Component for semiconductor etching process, and manufacturing method therefor
Patent Information
- Application Number
- PCT/KR2024/005834
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-07
AI Technical Summary
The semiconductor etching process faces challenges with plasma resistance, particularly when using high-density fluorine-based gases, leading to local erosion and contaminant particle generation, which increases defects and reduces production yield.
A coating layer containing metal fluoride is formed on the surface of components used in the semiconductor etching process through a reaction with plasma from etching gases, enhancing plasma resistance without altering the physical properties of the substrate.
The metal fluoride coating improves durability and extends the usage time of components, reducing defects and increasing the replacement cycle by enhancing plasma resistance during the semiconductor etching process.
Smart Images

Figure KR2024005834_07112024_PF_FP_ABST
Abstract
Description
Components for semiconductor etching processes and their manufacturing methods
[0001] This invention claims the benefit of Korean Patent Application No. 10-2023-0058679 filed with the Korean Intellectual Property Office on May 4, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a component for a semiconductor etching process and a method for manufacturing the same, and more particularly, to a component for a semiconductor etching process capable of improving plasma resistance by including a coating layer containing a metal fluoride on the surface of the component used in the semiconductor etching process, and a method for manufacturing the same.
[0003] During the manufacturing process of semiconductors and / or displays, plasma-based etching processes are used to form precise patterns. Recently, with the adoption of processes for forming nano-patterns in semiconductors, the difficulty of etching has increased.
[0004] Furthermore, high-density plasma is applied to apply a precise process, and the internal components applied to the chamber used in the process for manufacturing semiconductors exposed to such a high-density plasma environment are mainly made of oxide ceramics such as alumina (Al2O3) and yttria (Y2O3) that have corrosion resistance.
[0005] However, when polycrystalline materials are exposed to a high-density plasma etching environment using fluorine-based gases for a long period of time, particles are removed due to local erosion, which increases the probability of generating contaminant particles. This phenomenon causes defects in semiconductors / displays and adversely affects production yield.
[0006] Therefore, it was necessary to develop a technology that could easily improve plasma resistance without changing the properties of the existing material itself.
[0007] The technical problem to be achieved by the present invention is to provide a component for a semiconductor etching process and a method for manufacturing the same, which can improve resistance to plasma etching performed in a semiconductor manufacturing process by forming a coating layer containing a metal fluoride formed through a reaction with plasma generated from an etching gas on the surface of the component used in the semiconductor etching process.
[0008] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0009] One embodiment of the present invention provides a component (100) for a semiconductor etching process, which includes a substrate (110); and a coating layer (130) provided on at least a portion of the surface of the substrate and containing a metal fluoride.
[0010] According to one embodiment of the present invention, the melting point of the coating layer (130) may be 1,200°C or higher and 2,000°C or lower.
[0011] According to one embodiment of the present invention, the metal fluoride may be one selected from the group consisting of alkali metal fluoride, alkaline earth metal fluoride, transition metal fluoride, and combinations thereof.
[0012] According to one embodiment of the present invention, the metal fluoride may be one selected from the group consisting of AlF3, Al2F3, CaF2, MgF2, MgF3, BaF2, LaF3, LiF, SrF2, and combinations thereof.
[0013] According to one embodiment of the present invention, the thickness of the coating layer (130) may be 0.1 nm or more and 1,000 nm or less.
[0014] According to one embodiment of the present invention, the substrate (110) includes silicon oxide, and the substrate (110) may further include one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, and combinations thereof.
[0015] According to one embodiment of the present invention, the substrate (110) may be amorphous.
[0016] One embodiment of the present invention provides a method for manufacturing a component (100) for a semiconductor etching process, comprising the steps of: providing a substrate (110) (S10); and providing a coating layer (130) by treating the surface of the substrate (110) with plasma derived from an etching gas (S30).
[0017] According to one embodiment of the present invention, the etching gas may include one selected from the group consisting of carbon halides, halogen elements, halogen gases, and combinations thereof.
