Novel aromatic textile and manufacturing method therefor

By attaching anionic resin film and covering film resin layer to the textile, the problem of difficult irritation and release control of traditional chemical fragrances is solved, and the odor removal and comfort maintenance of textiles is achieved, which is suitable for the design of new aromatic textiles.

WO2024229762A1PCT designated stage expired Publication Date: 2024-11-14FUJIAN BILLION POLYMERIZATION FIBER TECHNOLOGY IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093303
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Traditional chemical fragrances are prone to irritating and allergic reactions in textiles, and the release time is not easy to control, affecting the comfort and user experience of textiles.

Method used

Cotton fabrics with different yarn branches and fabric structures are adopted. Anionic resin film is attached to the surface of the cotton fabric. The yarn surface is covered with the film resin layer obtained by the reaction of the bridge agent, and the film consisting of organic substances and modified polyether substances. The resin layer, combined with the design of anionic resin film and film resin layer, has prepared a new type of aromatic textile.

Benefits of technology

Effectively eliminates the odor of textiles, maintains comfort, breathability and durability, and is simple in preparation, low in cost, and has a wide range of application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023093303_14112024_PF_FP_ABST
    Figure CN2023093303_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a novel aromatic textile and a manufacturing method therefor. The textile comprises cotton fabrics having different yarn counts and fabric weave structures, anionic resin films being attached to surfaces of the cotton fabrics, and surfaces of yarns being covered with film resin layers obtained by means of a cross-linking agent reaction. The present invention can effectively eliminate an odor while not affecting comfort, air permeability and durability.
Need to check novelty before this filing date? Find Prior Art

Description

A novel aromatic textile and its manufacturing method Technical Field

[0001] The present invention relates to the field of fiber technology, in particular to a novel aromatic textile and a manufacturing method thereof. Background Art

[0002] Textiles are widely used in daily life, but due to various factors, they are prone to odor, which affects people's experience. To address this problem, various methods and materials have been developed to eliminate odors, one of which is the use of scented textiles. However, traditional chemical fragrances are often irritating and allergenic, and the release time is difficult to control, which can easily cause adverse reactions.

[0003] In view of this, the present invention is proposed. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a new type of aromatic textile and a manufacturing method thereof, which can effectively eliminate odor without affecting comfort, breathability and durability.

[0005] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:

[0006] A novel aromatic textile comprises cotton fabrics with different yarn counts and fabric structures, wherein an anionic resin film is attached to the surface of the cotton fabric, and the surface of the yarn is covered with a film resin layer obtained by a bridging agent reaction.

[0007] In a preferred embodiment of any of the above schemes, the film resin layer is composed of an organic substance and a modified polyether substance.

[0008] In a preferred embodiment of any of the above schemes, the yarn count is 20-70S, the pore size distribution range is 2-16 μm, and the yarn diameter is between 6-18 μm.

[0009] In a preferred embodiment of any of the above schemes, the organic substance is one or a mixture of benzenesulfonic acid, xylenesulfonic acid, 4-hydroxybenzoic acid, 4-aminobenzoic acid, p-hydroxybenzoic acid, etc.

[0010] In a preferred embodiment of any of the above schemes, the cotton fabric is made of 100% cotton or a blend of cotton and fiber.

[0011] In a preferred embodiment of any of the above schemes, the thickness of the film resin layer is 0.5 to 2 μm.

[0012] In a preferred embodiment of any of the above schemes, the anionic resin membrane is an alkaline polyurethane resin or a modified naphthalenesulfonic acid resin.

[0013] In a preferred embodiment of any of the above solutions, the pore size distribution range of the textile is 4 to 10 μm.

