an embodiment of the glycerogel stretchable supercapacitor of the present invention, the glycerogel stretchable electrode is made of glycerogel containing PEDOT:PSS as an electrically conductive polymer and polyvinyl alcohol (PVA) as a gel-forming polymer, and when the glycerogel stretchable electrolyte is made of glycerogel containing LiClO4 as an ion-conducting material and polyvinyl alcohol (PVA) as a gel-forming polymer, the glycerogel stretchable supercapacitor has a capacity of 26.27 mF cm at room temperature and 0.1 mA. -2It was able to exhibit the capacitance of. Here, when the current increased 20 times from 0.1 mA to 2 mA, the retention rate of the capacitance was 85% or more, and when the current increased 50 times from 0.1 mA to 5 mA, the retention rate of the capacitance was 50% or more. In addition, the retention rates of the capacitance were 90% or more after being left for 7 days at 80°C and -20°C, and the retention rates of the capacitance were 80% or more at 1.2 V and 90% or more at 0.8 V after 10,000 charge / discharge cycles, and it exhibited extreme resistance that stretched and recovered without being damaged at -20 to 80°C.

[0101] Thus, the glycerogel stretchable supercapacitor of the present invention has extreme resistance to sub-zero and high temperature conditions for a very long time, and exhibits very stable electrochemical performance even in a mechanically deformed state. In addition, the electrode has a 1,089 Sm -1 Because it has a reasonably high electrical conductivity, no additional packaging, such as using an additional substrate and current collector, was required.

[0102] The glycerogel stretchable supercapacitor of the present invention having these characteristics can be obtained in a simple manner by the above-described method for manufacturing a glycerogel stretchable supercapacitor.

[0103] As can be seen from the experimental examples described below, the glycerogel stretchable supercapacitor according to the present invention has excellent capacitance and can operate over a wide temperature range, and has long-term electrochemical stability, mechanical durability, and flexibility, so it has high potential for use as a power source for driving wearable and stretchable electronic devices.

[0104] Using the materials described below, glycerogel stretchable electrodes, glycerogel stretchable electrolytes, and glycerogel stretchable supercapacitors according to various examples and comparative examples of the present invention were manufactured, and the characteristics of the manufactured electrodes, electrolytes, and supercapacitors were confirmed using the experimental methods described below.

[0105] 1. Materials

[0106] Poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate) (PEDOT:PSS) dry redispersible pellets and poly(vinyl alcohol) (PVA) (Mw 89,000–98,000, 99+% hydrolyzed) were purchased from Sigma-Aldrich (Belgium). Lithium perchlorate anhydrous (99%) was purchased from Thermo Scientific (USA). Glycerol (99%) was purchased from Samchun Pure Chemicals & Metals Co., Ltd (South Korea). Dimethyl sulfoxide (>99.5%) was purchased from Daejung Chemicals & Metals Co., Ltd (South Korea). Carbon nanotube films were purchased from Chengdu Organic Chemicals Co., Ltd., Chinese Academy of Sciences (China). All chemicals were used as received without further purification. Ultrapure deionized water was used as needed in all experiments.

[0107] 2. Experimental method

[0108] (1) Mechanical properties

[0109] The mechanical properties were performed using a universal testing machine (TEST ONE TO-100-1C, Republic of Korea) with a 10 kgf load cell under ambient conditions (humidity: 30%-60%, temperature: ~25°C). For tensile tests, the fabricated PVA-PEDOT:PSS glycerogel (GG) electrodes and PVA GG electrolyte were cut into dumbbell-shaped samples with cross-sections of ~3 mm x (0.2-0.4) mm and ~3 mm x 0.5 mm at the midsection, respectively. The specimens were clamped in the universal testing machine with an initial distance of ~15 mm (between clamps) along the longitudinal direction and subjected to a tensile test at 500% min. -1 Tests were performed at a constant rate. To evaluate the mechanical robustness of the gels at different temperatures, gel samples were incubated in a temperature-controlled chamber at each temperature for 7 days. Tests were performed immediately after removing the samples from each temperature-controlled chamber.

[0110] (2)Interface structure

[0111] Broken AGG-SSC samples were obtained by freezing the gel under liquid nitrogen and then coating it with platinum to observe the electrolyte / electrode self-healing interface using a scanning electron microscope (SEM; SU-70, Hitachi, Japan). The interface was further analyzed using a polarizing optical microscope (POM; BX53, Olympus, Japan).

[0112] (3) Resistance and electrical conductivity measurement

[0113] To measure the resistance of the PVA-PEDOT:PSS GG electrode, three samples of each gel with a thickness ranging from 0.2 to 0.4 mm were cut into rectangular specimens measuring ~25 mm × 5 mm (length × width). The resistance of each specimen was measured using an LCR meter connected to a Kelvin probe (4284A, Hewlett-Packard Inc., USA). The gel specimens were maintained at the corresponding temperature in a temperature-controlled chamber for 1 h, and the resistance was measured. The samples were then maintained at each temperature for another 7 days, and the electrical conductivity was measured to investigate the long-term stability. The electrical conductivity (σ(Scm)) of each specimen -1 )) was calculated using mathematical formula 1.

[0114] (Equation 1)

[0115] Here, l, R and A are the length, resistance and cross-sectional area of ​​the gel specimen, respectively.

[0116] The change in resistance due to stretching of the gel was also measured using an LCR meter connected to a Kelvin probe. A universal testing machine (TEST ONE TO-100-1C) was used to measure the resistance at 100% min in the vertical direction. -1 A constant strain was applied. Simultaneously, the change in resistance was measured, which can be calculated using Equation 2.

[0117] (Equation 2)

[0118] Here, x is the change in resistance from the initial resistance, R is the final resistance, and R0 is the initial resistance.

