Method for manufacturing metal screen mask for fine pattern

The method of forming a metal screen mask with a bridge pattern and protective bridge photomask addresses printing defects and stencil damage, enabling uniform coating and improved printing quality for fine patterns.

WO2024228450A1PCT designated stage expired Publication Date: 2024-11-07KOREA ELECTROTECH RES INST
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/001668
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2024-02-05
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing methods for manufacturing metal screen masks for fine patterns face challenges such as printing defects due to screen mesh obstruction, stencil damage during printing, and uneven coating of high-viscosity materials, particularly in creating closed curve patterns and maintaining printing quality.

Method used

A method involving the formation of a stencil pattern with a bridge that crosses the pattern at a height smaller than the stencil, supported by a protective bridge photomask and metal plating, which prevents stencil damage and allows for uniform coating of high-viscosity materials by adjusting the coating thickness and pattern design.

Benefits of technology

This approach prevents stencil damage, enhances printing quality, and enables uniform thin film coating of high-viscosity materials, allowing for the production of closed curve patterns and improved rigidity of the metal screen mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024001668_07112024_PF_FP_ABST
    Figure KR2024001668_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a metal screen mask for a fine pattern, the metal screen mask comprising: a stencil pattern corresponding to a fine printing pattern; and bridges formed across the stencil pattern at a height smaller than the height of the stencil pattern to support the shape of the stencil pattern, wherein the metal screen mask having the stencil pattern with protective bridges formed therein is manufactured by separately forming photoresist layers for forming the stencil pattern and protective bridge pattern on a substrate, and independently exposing each layer to light. The present invention has advantages in that the stencil manufacturing method for printing a fine pattern enables: preventing damage to the stencil even when the stencil has an increased length and pattern density; manufacturing a stencil having a closed-curve pattern; improving the quality of printing; and arbitrarily adjusting the thickness of a thin film coating on a high-viscosity material while applying the coating evenly.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a metal screen mask for micropatterns

[0001] The present invention relates to a technology in the field of micro- or nano-scale electronic printing technology, and relates to a method for manufacturing a metal screen mask for a micro-pattern, the metal screen mask including a stencil pattern corresponding to a micro-printing pattern and a bridge formed across the stencil pattern and having a height smaller than the height of the stencil pattern to support the shape of the stencil pattern.

[0002] Recently, the electronics manufacturing market has been making various attempts to reduce production costs, improve material consumption efficiency, and create a clean production environment through the introduction of new production processes.

[0003] A representative example is printed electronics technology. Printed electronics technology refers to a next-generation printing technology that uses a printing process on a micro or nano scale to create electronic circuits, sensors, components, and various electronic products as if they were printed.

[0004] The printing processes used for this include inkjet printing, screen printing, roll-to-roll printing, and imprinting. Among them, the method of printing metallic ink using screen printing or spray printing is mainly used for printing conductive circuits with fine patterns.

[0005]

[0006] The above screen printing method uses a stencil combined with a screen mesh, and the screen mesh generally has a diameter of about 40㎛.

[0007] At this time, when printing a pattern of a size smaller than the diameter of the screen mesh, there was a problem in that the printed pattern formed on the stencil was covered by the screen mesh, resulting in poor printing depending on the location, resulting in unevenness of the pattern.

[0008]

[0009] The applicant is conducting a series of studies to improve these problems, and the research history is as follows.

[0010] In order to solve the above-mentioned problem, the applicant discloses a micro stencil including a mask portion in which a through hole of a shape corresponding to a printing pattern is formed, and a reinforcing portion that is protruded on one surface of the mask portion and provided in a portion where the through hole is not formed, in Korean Patent Publication No. 10-2020-0043796 entitled 'Micro stencil and manufacturing method thereof'.

[0011] However, according to the above-described method, since the mask portion is supported by the reinforcing portion and is spaced apart from the substrate, the mask portion does not come into contact with the printed metal ink, and thus, although the effect of preventing the metal ink from getting stuck in the through hole can be obtained, there is a limit to clearly printing the pattern, and therefore, development of a new technology for this has become necessary.

