Asymmetric suction magnet and manufacturing method therefor, and magnet assembly

By using single-sided or double-sided oriented magnetic field pressing method in magnet preparation, the difficulties in the preparation of small-volume asymmetric suction magnets are solved, and efficient and crack-free magnet molding is achieved, ensuring suction asymmetry and performance consistency.

WO2024230007A1PCT designated stage expired Publication Date: 2024-11-14CHENG MUYANG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/113776
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2023-08-18
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently prepare asymmetric suction magnets with small volume and multi-magnetic units, and there are problems such as unstable bonding and cracking.

Method used

The magnetic powder is pressed into a blank by using single-sided or double-sided orientation magnetic field pressing method, and through post-treatment such as vacuum sintering, heat treatment, isostatic pressure and mechanical processing, an integrated asymmetric suction magnet is formed to eliminate hidden dangers in the splicing process. .

Benefits of technology

It realizes efficient preparation of asymmetric suction magnets, improves production efficiency, eliminates the risk of cracking, and ensures the performance consistency and suction asymmetry of the magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023113776_14112024_PF_FP_ABST
    Figure CN2023113776_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An asymmetric suction magnet and a manufacturing method therefor, and a magnet assembly, relating to the technical field of magnetic materials and magnet assemblies. The manufacturing method for an asymmetric suction magnet comprises the following steps: placing magnetic powder into a pressing die, and pressing the magnetic powder into a compact in a single-sided oriented magnetic field, wherein the single-sided oriented magnetic field means that in a die cavity of the pressing die, only one surface in the die cavity is provided with an oriented magnetic field; and carrying out post-treatment on the compact to obtain an asymmetric suction magnet. A special oriented pressing method is used to integrally form an asymmetric suction magnet, thereby achieving high manufacturing efficiency, and eliminating hidden dangers such as cracking in existing methods for manufacturing an asymmetric suction magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Asymmetric attraction magnet and preparation method thereof, and a magnet assembly

[0001] This disclosure claims priority to a Chinese patent application filed with the Patent Office of China on May 8, 2023, with application number 202310509682.8 and invention name “Asymmetric attractive magnet, preparation method thereof, and a magnet assembly”, the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0002] The present invention relates to the technical field of magnetic materials and magnet assemblies, and in particular to an asymmetric attraction magnet and a preparation method thereof, and a magnet assembly. Background Art

[0003] Magnetic materials are fundamental functional materials with a wide range of applications. Different industries have varying requirements for a magnet's magnetic circuit structure, magnetic field strength, magnetic field distribution, and suction force. Some industries require magnets or magnetic components to exhibit maximum suction in a specific direction, while minimizing suction in the opposite direction. These applications include magnetic buttons, magnetic luggage buckles, magnetic clasps on mobile phone cases, and magnetic clasps on iPad cases. These magnets are commonly referred to as asymmetric suction magnets or components (devices), and HALBACH magnets are one such component.

[0004] Magnets with a difference of more than 1x between the suction forces of their two attractive surfaces are generally referred to as asymmetric magnets. For magnets of the same shape and size, the suction force is proportional to the magnetic field strength on the magnet's surface: the higher the surface magnetic field strength, the greater the suction force, and vice versa. Therefore, to create asymmetric suction between the front and back sides of a magnet, one must ensure that the surface magnetic field strengths on the two sides are asymmetric. Conventional magnets have symmetrically distributed north and south poles on the front and back sides. Generally, the surface magnetic field strengths on the two sides are similar, and therefore the suction force is also similar. To create asymmetric magnetic field strength between the two sides, one must alter the distribution of the magnetic lines of force within the magnet. This means altering the orientation of the magnet so that the majority of the magnetic lines of force are concentrated on one pole face, thereby increasing the suction force on that pole face and reducing the suction force on the opposite pole face.

[0005] Currently, the methods for preparing asymmetric suction magnets are almost all: magnet units with different orientations are processed separately and then fastened together with glue or fasteners according to the designed arrangement. For asymmetric suction magnet assemblies with larger volume and simpler structure, this preparation method is simple and fast. However, if the asymmetric suction magnet or assembly is smaller and the number of magnet units with different orientations is large, many difficulties will be encountered. For example, if the magnetic assembly is small, the magnet units with different orientations cannot be fastened together with fasteners; if the contact area between magnet units with different orientations is small, there is a risk of cracking when using adhesives to combine them, etc.

[0006] Summary of the Invention

[0007] In view of this, the present invention provides an asymmetric attraction magnet, a preparation method thereof, and a magnet assembly. The main purpose is to adopt a special oriented pressing method to integrally form an asymmetric attraction magnet, which has high preparation efficiency and eliminates the hidden dangers such as cracking in the existing method of preparing asymmetric attraction magnets.

[0008] To achieve the above objectives, the present invention mainly provides the following technical solutions:

[0009] In one aspect, an embodiment of the present invention provides a method for preparing an asymmetric attractive magnet, comprising the following steps:

[0010] Compacting step: placing magnetic powder into a compacting die and pressing the magnetic powder into a compact in a unilaterally oriented magnetic field; wherein the unilaterally oriented magnetic field means that an oriented magnetic field is provided on only one surface of the cavity of the compacting die; wherein the magnetic powder is magnetic powder for sintering magnets;

[0011] Post-processing step: post-processing the blank to obtain an asymmetric attraction magnet.

[0012] Preferably, the pressing mold includes a mold side plate, an upper punch, and a lower punch; wherein, the mold cavity of the pressing mold is surrounded by the mold side plate, the upper punch, and the lower punch; preferably, the mold cavity has multiple surfaces, and the orientation magnetic field is arranged on one of the multiple surfaces; further preferably, the mold cavity has six surfaces.

