Method for smelting magnesium by means of dolomite vacuum carbon thermal reduction
By performing carbon-heat reduction reaction of the mixed powder of dolomite and coking coal under vacuum, the problems of high energy consumption and environmental pollution in magnesium smelting technology are solved, and a low-cost and efficient magnesium smelting process is achieved, and magnesium is improved. purity.
Patent Information
- Application Number
- PCT/CN2023/101205
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2023-06-20
- Publication Date
- 2024-11-14
AI Technical Summary
Among the existing magnesium smelting technology, Pijiang method has problems such as high energy consumption, high resource consumption, large CO2 emissions, high price of reducing agent ferrosilicon and serious environmental pollution.
The mixed powder of dolomite and coking coal is used to carry out carbon-heat reduction reaction under vacuum conditions, and is directly heated to obtain crystalline magnesium, eliminating the addition of auxiliary materials, controlling the heating rate and insulation temperature to reduce energy consumption, and completing it in the same vacuum environment Thermal decomposition and carbon-thermal reduction of dolomite.
It has achieved the reduction of production costs and energy consumption and reduced environmental pollution, and the obtained crystalline magnesium has a high purity, reaching 83.62-91.20%.
Smart Images

Figure CN2023101205_14112024_PF_FP_ABST
Abstract
Description
A method for smelting magnesium by vacuum carbothermal reduction of dolomite
[0001] This application claims priority to a Chinese patent application filed with the Patent Office of China on May 10, 2023, with application number CN202310524049.6 and invention name “A method for smelting magnesium by vacuum carbon thermal reduction of dolomite”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The invention belongs to the technical field of vacuum smelting of metallic magnesium, and in particular relates to a method for smelting magnesium through vacuum carbothermic reduction of dolomite. Background Art
[0003] Magnesium-based materials are the lightest engineering metals used in industrial applications, with a density only 64% that of aluminum and 25% that of zinc. They are expected to replace steel and aluminum as a new generation of structural materials, and are hailed as "21st-century green engineering materials" and "revolutionary medical metal materials." Global demand for primary magnesium has grown at an average annual rate of over 10% over the past five years, with production expected to reach 1 million tons in 2022. As the upstream component of the magnesium industry chain, the development of magnesium smelting directly impacts the overall industry, and therefore holds promising prospects.
[0004] Currently, over 80% of primary magnesium in my country is produced by the silicothermic process (Pidgeon process). The Pidgeon process has a history of over 80 years and is relatively mature. However, equipment upgrades have been unable to address the high energy consumption, resource consumption, high raw material requirements, and high CO2 emissions associated with the Pidgeon process. In particular, the reducing agent, ferrosilicon, is not only expensive but also severely polluting during its production, seriously violating the "green and low-carbon" development strategy.
[0005] Chinese patent CN1769505A discloses a method for extracting metallic magnesium by vacuum coal thermal reduction of magnesium oxide ore. The method comprises using magnesium oxide or its mineral dolomite as raw material, and reducing agent coal crushed to 1-3 mm, and then mixing the raw materials according to a ratio of C:MgO = 2-3.5:1. Then, 5-10 wt% of the mixture of one or both of CaF2 and NaF as additives are added to the mixture. After further mixing, the mixture is pressed into pellets with a diameter of 10-40 mm. The pellets are then placed in a vacuum furnace with a controlled vacuum degree of 5-45 Pa, first coked at 500-800°C for 30-60 minutes, and then heated to 1300-1600°C for a reduction reaction for 45-60 minutes. However, the above method not only requires the use of CaF2 or NaF as an additive, but also requires coking at a relatively high temperature to coat the reducing coal with the surface of the magnesium oxide or its mineral dolomite raw material, forming a bonded structure. The temperature is then raised to carry out the reduction reaction, which allows the reducing coal and magnesium oxide or its mineral dolomite raw material to fully react. However, the above method still suffers from the problems of high heat consumption and high cost.
