Polypropylene composition, and preparation method therefor and use thereof
By using components such as N-substituted alkoxy-hindered amines and hypophosphites in polypropylene materials, combined with thioester antioxidants, the problem of polypropylene flame retardant materials being prone to failure at high temperatures and discoloration during processing is solved. , achieving longer powdering time and better high temperature flame retardant performance.
Patent Information
- Application Number
- PCT/CN2024/089361
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-14
AI Technical Summary
The existing polypropylene flame retardant materials are prone to failure at high temperatures, have short service life, and are prone to discoloration during processing. The traditional bromine flame retardant has poor compatibility with PP resin, resulting in product appearance problems.
Using N-substituted alkoxy-hindered amine as flame retardant synergistic agent, combined with hypophosphite and thioester antioxidants, select flame retardant synergistic agents with low decomposition volatility and hindered amine light stabilizers with low alkalinity. The modified polypropylene composition is formed by melt blending by an extruder.
It extends the powdering time of flame retardant materials, improves high temperature resistance, reduces the discoloration and powdering of materials, extends the flame retardant failure time, and improves the processing performance and appearance effect of materials.
Smart Images

Figure PCTCN2024089361-FTAPPB-I100001 
Figure PCTCN2024089361-FTAPPB-I100002 
Figure PCTCN2024089361-FTAPPB-I100003
Abstract
Description
A polypropylene composition and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of modified materials, and in particular to a polypropylene composition, a preparation method and an application thereof. Background Art
[0002] Polypropylene, due to its excellent processing properties and superior mechanical, physical, and chemical properties, combined with its lightweight and low price, is widely used in a wide range of industries, including automotive interior and exterior trim, home appliances and electronics, packaging, textiles, building materials, automotive, electronics / electrical, office supplies, and daily necessities. However, polypropylene is highly flammable, with a limiting oxygen index of only 17.0-18.0%. It does not self-extinguish after ignition in air, posing a significant fire hazard and necessitating flame retardant modification.
[0003] For components such as home appliances, automotive parts, and electrical components, the UL94 V-2 flame retardancy rating is generally adopted in the industry. Traditional flame-retardant V-2 polypropylene typically uses brominated flame retardants such as tetrabromobisphenol A-bis(2,3-dibromopropyl) ether, tetrabromobisphenol S-bis(2,3-dibromopropyl) ether, or tris(2,3-dibromopropyl) isocyanurate, compounded with antimony trioxide. However, these brominated flame retardants have poor compatibility with the PP resin substrate and easily migrate to the PP surface (blooming), seriously affecting the appearance of the finished part. Furthermore, brominated flame retardants, particularly tetrabromobisphenol A-bis(2,3-dibromopropyl) ether and tetrabromobisphenol S-bis(2,3-dibromopropyl) ether flame retardant systems, have poor heat resistance during injection molding and are prone to yellowing. Finally, the bromine-antimony synergistic flame retardant system produces a large amount of thick smoke when burned, which may reduce the probability of escape in actual applications.
[0004] Another flame retardant system is a phosphorus-nitrogen-bromine free radical-initiated flame retardant system. In this system, the bromine flame retardant is melamine hydrobromide, and the phosphorus flame retardant is a metal hypophosphite (phosphine) salt. Most of these products on the market use 2,3-dimethyl-2,3-diphenylbutane as the free radical initiator. A total flame retardant addition of 1-2% can achieve a UL94V-2 flame retardant effect, and this flame retardant system does not exhibit blooming. However, long-term use at high temperatures can reduce the flame retardant efficiency of flame-retardant polypropylene. If the temperature rises above 100°C, its service life is even shorter.
[0005] Therefore, it is of great significance to avoid the problems of flame retardant polypropylene materials such as easy flame retardant failure at high temperatures, short service life and easy powdering, as well as easy discoloration during processing.
[0006] Summary of the Invention
[0007] In order to overcome the above-mentioned defects of the prior art, the present invention provides a polypropylene composition, a preparation method and an application thereof.
