Frit, preparation method of frit, glaze, ceramic tile and preparation method of ceramic tile

By adjusting the composition of raw materials, a fuse with strong water retention is prepared for large-scale screen printing, which solves the problem of easy sticking and falling off of large-scale ceramic tiles, and achieves high-quality production of large-scale marble tiles, with good quality Anti-slip, wear and stain resistance.

CN118930049AActive Publication Date: 2024-11-12QINGYUAN GANI CERAMICS CO LTD +2

Patent Information

Application Number
CN202411121231.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

When preparing marble tiles in large-scale screen printing, the glaze in the prior art is prone to stick to the mesh and fall off easily, poor water retention, and uneven printing, resulting in problems such as glaze adhesion and pattern layer adhesion.

Method used

A new fuse is adopted, including raw materials such as sodium feldspar, strontium carbonate, alumina, corundum, borax, diopside, spherical soil, fluorite, quartz, dolomite and chrystalline. By adjusting the composition and proportion of raw materials, Prepare glaze with strong water retention and good mesh retention, and is used in large-scale screen printing technology.

Benefits of technology

Solve the problems of glaze sticking, falling off, poor water retention and uneven printing in large-scale screen printing, and achieve high-quality production of large-scale marble tiles, with high color saturation of glaze, good anti-slip effect, and wear-resistant High, strong anti-fouling, simple production process and high stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930049A_ABST
    Figure CN118930049A_ABST
Patent Text Reader

Abstract

The invention discloses a frit, which is prepared from the following raw materials in parts by weight: 8 to 10 parts of albite, 5 to 10 parts of strontium carbonate, 5 to 15 parts of aluminum oxide, 1 to 6 parts of corundum, 3 to 6 parts of borax, 10 to 15 parts of diopside, 5 to 10 parts of ball clay, 10 to 15 parts of fluorite, 15 to 20 parts of quartz, 4 to 10 parts of dolomite and 1 to 2 parts of nepheline. The frit has the advantages of strong water-retaining property and good net-refreshing property, and the glaze prepared by adopting the frit can solve the problems that the glaze is easy to stick to a net, easy to fall off, poor in water-retaining property and non-uniform in printing in the production of marble tiles prepared by large-specification silk-screen printing, and pattern layer adhesion is caused by large size of a screen printing plate and slow net lifting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building ceramics, and in particular to a frit and a preparation method thereof, a glaze, a ceramic tile and a preparation method thereof. Background Art

[0002] In the field of ceramics, the continuous advancement of screen printing technology has made its application more and more extensive. The ceramic decorative patterns printed by screen printing are more delicate, the colors are more vivid, the pictures and texts are more three-dimensional, and they are durable and do not fade.

[0003] The existing screen printing is mainly used for small-sized ceramic tile products, and the technology is relatively mature. However, large-sized screen printing has the following two problems due to the large screen size and slow screen closing after printing:

[0004] 1. During the printing process, the glaze and the inkjet color image are in contact for too long, which causes the inkjet image to stick when the screen is lifted, and the inkjet layer is easily adhered;

[0005] 2. After brushing, the glaze layers overlap each other, the glaze amount is large and the glaze surface is not easy to dry. Different silk screens overlap each other, and the next silk screen will adhere to the glaze of the previous silk screen, resulting in white spots.

[0006] Therefore, it is necessary to develop a glaze that can be applied to the production of large-sized (900*1800mm or more) marble tiles to solve the problems of marble tiles being easy to stick to the screen, easy to fall off, poor water retention of the glaze, and uneven printing when using the screen printing process in the existing technology for large-sized production. Summary of the invention

[0007] The main purpose of the present invention is to provide a frit suitable for large-scale screen printing of ceramic tiles. The glaze made from the frit can solve the problems in the prior art of easy sticking to the screen, easy falling off, poor water retention of the glaze, uneven printing, etc. when preparing marble tiles by large-scale screen printing.

[0008] To achieve the above purpose, the present invention provides a frit, which includes the following raw materials, in parts by weight: 8 to 10 parts of albite, 5 to 10 parts of strontium carbonate, 5 to 15 parts of aluminum oxide, 1 to 6 parts of corundum, 3 to 6 parts of borax, 10 to 15 parts of diopside, 5 to 10 parts of ball clay, 10 to 15 parts of fluorite, 15 to 20 parts of quartz, 4 to 10 parts of dolomite and 1 to 2 parts of nepheline.

