Hydrorefining method of bimetallic carbonate dolomite
By preparing dolomite with a specific crystal structure and using hydrogenation reaction method, the problems of high temperature and high carbon dioxide emissions during dolomite refining are solved, energy consumption and treatment costs are reduced, and by-product generation possibilities are provided. , improves economic value.
Patent Information
- Application Number
- CN202411165932.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-23
AI Technical Summary
In the prior art, high temperature conditions are required during the refining of dolomite, resulting in high production costs and serious carbon dioxide emissions, and the treatment cost of carbon dioxide after refining is high.
By preparing dolomite with a specific crystal structure, the hydrogenation reaction method is used to reduce the refining temperature of dolomite without using a catalyst, and the carbon in the dolomite is converted into carbon monoxide and methane to reduce the formation of carbon dioxide.
It reduces the dolomite refining temperature and energy consumption, reduces the generation of carbon dioxide, reduces the treatment costs, increases economic value, and provides the possibility of generation of by-products to improve economic value.
Smart Images

Figure CN118954980A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of carbonate decomposition, and in particular to a method for hydrogenating and refining bimetallic carbonate dolomite. Background Art
[0002] my country is the world's largest magnesium producer and exporter. At present, the annual output of raw magnesium is about 900,000 tons, accounting for more than 85% of the world's raw magnesium output. Dolomite is a mineral containing calcium and magnesium elements. Its chemical formula is CaMg(CO 3 ) 2 Dolomite is abundant in China, with proven reserves reaching 20 billion tons. Dolomite is easy to mine and is relatively cheap, so it is an important raw material for producing calcium and magnesium products.
[0003] At present, thermal reduction is one of the main magnesium smelting processes. The thermal reduction method represented by the Pidgeon process is the main method for producing raw magnesium in my country, and its raw magnesium output accounts for more than 90% of the total raw magnesium output in my country. The Pidgeon process uses dolomite as raw material, produces calcined white through high-temperature refining, and then uses ferrosilicon as a reducing agent to reduce the magnesium in the calcined white to magnesium vapor under vacuum and high temperature conditions, and then condenses to obtain metallic magnesium. However, the Pidgeon process involves high temperature conditions during pyrolysis, which not only increases production costs, but also emits a large amount of carbon dioxide, causing serious impacts on the ecological environment.
[0004] CN115583665B discloses a method for co-producing calcium carbonate and magnesium building materials from dolomite ore. The method uses dolomite ore to obtain calcium oxide and magnesium oxide. After the calcium oxide and magnesium oxide undergo selective sedimentation reaction, the filtered filtrate is carbonated to obtain a calcium carbonate product, and the filter residue is used as a raw material for preparing magnesium building materials. However, the dolomite ore needs to be refined at 950°C, and the generated carbon dioxide needs to be recovered and processed, which increases the preparation cost.
[0005] It can be seen that how to lower the refining temperature of dolomite and reduce the emission of carbon dioxide after refining is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for hydrogenating and refining bimetallic carbonate dolomite. The method prepares dolomite with a specific crystal structure, which can reduce the refining temperature of dolomite without using a catalyst, and at the same time convert the carbon in the dolomite into carbon monoxide and methane, thereby reducing the generation of carbon dioxide.
[0007] The present invention provides a method for hydrogenating and refining bimetallic carbonate dolomite, wherein reducing gas is introduced into the dolomite for hydrogenation reaction, and the method does not require the use of a catalyst; the crystal structure of the dolomite has two characteristics in the X-ray diffraction spectrum: (1) d104=2.88Å; (2) superstructure (h0l) and (0kl) diffraction lines (l is an odd number) appear on the spectrum, and at a 2θ angle of 22.05 o , 30.9 o , 35.3 o , 41.1 o At 44.9°, the dolomite has characteristic diffraction peaks of (101), (104), (015), (113), and (202).
[0008] Furthermore, the preparation method of the dolomite is: dissolving magnesium chloride and calcium chloride in a molar ratio of (0.5-2):1 in deionized water to prepare a mixed solution with a concentration of 1.5-3 mol / L, first taking 1-3 g of calcium carbonate and adding it to a polytetrafluoroethylene liner, then adding 150-450 ml of the mixed solution, and placing it in a forced air drying oven for crystallization, centrifuging after crystallization and washing with deionized water, and finally drying.
[0009] Furthermore, the temperature of the crystallization treatment is 200-260 o C.
[0010] Furthermore, the crystallization treatment time is 24-60h.
