Manufacturing method for metal interconnect structure, metal interconnect structure, and semiconductor assembly
The cobalt metal layer was prepared by atomic layer deposition method, and the selective adsorption characteristics of cobalt organic compounds were used to solve the problems of insufficient controllability and quality of cobalt films in traditional technology, and achieved high proportion and high uniformity cobalt film deposition. Suitable for smaller semiconductor devices.
Patent Information
- Application Number
- PCT/CN2023/129331
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-14
AI Technical Summary
With the reduction of the key size of semiconductor devices, the controllability and thin film quality of traditional chemical vapor deposition methods are difficult to meet the needs, and cobalt atoms are prone to diffuse into the dielectric layer, resulting in device failure.
The cobalt metal layer is prepared on the metal interconnection layer by atomic layer deposition method using raw materials including cobalt organic compounds. The cobalt atoms are bonded with four nitrogen atoms in a single bond, and the nitrogen atoms are connected in pairs with organic groups. Selective Deposition on the metal interconnect layer, controlling the reaction temperature and cycle number of the deposition process, using a reducing gas environment.
The controllability of cobalt film preparation and film quality are improved, ensuring that cobalt atoms account for more than 90%, and the surface roughness is less than 2nm, meeting the needs of smaller-sized devices, and reducing the risk of cobalt atoms diffusing to the dielectric layer.
Smart Images

Figure CN2023129331_14112024_PF_FP_ABST
Abstract
Description
Preparation method of metal interconnect structure, metal interconnect structure and semiconductor component
[0001] Related applications
[0002] The present disclosed embodiments claim priority to Chinese patent application number CN202310516214.3, filed on May 9, 2023, entitled “Method for preparing metal interconnection structure, metal interconnection structure and semiconductor component,” the entire text of which is hereby incorporated by reference. Technical Field
[0003] The present disclosure relates to the field of metal interconnect technology, and in particular to a method for preparing a metal interconnect structure, a metal interconnect structure, and a semiconductor component. Background Art
[0004] Metal interconnects are a common structure in semiconductor devices. They typically consist of a dielectric layer and interconnect lines separated by the dielectric layer. Interconnect lines are typically used to electrically connect multiple devices. To improve their conductivity, they are typically made of metal, such as copper. Metal atoms easily diffuse into the dielectric layer, potentially causing device failure. Therefore, metal interconnects often incorporate a barrier layer between the dielectric layer and the interconnect lines.
[0005] Currently, chemical vapor deposition (CVD) is commonly used to prepare cobalt films as barrier materials. However, as integrated circuit manufacturing processes continue to advance, the critical dimensions of semiconductor devices are shrinking, and the controllability and film quality of cobalt film preparation are gradually failing to meet the needs of semiconductor devices.
[0006] Summary of the Invention
[0007] According to some embodiments of the present disclosure, a method for preparing a metal interconnect structure is provided, which includes the following steps:
[0008] providing a dielectric layer having interconnect grooves therein;
[0009] preparing a metal interconnection layer in the interconnection groove; and,
[0010] A cobalt metal layer is prepared on the metal interconnect layer by atomic layer deposition using raw materials including a cobalt organic compound. In the cobalt organic compound, a cobalt atom is bonded to four nitrogen atoms by a single bond, the four nitrogen atoms form pairs, and each pair of nitrogen atoms is connected by an organic group.
[0011] In some embodiments of the present disclosure, the cobalt organic compound has a structure as shown in formula (1):
[0012] wherein R1, R2, R3 and R4 are each independently selected from substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, or substituted or unsubstituted C3-C20 cycloalkyl;
[0013] L1 and L2 are each independently selected from substituted or unsubstituted C1-C20 alkylene, substituted or unsubstituted C2-C20 alkenylene, and substituted or unsubstituted C2-C20 alkynylene;
[0014] When the groups of R1, R2, R3, R4, L1 and L2 are substituted, the substituents include R5, and each occurrence of R5 is independently selected from an alkyl group, a halogen atom, a C1-C10 alkoxy group, a C1-C10 haloalkyl group, a C1-C10 haloalkoxy group or a C6-C20 aryl group.
[0015] In some embodiments of the present disclosure, R1, R2, R3 and R4 are each independently selected from n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl.
[0016] In some embodiments of the present disclosure, L1 and L2 are each independently selected from methylene, 1,2-ethylene, 1,1-ethylene, 1,2-vinylene, or ethynyl.
[0017] In some embodiments of the present disclosure, R1 and R2 are the same group.
[0018] In some embodiments of the present disclosure, R3 and R4 are the same group.
[0019] In some embodiments of the present disclosure, L1 and L2 are the same group.
[0020] In some embodiments of the present disclosure, the cobalt organic compound is selected from one of the following structures:
[0021] In some embodiments of the present disclosure, in the step of preparing the cobalt metal layer, the raw material further includes a reaction material capable of reacting with the cobalt organic compound, and the reaction material includes one or more of tert-butylamine and diethylamine.
[0022] In some embodiments of the present disclosure, during the deposition of the cobalt metal layer, the reaction temperature of the deposition process is controlled to be 100° C. to 400° C.
[0023] In some embodiments of the present disclosure, the process of depositing a cobalt metal layer includes one or more deposition cycles, each deposition cycle including introducing a cobalt organic compound, purging the cobalt organic compound, introducing a reaction material, and purging the reaction material, wherein the duration of introducing the cobalt organic compound is 1s to 30s, the duration of purging the cobalt organic compound is 1s to 30s, the duration of introducing the reaction material is 1s to 30s, and the duration of purging the reaction material is 1s to 30s.
[0024] In some embodiments of the present disclosure, during the deposition of the cobalt metal layer, the number of deposition cycles is controlled to be ≤300.
[0025] In some embodiments of the present disclosure, the process of depositing the cobalt metal layer is performed in a reducing gas atmosphere.
[0026] In some embodiments of the present disclosure, after depositing the cobalt metal layer, the method further includes treating the cobalt metal layer with a reducing gas or plasma.
[0027] In some embodiments of the present disclosure, the material of the dielectric layer is selected from one or more of silicon dioxide, silicon-based polymer materials, and carbon-doped silicon oxide.
[0028] In some embodiments of the present disclosure, the material of the metal interconnection layer is selected from one or more of platinum, cobalt, copper and ruthenium.
[0029] In some embodiments of the present disclosure, before forming the metal interconnection layer in the interconnection groove, the method further includes:
[0030] preparing a barrier layer covering the walls of the interconnected grooves;
[0031] A liner layer is prepared on the barrier layer, and the metal interconnection layer is prepared on the liner layer.
[0032] Furthermore, the present disclosure also provides a metal interconnection structure, which includes: a dielectric layer, a metal interconnection layer and a cobalt metal layer; the dielectric layer has an interconnection groove, the metal interconnection layer is located in the interconnection groove, the cobalt metal layer is arranged on the metal interconnection layer, and the cobalt metal layer is prepared on the metal interconnection layer by atomic layer deposition.
[0033] In some embodiments of the present disclosure, in the step of preparing the cobalt metal layer, the raw material further includes a reaction material capable of reacting with the cobalt organic compound, and the reaction material includes one or more of tert-butylamine and diethylamine.
[0034] In some embodiments of the present disclosure, in the raw material, during the process of depositing the cobalt metal layer, the reaction temperature of the deposition process is controlled to be 100° C. to 400° C.
[0035] In some embodiments of the present disclosure, the thickness of the cobalt metal layer is ≤30 nm, and the surface roughness of the cobalt metal layer is ≤2 nm.