[0009] The present invention develops a frit with strong water retention and good screen refreshing property by adjusting the raw material composition and ratio. The glaze prepared by the frit can solve the problems of easy sticking to the screen and easy falling off in different screen printing processes, poor water retention of the glaze, uneven printing, etc. It is particularly suitable for the production of marble tiles prepared by large-scale screen printing, avoiding the problems of glaze adhesion or pattern layer adhesion caused by large screen size and slow lifting of the screen in large-scale screen printing process.

[0010] Preferably, the chemical composition of the frit includes, by mass percentage, SiO2 43-50%, Al2O3 16-21%, Fe2O3 1-3%, CaO 5-10%, MgO 1-3%, K2O 1-5%, Na2O 5-10%, ZnO 5-15% and loss on ignition 1-3%, with the remainder being impurities.

[0011] In addition, the present invention also discloses a method for preparing the above frit, comprising the following steps:

[0012] (1) Mix the raw materials uniformly according to the proportion;

[0013] (2) sintering the raw materials at 1300-1400°C to melt into glass liquid, and quenching with water;

[0014] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 30 to 40 minutes, dried at 120 to 150° C., and sieved to obtain the frit.

[0015] The present invention also discloses a glaze, which comprises the following raw materials in parts by weight: 10 to 25 parts of potassium feldspar, 15 to 25 parts of frit, 3 to 5 parts of dolomite, 10 to 15 parts of limestone, 1 to 5 parts of barium carbonate, 10 to 15 parts of lithium feldspar, 6 to 10 parts of kaolin, 5 to 10 parts of zinc oxide and 10 to 15 parts of strontium carbonate; the frit is the frit according to any one of claims 1 to 2.

[0016] The present invention obtains the above-mentioned raw material component ratio through multiple adjustments. The prepared glaze not only has good water retention and can be suitable for preparing marble tiles by large-scale screen printing technology, but also has a delicate and soft glaze surface, good glaze slurry performance, which is conducive to the coloring of colorants, high glaze slurry density, good anti-slip effect, high wear resistance, good anti-fouling and easy cleaning.

[0017] The present invention also discloses a method for preparing a ceramic tile, using the glaze as claimed in claim 4, comprising the following steps:

[0018] A. preparing a ceramic body;

[0019] B. applying a glaze on the surface of the ceramic body to obtain a glaze layer; and printing a preset pattern on the glaze layer;

[0020] C. preparing the glaze, and applying the glaze on a preset pattern by screen printing;

[0021] D. After calcination, the ceramic brick is obtained.

[0022] The above method can be used to prepare extra-large-sized marble tiles using a screen printing process. The prepared tiles have high color saturation, good anti-slip effect, high wear resistance, good anti-fouling, and are easy to clean. They can meet the current high-quality needs of people for extra-large-sized marble tiles, and are also conducive to improving production efficiency and simplifying the production process.

[0023] Preferably, in the above preparation method, in step C, the preparation method of the glaze comprises the following steps:

[0024] The raw materials of the glaze, printing paste, printing oil and water are uniformly mixed and ball-milled. After ball-milling for 25 minutes, every 100g is passed through a 400-mesh sieve to obtain the glaze. The amount of water added is 10-15% of the total weight of the raw materials of the glaze.

[0025] Preferably, in the above preparation method, in the step D, the calcination temperature is 1180-1210° C., and the calcination time is 60-70 min.

[0026] The invention also discloses a ceramic tile prepared by the preparation method.

[0027] Compared with the prior art, the present invention has at least the following beneficial effects: it solves the problems of glaze sticking to the screen, falling off, poor water retention and uneven printing in super-large screen (900*1800mm) printing technology, and can realize the production of marble tiles by super-large screen printing technology to enhance the thickness of super-large glaze color, reduce the amount of inkjet ink used, make the glaze color more vivid and three-dimensional, and the tiles have good anti-slip effect, high wear resistance, good anti-fouling, and easy cleaning. The product production process is simple, stable and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.