[0012] Meanwhile, in order to solve the size problem of the stencil for fine patterns in the conventional technology, when the length of the stencil was lengthened and the pattern density was increased, there was a problem of damage such as the stencil being separated during the printing process, and in the case of a closed curve pattern, it was impossible to produce a stencil, and there was a problem of the printing quality being lowered due to the adhesive force between the nickel stencil and the printing substrate.

[0013]

[0014] In order to solve such problems, the applicant disclosed Republic of Korea Patent Publication No. 10-2022-0056359, 'Metal stencil mask for fine pattern printing equipped with stencil protection bridge and manufacturing method thereof', thereby disclosing a technology for protecting a stencil pattern of a certain size or larger with a protection bridge.

[0015] However, although the stencil pattern protection effect of the protection bridge in the above technology is excellent, there was a problem in that the printing surface was affected by the protection bridge because two exposures were performed on the printing surface to form the protection bridge.

[0016]

[0017] To solve this problem, the applicant is improving the process in Korean Patent Application No. 10-2021-0139842, 'Method for Manufacturing a Stencil for Fine Pattern Printing Equipped with a Protective Bridge', by making the stencil pattern, which is the printing surface, and the protective bridge formation surface different from each other so that the printing surface is protected.

[0018] However, despite these process improvements, the formation of protective bridges has been found to have an impact on the stencil pattern, and the need for improvement has arisen.

[0019]

[0020] Meanwhile, conventional techniques for thin film coating of high viscosity materials, such as thin film coating for multilayer ceramic capacitors (MLCCs), include the doctor blade method or the bar coating method. However, these conventional techniques have the problem that thin films of 10 μm or less cannot be uniformly coated due to limitations in machining precision.

[0021] The present invention is intended to solve the above-mentioned problems, and provides a method for manufacturing a stencil for fine pattern printing, which prevents damage to the stencil even when the length of the stencil is increased and the pattern density is increased, enables the production of a closed curve pattern stencil, improves printing quality, and enables uniform coating while arbitrarily adjusting the thickness of a thin film coating on a high-viscosity material.

[0022] In order to achieve the above object, the present invention relates to a method for manufacturing a metal screen mask for a fine pattern, comprising: a stencil pattern corresponding to a fine printing pattern; and a bridge formed across the stencil pattern and having a height smaller than the height of the stencil pattern to support the shape of the stencil pattern; the method comprising: a step of forming a fine protection bridge pattern on a glass substrate with chrome to manufacture a protection bridge photomask; a step of applying a primary photoresist to a glass substrate having a seed layer formed thereon to manufacture a primary exposure substrate; a step of placing the protection bridge photomask on the primary exposure substrate and exposing it to ultraviolet rays; a step of developing the exposed primary exposure substrate in a developer to manufacture a protection bridge exposure pattern; a step of applying a secondary photoresist to the protection bridge exposure pattern to manufacture a secondary exposure substrate; a step of forming a fine stencil pattern to be printed on a glass substrate with chrome to manufacture a stencil pattern photomask; The technical gist of the present invention is a method for manufacturing a metal screen mask for a fine pattern, comprising the steps of: placing a stencil pattern photomask on the secondary exposure substrate and exposing it to ultraviolet rays; developing the exposed secondary exposure substrate in a developer to produce a stencil exposure pattern; performing metal plating on the stencil exposure pattern; and obtaining a metal screen mask on which the stencil master pattern is formed by removing the stencil exposure pattern and leaving only the metal plating portion.

[0023] The present invention also preferably provides a method for manufacturing a metal screen mask for a fine pattern, characterized in that after the step a, a step of performing metal plating on the protection bridge exposure pattern to fill the protection bridge pattern trench with metal plating is performed.

[0024] In addition, it is preferable that the stencil pattern photomask of the step b further includes a metal screen mask protection pattern that reduces tensile stress added to the printing area outside the printing area, which is a method for manufacturing a metal screen mask for a fine pattern.