[0018] According to one embodiment of the present invention, the plasma may be generated by any one of inductively coupled plasma (ICP), capacitively coupled plasma (CCP), reactive ion etching (RIE), magnetically enhanced reactive ion etching (MERIE), electron cyclotron resonance plasma (ECR), remote plasma, or atmospheric pressure plasma (dielectric barrier discharge plasma (DBD plasma).
[0019]
[0020] A component for a semiconductor etching process according to one embodiment of the present invention can increase the durability of the component by improving plasma resistance and increase the use time in a semiconductor etching process, thereby increasing the replacement cycle of the component.
[0021] A method for manufacturing a component for a semiconductor etching process according to one embodiment of the present invention can easily form a coating layer containing a metal fluoride on a substrate through plasma treatment.
[0022] Figure 1 is a schematic diagram showing an enlarged portion of a semiconductor etching process component according to one embodiment of the present invention.
[0023] Figure 2 is a flowchart of a method for manufacturing a component for a semiconductor etching process according to one embodiment of the present invention.
[0024] Figure 3 is a graph showing the atomic content of the surface analyzed by XPS according to the etching time of Example 1.
[0025] Figure 4 is a graph analyzed by SIMS of Comparative Example 1.
[0026] Figure 5 is a graph analyzed by SIMS of Example 1.
[0027] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0028] In this specification, “A and / or B” means “A and B, or A or B.”
[0029] The drawings attached to this specification illustrate preferred embodiments of the invention and, together with the description of the invention, serve to explain the principles of the invention, but are not intended to limit the scope of the invention. Furthermore, the shape, size, scale, or ratio of elements in the drawings included in this specification may be exaggerated for clarity.
[0030]
[0031] Hereinafter, the present invention will be described in more detail.
[0032]
[0033] One embodiment of the present invention provides a component (100) for a semiconductor etching process, which includes a substrate (110); and a coating layer (130) provided on at least a portion of the surface of the substrate and containing a metal fluoride.
[0034] A component (100) for a semiconductor etching process according to one embodiment of the present invention can increase the durability of the component by improving plasma resistance and increase the use time in the semiconductor etching process, thereby increasing the replacement cycle of the component.
[0035] FIG. 1 is a schematic diagram illustrating an enlarged portion of a semiconductor etching process component (100) according to an embodiment of the present invention. Referring to FIG. 1, the semiconductor etching process component (100) according to an embodiment of the present invention will be described in detail.
[0036] According to one embodiment of the present invention, the component for a semiconductor etching process includes a substrate (110). By including the component for a semiconductor etching process as described above, plasma resistance can be improved in the etching process of manufacturing a semiconductor.
[0037] According to one embodiment of the present invention, the substrate (100) may have any one shape among a focus ring, an edge ring, a covering ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By selecting the shape of the above-described substrate as described above, it is possible to apply the substrate to a product in a chamber that performs an etching process in the semiconductor manufacturing process, and by applying it to the etching process chamber, the lifespan of the product can be improved, and foreign substances generated during the etching process can be minimized, thereby reducing the occurrence of defects in the semiconductor.
[0038] According to one embodiment of the present invention, the component for a semiconductor etching process includes a coating layer (130) provided on at least a portion of the surface of the substrate. Specifically, the component for a semiconductor etching process may be one in which the coating layer (130) is provided on a portion of the surface of the substrate or on the entire surface of the substrate. More specifically, the component for a semiconductor etching process may be one in which the coating layer is provided on a portion etched by the plasma, and preferably, the coating layer may be provided so as to have a predetermined additional area on the outer portion of the portion etched by the plasma. As described above, by providing the coating layer on the surface of the substrate or on the entire surface of the substrate, plasma resistance can be improved.
[0039] According to one embodiment of the present invention, the coating layer (130) contains a metal fluoride. The metal fluoride may be formed by a reaction between plasma derived from an etching gas and a component contained on the surface of the substrate and included in the coating layer. As described above, by including the metal fluoride in the coating layer, the plasma resistance against plasma generated during the etching process of the semiconductor manufacturing process can be improved.
[0040] According to one embodiment of the present invention, the coating layer (130) may include silicon oxide. Specifically, the surface of the substrate may react with plasma derived from an etching gas to form a metal fluoride, and some unreacted portions may contain silicon oxide, which is a main component contained in the substrate. As described above, since the coating layer (130) includes silicon oxide, even if the coating layer is provided on the substrate, changes in physical properties may be minimized.
