Lithium battery separator with low short circuit rate and preparation method therefor

By using the combination of surface and intermediate layers of specific polyolefin resins in lithium battery separators, combined with coextrusion processing and thermal setting technology, the short-circuit problem of lithium battery is solved, the pressure resistance and yield of the separator are improved, and the risk of short-circuit is reduced. .

WO2024230365A1PCT designated stage expired Publication Date: 2024-11-14SHENZHEN ZHONGXING NEW MATERIAL TECH CO LTD

Patent Information

Application Number
PCT/CN2024/085363
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-06
Filing Date
2024-04-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Lithium batteries are prone to short circuits during production, resulting in high defective yields and affecting product costs. The existing diaphragms are easily broken down under voltage, forming weak points and causing short circuits.

Method used

Use polyolefin resin with a crystallinity of 20%-30%, isometric not less than 98%, and a melting index of 2-4g/10min as the surface layer, and combines the high crystallinity and low isometricity of the intermediate layer to form The lithium battery separator with A/B/A structure improves the pressure resistance of the separator through coextrusion processing, annealing, stretching and heat setting processes.

Benefits of technology

It reduces the short-circuit rate of the lithium battery separator, improves the voltage resistance of the separator, reduces the occurrence of weak points, reduces the risk of short-circuit, and improves the product yield rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085363_14112024_PF_FP_ABST
    Figure CN2024085363_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a lithium battery separator with a low short circuit rate and a preparation method therefor. The lithium battery separator with the low short circuit rate comprises a middle layer and two surface layers, and the middle layer is provided with a first surface and a second surface located at a side opposite to the first surface; the two surface layers are respectively attached to the first surface and the second surface; and the surface layers are made of polyolefin resin with the crystallinity of 20%-30%, the isotacticity not lower than 98 and the melting index of 2-4 g / 10min. According to the present application, polyolefin with certain crystallinity, isotacticity and melting index is selected as the surface layers of the lithium battery separator, so that the surface of the lithium battery separator has the characteristic of low hardness, and if the surface layers of the lithium battery separator are subjected to external force such as extrusion and friction during preparation, the surface layers can be subjected to elastic deformation and stress relaxation by virtue of the characteristic of low hardness, so as to reduce surface damage, reduce weak points, and improve the overall pressure resistance of the lithium battery separator, thereby reducing the short circuit risk.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium battery separator with low short circuit rate and preparation method thereof Technical Field

[0001] The present invention relates to the field of lithium batteries, and in particular to a lithium battery separator with a low short-circuit rate and a preparation method thereof. Background Art

[0002] Lithium-ion batteries, with their high energy density, excellent safety, and long cycle life, are widely used in power, energy storage, 3C, and other fields. They have achieved mature commercial applications and have become indispensable products in people's daily lives, work, and commercial activities. Among them, the safety performance of lithium batteries is one of the most important basic performance characteristics for various consumer groups. The separator in the lithium battery system has the function of isolating the positive and negative electrodes and conducting ions, effectively preventing unsafe factors such as short circuits in lithium batteries.

[0003] In lithium battery products, the yield rate in the product manufacturing process is an important factor affecting the cost. The higher the yield rate, the lower the product cost. However, an excessively low yield rate will affect the cost of lithium battery products. Therefore, how to improve the yield rate is one of the focuses in this field.

[0004] Short circuits during the lithium battery manufacturing process are a common factor that primarily contributes to poor battery performance. As one of the four main components of a lithium battery system, the separator is closely linked to whether or not a battery experiences short circuits. In particular, separators are susceptible to damage during the production process, forming weak points that can easily break down at certain voltages, leading to short circuits. These issues represent a pressing technical challenge in this field.

[0005] Summary of the Invention

[0006] The present invention provides a lithium battery separator with low short-circuit rate and a preparation method thereof, which can effectively reduce the short-circuit rate after the separator is assembled into a battery.

[0007] According to a first aspect, the present application provides a lithium battery separator with a low short circuit rate, comprising:

[0008] an intermediate layer and two surface layers, wherein the intermediate layer has a first surface and a second surface located opposite to the first surface; and the two surface layers are attached to the first surface and the second surface respectively;

[0009] The surface layer is a polyolefin resin with a crystallinity of 20%-30%, an isotacticity of not less than 98, and a melt index of 2-4 g / 10 min.

[0010] In an optional embodiment, the intermediate layer is a polyolefin resin with a crystallinity of not less than 42%, an isotacticity of 90-95, and a melt index of 0.5-2 g / 10 min.