[0119] (4) Electrochemical measurement

[0120] All electrochemical measurements of the PVA GG electrolyte were performed using a Metrohm Multi Autolab / M204 multichannel potentiogalvanostat (Netherlands). Electrochemical impedance spectroscopy (EIS) of the electrolyte was performed by placing a rectangular PVA GG electrolyte (width: 2 × 2 × 0.5 mm) between two stainless steel plates. Initial data were obtained by maintaining the measurement setup with the PVA GG electrolyte at the specified temperature for 1 h, and further evaluations were performed over a period of 7 days. EIS was performed in the frequency range 106–0.1 Hz and an amplitude of 10 mV. The resistance (R) of the sample was obtained from the Nyquist plot, and the ionic conductivity (s) was calculated using Equation 3.

[0121] (Equation 3)

[0122] Here, l, R and A are the thickness, resistance and cross-sectional area of ​​the gel specimen, respectively.

[0123] Electrochemical characterization of the supercapacitors was performed using a Battery Cycler WBCS3000 (Republic of Korea). Carbon nanotube films were used as wires at both ends because of their excellent adhesion to the supercapacitor. To evaluate the electrochemical stability of the supercapacitors at different temperatures, the devices were maintained at each temperature for up to 7 days, and daily data were collected. Cyclic voltammetry (CV) and galvanostatic charge-discharge (GCD) were performed in the range of 1–100 mV s over a potential window of 1.2 V, respectively. -1 and was performed at 0.1 mA to 5 mA.

[0124] Examples 1 to 6

[0125] To obtain glycerogel stretchable electrodes, the following method was performed to obtain PVA-PEDOT:PSS glycerogel (GG) electrodes 1 to 6 containing various ratios of PVA and PEDOT:PSS.

[0126] 1. Step of preparing a polymer solution for gel formation and a conductive polymer solution

[0127] First, to obtain a polymer solution for gel formation, PVA powder was dissolved in a DMSO-water mixture (50:50, w / w) in a sealed vial to prepare a 10 wt% PVA solution. The 10 wt% PVA solution was stirred at 140°C for 1 day to obtain a transparent homogeneous solution.

[0128] To obtain a conductive polymer solution, PEDOT:PSS dry redispersible pellets were dissolved in a DMSO-water mixture (50:50, w / w) in a sealed vial to prepare a 2.5 wt% PEDOT:PSS stock solution. The solution was continuously stirred at ~25°C for 14 days to obtain a homogeneously dispersed PEDOT:PSS stock solution.

[0129] 2. Step 2: Preparing a mixed solution

[0130] A 10 wt% PVA solution and a 2.5 wt% PEDOT:PSS stock solution prepared in a DMSO-water mixture solvent were added in appropriate amounts so that PVA and PEDOT:PSS were included in the contents as shown in Table 1, and the mixture was prepared by stirring at ~25 °C for 90 minutes.

[0131] ClassificationPEDOT:PSS 1 wt%PEDOT:PSS 1.25 wt%PEDOT:PSS 1.5 wt%PVA 3 wt%Mixed solution 1 (3-1)Mixed solution 2 (3-1.25)Mixed solution 3 (3-1.5)PVA 4 wt%Mixed solution 4 (4-1)Mixed solution 5 (4-1.25)Mixed solution 6 (4-1.5)

[0132] 3. Step of filling the mixed solution into the mold Mixed solutions 1 to 6 prepared with the same contents as in Table 1 were each filled into a 2 mm thick rectangular plastic mold (prepared by inserting a silicone rubber gasket between two plastic plates).

[0133] 4. Gel formation step

[0134] The mold filled with the mixed solution was placed inside the chamber at -50°C for 12 hours, then removed and thawed at ~25°C for 6 hours. The freeze-thaw cycle was repeated three times.

[0135] 5. First drying stage

[0136] The formed gel was vacuum dried inside a chamber at 50°C for 24 hours at a pressure of -0.08 MPa.

[0137] 6. First immersion stage

[0138] The dried gel was taken out and immersed in a glycerol-water solution (15:85, w / w) for 24 hours.

[0139] 6. Second drying stage

[0140] The gel that had undergone the first immersion step was dried in a chamber at 50°C for 24 hours.

[0141] 7. Second immersion stage

[0142] The dried gel was taken out and immersed in LiClO4-glycerol solution (20:80, w / w) at ~25°C for 24 h.

[0143] 8. Cooling step after annealing

[0144] The second immersed gel was annealed at 120°C for 12 hours and sequentially cooled to 25°C to obtain PVA-PEDOT:PSS GG electrodes 1 to 6 (3-1, 3-1.25, 3-1.5, 4-1, 4-1.25, 4-1.5), respectively.

[0145] Experimental Example 1

[0146] The electrical conductivity and mechanical properties of the PVA-PEDOT:PSS GG electrodes 1 to 6 obtained in Examples 1 to 6 were investigated, and the results are shown in Table 2 and FIGS. 2a to 2e.

[0147] PropertiesPVA-PEDOT:PSS (xy) Glycerogel3-13-1.253-1.54-14-1.254-1.5Young's modulus (MPa)0.45±0.081.41±0.142.00±0.170.83±0.041.57±0.210.78±0.06Tensile strength (MPa)1.88±0.152.225±0.211.94±0.211.92±0.422.26±0.342.09±0.35Fracture strain (%)394±42262±81110±16181±39162±31232±41Electrical Conductivity (S / m)620±40650±801040±40475±40510±471089±49

[0148] As can be seen from Table 2 and FIGS. 2a to 2e, the electrical conductivity increased rapidly as the PEDOT:PSS concentration increased from 1 to 1.5 wt% at a fixed PVA concentration of 3 to 4 wt%. However, it can be seen that the mechanical properties gradually increased as the PVA concentration increased from 3 to 4 wt% at a fixed PEDOT:PSS concentration of 1.5 wt%. The PVA-PEDOT:PSS GG electrode 6(4-1.5) had the best mechanical properties (Young's modulus 0.78 ± 0.06 MPa, tensile strength 2.09 ± 0.35 MPa, strain at break 232 ± 41%) and electrical conductivity (1089 ± 49 S m -1 ) can be seen.