[0013] Preferably, the number of magnetic poles in the orientation magnetic field is odd; preferably, there is only one S pole in the orientation magnetic field or there is only one N pole in the orientation magnetic field; preferably, there is only one S pole and two N poles in the orientation magnetic field; or there is only one N pole and two S poles in the orientation magnetic field.

[0014] Preferably, the orientation magnetic field has at least two magnetic poles, and each magnetic pole is strip-shaped; wherein, in the orientation magnetic field, the strip-shaped N poles and the strip-shaped S poles are arranged at intervals.

[0015] Preferably, the orientation magnetic field is a grid-shaped orientation magnetic field; wherein, the grid-shaped orientation magnetic field has multiple magnetic poles, and the multiple magnetic poles are arranged in a grid structure, and each magnetic pole serves as a grid unit; preferably, all magnetic poles in the grid-shaped orientation magnetic field are S poles; or all magnetic poles in the grid-shaped orientation magnetic field are N poles; preferably, the grid-shaped orientation magnetic field includes N poles and S poles, and the grid units of the N poles and the grid units of the S poles are arranged at intervals.

[0016] Preferably, the orientation magnetic field includes a plurality of magnetic poles, and the plurality of magnetic poles are arranged concentrically from the inside to the outside. Preferably, the orientation magnetic field includes at least one annular N pole and at least one annular S pole, and the annular N pole and the annular S pole are arranged at intervals. Preferably, the orientation magnetic field includes at least one annular magnetic pole and one circular magnetic pole; wherein the annular magnetic pole is arranged around the circular magnetic pole; wherein the S pole and the N pole in the orientation magnetic field are arranged at intervals. Preferably, the orientation magnetic field includes a plurality of annular magnetic poles arranged concentrically from the inside to the outside; wherein each annular magnetic pole is composed of at least one arc-shaped N pole and at least one arc-shaped S pole; wherein the N pole and the S pole in the orientation magnetic field are arranged at intervals; further preferably, each annular magnetic pole is composed of two quarter-arc-shaped N poles and two quarter-arc-shaped S poles.

[0017] Preferably, the particle size of the magnetic powder is 2.0-6.0 μm.

[0018] Preferably, before the pressing step, the method further comprises:

[0019] The steps of preparing magnetic powder are as follows: melting raw materials into alloy according to the chemical composition of magnetic powder; crushing and grinding the alloy into magnetic powder.

[0020] Preferably, the post-processing step comprises:

[0021] Vacuum sintering and heat treatment steps: vacuum sintering and heat treating the blank in sequence to obtain an asymmetric attraction magnet blank;

[0022] Preferably, the temperature of the vacuum sintering treatment is 1000-1200°C; further preferably, the time of the vacuum sintering treatment is 2-4 hours;

[0023] Preferably, the heat treatment includes a first heat treatment and a second heat treatment; wherein the temperature of the first heat treatment is 850-950°C, and the temperature of the second heat treatment is 450-550°C; further preferably, the time of the first heat treatment is 2-4 hours, and the time of the second heat treatment is 2-4 hours;

[0024] Preferably, before the vacuum sintering step, the method further comprises:

[0025] Isostatic pressing step: performing isostatic pressing on the green block to increase the density of the green block and reduce the deformation during the sintering stage; preferably, the isostatic pressing is liquid isostatic pressing or dry isostatic pressing.

[0026] Preferably, the post-processing step further comprises:

[0027] Machining and magnetizing treatment steps: machining the asymmetric attraction magnet blank to a desired size and then magnetizing it to obtain the asymmetric attraction magnet.

[0028] On the other hand, an embodiment of the present invention provides an asymmetric attraction magnet, wherein the asymmetric attraction magnet is an integrated structure; preferably, the asymmetric attraction magnet is prepared by any of the above-mentioned methods for preparing an asymmetric attraction magnet. Preferably, the asymmetric attraction magnet has a first surface (i.e., the front surface of the asymmetric attraction magnet) and a second surface (i.e., the back surface of the asymmetric attraction magnet) relative to each other; wherein the surface magnetic field strength of the first surface is more than twice the surface magnetic field strength of the second surface.

[0029] In yet another aspect, an embodiment of the present invention provides a method for preparing an asymmetric attraction magnet, wherein magnetic powder is pressed into a compact, and the compact is then post-processed to obtain the asymmetric attraction magnet; wherein, the magnetic powder is magnetic powder for sintering magnets;

[0030] In the pressing step: magnetic powder is placed in a pressing mold and pressed into a blank under a set double-sided orientation magnetic field; wherein the set double-sided orientation magnetic field means: in the mold cavity of the pressing mold, there are two groups of orientation magnetic fields; wherein the first group of orientation magnetic fields is set on the first surface of the mold cavity, and the second group of orientation magnetic fields is set on the second surface of the mold cavity; wherein the first surface and the second surface are arranged opposite to each other; wherein the magnetic poles in the first group of orientation magnetic fields are first magnetic poles, and the magnetic poles in the second group of orientation magnetic fields are second magnetic poles; wherein the number of first magnetic poles and second magnetic poles is the same and they are opposite to each other; wherein the magnetic polarity of the first magnetic pole and the second magnetic pole opposite to it are the same, both are N poles or both are S poles;

[0031] In which, the orientation degree of the two surfaces of the block in contact with the orientation magnetic field poles is greater than the orientation degree at the middle position of the block; at the middle position, the block is cut into two pieces along a surface parallel to the surface where the orientation magnetic field poles are located or cut in any step of post-processing, and finally an asymmetric suction magnet is obtained.

[0032] On the other hand, an embodiment of the present invention provides an asymmetric attraction magnet, which is an integrated structure; preferably, the asymmetric attraction magnet is prepared by the above-mentioned method for preparing the asymmetric attraction magnet.

[0033] On the other hand, an embodiment of the present invention provides a magnetic assembly, characterized in that the magnetic assembly includes the above-mentioned asymmetric attractive magnet.