[0011] In an optional embodiment, the surface layer is a polypropylene resin; and / or

[0012] The middle layer is made of polypropylene resin.

[0013] In an optional embodiment, the thickness of the surface layer accounts for 20%-50% of the total thickness.

[0014] In an optional embodiment, the porosity of the lithium battery separator is 35%-55%.

[0015] In an optional embodiment, the total thickness of the intermediate layer and the two surface layers is 10-25 μm.

[0016] According to a second aspect, the present application provides a method for preparing the above-mentioned lithium battery separator with low short circuit rate, comprising the following steps:

[0017] Co-extruding the raw materials of the surface layer and the raw materials of the middle layer and cooling them so that the surface layer is attached to opposite sides of the middle layer to obtain a cast film;

[0018] annealing the cast film;

[0019] The cast film after annealing is stretched and heat-set in sequence to obtain a lithium battery separator.

[0020] In an optional embodiment, in the step of co-extrusion and cooling:

[0021] The extrusion temperature of the surface layer is 250-300°C; and / or

[0022] The extrusion temperature of the intermediate layer is 190-230°C; and / or

[0023] The cooling temperature is 70-100°C.

[0024] In an optional embodiment, in the step of annealing the cast film, the annealing temperature is 135-150° C. and the annealing time is 10-16 hours.

[0025] In an optional embodiment, the stretching step comprises: cold drawing at a stretching ratio of 1.1-1.5 and a temperature of 80-100° C., and then hot drawing at a stretching ratio of 1.6-2.4 and a hot drawing temperature of 135-153° C.; and / or

[0026] The temperature of the heat setting is 150-165°C.

[0027] The beneficial effect of the present application is that: the present application selects polyolefins with a certain degree of crystallinity, isotacticity and melt index as the surface layer of the lithium battery separator, so that the surface of the lithium battery separator has the characteristics of low hardness. If it is subjected to external forces such as extrusion and friction during the manufacturing process, the surface layer can use its own low hardness to reduce surface damage through elastic deformation and stress relaxation, reduce the occurrence of weak points, improve the overall pressure resistance of the lithium battery separator, and thus reduce the risk of short circuit. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG1 is a schematic diagram of a layered structure according to an embodiment of the present application.

[0029] Reference numerals: surface layer 1 , intermediate layer 2 . DETAILED DESCRIPTION

[0030] The present invention will be further described in detail below by means of specific embodiments in conjunction with the accompanying drawings. Similar elements in different embodiments are numbered with associated similar elements. In the following embodiments, many detailed descriptions are provided to enable the present application to be better understood. However, those skilled in the art will readily appreciate that some of the features may be omitted in different circumstances, or may be replaced by other elements, materials, or methods. In some cases, some operations related to the present application are not shown or described in the specification. This is to avoid the core portion of the present application being overwhelmed by excessive descriptions, and for those skilled in the art, it is not necessary to describe these related operations in detail. They will fully understand the related operations based on the description in the specification and the general technical knowledge in the art.

[0031] In addition, the features, operations, or characteristics described in the specification may be combined in any appropriate manner to form various embodiments. Furthermore, the steps or actions in the method description may be reordered or adjusted in a manner readily apparent to those skilled in the art. Therefore, the various sequences in the specification and drawings are provided solely for the purpose of clearly describing a particular embodiment and are not intended to be mandatory, unless otherwise specified.

[0032] The serial numbers assigned to components herein, such as "first," "second," etc., are used solely to distinguish the objects being described and do not convey any sequential or technical meaning. References to "connection" and "coupling" herein, unless otherwise specified, include both direct and indirect connections (couplings).

[0033] On one hand, the present application discloses a lithium battery separator with low short-circuit rate, which includes an intermediate layer 2 and two surface layers 1. Specifically, the intermediate layer 2 has a first surface and a second surface, which are arranged opposite to each other. For example, as shown in FIG1 , the upper surface of the intermediate layer 2 is the first surface, and the lower surface of the intermediate layer 2 is the second surface. The two surface layers 1 are respectively attached to the first surface and the second surface, that is, when the first surface and the second surface of the intermediate layer 2 are the upper and lower surfaces of the intermediate layer 2, respectively, the surface layer 1 is respectively located on the upper side and the lower side of the intermediate layer 2. This allows the present application to form a three-layer separator with an A / B / A structure, wherein layer A is the surface layer 1 and layer B is the intermediate layer 2.