[0006] Summary of the Invention
[0007] The purpose of the present invention is to provide a method for vacuum carbothermic reduction of dolomite to smelt magnesium. The method provided by the present invention does not require the addition of auxiliary materials, thereby reducing production costs; and has low heat consumption, thereby reducing energy consumption; at the same time, it achieves full utilization of CO2 and reduces environmental pollution.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] The present invention provides a method for magnesium smelting by vacuum carbothermal reduction of dolomite, comprising the following steps:
[0010] The mixed powder of dolomite and coking coal is pressed to obtain a formed body;
[0011] Under vacuum conditions, the molded body is heated to directly undergo a carbothermic reduction reaction, and the resulting reducing vapor is condensed to obtain crystalline magnesium; the heating rate of the heating is ≤12K / min; the holding temperature of the carbothermic reduction reaction is ≥1400K, and the holding time is ≤2h.
[0012] Preferably, the heating rate is 8-12 K / min.
[0013] Preferably, the holding temperature of the carbothermal reduction reaction is 1400-1600 K, and the holding time is 1-2 h.
[0014] Preferably, the pressing pressure is 6-16 MPa.
[0015] Preferably, in the mixed powder of dolomite and coking coal, the dolomite is calculated based on the content of CaMg(CO3)2, the coking coal is calculated based on the content of element C, and the molar ratio of the coking coal to the dolomite is 2:1.
[0016] Preferably, the particle size of the mixed powder of dolomite and coking coal is ≤8.5 μm.
[0017] Preferably, the vacuum degree of the carbothermal reduction reaction is 50-150 Pa.
[0018] Preferably, the condensation temperature is 623-760K.
[0019] Preferably, the chemical composition of the dolomite includes: MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu<0.005wt%, SiO21.14wt%, Al2O31.46wt%.
[0020] Preferably, the coking coal has a moisture content of less than 0.2%, an ash content of 26.21%, a volatile content of 10.17%, and a fixed carbon content of ≥63.42 wt%.
[0021] The present invention provides a method for vacuum carbothermic reduction of magnesium from dolomite, comprising the following steps: pressing a mixed powder of dolomite and coking coal to obtain a shaped body; heating the shaped body under vacuum conditions to directly undergo a carbothermic reduction reaction, condensing the resulting reducing vapor to obtain crystalline magnesium; the heating temperature is increased at a rate of ≤12K / min; the carbothermic reduction reaction is held at a temperature of ≥1400K for a holding time of ≤2h. The method does not require the addition of auxiliary materials to the raw materials, effectively reducing production costs. Furthermore, by controlling the heating temperature at a rate of ≤12K / min, the shaped body obtained from dolomite and coking coal can directly undergo a carbothermic reduction reaction, eliminating the need for heat preservation and coking, thereby effectively reducing energy consumption. Finally, the method performs both thermal decomposition and carbothermic reduction of the dolomite in the same vacuum environment, shortening the dolomite magnesium refining process, reducing energy consumption, and fully utilizing CO2, thereby minimizing environmental pollution. Results from the examples show that the purity of the crystalline magnesium obtained by the method of the present invention ranges from 83.62% to 91.20%. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is a flow chart of an embodiment of the present invention;
[0023] FIG2 is an XRD spectrum of crystalline magnesium prepared in Example 2 and Example 3 of the present invention;
[0024] FIG3 is an SEM and EDS image of the crystalline magnesium prepared in Example 1 of the present invention;
[0025] FIG4 is an SEM and EDS image of the crystalline magnesium prepared in Example 2 of the present invention;
[0026] FIG5 is an SEM and EDS image of the crystalline magnesium prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0027] The present invention provides a method for magnesium smelting by vacuum carbothermal reduction of dolomite, comprising the following steps:
[0028] The mixed powder of dolomite and coking coal is pressed to obtain a formed body;
[0029] Under vacuum conditions, the molded body is heated to directly undergo a carbothermic reduction reaction, and the resulting reducing vapor is condensed to obtain crystalline magnesium; the heating rate of the heating is ≤12K / min; the holding temperature of the carbothermic reduction reaction is ≥1400K, and the holding time is ≤2h.
[0030] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0031] The present invention compresses mixed powder of dolomite and coking coal to obtain a formed body.