[0025] In addition, it is preferable that the metal screen mask protection pattern be a method for manufacturing a fine pattern metal screen mask, characterized in that it is a pattern that is elastically stretched against tensile stress.

[0026] In addition, it is preferable that the metal screen mask protection pattern be formed by a method for manufacturing a metal screen mask for a fine pattern, characterized in that the metal screen mask protection pattern is formed by a straight line pattern, a diagonal pattern, a sawtooth pattern, a curved pattern, a mesh pattern, or a combination thereof.

[0027] In addition, it is preferable that the metal screen mask protection pattern be formed with a pattern line width of 1 to 20 um and a pattern pitch range of 20 to 200 um, which is a method for manufacturing a metal screen mask for a fine pattern.

[0028] In addition, it is preferable that the first photosensitive agent be formed to a thickness in the range of 5 um to 50 um by a liquid photosensitive agent coating process using spin coating or spray coating or a laminating process using a film-type photosensitive agent, using a method for manufacturing a metal screen mask for a fine pattern.

[0029] In addition, it is preferable that the secondary photosensitive agent be a method for manufacturing a metal screen mask for a fine pattern, characterized in that it is formed to a thickness in the range of 5 um to 50 um through a laminating process using a film-type photosensitive agent.

[0030] According to the present invention described above, there is an advantage in that a method for manufacturing a stencil for fine pattern printing is provided, which prevents damage to the stencil even when the length of the stencil is increased and the pattern density is increased, enables the production of a closed curve pattern stencil, improves printing quality, and enables uniform coating of a thin film coating thickness on a high-viscosity material while arbitrarily adjusting the thickness.

[0031] Figure 1 is a process diagram of the present invention.

[0032] Figure 2 is a stencil pattern structure diagram of a stencil for fine pattern printing formed by the present invention, wherein Figure 2a is a cross-sectional view, Figure 2b is a bottom perspective view of Figure 2a, and Figure 2c is a top perspective view of Figure 2a.

[0033] Figure 3 is a printing execution diagram using a stencil for fine pattern printing formed by the present invention.

[0034] Figure 4 is a process diagram for another embodiment of the present invention.

[0035] Figure 5 is a process diagram of an embodiment of forming a metal screen mask protection pattern in the present invention.

[0036] Figure 6 is a plan view of an embodiment of a stencil pattern photomask on which a metal screen mask protection pattern of the present invention is formed.

[0037] Fig. 7 is a plan view of a metal screen mask formed by Fig. 6.

[0038] The present invention will be described with reference to the drawings below. In explaining the present invention, if it is determined that a detailed description of a related known technology or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.

[0039] And the terms described below are terms defined in consideration of their functions in the present invention, and may vary depending on the intention or custom of the user or operator, so their definitions should be made based on the contents throughout this specification explaining the present invention.

[0040] The following drawing 1 is a process diagram of the present invention, and drawing 2 is a stencil pattern structure diagram of a fine pattern printing stencil formed by the present invention, wherein drawing 2a is a cross-sectional view, drawing 2b is a bottom perspective view of drawing 2a, drawing 2c is a top perspective view of drawing 2a, drawing 3 is a printing execution diagram using a fine pattern printing stencil formed by the present invention, drawing 4 is a process diagram of another embodiment of the present invention, drawing 5 is a process diagram of an embodiment of forming a metal screen mask protection pattern in the present invention, drawing 6 is a plan view of one embodiment of a stencil pattern photomask on which a metal screen mask protection pattern of the present invention is formed, and drawing 7 is a plan view of a metal screen mask formed by drawing 6.

[0041]

[0042] The present invention relates to a method for manufacturing a metal screen mask for a fine pattern, wherein the metal screen mask for a fine pattern is characterized in that, as illustrated in FIG. 2, a micro- or nano-scale fine printing pattern is formed as a stencil pattern (100') on a metal screen mask (400), and a bridge pattern (10') is formed across the stencil pattern (100') and has a height smaller than the height of the stencil pattern to support the shape of the stencil pattern (100'). (In the following description, the stencil pattern and the bridge pattern are illustrated and described with the same drawing number without distinction between relief and intaglio.)