[0014] In a second aspect, a method for preparing a novel aromatic textile is provided, the method comprising the following steps:

[0015] Prepare cotton fabric and yarn;

[0016] Immersing the surface of the cotton fabric in an anionic resin membrane solution, and allowing the cotton fabric to dry naturally to obtain an anionic resin membrane attached to the surface of the cotton fabric;

[0017] The yarn is immersed in a solution containing an organic substance and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer;

[0018] Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric;

[0019] The obtained fabric is dried at 160° C. for 30 minutes to solidify the film resin layer and adhere it to the cotton fabric, thereby obtaining a novel aromatic textile.

[0020] In a preferred embodiment of any of the above schemes, the thickness of the film resin layer is 0.5 to 2 μm.

[0021] In a preferred embodiment of any of the above schemes, the surface of the cotton fabric is immersed in an anionic resin membrane solution and then naturally dried to obtain an anionic resin membrane attached to the surface of the cotton fabric, comprising the following steps:

[0022] preparing the anionic resin membrane solution;

[0023] Soaking the cotton fabric in the anionic resin membrane solution to fully wet the surface of the cotton fabric;

[0024] Take out the impregnated cotton fabric and hang it up or lay it flat to allow it to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch. The anionic resin film will be attached to the surface of the cotton fabric.

[0025] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art.

[0026] By attaching an anionic resin film to the surface of cotton fabric and simultaneously covering the yarn surface with a film resin layer, the odor-eliminating effect can be achieved without affecting comfort, breathability, and durability. The preparation method of the present invention is simple, low-cost, and has broad application prospects.

[0027] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation of the present application. Some specific embodiments of the present application will be described in detail in an illustrative and non-restrictive manner with reference to the drawings. The same reference numerals in the drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the drawings:

[0029] FIG1 is a schematic diagram of a method for preparing a novel aromatic textile of the present invention.

[0030] It should be noted that these drawings and text descriptions are not intended to limit the scope of the present invention in any way, but rather to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. The elements in the drawings are schematic and not drawn to scale. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0032] The following embodiments of the present application take the novel aromatic textile and its manufacturing method as an example to explain the scheme of the present application in detail, but this embodiment does not limit the scope of protection of the present application.

[0033] Example 1

[0034] The present invention provides a novel aromatic textile, which comprises cotton fabrics of different yarn counts and fabric structures, an anionic resin membrane attached to the surface of the cotton fabric, and a membrane resin layer obtained by a bridging agent reaction covering the surface of the yarn, wherein the membrane resin layer is composed of an organic substance and a modified polyether substance. The yarn count is 20S, the pore size distribution range is 2μm, and the yarn diameter is between 6μm. The organic substance is benzenesulfonic acid, the cotton fabric is made of 100% cotton or a blend of cotton and fiber, the thickness of the membrane resin layer is 0.5μm, the anionic resin membrane is an alkaline polyurethane resin or a modified naphthalenesulfonic acid resin, and the pore size distribution range of the textile is 4μm.

[0035] In an embodiment of the present invention, cotton fabrics with different yarn counts and fabric structures: this method can be applied to different types of cotton fabrics and has a wide range of applications. Anionic resin membrane: by attaching anionic resin membrane to the surface of cotton fabric, the odor of textiles can be eliminated and the user experience can be improved. Film resin layer: by covering the yarn surface with a film resin layer, the structural strength and stability of the yarn can be enhanced to prevent yarn breakage and damage. Organic substance: the organic substance used in this method is benzenesulfonic acid, which can be used as one of the raw materials for the bridging agent reaction and participate in the formation of the film resin layer. Modified polyether substance: the modified polyether substance used in this method can replace commonly used organic solvents, making this method more environmentally friendly and reliable. The yarn count is 20S, the pore size distribution range is 2μm, and the yarn diameter is between 6μm: it can ensure the appropriate fineness of the yarn and the size of the pore size, which is conducive to the formation of the film resin layer and the overall effect of the textile. Using cotton fabrics made of 100% cotton or cotton and fiber blends can ensure the softness and breathability of the textile and improve the comfort of use. By controlling the thickness of the membrane resin layer, new aromatic textiles can achieve improved performance stability and longevity. The anionic resin membrane is composed of either alkaline polyurethane resin or modified naphthalenesulfonic acid resin. Choosing the appropriate anionic resin membrane based on the needs can ensure a more sustained and effective release of active substances from the textile. The pore size distribution of the textile is within a range of 4 μm. By controlling the pore size distribution of the textile, the release of active substances from the textile can be more uniform and stable.