[0041] According to one embodiment of the present invention, the coating layer (130) may further include one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, and combinations thereof. More specifically, the coating layer (130) may further include one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, lanthanide oxides, other metal oxides, metalloid oxides, and combinations thereof. By further including the components included in the coating layer as described above, the plasma resistance of the component for the semiconductor etching process can be improved, thermal shock can be prevented, and the permittivity of the component for the semiconductor etching process can be controlled.
[0042] According to one embodiment of the present invention, the coating layer (130) may include a metal fluoride formed by the reaction of the surface of the substrate (110) with an etching gas. Specifically, the coating layer (130) may have a coating layer including a metal fluoride by forming a metal fluoride by reacting a metal oxide included in the surface of the substrate layer with plasma derived from an etching gas. As described above, since the coating layer (130) includes a metal fluoride formed by the reaction of the surface of the substrate (110) with an etching gas, the thickness of the coating layer can be implemented to be thin, and resistance to plasma can be improved during the etching process, thereby extending the replacement cycle of components for a semiconductor etching process.
[0043] According to one embodiment of the present invention, the content of the metal fluoride in the coating layer may be 50 parts by weight or more and 100 parts by weight or less with respect to 100 parts by weight of the coating layer. Specifically, the content of the metal fluoride in the coating layer may be 60 parts by weight or more and 100 parts by weight or less, 70 parts by weight or more and 100 parts by weight or less, 80 parts by weight or more and 100 parts by weight or less, 85 parts by weight or more and 100 parts by weight or less, 90 parts by weight or more and 100 parts by weight or less, 95 parts by weight or more and 100 parts by weight or less, 90 parts by weight or more and 99 parts by weight or less, 91 parts by weight or more and 98 parts by weight or less, 92 parts by weight or more and 97 parts by weight or less, 93 parts by weight or more and 96 parts by weight or less, or 94 parts by weight or more and 95 parts by weight or less with respect to 100 parts by weight of the coating layer. By controlling the content of the metal fluoride in the coating layer within the above-described range, the plasma resistance of the coating layer can be improved and the physical properties of the substrate can be prevented from changing.
[0044] According to one embodiment of the present invention, the coating layer (130) may include unavoidable impurities. As described above, the coating layer (130) includes unavoidable impurities, and by minimizing the total weight of the unavoidable impurities contained in the coating layer, the coating layer can prevent deterioration of the physical properties required for a component for a semiconductor etching process.
[0045] According to one embodiment of the present invention, the melting point of the coating layer (130) may be 1,200°C or more and 2,000°C or less. Specifically, the melting point of the coating layer (130) may be 1,300°C or more and 1,900°C or less, 1,400°C or more and 1,800°C or less, or 1,500°C or more and 1,700°C or less. By controlling the melting point of the coating layer within the above-described range, the resistance of the semiconductor etching process component to plasma can be improved, and the replacement cycle of the component can be extended.
[0046] According to one embodiment of the present invention, the metal fluoride may be one selected from the group consisting of alkali metal fluorides, alkaline earth metal fluorides, transition metal fluorides, and combinations thereof. Specifically, the metal fluoride may be one selected from the group consisting of alkali metal fluorides, alkaline earth metal fluorides, transition metal fluorides, lanthanide oxides, other metal oxides, metalloid oxides, and combinations thereof. By selecting the metal fluoride from the above, the plasma resistance of the component for the semiconductor etching process can be improved, and the replacement cycle of the component can be extended.
[0047] According to one embodiment of the present invention, the metal fluoride may be one selected from the group consisting of AlF3, Al2F3, CaF2, MgF2, MgF3, BaF2, LaF3, LiF, SrF2, and combinations thereof. By selecting the metal fluoride from the above, the plasma resistance of the semiconductor etching process component can be improved, and the replacement cycle of the component can be extended.