[0043]

[0044] Hereinafter, a method for manufacturing a metal screen mask for a micro-pattern of the present invention will be described with reference to FIG. 1.

[0045] The embodiment of Fig. 1 is described using a positive type photosensitizer, and since anyone with average knowledge in the art can perform the negative type photosensitizer by reversing the pattern according to the contents of the present invention, a description thereof will be omitted.

[0046] In FIG. 1, the first step (S100) of the present invention is a step (S100) of forming a micro-protection bridge pattern (10') on a glass substrate (13) using chrome (11) to produce a protection bridge photomask (10).

[0047] The above-mentioned micro protection bridge pattern (10') is formed by printing only the bridge shape crossing the stencil pattern (100') that forms the printing surface, and as shown in Fig. 1, the micro protection bridge pattern (10') is formed in a shade that is transparently exposed.

[0048] The above bridge shape can be designed to fit the stencil pattern (100') to be protected. In the drawing of the present invention, when the stencil pattern (100') is a narrow and long line, the bridge shape is depicted as lines crossing the line, but it is not necessarily limited thereto. When protecting a wide surface, it can be formed as a mesh covering the surface.

[0049]

[0050] The next step (S200) is to manufacture a first exposure substrate (30-1) by applying a first photosensitive agent (35) to a glass substrate (31) on which a seed layer (33) is formed.

[0051] This step (S200) is a step of first applying a photosensitive agent of a certain thickness on a glass substrate (31) for exposure. The photosensitive agent can be applied by applying a liquid process such as spin coating or spray coating, or a laminating process using a photosensitive agent in a film form. It is preferable that the thickness of the photosensitive agent be formed in the range of 5 um to 50 um.

[0052]

[0053] The next step (S300) is to place a protective bridge photomask (10) on the first exposure substrate (30-1) and expose it to ultraviolet rays.

[0054] In this step (S300), when the protective bridge photomask (10) is placed on the primary exposure substrate (30-1) on which the primary photosensitive agent (35) is applied and ultraviolet rays are irradiated, only the fine protective bridge pattern (10') portion of the protective bridge photomask (10) is transparent and is therefore exposed to ultraviolet rays.

[0055]

[0056] The next step (S400) is step a (S400) in which the exposed first exposure substrate (30-1) is developed in a developer to produce a protective bridge exposure pattern (300).

[0057] In step a (S400), the exposed first exposure substrate (30-1) undergoes a development process, and only the area of ​​the protective bridge pattern (10') exposed to ultraviolet rays is removed to form a protective bridge exposure pattern (300) in which the protective bridge pattern (10') is engraved on the first photosensitive agent (35).

[0058]

[0059] The next step (S500) is a step of manufacturing a secondary exposure substrate (30-2) by applying a secondary photosensitive agent (350) to the above-mentioned protective bridge exposure pattern (300).

[0060] In this step (S500), the application of the secondary photosensitive agent (350) is performed by a laminating process using a film-type photosensitive agent to protect the protective bridge pattern (10') formed on the primary photosensitive agent (35), and it is preferable to form it in a thickness range of 5 um to 50 um.

[0061]

[0062] The next step (S600) is step b (S600) of forming a fine stencil pattern (100') to be printed on a glass substrate (130) using chrome (110) to produce a stencil pattern photomask (100).

[0063] In the present invention, the above steps (S100) and step b (S600) are not restricted to a specific order, and are arranged in order only to explain the process.

[0064] The above stencil pattern photomask (100) is formed as a stencil pattern (100') with a fine-scale printing pattern to be printed using a screen technique, and as shown in step (S600) of FIG. 1, the stencil pattern (100') portion is formed as an opaque shade.

[0065]

[0066] The next step (S700) is to place a stencil pattern photomask (100) on the secondary exposure substrate (30-2) and expose it to ultraviolet rays.

[0067] In this step (S700), only the stencil pattern (100') portion of the stencil pattern photomask (100) is opaque, so only the portion other than the stencil pattern (100') is exposed to ultraviolet rays.