[0008] This is achieved specifically through the following technical solutions:
[0009] A polypropylene composition comprising the following components in parts by weight:
[0010] The flame retardant synergist is one or more N-substituted alkoxy hindered amines; and the pKa value of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is less than 8.1.
[0011] Furthermore, the polypropylene is selected from one or more of homopolypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer, and propylene-1-butene random block copolymer. The polypropylene has a melt flow rate of 8 to 18 g / 10 min. The melt flow rate is tested in accordance with ISO 1133-2-2011 at 230°C and a load of 2.16 kg.
[0012] Furthermore, the hypophosphite may be one or more of sodium hypophosphite, aluminum hypophosphite, calcium hypophosphite, organic aluminum hypophosphite and organic lithium hypophosphite. 50 The particle size is 10-30μm.
[0013] Furthermore, the flame retardant synergist is one or more N-substituted alkoxy hindered amines. While conventional flame retardant synergists decompose and volatilize during thermal oxidative aging, causing the flame retardant function of the entire system to decline, the flame retardant synergist selected in the present invention has low decomposition volatility and a higher decomposition temperature, thereby improving the flame retardant failure problem.
[0014] Furthermore, the N-substituted alkoxy hindered amine is one or more of tris(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl)phosphite, bis(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate or bis(1-alkoxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate.
[0015] Furthermore, the primary antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] and 3,9-bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, preferably tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol.
[0016] Furthermore, the auxiliary antioxidant is one or more of 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl), pentaerythritol bis(2,4-tert-butylphenyl)diphosphite, or a thioester antioxidant, preferably a thioester auxiliary antioxidant. By selecting the primary antioxidant and the thioester auxiliary antioxidant, it is beneficial to form intermolecular hydrogen bonds between the phenolic hydroxyl group of the symmetrically hindered phenol antioxidant and the thioester, which is beneficial to the effective decomposition of polymer hydroperoxides and their conversion into stable alcohol products, thereby improving the high-temperature flame retardant failure resistance of the material.
[0017] Furthermore, the thioester antioxidant is at least one of dialkyl esters of thiodipropionic acid or pentaerythritol tetrakis (3-laurylthiopropionate), preferably dialkyl esters of thiodipropionic acid.
[0018] Furthermore, the pKa value of the hindered amine light stabilizer is less than 8.1. Examples include the high molecular weight, low alkalinity hindered amine light stabilizer N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine methylated polymer with morpholine-2,4,6-trichloro-1,3,5-triazine (CYASORB UV-3529) (pKa = 8.1) produced by Cytec (USA), and Uvinul 5050H (pKa = 7.5) produced by BASF (China). Using a hindered amine light stabilizer with a basicity lower than 8.1 is less likely to react with acidic substances produced by flame retardants, thereby reducing the effectiveness of the light stabilizer.
[0019] Furthermore, the brominated flame retardant is one or more of the bromine-phosphonium flame retardants tris(tribromoneopentyl) phosphate, tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tris(2,3-dibromopropyl) isocyanurate, tetrabromobisphenol S bis(2,3-dibromopropyl) ether, melamine hydrobromide and 1,2-bis(pentabromophenyl)ethane.
[0020] Furthermore, the general structural formula of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is:
[0021] Wherein, X is CH3, -CH2CH3, -OCHCH3 or
[0022] When X in the above general structural formula is replaced by H, the basicity of the hindered amine light stabilizer is relatively strong, and it is easy to react with the acidic flame retardant, thereby consuming the hindered amine light stabilizer and causing the light aging protection effect of the material to be weakened.
[0023] Furthermore, the structure of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is:
[0024] The CAS number is 65447-77-0.
[0025] The present invention also provides a method for preparing the polypropylene composition, comprising the following steps:
[0026] S1: Weigh and pre-mix the components according to the ratio to obtain a premix;
[0027] S2: The premix of step S1 is put into an extruder for melt blending and extrusion granulation to obtain the polypropylene composition.