[0149] Experimental Example 2

[0150] To investigate the long-term temperature stability, the PVA-PEDOT:PSS GG electrode 6(4-1.5) was maintained at -20°C, 25°C, and 80°C for one week, and the weight change, electrical conductivity, and mechanical properties of the gel were investigated, and the results are shown in Table 3 and Figs. 2f to 2k.

[0151] As shown in Fig. 2f, the weight change of the PVA-PEDOT:PSS GG electrode 6(4-1.5) remained within ±10 wt% even after prolonged exposure to harsh conditions. The small increase or decrease in weight was attributed to the absorption of atmospheric moisture or the loss of a small amount of glycerol from the gel network.

[0152] As shown in Fig. 2g, the electrical conductivity of the PVA-PEDOT:PSS GG electrode 6(4-1.5) remained almost unchanged even after being left at each temperature for 7 days.

[0153] Additionally, the mechanical properties were similar after exposure to -20°C, 25°C, and 80°C for one week, as shown in Fig. 2h, Table 3, and Fig. 2i.

[0154] PropertiesPVA-PEDOT:PSSGlycerogel electrode 6 (4-1.5)-20℃25 ℃ 80 ℃ Young's modulus (MPa)0.92±0.130.95±0.021.02±0.13Tensile strength (MPa)1.87±0.111.40±0.171.79±0.12Fracture strain (%)264±51211±53266±16Conductivity (S / cm) (7 days)10.27±0.3611.06±0.3611.77±0.23Conductivity (S / m) (initial)1125±581089±491176±24

[0155] In the tensile test, the resistance of the PVA-PEDOT:PSS GG electrode 6(4-1.5) increased minimally with strain. As shown in Fig. 2i, the normalized resistance change (ΔR / Ro) of the GG electrode at 25% strain was 0.15, and a minimum increase of 1.66 was observed even at 100% strain. As shown in Fig. 2k, the PVA-PEDOT:PSS GG electrode 6(4-1.5) showed higher electrical conductivity and stretchability among many reported conducting polymer gels. The reported pure PEDOT:PSS hydrogel has a tensile strength of 4,000 Sm -1 Although it exhibited high conductivity, its elasticity was poor (<30% strain at break). Conductive polymers were mixed with nonconductive polymers to obtain elasticity, but the electrical conductivity was low. Recently reported PVA-PEDOT:PSS double network hydrogel had a conductivity of 1,000 Sm -1 The glycerogel stretchable electrode according to the present invention showed an electrical conductivity of 1,089 Sm and a fracture strain of 150%, compared to many reported studies. -1 It has advantageous properties for many applications, such as electrical conductivity, a breaking strain of 231 ± 41%, and long-term stability over a wide temperature range (-20 ℃ to 80 ℃).

[0156] Example 7

[0157] To obtain a glycerogel stretchable electrolyte, the following method was performed to obtain PVA-LiClO4 glycerogel (GG) electrolytes 1 to 5 containing various ratios of PVA and LiClO4.

[0158] 1. Step for preparing a polymer solution for gel formation

[0159] A polymer solution for gel formation was prepared by dissolving 5 wt% PVA in a DMSO / water (75:25 w / w) solution at 140°C for 1 day.

[0160] 2. Step of filling the mold with a polymer solution for gel formation

[0161] The prepared polymer solution for gel formation was filled into a 1 mm thick plastic mold.

[0162] 3. Gel formation step

[0163] A mold filled with a polymer solution for gel formation was frozen at -50°C for 1 day and then thawed at room temperature for 12 hours to form a gel.

[0164] 4. Steps for obtaining hydrogel

[0165] The obtained 5 wt% PVA organogel was equilibrated in water for 3 days to obtain a hydrogel.

[0166] 5. Steps for obtaining glycerogel

[0167] The obtained hydrogel was sequentially immersed in a 25% glycerol aqueous solution for 12 hours and a 50% glycerol aqueous solution for 12 hours to replace the water molecules of the hydrogel with glycerol, thereby obtaining a glycerogel.

[0168] 6. Step of immersing in a metal salt-glycerol solution

[0169] PVA-LiClO4GG electrolyte 1(5-20) was obtained by immersing in 75% and 100% glycerol (w / w) containing 20% ​​LiClO4 (w / w) for 24 hours, respectively.

[0170] Examples 8 and 9

[0171] The same method as Example 7 was performed except that 3 wt% and 8 wt% of PVA were used, to obtain PVA-LiClO4GG electrolyte 2 (3-20) and PVA-LiClO4GG electrolyte 3 (8-20), respectively.

[0172] Examples 10 and 11

[0173] The same method as Example 7 was performed except that metal salt-glycerol solutions having LiClO4(w / w) concentrations of 15% and 25%, respectively, were used to obtain PVA-LiClO4GG electrolyte 4(5-15) and PVA-LiClO4GG electrolyte 5(5-25), respectively.

[0174] Experimental Example 3

[0175] The ionic conductivity and mechanical properties of the PVA-LiClO4GG electrolytes 1 to 5 obtained in Examples 7 to 11 were investigated, and the results are shown in Table 4, Table 5, and Figs. 3a and 3b.

[0176] TestPVA-LiClO4GG Electrolyte2(3-20)PVA-LiClO4GG Electrolyte1(5-20)PVA-LiClO4GG Electrolyte3(8-20)Young's modulus (MPa)0.197±0.0030.392±0.0290.696±0.041Stretchability (%)630.44±30728.13±20.86695.52±37.76Tensile stress (MPa)0.437±0.0501.129±0.0252.146±0.094Ionic conductivity0.030±0.0030.034±0.0030.021±0.002

[0177] TestPVA-LiClO4GG Electrolyte4(5-15)PVA-LiClO4GG Electrolyte1(5-20)PVA-LiClO4GG Electrolyte5(5-25)Young's modulus (MPa)0.473±0.0090.392±0.0290.286±0.011Stretchability (%)850.93±26.850728.13±20.860762.96±50.316Tensile stress (MPa)1.315±0.0161.129±0.0290.883±0.054Ionic conductivity0.028±0.0010.034±0.0030.03±0.001