[0034] In addition, an embodiment of the present invention further provides a method for preparing an asymmetric attraction bonding magnet, characterized in that it comprises the following steps:

[0035] The pressing step comprises placing the anisotropic bonded magnetic powder into a pressing die and pressing the anisotropic bonded magnetic powder into a compact in a unilateral orientation magnetic field; wherein the unilateral orientation magnetic field refers to providing an orientation magnetic field on only one surface of the die cavity of the pressing die;

[0036] Baking: Baking the compact to obtain an asymmetric attraction bonding magnet.

[0037] In addition, an embodiment of the present invention further provides an asymmetric suction bonding magnet, characterized in that the asymmetric suction bonding magnet is prepared by the above-mentioned preparation method of the asymmetric suction bonding magnet.

[0038] In addition, an embodiment of the present invention provides a magnetic assembly, characterized in that the magnetic assembly includes the above-mentioned asymmetric attraction bonding magnet.

[0039] Compared with the prior art, the asymmetric attractive magnet and its preparation method, as well as a magnetic assembly provided by the present invention have at least the following beneficial effects:

[0040] On the one hand, the embodiment of the present invention proposes a method for preparing an asymmetric attraction magnet, which proposes for the first time that magnetic powder is pressed into a slab in a single-sided orientation magnetic field, and the slab is subjected to post-processing to obtain an asymmetric attraction magnet. Specifically, the method of the present invention only sets an orientation magnetic field on one surface in the mold cavity, so that the magnetic field at one end of the mold cavity (the end close to the orientation magnetic field pole) is strong, and the magnetic lines of force near the magnetic pole are approximately arranged in parallel, while the magnetic field at the other end (the end away from the orientation magnetic field pole) is weak, and most of the magnetic lines of force are curved. Therefore, the magnetic powder near one end of the orientation magnetic field is arranged in an orderly manner and has a high degree of orientation, and the magnetic properties of the magnet at this end are high, while the magnetic powder at the other end (the end away from the orientation magnetic field) has a low degree of orientation, and the magnetic properties of the magnet at this end are low. Therefore, in the single-sided orientation magnetic field proposed by the present invention, the slab is pressed into a slab, and after post-processing, an asymmetric attraction magnet can be obtained. This is a concept proposed for the first time by the present invention and has not been proposed in the prior art.

[0041] Furthermore, an embodiment of the present invention proposes a method for preparing an asymmetric attractive magnet, in which multiple magnetic poles in a unilaterally oriented magnetic field are arranged into any one of a strip, ring, and grid shape. Different arrangements are suitable for producing magnets and components with different uses or shapes. For example, magnetic poles arranged in strips are suitable for producing rectangular magnets with relatively small dimensions in the strip direction; during production, the mold dimensions of the other two directions are designed as required, and the dimensions in the strip direction can be very long. After the blank is produced, it is cut into many sections, and one bar magnet can be processed into many small rectangular magnetic pieces. For example, the ring shape is suitable for the production of circular magnets and components (such as magnetic buttons). The grid arrangement is suitable for the production of square magnets or components. During production, a relatively large square magnet can be produced and then cut into multiple small square pieces. The above arrangement is considered to improve production efficiency.

[0042] On the other hand, an embodiment of the present invention proposes a method for preparing an asymmetric attractive magnet, which for the first time proposes that in a pressing step, magnetic powder is placed in a pressing mold and pressed into a blank under a set double-sided orientation magnetic field; wherein the set double-sided orientation magnetic field means: in the mold cavity of the pressing mold, there are two groups of orientation magnetic fields; wherein the first group of orientation magnetic fields is set on the first side of the mold cavity, and the second group of orientation magnetic fields is set on the second side of the mold cavity; wherein the first side and the second side are arranged opposite to each other; wherein the magnetic poles in the first group of orientation magnetic fields are first magnetic poles, and the magnetic poles in the second group of orientation magnetic fields are second magnetic poles; wherein the number of first magnetic poles and second magnetic poles is the same and they are opposite to each other; wherein the magnetic pole polarity of the first magnetic pole and the second magnetic pole opposite to it are the same, both are N poles or both are S poles (unlike the prior art, although the prior art also adopts a double-sided orientation magnetic field, in the double-sided orientation magnetic field of the prior art, the magnetic pole polarity of the first magnetic pole and the second magnetic pole opposite to it are opposite). wherein the orientation degree at both ends of the blank is greater than the orientation degree at the middle position of the blank. This is equivalent to treating the two orientation magnetic fields as a single-sided orientation magnetic field. The magnet prepared by this orientation magnetic field can be divided into two pieces of asymmetric attractive magnets by splitting it in half from the middle.

[0043] In summary, the asymmetric attraction magnet prepared by the method proposed in the embodiment of the present invention is an integrated structure, and is not spliced ​​together as in the prior art. Moreover, the method of the present invention has high preparation efficiency and eliminates the hidden dangers such as cracking proposed in the existing method for preparing asymmetric attraction magnets.

[0044] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] FIG1 is a schematic diagram of a unilateral orientation magnetic field provided in a pressing mold according to the present invention;

[0046] FIG2 is a schematic diagram of the magnetic poles in the orientation magnetic field of the present invention arranged in a strip-like manner;

[0047] FIG3 is a schematic diagram of the magnetic poles in the orientation magnetic field of the present invention arranged in a grid-like manner;

[0048] FIG4 is a schematic diagram showing a magnetic pole arrangement in a circular manner in an orientation magnetic field of the present invention;

[0049] FIG5 is another schematic diagram of the magnetic poles in the orientation magnetic field of the present invention arranged in a circular manner;

[0050] FIG6 is another schematic diagram of the magnetic poles in the orientation magnetic field of the present invention arranged in a circular manner;

[0051] FIG7 is a schematic diagram of two sets of orientation magnetic fields provided in a pressing mold according to the present invention;

[0052] FIG8 is a schematic diagram of a grid-shaped unilateral orientation magnetic field with four magnetic poles arranged in a pressing mold according to the present invention. DETAILED DESCRIPTION

[0053] To further illustrate the technical means and effects employed by the present invention to achieve its intended objectives, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention is provided in conjunction with the accompanying drawings and preferred embodiments. In the following description, different references to "one embodiment" or "embodiment" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics of one or more embodiments may be combined in any suitable manner.