[0028] Furthermore, the extruder is a twin-screw extruder, the screw speed of the twin-screw extruder is 250-350rpm, the temperatures of each section of the screw of the twin-screw extruder from the feeding port to the die are 150-160°C in zone 1, 180-190°C in zone 2, 180-190°C in zone 3, 180-190°C in zone 4, and 180-190°C in zone 5, the die temperature is 190-200°C, the main engine speed is 300-500r / min, and the vacuum degree is lower than 0.1MPa.
[0029] The present invention also provides use of the polypropylene composition in the preparation of vehicles and household appliances.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] By selecting a specific flame retardant synergist and combining it with an antioxidant, the flame retardant synergist's effect on polypropylene chain scission can be mitigated, alleviating material pulverization and extending the time it takes for the flame retardant to fail. The presence of a hindered amine light stabilizer (HALS) can prevent further oxidation of aldehydes to acids, which can lead to polypropylene degradation. This improves both the material's pulverization performance and its discoloration. The flame retardant synergist of this invention affects processing and thermal oxidative aging, which are major factors in flame failure. By selecting an antioxidant suitable for high-temperature operation to extend the pulverization time, and then adding a HALS that works synergistically with the antioxidant, this delays material pulverization and mitigates discoloration. DETAILED DESCRIPTION
[0032] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0033] <Preparation of Examples and Comparative Examples>
[0034] The raw materials used in the examples and comparative examples of the present invention are all commercially available, but are not limited to these materials:
[0035] Polypropylene: homopolymer polypropylene, PP Moplen HP500N, LyondellBasell;
[0036] Hypophosphite: aluminum hypophosphite, HT-220 (D50 = 15 μm), Shandong Taixing New Materials Co., Ltd.
[0037] Brominated flame retardant A: melamine hydrobromide, MHB, Nanjing Yite;
[0038] Brominated flame retardant B: Tetrabromobisphenol S-bis(2,3-dibromopropyl) ether, Inner Mongolia Pulitai Material Technology Co., Ltd.
[0039] Flame retardant synergist A: tris(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl)phosphite (NORPM), Qingdao University;
[0040] Flame retardant synergist B: bis(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate (NORSM), Qingdao University;
[0041] Flame retardant synergist C: 2,3-dimethyl-2,3-diphenylbutane, Wuxi Zhufeng Fine Chemical Co., Ltd.
[0042] Flame retardant synergist D: p-isopropylbenzene polymer (C12H18)x, x = 3-5, Wuxi Zhufeng Fine Chemical Co., Ltd.
[0043] Primary antioxidant: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, Irganox 1010, BASF, Germany;
[0044] Auxiliary antioxidant A: triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl), Irganox 168, BASF, Germany;
[0045] Secondary antioxidant B: dialkyl ester of thiodipropionic acid, PS802FL, BASF, Germany;
[0046] Auxiliary antioxidant C: bis(2,4-di-tert-butylphenyl) propionate] pentaerythritol diphosphite, antioxidant 626, Li'anlong New Materials Co., Ltd.
[0047] Hindered amine light stabilizer A: reaction product of α-olefin (C20-C24) containing polymer of maleic anhydride and 2,2,6,6-tetramethyl-4-piperidine, Uvinul 5050H (pKa=7.5), BASF (China);
[0048] Hindered amine light stabilizer B: poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}, CHIMASSORB 944 FDL, pKa=8.6, BASF (China);
[0049] Hindered amine light stabilizer C: polymer of succinic acid and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol, its structure is:
[0050] The CAS number is 65447-77-0, the number average molecular weight is 3000-4000, pKa = 5.6, BASF Schweiz AG. The preparation methods of the examples and comparative examples of the present invention are as follows:
[0051] S1: According to the ratios in Table 1 and Table 3, weigh and pre-mix the components to obtain a premix;
[0052] S2: The premix of step S1 is put into a twin-screw extruder for melt blending and extrusion granulation to obtain a polypropylene composition.