[0029] Figure 1 This is a rendering of the ceramic tile surface obtained in Example 5.

[0030] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0032] The invention provides a frit, which comprises the following raw materials in parts by weight: 8-10 parts of albite, 5-10 parts of strontium carbonate, 5-15 parts of aluminum oxide, 1-6 parts of corundum, 3-6 parts of borax, 10-15 parts of diopside, 5-10 parts of ball clay, 10-15 parts of fluorite, 15-20 parts of quartz, 4-10 parts of dolomite and 1-2 parts of nepheline.

[0033] Its chemical composition, measured by mass percentage, includes: SiO2 43-50%, Al2O3 16-21%, Fe2O31-3%, CaO 5-10%, MgO1-3%, K2O 1-5%, Na2O 5-10%, ZnO 5-15% and ignition loss 1-3%, with the remainder being impurities.

[0034] The frit has strong water retention and good screen-cleaning properties, and can be used in glazes to solve problems such as easy sticking to the screen, easy falling off, poor water retention, and uneven printing in different screen printing processes; it is particularly suitable for ultra-large-scale screen printing technology, and can avoid problems such as glaze adhesion or pattern layer adhesion caused by large screen size and slow screen lifting.

[0035] The method for preparing the above frit comprises the following steps:

[0036] (1) Mix the raw materials uniformly according to the proportion;

[0037] (2) sintering the raw materials at 1300-1400°C to melt into glass liquid, and quenching with water;

[0038] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 30 to 40 minutes, dried at 120 to 150° C., and sieved to obtain the frit.

[0039] A glaze containing the above-mentioned frit includes the following raw materials in parts by weight: 10-25 parts of potassium feldspar, 15-25 parts of frit, 3-5 parts of dolomite, 10-15 parts of limestone, 1-5 parts of barium carbonate, 10-15 parts of lithium feldspar, 6-10 parts of kaolin, 5-10 parts of zinc oxide and 10-15 parts of strontium carbonate. The prepared glaze layer has the best comprehensive performance, good anti-slip effect, best wear resistance and anti-fouling performance, high glaze color saturation, good glaze coloring, and only half the amount of conventional ink is needed to achieve the same color effect.

[0040] A method for preparing a ceramic tile using the above glaze comprises the following steps:

[0041] A. Prepare a ceramic body and dry it for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0042] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0043] C. Evenly mix the raw materials of the above glaze, printing paste, printing oil and water, and ball-mill them. After ball-milling for 25 minutes, every 100g is passed through a 400-mesh sieve to obtain the above glaze, wherein the amount of water added is 10-15% of the total weight of the raw materials of the glaze; as a preferred embodiment, 50-60 parts of printing paste, 10-20 parts of printing oil and 10-15g of water are used. The glaze is applied on the preset pattern by screen printing;

[0044] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1180-1210° C. for 60-70 min to obtain the ceramic tile.

[0045] The embodiments of the present invention will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0046] The present invention can use any conventional ceramic powder on the market to make a ceramic green body. A group of green bodies are provided herein for the preparation of the ceramic green bodies in the following embodiments. The chemical composition of the green body powder includes, by mass percentage: SiO2: 40%, Al2O3: 20%; Fe2O3: 0.01%; CaO: 3.5%; MgO: 6%; K2O: 1%; Na2O: 17%; TiO2: 2%; BaO: 7%; ZnO: 2.5%; MnO<0.01%; P2O5<0.01%; SO3<0.02%; ZrO2<0.4%; SrO<0.04%, and the loss on ignition is 0.5%.

[0047] The present invention can use any conventional glaze raw materials on the market to prepare the glaze layer. A set of raw material compositions for the glaze layer is provided herein for use in the preparation of the glaze layer in the following embodiments, which include the following raw materials, in parts by weight: 42 parts of lithium feldspar, 10 parts of quartz, 10 parts of wollastonite, 9 parts of kaolin, 5 parts of zinc oxide, 11 parts of aluminum oxide, 13 parts of zirconium silicate, 0.15 parts of methyl cellulose and 0.55 parts of sodium tripolyphosphate.