[0048] According to one embodiment of the present invention, the thickness of the coating layer (130) may be 0.1 nm or more and 1,000 nm or less. In the present specification, the thickness may mean an average thickness or a thickness at a specific point. Specifically, the thickness of the coating layer (130) may be 0.1 nm or more and 1,000 nm or less, 1 nm or more and 950 nm or less, 5 nm or more and 900 nm or less, 10 nm or more and 850 nm or less, 50 nm or more and 800 nm or less, 100 nm or more and 700 nm or less, 200 nm or more and 600 nm or less, or 300 nm or more and 500 nm or less. By controlling the thickness of the coating layer within the above-described range, the plasma resistance can be improved while maintaining the physical properties of the substrate.
[0049] According to one embodiment of the present invention, the substrate (110) may include silicon oxide. Specifically, the substrate (110) may include SiO2. More specifically, the substrate may be a network formed by silicon atoms and oxygen atoms in an amorphous form. Furthermore, the substrate may include only silicon oxide. Including only silicon oxide may mean that no components other than inevitable impurities are included. As described above, by the substrate including silicon oxide, the plasma resistance of the component for the semiconductor etching process can be improved.
[0050] According to one embodiment of the present invention, the substrate (110) may further include one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, and combinations thereof. Specifically, the substrate may further include one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, lanthanide oxides, other metal oxides, metalloid oxides, and combinations thereof. More specifically, the substrate may be one in which one selected from the group consisting of alkali metal atoms, alkaline earth metal atoms, transition metal atoms, lanthanide atoms, other metal atoms, metalloid atoms, and combinations thereof and oxygen atoms form a network in an amorphous form. By selecting the components included in the substrate from the above-described components, the plasma resistance of the component for the semiconductor etching process can be improved, and the plasma resistance can be improved by controlling the components of the metal fluoride included in the coating layer.
[0051] According to one embodiment of the present invention, the above-mentioned substrate (110) may be included without limitation as long as it corresponds to a component capable of being vitrified.
[0052] According to one embodiment of the present invention, the substrate (110) may include unavoidable impurities. As described above, the substrate (110) includes unavoidable impurities, and by minimizing the total weight of the unavoidable impurities contained in the substrate, the substrate can prevent deterioration of the physical properties required as a component for a semiconductor etching process.
[0053] According to one embodiment of the present invention, the substrate (110) may be amorphous. In the present specification, "amorphous" may mean glassy, meaning that it does not form a particle structure or a regular structure. By implementing the structure of the substrate as amorphous as described above, the plasma resistance of the semiconductor etching process component can be improved.
[0054] According to one embodiment of the present invention, the alkali metal may be a Group 1 element. Specifically, the alkali metal may be one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), and combinations thereof. Furthermore, the alkaline earth metal may be a Group 2 element. Specifically, the alkaline earth metal may be one selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), and combinations thereof. In addition, the transition metal may be a Group 3 to 12 element. By selecting the alkali metal, the alkaline earth metal, and the transition metal from the above, the plasma resistance of the component for the semiconductor etching process can be improved.
[0055] According to one embodiment of the present invention, the component for the semiconductor etching process may be a component placed inside a chamber in which etching applied in a semiconductor manufacturing process is performed. Specifically, the component for the semiconductor etching process may be any one of a focus ring, an edge ring, a covering ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By using the semiconductor etching process component described above, the resistance to plasma in the semiconductor manufacturing process can be improved, thereby extending the usage time, and minimizing the cost required for semiconductor manufacturing.
[0056]
[0057] One embodiment of the present invention provides a method for manufacturing a component (100) for a semiconductor etching process, comprising the steps of: providing a substrate (110) (S10); and providing a coating layer (130) by treating the surface of the substrate (110) with plasma derived from an etching gas (S30).
[0058] A method for manufacturing a component for a semiconductor etching process according to one embodiment of the present invention can easily form a coating layer containing a metal fluoride on a substrate through plasma treatment.
[0059] FIG. 2 is a flowchart of a method for manufacturing a component for a semiconductor etching process according to an embodiment of the present invention. Referring to FIG. 2, a method for manufacturing a component for a semiconductor etching process according to an embodiment of the present invention will be described in detail.