[0178] As shown in Table 4 and Fig. 3a, when the PVA content was increased by 3, 5, and 8 wt%, the mechanical properties of the gel gradually increased, but the ionic conductivity decreased due to the increase in the non-conductive polymer portion within the gel. However, as shown in Table 5 and Fig. 3b, when the PVA content was fixed at 5 wt%, the mechanical properties of the gel electrolyte decreased as the salt concentration changed from 15 wt% to 25 wt%, and the ionic conductivity reached the optimal value at 20 wt% salt concentration. As a result, it was found that PVA-LiClO4GG electrolyte 1(5-20) exhibited the best ionic conductivity (0.034 ± 0.0029) and excellent mechanical properties. Experimental Example 4

[0179] As described below, the ionic conductivities of the PVA GG electrolyte at different temperatures were similar to those of other reported electrolytes used in energy storage devices. To investigate the long-term mechanical stability of the PVA GG electrolyte over a wide temperature range (-20°C, 25°C, and 80°C), the PVA-LiClO4 GG electrolyte 1(5-20) was maintained at -20°C, 25°C, and 80°C for one week, and the weight change, ionic conductivity, and mechanical properties of the gel were investigated. The results are presented in Tables 6 and 7, and Figs. 3c to 3j.

[0180] As shown in Fig. 3c, the weight change of the PVA-LiClO4GG electrolyte 1(5-20) remained within 10 wt% after exposure to air at -20°C, 25°C, and 80°C for one week. The slight weight change may be due to the absorption of atmospheric moisture or the loss of a small amount of glycerol from the gel network.

[0181] As illustrated in Fig. 3d, the ionic conductivity of the PVA GG electrolyte remained unchanged even after one week of incubation at extreme temperatures (-20°C, 25°C, and 80°C). The increase and decrease in ionic conductivity at high and low temperatures may be due to changes in solvent viscosity with temperature.

[0182] As shown in FIGS. 3d and 3h, the PVA GG electrolyte exhibited high ionic conductivity of 0.034 ± 0.0029 S / m at room temperature and 0.18 ± 0.021 S / m and 0.0032 ± 0.00013 S / m at 80°C and -20°C, respectively, maintaining excellent performance.

[0183] As shown in Tables 6, 7, and Figures 3e and 3g, the mechanical properties of the PVA GG electrolyte remained similar to the initial room temperature behavior even after 7 days. The performance of the electrolyte was also evaluated according to the change in strain.

[0184] Test-20 ℃25 ℃80 ℃InitialYoung's modulus(MPa)0.434±0.0200.407±0.0060.239±0.0080.392±0.028Stretchability (%)748.888±20.640719.999±26.940819.44±11.220728.13±20.860Tensile stress(MPa)1.23±0.0101.091±0.0081.586±0.0401.129±0.020

[0185] Test25 ℃Young's modulus (MPa)1.00±0.020Stretchability (%)719.99±26.940Tensile stress (MPa)1.09±0.008Ionic conductivity (S / m)0.009

[0186] As shown in Fig. 3f, the change in resistance (ΔR / Ro) was observed to follow a linearly increasing trend with strain. The aforementioned results confirm the long-term stability and operating capability of the PVA GG electrolyte from -20°C to 80°C, demonstrating its wide range of applications in extreme-resistant and stretchable energy storage devices. Furthermore, the PVA GG electrolyte prepared by the sequential solvent exchange method of the present invention can achieve low modulus and high ionic conductivity of the PVA GG electrolyte by preserving the original swollen structure of the hydrogel, a prerequisite for stretchable energy storage devices.

[0187] On the other hand, from Figs. 3i and 3j, which show the Nyquist EIS plot and tensile stress-strain curve of PVA GG electrolyte prepared by direct equilibration hydrogel in 100% glycerol containing 20% ​​LiClO4 (w / w), respectively, it can be seen that direct solvent exchange from hydrogel to glycerogel electrolyte results in a hard glassy behavior due to polymer aggregation, resulting in low ionic conductivity (0.0085 S / m) and high modulus (1±0.0219 MPa).

[0188] Example 12

[0189] To obtain a glycerogel stretchable supercapacitor, the following method was performed to obtain a glycerogel stretchable supercapacitor (AGG-SSC).

[0190] 1. Step 1: Prepare two glycerogel stretchable electrodes

[0191] Two PVA-PEDOT:PSS GG electrodes were prepared by performing any one of the methods of Examples 1 to 6 using glycerogel stretchable electrodes.

[0192] 2. Step 2: Preparing a glycerogel elastic electrolyte

[0193] A rectangular PVA GG electrolyte was prepared by performing any one of the methods of Examples 7 to 11 using a glycerol stretchable electrolyte.

[0194] 3. Step of forming a laminate

[0195] After the PVA-PEDOT:PSS GG electrodes were placed so that the PVA GG electrolyte (thickness: ~0.5 mm) was inserted between two PVA-PEDOT:PSS GG electrodes (thickness: ~0.2-0.4 mm), the PVA GG electrolyte (thickness: ~0.5 mm) was placed on the upper surface, and then the PVA-PEDOT:PSS GG electrodes were placed on the upper surface to form a laminate.

[0196] 4. Self-healing stage

[0197] We introduced a simple heat-mediated self-healing process to attach the PVA-PEDOT:PSS GG electrode and the PVA GG electrolyte. Specifically, a self-healing process was performed at 95°C for 1 h, followed by 12 h at room temperature to obtain a fully self-healed glycerogel stretchable supercapacitor (AGG-SSC).

[0198] 5. Step 5: Cut to desired size

[0199] The obtained glycerogel stretchable supercapacitor was cut into pieces measuring 2 cm x 1 cm.

[0200] Experimental Example 5

[0201] To determine the bonding strength, the glycerogel stretchable supercapacitors obtained in Example 12 were cut to 5 mm widths and subjected to lap shear tests at a rate of 500% / min over an initial length of ~10 mm (between clamps). The shear stress was calculated as the maximum force required to fracture the interface divided by the overlapping shear area, and the results are shown in Fig. 4b.