[0048] Example 1

[0049] Preparation of frit:

[0050] (1) Mix the raw materials according to the proportions shown in Table 1;

[0051] (2) Firing at 1350°C to melt into glass liquid and quenching with water;

[0052] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 35 min, dried at 125° C., and sieved through a 325-mesh sieve to obtain a frit for later use.

[0053] The chemical composition of the prepared frit is shown in Table 2.

[0054] Prepare raw glaze powder, mix the raw material components shown in Table 3, add 55 parts of printing paste, 15 parts of printing oil and 15g of water, ball mill for 25min per 100g, pass through a 400-mesh sieve, and prepare glaze for standby use.

[0055] A method for preparing a ceramic tile comprises the following steps:

[0056] A. Prepare the ceramic powder into a ceramic body with a specification of 900*1800mm, dry it and set it aside for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0057] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0058] C. Apply glaze on the preset pattern by screen printing;

[0059] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1190° C. for 65 min to obtain the ceramic tile.

[0060] Example 2

[0061] Preparation of frit:

[0062] (1) Mix the raw materials according to the proportions shown in Table 1;

[0063] (2) Firing at 1380°C to melt into glass liquid and quenching with water;

[0064] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 38 min, dried at 130° C., and sieved through a 325-mesh sieve to obtain a frit for later use.

[0065] The chemical composition of the prepared frit is shown in Table 2.

[0066] Prepare raw glaze powder, mix the raw material components shown in Table 3, add 57 parts of printing paste, 13 parts of printing oil and 12g of water, ball mill for 25min per 100g, pass through a 400-mesh sieve, and prepare glaze for standby use.

[0067] A method for preparing a ceramic tile comprises the following steps:

[0068] A. Prepare the ceramic powder into a ceramic body with a specification of 900*1800mm, dry it and set it aside for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0069] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0070] C. Apply glaze on the preset pattern by screen printing;

[0071] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1200° C. for 68 min to obtain the ceramic tile.

[0072] Example 3

[0073] Preparation of frit:

[0074] (1) Mix the raw materials according to the proportions shown in Table 1;

[0075] (2) Firing at 1385°C to melt into glass liquid and quenching with water;

[0076] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 40 min, dried at 135° C., and sieved through a 325-mesh sieve to obtain a frit for later use.

[0077] The chemical composition of the prepared frit is shown in Table 2.

[0078] Prepare raw glaze powder, mix the raw material components shown in Table 3, add 54 parts of printing paste, 14 parts of printing oil and 14g of water, ball mill for 25min per 100g, pass through a 400-mesh sieve, and prepare glaze for standby use.

[0079] A method for preparing a ceramic tile comprises the following steps:

[0080] A. Prepare the ceramic powder into a ceramic body with a specification of 900*1800mm, dry it and set it aside for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0081] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0082] C. Apply glaze on the preset pattern by screen printing;

[0083] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1195° C. for 67 min to obtain the ceramic tile.

[0084] Example 4

[0085] Preparation of frit:

[0086] (1) Mix the raw materials according to the proportions shown in Table 1;

[0087] (2) Firing at 1395°C to melt into glass liquid and quenching with water;

[0088] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 40 min, dried at 138° C., and sieved through a 325-mesh sieve to obtain a frit for later use.

[0089] The chemical composition of the prepared frit is shown in Table 2.

[0090] Prepare raw glaze powder, mix the raw material components shown in Table 3, add 58 parts of printing paste, 16 parts of printing oil and 14g of water, ball mill for 25min per 100g, pass through a 400-mesh sieve, and prepare glaze for standby use.

[0091] A method for preparing a ceramic tile comprises the following steps:

[0092] A. Prepare the ceramic powder into a ceramic body with a specification of 900*1800mm, dry it and set it aside for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0093] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0094] C. Apply glaze on the preset pattern by screen printing;

[0095] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1200° C. for 66 minutes to obtain the ceramic tile.

[0096] Example 5

[0097] Preparation of frit:

[0098] (1) Mix the raw materials according to the proportions shown in Table 1;

[0099] (2) Firing at 1400°C to melt into glass liquid and quenching in water;

[0100] (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 39 minutes, dried at 140°C, and sieved through a 325-mesh sieve to obtain a frit for later use.

[0101] The chemical composition of the prepared frit is shown in Table 2.

