Plastic-carbon material based on waste plastic reuse, method for preparing same, and use thereof

By mixing waste plastic with ferric chloride for freeze-drying and pyrolysis, a high yield and strong adsorption plastic carbon material was prepared, which solved the environmental pollution caused by the use of organic solvents in the prior art, and improved the water intake The adsorption performance of bisphenol A realizes resource reuse and environmental protection of waste plastics.

WO2024230581A1PCT designated stage expired Publication Date: 2024-11-14KUNMING UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090803
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-06
Filing Date
2024-04-30
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The prior art has the risk of environmental pollution caused by using organic solvents when removing endocrine disturbances in water, and is only for the carbonization of waste plastics containing cyano groups, and cannot effectively treat other types of waste plastics.

Method used

Use water instead of organic solvents to mix waste plastics such as polyethylene, polypropylene, polyethylene terephthalate with iron trichloride, and freeze-dry and pyrolysis to prepare high-yield and strong adsorption plastic carbon Material, used to adsorb bisphenol A in water.

Benefits of technology

Reuse of waste plastics without the use of toxic reagents or organic solvents is achieved, reducing the risk of environmental pollution, improving the yield of plastic carbon materials and adsorption performance of bisphenol A, and the process is simple and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024090803_14112024_PF_FP_ABST
    Figure CN2024090803_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the field of wastewater treatment technology, and in particular, to a plastic-carbon material based on waste plastic reuse, a method for preparing same, and use thereof. The method comprises the following steps: mixing a treated waste plastic particle with ferric trichloride, and after adding water, lyophilizing the mixture; and pyrolyzing the lyophilized mixture to give the plastic-carbon material. The waste plastic particle is at least one of polyethylene, polypropylene, polyethylene terephthalate, and polymethyl methacrylate. The method features ease to operate, fewer procedures, cost-efficiency, high yield, and good bisphenol A adsorption performance, and avoids the use of toxic reagents or organic solvents, thus achieving waste plastic reuse and environment conservation.
Need to check novelty before this filing date? Find Prior Art

Description

A plastic carbon material based on waste plastic recycling and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 6, 2023, with application number CN202310504063.X and invention name “A plastic carbon material based on waste plastic recycling and its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application belongs to the field of wastewater treatment technology, and specifically relates to a plastic carbon material based on the recycling of waste plastics, and a preparation method and application thereof. Background Art

[0003] Endocrine disrupting chemicals (EDCs) are environmental pollutants widely present in human life. They affect the human endocrine system through environmental exposure or dietary intake, interfering with the synthesis, secretion, and ultimately metabolic elimination of endocrine hormones required for maintaining internal homeostasis. BPA, one of these EDCs, is widely used in the manufacture of plastics such as polycarbonate and epoxy resin. It is reported to be widely distributed in soil, air, sediment, and water. It is difficult to biodegrade and highly resistant to chemical degradation. It can also accumulate in organisms through the food chain, posing a serious threat to the ecological environment and human health. Currently, EDC removal technologies primarily include adsorption, advanced oxidation processes, and biological methods. Adsorption, due to its simplicity, low energy consumption, high efficiency, and lack of secondary pollution, is considered one of the most direct, widely used, effective, and economical methods for removing organic pollutants from water. Carbon materials, due to their low cost, have long been considered an ideal solid adsorbent.

[0004] Plastics are essential synthetic materials used in industrial production and daily life. Global plastic production has increased from 1.5 million tons in the 1950s to 335 million tons in 2016, and reached 348 million tons in 2017, with an annual growth rate of approximately 5%. Research shows that 79% of plastic products are not properly processed, ultimately ending up in landfills or the natural environment. The recalcitrant nature of plastic waste and its incineration lead to severe pollution of water, air, soil, and oceans, directly posing a threat to human health.