[0036] A method for preparing a novel aromatic textile comprises the following steps:

[0037] Prepare cotton fabric and yarn;

[0038] preparing the anionic resin membrane solution; soaking cotton fabric in the anionic resin membrane solution to fully wet the surface of the cotton fabric; taking out the impregnated cotton fabric, hanging it up or laying it flat, and allowing the impregnated cotton fabric to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch, and the anionic resin membrane is attached to the surface of the cotton fabric;

[0039] The yarn is immersed in a solution containing benzenesulfonic acid and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer;

[0040] Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric;

[0041] The obtained fabric was dried at 160° C. for 30 minutes to solidify the film resin layer and adhere it to the cotton fabric, thereby obtaining a novel aromatic textile. The film resin layer had a thickness of 0.5 μm.

[0042] In the embodiments of the present invention, it should be noted that cotton fabric and yarn are prepared: the raw materials for preparing the new aromatic textile are determined. The anionic resin membrane solution is prepared: the anionic resin membrane solution is prepared for soaking the cotton fabric, thereby eliminating odor and improving the user experience. The cotton fabric is soaked in the anionic resin membrane solution so that the surface of the cotton fabric is fully wetted: the cotton fabric is soaked in the anionic resin membrane solution so that the anionic resin membrane is fully attached to the surface of the cotton fabric. The impregnated cotton fabric is taken out and hung or flattened, and the impregnated cotton fabric is allowed to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch. The surface of the cotton fabric will be attached with the formed anionic resin membrane: the anionic resin membrane on the surface of the cotton fabric is formed into a fixed layer by natural drying, thereby improving the adhesion and stability of the anionic resin membrane. The yarn is immersed in a solution containing benzenesulfonic acid and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer. The yarn is immersed in a solution containing benzenesulfonic acid and a modified polyether substance to prepare a film resin layer to improve the structural strength and stability of the yarn. The treated yarn is woven into a plain cotton textile, a twill cotton textile, or a satin cotton textile, so that the film resin layer covers the cotton fabric and fixes the film resin layer to the surface of the cotton fabric. The treated yarn is woven into different types of cotton textiles so that the film resin layer covers the cotton fabric and can be fixed to the surface of the cotton fabric, thereby realizing the processing and preparation of the textile. The resulting fabric is dried at 160°C for 30 minutes to solidify the film resin layer and adhere to the cotton fabric to obtain a new aromatic textile. The drying method allows the film resin layer and the cotton fabric to undergo a curing reaction, so that the film resin layer and the cotton fabric are firmly bonded together, thereby preparing a new aromatic textile. The film resin layer has a thickness of 0.5 μm. Controlling the film resin layer's thickness to 0.5 μm ensures the performance and longevity of the new aromatic textile. Each step and method employed in the novel aromatic textile production method has its own unique purpose and specificity. By mastering and implementing each step, the production of the novel aromatic textile can be made more stable and reliable.

[0043] Example 2

[0044] The present invention provides a novel aromatic textile, comprising cotton fabrics of different yarn counts and fabric structures, an anionic resin membrane attached to the surface of the cotton fabric, a membrane resin layer obtained by a bridging agent reaction covering the surface of the yarn, the membrane resin layer consisting of an organic substance and a modified polyether substance, the yarn count being 30S, the pore size distribution being 5 μm, the yarn diameter being between 8 μm, the organic substance being a mixture of benzenesulfonic acid and xylenesulfonic acid, the cotton fabric being 100% cotton or a blend of cotton and fiber, the membrane resin layer having a thickness of 0.5 to 2 μm, the anionic resin membrane being an alkaline polyurethane resin or a modified naphthalenesulfonic acid resin, and the pore size distribution being 5 μm.