[0068]

[0069] The next step (S800) is to develop the exposed secondary exposure substrate (30-2) in a developer to create a stencil exposure pattern (3000).

[0070] In this step (S800), the exposed secondary exposure substrate (30-2) undergoes a development process, and only the area other than the stencil pattern (100') exposed to ultraviolet rays is removed as shown in step (S800) of FIG. 1, thereby forming a stencil exposure pattern (3000) in which the stencil pattern (100') is embossed on the photosensitive agent.

[0071] In this step (S800), only the stencil pattern (100') is engraved, so the bridge pattern (10') that falls outside the stencil pattern area is removed during the developing process.

[0072] Accordingly, only the stencil pattern (100') shape is engraved, and the bridge pattern (10') remains below the stencil pattern (100') shape.

[0073]

[0074] The next step (S900) is a step of performing metal plating (40) on the stencil exposure pattern (3000).

[0075] In this step (S900), the remaining area except for the stencil pattern (100') is filled with metal using a metal plating process such as nickel or nickel alloy plating.

[0076] As shown in step (S900) of Fig. 1, it is noteworthy that in this step (S900), the bridge pattern (10') formed on the lower side of the stencil pattern (100') shape by the metal plating process is also filled with metal plating (40).

[0077]

[0078] At this time, it is preferable that the thickness of the metal plating (400) be formed lower than the relief of the stencil pattern (100') and higher than the intaglio of the protective bridge pattern (10').

[0079] This is because the stencil pattern (100') must be formed as a through hole through which printing ink passes to form a pattern in a subsequent process.

[0080]

[0081] The next step (S1000) is a step of removing the stencil exposure pattern (3000) and leaving only the metal plating (40) portion to obtain a metal screen mask (400) on which the stencil pattern (100') is formed.

[0082] In this step (S1000), the entire photosensitive agent is removed to obtain a metal screen mask (400) having a stencil pattern (100') including a bridge pattern (10') engraved thereon, as shown in FIG. 2.

[0083]

[0084] The metal screen mask (400) of the present invention manufactured as described above has a bridge pattern (10') formed at a certain height in a stencil pattern (100') penetrating the mask, as shown in the cross-sectional structural diagram of FIG. 2a.

[0085] Accordingly, the metal screen mask is divided into a side where a bridge pattern (10') is formed on the mask surface as shown in FIG. 2b, and a side where a stencil pattern (100') remains circular on the mask surface as shown in FIG. 2c.

[0086]

[0087] When screen printing is performed as shown in Fig. 3 using a metal screen mask formed in this manner, ink is injected in the direction of the surface where the bridge pattern (10') is formed, and the stencil pattern (100') is printed on the surface where the original shape of the stencil pattern (100') remains.

[0088] The above bridge pattern (10') enables the size of the stencil pattern (100') to be controlled on a microscopic scale and has the effect of increasing the rigidity of the metal screen mask (400).

[0089] In addition, since the shape of the stencil pattern (100') consisting of a closed curve can be maintained, a great degree of freedom is provided in the design of the stencil pattern (100').

[0090]

[0091] Meanwhile, since the formation of the bridge pattern (10') affects the stencil pattern (100') and the printing quality, it is preferable to form it independently from the stencil pattern (100') as much as possible.

[0092] To this end, the present invention further includes a step (S450) of filling the trench of the protection bridge pattern (10') with metal plating by performing metal plating on the protection bridge exposure pattern (300) after the step a (S400) as shown in FIG. 4.

[0093] By adding this step (S450), the protective bridge exposure pattern (300) is filled with a bridge pattern (10') in advance with metal plating, thereby preserving the original shape of the bridge pattern (10').

[0094] The addition of this step (S450) has the advantage of preventing damage to the original bridge pattern (10') due to ultraviolet interference that may occur in step (S700).

[0095] In the above step (450), the height of the metal plating is formed lower than the height of the primary photosensitive agent so that the metal plating is not disturbed in the subsequent procedure.