[0202] As shown in Fig. 4b, the self-healed sample of the present invention, i.e., the glycerogel stretchable supercapacitor, exhibited excellent bonding toughness with a stretching of ~100% and an appropriate bonding strength of 0.044 MPa, compared to reported results.

[0203] Additionally, the one-sided adhesive interface of the self-healed glycerogel stretchable electrode and the glycerogel stretchable electrolyte was analyzed using SEM and optical microscope images, and the results are shown in Fig. 4c.

[0204] As shown in Figure 4c, a fully healed interface is clearly demonstrated, indicating proper polymer chain reorganization between the glycerogel stretchable electrode and the glycerogel stretchable electrolyte. Unlike previously proposed self-welding processes, the present invention achieves a strong bond between the electrode and the electrolyte using a simple, one-step approach without any external additives. This process can offer significant advantages in the development of stretchable energy storage devices and the formation of a stable interface between the electrode and the electrolyte, as the glycerogel stretchable supercapacitor acts as a single material under mechanical strain.

[0205] Experimental Example 6

[0206] The electrochemical performance of the glycerogel stretchable supercapacitor obtained in Example 12 was evaluated by cyclic voltammetry (CV), galvanostatic charge-discharge (GCD), and electrochemical impedance spectroscopy (EIS).

[0207] As shown in Fig. 5a, CV was performed at 1, 5, 10, 20, 50, and 100 mV s in a voltage window of 1.2 V. -1The experiments were performed at different scan rates. However, the symmetry for forward and backward scans was maintained throughout, suggesting excellent electrochemical reversibility of the system. Faster sweep rates lead to a thinner diffusion layer, which results in higher currents, as electrolyte ions cannot participate in the desired charge transfer reactions. The absence of a redox peak indicates that the electric double layer capacitance (EDLC) contributes maximally to the charge storage mechanism of the supercapacitor.

[0208] To understand the capacitance effect of PEDOT:PSS based supercapacitors, CV data were collected at 0.5, 1, 2, 3, 4, and 5 mV s. -1 was collected from. Dunn's method was used to understand the diffusion (pseudocapsulation) and non-diffusion (EDLC) control dynamics based on Equation 4.

[0209] (Equation 4)

[0210] Here, i(V) is the total current at a specific potential, ν is the scan rate, k1 and k2 are constants, k1ν and k2ν 1 / 2 are the capacitive and diffusion currents, respectively. 0.5 mV s -1 For , the EDLC and pseudocapacitance contributions were 90.13% and 9.87%, respectively (see Fig. 5e). As the scan rate increased, the EDLC capacitance contribution became dominant because the interaction residence time of electrolyte ions at the active site became shorter.

[0211] The charge-discharge behavior of the supercapacitor was investigated at different currents of 0.1, 0.2, 0.5, 1, 2, and 5 mA (Fig. 5b,c). The triangular GCD curves reflect the excellent reversibility and near-EDLC characteristics of the supercapacitor. The areal capacitance values ​​at different currents were calculated using Equation 5.

[0212] (Equation 5)

[0213] Here i, t d, A t and ΔV are the current, discharge time, total area of ​​the supercapacitor, and voltage window of the system, respectively.

[0214] The glycerogel stretchable supercapacitor of the present invention has a current density of 26.27 mF cm at 0.1 mA. -2 The device exhibited an areal capacitance of 87.24% and negligible resistance drop (IR drop). Even when the current increased 20-fold to 2 mA, it showed an impressive areal capacitance retention of 87.24%. Interestingly, the device could retain more than 50% of its capacitance when the current increased 50-fold (5 mA). This high capacitance retention may be due to the excellent integrity and electrochemical stability of all gel supercapacitors. The Cac tended to decrease with increasing current (b in Fig. 5e), which may be attributed to the IR drop and slow electrochemical kinetics at higher currents. The Nyquist plot obtained from EIS (Fig. 5c) provides information about the equivalent series resistance (Req) and charge transfer resistance (Rct) of the system. The initial intersection of the real impedance axes in the high-frequency region provides the Req value, and Rct was estimated from the diameter of the semicircle on the same axis. Req is the collective resistance arising from the ionic resistance of the electrolyte and the contact resistance between the gel electrode and the electrolyte. Similarly, Rct is the contribution of charge transfer resistance associated with the EDLC particle surface and the Faradic reaction. The Req and Rct values ​​are 39Ω and 16Ω, respectively. A slanted linear portion is observed in the intermediate frequency region due to ion transport resistance (diffusion resistance).

[0215] The cycling stability of the glycerogel stretchable supercapacitor of the present invention was tested at 2 mA for 10,000 charge-discharge cycles. A nearly vertical line (parallel to the virtual impedance axis) in the low-frequency region was observed, consistent with the device's charge-transfer saturation and EDLC behavior. Notably, all components were composed of glycerogel, resulting in no additional resistance in the current collector. As shown in Figure 5c, the capacitance retention was 81.48% in the 1.2 V voltage window and 91.76% at 0.8 V. The device exhibited excellent Coulombic efficiencies of over 99.5% across both voltage windows, demonstrating excellent electrochemical reversibility and the absence of any adverse effects on the device. An unusual behavior of increased capacitance was observed during the initial cycles, which may be attributed to surface activation of the electrodes by the electrolyte. The flexibility, stretchability, and strong adhesion between the electrode and the electrolyte can effectively accommodate rapid expansion and contraction during continuous charge-discharge cycles, providing high cycle stability. The practical and useful applications of the fabricated device can be experienced by obtaining the area-specific energy (Eae) and power (Pap), which represent the charge holding capacity and charge transfer readiness, respectively. Unlike other scalable and flexible supercapacitors, the glycerogel stretchable supercapacitor (AGG-SSC) of the present invention can provide continuous energy and power while operating under extreme environmental conditions due to its freeze-proof and dry-proof properties. Eae (μWh cm -2 ) and Pap (μW cm -2 ) were evaluated from current-discharge (CD) curves at different currents using Equations 6 and 7.