[0060]
[0061] According to one embodiment of the present invention, the method for manufacturing a component for a semiconductor etching process includes a step (S10) of providing a substrate (110). Specifically, the step of providing the substrate may include melting a component included in the above-described substrate to produce a melt, injecting the melt into a mold having an internal space in the shape of the component for a semiconductor etching process, and cooling the melt to provide the substrate. Alternatively, the step of providing the substrate may include melting and cooling the component included in the above-described substrate, and then melting it again to produce a melt, injecting the resulting melt into a mold having an internal space in the shape of the component for a semiconductor etching process, to provide the substrate. Furthermore, the step of providing the substrate may include injecting a component included in the substrate or a material obtained by melting and then cooling the component included in the substrate into a mold having an internal space in the shape of the component for a semiconductor etching process, and heating and sintering the material to provide the substrate. In addition, the step of providing the substrate may include preparing a substrate that is a commercial product. That is, as long as the substrate is placed in a space for plasma processing, the method of providing the substrate may be applied without limitation. As described above, since the method for manufacturing the component for the semiconductor etching process includes the step (S10) of providing a substrate (110), the plasma resistance can be easily improved without changing the physical properties of the existing component for the semiconductor etching process.
[0062] According to one embodiment of the present invention, the method for manufacturing a component for a semiconductor etching process includes a step (S30) of forming a coating layer (130) by treating the surface of the substrate (110) with plasma derived from an etching gas. As described above, by forming the coating layer through a reaction between the surface of the substrate (110) and the plasma derived from the etching gas, the coating layer can be easily formed, and the thickness of the coating layer can be implemented thinner than that of a conventional method for forming a coating layer without changing the physical properties of the substrate, and the plasma resistance of the component can be improved.
[0063] According to one embodiment of the present invention, the plasma may be derived from an etching gas. By generating plasma from the etching gas as described above, the components of the coating layer can be controlled, and the plasma resistance of the component can be improved.
[0064] According to one embodiment of the present invention, in the method for manufacturing a component for a semiconductor etching process, the step (S30) of providing the coating layer may be such that a substrate having a shape of a component for a semiconductor etching process is used in an etching process during a process of manufacturing a semiconductor, and the coating layer is formed by plasma used in the etching process. As described above, even if the coating layer is not formed by separately treating plasma to the substrate, the plasma resistance of the component can be improved by providing the coating layer on the substrate during the semiconductor manufacturing process.
[0065] According to one embodiment of the present invention, the etching gas may include one selected from the group consisting of carbon halides, halogen elements, halogen gases, and combinations thereof. By controlling the components of the etching gas as described above, the type and content of the metal fluoride included in the coating layer can be controlled, and the plasma resistance of the component can be improved.
[0066] According to one embodiment of the present invention, the etching gas may include one selected from the group consisting of CF4, C4F6, CF3, CF2, CF, F, F2, BrF3, BrF5, ClF3, and combinations thereof. By controlling the components of the etching gas as described above, the type and content of the metal fluoride included in the coating layer can be controlled, and the plasma resistance of the component can be improved.
[0067] According to one embodiment of the present invention, the plasma may be generated by any one of inductively coupled plasma (ICP), capacitively coupled plasma (CCP), reactive ion etching (RIE), magnetically enhanced reactive ion etching (MERIE), electron cyclotron resonance plasma (ECR), remote plasma, or atmospheric pressure plasma (dielectric barrier discharge plasma) methods. Specifically, the plasma may be applied without limitation as long as it is a method capable of generating a conventional plasma. Preferably, the plasma may be a plasma generating method used in an etching process during a semiconductor manufacturing process. By selecting a method for generating the plasma as described above, a coating layer can be easily formed on the substrate, and the plasma resistance of the component can be improved.
[0068] According to one embodiment of the present invention, the RF power applied for generating the plasma may be 100 W or more and 900 W or less. Specifically, the RF power applied for generating the plasma may be 150 W or more and 850 W or less, 200 W or more and 800 W or less, 250 W or more and 750 W or less, 300 W or more and 700 W or less, 350 W or more and 650 W or less, 400 W or more and 600 W or less, or 450 W or more and 550 W or less. By controlling the RF power applied for generating the plasma within the above-described range, the component and content of the metal fluoride included in the coating layer can be controlled.