[0032] In the present invention, the mixed powder of dolomite and coking coal is preferably 2:1 in molar ratio, with the dolomite being calculated based on the CaMg(CO3)2 content and the coking coal being calculated based on the C element content. The coking coal serves as a reducing agent, and the dolomite is reduced to crystalline magnesium in a vacuum carbothermal reaction.
[0033] In the present invention, the particle size of the mixed powder of dolomite and coking coal is preferably ≤8.5 μm. In a specific embodiment of the present invention, the mesh size of the mixed powder of dolomite and coking coal is preferably 250 mesh or 300 mesh. In the present invention, the particle size of the mixed powder of dolomite and coking coal is preferably ≤8.5 μm. This can increase the contact area between the dolomite and coking coal in the mixed powder, thereby increasing the contact area between the solid-solid reactants during the carbothermal reduction reaction and improving the efficiency of the carbothermal reduction.
[0034] In the present invention, the method for preparing the mixed powder of dolomite and coking coal preferably comprises the following steps:
[0035] Dolomite and coking coal are mixed and then crushed and ground in sequence to obtain mixed powder of dolomite and coking coal.
[0036] In a specific embodiment of the present invention, the chemical composition of the dolomite includes: MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu<0.005wt%, SiO21.14wt%, Al2O31.46wt%.
[0037] In a specific embodiment of the present invention, the moisture content of the coking coal is less than 0.2%, the ash content is 26.21%, the volatile matter is 10.17%, and the fixed carbon is ≥63.42wt%.
[0038] The present invention has no special requirements on the specific implementation process of the crushing and the grinding.
[0039] In the present invention, the pressing pressure is preferably 6 to 16 MPa, more preferably 8 to 15 MPa.
[0040] In the present invention, the molded body is preferably a block.
[0041] The present invention preferably sets the pressing pressure to 6-16 MPa, which can ensure close contact between dolomite particles and coking coal particles in the obtained molded body, enhance the mass transfer efficiency of the solid-solid phase reaction during vacuum carbothermal reduction, and thus make the reduction reaction more complete.
[0042] After obtaining the molded body, the present invention heats the molded body under vacuum conditions to directly perform a carbothermal reduction reaction, and the obtained reducing vapor is condensed to obtain crystalline magnesium; the heating rate of the heating is ≤12K / min; the holding temperature of the carbothermal reduction reaction is ≥1400K, and the holding time is ≤2h.
[0043] In the present invention, the carbothermic reduction reaction is preferably carried out in a vacuum furnace. The vacuum furnace is divided into a reaction chamber and a condensation chamber. The condensation chamber is located above the reaction chamber, and the condensation chamber and the reaction chamber are connected by a connecting pipe. The molded body undergoes a carbothermic vacuum reduction reaction in the reaction chamber of the vacuum furnace, and the resulting reducing vapor enters the condensation chamber through the connecting pipe and condenses to produce crystalline magnesium.
[0044] Before the heating, the present invention preferably flushes the vacuum furnace with nitrogen, then places the formed body into the vacuum furnace, turns on the circulating water cooling system, control system and vacuum system, and uses the vacuum system to evacuate the vacuum furnace to a vacuum condition.
[0045] In the present invention, the vacuum degree of the carbothermal reduction reaction is preferably 50-150 Pa, more preferably 60-140 Pa.
[0046] In the present invention, the heating rate is preferably 8 to 12 K / min, more preferably 9 to 11 K / min.
[0047] In the present invention, the holding temperature of the carbothermal reduction reaction is preferably 1400-1600 K, and the holding time is preferably 1-2 h.
[0048] The method provided by the present invention directly and continuously heats the material to the carbon thermal reduction temperature to carry out the carbon thermal reduction reaction. By adjusting the heating rate to preferably 8 to 12 K / min, the dolomite and coke in the formed body can be bonded together during the heating process, thereby eliminating the need for heat preservation and coking before the carbon thermal reduction reaction. This not only simplifies the smelting steps but also reduces energy consumption.
[0049] In the present invention, the condensation temperature is preferably 623-760K, more preferably 630-750K.