[0216] (Equation 6)

[0217] (Equation 7)

[0218] The obtained Eae was 5.25 μWh cm -2 , and at 0.1 mA, Pap was 15 μW cm -2was 750 μW cm at a high current of 5 mA (50 times). -2 The excellent Pap of the AGG-SSC can maintain an energy density of nearly 59%. At higher currents, the electrolyte ions do not have enough residence time to participate in the desired reaction. Therefore, the device exhibited low charge storage capacity at high currents, and the short discharge time made the power transferability the dominant characteristic (according to Eq. 7). As shown in Fig. 5d, which shows the area Ragone plot of the AGG-SSC compared to other reported supercapacitors, the calculated Eae and Pap (see Fig. 5d) are comparable to those of MWCNT / Mn / Mo (Eae = 4.2 μWh cm -2 and Pap=0.3μWcm -2 ), CNT / PPY (Pap = 176.5 μW cm -2 at Eae=0.44 μWh cm -2 ), Au / MWCNT (Eae=0.34 μWh cm -2 and Pap=6 μW cm -2 ), V-AuNW / PANI (Eae and Pap of 0.71 μWh) cm -2 and 40 μW cm -2 ), PEDOT:PSS / ferritin / MWNT fibers (0.82 μWh cm of Eae and Pap, respectively -2 and 150 μW cm -2 ) and PANI (Eae=1.28 μWh cm -2 at Pap=12.1 μW cm -2 )am.

[0219] Experimental Example 7

[0220] The electrochemical stability of the glycerogel stretchable supercapacitor (AGG-SSC) obtained in Example 12 under mechanical deformation conditions such as tensile, bending, and torsion was investigated.

[0221] Figure 6a shows the AGG-SSC under pristine and 100% stretch conditions. Electrochemical data were initially collected at different percentages of strain and relaxation (Figures 6a and 7a). The CV and GCD plots were very stable even under extreme stretching conditions. It is noteworthy that the areal capacitance values ​​increased by approximately 2.7% when the supercapacitor was stretched by 50% and 75%. The small change in values ​​may be due to the thickness reduction of the AGG-SSC during stretching, which would have accelerated the electrolyte ion permeation at the electrolyte / electrode interface. At 100% stretch, the device exhibited the same Cac value as that obtained in the unstretched condition. The unchanged values ​​indicate that no delamination issues occurred in the device, demonstrating the robust mechanical integrity of the individual gel components. The bending (180°) and torsion (90°) representations are depicted in Figure 6b. As shown in Fig. 6b, there was no change in the CV shape even under extreme bending and twisting. The Cac value calculated from the GCD curve (see Fig. 7b) indicates that ~100% of the capacitance was preserved under deformation. The excellent electrochemical behavior during mechanical deformation was attributed to the strong interfacial connection (integrated contact area) between the electrolyte and electrode, which provided an unobstructed permeation and diffusion path for electrolyte ions.

[0222] Operating supercapacitors at temperatures other than room temperature (high and low) is challenging. Unlike aqueous, hydrogel, and organohydrogel-based supercapacitors (SCs), the AGG-SSC according to the present invention can maintain its electrochemical properties even at a high temperature of 80°C, as evidenced by the CV plot (see Figure 6c) and the GCD plot (see Figure 6d). At an extremely low temperature of -20°C, where most aqueous and hydrogel-based SCs cease to function due to almost complete ion transport disruption caused by the freezing of the electrolyte, the AGG-SSC of the present invention still functioned. Although the AGG-SSC generated less current, it maintained excellent reversibility during the forward and reverse scans during the CV. Furthermore, altered CV morphology was observed at sub-zero temperatures. Similarly, a higher IR drop and shorter discharge time were observed at -20°C due to reduced ion transport. Nevertheless, the AGG-SSC of the present invention has a thermal conductivity of 26.27 mF cm at room temperature. -2 12.62mF cm compared to -2 It had a reasonable electrostatic capacity, which was possible because the constituent materials were not frozen due to the presence of glycerol in the electrodes and electrolyte. The greatest advantage of the fabricated glycerol-based AGG-SSC is that it maintains long-term stability under all environmental conditions (-20°C, room temperature, and 80°C).

[0223] The electrochemical stability was evaluated over a week, and the shapes of the CV and GCD curves were almost the same after 7 days, as shown in Figs. 8a to 8f, and the capacitance retention was 100%, as shown in Fig. 6e. However, slightly deteriorated CV and GCD plots were obtained at -20°C and 80°C, respectively, due to the hindrance of ion migration and a slight decrease in solvent concentration. After one week, the AGG-SSC exhibited excellent areal capacitance retention of 93.27% and 90.92% at 80°C and -20°C, respectively (see Fig. 6e). To demonstrate the feasibility of the AGG-SSC in real-world applications, the LED was made to glow in a stretched state under extreme temperature conditions, as shown in Fig. 6f. In the AGG-SSC of the present invention, the physical integrity between the electrode and the electrolyte due to heat-mediated self-healing along with the extremely resistant behavior of the glycerogel played a significant role in maintaining the mechanical and electrochemical stability of the AGG-SSC under extreme temperatures and strain conditions.

[0224] Depending on the application, supercapacitors can be connected in series or parallel to increase energy and power density. When the AGG-SSCs of the present invention are used in series and parallel connections, all supercapacitors have nearly identical components. Two AGG-SSCs connected in series exhibited twice the voltage, half the current, and nearly the same discharge time compared to a single AGG-SSC (see the CV and GCD curves in Figure 6h). Furthermore, the parallel-connected AGG-SSCs exhibited nearly twice the current and discharge time compared to individual AGG-SSCs. The unchanged shape of the CV voltage profiles suggests that the connected AGG-SSCs operated stably without performance degradation, as reported by other results.