[0034] In the embodiments disclosed in the present application, the surface layer 1 is made of a polyolefin resin having a crystallinity of 20%-30%, an isotacticity of not less than 98, and a melt index of 2-4 g / 10 min. For example, the polyolefin resin may be a polypropylene resin, which may be a modified or unmodified polypropylene that meets the above-mentioned parameter requirements, and the present application does not make any specific limitations.

[0035] Since the crystallinity, isotacticity and melt index of polypropylene will affect the hardness of the material to a certain extent, this application selects polyolefin with relatively low crystallinity, relatively high isotacticity and a certain melt index as the surface layer 1 of the lithium battery separator, so that the surface of the lithium battery separator has a certain elasticity and low hardness. Furthermore, during the manufacturing process, when the surface of the lithium battery separator is subjected to extrusion, friction, etc., the lithium battery separator can undergo elastic deformation and stress relaxation through the surface layer 1 on its surface, thereby effectively reducing surface damage and reducing the risk of short circuit.

[0036] In some optional designs, the above-mentioned intermediate layer 2 can be made of a polyolefin resin with a crystallinity of not less than 42%, an isotacticity of 90-95, and a melt index of 0.5-2g / 10min. Similarly, the polyolefin resin can be modified or unmodified polypropylene resin. This application does not make specific restrictions on this.

[0037] Since the crystallinity, isotacticity and melt index of polypropylene will affect the pore size of the material to a certain extent, the present application selects polyolefins with relatively high crystallinity, relatively low isotacticity and a certain melt index as the intermediate layer 2 of the lithium battery separator, so that the intermediate layer 2 can form a small pore structure. The pore size in the lithium battery separator is mainly to allow lithium ions to pass through the separator better and reach the opposite positive or negative electrode. If the pore size structure of the intermediate layer 2 is too large, active substances other than lithium ions will also pass through the separator, thereby causing an internal short circuit in the battery using the lithium battery separator; therefore, the present application can further improve the pressure resistance of the lithium battery separator by reducing the pore size of the intermediate layer 2.

[0038] In some optional designs, the thickness of the surface layer 1 accounts for 20%-50% of the total thickness. The thickness of the above-mentioned surface layer 1 can be the same or different. Preferably, the thickness of the above-mentioned two surface layers 1 is the same; for example, when the thickness of the lithium battery separator is 14μm, the thickness of the above-mentioned surface layer 1 can be between 2.8 and 7μm, and the thickness of each surface layer 1 can be between 1.4 microns and 3.5 microns.

[0039] In some optional designs, the overall porosity of the lithium battery separator finally formed is 35%-55%, and the specific porosity can be controlled during the stretching stage.

[0040] In some optional designs, the total thickness of the middle layer 2 and the two surface layers 1 is 10-25 μm, which can be controlled during the extrusion and stretching stages.

[0041] In a second aspect, the present application further provides a method for preparing the above-mentioned lithium battery separator with low short circuit rate, comprising the following steps:

[0042] Step S1: The raw materials for the surface layer 1 and the middle layer 2 are put into a co-extrusion device for melting, and then extruded through the die head of the co-extrusion device to obtain a pre-film in which the surface layer 1 is attached to opposite sides of the middle layer 2. The pre-film is cooled to obtain a cast film;

[0043] Specifically, in this step, the material A constituting the surface layer 1 and the material B constituting the middle layer 2 are respectively added to the co-extrusion equipment to melt the material A and the material B; illustratively, the above-mentioned material A can be extruded through the two surface layer outlets of the die head at 250-300°C, and the above-mentioned material B can be extruded from the middle outlet of the die head at 190-230°C, thereby forming a prefabricated film with a three-layer structure of A / B / A.

[0044] The prefabricated film is then cooled by a casting cooling roller. Specifically, the cooling temperature of the casting cooling roller can be set between 70-100°C. For example, the surface temperature of the casting cooling roller can be set to 70°C or 100°C. After cooling the prefabricated film, a cast film can be obtained.

[0045] In this step, the above-mentioned material A is a polyolefin resin particle with a crystallinity of 20%-30%, an isotacticity of not less than 98, and a melt index of 2-4g / 10min. For example, polypropylene resin particles are used as material A in this application; the above-mentioned material B is a polyolefin resin particle with a crystallinity of not less than 42%, an isotacticity of 90-95, and a melt index of 0.5-2g / 10min. For example, polypropylene resin particles are used as material B in this application.

[0046] Step S2: Annealing the cast film prepared in step S1.