[0050] In the present invention, after the carbon thermal reduction reaction is completed, the present invention preferably closes the vacuum system after the temperature in the vacuum furnace drops to room temperature, opens the vent valve to restore the pressure in the furnace to normal pressure, and closes the circulating water cooling system and the control system.
[0051] In the present invention, the crystalline magnesium is in the shape of needle strips.
[0052] The present invention preferably uses chemical analysis methods such as X-ray diffractometer (XRD), scanning electron microscope (SEM), and energy dispersive spectrometer (EDS) to analyze the obtained crystalline magnesium. XRD analyzes the physical phases of the residue (slag from the carbothermal reduction reaction) and the condensate (crystalline magnesium), SEM characterizes the structural characteristics of the residue and condensate, and EDS characterizes the chemical composition of the condensate.
[0053] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0054] Example 1
[0055] According to the flow chart shown in Figure 1: dolomite (MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu <0.005wt%, SiO21.14wt%, Al2O31.46wt%) and coking coal are crushed and ground to 300 mesh. The dolomite is calculated based on the CaMg(CO3)2 content, and the coking coal is calculated based on the C element content. The dolomite and coking coal are mixed according to the C:CaMg(CO3)2 molar ratio of 2:1. After uniform mixing, they are die-cast into block materials under a pressure of 8MPa. The vacuum reduction furnace was flushed with argon, the block material was placed in the vacuum reduction furnace, the circulating water cooling system, the control system, and the vacuum system were turned on, the heating rate was set to 10K / min, and the vacuum degree was controlled to 30-50Pa. When the temperature rose to 1500±100K, the reduction reaction was carried out for 1h to obtain crystalline magnesium with a purity of 83.62%. The weight loss rate of the raw material was 81.2% (wherein the weight loss rate is the percentage of the reducing slag obtained after the reduction reaction and the raw material).
[0056] Example 2
[0057] According to the flow chart shown in Figure 1: dolomite (MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu <0.005wt%, SiO2 1.14wt%, Al2O3 1.46wt%) and coking coal are crushed and ground to 250 mesh. The dolomite is calculated based on the content of CaMg(CO3)2, and the coking coal is calculated based on the content of C element. The dolomite and coking coal are mixed according to the molar ratio of C:CaMg(CO3)2 of 2. After being mixed evenly, they are die-cast into blocks under a pressure of 8MPa. The vacuum reduction furnace is flushed with argon gas, and the blocks are placed in the vacuum reduction furnace. The circulating water cooling system, control system, and vacuum system are turned on. The vacuum degree is controlled at 30-50Pa and the heating rate is 10K / min. When the temperature rises to 1500±100K, the reduction reaction is carried out for 1 hour to obtain crystalline magnesium.
[0058] The crystalline magnesium prepared in this example exhibited clear XRD peaks, indicating good crystallinity, a purity of 89.82%, and a weight loss of 84.6%. Compared to the 300-mesh particle size used in Example 1, it can be concluded that the smaller the particle size, the more pronounced the reduction effect. This is because the smaller the particle size, the greater the contact area between the carbon and the dolomite, enhancing the solid-solid reaction.
[0059] Example 3
[0060] According to the flow chart shown in Figure 1: dolomite (MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu <0.005wt%, SiO2 1.14wt%, Al2O3 1.46wt%) and coking coal are crushed and ground to 250 mesh. The dolomite is calculated based on the content of CaMg(CO3)2, and the coking coal is calculated based on the content of C element. The ingredients are prepared according to the molar ratio of C:CaMg(CO3)2 of 2. After being mixed evenly, they are die-cast into block materials under a pressure of 8MPa. The vacuum reduction furnace is flushed with argon gas, and the block materials are placed in the vacuum reduction furnace. The circulating water cooling system, control system, and vacuum system are turned on. The vacuum degree is controlled at 30-50Pa and the heating rate is 10K / min. When the temperature rises to 1500±100K, a reduction reaction is carried out for 2h to obtain crystalline magnesium. The purity of the crystalline magnesium is 91.20%, and the weight loss rate is 87.8%.
[0061] Compared with the 1 hour holding time in Implementation 2, it can be concluded that the longer the holding time, the more obvious the reduction effect. This is because the material has more sufficient reaction time, and the magnesium vapor crystallization time is extended, the nucleation growth is more sufficient, and the purity is higher.