[0054] The purpose of the present invention is to overcome the difficulties and shortcomings in the preparation of asymmetric attraction magnets, especially small-volume asymmetric attraction magnets or components mentioned in the background technology.

[0055] The solution of the present invention is not "first processed into magnet monomers and then fastened together by physical methods (such as adhesive bonding)" as mentioned in the background technology, but is prepared by integrated molding using a special oriented pressing method. Therefore, the solution of the present invention not only has high preparation efficiency but also completely eliminates hidden dangers such as cracking.

[0056] Here, the main inventive concept of the present invention is analyzed and explained as follows:

[0057] The magnetic properties of a magnet are closely related to the size and direction of the orientation magnetic field during the magnetic powder molding process. A high and orderly orientation magnetic field in the mold results in a high degree of orientation for the magnetic powder, resulting in high magnetic properties for the magnet. This results in a high surface magnetic field strength and strong suction for magnets of the same size. A weak orientation magnetic field in the mold results in a low degree of orientation for the magnetic powder, resulting in low magnetic properties for the magnet. This results in low surface magnetic field strength and weak suction for magnets of the same size. Prior art methods aim to achieve both high and uniform magnetic properties for the entire magnet. During the magnetic powder molding process, a uniform parallel magnetic field is set (i.e., all magnetic powder is in a parallel magnetic field). This results in uniform magnetic properties for the resulting magnet, with similar magnetic properties across any part of the magnet. Compared to prior art methods, the present invention employs a specifically non-uniform magnetic field in the mold, allowing different degrees of orientation for different surfaces of the magnetic powder in the mold. This results in a magnet with different magnetic properties on its two corresponding surfaces (i.e., the front and back surfaces), resulting in a magnet with asymmetric suction.

[0058] The first concept of the present invention is shown in Figure 1: In the present invention, magnetic powder is pressed into a slab in a single-sided oriented magnetic field, and after post-processing, the slab can be used to obtain an asymmetric attraction magnet. As shown in Figure 1, the oriented magnetic field is set only on one surface in the mold cavity, so that the magnetic field of the oriented magnetic field surface of the mold cavity is strong, and the magnetic lines of force are arranged approximately in parallel near the surface of the magnetic pole of the oriented magnetic field. The farther away from the magnetic pole surface, the lower the magnetic field strength and the less parallel the magnetic lines of force. Therefore, the magnetic powder on the side close to the oriented magnetic field has a high degree of orientation and high magnetic properties, while the magnetic powder on the side away from the oriented magnetic field has a low degree of orientation and low magnetic properties. Therefore, in a single-sided oriented magnetic field, the slab is pressed into a slab and then post-processed to obtain an asymmetric attraction magnet.

[0059] Here, with respect to the first concept proposed by the present invention, a method for preparing an asymmetric attractive magnet is proposed by the present invention, as shown in FIG1 , and comprises the following steps:

[0060] The steps of preparing magnetic powder are as follows: melting raw materials into alloy according to the chemical composition of magnetic powder; crushing and grinding the alloy into magnetic powder.

[0061] The particle size of the magnetic powder is 2.0-6.0 μm.

[0062] Pressing step: placing magnetic powder into a pressing mold and pressing the magnetic powder into a block in a unilaterally oriented magnetic field; wherein the unilaterally oriented magnetic field means that in the mold cavity 3 of the pressing mold, an oriented magnetic field 4 is set only on one surface of the mold cavity.

[0063] In this step, as shown in Figure 1, the pressing mold includes a mold side plate 2, an upper punch 1, and a lower punch 5. The mold cavity 3 of the pressing mold is enclosed by the mold side plate 2, the upper punch 1, and the lower punch 5. The mold cavity 3 has multiple faces, and the orientation magnetic field 4 is arranged on one of the multiple faces. More preferably, the mold cavity 3 has six faces (the mold cavity has six faces: top, bottom, left, right, front, and back, and the orientation magnetic field 4 can be arranged on any of the faces).

[0064] In addition, the arrangement of the magnetic poles in the orientation magnetic field can meet any of the following characteristics: (1) the number of magnetic poles in the orientation magnetic field can be odd, for example, there is only one S pole or one N pole, or there is one S pole and two N poles, etc.; (2) if the orientation magnetic field has two or more different magnetic poles, the N pole and the S pole are arranged at intervals.

[0065] Specifically, the arrangement of the magnetic poles in the unilateral orientation magnetic field of the present invention can be carried out in the following ways:

[0066] The first type, as shown in FIG2 , is that the magnetic poles in the orientation magnetic field are arranged in a strip-like manner: the orientation magnetic field has at least two magnetic poles, and each magnetic pole is in the shape of a strip; wherein, in the orientation magnetic field, the strip-like N poles and the strip-like S poles are arranged at intervals.

[0067] The second type is that the magnetic poles in the orientation magnetic field are arranged in a grid-like manner:

[0068] The orientation magnetic field is a grid-shaped orientation magnetic field; wherein the grid-shaped orientation magnetic field has a plurality of magnetic poles, and the plurality of magnetic poles are arranged in a grid-shaped structure, and each magnetic pole serves as a grid unit.

[0069] One grid arrangement is: all magnetic poles in the grid-shaped orientation magnetic field are S poles; or all magnetic poles in the grid-shaped orientation magnetic field are N poles.

[0070] Another grid arrangement is as shown in FIG3 , in which the grid-shaped orientation magnetic field includes N poles and S poles, and the grid units of the N pole and the grid units of the S pole are arranged alternately.