[0045] A method for preparing a novel aromatic textile comprises the following steps:

[0046] Prepare cotton fabric and yarn;

[0047] preparing the anionic resin membrane solution; soaking cotton fabric in the anionic resin membrane solution to fully wet the surface of the cotton fabric; taking out the impregnated cotton fabric, hanging it up or laying it flat, and allowing the impregnated cotton fabric to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch, and the anionic resin membrane is attached to the surface of the cotton fabric;

[0048] The yarn is immersed in a solution containing benzenesulfonic acid, xylenesulfonic acid and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer;

[0049] Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric;

[0050] The obtained fabric was dried at 160° C. for 30 minutes to solidify the film resin layer and adhere it to the cotton fabric, thereby obtaining a novel aromatic textile. The film resin layer had a thickness of 0.8 μm.

[0051] Example 3

[0052] The present invention provides a novel aromatic textile, comprising cotton fabrics of different yarn counts and fabric structures, an anionic resin membrane attached to the surface of the cotton fabric, a membrane resin layer obtained by a bridging agent reaction covering the surface of the yarn, the membrane resin layer consisting of an organic substance and a modified polyether substance, the yarn count being 40S, the pore size distribution being 9 μm, the yarn diameter being between 8 μm, the organic substance being a mixture of benzenesulfonic acid, xylenesulfonic acid, and 4-hydroxybenzoic acid, the cotton fabric being 100% cotton or a blend of cotton and fiber, the membrane resin layer having a thickness of 0.9 μm, the anionic resin membrane being an alkaline polyurethane resin or a modified naphthalenesulfonic acid resin, and the pore size distribution being 6 μm.

[0053] A method for preparing a novel aromatic textile comprises the following steps:

[0054] Prepare cotton fabric and yarn;

[0055] preparing the anionic resin membrane solution; soaking cotton fabric in the anionic resin membrane solution to fully wet the surface of the cotton fabric; taking out the impregnated cotton fabric, hanging it up or laying it flat, and allowing the impregnated cotton fabric to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch, and the anionic resin membrane is attached to the surface of the cotton fabric;

[0056] The yarn is immersed in a solution containing benzenesulfonic acid, xylenesulfonic acid, 4-hydroxybenzoic acid and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer;

[0057] Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric;

[0058] The obtained fabric was dried at 160° C. for 30 minutes to solidify the film resin layer and adhere it to the cotton fabric, thereby obtaining a novel aromatic textile. The film resin layer had a thickness of 1 μm.

[0059] Example 4

[0060] The present invention provides a novel aromatic textile, comprising cotton fabrics of different yarn counts and fabric structures, an anionic resin membrane attached to the surface of the cotton fabric, a membrane resin layer obtained by a bridging agent reaction covering the surface of the yarn, the membrane resin layer consisting of an organic substance and a modified polyether substance, the yarn count being 70S, the pore size distribution being 16 μm, the yarn diameter being between 18 μm, the organic substance being a mixture of benzenesulfonic acid, xylenesulfonic acid, 4-hydroxybenzoic acid, and 4-aminobenzoic acid, the cotton fabric being 100% cotton or a blend of cotton and fiber, the membrane resin layer being 2 μm thick, the anionic resin membrane being an alkaline polyurethane resin or a modified naphthalenesulfonic acid resin, and the pore size distribution being 10 μm.