[0102] Prepare raw glaze powder, fully mix the raw material components shown in Table 3, add 60 parts of printing paste, 18 parts of printing oil and 15g of water, ball mill for 25min per 100g, pass through a 400-mesh sieve, and prepare glaze for standby use.

[0103] A method for preparing a ceramic tile comprises the following steps:

[0104] A. Prepare the ceramic powder into a ceramic body with a specification of 900*1800mm, dry it and set it aside for use; moisten the dried ceramic body with water so that the surface of the body contains 4-6% moisture;

[0105] B. Prepare materials according to the ratio of each raw material of the glaze layer, mix them thoroughly, add 40% water of the total weight of each raw material of the glaze layer, ball mill for 25 minutes per 100g, pass through a 325-mesh sieve to obtain a glaze material, apply the glaze on the surface of the ceramic body to obtain a glaze layer; print a preset pattern on the glaze layer;

[0106] C. Apply glaze on the preset pattern by screen printing;

[0107] D. The green body obtained in step C is calcined in a kiln at a high temperature of 1210° C. for 70 min to obtain the ceramic tile.

[0108] Table 1 Raw material composition of frit (parts by weight)

[0109]

[0110]

[0111] Table 2 Chemical composition of frit (mass percentage)

[0112] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> ZnO LOI Example 1 44 20 1 7 3 5 7 11 2 Example 2 46 18 2 8 2 4 8 10 2 Example 3 48 17 1 6 1 2 10 14 1 Example 4 49 16 3 6 2 4 6 12 2 Example 5 43 21 2 5 3 5 7 13 1

[0113] Table 3 Raw material composition of glaze (parts by weight)

[0114] Example 1 Example 2 Example 3 Example 4 Example 5 Potassium feldspar 12 18 20 23 25 Frit 15 16 18 21 24 dolomite 5 4 4 3 4 limestone 15 14 12 13 11 Barium carbonate 5 3 4 5 2 Lithium feldspar 15 14 10 11 10 Kaolin 8 9 10 8 7 Zinc Oxide 10 9 8 6 7 Strontium carbonate 15 13 14 10 10

[0115] Comparative Example 1

[0116] The same preparation steps and parameters as those in Example 3 were used, except that no frit was added in this comparative example.

[0117] Comparative Example 2

[0118] The same preparation steps and parameters as those in Example 3 were adopted, except that the frit was replaced with a conventional frit, whose chemical composition, by mass percentage, included: SiO2 35%, Al2O3 12%, Fe2O3 0.2%, CaO 3.5%, MgO 5.5%, K2O 9%, Na2O 3%, ZnO 2%, ignition loss 2%, and the remainder being impurities.

[0119] The sizes of the prepared ceramic bodies are shown in the following table (Note: the specifications of the ceramic bodies correspond to the specifications of the corresponding finished bricks):

[0120]

[0121] Comparative Example 3

[0122] The same preparation steps and parameters as those in Example 3 were used, except that in the preparation of the frit in this comparative example, the frit was not dried after soaking in hydrochloric acid in step (3), but was directly dried and ground after quenching with water.

[0123] The comprehensive performance of the ceramic tiles prepared in Examples 1 to 5 and Comparative Examples 1 to 3 was tested using the following testing methods and standards:

[0124] (1) Glaze pattern effect: A colorimeter is used to test the saturation of the color on the surface of the ceramic tile. The higher the saturation value, the better the color. Specifically, if the saturation value is ≥90%, the glaze effect is excellent; if the saturation value is set to 80-90%, the glaze effect is good; if the saturation value is less than 80%, the glaze effect is poor. In the actual production process, a good glaze effect is considered to meet the large-scale production standards.

[0125] (2) Anti-slip performance: According to the national standard GB / T4100-2015 Appendix M "Determination of friction coefficient", the static friction coefficient is used to test the anti-slip performance. The larger the static friction coefficient, the higher the anti-slip performance.

[0126] (3) Wear resistance determination: The wear resistance of the glaze surface of the product is tested using the test method in the national standard GB / T3810.7-2016 "Ceramic Tile Test Methods Part 7: Determination of Surface Wear Resistance of Glazed Tiles". The wear resistance of the ceramic tile is evaluated by placing abrasive media on the glaze surface and rotating it, and observing and comparing the worn and unworn samples.