[0011] Furthermore, the rotation speed of the centrifugal treatment is 8000-15000r / min.
[0012] Furthermore, the drying temperature is 60-80 o C. Furthermore, the reducing gas includes hydrogen, and based on the total volume of the reducing gas, the volume of the hydrogen is 20-100% of the total volume.
[0013] Furthermore, the reducing gas also includes nitrogen or argon.
[0014] Furthermore, the flow rate of the reducing gas is 30-100 ml / min.
[0015] Furthermore, the pressure of the reducing gas is 1-5 bar.
[0016] Furthermore, the temperature of the dolomite hydrogenation refining is 400-600 o C.
[0017] Furthermore, after the dolomite is hydrogenated and refined, the refined products include calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide.
[0018] Furthermore, the decomposition rate of the dolomite is the ratio of the molar number of carbon monoxide to the molar number of carbon in the dolomite, and the decomposition rate of the dolomite is 87-100%.
[0019] Furthermore, the selectivity of carbon monoxide is the ratio of the molar number of carbon monoxide to the total molar number of gas in the refined product, and the selectivity of carbon monoxide is 80-96%.
[0020] Furthermore, an excess amount of the reducing gas is introduced during the dolomite hydrogenation refining process, and the molar ratio of unreacted hydrogen to the carbon monoxide is (4-8):1.
[0021] Beneficial Effects of the Invention 1. The prior art generally uses high-temperature conditions to refine dolomite, and a large amount of carbon dioxide will be generated after refining; however, the present invention prepares dolomite with a specific crystal structure, which can reduce the refining temperature of dolomite without using a catalyst, and at the same time converts the carbon in the dolomite into carbon monoxide and methane, thereby reducing the generation of carbon dioxide. Therefore, the present invention not only reduces energy consumption, but also reduces the treatment cost of carbon dioxide, and the overall solution has a high economic value.
[0022] 2. In the process of dolomite refining, the present invention introduces excess reducing gas, and the unreacted hydrogen and the generated carbon monoxide can produce different by-products under different conditions, such as (1) Fischer-Tropsch synthesis reaction: using cobalt or iron as a catalyst, hydrogen and carbon monoxide react to produce hydrocarbon products, including straight-chain alkanes and low-carbon olefins; (2) synthetic alcohol reaction: using copper as a catalyst, hydrogen and carbon monoxide react to produce alcohol products, mainly low-carbon alcohols; (3) methanation reaction: using nickel as a catalyst, hydrogen and carbon monoxide react to produce methane and water. Therefore, the generation of by-products can further improve the economic value of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The X-ray derivative images of dolomite of different proportions prepared in Examples 1-3; Figure 2 X-ray derivative images of the homemade dolomite in Example 1, the natural dolomite in Comparative Example 1, and the calcium carbonate in Comparative Example 2; Figure 3a-3c The scanning electron microscope images are of the homemade dolomite in Example 1, the natural dolomite in Comparative Example 1, and the calcium carbonate in Comparative Example 2. DETAILED DESCRIPTION
[0024] Example 1 A method for hydrogenating and refining bimetallic carbonate dolomite comprises the following steps: Step 1: Preparation of dolomite: Dissolve 0.5 mol of magnesium chloride and 1 mol of calcium chloride in deionized water to prepare a mixed solution with a concentration of 1.5 mol / L. First, add 1g of calcium carbonate to the polytetrafluoroethylene liner, then add 150ml of the mixed solution, and place it in a blast drying oven for crystallization at a temperature of 200 o C, the time is 24h, after crystallization, centrifuge and wash with deionized water, the centrifugal speed is 8000r / min, and finally dry, the drying temperature is 60 o C, dolomite is obtained, and the crystal structure of dolomite is trigonal.
[0025] Step 2: Refining dolomite: 1000 mg of dolomite was placed in a quartz tube with a diameter of 40 mm, and the reducing gas was introduced for refining. The volume of hydrogen was 20% of the total volume, and the rest was argon. The flow rate of the reducing gas was 30 ml / min, the pressure was 1 bar, and the refining temperature was 400 o C, the time is 30 minutes, the refining products are calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide. The end of the quartz tube is connected to a silica gel drying device, and the dried gas enters a mass spectrometer for detection. The decomposition rate of dolomite is 87%, the selectivity of carbon monoxide is 80%, and the molar ratio of unreacted hydrogen to generated carbon monoxide is 8:1.