[0036] In some embodiments of the present disclosure, the proportion of cobalt atoms in the cobalt metal layer is ≥90%.
[0037] In some embodiments of the present disclosure, the material of the dielectric layer is selected from one or more of silicon dioxide, silicon-based polymer materials, and carbon-doped silicon oxide.
[0038] In some embodiments of the present disclosure, the material of the metal interconnection layer is selected from one or more of platinum, cobalt, copper and ruthenium.
[0039] In some embodiments of the present disclosure, the metal interconnect structure further includes a barrier layer, a liner layer, and a metal seed layer arranged between the metal interconnect layer and the dielectric layer, and the barrier layer, the liner layer, and the metal seed layer are stacked in sequence from the dielectric layer to the metal interconnect layer.
[0040] Furthermore, the present disclosure also provides a semiconductor component, which includes the metal interconnect structure as described in any of the above embodiments and a plurality of semiconductor devices, wherein the plurality of semiconductor devices are electrically connected through the metal interconnect structure.
[0041] In some embodiments of the present disclosure, the semiconductor component is a memory. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, without paying any creative work, they can also obtain drawings of other embodiments based on these drawings.
[0043] FIG1 is a schematic diagram of the steps of a method for preparing a metal interconnect structure disclosed herein;
[0044] FIG2 is a schematic structural diagram of a dielectric layer provided by the present disclosure;
[0045] FIG3 is a schematic diagram of a structure for preparing a barrier layer based on the structure shown in FIG2 ;
[0046] FIG4 is a schematic diagram of a structure for preparing a liner layer based on the structure shown in FIG3 ;
[0047] FIG5 is a schematic diagram of a structure for preparing a metal seed layer and a metal interconnection layer based on the structure shown in FIG4 ;
[0048] FIG6 is a schematic diagram of a structure after planarization processing is performed on the structure shown in FIG5 ;
[0049] FIG7 is a schematic diagram of a structure for preparing a cobalt metal layer based on the structure shown in FIG6 ;
[0050] The reference numerals and their meanings are as follows:
[0051] 110 , dielectric layer; 111 , interconnection groove; 120 , barrier layer; 130 , liner layer; 140 , metal seed layer; 150 , metal interconnection layer; 160 , cobalt metal layer. DETAILED DESCRIPTION
[0052] To facilitate understanding of the present disclosure, a more comprehensive description of the present disclosure will be provided below with reference to the accompanying drawings. The drawings illustrate preferred embodiments of the present disclosure. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the present disclosure.
[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this disclosure pertains. The terms used herein in the specification of this disclosure are for the purpose of describing specific embodiments only and are not intended to limit this disclosure. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0054] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," etc., may be used herein for convenience of description to describe the relationship of one element or feature shown in the figures to other elements or features. It should be understood that the spatially relative terms are intended to include different orientations of the device in use and operation in addition to the orientations shown in the figures. For example, if the device in the drawings is flipped, then the elements or features described as "under" or "beneath" or "beneath" the other elements will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both the upper and lower orientations. The device may be oriented otherwise (rotated 90 degrees or in other orientations) and the spatial descriptors used herein are interpreted accordingly.
[0055] The purpose of the terms used herein is only to describe specific embodiments and is not intended to limit the present disclosure. When used herein, the singular forms "a", "an", and "the" are intended to include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "comprising" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0056] In this article, the technical solutions described in an open manner may include open technical solutions that contain the listed technical features, or closed technical solutions composed of the listed features.
[0057] As used herein, alkyl refers to a saturated hydrocarbon group containing primary (normal) carbon atoms, secondary carbon atoms, tertiary carbon atoms, quaternary carbon atoms, or a combination thereof, with one bonding site. An alkyl group can be considered to be a hydrocarbon group with one hydrogen atom removed from the corresponding alkane, resulting in a corresponding bonding site. Phrases containing this term, such as "C1-C20 alkyl" are phrases where the alkyl portion contains 1 to 20 carbon atoms. Suitable examples include, but are not limited to, methyl (-CH3), ethyl (-CH2CH3), 1-propyl (n-propyl, -CH2CH2CH3), 2-propyl (isopropyl, -CH(CH3)2), 1-butyl (n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (-CH2CH(CH3)2), 2-butyl (-CH(CH3)CH2CH3), 1,1-dimethylethyl (tert-butyl, -C(CH3)3 ), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl (-CH2CH2CH(CH3)2), 2-methyl-1-butyl (-C H2CH(CH3)CH2CH3), 1-hexyl (n-hexyl, -CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH(CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 and octyl (-(CH2)7CH3).
[0058] As used herein, an alkylene group refers to a saturated hydrocarbon group with two bonding sites. An alkylene group can be considered a hydrocarbon group with two hydrogen atoms removed from the corresponding alkane, resulting in two corresponding bonding sites. Phrases containing this term, such as "C1-C20 alkylene," mean that the alkylene portion contains 1 to 20 carbon atoms. An alkylene group can be a group with one hydrogen atom removed from the above alkyl group, resulting in a bonding site at the corresponding position. Suitable examples include, but are not limited to, methylene (-CH2-), ethylene (-CH(CH3)-), and 1,2-ethylene (-CH2CH2-).
[0059] As used herein, an alkenyl group may also be referred to as an alkene group, and refers to an unsaturated hydrocarbon group having one or more carbon-carbon double bonds and one bonding site. An alkenyl group can be considered to be a hydrocarbon group with one hydrogen atom removed from the corresponding alkene, resulting in a corresponding bonding site. Terms containing this phrase, such as "C1-C20 alkenyl" are hydrocarbon groups with 1 to 20 carbon atoms in the alkenyl portion. An alkenyl group can be a hydrocarbon group with two hydrogen atoms removed from the above-mentioned alkyl group, resulting in a double bond between the two carbon atoms. Suitable examples include, but are not limited to, vinyl (-CH=CH2) and allyl (-CH2CH=CH2).
[0060] As used herein, an alkenylene group refers to an unsaturated hydrocarbon group having one or more carbon-carbon double bonds and two bonding sites. An alkenylene group can be considered to be a hydrocarbon group in which two hydrogen atoms are removed from the corresponding alkene, resulting in two corresponding bonding sites. Phrases containing this term, such as "C1 to C20 alkenylene" are groups in which the alkenylene portion contains 1 to 20 carbon atoms. An alkenylene group can be a group in which one hydrogen atom is removed from the above alkenyl group and a bonding site is formed at the corresponding position. Suitable examples include, but are not limited to, 1,2-vinylene (-CH=CH-) and 1-methyl-1,2-vinylene (-C(CH3)=CH-).
[0061] As used herein, an alkynyl group may also be referred to as an alkyne group, which refers to an unsaturated hydrocarbon group having one or more carbon-carbon triple bonds and one bonding site. An alkynyl group can be considered to be a hydrocarbon group with one hydrogen atom removed from the corresponding alkyne, resulting in a corresponding bonding site. Terms containing this phrase, such as "C1-C20 alkynyl" refer to an alkynyl group having 1 to 20 carbon atoms. An alkynyl group can be a hydrocarbon group with four hydrogen atoms removed from the above-mentioned alkyl group, resulting in a triple bond between two carbon atoms. Suitable examples include, but are not limited to, ethynyl (-C≡CH) and propargyl (-CH2C≡CH).