[0127] (4) Determination of anti-fouling grade: The anti-fouling performance of the product glaze is tested using the test method of the national standard GB / T3810.14-2016 "Ceramic Tile Test Methods Part 14 Determination of Anti-fouling Performance". The anti-fouling agents include paste-like contaminants, contaminants that can undergo oxidation reactions, contaminants that can form thin films, olive oil, etc. The anti-fouling performance is divided into 1 to 5 levels according to the difficulty of cleaning. The higher the level, the better the anti-fouling performance.

[0128] The test results are shown in Table 4.

[0129] Table 4 Test results of Examples 1 to 5 and Comparative Examples 1 to 3

[0130]

[0131]

[0132] It can be seen from Table 4 that when conventional frits are used, when the specifications of the ceramic green body are small (600*600mm, 600*900mm), the surface patterns of the ceramic tiles obtained in Examples 2-1 and 2-2 are complete and flawless. However, when the specifications of the ceramic green body are large (900*1800mm), white spots appear on the surface of the ceramic tiles obtained in Example 2-3, indicating that the screen size is too large and the glaze is sticking, which affects the depth of the pattern printing and the color of the overall pattern. When large-sized ceramic tiles were produced in Example 1, the frit in this scheme was not added to the glaze, and the ceramic tiles obtained had poor glaze, poor wear resistance, and poor anti-fouling. In Example 3, since the frit was not dried after soaking in hydrochloric acid, the anti-fouling and wear-resistant properties of the ceramic obtained were slightly poor. The large-sized ceramic tiles obtained in Examples 1 to 5 have complete surface patterns and high color saturation, and at the same time have good anti-slip properties, high wear resistance, and good anti-fouling effects. Figure 1 As shown, the ceramic tile surface prepared in Example 5 has high color saturation, clear texture, and no pattern problems caused by glaze adhesion.

[0133] Comparative Example 4

[0134] This comparative example adopts the same preparation steps and parameters as Example 5, except that the raw material components of the glaze are adjusted as shown in the following table (parts by weight):

[0135]

[0136]

[0137] The comprehensive performance of the ceramic tile prepared in Comparative Example 4 was tested, and the test results are shown in Table 5.

[0138] Table 5 Test results of comparative example 4

[0139] Glaze effect Static friction coefficient Wear resistance Antifouling performance Comparative Example 4 good 0.68 2100 rpm 4th level Level 5

[0140] As shown in Table 5, Comparative Example 4 uses a glaze formula different from that of the present solution, and the frit described in the present solution is added to the formula, so that large-sized ceramic tiles can still be produced by screen printing, and the glaze pattern effect is good, but the wear resistance of the ceramic tile surface is slightly poor, and the color saturation is not optimal. This shows that the glaze layer prepared by using the glaze formula used in the present solution and the frit has the best comprehensive performance, good anti-slip effect, best wear resistance and anti-fouling performance, and high glaze color saturation.

[0141] Example 6

[0142] This embodiment adopts the same preparation steps and parameters as those of embodiment 3, except that the amount of water added when preparing the glaze is adjusted as shown in the following table:

[0143]

[0144] The comprehensive properties of the ceramic tile prepared in Example 6 were tested, and the test results are shown in Table 6.

[0145] Table 6 Test results of Example 6

[0146] Glaze effect Static friction coefficient Wear resistance Antifouling performance Example 6-1 good 0.66 2100 rpm 4th level Level 5 Example 6-2 good 0.67 2100 rpm 4th level Level 5 Example 6-3 excellent 0.70 6000 rpm 4th level Level 5 Example 6-4 excellent 0.71 6000 rpm 4th level Level 5

[0147] As shown in Table 6, the amount of water added to the glaze directly affects the viscosity and fluidity of the glaze performance. The anti-skid effect, wear resistance, anti-fouling performance and glaze effect of the ceramic tiles prepared in Examples 6-3 and 6-4 are the best, indicating that after debugging, when 12-15% of the total weight of the glaze slurry is added to the glaze, the comprehensive quality of the glaze layer of the ceramic tiles after firing is the best.