[0026] Example 2 A method for hydrogenating and refining bimetallic carbonate dolomite comprises the following steps: Step 1: Preparation of dolomite: Dissolve 1 mol of magnesium chloride and 1 mol of calcium chloride in deionized water to prepare a mixed solution with a concentration of 2 mol / L. First, add 2 g of calcium carbonate to the polytetrafluoroethylene liner, then add 300 ml of the mixed solution, and place it in a blast drying oven for crystallization at a temperature of 230 o C, the time is 40h, after crystallization, centrifuge and wash with deionized water, the centrifugal speed is 12000r / min, and finally dry, the drying temperature is 70 o C, dolomite is obtained, and the crystal structure of dolomite is trigonal.
[0027] Step 2: Refining dolomite: 1000 mg of dolomite was placed in a quartz tube with a diameter of 40 mm, and the reducing gas was introduced for refining. The volume of hydrogen was 50% of the total volume, and the rest was argon. The flow rate of the reducing gas was 50 ml / min, the pressure was 3 bar, and the refining temperature was 500 oC, the time is 30 minutes, the refining products are calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide. The end of the quartz tube is connected to a silica gel drying device. The dried gas enters a mass spectrometer for detection. The decomposition rate of dolomite is 94%, the selectivity of carbon monoxide is 89%, and the molar ratio of unreacted hydrogen to generated carbon monoxide is 6:1.
[0028] Example 3 A method for hydrogenating and refining bimetallic carbonate dolomite comprises the following steps: Step 1: Preparation of dolomite: Dissolve 2 mol of magnesium chloride and 1 mol of calcium chloride in deionized water to prepare a mixed solution with a concentration of 3 mol / L. First, add 3 g of calcium carbonate to the polytetrafluoroethylene liner, then add 450 ml of the mixed solution, and place it in a blast drying oven for crystallization at a temperature of 260 o C, time for 60h, after crystallization, centrifugation and washing with deionized water, the centrifugal speed is 15000r / min, and finally drying, the drying temperature is 80 o C, dolomite is obtained, and the crystal structure of dolomite is trigonal.
[0029] Step 2: Refining dolomite: 1000 mg of dolomite was placed in a quartz tube with a diameter of 40 mm, and reduced gas was introduced for refining. The volume of hydrogen was 100% of the total volume, and the rest was argon. The flow rate of the reducing gas was 100 ml / min, the pressure was 5 bar, and the refining temperature was 600 o C, the time is 30 minutes, the refining products are calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide. The end of the quartz tube is connected to a silica gel drying device, and the dried gas enters a mass spectrometer for detection. The decomposition rate of dolomite is 100%, the selectivity of carbon monoxide is 96%, and the molar ratio of unreacted hydrogen to generated carbon monoxide is 4:1.
[0030] Comparative Example 1 Step 1: Refining natural dolomite: 1000 mg of natural dolomite produced in Huahuan, Hunan was placed in a quartz tube with a diameter of 40 mm, and reduced gas was introduced for refining. The volume of hydrogen was 20% of the total volume, and the rest was argon. The flow rate of the reducing gas was 30 ml / min, the pressure was 1 bar, and the refining temperature was 600 o C, the time is 30 minutes, the refining products are calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide. The end of the quartz tube is connected to a silica gel drying device, and the dried gas enters a mass spectrometer for detection. The decomposition rate of dolomite is 64%, the selectivity of carbon monoxide is 73%, and the molar ratio of unreacted hydrogen to generated carbon monoxide is 10:1.
[0031] Comparative Example 2 Step 1: Refining calcium carbonate: Take 100 mg of calcium carbonate powder and place it in a glass tube reactor body, and introduce reducing gas from the bottom for refining. Based on the total volume of reducing gas, the volume of hydrogen is 20% of the total volume, and the rest is argon. The flow rate of the reducing gas is 50 ml / min, the pressure is 1 bar, the calcium carbonate powder is in a suspended state, the refining temperature is 700°C, the time is 30 min, and the refining products are calcium oxide, carbon monoxide, methane and carbon dioxide. The end of the quartz tube is connected to a silica gel drying device, and the dried gas enters a mass spectrometer for detection. The decomposition rate of the calcium carbonate powder is 55%, the selectivity of carbon monoxide is 62%, and the molar ratio of unreacted hydrogen to generated carbon monoxide is 10:1.