[0062] As used herein, an alkynylene group refers to an unsaturated hydrocarbon group having one or more carbon-carbon triple bonds and two bonding sites. An alkynylene group can be considered to be a hydrocarbon group in which two hydrogen atoms are removed from the corresponding alkyne, resulting in two corresponding bonding sites. Phrases containing this term, such as "C1-C20 alkynylene" are groups in which the alkynylene moiety contains 1 to 20 carbon atoms. An alkynylene group can be a group in which one hydrogen atom is removed from the above-mentioned alkynyl group and a bonding site is formed at the corresponding position. Suitable examples include, but are not limited to, ethynylene (-C≡C-) and propargylene (-CH2C≡C-).
[0063] As used herein, "alkoxy" refers to an alkyl group connected to an oxygen atom, i.e., an alkyl group as defined above is connected to a parent nucleus via an oxygen atom. "Haloalkoxy" refers to a structure in which the hydrogen atom of the alkyl portion of an alkoxy group is replaced by a halogen atom.
[0064] Herein, the "halogen atom" refers to F, Cl, Br or I.
[0065] The present disclosure provides a method for preparing a metal interconnect structure, which comprises the following steps:
[0066] providing a dielectric layer having interconnect grooves therein;
[0067] preparing a metal interconnect layer in the interconnect groove; and,
[0068] A cobalt metal layer is prepared on a metal interconnect layer by atomic layer deposition using raw materials including a cobalt organic compound. In the cobalt organic compound, a cobalt atom is bonded to four nitrogen atoms by a single bond, the four nitrogen atoms form pairs, and each pair of nitrogen atoms is connected by an organic group.
[0069] A metal interconnect structure refers to a structure that connects multiple devices simultaneously and is used to conduct electricity. In current processes, a metal interconnect structure typically includes a dielectric layer and a metal interconnect layer formed within the dielectric layer. The metal interconnect structure also includes a cobalt metal layer located above the metal interconnect layer, and a cobalt precursor can be used to form this cobalt metal layer.
[0070] For the preparation of cobalt metal layers, it is required that the cobalt metal layer can be selectively deposited only on the metal interconnect layer, and basically not deposited on the dielectric layer. However, due to the limitations of specific raw materials and actual preparation processes, traditional technologies can only achieve selective preparation through chemical vapor deposition, and have not been able to achieve selective preparation of cobalt through atomic layer deposition. However, as the critical dimensions of devices continue to shrink, problems such as poor controllability of chemical vapor deposition and poor quality of cobalt films have become increasingly prominent.
[0071] It can be understood that the material of the dielectric layer should be an insulating material, usually a non-metallic insulating material.
[0072] Among them, the cobalt organic compound with the above structure can be selectively adsorbed on substrates of different materials. Specifically, the cobalt organic compound can selectively adsorb on metal materials including copper, ruthenium and platinum, but is difficult to adsorb on non-metallic dielectric materials including silicon, silicon dioxide and silicon nitride. The preparation process of the atomic layer deposition method requires the precursor material to be adsorbed on the deposition substrate first. Therefore, using this type of cobalt organic compound as a precursor can enable the cobalt film to be selectively formed on the metal interconnect layer, while the dielectric layer basically has no cobalt atoms or it is difficult to form a cobalt film.
[0073] In the preparation method of the metal interconnect structure provided by the present disclosure, a raw material including a cobalt organic compound is used to prepare a cobalt metal layer on the metal interconnect layer by atomic layer deposition. In the cobalt organic compound, the cobalt atom is bonded to four nitrogen atoms with a single bond, and the four nitrogen atoms are paired in pairs, and each pair of nitrogen atoms is connected by an organic group. The cobalt organic compound having the above structure can be used as a reaction raw material for the atomic layer deposition method, and during the atomic layer deposition process, the cobalt organic compound can be selectively adsorbed on the metal interconnect layer and basically not adsorbed on the dielectric layer, so that the formed cobalt film is also selectively formed on the metal interconnect layer. Compared with traditional technology, preparing a cobalt film by atomic layer deposition can effectively improve the controllability of the preparation of the cobalt film and the film quality.
[0074] It is understood that the controllability of the cobalt film preparation can include parameters such as the minimum thickness of the cobalt film, surface roughness, and the proportion of cobalt atoms in the cobalt metal layer. Generally, the higher the controllability of the cobalt film preparation, the more likely it is to produce a thinner cobalt film with lower surface roughness and / or a higher proportion of cobalt atoms.
[0075] It is understood that in the process of preparing a cobalt metal film using the cobalt precursor, a reaction material that can react with the cobalt precursor is usually required.
[0076] Furthermore, in some examples of this embodiment, the cobalt organic compound has a structure as shown in formula (1):
[0077] wherein R1, R2, R3 and R4 are each independently selected from substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, or substituted or unsubstituted C3-C20 cycloalkyl;
[0078] L1 and L2 are each independently selected from substituted or unsubstituted C1-C20 alkylene, substituted or unsubstituted C2-C20 alkenylene, and substituted or unsubstituted C2-C20 alkynylene;
[0079] When the groups of R1, R2, R3, R4, L1 and L2 are substituted, the substituents include R5, and each occurrence of R5 is independently selected from an alkyl group, a halogen atom, a C1-C10 alkoxy group, a C1-C10 haloalkyl group, a C1-C10 haloalkoxy group or a C6-C20 aryl group.
[0080] It can be understood that in the cobalt organic compound provided by formula (1), the cobalt atom is bonded to four nitrogen atoms by single bonds, and the four nitrogen atoms are paired, with the two nitrogen atoms in a pair being connected by an organic chain segment, and each nitrogen atom may also be connected to a substituent.
[0081] In some examples of this embodiment, R1, R2, R3, and R4 can each independently be selected from a C1-C10 alkyl group, a C2-C10 alkenyl group, or a C2-C10 alkynyl group. Furthermore, R1, R2, R3, and R4 can each independently be selected from a C1-C5 alkyl group, a C2-C5 alkenyl group, or a C2-C5 alkynyl group. Selecting a group with fewer carbon atoms helps the cobalt organic compound to be more easily vaporized and adsorbed onto the metal interconnect layer during the preparation process, thereby improving the uniformity and manufacturing efficiency of the cobalt metal layer.
[0082] In some examples of this embodiment, R1, R2, R3, and R4 are each independently selected from a C3-C4 alkyl group, such as n-propyl, isopropyl, n-butyl, isobutyl, or tert-butyl. The structural formula of n-propyl is -CH2CH2CH3, the structural formula of isopropyl is -CH(CH3)2, the structural formula of n-butyl is -CH2CH2CH2CH3, the structural formula of isobutyl is -CH(CH3)CH2CH3, and the structural formula of tert-butyl is -C(CH3)3.
[0083] In some examples of this embodiment, L1 and L2 are each independently selected from a C1-C10 alkylene group, a C2-C10 alkenylene group, or a C2-C10 alkynylene group. Furthermore, R1, R2, R3, and R4 can each independently be selected from a C1-C5 alkylene group, a C2-C5 alkenylene group, or a C2-C5 alkynylene group. Selecting shorter chain segments helps increase the reactivity of the cobalt organic compound, improving the uniformity and manufacturing efficiency of the cobalt metal layer.
[0084] In some examples of this embodiment, L1 and L2 are each independently selected from a C1-C2 alkylene group, a C2 alkenylene group, and a C2 alkynylene group. For example, L1 and L2 are each independently selected from a methylene group (-CH2-), a 1,2-ethylene group (-CH2CH2-), a 1,1-ethylene group (-CH(CH3)-), a 1,2-vinylene group (-CH=CH-), or an ethynyl group (-C≡C-).