[0069] According to one embodiment of the present invention, the time for treating the plasma to form the coating layer may be 30 minutes or more and 300 minutes or less. Specifically, the time for treating the plasma to form the coating layer may be 60 minutes or more and 270 minutes or less, 90 minutes or more and 240 minutes or less, 120 minutes or more and 210 minutes or less, or 150 minutes or more and 180 minutes or less. By controlling the time for treating the plasma to form the coating layer within the above-described range, the thickness of the coating layer can be controlled.
[0070] According to one embodiment of the present invention, the pressure of the etching gas may be 1 mTorr or more and 20 mTorr or less. In the present specification, the pressure of the etching gas may mean the partial pressure of the etching gas in a space provided for plasma treatment, i.e., a chamber. Specifically, the pressure of the etching gas may be 2 mTorr or more and 19 mTorr or less, 3 mTorr or more and 18 mTorr or less, 4 mTorr or more and 17 mTorr or less, 5 mTorr or more and 16 mTorr or less, 6 mTorr or more and 15 mTorr or less, 8 mTorr or more and 14 mTorr or less, 9 mTorr or more and 13 mTorr or less, or 0 mTorr or more and 12 mTorr or less. By controlling the pressure of the etching gas within the above-described range, the content of the metal fluoride included in the coating layer can be controlled, and the thickness of the coating layer can be controlled.
[0071] According to one embodiment of the present invention, the range of the bias voltage formed for generating the plasma may be 100 W or more and 300 W or less. Specifically, the range of the bias voltage formed for generating the plasma may be 110 W or more and 290 W or less, 120 W or more and 280 W or less, 130 W or more and 270 W or less, 140 W or more and 260 W or less, 150 W or more and 250 W or less, 160 W or more and 240 W or less, 170 W or more and 230 W or less, 180 W or more and 220 W or less, or 190 W or more and 210 W or less. By controlling the range of the bias voltage formed for generating the plasma within the above-described range, the thickness of the coating layer and the content of the metal fluoride included in the coating layer can be controlled.
[0072] According to one embodiment of the present invention, the etching gas may further contain an inert gas and oxygen. As described above, by the etching gas further containing an inert gas and oxygen, it is possible to prevent impurities from being included in the coating layer due to other components contained in the plasma treatment atmosphere.
[0073] According to one embodiment of the present invention, the flow rate of the etching gas may be 5 sccm or more and 40 sccm or less. Specifically, the flow rate of the etching gas may be 7 sccm or more and 38 sccm or less, 9 sccm or more and 36 sccm or less, 11 sccm or more and 34 sccm or less, 13 sccm or more and 32 sccm or less, 15 sccm or more and 30 sccm or less, 17 sccm or more and 28 sccm or less, 19 sccm or more and 26 sccm or less, or 21 sccm or more and 24 sccm or less. By controlling the flow rate of the etching gas within the above-described range, the thickness of the coating layer can be controlled, and the content of metal fluoride included in the coating layer can be controlled to improve plasma resistance.
[0074] According to one embodiment of the present invention, the flow rate of the inert gas may be 5 sccm or more and 80 sccm or less. Specifically, the flow rate of the inert gas may be 10 sccm or more and 75 sccm or less, 15 sccm or more and 70 sccm or less, 20 sccm or more and 65 sccm or less, 25 sccm or more and 60 sccm or less, 30 sccm or more and 55 sccm or less, 35 sccm or more and 50 sccm or less, or 40 sccm or more and 45 sccm or less. By controlling the flow rate of the inert gas within the above-described range, inevitable impurities that may be included in the coating layer can be minimized.
[0075] According to one embodiment of the present invention, the flow rate of the oxygen may be 1 sccm or more and 20 sccm or less. Specifically, the flow rate of the oxygen may be 2 sccm or more and 19 sccm or less, 3 sccm or more and 18 sccm or less, 4 sccm or more and 17 sccm or less, 5 sccm or more and 16 sccm or less, 6 sccm or more and 15 sccm or less, 7 sccm or more and 14 sccm or less, 8 sccm or more and 13 sccm or less, 9 sccm or more and 12 sccm or less, or 10 sccm or more and 11 sccm or less. By controlling the flow rate of the oxygen within the above-described range, it is possible to minimize unavoidable impurities that may be included in the coating layer, and to minimize changes in the physical properties of the substrate.