[0225] The above experimental results demonstrate that the present invention has developed a well-integrated glycerogel stretchable supercapacitor with robust electrochemical and mechanical behavior under extreme temperature conditions using a glycerogel stretchable electrode and a glycerogel stretchable electrolyte. The glycerogel electrolyte [gel-forming polymer (egPVA) / glycerol] and electrode [gel-forming polymer / conductive polymer (egPVA / PEDOT:PSS) / glycerol] can suppress the drying and freezing problems associated with aqueous and polymer (hydrogel)-based electrolytes at high and sub-zero temperatures.

[0226] Therefore, the glycerogel stretchable supercapacitor of the present invention exhibited excellent capacitance retention rates of 93.27% and 90.92% after 7 days of storage at 80°C and -20°C, respectively. Due to the self-healing ability of the gel, the device did not experience any peeling issues, and the capacitance did not change even after bending, twisting, and stretching. In addition, the AGG-SSC exhibited capacitance retention rates of 81.48% at a voltage window of 1.2 V and 91.76% at 0.8 V after 10,000 charge / discharge cycles. The glycerogel stretchable supercapacitor of the present invention is the first glycerol-based stretchable supercapacitor with stable and intrinsic mechanical robustness that demonstrates stretchability with excellent freeze-thaw and drying capabilities over a wide temperature range of -20°C to 80°C, and thus has potential applications in various wearable and stretchable electronic devices under all environmental conditions.

[0227] Although the present invention has been illustrated and described with reference to preferred embodiments as described above, it is not limited to the above-described embodiments, and various changes and modifications may be made by a person skilled in the art to which the invention pertains within a scope that does not depart from the spirit of the present invention.

Claims

1. Step of preparing a polymer solution for gel formation and a conductive polymer solution; A step of preparing a mixed solution by mixing the above gel-forming polymer solution and the conductive polymer solution and stirring them; A step of filling the above mixed solution into a mold of a desired shape; A step of forming a gel by repeating the cycle of freezing and then thawing the mold filled with the above mixed solution at least once; A first drying step of drying the formed gel in a vacuum; A first immersion step of immersing the dried gel in a glycerol-water solution; A second drying step of drying the gel in which glycerol and water have been absorbed at a temperature below 100°C; A second immersion step of immersing the gel that has undergone the second drying step in a metal salt-glycerol solution at a temperature below room temperature; and A method for manufacturing a glycerogel elastic electrode, comprising: a step of annealing the gel that has undergone the second immersion step and then cooling it to room temperature.

2. In paragraph 1, The above gel-forming polymer solution is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), comprising any one selected from the group consisting of cellulose, A method for manufacturing a stretchable glycerogel electrode, characterized in that the conductive polymer solution comprises at least one selected from the group consisting of polyacetylene, polypyrrole, polythiophene, poly(3,4-ethylene dioxythio-phene)(PEDOT), polyaniline, and poly(3,4-ethylenedioxythiophene:poly(styrenesulfonate)(PEDOT:PSS).

3. In paragraph 1, A method for manufacturing a glycerogel stretchable electrode, characterized in that the above mixed solution contains a gel-forming polymer: conductive polymer in a weight ratio of 2.5 to 4.5: 0.5 to 2.

4. In paragraph 3, A method for manufacturing a glycerogel stretchable electrode, characterized in that the gel-forming polymer included in the above mixed solution is polyvinyl alcohol (PVA), the conductive polymer is PEDOT:PSS, and the solvent is a DMSO-water mixed solution.

5. In paragraph 1, A method for manufacturing a glycerol elastic electrode, characterized in that in the freezing and thawing cycle, the freezing is performed by leaving the mold at -20°C or lower for 12 hours or longer, and the thawing is performed by leaving the frozen mold at 25°C or lower for 6 hours or shorter.

6. In paragraph 1, A method for manufacturing a glycerol-water solution, characterized in that in the first immersion step, the glycerol-water solution contains glycerol:water in a weight ratio of 10 to 20: 80 to 90, and the immersion time is 12 hours or more.

7. In paragraph 1, A method for manufacturing a glycerogel elastic electrode, characterized in that in the second immersion step, the metal salt-glycerol solution contains metal salt:glycerol in a weight ratio of 15 to 25:75 to 85, and the immersion time is 12 hours or more.

8. In paragraph 7, A method for manufacturing a glycerogel elastic electrode, characterized in that the metal salt is any one selected from the group consisting of LiClO4, NaCl, and LiCl.

9. In paragraph 1, A method for manufacturing a glycerogel elastic electrode, characterized in that the above annealing is performed at 100°C to 150°C for 10 hours or more.

10. A glycerogel stretchable electrode comprising glycerogel containing 0.5 to 2 wt% of a conductive polymer.

11. In paragraph 10, The conductive polymer is at least one selected from the group consisting of polyacetylene, polypyrrole, polythiophene, poly(3,4-ethylene dioxythio-phene) (PEDOT), polyaniline, and poly(3,4-ethylenedioxythiophene:poly(styrenesulfonate)(PEDOT:PSS). In the above glycerogel, the gel-forming polymers are polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), a glycerogel stretchable electrode characterized by being any one selected from the group consisting of cellulose.

12. In paragraph 10, A glycerogel stretchable electrode characterized in that the glycerogel comprises PEDOT:PSS as the electrically conductive polymer and polyvinyl alcohol (PVA) as the gel-forming polymer.

13. In paragraph 12, A glycerogel stretchable electrode characterized by a Young's modulus of 0.78 ± 0.06 MPa, a tensile strength of 2.09 ± 0.35 MPa, and a breaking strain of 232 ± 41%.

14. In paragraph 12, Electrical conductivity is 1089 ± 49 S m -1 A glycerogel stretchable electrode characterized by:

15. In paragraph 12, A glycerogel stretchable electrode characterized in that the weight change is maintained within ±10 wt% after exposure to temperature conditions of -20 ℃ to 80 ℃ for one week.