[0047] Specifically, in this step, the cast film can be rolled up and placed in an oven for annealing. For example, after the cast film is cooled, the cast film can be rolled into a roll, wherein the roll length is 2000-4000m and the roll width is 1-2m, and then the oven temperature is set to 135-150°C and annealed for 10-16h.

[0048] It can be understood that the annealing temperature and the annealing time are inversely proportional. Specifically, when the annealing temperature is higher, a shorter annealing time can be used. Conversely, when the annealing temperature is lower, a longer annealing time is required. For example, when the oven temperature is set to 150°C, the annealing time can be controlled at about 10 hours, and when the oven temperature is set to 135°C, the annealing time needs to be set at about 16 hours.

[0049] Step S3: The annealed cast film is sequentially stretched and heat-set to obtain a lithium battery separator.

[0050] In this step, the cast film after annealing is stretched and heat-set to form a porous structure inside the film. Specifically, the stretching can be performed by cold drawing and hot drawing in sequence. For example, when cold drawing is performed, the stretching ratio can be 1.1-1.5 and the temperature can be 80-100°C. When hot drawing is performed, the stretching ratio can be 1.6-2.4 and the temperature can be 135-150°C.

[0051] Finally, after stretching, the cast film is heat-set, that is, the separator is heat-treated at high temperature to reduce its thermal shrinkage and improve its dimensional stability, thereby obtaining a lithium battery separator; illustratively, the above heat setting can be carried out at 150-165°C.

[0052] In order to further illustrate the effects of this application, this application also provides the following more specific embodiments:

[0053] Control Example

[0054] Prepare material A, which is a polypropylene resin particle with an isotacticity of 96, a crystallinity of 34%, and a melt index of 2.0 g / 10 min; prepare material B, which is a polypropylene resin particle with an isotacticity of 98, a crystallinity of 38%, and a melt index of 1.0 g / 10 min.

[0055] Material A and material B are added to a co-extrusion device to form a prefabricated film with an A / B / A structure by co-extrusion (wherein, layer A is extruded from material A, and layer B is extruded from material B); wherein, the extrusion processing temperature of layer A is 230°C, and the extrusion processing temperature of layer B is 220°C; the prefabricated film is cooled by a casting roller at 85°C to form a cast film, and then wound up for 2500m, and then annealed at 143°C for 15h; and then longitudinally stretched, wherein, the cold drawing temperature is 85°C and the stretching ratio is 1.3, and the hot drawing temperature is 153°C and the stretching ratio is 2.1; after the stretching is completed, heat setting is performed at 163°C.

[0056] Finally, a lithium battery separator with a thickness of 14 μm and a porosity of 39% was prepared. The lithium battery separator included an intermediate layer 2 made of material B, and a surface layer 1 located on the upper and lower surfaces of the intermediate layer 2 and made of material A, wherein the surface layer 1 accounts for 30% of the total thickness of the lithium battery separator.

[0057] Example 1

[0058] Referring to the method disclosed in the control example, three groups of lithium battery separators were prepared, which were marked as sample 1, sample 2 and sample 3 respectively.

[0059] Among them, in sample 1, the raw material used for the surface layer is polypropylene with an isotacticity of 98, a crystallinity of 20%, and a melt index of 2.0 g / 10 min; the raw material used for the middle layer is polypropylene with an isotacticity of 98, a crystallinity of 38%, and a melt index of 1.0 g / 10 min; the remaining preparation steps and process parameters are the same as those of the control example.

[0060] The sample 1 finally obtained has a thickness of 14 μm, a porosity of 39%, and the surface layer 1 accounts for 30% of the total thickness of the lithium battery separator.

[0061] Among them, in sample 2, the raw material used for the surface layer is polypropylene with an isotacticity of 96, a crystallinity of 34%, and a melt index of 2.0 g / 10 min; the raw material used for the middle layer is polypropylene with an isotacticity of 94, a crystallinity of 42%, and a melt index of 1.0 g / 10 min. The remaining preparation steps and process parameters are the same as those of the control example.

[0062] The thickness of the sample 2 finally obtained was 14 μm, the porosity was 39%, and the surface layer 1 accounted for 30% of the total thickness of the lithium battery separator.

[0063] Among them, the raw materials used in sample 3 are the same as those in sample 1; during preparation, the preparation steps refer to control example 1, with the difference being that during the preparation process, the prefabricated film of the A / B / A structure is formed by increasing the extrusion temperature of the A layer to 260°C, while the other process parameters remain unchanged.