[0071] The third type is that the magnetic poles in the orientation magnetic field are arranged in a circular manner:

[0072] The orientation magnetic field includes multiple magnetic poles, which are arranged concentrically from the inside to the outside. Based on this, there are several types of circular arrangements:

[0073] One annular arrangement is: as shown in FIG5 , the orientation magnetic field includes at least one annular N pole and at least one annular S pole, and the annular N pole and the annular S pole are arranged at intervals.

[0074] Another arrangement is: as shown in Figure 4, the orientation magnetic field includes at least one annular magnetic pole and one circular magnetic pole; wherein, the annular magnetic pole is arranged around the circular magnetic pole (and when there are multiple annular magnetic poles, multiple annular magnets are arranged in sequence from the inside to the outside); wherein, the S pole and N pole in the orientation magnetic field are arranged at intervals.

[0075] Another arrangement is: as shown in Figure 6, the orientation magnetic field includes a plurality of annular magnetic poles arranged concentrically from the inside to the outside; wherein, each annular magnetic pole is composed of at least one arc-shaped N pole and at least one arc-shaped S pole; wherein, in the orientation magnetic field, the N pole and the S pole are arranged at intervals; further preferably, each annular magnetic pole is composed of two quarter-arc-shaped N poles and two quarter-arc-shaped S poles spliced ​​at intervals.

[0076] Preferably, the pressing step includes: loading the magnetic powder into the mold cavity of the pressing mold (press mold) to allow the unilaterally oriented magnetic field to generate a magnetic field; after the intensity of the unilaterally oriented magnetic field reaches a set value: the lower punch remains fixed, the upper punch moves downward, or the upper punch remains fixed, the lower punch moves upward, or the upper punch and the lower punch move toward the center of the mold cavity at the same time, applying pressure to the magnetic powder until the magnetic powder becomes a blank.

[0077] Post-processing step: post-processing the blank to obtain an asymmetric attraction magnet.

[0078] Here, the post-processing steps include isostatic pressing, vacuum sintering, heat treatment, machining and magnetization.

[0079] Isostatic pressing: The briquette is isostatically pressed to increase its density and reduce deformation during the sintering stage. Preferably, the isostatic pressing is liquid isostatic pressing or dry isostatic pressing. Preferably, the isostatic pressing step comprises placing the briquette in a plastic bag, evacuating the bag, heat-sealing the bag, and then isostatically pressing the bag in an isostatic press at a pressure of 150-250 MPa.

[0080] Vacuum sintering and heat treatment steps: the blank is subjected to vacuum sintering and heat treatment in sequence to obtain an asymmetric attraction magnet blank.

[0081] Preferably, the temperature of the vacuum sintering treatment is 1000-1200°C;

[0082] Preferably, the heat treatment includes a first stage heat treatment and a second stage heat treatment; wherein the temperature of the first stage heat treatment is 850-950°C, and the temperature of the second stage heat treatment is 450-550°C;

[0083] Machining and magnetizing treatment steps: machining the asymmetric attraction magnet blank to a desired size and then magnetizing it to obtain the asymmetric attraction magnet.

[0084] Regarding the magnetization of the present invention, it is necessary to explain as follows: the magnetization method for the asymmetric attraction magnet is a common magnetization method. For example, the magnetization method for the asymmetric attraction magnet prepared according to the unilateral orientation magnetic field shown in FIG1 is as follows: prepare a magnetization fixture that can produce three magnetic poles on each of the upper and lower surfaces. If the magnetic pole produced on the upper surface is an N pole, then the corresponding magnetic pole produced on the lower surface is an S pole. Similarly, the upper S pole corresponds to the lower N pole. The magnet is clamped between the two magnetizing pole heads. If a pulsed magnetic field is formed between the upper and lower magnetic poles, the magnetization of the asymmetric attraction magnet is completed.

[0085] The present invention also provides an asymmetric attraction magnet, characterized in that the asymmetric attraction magnet is prepared by any of the above-described methods for preparing an asymmetric attraction magnet. The asymmetric attraction magnet of the present invention has a high surface magnetic field strength on one side and a strong attraction, while the other side (the opposite side) has a low surface magnetic field strength and a weak attraction.

[0086] In addition, the present invention also proposes a second inventive concept, as shown in FIG7 . The difference between the second inventive concept and the first inventive concept is that:

[0087] As shown in FIG7 , in the pressing step, magnetic powder is placed in a pressing mold and pressed into a green block under a set double-sided orientation magnetic field; wherein the set double-sided orientation magnetic field means: in the mold cavity of the pressing mold, there are two groups of orientation magnetic fields; wherein the first group of orientation magnetic fields is set on the first surface of the mold cavity, and the second group of orientation magnetic fields is set on the second surface of the mold cavity; wherein the first surface and the second surface are arranged opposite to each other; wherein the magnetic poles in the first group of orientation magnetic fields are first magnetic poles, and the magnetic poles in the second group of orientation magnetic fields are second magnetic poles; wherein the number of first magnetic poles and second magnetic poles is the same and they are opposite to each other; wherein the magnetic polarity of the first magnetic pole and the second magnetic pole opposite to it are the same, both are N poles or both are S poles (it should be noted that this is different from the prior art. Although the prior art also adopts a double-sided orientation magnetic field, in the double-sided orientation magnetic field of the prior art, the magnetic polarity of the first magnetic pole and the magnetic pole opposite to it are opposite). wherein the orientation degree of the green block close to the magnetic pole is greater than the orientation degree at the middle position of the green block.

[0088] For the second inventive concept, the double-sided oriented magnetic field pressing shown in Figure 7 is adopted. It is only necessary to cut the block into two pieces at the middle position on a plane parallel to the surface where the oriented magnetic field poles are located, or to perform the middle cutting in any step of the post-processing, and finally two asymmetric attractive magnets can be obtained.