[0076] According to one embodiment of the present invention, the inert gas may be one selected from the group consisting of helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe), radon (Rn), oganesson (Og), and combinations thereof. By selecting the inert gas from the above, it is possible to minimize unavoidable impurities that may be included in the coating layer.
[0077] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0078]
[0079] <Manufacturing Example>
[0080]
[0081] A mixture containing 50 wt% silicon oxide (SiO2), 30 wt% aluminum oxide (Al2O3), and 20 wt% magnesium oxide (MgO) was heated and melted, and the melt was poured into an edge ring-shaped mold and solidified to form a substrate.
[0082]
[0083] <Example 1>
[0084] The substrate manufactured in the above manufacturing example was placed in the chamber of a plasma generator (MTM, NIE150) whose plasma source was ICP. Thereafter, CF4, Ar, and O2 were used as etching gases at flow rates of 10 sccm, 10 sccm, and 5 sccm, respectively, and an RF power of 120 W was applied to the plasma generator to generate plasma, thereby treating the substrate with plasma for 180 minutes to manufacture a component having a coating layer formed thereon.
[0085]
[0086] <Comparative Example 1>
[0087] The substrate manufactured in the above manufacturing example was used as a component.
[0088]
[0089] <Comparative Example 2>
[0090] A coating layer was formed by spraying a powder containing 50 wt% silicon oxide (SiO2), 29 wt% aluminum oxide (Al2O3), 19 wt% magnesium oxide (MgO), 1 wt% aluminum fluoride (AlF3), and 1 wt% magnesium fluoride (MgF2) onto the substrate manufactured in the above manufacturing example using an aerosol deposition.
[0091]
[0092] Fig. 3 is a graph showing the surface atomic content analyzed according to the etching time of Example 1 using XPS (X-ray photoelectron spectroscopy). Referring to Fig. 3, in Example 1, it was confirmed that a coating layer was formed from the confirmation of Mg 1s and F 1s at the beginning of etching.
[0093] Fig. 4 is a graph analyzed by SIMS (Secondary Ion Mass Spectrometry) of Comparative Example 1. Fig. 5 is a graph analyzed by SIMS (Secondary Ion Mass Spectrometry) of Example 1. Referring to Fig. 4, it was confirmed that magnesium fluoride was not formed in Comparative Example 1 because separate plasma treatment was not performed. In contrast, referring to Fig. 5, it was confirmed that in Example 1, a coating layer including magnesium fluoride and aluminum fluoride was formed through plasma treatment, and that after the etching process continued for 1,500 seconds, a substrate not including the metal fluoride was exposed.
[0094]
[0095] <Experimental Example 1: Evaluation of Plasma Resistance>
[0096] For Example 1, Comparative Example 1, and Comparative Example 2, an ICP device (MTM, NIE150) was used, and the RF power was set to 120 W. Then, the flow rates of Ar, CF4, and O2 were mixed at 10 sccm, 10 sccm, and 5 sccm, respectively, and plasma was generated to etch each of Example 1 and Comparative Example 1 for 180 minutes, and the etched depth was measured.
[0097]
[0098] <Experimental Example 2: Coating Layer Thickness Analysis>
[0099] For Example 1, Comparative Example 1, and Comparative Example 2, an ICP device (MTM, NIE150) was used, and the RF power was set to 120 W. Then, the flow rates of Ar, CF4, and O2 were mixed at 10 sccm, 10 sccm, and 5 sccm, respectively, and plasma was generated to etch Example 1 and Comparative Example 1, respectively, and the thickness of the coating layer was calculated using a confocal laser microscope.