[0085] The selection of the above groups can make the cobalt precursor have higher reactivity and make the reaction by-products easier to remove.
[0086] In some examples of this embodiment, R1, R2, R3 and R4 are selected from the same group, for example, R1, R2, R3 and R4 are all isopropyl or tert-butyl.
[0087] In some examples of this embodiment, L1 and L2 are also selected from the same group. For example, L1 and L2 may be 1,1-ethylene, 1,2-ethylene, 1,2-vinylene or ethynylene.
[0088] In some instances of this embodiment, the general formula (1) is selected from one of the following structures:
[0089] Among them, the cobalt precursor shown in the above structural formula is particularly suitable for atomic layer deposition. It can deposit a cobalt film with a cobalt atomic content of more than 90% on metal substrates such as platinum, copper and ruthenium, but will not deposit on substrates such as silicon and silicon dioxide.
[0090] Among them, the structural formula For example, in the structural formula, L1 and L2 are both 1,2-vinylene (-CH=CH-). However, due to the relatively symmetrical structure, the two pairs of nitrogen atoms and the connected chain segments can be conjugated and generate delocalized electron pairs, making the structure in the above formula more stable.
[0091] In some examples of this embodiment, the process of preparing the metal interconnect structure includes the following steps:
[0092] providing a dielectric layer having interconnect grooves therein;
[0093] preparing a metal interconnect layer in the interconnect groove; and,
[0094] A cobalt metal layer is prepared on the metal interconnection layer. The step of preparing the cobalt metal layer comprises: using a raw material including the cobalt precursor to deposit the cobalt metal layer on the metal interconnection layer by atomic layer deposition.
[0095] The cobalt precursor provided by the present disclosure can serve as the cobalt raw material required for atomic layer deposition (ALD) and can be selectively deposited on a metal substrate rather than on a dielectric layer. Compared to traditional chemical vapor deposition (CVD) methods, the use of this cobalt precursor via ALD allows for the layer-by-layer preparation of cobalt metal layers, improving the controllability of the cobalt metal layer in terms of film thickness and film uniformity. This also facilitates the production of higher-quality cobalt metal layers, meeting the needs of smaller devices.
[0096] To facilitate understanding of the application of the above cobalt precursor in preparing a metal interconnect structure, the present disclosure also provides a schematic diagram of the steps of a method for preparing a metal interconnect structure as shown in Figure 1. As shown in Figure 1, the method for preparing a metal interconnect structure includes steps S1 to S5.
[0097] Step S1: providing a dielectric layer.
[0098] Fig. 2 is a schematic structural diagram of a dielectric layer 110 provided by the present disclosure. Referring to Fig. 2 , the dielectric layer 110 is provided with interconnection grooves 111 .
[0099] It is understood that the interconnection groove 111 is used to be filled with the subsequently prepared metal interconnection layer 150. The interconnection groove 111 shown in Figure 2 is in a multi-layered stepped shape, but in the actual preparation process, the interconnection groove 111 can also be prepared in other shapes, for example, the cross-section of the hole can be trapezoidal, rectangular, or irregular, as long as it can be filled with the metal interconnection layer 150.
[0100] In some examples of this embodiment, the material of dielectric layer 110 may be a low-k material (also known as a low-K material). For example, the dielectric constant of the material of dielectric layer 110 is ≤3.9. Furthermore, the dielectric constant of the material of dielectric layer 110 is ≤2.8. By selecting a material with a lower dielectric constant for dielectric layer 110, parasitic capacitance between metal interconnect layers 150 can be reduced.
[0101] In some examples of this embodiment, the material of dielectric layer 110 may include a silicon compound. For example, the material of dielectric layer 110 may be selected from one or more of silicon dioxide, a silicon-based polymer material, carbon-doped silicon oxide, and a silicon-based aerogel. The silicon-based polymer material may be, for example, one or more of SiLK, HSQ (hydrogen silsesquioxane), and MSQ (methylsilsesquioxane). The carbon-doped silicon oxide may be, for example, one or more of Black Diamond, Coral, and Aurora.
[0102] In this embodiment, the material of the dielectric layer 110 includes silicon dioxide.
[0103] Step S2: preparing a barrier layer and a liner layer in the interconnection groove.
[0104] Figure 3 is a schematic diagram showing a structure in which a barrier layer 120 is prepared based on the structure shown in Figure 2. Referring to Figure 3, the barrier layer 120 is prepared in the interconnection groove 111 and covers the groove wall of the interconnection groove 111.
[0105] The barrier layer 120 is used to separate the dielectric layer 110 and the subsequently prepared metal interconnection layer 150 , and to prevent metal atoms in the metal interconnection layer 150 from diffusing into the dielectric layer.
[0106] In some examples of this embodiment, the material of barrier layer 120 may include one or more of tantalum, tantalum nitride, titanium, titanium nitride, and titanium silicon nitride. In this embodiment, the material of barrier layer 120 may include tantalum nitride.
[0107] In addition, in some examples of this embodiment, the barrier layer 120 may also be a composite layer formed of multiple materials. For example, the barrier layer 120 may be a composite layer formed by stacking a tantalum layer and a tantalum nitride layer.
[0108] In some examples of this embodiment, the method of preparing the barrier layer 120 may be a chemical vapor deposition method or an atomic layer deposition method.
[0109] 3 , in some examples of this embodiment, when preparing the barrier layer 120 , the material of the barrier layer 120 may also be deposited on the surface of the dielectric layer 110 outside the interconnection groove 111 .
[0110] The thickness of the barrier layer 120 can be limited according to actual needs. In some examples of this embodiment, the thickness of the barrier layer 120 can be 0.5 nm to 10 nm. Furthermore, the thickness of the barrier layer 120 can be 0.5 nm to 5 nm. Furthermore, the thickness of the barrier layer 120 can be 0.5 nm to 3 nm.
[0111] FIG4 is a schematic diagram showing a structure of preparing a liner layer 130 based on the structure shown in FIG3 .
[0112] It is understood that the liner layer 130 can also be used to separate the dielectric and the subsequently prepared metal interconnect layer 150. In addition, the liner layer 130 can also serve as a nucleation substrate for the subsequently prepared seed layer, thereby improving the uniformity and gap filling capability of the subsequently prepared layer.
[0113] In some examples of this embodiment, the material of the liner layer 130 may be one or more of cobalt and ruthenium.
[0114] In some examples of this embodiment, the method of preparing the liner layer 130 may be a chemical vapor deposition method or an atomic layer deposition method.
[0115] In some examples of this embodiment, the thickness of the liner layer 130 may be 1 nm to 10 nm. Further, the thickness of the liner layer 130 may be 1 nm to 5 nm. Further, the thickness of the liner layer 130 may be 1 nm to 3 nm.
[0116] In some examples of this embodiment, the material of the liner layer 130 may include cobalt. It is understood that by preparing cobalt by atomic layer deposition, the controllability of the preparation of the liner layer 130 can be improved, so as to obtain a thinner and more uniform liner layer 130.
[0117] In some examples of this embodiment, when the material of the liner layer 130 is cobalt, the thickness of the liner layer 130 can be controlled to be 1 nm to 10 nm.
[0118] In some examples of this embodiment, before preparing the liner layer 130 , plasma bombardment of the surface of the barrier layer 120 may be used to clean the surface of the barrier layer 120 , thereby reducing the difficulty of preparing the liner layer 130 .