[0089] For the second inventive concept, the arrangement of magnetic poles in the orientation magnetic field on each side, post-processing and other processes refer to the first inventive concept and will not be repeated here.

[0090] Here, let's explain the principle behind the second inventive concept: The corresponding first and second magnetic poles are of the same type, so the opposing first and second orientation magnetic fields repel each other. This results in the magnetic powder in the mold cavity having a high degree of orientation near the first orientation magnetic field and a high degree of orientation near the second orientation magnetic field, while the magnetic powder located between these two ends has a low degree of orientation. This is equivalent to treating the two orientation magnetic fields as a single-sided orientation magnetic field. A magnet fabricated using this orientation magnetic field, if split down the middle, becomes two asymmetric magnets.

[0091] The above-mentioned solutions (two inventive concepts) of the present invention are primarily directed to preparing asymmetric attraction magnets from magnetic powders used in sintered magnets. In fact, the above-mentioned inventive concepts of the present invention are also applicable to anisotropic bonded magnetic powders (such as anisotropic NdFeB bonded magnetic powders, anisotropic SmCo bonded magnetic powders, anisotropic SmFeN bonded magnetic powders, etc.). In the post-processing stage, sintering and heat treatment are eliminated, and instead a baking step (baking temperature of 150-300°C) is used to prepare asymmetric attraction bonded magnets.

[0092] The present invention is further described in detail below through specific embodiments:

[0093] Example 1

[0094] This embodiment prepares an asymmetric attractive magnet, which mainly includes the following steps:

[0095] 1) Smelt a NdFeB alloy according to the following formula (mass percentage): PrNd: 32.5%, Dy: 0.5%, B: 0.92%, Fe: 66.08%. The obtained NdFeB alloy is coarsely crushed and jet milled to produce magnetic powder with a particle size of 3-4 μm.

[0096] 2) Prepare a single-sided orientation magnetic field mold with three strip-shaped magnetic poles as shown in FIG1 . The arrangement of the magnetic field 4 is as shown in FIG2 . The upper and lower punch areas of the mold and the single-sided orientation magnetic field area are both 30 mm x 30 mm.

[0097] 3) Load 25 g of magnetic powder into the mold cavity 3 of the pressing mold (press mold) as shown in Figure 1, form a magnetic field >8000 Gs at the magnetic pole of the unilateral orientation magnetic field 4, keep the lower punch 5 fixed, and move the upper punch 1 downward to apply pressure to the magnetic powder until the magnetic powder becomes a block.

[0098] 4) The compact is isostatically pressed at 180 MPa to further increase the density.

[0099] 5) The isostatically pressed green block is vacuum sintered at 1065°C for 3 hours, then subjected to a first heat treatment at 900°C for 2 hours, and then subjected to a second heat treatment at 500°C for 3 hours to obtain an asymmetric attraction magnet blank.

[0100] 6) Use a surface grinder to remove the black skin and raised parts on the surface of the asymmetric suction magnet blank to form a sheet magnet.

[0101] 7) Place the sheet magnet obtained in (6) in a magnetizing fixture with three poles on each of its upper and lower surfaces. The poles of the magnetizing fixture are arranged such that if the upper pole is an N pole, the corresponding lower pole is an S pole. Similarly, the upper S pole corresponds to the lower N pole. A pulsed magnetic field is generated between the upper and lower poles using a magnetizer, thus completing the magnetization of the asymmetric magnet.

[0102] 8) Use a Gauss meter to detect the maximum surface magnetic field intensity of the three magnetic poles on the front and back surfaces. During molding, the maximum surface magnetic field intensity of the surface close to the unilateral orientation magnetic field is >2800Gs, and the maximum surface magnetic field intensity of the opposite surface is <600Gs. The surface magnetic field intensity of the two surfaces differs by more than 4 times.

[0103] In the magnets prepared in this example, the first end face (one end face) of the magnet is in close proximity to the orientation magnetic field during the pressing process, while the second end face (the other end face) is further away from the orientation magnetic field. The magnetic field strength at the first end face of the magnet is four times greater than that at the second end face. Experiments have shown that the greater the thickness of the magnet, the greater the difference in magnetic field strength between the two end faces.

[0104] Example 2

[0105] 1) Smelt a NdFeB alloy according to the following formula (mass percentage): PrNd: 32.5%, Dy: 0.5%, B: 0.92%, Fe: 66.08%. The obtained NdFeB alloy is coarsely crushed and jet milled to produce magnetic powder with a particle size of 3-4 μm.

[0106] 2) Prepare a unilateral orientation magnetic field with an area of ​​30 mm x 30 mm, as shown in FIG8 , which is composed of two N poles and two S poles arranged in a grid pattern.

[0107] 3) Replace the unilateral orientation magnetic field in FIG1 with the grid-shaped magnetic field shown in FIG8 , load 25 g of magnetic powder into the mold cavity 3 of the pressing mold (press mold) as shown in FIG1 , and form a magnetic field of >8000 Gs at the magnetic poles of the unilateral orientation magnetic field 8 , keep the lower punch 5 fixed, and move the upper punch 1 downward to apply pressure to the magnetic powder until the magnetic powder becomes a blank.

[0108] 4) The compact is isostatically pressed at 180 MPa to further increase the density.

[0109] 5) The isostatically pressed block is vacuum sintered at 1065° C. for 3 hours, then heat treated at 900° C. for 2 hours, and then heat treated at 500° C. for 3 hours to obtain an asymmetric magnet blank.

[0110] 6) Use a surface grinder to remove the black skin and raised parts on the surface of the asymmetric suction magnet blank to form a sheet magnet.

[0111] 7) Place the sheet magnet obtained in (6) in a magnetizing fixture with four poles on each of its upper and lower surfaces. The poles of the magnetizing fixture are arranged such that if the upper pole is an N pole, the corresponding lower pole is an S pole. Similarly, the upper S pole corresponds to the lower N pole. A pulsed magnetic field is generated between the upper and lower poles using a magnetizer, completing the magnetization of the asymmetric magnet.