[0100] Etching depth (㎛) Example 12.7 Comparative Example 13 Comparative Example 215.3
[0101] Referring to Table 1 above, it was confirmed that Example 1 and Comparative Example 1 had a small etching depth even under the same etching conditions due to the formation of a coating layer containing a metal fluoride. In contrast, it was confirmed that Comparative Example 2 had a larger etching depth than Example 1 and Comparative Example 1 due to the absence of a coating layer.
[0102] Thickness of coating layer (nm) Example 1 Less than 150 Comparative Example 1 - Comparative Example 210,000 or more
[0103] Referring to Table 2 above, the thickness of the coating layer could not be measured in Comparative Example 1 because the coating layer did not exist. It was confirmed that the coating layer of Comparative Example 2 was thicker than that of Example 1. This was because the strength of the substrate was reduced due to the stress generated by the thickness of the coating layer of Comparative Example 2. In contrast, it was confirmed that the strength of the substrate was not reduced due to the coating layer in Example 1 by forming a coating layer with a thickness of several tens of nm. Furthermore, Comparative Example 2 has a problem in that grain boundaries are formed on the surface because the components included in the coating are not vitrified, which leads to the generation of a large number of particles and weakened plasma resistance, and the uniformity of the fluoride is not secured. Furthermore, in Comparative Example 2, the adhesion between the coating layer and the substrate is weakened, weakening the plasma resistance, and even if the substrate is single-coated with fluoride, the same problem as in Comparative Example 2 may occur.
[0104]
[0105] A component for a semiconductor etching process according to one embodiment of the present invention and a method for manufacturing the same can easily form a coating layer containing a metal fluoride through surface treatment of a substrate with plasma, thereby improving the plasma resistance of the component.
[0106] [Explanation of symbols]
[0107] 100: Parts
[0108] 110: Description
[0109] 130: Coating layer
[0110] S10: Preparation stage
[0111] S30: Coating layer preparation stage
Claims
1. A component for a semiconductor etching process, comprising: a substrate; and a coating layer containing a metal fluoride, provided on at least a portion of the surface of the substrate.
2. In claim 1, A component for a semiconductor etching process, wherein the melting point of the above coating layer is 1,200 ℃ or more and 2,000 ℃ or less.
3. In claim 1, A component for a semiconductor etching process, wherein the metal fluoride is one selected from the group consisting of alkali metal fluoride, alkaline earth metal fluoride, transition metal fluoride, and combinations thereof.
4. In claim 1, A component for a semiconductor etching process, wherein the metal fluoride is one selected from the group consisting of AlF3, Al2F3, CaF2, MgF2, MgF3, BaF2, LaF3, LiF, SrF2, and combinations thereof.
5. In claim 1, A component for a semiconductor etching process, wherein the thickness of the coating layer is 0.1 nm or more and 1,000 nm or less.
6. In claim 1, The above description includes silicon oxide, A component for a semiconductor etching process, wherein the above-mentioned material further comprises one selected from the group consisting of alkali metal oxides, alkaline earth metal oxides, transition metal oxides, and combinations thereof.
7. In claim 1, The above description is a component for a semiconductor etching process that is amorphous.
8. Step of preparing the equipment; and A method for manufacturing a component for a semiconductor etching process, comprising: a step of treating the surface of the above-mentioned substrate with plasma derived from an etching gas to form a coating layer; 9. In claim 8, A method for manufacturing a component for a semiconductor etching process, wherein the etching gas comprises one selected from the group consisting of carbon halides, halogen elements, halogen gases, and combinations thereof.
10. In claim 8, A method for manufacturing a component for a semiconductor etching process, wherein the plasma is generated by any one of inductively coupled plasma (ICP), capacitively coupled plasma (CCP), reactive ion etching (RIE), magnetically enhanced reactive ion etching (MERIE), electron cyclotron resonance plasma (ECR), remote plasma, or atmospheric pressure plasma (DBD plasma, dielectric barrier discharge plasma).
Citation Information
Patent Citations
Ceramic protecting coat with excellent resistibility for high density plasma etching and method of coating the same
KR101322783B1
Plasma resistant crystal ceramic coating film and manufacturing method of the same
KR1020110118939A
Protective metal oxy-fluoride coatings
KR1020180132949A
Forklift navigation system using artificial intelligence
KR1020240017310A
KR20210131150A