[0119] In some examples of this embodiment, when preparing the liner layer 130 , the material of the liner layer 130 may also be deposited outside the interconnection groove 111 .
[0120] Step S3: preparing a metal interconnection layer in the interconnection groove.
[0121] FIG5 is a schematic diagram showing a structure in which a metal seed layer 140 and a metal interconnect layer 150 are prepared based on the structure shown in FIG4 . Referring to FIG5 , the metal seed layer 140 is stacked on the liner layer 130 , and the metal interconnect layer 150 is prepared in the interconnect groove 111 and stacked on the liner layer 130 .
[0122] In some examples of this embodiment, the metal interconnection layer 150 may be prepared by electroplating, which enables the metal interconnection layer 150 to be filled in the interconnection groove 111 as evenly and fully as possible.
[0123] In some examples of this embodiment, before forming the metal interconnection layer 150, a step of forming a metal seed layer 140 in the interconnection groove 111 is also included. The metal seed layer 140 can be used as a seed when forming the metal interconnection layer 150, so that the metal interconnection layer 150 can be more fully filled in the interconnection groove 111.
[0124] In some examples of this embodiment, the metal seed layer 140 may be prepared by a physical vapor deposition method.
[0125] In some examples of this embodiment, the material of the metal seed layer 140 is the same as the material of the metal interconnection layer 150 .
[0126] In some examples of this embodiment, the material of the metal interconnection layer 150 may be selected from one or more of platinum, cobalt, copper, and ruthenium. In this embodiment, the material of the metal interconnection layer 150 is copper.
[0127] It is understood that, during the actual fabrication process, the materials of the metal seed layer 140 and the metal interconnection layer 150 may also be deposited outside the interconnection groove 111. Therefore, in some examples of this embodiment, after the metal interconnection layer 150 is formed, a step of planarizing the dielectric layer 110 and the structure located on the dielectric layer 110 is also included to remove the materials of the metal interconnection layer 150, the metal seed layer 140, the liner layer 130, and the barrier layer 120 located outside the interconnection groove 111.
[0128] FIG6 illustrates a schematic diagram of the structure shown in FIG5 after planarization. Referring to FIG6 , in some examples of this embodiment, the top surface of metal interconnect layer 150 is flush with the notch of dielectric layer 110. Furthermore, the top surfaces of metal seed layer 140, liner layer 130, and barrier layer 120 are also flush with the notch of dielectric layer 110.
[0129] In some examples of this embodiment, the planarization process may be performed using chemical mechanical polishing (CMP). Using CMP to process the dielectric layer 110 and the layer structures on its surface can make the processed dielectric layer 110 and the metal interconnect layer 150 as flat as possible, facilitating the subsequent preparation of the cobalt metal layer 160.
[0130] Step S4: preparing a cobalt metal layer on the metal interconnection layer.
[0131] Figure 7 shows a schematic diagram of a structure in which a cobalt metal layer 160 is prepared based on the structure shown in Figure 6. As shown in Figure 7, the cobalt metal layer 160 is stacked on the metal interconnect layer 150, and the dielectric layer does not have the cobalt metal layer 160.
[0132] In this embodiment, the cobalt metal layer 160 can be prepared by atomic layer deposition using a cobalt organic compound. The structure of the cobalt organic compound has the following general formula:
[0133] wherein R1, R2, R3 and R4 are each independently selected from C1-C20 alkyl substituted or unsubstituted by R5, C2-C20 alkenyl substituted or unsubstituted by R5, C2-C20 alkynyl substituted or unsubstituted by R5, and C3-C20 cycloalkyl substituted or unsubstituted by R5;
[0134] L1 and L2 are each independently selected from R5 substituted or unsubstituted C1-C20 alkylene, R5 substituted or unsubstituted C2-C20 alkenylene, R5 substituted or unsubstituted C2-C20 alkynylene, and R5 substituted or unsubstituted C3-C20 cycloalkylene;
[0135] Each occurrence of R5 is independently selected from a halogen atom, a C1-C10 alkoxy group, a C1-C10 haloalkyl group, a C1-C10 haloalkoxy group or a C6-C20 aryl group.
[0136] It can be understood that in the cobalt organic compound, the cobalt atom is bonded to four nitrogen atoms via single bonds, and the four nitrogen atoms form pairs, with the two nitrogen atoms in a pair being connected by an organic chain segment, and each nitrogen atom may further be connected to a substituent.
[0137] The cobalt organic compound shown in formula (1) can be used as a cobalt precursor for preparing cobalt metal. For example, the cobalt organic compound can be used as a raw material in an atomic layer deposition method, and cobalt metal is generated during the deposition process. In particular, when the cobalt organic compound generates cobalt metal in a deposition reaction, the cobalt atoms have a high selectivity for the deposition substrate, and the cobalt atoms will be deposited on the surface of metal materials such as copper, platinum and ruthenium, but will not be deposited on the surface of some non-metallic dielectric materials such as silicon and silicon dioxide. Therefore, the present disclosure contemplates the application of the cobalt precursor in the preparation of metal interconnect structures. Cobalt metal is usually used as a barrier material to prevent the diffusion of metal atoms in metal interconnect structures. By applying the cobalt organic compound to the preparation of metal interconnect structures, the selectivity of the cobalt organic compound for the deposition substrate can be utilized to improve the controllability of the preparation of the cobalt metal layer in the metal interconnect structure.
[0138] In some examples of this embodiment, R1, R2, R3 and R4 are selected from the same group, for example, R1, R2, R3 and R4 are all isopropyl or tert-butyl.
[0139] In some examples of this embodiment, L1 and L2 are also selected from the same group. For example, L1 and L2 may be 1,1-ethylene, 1,2-ethylene, 1,2-vinylene or ethynylene.
[0140] In some instances of this embodiment, the cobalt precursor is selected from one of the following structures:
[0141] The cobalt-organic compound having the above-described structure is particularly suitable for atomic layer deposition. It can be selectively deposited on the metal interconnect layer 150 to form a cobalt metal layer 160 containing over 90% cobalt atoms, while no deposition occurs on the dielectric layer 110. Furthermore, the use of this cobalt-organic compound via atomic layer deposition enables the layer-by-layer deposition of the cobalt metal layer 160, improving the controllability of the cobalt metal layer 160 in terms of film thickness and film uniformity. This also facilitates obtaining a higher-quality cobalt metal layer 160, meeting the needs of smaller devices.
[0142] It is understood that atomic layer deposition is a method of forming a deposited film by alternately passing a gaseous precursor pulse into a reactor and chemically adsorbing and reacting on a deposition substrate. Therefore, the atomic layer deposition method requires the use of raw materials, which should include the above-mentioned cobalt organic compound. It is understood that in the process of preparing a cobalt metal film using the cobalt organic compound, a reactant that can react with the cobalt precursor is usually also required. Although the cobalt organic compound can be selectively adsorbed on the metal interconnect layer, if a cobalt film with a more uniform, lower roughness and a higher proportion of cobalt atoms is to be prepared, it is also necessary to ensure the uniform deposition of cobalt atoms in the process of forming cobalt atoms from the cobalt organic compound, otherwise the quality of the cobalt film will still be difficult to improve.
[0143] In some examples of this embodiment, during the preparation of the cobalt metal layer 160, the raw materials further include a reactant capable of reacting with the cobalt organic compound, wherein the reactant includes one or more of tert-butylamine (C(CH3)3NH2) and diethylamine ((CH3CH2)2NH). The reaction of the reactant with the cobalt organic compound facilitates uniform deposition of cobalt atoms, thereby obtaining a cobalt film with a lower thickness, lower surface roughness, and a higher proportion of cobalt atoms.