[0053] The screw speed of the twin-screw extruder is 300rpm. The temperatures of each section of the screw of the twin-screw extruder from the feeding port to the die are 150℃ in zone 1, 180℃ in zone 2, 180℃ in zone 3, 180℃ in zone 4, and 180℃ in zone 5. The die temperature is 200℃, the main engine speed is 400r / min, and the vacuum degree is lower than 0.1MPa.
[0054] <Test Standard>
[0055] The performance test standards of the embodiments and comparative examples of the present invention are as follows:
[0056] Pka test method:
[0057] Add approximately 60 ml of 0.100 mol·L-1 hexafluoropropanol (or oxalic acid if measuring weak acids with a pKa < 2.3) to a dry 150 ml beaker. Rinse the burette with this solution and fill it to 0.00 ml. Accurately dispense a predetermined volume of solution (49.95 ml in this experiment) into another clean, dry 150 ml beaker.
[0058] Place the electromagnetic stirrer in the solution, place the beaker on the electromagnetic stirrer, carefully insert the pH electrode calomel electrode into the solution, and connect it to the potentiometer to record the initial pH value.
[0059] Draw a pH-V curve. Initially, record the pH value after adding 1 ml of NaOH until the slope of the curve approaches 1.0. Then, add 0.20 ml of alkali solution and record the pH value until the slope of the curve approaches infinity, which is the endpoint. Repeat the titration twice to determine the exact endpoint volume.
[0060] Find the pKa from the curve. From the pH-V curve, you can find the exact value corresponding to the titrant halfway between the end point and the titration endpoint. The corresponding pH value is the apparent pKa.
[0061] Powdering time: According to ASTM D5423-93 (2005), the time required for 10% of the surface of the test specimen to crack or powder is 10% in an oven with an air exchange rate of 5-20 times / hour and a temperature setting of 150°C.
[0062] Flame retardant failure time: According to ASTM D5423-93 (2005), an oven with an air exchange rate of 5-20 times / hour and a temperature set to 150°C was used to bake combustion specimens with dimensions of 125mm×13mm×1.6mm and 125mm×13mm×3.2mm. The combustion specimens were then periodically extracted and tested for flame retardancy according to UL94-2016. The first flame time during the UL94 test was recorded as t1, and the second flame time was t2. The shorter t1+t2, the better the combustion performance. Flame retardant failure was judged based on the ∑(t1+t2) time of the five specimens tested according to UL94. A time greater than 250 seconds was considered a flame retardant failure.
[0063] Yellowing index: Set the temperature of a 160-ton injection molding machine to 190°C, allow the material to remain in the single screw for 3 minutes, and injection mold a 100 mm × 100 mm × 2.00 mm square plate. Test the yellowing index in accordance with HG / T 3862-2006, Test Method for Yellowness Index of Plastics.
[0064] Table 1. Formula of Examples 1-8 (parts by weight)
[0065] Table 2. Performance test results of Examples 1-8
[0066] Table 3. Comparative Examples 1-8 formulations (parts by weight)
[0067] Table 4. Performance test results of comparative examples 1-8
[0068] The polypropylene composition provided by the present invention has a powdering time of more than 550 hours, a powdering flame retardant performance @1.60mm of less than 28 seconds, a powdering flame retardant performance @3.20mm of less than 46 seconds, and a yellowing index of less than 30. It has the advantages of high-temperature failure resistance, a long powdering time, and is not prone to discoloration during processing.
[0069] Compared with Example 1, Comparative Examples 1 and 2 have too little amount of flame retardant synergist used in Comparative Example 1, resulting in a shorter powdering time, powdering flame retardant failure, longer flame retardant failure time @1.60 mm and flame retardant failure time @3.20 mm, and an increased yellowing index. The amount of flame retardant synergist used in Comparative Example 2 exceeds the upper limit, resulting in a shorter powdering time, longer flame retardant failure time @1.60 mm, and an increased yellowing index.
[0070] Compared with Example 1, Comparative Example 3 did not add a flame retardant synergist, and Comparative Example 3 failed to pulverize and flame retardant.