16. Step of preparing a polymer solution for gel formation; A step of filling the polymer solution for gel formation into a mold of a desired shape; A step of forming a gel by freezing and then thawing a mold filled with the polymer solution for gel formation; A step of equilibrating the formed gel in water to obtain a hydrogel; A step of sequentially immersing the hydrogel in glycerol aqueous solutions having different concentrations at least once to obtain a glycerogel in which the water molecules of the hydrogel are replaced with glycerol; and A method for producing a glycerogel stretchable electrolyte, comprising the step of immersing the glycerogel in a metal salt-glycerol solution.

17. In paragraph 16, The above gel-forming polymer solution is polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), comprising any one selected from the group consisting of cellulose, A method for producing a glycerogel elastic electrolyte, characterized in that it comprises a mixed solution containing DMSO and water in a weight ratio of 50 to 90: 10 to 50 as a solvent.

18. In paragraph 16, A method for producing a glycerogel elastic electrolyte, characterized in that, in the step of obtaining the glycerogel, when the hydrogel is immersed in a glycerol aqueous solution twice or more, the glycerol concentration of the subsequent glycerol aqueous solution is higher than the concentration of the preceding glycerol aqueous solution.

19. In paragraph 16, The above metal salt-glycerol solution contains metal salt: glycerol in a weight ratio of 15 to 25: 75 to 85, A method for producing a glycerogel elastic electrolyte, characterized in that the metal salt is any one selected from the group consisting of LiClO4, NaCl, and LiCl.

20. A glycerogel stretchable electrolyte comprising glycerogel containing 15 to 25 wt% of an ionic conductive material.

21. In paragraph 20, The above ion conductive material is a metal salt selected from the group consisting of LiClO4, NaCl, and LiCl, In the above glycerogel, the gel-forming polymers are polyacrylamide (PAAm), polyvinyl alcohol (PVA), poly(acrylamide-co-acrylic acid) / iron(III) (P(AAm-co-AAc) / Fe 3+ ), a glycerogel stretchable electrolyte characterized by being any one selected from the group consisting of cellulose.

22. In paragraph 20, A glycerogel stretchable electrolyte characterized by an ionic conductivity of 0.18 ± 0.021 S / m at 80°C, 0.034 ± 0.0029 S / m at room temperature, and 0.0032 ± 0.00013 S / m at -20°C.

23. In paragraph 20, A glycerogel stretchable electrolyte characterized in that the weight change is maintained within 10 wt% after exposure to temperature conditions of -20 ℃ to 80 ℃ for one week.

24. In paragraph 20, A glycerogel stretchable electrolyte characterized in that its mechanical properties remain similar to the initial room temperature behavior even after exposure to temperature conditions of -20°C to 80°C for one week.

25. A step of preparing two glycerogel elastic electrodes by the method of any one of claims 1 to 9; A step of preparing a glycerogel elastic electrolyte by the method of any one of claims 16 to 19; A step of forming a laminate by laminating the two prepared glycerogel stretchable electrodes and the glycerogel stretchable electrolyte, wherein the electrolyte is disposed between the two electrodes; and A method for manufacturing a glycerogel stretchable supercapacitor, comprising a self-healing step in which two electrodes forming the laminate and an electrolyte are bonded to each other to form a stable adhesive interface.

26. In paragraph 25, A method for manufacturing a glycerogel stretchable supercapacitor, characterized in that the self-healing step is performed including a heating step of treating the laminate at 80°C to 120°C for 30 to 90 minutes and a cooling step of leaving the laminate subjected to the heating step at room temperature for 10 hours or more.

27. Glycerogel elastic first electrode; A glycerogel stretchable electrolyte having the upper surface and the lower surface of the above glycerogel stretchable first electrode bonded thereto; A glycerogel stretchable electrode having its lower surface bonded to the upper surface of the glycerogel stretchable electrolyte; A glycerogel stretchable supercapacitor, wherein a first adhesive interface formed between the upper surface of the first electrode and the lower surface of the electrolyte and a second adhesive interface formed between the upper surface of the electrolyte and the lower surface of the second electrode are formed by mutual penetration of polymer chains included in the first electrode, the electrolyte, and the second electrode.

28. In paragraph 27, The first electrode and the second electrode are a glycerogel stretchable electrode manufactured by the method of any one of claims 1 to 9 or a glycerogel stretchable electrode manufactured by any one of claims 10 to 15, A glycerogel stretchable supercapacitor, characterized in that the electrolyte is a glycerogel stretchable electrolyte manufactured by the method of any one of claims 16 to 19 or a glycerogel stretchable electrolyte of any one of claims 20 to 24.

29. In paragraph 28, 26.27 mF cm at room temperature and 0.1 mA -2 A glycerogel stretchable supercapacitor characterized by having a capacitance of .

30. In paragraph 29, A glycerogel stretchable supercapacitor characterized in that the retention rate of the electrostatic capacity is 85% or more when the current increases 20-fold from 0.1 mA to 2 mA.

31. In paragraph 29, A glycerogel stretchable supercapacitor characterized in that the retention rate of the electrostatic capacity is 50% or more when the current increases 50 times from 0.1 mA to 5 mA.

32. In paragraph 28, A glycerogel stretchable supercapacitor characterized by a capacitance retention rate of 90% or more after being left at 80°C and -20°C for 7 days, respectively.

33. In paragraph 28, A glycerogel stretchable supercapacitor characterized by a capacitance retention rate of 80% or more at 1.2 V and 90% or more at 0.8 V after 10,000 charge / discharge cycles.

34. In paragraph 28, A glycerogel stretchable supercapacitor characterized by stretching and recovering without damage at temperatures from -20 to 80°C.

Citation Information

Patent Citations

  • Method and apparatus for transmitting frame through expanded channel in wide-band wireless communication network

    KR1020200126936A

  • Loading jig

    KR102495779B1

Cited By

  • Preparation method of high-strength, environment-friendly and conductive composite gel material

    CN119978445A

  • Conductive organic hydrogel based on PVA / PEDOT: PSS and preparation method and application thereof

    CN120682492A

  • Multifunctional flexible sensor

    CN121230923A