[0148] In summary, the frit of the present invention has strong water retention and good screen-cleaning properties. The glaze obtained can solve the problems of glaze adhesion or pattern layer adhesion caused by too large a screen and slow lifting of the screen when large-scale screen printing technology is used to produce ceramic tiles. By optimizing the glaze raw material components, a glaze layer with the best comprehensive performance can be obtained, which has good anti-slip performance, high wear resistance, good anti-fouling effect, and high color saturation.

[0149] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A frit, characterized in that: The invention comprises the following raw materials in parts by weight: 8 to 10 parts of albite, 5 to 10 parts of strontium carbonate, 5 to 15 parts of aluminum oxide, 1 to 6 parts of corundum, 3 to 6 parts of borax, 10 to 15 parts of diopside, 5 to 10 parts of ball clay, 10 to 15 parts of fluorite, 15 to 20 parts of quartz, 4 to 10 parts of dolomite and 1 to 2 parts of nepheline.

2. The frit according to claim 1, characterized in that Its chemical composition, measured by mass percentage, includes: SiO2 43-50%, Al2O3 16-21%, Fe2O3 1-3%, CaO 5-10%, MgO1-3%, K2O 1-5%, Na2O 5-10%, ZnO 5-15% and ignition loss 1-3%, with the remainder being impurities.

3. The method for preparing a frit according to any one of claims 1 to 2, characterized in that: The steps include: (1) Mix the raw materials uniformly according to the proportion; (2) sintering the raw materials at 1300-1400°C to melt into glass liquid, and quenching with water; (3) The water-quenched frit is dried and ground, then soaked in hydrochloric acid for 30 to 40 minutes, dried at 120 to 150° C., and sieved to obtain the frit.

4. A glaze, characterized in that: The invention comprises the following raw materials in parts by weight: 10 to 25 parts of potassium feldspar, 15 to 25 parts of frit, 3 to 5 parts of dolomite, 10 to 15 parts of limestone, 1 to 5 parts of barium carbonate, 10 to 15 parts of lithium feldspar, 6 to 10 parts of kaolin, 5 to 10 parts of zinc oxide and 10 to 15 parts of strontium carbonate; the frit is the frit according to any one of claims 1 to 2.

5. A method for preparing a ceramic tile, characterized in that: Using the glaze as claimed in claim 4 comprises the following steps: A. preparing a ceramic body; B. applying a glaze on the surface of the ceramic body to obtain a glaze layer; and printing a preset pattern on the glaze layer; C. preparing the glaze as claimed in claim 4, and applying the glaze on a preset pattern by screen printing; D. After calcination, the ceramic brick is obtained.

6. The method for preparing a ceramic tile according to claim 5, characterized in that: In step C, the method for preparing the glaze comprises the following steps: The raw materials of the glaze, printing paste, printing oil and water are uniformly mixed and ball-milled. After ball-milling for 25 minutes, every 100g is passed through a 400-mesh sieve to obtain the glaze. The amount of water added is 10-15% of the total weight of the raw materials of the glaze.

7. The method for preparing a ceramic tile according to claim 5, characterized in that: In the step D, the calcination temperature is 1180-1210° C., and the calcination time is 60-70 minutes.

8. A ceramic tile, characterized in that: The ceramic tile is prepared by the method for preparing the ceramic tile as described in any one of claims 5 to 7.

Citation Information

Patent Citations

  • Matte glaze and preparation method thereof

    CN110510876A

  • High-transmittance anti-pollution full-polished glaze and preparation method of glazed brick applying high-transmittance anti-pollution full-polished glaze

    CN112592059A

  • Low-gloss transparent glaze, ceramic tile using low-gloss transparent glaze and preparation method of ceramic tile

    CN112707644A

  • Antibacterial purification glaze and preparation method of glazed tile using same

    CN112723745A

  • Fabric texture matt glaze, matt frit, ceramic tile, application and preparation method

    CN113968675A

Cited By

  • White gold dry granules, white gold dry granule glaze, marble ceramic tile and preparation method of marble ceramic tile

    CN119912165A

  • Unyielding Gold Granules, Unyielding Gold Granular Glaze, Marble Tiles and Their Preparation Methods

    CN119912165B