[0032] In summary, it is generally expected in the prior art that the decomposition rate of natural dolomite is about 60% and the selectivity of carbon monoxide is about 70% under the conditions of a refining temperature of 600°C and a refining time of 30 min; the decomposition rate of calcium carbonate is about 50% and the selectivity of carbon monoxide is about 60% under the conditions of a refining temperature of 700°C and a refining time of 30 min. That is, under the conditions of a temperature higher than or equal to that of the embodiment, the decomposition rate of natural dolomite and calcium carbonate and the selectivity of carbon monoxide in the comparative examples 1-2 of the present invention are lower than those in the embodiments 1-3, while the molar ratio of unreacted hydrogen to generated carbon monoxide in the comparative examples 1-2 is higher than that in the embodiments 1-3. This is because the present invention prepares dolomite with a specific crystal structure [having two characteristics in the X-ray diffraction spectrum: (1) d104=2.88Å; (2) the appearance of superstructure (h0l) and (0kl) diffraction lines (l is an odd number) in the spectrum, and at a 2θ angle of 22.05 o , 30.9 o , 35.3 o , 41.1 o At 44.9°, the dolomite has characteristic diffraction peaks of (101), (104), (015), (113), and (202), which produces an unexpected technical effect, namely, without using a catalyst, the refining temperature of dolomite can be reduced, while the decomposition rate of dolomite and the selectivity of carbon monoxide can be improved, and the overall solution has a high economic value.
[0033] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A method for hydrogenating and refining bimetallic carbonate dolomite, characterized in that: The method comprises introducing reducing gas into the dolomite for hydrogenation reaction, and the method does not require the use of a catalyst; the crystal structure of the dolomite is: having two characteristics in the X-ray diffraction spectrum: (1) d104=2.88Å; (2) superstructure (h0l) and (0kl) diffraction lines (l is an odd number) appear in the spectrum, and at a 2θ angle of 22.05 o , 30.9 o , 35.3 o , 41.1 o At 44.9°, the dolomite has characteristic diffraction peaks of (101), (104), (015), (113), and (202).
2. The method according to claim 1, characterized in that The preparation method of dolomite is as follows: dissolving magnesium chloride and calcium chloride in a molar ratio of (0.5-2):1 in deionized water to prepare a mixed solution with a concentration of 1.5-3 mol / L, first taking 1-3 g of calcium carbonate and adding it into a polytetrafluoroethylene liner, then adding 150-450 ml of the mixed solution, and placing it in a forced air drying oven for crystallization, centrifuging after crystallization, washing with deionized water, and finally drying.
3. The method according to claim 2, characterized in that The temperature of the crystallization treatment is 200-260 o C.
4. The method according to claim 1, characterized in that: The reducing gas includes hydrogen. Based on the total volume of the reducing gas, the volume of the hydrogen is 20-100% of the total volume.
5. The method according to claim 4, characterized in that The flow rate of the reducing gas is 30-100 ml / min.
6. The method according to claim 1, characterized in that The temperature of the dolomite hydrogenation refining is 400-600 o C.
7. The method according to claim 6, characterized in that After the dolomite is hydrogenated and refined, the refined products include calcium oxide, magnesium oxide, carbon monoxide, methane and carbon dioxide.
8. The method according to claim 7, characterized in that The decomposition rate of the dolomite is the ratio of the mole number of carbon monoxide to the mole number of carbon in the dolomite, and the decomposition rate of the dolomite is 87-100%.
9. The method according to claim 7, characterized in that: The selectivity of carbon monoxide is the ratio of the molar number of carbon monoxide to the total molar number of gas in the refined product, and the selectivity of carbon monoxide is 80-96%.
10. The method according to claim 7, characterized in that During the dolomite hydrogenation refining process, an excess amount of the reducing gas is introduced, and the molar ratio of unreacted hydrogen to carbon monoxide is (4-8):1.
Citation Information
Patent Citations
A method for co-producing high-quality calcium carbonate and magnesium building material raw materials from dolomite ore
CN115583665B
Method for co-production of synthesis gas by carbonate hydrogenation refining for carbon dioxide emission reduction
CN113582208A
Method for producing magnesium oxide and co-producing methanol through hydrogenation refining of magnesium carbonate
CN117566775A
Method for producing dolomite, and synthesized dolomite
JP2016216269A
Catalyst and method of preparing light olefin directly from synthesis gas by one-step process
WO2017000427A1
Cited By
System and method for co-production of synthesis gas with controllable hydrogen-carbon ratio through carbonate reduction refining
CN119971931A
Low-carbon cement production method for co-producing high-value chemicals
CN120398448A