[0144] In some examples of this embodiment, the process of depositing the cobalt metal layer includes one or more deposition cycles, each deposition cycle including introducing a cobalt organic compound, purging the cobalt organic compound, introducing a reaction material, and purging the reaction material, wherein the duration of introducing the cobalt organic compound is 1 second to 30 seconds, the duration of purging the cobalt organic compound is 1 second to 30 seconds, the duration of introducing the reaction material is 1 second to 30 seconds, and the duration of purging the reaction material is 1 second to 30 seconds. A protective gas may be used to purge the cobalt organic compound and the reaction material, and the protective gas may be one or more of nitrogen, helium, neon, and argon.
[0145] It can be understood that during a deposition cycle, the purpose of introducing the cobalt-organic compound is to cause the cobalt-organic compound to adsorb on the surface of the substrate to be coated, and the purpose of purging the cobalt-organic compound is to remove excess cobalt-organic compound from the reaction chamber, retaining only the cobalt-organic compound adsorbed on the surface of the substrate to be coated. Controlling the duration of introducing the cobalt-organic compound and the duration of purging the cobalt-organic compound can ensure that the cobalt-organic compound fully and selectively adheres to the metal interconnect layer 150. The purpose of introducing the reactant is to react with the adhered cobalt-organic compound to generate cobalt metal atoms, while the purpose of purging the reactant is to clean the reaction chamber and prepare for the next deposition cycle. Controlling the duration of introducing the reactant allows the cobalt-organic compound to fully react to form a cobalt metal layer 160 that completely covers the metal interconnect layer 150.
[0146] In some examples of this embodiment, during the deposition of the cobalt metal layer 160, the number of deposition cycles is ≤300. If the number of deposition cycles is too high, atoms of the already prepared cobalt metal layer 160 may gradually diffuse to the surface of the dielectric layer 110, and the surface state of the dielectric layer 110 may also change, thereby causing a decrease in the selectivity of cobalt during the deposition process. Therefore, by controlling the number of deposition cycles to ≤300, it is possible to minimize the deposition of the cobalt metal layer 160 on the surface of the dielectric layer 110.
[0147] In some examples of this embodiment, during the deposition of the cobalt metal layer 160, the number of deposition cycles can be controlled to be ≤ 300. Furthermore, the number of deposition cycles can be controlled to be between 10 and 300. For example, the number of deposition cycles can be 10, 30, 50, 100, 150, 200, 250, or 300. The number of deposition cycles can also be within a range between the above numbers.
[0148] In addition, it can be understood that by selecting a silicon-based material as the material of the dielectric layer 110 , it is also beneficial to avoid the deposition of cobalt atoms on the dielectric layer 110 during the preparation process of the cobalt metal layer 160 .
[0149] In some examples of this embodiment, during the deposition of the cobalt metal layer 160 , the reaction temperature of the deposition process is controlled to be 100° C. to 400° C. By controlling the appropriate reaction temperature, the cobalt metal layer 160 can be deposited as uniformly as possible, and the deposition rate of the cobalt metal layer 160 can also be controlled.
[0150] In some examples of this embodiment, during the deposition of the cobalt metal layer 160 , the thickness of the cobalt metal layer 160 is controlled to be 1 nm to 30 nm.
[0151] In some examples of this embodiment, the process of depositing the cobalt metal layer 160 can be performed in a reducing gas atmosphere to ensure the uniformity of the cobalt metal layer 160. It is understood that the reducing gas helps prevent oxidation of the cobalt metal layer 160 during the preparation process, and thus avoids the problem of uneven cobalt metal layer 160 caused by the selective adsorption and deposition of the cobalt organic compound.
[0152] After the cobalt metal layer 160 is deposited, a small amount of oxide layer may be formed on the surface of the cobalt metal layer 160. In some examples of this embodiment, the step of removing the oxide layer on the surface of the cobalt metal layer 160 is further included.
[0153] In some examples of this embodiment, the natural oxide layer on the surface of the cobalt metal layer 160 can be removed by plasma treatment of the surface of the cobalt metal layer 160 or by treatment of the surface of the cobalt metal layer 160 with a reducing gas. The reducing gas can be hydrogen. During the process of treating the metal interconnect layer 150 with the reducing gas, a protective gas, such as nitrogen, can also be introduced.
[0154] Before depositing the cobalt metal layer 160, a small amount of natural oxide layer may exist on the surface of the metal interconnect layer 150, which may affect the uniformity of the prepared cobalt metal layer 160. Therefore, in some examples of this embodiment, before preparing the cobalt metal layer 160, a step of removing the natural oxide layer on the surface of the metal interconnect layer 150 is also included.
[0155] In some examples of this embodiment, the natural oxide layer on the surface of the metal interconnect layer 150 can be removed by plasma treatment of the metal interconnect layer 150 surface, or by treatment of the metal interconnect layer 150 surface with a reducing gas. The reducing gas can be hydrogen. During the process of treating the metal interconnect layer 150 with the reducing gas, a protective gas, such as nitrogen, can also be introduced.
[0156] In some examples of this embodiment, during the deposition process, the surface roughness of the cobalt metal layer can be controlled to be ≤2 nm. The surface roughness of the cobalt metal layer is defined as the height difference between the highest point and the lowest point of the cobalt metal layer, and the roughness can be measured using an atomic force microscope.
[0157] In some examples of this embodiment, during the deposition process, the surface roughness of the cobalt metal layer can be controlled to be ≤1 nm. Further, the surface roughness of the cobalt metal layer can be controlled to be ≤0.5 nm.
[0158] It is understandable that although the cobalt metal layer is prepared using a cobalt organic compound, in the actual preparation product, due to the influence of reaction by-products or the environment such as the reaction chamber, the cobalt metal layer does not necessarily include only cobalt atoms, that is, the proportion of cobalt atoms in the cobalt metal layer may not reach 100%.
[0159] By selecting appropriate reactants, the cobalt organic compound used in this embodiment can produce a cobalt metal layer with a relatively high cobalt atomic ratio. In some examples of this embodiment, the cobalt atomic ratio in the cobalt metal layer is ≥ 90%. Furthermore, the cobalt atomic ratio in the cobalt metal layer is ≥ 95%. Even further, the cobalt atomic ratio in the cobalt metal layer is ≥ 98%.
[0160] In some examples of this embodiment, the cobalt metal layer 160 may also be stacked on the metal seed layer 140 and the liner layer 130. It is understood that this mainly depends on whether cobalt atoms can be deposited on the metal seed layer 140 and the liner layer 130, but this does not affect the preparation of the cobalt metal layer 160.
[0161] In addition, in this embodiment, the material of the liner layer 130 includes cobalt. The cobalt metal layer 160 prepared in this step can be connected to the liner layer 130. The cobalt metal layer 160 and the liner layer 130 together form a cobalt layer surrounding the metal interconnection layer 150, preventing the atoms of the metal interconnection layer 150 from diffusing into the surrounding dielectric layer 110.
[0162] Compared with the traditional chemical vapor deposition method, the use of the cobalt organic compound in the atomic layer deposition method can realize the layer-by-layer preparation of the cobalt metal layer 160, improve the controllability of the cobalt metal layer 160 in terms of film thickness and film uniformity, and is also conducive to obtaining a higher quality cobalt metal layer 160 to meet the needs of smaller-sized devices.