[0064] The sample 3 finally obtained has a thickness of 14 μm, a porosity of 39%, and the surface layer 1 accounts for 30% of the total thickness of the lithium battery separator.

[0065] The various properties of the above control example and samples 1 to 3 were tested.

[0066] Among them, the thickness is measured by a Marr thickness gauge; the air permeability is tested by a Gurley air permeability instrument; the porosity is calculated by the mass method; the pore size is tested by a PMI tester, and the test principle is the bubble point method. The measured pore size is the pore size value of the narrowest part of the diaphragm pore structure; the withstand voltage value is tested by a withstand voltage tester, and the lithium battery diaphragm is placed under simulated positive and negative electrode conditions, and the voltage is gradually increased, and finally the diaphragm breaks down. The voltage value corresponding to the breakdown is the withstand voltage value, among which the higher the withstand voltage value, the stronger the diaphragm's ability to resist short circuits; the hardness test of the lithium battery diaphragm adopts a nano-comprehensive mechanical properties tester, which is based on a nano-mechanical microprobe system and can perform nano-indentation hardness testing.

[0067] The final test results are shown in Table 1:

[0068] Table 1

[0069] It can be seen from the above experimental data that the withstand voltage values ​​of Samples 1, 2 and 3 are improved compared with the control example.

[0070] Comparing the control and Sample 1, we can see that the porosity and pore size of Sample 1 are similar to those of the control, but the surface hardness is significantly reduced. This indicates that by reducing the crystallinity and increasing the isotacticity of the surface layer 1, the hardness of the lithium battery separator can be reduced, thereby increasing the withstand voltage.

[0071] Comparing Sample 2 with Sample 1 and the control, we can see that while the hardness of Sample 2 does not decrease as much as Sample 1, its pore diameter at its narrowest point is significantly smaller than that of the control. This indicates that reducing the isotacticity and crystallinity of the intermediate layer 2 material can effectively reduce the pore diameter of the lithium battery separator, thereby improving the withstand voltage.

[0072] Comparing Sample 3 with Sample 1, it can be found that the withstand voltage of Sample 3 is further improved compared to Sample 1, and the hardness is further reduced compared to Sample 1. This shows that during the production process, increasing the extrusion temperature of the surface layer 1 can further reduce the hardness of the lithium battery separator, thereby improving the withstand voltage.

[0073] Example 2

[0074] Prepare material A, which is polypropylene with an isotacticity of 98, a crystallinity of 22%, and a melt index of 2.0 g / 10 min; prepare material B, which is polypropylene with an isotacticity of 93, a crystallinity of 45%, and a melt index of 1.0 g / 10 min.

[0075] Material A and material B are added to a co-extrusion device to form a prefabricated film with an A / B / A structure through co-extrusion; wherein, the extrusion processing temperature of layer A is 260°C, and the extrusion processing temperature of layer B is 220°C; the prefabricated film is cooled by a casting roller at 85°C to form a cast film, and then wound up to 2500m, and then annealed at 143°C for 15h; and then longitudinally stretched, wherein, the cold drawing temperature is 85°C and the stretching ratio is 1.3, and the hot drawing temperature is 153°C and the stretching ratio is 2.1; after the stretching is completed, heat setting is performed at 163°C.

[0076] Finally, a 14 μm thick, 39% porosity lithium battery separator was prepared, comprising an intermediate layer 2 made of material B and surface layers 1 made of material A located on the upper and lower surfaces of the intermediate layer 2. The surface layer 1 accounted for 30% of the total thickness of the lithium battery separator. The various properties of Example 2 were then tested using the methods disclosed in Example 1. The results are shown in Table 2.

[0077] Table 2

[0078] It can be seen from the above experimental results that the withstand voltage value finally obtained in Example 2 is higher than that in the control example and samples 1 to 3, indicating that while reducing the hardness, the withstand voltage value of the lithium battery separator can be greatly improved by reducing the pore size of the intermediate layer.

[0079] Example 3

[0080] Prepare layer A material, which is polypropylene with an isotacticity of 98, a crystallinity of 30%, and a melt index of 4.0 g / 10 min; prepare layer B material, which is polypropylene with an isotacticity of 95, a crystallinity of 42%, and a melt index of 2 g / 10 min.