[0112] 8) Use a Gauss meter to detect the maximum surface magnetic field intensity of the three magnetic poles on the front and back surfaces. During molding, the maximum surface magnetic field intensity of the surface close to the unilateral orientation magnetic field is >2500Gs, and the maximum surface magnetic field intensity of the opposite surface is <600Gs. The surface magnetic field intensity of the two surfaces differs by more than 4 times.

[0113] Example 3

[0114] 1) Smelt a NdFeB alloy according to the following formula (mass percentage): PrNd: 32.5%, Dy: 0.5%, B: 0.92%, Fe: 66.08%. The obtained NdFeB alloy is coarsely crushed and jet milled to produce magnetic powder with a particle size of 3-4 μm.

[0115] 2) Prepare a set of molds as shown in FIG7 , the double-sided orientation magnetic field 4 is a single-sided orientation magnetic field with three strip-shaped magnetic poles arranged as shown in FIG2 , and the upper and lower punch areas and the orientation magnetic field area are both 30 mm x 30 mm.

[0116] 3) Load 50 g of magnetic powder into the mold cavity 3 of the pressing mold (press mold) as shown in Figure 7, form a magnetic field >8000 Gs at the magnetic pole of the orientation magnetic field 4, keep the lower punch 5 fixed, and move the upper punch 1 downward to apply pressure to the magnetic powder until the magnetic powder becomes a block.

[0117] 4) The compact is isostatically pressed at 180 MPa to further increase the density.

[0118] 5) The isostatically pressed block is vacuum sintered at 1065°C for 3 hours, then subjected to a first heat treatment at 900°C for 2 hours, and then subjected to a second heat treatment at 500°C for 3 hours to obtain an asymmetric attraction magnet blank.

[0119] 6) Use a surface grinder to remove the black skin and raised parts on the surface of the asymmetric suction magnet blank to form a sheet magnet.

[0120] 7) The sheet magnet obtained in (6) is cut into two pieces in the thickness direction by wire cutting to form two pieces of magnet.

[0121] 8) The sheet magnet obtained in (7) is magnetized according to the magnetization method of Example 1.

[0122] 9) A gauss meter is used to detect the maximum surface magnetic field intensity of the three magnetic poles on the front and back surfaces. During molding, the maximum surface magnetic field intensity of the surface in close contact with the orientation magnetic field is >2600Gs, and the maximum surface magnetic field intensity of the middle surface is <600Gs. It can be seen that the surface magnetic field intensity of the surface in close contact with the orientation magnetic field and the middle surface differs by more than 4 times.

[0123] In summary, the embodiments of the present invention provide an asymmetric attraction magnet and a preparation method thereof, and a magnet assembly which mainly adopt a special orientation pressing method to integrally form an asymmetric attraction magnet, which has high preparation efficiency and eliminates the hidden dangers such as cracking in the existing method of preparing asymmetric attraction magnets.

[0124] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Any simple modifications, equivalent changes and modifications made to the above embodiment based on the technical essence of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing an asymmetric attraction magnet, It is characterized in that It includes the following steps: Pressing step: placing magnetic powder into a pressing mold, and pressing the magnetic powder into a compact in a single-sided orientation magnetic field; wherein the single-sided orientation magnetic field means that in a mold cavity of the pressing mold, an orientation magnetic field is set only on one surface of the mold cavity; wherein the magnetic powder is magnetic powder for sintering magnets; Post-processing step: post-processing the blank to obtain an asymmetric attraction magnet.

2. The method for preparing the asymmetric attraction magnet according to claim 1, It is characterized in that The pressing die includes a die side plate, an upper punch, and a lower punch; wherein, The die cavity of the pressing die is surrounded by a die side plate, an upper punch and a lower punch; Preferably, the mold cavity has a plurality of surfaces, and the orientation magnetic field is arranged on one of the plurality of surfaces; further preferably, the mold cavity has six surfaces.

3. The method for preparing the asymmetric attraction magnet according to claim 1, It is characterized in that The number of magnetic poles in the orientation magnetic field is odd; Preferably, there is only one S pole in the orientation magnetic field or there is only one N pole in the orientation magnetic field; Preferably, there is only one S pole and two N poles in the orientation magnetic field; or there is only one N pole and two S poles in the orientation magnetic field.

4. The method for preparing the asymmetric attraction magnet according to claim 1, It is characterized in that The orientation magnetic field has at least two magnetic poles, and each magnetic pole is in a strip shape; wherein, in the orientation magnetic field, the strip-shaped N poles and the strip-shaped S poles are arranged at intervals.

5. The method for preparing the asymmetric attraction magnet according to claim 1, It is characterized in that The orientation magnetic field is a grid-shaped orientation magnetic field; wherein the grid-shaped orientation magnetic field has a plurality of magnetic poles, and the plurality of magnetic poles are arranged in a grid-shaped structure, and each magnetic pole serves as a grid unit; Preferably, all the magnetic poles in the grid-shaped orientation magnetic field are S poles; or all the magnetic poles in the grid-shaped orientation magnetic field are N poles; Preferably, the grid-shaped orientation magnetic field includes an N pole and an S pole, and the grid units of the N pole and the grid units of the S pole are arranged at intervals.