[0071] Compared with Example 1, Comparative Example 4 does not add hindered amine light stabilizer. The powdering time of Comparative Example 4 is shortened and the yellowing index is increased.
[0072] Compared with the examples, the comparative examples 5 and 6 use inappropriate flame retardant synergists, resulting in failure of high-temperature flame retardancy, easy powdering, and increased yellowing index in the comparative examples 5 and 6.
[0073] Compared with Example 3, Comparative Example 7 is different in that the pKa of the hindered amine light stabilizer used in Comparative Example 7 exceeds 8.1, the powdering time of Comparative Example 7 is shortened, the powdering flame retardant fails, and the yellowing index increases.
[0074] Comparing Comparative Example 8 with Example 1, while no flame retardant synergist was added, the total amount of hindered amine material remained unchanged. It can be seen that Comparative Example 8 is prone to flame retardant failure. The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention are intended to be included within the scope of protection of the present invention.
Claims
1. A polypropylene composition, characterized in that By weight, it includes the following components: The flame retardant synergist is one or more N-substituted alkoxy hindered amines; and the pKa value of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is less than 8.
1.
2. The polypropylene composition according to claim 1, characterized in that The polypropylene is selected from one or more of homopolymer polypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer and propylene-1-butene random block, and the polypropylene melt flow rate is 8-18g / 10min.
3. The polypropylene composition according to claim 2, characterized in that The N-substituted alkoxy hindered amine is one or more of tris(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl)phosphite, bis(1-methoxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate or bis(1-alkoxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate.
4. The polypropylene composition according to claim 1, characterized in that The primary antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl 4-hydroxyphenyl) propionate] pentaerythritol ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2.6-dimethylbenzyl) isocyanurate, ethylene bis(ethylene oxide)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl) propionate] and 3,9-bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl) propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane.
5. The polypropylene composition according to claim 1, characterized in that The auxiliary antioxidant is one or more of 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, triethylene glycol bis-β-(3-tert-butyl-4-hydroxy-5-methylphenyl), pentaerythritol bis(diphosphite)(2,4-tert-butylphenyl) ester or thioester antioxidant.
6. The polypropylene composition according to claim 5, characterized in that The thioester antioxidant is at least one of dialkyl esters of thiodipropionic acid or pentaerythritol tetrakis (3-laurylthiopropionate).
7. The polypropylene composition according to claim 1, characterized in that The brominated flame retardant is one or more of tris(tribromoneopentyl) phosphate, tetrabromobisphenol A-bis(2,3-dibromopropyl) ether, tris(2,3-dibromopropyl) isocyanurate, tetrabromobisphenol S-bis(2,3-dibromopropyl) ether, melamine hydrobromide and 1,2-bis(pentabromophenyl)ethane.
8. The polypropylene composition according to any one of claims 1 to 7, characterized in that The general structural formula of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is: Wherein, X is CH3, -CH2CH3, -OCHCH3 or 9. The polypropylene composition according to any one of claims 1 to 7, characterized in that The structure of the hindered amine light stabilizer other than the N-substituted alkoxy hindered amine is: The CAS number is 65447-77-0.
10. A method for preparing a polypropylene composition according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1: According to the ratio, weigh and pre-mix the components to obtain a premix; S2: putting the premix of step S1 into an extruder, performing melt blending and extrusion granulation to obtain the polypropylene composition.
11. Use of the polypropylene composition according to any one of claims 1 to 9 in the preparation of vehicles and household appliances.
Citation Information
Patent Citations
Flame-retardant polypropylene compound for sanitary ware product
CN101759930A
Polypropylene resin composition and molded article made thereof
CN101903464A
Polypropylene resin composition and molded article
CN101939374A
Flame retardant polypropylene material with good light stability and preparation method thereof
CN108659339A
Flame-retardant polypropylene material with good photothermal stability and preparation method of flame-retardant polypropylene material
CN109867860A
Cited By