[0163] Through steps S1 to S4, the preparation of the metal interconnect structure disclosed in the present invention can be completed.
[0164] The cobalt metal layer prepared by atomic layer deposition using the cobalt organic compound has the characteristics of controllable thickness and uniformity, and is suitable for the preparation of smaller-sized devices.
[0165] Furthermore, the present disclosure also provides a metal interconnect structure prepared by the method for preparing the metal interconnect structure in the above embodiment. An embodiment of the metal interconnect structure can be shown in FIG7 .
[0166] 7 , the metal interconnect structure includes: a dielectric layer 110 , a metal interconnect layer 150 and a cobalt metal layer 160 ;
[0167] The dielectric layer 110 has an interconnection groove 111 therein. The metal interconnection layer 150 is located in the interconnection groove 111 . The cobalt metal layer 160 is located on the surface of the metal interconnection layer 150 and does not contact the dielectric layer 110 .
[0168] In some examples of this embodiment, the thickness of the cobalt metal layer 160 is ≤30 nm, and the surface roughness of the cobalt metal layer 160 is ≤2 nm. The surface roughness of the cobalt metal layer 160 is defined as the height difference between the highest point and the lowest point of the cobalt metal layer 160, and the roughness can be measured using an atomic force microscope.
[0169] In some examples of this embodiment, the surface roughness of the cobalt metal layer 160 is ≤1 nm. Further, the surface roughness of the cobalt metal layer 160 is ≤0.5 nm.
[0170] In some examples of this embodiment, the thickness of the cobalt metal layer 160 is 1 nm to 10 nm. For example, the thickness of the cobalt metal layer 160 can be 1 nm, 2 nm, 3 nm, 5 nm, 8 nm, or 10 nm. The thickness of the cobalt metal layer 160 can also be in a range between the above thicknesses.
[0171] In some examples of this embodiment, the proportion of cobalt atoms in the cobalt metal layer 160 is ≥ 90%. Further, the proportion of cobalt atoms in the cobalt metal layer 160 is ≥ 95%. Furthermore, the proportion of cobalt atoms in the cobalt metal layer 160 is ≥ 98%.
[0172] For cobalt metal layer 160 prepared by conventional chemical vapor deposition (CVD), the surface roughness of the prepared cobalt metal layer 160 typically exceeds 2 nm due to the limited precision of CVD. Furthermore, to obtain a void-free thin film, the thickness of the cobalt metal layer 160 prepared by CVD typically needs to be at least 30 nm. Furthermore, the proportion of cobalt atoms in the cobalt metal layer 160 prepared by CVD is typically less than 90%.
[0173] The present disclosure utilizes the aforementioned cobalt organic compound to achieve selective atomic layer deposition of a cobalt metal layer 160. Due to the layer-by-layer deposition of cobalt atoms during the atomic layer deposition process, by selecting appropriate reactants and preparation processes, the roughness of the cobalt metal layer 160 can be controlled to below 2 nm when the thickness reaches 30 nm, and the proportion of cobalt atoms in the cobalt metal layer 160 can reach over 90%. Therefore, compared to conventional technologies, the application provided by the present disclosure can effectively improve the controllability of the cobalt metal layer 160 during the preparation process, and the quality of the film can also be effectively improved.
[0174] In some examples of this embodiment, the metal interconnect structure may further include a barrier layer 120, a pad layer 130 and a metal seed layer 140 arranged between the metal interconnect layer 150 and the dielectric layer 110, and the barrier layer 120, the pad layer 130 and the metal seed layer 140 are stacked in sequence from the dielectric layer 110 to the metal interconnect layer 150.
[0175] Furthermore, the present disclosure also provides a semiconductor assembly, which includes the above-mentioned metal interconnection structure and a plurality of semiconductor devices, wherein the plurality of semiconductor devices are electrically connected via the metal interconnection structure.
[0176] In some examples of this embodiment, the semiconductor component may be an integrated circuit, such as a logic chip or a memory.
[0177] In some examples of this embodiment, the semiconductor component may be a memory.
[0178] To facilitate understanding and implementation of the present invention, the following more specific and detailed examples and comparative examples are provided below for reference. The various embodiments of the present invention and their advantages will become apparent through the descriptions and performance results of the following specific examples and comparative examples. Unless otherwise specified, the raw materials used in the following examples and comparative examples are all commercially available.
[0179] The substrate used in each embodiment and comparative example includes a dielectric layer made of silicon dioxide. The dielectric layer has an interconnection groove formed therein, and a barrier layer, a liner layer, a metal seed layer, and a metal interconnect layer are sequentially stacked on the walls of the interconnection groove. The barrier layer comprises a stacked tantalum / tantalum nitride film, the liner layer comprises a cobalt film, and the metal seed layer and metal interconnect layer are made of copper. The surface of the metal interconnect layer is flush with the surface of the dielectric layer.
[0180] Example 1
[0181] The substrate was placed in an atomic layer deposition chamber, using a cobalt organic compound and tert-butylamine as reactants, and argon as a purge gas. In each deposition cycle, the duration of the cobalt organic compound introduction was controlled to be 3 seconds, the duration of the cobalt organic compound purge was 10 seconds, the duration of the reaction material introduction was controlled to be 5 seconds, and the duration of the reaction material purge was 15 seconds. A cobalt metal layer was deposited on the substrate at 200°C, and the number of deposition cycles was 100. After deposition was completed, the substrate was removed. The structural formula of the cobalt organic compound used in Example 1 is as follows:
[0182] Example 2
[0183] The substrate was placed in an atomic layer deposition chamber, using a cobalt organic compound and tert-butylamine as reactants, and argon as a purge gas. In each deposition cycle, the duration of the cobalt organic compound introduction was controlled to be 3 seconds, the purge duration was 10 seconds, the duration of the reaction material introduction was controlled to be 5 seconds, and the duration of the reaction material purge was 15 seconds. A cobalt metal layer was deposited on the substrate at 200°C, and the number of deposition cycles was 100. After deposition, the substrate was removed. The structural formula of the cobalt organic compound used in Example 2 is as follows:
[0184] Example 3
[0185] A substrate was placed in an atomic layer deposition chamber. A cobalt organo compound and tert-butylamine were used as reactants, and argon was used as a purge gas. In each deposition cycle, the cobalt organo compound was introduced for 3 seconds, and the purge was continued for 10 seconds. The reaction material was introduced for 5 seconds, and the purge was continued for 15 seconds. A cobalt metal layer was deposited on the substrate at 200°C for 100 deposition cycles. The substrate was removed after deposition. The structural formula of the cobalt organo compound used in Example 3 is as follows:
[0186] Experiment: The thickness and surface roughness of the cobalt metal layer of each of the above examples were measured by atomic force microscopy, and the cobalt atomic content in the cobalt metal layer of each of the above examples was measured by atomic energy dispersive spectroscopy. The results are shown in Table 1.
[0187] Table 1
[0188] Referring to the results shown in Table 1, the cobalt organic compound provided in the embodiment of the present disclosure can be selectively deposited on the metal interconnect layer by atomic layer deposition. Moreover, when the thickness of the prepared cobalt metal layer is 10 nm, its roughness can be controlled to be below 1 nm, and the cobalt atomic content in the cobalt metal layer reaches more than 90%. It can be understood that for other cobalt organic compounds with similar structures, the prepared cobalt metal layers also have similar effects. Therefore, the present disclosure applies the above-mentioned cobalt organic compound to the preparation of metal interconnect structures, and can utilize the selectivity of the cobalt organic compound for the deposition substrate to improve the controllability of the preparation of cobalt metal in the metal interconnect structure, improve the controllability of the preparation of the cobalt film and the quality of the film, thereby meeting the needs of smaller devices.