[0061] A method for preparing a novel aromatic textile comprises the following steps:

[0062] Prepare cotton fabric and yarn;

[0063] preparing the anionic resin membrane solution; soaking cotton fabric in the anionic resin membrane solution to fully wet the surface of the cotton fabric; taking out the impregnated cotton fabric, hanging it up or laying it flat, and allowing the impregnated cotton fabric to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch, and the anionic resin membrane is attached to the surface of the cotton fabric;

[0064] The yarn is immersed in a solution containing benzenesulfonic acid, xylenesulfonic acid, 4-hydroxybenzoic acid, 4-aminobenzoic acid and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer;

[0065] Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric;

[0066] The obtained fabric was dried at 160° C. for 30 minutes to solidify the film resin layer and adhere it to the cotton fabric, thereby obtaining a novel aromatic textile. The film resin layer had a thickness of 2 μm.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A novel aromatic textile, characterized in that: The textiles include cotton fabrics with different yarn counts and fabric structures, anionic resin films are attached to the surfaces of the cotton fabrics, and the surfaces of the yarns are covered with a film resin layer obtained by reacting a bridging agent.

2. The novel aromatic textile according to claim 1, characterized in that: The film resin layer is composed of organic matter and modified polyether matter.

3. The novel aromatic textile according to claim 2, characterized in that: The yarn count is 20-70S, the pore size distribution range is 2-16 μm, and the yarn diameter is between 6-18 μm.

4. The novel aromatic textile according to claim 3, characterized in that: The organic substance is one of benzenesulfonic acid, xylenesulfonic acid, 4-hydroxybenzoic acid, 4-aminobenzoic acid, p-hydroxybenzoic acid or a mixture of several thereof, and the cotton fabric is made of 100% cotton or a blend of cotton and fiber.

5. The novel aromatic textile according to claim 4, characterized in that: The thickness of the film resin layer is 0.5 to 2 μm.

6. The novel aromatic textile according to claim 5, characterized in that: The anionic resin membrane is alkaline polyurethane resin or modified naphthalenesulfonic acid resin.

7. The novel aromatic textile according to claim 6, characterized in that: The pore size distribution range of the textile is 4-10 μm.

8. A method for preparing a novel aromatic textile as claimed in any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Prepare cotton fabric and yarn; The surface of the cotton fabric is immersed in an anionic resin membrane solution, and the cotton fabric is dried naturally to obtain an anionic resin membrane attached to the surface of the cotton fabric; The yarn is immersed in a solution containing an organic substance and a modified polyether substance, and a bridging agent is used to react to obtain a film resin layer; Weaving the treated yarn into plain cotton textiles, twill cotton textiles or satin cotton textiles, so that the film resin layer covers the cotton fabric and the film resin layer is fixed on the surface of the cotton fabric; The obtained fabric is dried at 160°C for 30 minutes to solidify the film resin layer and adhere to the cotton fabric to obtain a novel aromatic textile.

9. The method for preparing the novel aromatic textile according to claim 8, characterized in that: The thickness of the film resin layer is 0.5 to 2 μm.

10. The method for preparing the novel aromatic textile according to claim 9, characterized in that: The surface of the cotton fabric is immersed in an anionic resin membrane solution, and then dried naturally to obtain an anionic resin membrane attached to the surface of the cotton fabric, comprising the following steps: preparing the anionic resin membrane solution; Soaking cotton fabric in anionic resin membrane solution to fully wet the surface of the cotton fabric; Take out the impregnated cotton fabric, and hang it up or lay it flat to allow it to dry naturally until there is no obvious liquid residue on the surface of the impregnated cotton fabric and it feels dry to the touch. The anionic resin film formed will be attached to the surface of the cotton fabric.

Citation Information

Patent Citations

  • Finishing technology for aromatic anti-bacteria cotton textile

    CN102733184A

  • Durable antistatic nylon textile

    CN107780221A

  • Textile easy for removing solid contaminants

    CN108071015A

  • One-pack type aqueous resin composition and fiber laminate

    CN108884314A

  • Preparation method of knitted fabric with gradient release of aromatic substances and lasting fragrance

    CN113802385A