[0096] In addition to this step (S450), in step (S500), since the protective bridge pattern (10') formed on the first photosensitive agent (35) is protected by metal plating, the photosensitive agent can be applied by selectively applying a liquid process such as spin coating or spray coating or a laminating process using a film-type photosensitive agent. It is preferable that the thickness of the photosensitive agent be formed in the range of 5 um to 50 um.

[0097]

[0098] The present invention manufactures a metal screen mask (400) for a fine pattern as described above, and as described above, the thickness of the metal screen mask (400) for a fine pattern is formed to be lower than the thickness of the entire photosensitive material laminated on the secondary exposure substrate (30-2).

[0099] Therefore, since the actual size is an ultra-thin film, there is a concern that the printing area (1000) where the stencil pattern (100') is perforated may be damaged during screen printing.

[0100]

[0101] As shown in FIGS. 5 and 6, the metal screen mask (400) for fine patterns is divided into a printing area (1000) where a stencil pattern (100') is formed as the center of the film and printing is performed, and a peripheral area that forms the printing area (1000).

[0102] The main cause of defects in screen printing using a metal screen mask (400) for fine patterns is the difference in stress between the printing area (1000) where the stencil pattern (100') is formed on the film surface of the metal screen mask (400) and the surrounding area.

[0103] In detail, after printing, when the metal screen mask (400) is peeled off, the force transmitted to the metal screen mask (400) is transmitted toward the printing area (1000) where the stencil pattern (100') is formed, causing the stencil pattern (100') to be damaged, thereby degrading the printing quality.

[0104] The present invention has a feature of forming a metal screen mask protection pattern (120) that reduces tensile stress on the periphery of the printing surface of the metal screen mask (400) for the micro-pattern in order to prevent damage to the stencil pattern (100').

[0105]

[0106] To this end, the present invention forms a metal screen mask protection pattern (120) outside the printing area of ​​the stencil pattern photomask (100) in step b (S600) as shown in FIG. 5.

[0107] The above metal screen mask protection pattern (120) is preferably formed as a pattern that is elastically stretched against tensile stress, and can be formed as a straight line pattern, diagonal pattern, sawtooth pattern, curved pattern, mesh pattern, or a combination thereof with a pattern line width of 1 to 20 um and a pattern pitch range of 20 to 200 um.

[0108] As shown in more detail in the embodiment of FIG. 6, when a metal screen mask protection pattern (120) is formed on a stencil pattern photomask (100) in the step b (600), as shown in FIG. 5, the metal screen mask protection pattern (120) is formed together in a subsequent process, so that the metal screen mask protection pattern (120) is formed on a metal screen mask (400) for a fine pattern, as in the embodiment of FIG. 7.

[0109] When force is applied to the surrounding area to peel off the metal screen mask (400), the above metal screen mask protection pattern (120) reduces stress by deformation of the shape of the protection pattern, thereby protecting the screen printing surface.

[0110]

[0111] According to the metal screen mask (400) for fine patterns of the present invention formed in this manner, a thin film coating with high uniformity over a wide area is possible on a high-viscosity material such as a thin film coating for a multilayer ceramic capacitor (MLCC).

[0112] In such large area pattern printing, the bridge shape formed to protect the pattern shape can be designed in a mesh shape.

[0113]

[0114] In addition, the present invention has the advantage of being able to control the thin film coating thickness by controlling the thickness of the photosensitive coating, and forming a highly uniform thin film thickness by controlling the viscosity of the coating solution, the line width, pitch, height of the mesh pattern, and the height of the opening for thin film coating.

[0115]

[0116] The drawings shown for the purpose of explaining the present invention are one embodiment in which the present invention is embodied, and it can be seen that various combinations of forms are possible in order to realize the gist of the present invention as shown in the drawings.

[0117] Accordingly, the present invention is not limited to the above-described embodiments, and as claimed in the following claims, it is possible for anyone with ordinary skill in the art to make various modifications without departing from the spirit of the present invention, and it is said that the technical spirit of the present invention exists to the extent that it is possible to make various modifications without departing from the spirit of the present invention.