6. The method for preparing the asymmetric attraction magnet according to claim 1, It is characterized in that The orientation magnetic field includes a plurality of magnetic poles, and the plurality of magnetic poles are arranged concentrically from the inside to the outside; Preferably, the orientation magnetic field includes at least one annular N pole and at least one annular S pole, and the annular N pole and the annular S pole are arranged at intervals; Preferably, the orientation magnetic field includes at least one annular magnetic pole and one circular magnetic pole; wherein the annular magnetic pole is arranged around the circular magnetic pole; wherein the S pole and the N pole in the orientation magnetic field are arranged alternately; Preferably, the orientation magnetic field includes a plurality of annular magnetic poles which are arranged concentrically in sequence from the inside to the outside; wherein each annular magnetic pole is composed of at least one circular arc-shaped N pole and at least one circular arc-shaped S pole; wherein the N pole and S pole in the orientation magnetic field are arranged at intervals; further preferably, each annular magnetic pole is composed of two quarter-circular arc-shaped N poles and two quarter-circular arc-shaped S poles which are spliced ​​at intervals.

7. A method for preparing an asymmetric attraction magnet according to any one of claims 1 to 6, It is characterized in that The particle size of the magnetic powder is 2.0-6.0 μm; and / or Before the pressing step, the method further comprises: Steps for preparing magnetic powder: melting the raw materials into alloys according to the chemical composition of the magnetic powder; The alloy is crushed and ground into magnetic powder.

8. A method for preparing an asymmetric attraction magnet according to any one of claims 1 to 7, It is characterized in that The post-processing step comprises: Vacuum sintering and heat treatment steps: vacuum sintering and heat treatment are performed on the blank in sequence to obtain an asymmetric attraction magnet blank; Preferably, the temperature of the vacuum sintering treatment is 1000-1200° C.; further preferably, the time of the vacuum sintering treatment is 2-4 hours; Preferably, the heat treatment includes a first stage heat treatment and a second stage heat treatment; wherein the temperature of the first stage heat treatment is 850-950°C, and the temperature of the second stage heat treatment is 450-550°C; further preferably, the time of the first stage heat treatment is 2-4 hours, and the time of the second stage heat treatment is 2-4 hours; Preferably, before the vacuum sintering step, the method further comprises: Isostatic pressing step: isostatic pressing the briquettes to increase the density of the briquettes and reduce the deformation during the sintering stage; preferably, the isostatic pressing is liquid isostatic pressing or dry isostatic pressing. Static pressure treatment.

9. The method for preparing the asymmetric attraction magnet according to claim 8, It is characterized in that The post-processing step further comprises: Machining and magnetizing treatment steps: machining the asymmetric attraction magnet blank to a desired size and then magnetizing it to obtain the asymmetric attraction magnet.

10. An asymmetric attraction magnet, It is characterized in that The asymmetric attraction magnet is an integrated structure; preferably, the asymmetric attraction magnet is prepared by the preparation method of the asymmetric attraction magnet according to any one of claims 1 to 9; Preferably, the asymmetric attractive magnet has a first surface and a second surface opposite to each other; wherein the surface magnetic field strength of the first surface is more than twice the surface magnetic field strength of the second surface.

11. A method for preparing an asymmetric attraction magnet, It is characterized in that The magnetic powder is pressed into a compact, and then the compact is post-processed to obtain an asymmetric attraction magnet; wherein, In the pressing step: the magnetic powder is placed in a pressing mold, and pressed into a blank under a set double-sided orientation magnetic field; wherein the set double-sided orientation magnetic field means: in the mold cavity of the pressing mold, there are two groups of orientation magnetic fields; wherein the first group of orientation magnetic fields is arranged on the first surface of the mold cavity, and the second group of orientation magnetic fields is arranged on the second surface of the mold cavity; wherein the first surface and the second surface are arranged opposite to each other; wherein the magnetic pole in the first group of orientation magnetic fields is the first magnetic pole, and the magnetic pole in the second group of orientation magnetic fields is the second magnetic pole; wherein the number of the first magnetic pole and the second magnetic pole is the same, and they are opposite to each other one by one; wherein the magnetic pole polarity of the first magnetic pole and the second magnetic pole opposite to it is the same, both are N poles or both are S poles; wherein the magnetic powder is the magnetic powder used for sintering magnets; Among them, the orientation degree of the two surfaces of the block in contact with the orientation magnetic field poles is greater than the orientation degree at the middle position of the block; at the middle position, the block is cut into two pieces along a surface parallel to the surface where the orientation magnetic field poles are located, or cut in any step of post-processing, and finally an asymmetric suction magnet is obtained.

12. An asymmetric attraction magnet, It is characterized in that The asymmetric attraction magnet is an integrated structure; preferably, the asymmetric attraction magnet is prepared by the preparation method of the asymmetric attraction magnet according to claim 11.

13. A magnetic component, It is characterized in that The magnetic assembly comprises the asymmetric attractive magnet according to claim 10 or 12.

14. A method for preparing an asymmetric suction bonding magnet, It is characterized in that It includes the following steps: The pressing step includes placing the anisotropic bonded magnetic powder into a pressing mold, and pressing the anisotropic bonded magnetic powder into a compact in a unilateral orientation magnetic field; wherein the unilateral orientation magnetic field refers to that in a mold cavity of the pressing mold, an orientation magnetic field is set only on one surface in the mold cavity; Baking: Baking the blank to obtain an asymmetric suction bonding magnet.

15. An asymmetric suction bonding magnet, It is characterized in that The asymmetric suction bonding magnet is prepared by the preparation method of the asymmetric suction bonding magnet described in claim 14.

16. A magnetic component, It is characterized in that The magnetic assembly comprises the asymmetric attraction bonding magnet as claimed in claim 15 .

Citation Information

Patent Citations

  • Method for shifting neutral magnetic layer of permanent magnet and quasi-monopole permanent magnet

    CN114765087A

  • Full-automatic magnet integrated forming device and method using one-way movement device

    CN115780807A

  • Use of a flat, permanently magnetised device with an asymmetrical force of attraction for an intermittent connection and method of producing it

    FR2539551A1

  • Lightweight Asymmetric Magnet Arrays with Mixed-Phase Magnet Rings

    US20200176163A1

  • Rare-earth alloy powder pressing apparatus and rare-earth alloy powder pressing method

    US6352598B1