[0062] The condensed products from Examples 1, 2, and 3 were subjected to XRD, SEM, and EDS analysis. The results are shown in Figures 2 to 5. Figure 2 shows the XRD spectra of the crystalline magnesium prepared in Examples 2 and 3 of the present invention; Figure 3 shows the SEM and EDS images of the crystalline magnesium prepared in Example 1 of the present invention; Figure 4 shows the SEM and EDS images of the crystalline magnesium prepared in Example 2 of the present invention; and Figure 5 shows the SEM and EDS images of the crystalline magnesium prepared in Example 3 of the present invention. Figures 2 to 5 indicate that the condensate from the carbothermal reduction of dolomite is crystalline magnesium. The XRD peaks of the crystalline magnesium are clear, indicating good crystallinity, and the purity is above 83.62%.
[0063] Although the above embodiment provides a detailed description of the present invention, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for magnesium smelting by vacuum carbothermal reduction of dolomite, characterized in that: The following steps are involved: The mixed powder of dolomite and coking coal is pressed to obtain a shaped body; Under vacuum conditions, the molded body is heated to directly perform a carbon thermal reduction reaction, and the obtained reducing vapor is condensed to obtain crystalline magnesium; the heating rate of the heating is ≤12K / min; the insulation temperature of the carbon thermal reduction reaction is ≥1400K, and the insulation time is ≤2h.
2. The method according to claim 1, characterized in that: The heating rate of the heating is 8-12 K / min.
3. The method according to claim 1 or 2, characterized in that: The insulation temperature of the carbon thermal reduction reaction is 1400-1600K, and the insulation time is 1-2h.
4. The method according to claim 1, characterized in that: The pressing pressure is 6-16 MPa.
5. The method according to claim 1, characterized in that In the mixed powder of dolomite and coking coal, the dolomite is measured by the content of CaMg(CO3)2, the coking coal is measured by the content of C element, and the molar ratio of the coking coal to the dolomite is 2:
1.
6. The method according to claim 1 or 5, characterized in that: The method for preparing the mixed powder of dolomite and coking coal comprises the following steps: The dolomite and coking coal are mixed and then crushed and ground in sequence to obtain a mixed powder of the dolomite and coking coal.
7. The method according to claim 1 or 5, characterized in that: The particle size of the mixed powder of dolomite and coking coal is ≤8.5 μm.
8. The method according to claim 1, characterized in that The vacuum degree of the carbon thermal reduction reaction is 50-150Pa.
9. The method according to claim 1, characterized in that: The condensation temperature is 623-760K.
10. The method according to claim 1, characterized in that The chemical composition of the dolomite includes: MgO 19.35wt%, CaO 27.48wt%, Fe 3.69wt%, Cu<0.005wt%, SiO21.14wt%, Al2O31.46wt%.
11. The method according to claim 1, characterized in that: The coking coal has a moisture content of <0.2%, an ash content of 26.21%, a volatile content of 10.17%, and a fixed carbon content of ≥63.42wt%.
12. The method according to claim 1 or 8, characterized in that: The carbon thermal reduction reaction is carried out in a vacuum furnace, which is divided into a reaction chamber and a condensation chamber. The condensation chamber is located above the reaction chamber, and the condensation chamber and the reaction chamber are connected through a connecting pipe. The molded body undergoes a carbon thermal vacuum reduction reaction in the reaction chamber of the vacuum furnace, and the obtained reducing vapor enters the condensation chamber through the connecting pipe and is condensed to obtain crystalline magnesium.
Citation Information
Patent Citations
Method for preparing magnesium metal by giobertite vacuum carbon thermal reduction
CN101397609A
Method adopting reduction of basic magnesium carbonate to prepare magnesium metal
CN103184351A
Technique method for manufacturing magnesium metal by dolomite
CN103184352A
Method for smelting magnesium through vacuum carbon thermal reduction
CN115747523A
Vacuum, heat and coal reduction method for extracting metal magnesium from magnesium oxide ore
CN1769505A