[0189] Please note that the above embodiments are for illustrative purposes only and are not intended to limit the present disclosure.
[0190] It should be understood that, unless otherwise expressly stated herein, the steps described are not strictly limited in order of execution, and the steps may be executed in other orders. Furthermore, at least a portion of the steps described may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times. The sub-steps or stages are not necessarily executed sequentially, but may be executed in rotation or alternation with other steps or at least a portion of the sub-steps or stages of other steps.
[0191] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0192] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for preparing a metal interconnect structure, comprising the following steps: providing a dielectric layer having interconnect recesses therein; preparing a metal interconnection layer in the interconnection groove; and, A cobalt metal layer is prepared on the metal interconnect layer by atomic layer deposition using raw materials including cobalt organic compounds. In the cobalt organic compounds, cobalt atoms are bonded to four nitrogen atoms by single bonds, the four nitrogen atoms form pairs, and each pair of nitrogen atoms is connected by an organic group.
2. The method for preparing a metal interconnect structure according to claim 1, wherein the cobalt organic compound has a structure as shown in general formula (1): in, R1, R2, R3 and R4 are each independently selected from substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, substituted or unsubstituted C3-C20 cycloalkyl; L1 and L2 are each independently selected from substituted or unsubstituted C1-C20 alkylene, substituted or unsubstituted C2-C20 alkenylene, substituted or unsubstituted C2-C20 alkynylene; When the groups of R1, R2, R3, R4, L1 and L2 are substituted, the substituents include R5, and each occurrence of R5 is independently selected from an alkyl group, a halogen atom, a C1-C10 alkoxy group, a C1-C10 haloalkyl group, a C1-C10 haloalkoxy group or a C6-C20 aryl group.
3. The method for preparing a metal interconnect structure according to claim 2, wherein R1, R2, R3 and R4 are each independently selected from n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl.
4. The method for preparing a metal interconnect structure according to claim 2 or 3, wherein L1 and L2 are each independently selected from methylene, 1,2-ethylene, 1,1-ethylene, 1,2-vinylene or ethynyl.
5. The method for preparing a metal interconnect structure according to any one of claims 2 to 4, wherein R1 and R2 are the same group.
6. The method for preparing a metal interconnect structure according to any one of claims 2 to 5, wherein R3 and R4 are the same group. 7 . The method for preparing a metal interconnect structure according to claim 2 , wherein L1 and L2 are the same group.
8. The method for preparing a metal interconnect structure according to claim 2, wherein the cobalt organic compound is selected from one of the following structures:
9. The method for preparing a metal interconnect structure according to any one of claims 1 to 8, wherein in the step of preparing the cobalt metal layer, the raw material further comprises a reaction material capable of reacting with the cobalt organic compound, and the reaction material comprises one or more of tert-butylamine and diethylamine.
10. The method for preparing a metal interconnect structure according to any one of claims 1 to 9, wherein during the deposition of the cobalt metal layer, the reaction temperature of the deposition process is controlled to be 100°C to 400°C.
11. The method for preparing a metal interconnect structure according to any one of claims 1 to 10, wherein the process of depositing the cobalt metal layer comprises one or more deposition cycles, each deposition cycle comprising introducing a cobalt organic compound, purging the cobalt organic compound, introducing a reaction material, and purging the reaction material, wherein: The duration of introducing the cobalt organic compound is 1s to 30s, the duration of purging the cobalt organic compound is 1s to 30s, the duration of introducing the reaction material is 1s to 30s, and the duration of purging the reaction material is 1s to 30s. 12 . The method for preparing a metal interconnect structure according to claim 1 , wherein during the deposition of the cobalt metal layer, the number of deposition cycles is controlled to be ≤300.
13. According to the method for preparing a metal interconnect structure according to any one of claims 1 to 12, the process of depositing the cobalt metal layer is carried out in an atmosphere of reducing gas. 14 . The method for preparing a metal interconnect structure according to claim 1 , further comprising treating the cobalt metal layer with a reducing gas or plasma after depositing the cobalt metal layer. 15 . The method for preparing a metal interconnect structure according to claim 1 , wherein a material of the dielectric layer is selected from one or more of silicon dioxide, silicon-based polymer materials and carbon-doped silicon oxide. 16 . The method for preparing a metal interconnect structure according to claim 1 , wherein the material of the metal interconnect layer is selected from one or more of platinum, cobalt, copper and ruthenium.
17. The method for preparing a metal interconnection structure according to any one of claims 1 to 16, before preparing a metal interconnection layer in the interconnection groove, further comprising: preparing a barrier layer covering the walls of the interconnection grooves; A liner layer is prepared on the barrier layer, and the metal interconnection layer is prepared on the liner layer.
18. A metal interconnect structure, comprising: A dielectric layer, a metal interconnection layer and a cobalt metal layer; the dielectric layer has an interconnection groove, the metal interconnection layer is located in the interconnection groove, the cobalt metal layer is arranged on the metal interconnection layer, and the cobalt metal layer is prepared on the metal interconnection layer by atomic layer deposition.
19. The metal interconnect structure according to claim 18, wherein in the step of preparing the cobalt metal layer, the raw material further comprises a reaction material capable of reacting with the cobalt organic compound, and the reaction material comprises one or more of tert-butylamine and diethylamine. 20 . The metal interconnect structure according to claim 18 or 19 , wherein in the raw material, during the process of depositing the cobalt metal layer, the reaction temperature of the deposition process is controlled to be 100° C. to 400° C. 21 . The metal interconnect structure according to claim 18 , wherein the thickness of the cobalt metal layer is ≤30 nm, and the surface roughness of the cobalt metal layer is ≤2 nm. 22 . The metal interconnect structure according to claim 18 , wherein the proportion of cobalt atoms in the cobalt metal layer is ≥ 90%.
23. The metal interconnect structure according to any one of claims 18 to 22, wherein a material of the dielectric layer is selected from one or more of silicon dioxide, silicon-based polymer materials and carbon-doped silicon oxide.
24. The metal interconnect structure according to any one of claims 18 to 23, wherein the material of the metal interconnect layer is selected from one or more of platinum, cobalt, copper and ruthenium.
25. The metal interconnect structure according to any one of claims 18 to 24, further comprising a barrier layer, a liner layer and a metal seed layer arranged between the metal interconnect layer and the dielectric layer, wherein the barrier layer, the liner layer and the metal seed layer are stacked in sequence from the dielectric layer to the metal interconnect layer. 26 . A semiconductor component, comprising the metal interconnect structure according to claim 18 and a plurality of semiconductor devices, wherein the plurality of semiconductor devices are electrically connected via the metal interconnect structure. The semiconductor device according to claim 26 , wherein the semiconductor device is a memory.
Citation Information
Patent Citations
Dielectric barrier layer and manufacturing method thereof, interconnection structure and manufacturing method thereof
CN108962875A
Metal structure, device and method
CN110634836A
Preparation method of metal interconnection structure, metal interconnection structure and semiconductor assembly
CN116230631A
Cobalt precursors useful for forming cobalt-containing films on substrates
US20090208637A1
Cobalt deposition selectivity on copper and dielectrics
US20180130706A1