[0081] Layer A material and layer B material are added to a co-extrusion device to form a prefabricated film with an A / B / A structure through co-extrusion; wherein, the extrusion processing temperature of layer A is 300°C, and the extrusion processing temperature of layer B is 230°C; the prefabricated film is cooled by a 100°C casting roller to form a cast film, and then wound up for 2500m, and then annealed at 150°C for 10 hours; and then longitudinally stretched, wherein, the cold drawing temperature is 100°C and the stretching ratio is 1.5, and the hot drawing temperature is 150°C and the stretching ratio is 2.4; after the stretching is completed, heat setting is performed at 165°C.

[0082] Example 4

[0083] Prepare layer A material, which is polypropylene with an isotacticity of 98, a crystallinity of 20%, and a melt index of 2.0 g / 10 min; prepare layer B material, which is polypropylene with an isotacticity of 90, a crystallinity of 42%, and a melt index of 0.5 g / 10 min.

[0084] Layer A material and layer B material are added to a co-extrusion device to form a prefabricated film with an A / B / A structure through co-extrusion; wherein, the extrusion processing temperature of layer A is 250°C, and the extrusion processing temperature of layer B is 190°C; the prefabricated film is cooled by a 70°C casting roller to form a cast film, and then wound up to 2500m, and then annealed at 135°C for 16h; and then longitudinally stretched, wherein, the cold drawing temperature is 80°C and the stretching ratio is 1.1, and the hot drawing temperature is 135°C and the stretching ratio is 1.6; after the stretching is completed, heat setting is performed at 150°C.

[0085] The above examples are used to illustrate the present invention, which are only used to help understand the present invention and are not intended to limit the present invention. Those skilled in the art can make several simple deductions, modifications or substitutions based on the concept of the present invention.

Claims

1. A lithium battery separator with low short circuit rate, characterized in that: include: an intermediate layer and two surface layers, the intermediate layer having a first surface and a second surface located on an opposite side of the first surface; The two surface layers are respectively attached to the first surface and the second surface; The middle layer is a polyolefin resin with a crystallinity of not less than 42%, an isotacticity of 90-95, and a melt index of 0.5-2g / 10min; the surface layer is a polyolefin resin with a crystallinity of 20%-30%, an isotacticity of not less than 98, and a melt index of 2-4g / 10min.

2. The lithium battery separator with low short circuit rate according to claim 1, characterized in that: The surface layer is a polypropylene resin; and / or The middle layer is made of polypropylene resin.

3. The lithium battery separator with low short circuit rate according to claim 1, characterized in that: The thickness of the surface layer accounts for 20%-50% of the total thickness.

4. The lithium battery separator with low short circuit rate according to claim 1, characterized in that: The porosity of the lithium battery separator is 35%-55%.

5. The lithium battery separator with low short circuit rate according to claim 1, characterized in that: The total thickness of the intermediate layer and the two surface layers is 10-25 μm.

6. A method for preparing a lithium battery separator with low short circuit rate as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Co-extruding and cooling the raw materials of the surface layer and the middle layer, so that the surface layer is attached to the opposite sides of the middle layer to obtain a cast film; annealing the cast film; The cast film after annealing is stretched and heat-set in sequence to obtain a lithium battery separator.

7. The method for preparing a lithium battery separator according to claim 6, characterized in that: In the step of co-extrusion processing and cooling: The extrusion temperature of the surface layer is 250-300°C; and / or The extrusion temperature of the intermediate layer is 190-230°C; and / or The cooling temperature is 70-100℃.

8. The method for preparing a lithium battery separator according to claim 6, characterized in that: In the step of annealing the cast film, the annealing temperature is 135-150° C. and the annealing time is 10-16 hours.

9. The method for preparing a lithium battery separator according to claim 6, characterized in that: The steps of sequentially stretching and heat setting the annealed cast film include: cold drawing at a stretching ratio of 1.1-1.5 and a temperature of 80-100° C., and then hot drawing at a stretching ratio of 1.6-2.4 and a hot drawing temperature of 135-153° C.; and / or The temperature of the heat setting is 150-165°C.

Citation Information

Patent Citations

  • Three-layer co-extruded lithium-ion battery separation membrane and production method thereof

    CN104979513A

  • Dry unilateral-stretching production technology of lithium battery separator

    CN111391267A

  • Thin film, preparation method thereof and battery

    CN114188658A

  • High-strength three-layer co-extrusion lithium ion battery diaphragm and preparation method thereof

    CN114497896A

  • Lithium battery diaphragm with low short circuit rate and preparation method thereof

    CN116207446A

Cited By

  • Method for improving dense flaws of dry diaphragm of lithium battery

    CN121440036A