[0118] [Explanation of symbols]

[0119] 10: Protective bridge photomask

[0120] 10': Bridge pattern

[0121] 30-1: 1st exposure substrate

[0122] 30-2: Second exposure substrate

[0123] 31: Glass substrate

[0124] 33: Seed layer

[0125] 35: Primary photosensitizer

[0126] 100: Stencil Pattern Photomask

[0127] 100': Stencil pattern

[0128] 120: Metal Screen Mask Protection Pattern

[0129] 300: Protective bridge exposure pattern

[0130] 350: Secondary photosensitizer

[0131] 400: Metal Screen Mask

[0132] 1000: Print area

[0133] 3000: Stencil exposure pattern

Claims

1. A method for manufacturing a metal screen mask for a fine pattern, comprising: a stencil pattern corresponding to a fine printing pattern; and a bridge formed across the stencil pattern and having a height smaller than the height of the stencil pattern to support the shape of the stencil pattern; A step of manufacturing a protective bridge photomask by forming a fine protective bridge pattern on a glass substrate using chrome; A step of manufacturing a first exposure substrate by applying a first photosensitive agent to a glass substrate on which a seed layer has been formed; A step of placing a protective bridge photomask on the first exposure substrate and exposing it to ultraviolet rays; Step a: developing the exposed first exposure substrate in a developer to create a protective bridge exposure pattern; A step of manufacturing a secondary exposure substrate by applying a secondary photosensitive agent to the above-mentioned protective bridge exposure pattern; Step b: forming a fine stencil pattern to be printed on a glass substrate with chrome to produce a stencil pattern photomask; A step of placing a stencil pattern photomask on the above second exposure substrate and exposing it to ultraviolet rays; A step of developing the exposed secondary exposure substrate in a developer to create a stencil exposure pattern; A step of performing metal plating on the above stencil exposure pattern; A step of removing the above stencil exposure pattern and leaving only the metal plating portion to obtain a metal screen mask on which the stencil master pattern is formed; A method for manufacturing a metal screen mask for a micro-pattern, characterized in that it comprises:

2. After step a in paragraph 1, A method for manufacturing a metal screen mask for a fine pattern, characterized by performing a step of filling a protective bridge pattern trench with metal plating by performing metal plating on the above protective bridge exposure pattern.

3. In the stencil pattern photomask of step b in paragraph 1, A method for manufacturing a metal screen mask for a fine pattern, characterized in that a metal screen mask protection pattern is further included outside the printing area to reduce tensile stress added to the printing area.

4. In the third paragraph, the metal screen mask protection pattern A method for manufacturing a metal screen mask for a micro-pattern, characterized in that the pattern is elastically stretched against tensile stress.

5. In the fourth paragraph, the metal screen mask protection pattern A method for manufacturing a metal screen mask for a micro-pattern, characterized in that the metal screen mask is formed by a straight line pattern, a diagonal pattern, a sawtooth pattern, a curved pattern, a mesh pattern, or a combination thereof.

6. In the fifth paragraph, the metal screen mask protection pattern A method for manufacturing a metal screen mask for a fine pattern, characterized in that the pattern line width is formed in a range of 1 to 20 um and the pattern pitch is formed in a range of 20 to 200 um.

7. In paragraph 1, the first photosensitizer or the second photosensitizer A method for manufacturing a metal screen mask for a fine pattern, characterized in that the metal screen mask is formed to a thickness in the range of 5 um to 50 um by a liquid photosensitive coating process using spin coating or spray coating or a laminating process using a film-type photosensitive agent.

8. A metal screen mask for a micropattern manufactured by any one of claims 1 to 7.

9. For metal screen masks for micro-patterns A metal screen mask for a fine pattern, characterized in that a metal screen mask protection pattern is formed around a printing area to reduce tensile stress.

Citation Information

Patent Citations

  • Production of screen mask

    JP1997300840A

  • Suspend metal mask using dummy pattern, and method for manufacturing suspend metal mask using dummy pattern

    JP2016182709A

  • Retractable Structure for Tong Post of Rig Floor

    KR1020210126248A

  • Polishing device and substrate polishing system including the same

    KR1020240159182A

  • KR20220056359A