[0005] Patent CN201610363150.8 discloses a method for preparing adsorption materials by carbonizing plastics or waste plastics. The plastics or waste plastics are dissolved in an organic solvent and pyrolyzed and carbonized under the action of a catalyst to obtain the adsorption material. However, the above patent introduces an organic solvent, which poses a risk of environmental pollution and is only targeted at the carbonization treatment of waste plastics containing cyanide groups.

[0006] Summary of the Invention

[0007] To address the shortcomings of the above-mentioned prior art, the present application provides a plastic carbon material based on the recycling of waste plastics, as well as a preparation method and application. The present application uses water instead of organic solvents with environmental risks to carbonize waste plastics such as polyethylene, polypropylene, polyethylene terephthalate, and polymethyl methacrylate to obtain a plastic carbon material with high yield and strong adsorption properties.

[0008] To achieve the above objectives, the technical solutions adopted in this application are:

[0009] A method for preparing a plastic carbon material based on the recycling of waste plastics comprises the following steps: mixing treated waste plastic particles with ferric chloride, adding water and freeze-drying the mixture; then pyrolyzing the freeze-dried mixture to obtain a plastic carbon material; the waste plastic particles are at least one of polyethylene, polypropylene, polyethylene terephthalate and polymethyl methacrylate.

[0010] As a preferred embodiment of the present application, the mass ratio of the waste plastic particles to ferric chloride is 1-5:1.

[0011] Mixing plastic particles and FeCl3 in different weight ratios will have different effects on the pyrolysis process. The degree of graphitization of the plastic carbon after pyrolysis increases with the decrease of iron addition, which leads to a decrease in the adsorption performance of the material.

[0012] More preferably, the mass ratio of the waste plastic particles to ferric chloride is 1:1.

[0013] In the preparation method described in the present application, the amount of water added is sufficient to submerge the ferric chloride and the plastic particles.

[0014] As a preferred embodiment of the present application, the treated waste plastic particles are waste plastic particles that have been washed with water and then dried, and the drying temperature is 60°C.

[0015] As a preferred embodiment of the present application, the pyrolysis temperature is 700° C., the time is 4 hours, the heating rate to the pyrolysis temperature is 5° C. / min, and the pyrolysis is carried out under a nitrogen atmosphere.

[0016] As a preferred embodiment of the present application, the pyrolysis is carried out in a tube furnace.

[0017] As a preferred embodiment of the present application, after the pyrolysis, the method further comprises: grinding and filtering the pyrolysis products in sequence; the filtration is performed through a 200-mesh sieve.

[0018] As a preferred embodiment of the present application, before the freeze-drying, the method further comprises: continuously stirring the mixture of the waste plastic particles, ferric chloride and water for 24 hours.

[0019] As a preferred embodiment of the present application, the freeze-drying temperature is -40°C, and the freeze-drying time is 72 hours.

[0020] As a preferred embodiment of the present application, the yield of the plastic carbon material is 12.1%, 11.1%, 14.3%, 10.1%, 15.6% or 9.8%.

[0021] This application also claims protection for the plastic carbon material prepared by the preparation method described in the above technical solution.

[0022] This application also claims protection for the use of the plastic carbon material described in the above technical solution in adsorbing bisphenol A in water.

[0023] As a preferred embodiment of the present application, the application method is: adding the plastic carbon material into water containing bisphenol A for adsorption.

[0024] As a preferred embodiment of the present application, the adsorption is carried out under oscillation conditions; the rotation speed of the oscillation is 180 rpm.

[0025] As a preferred embodiment of the present application, the adsorption temperature is 25° C.; and the adsorption time is 24 h.

[0026] As a preferred embodiment of the present application, the pH value of the water containing bisphenol A is 7.

[0027] As a preferred embodiment of the present application, the concentration of bisphenol A in the bisphenol A-containing water is 5 mg / L, 10 mg / L, 15 mg / L, 25 mg / L, 50 mg / L or 75 mg / L.

[0028] As a preferred embodiment of the present application, the dosage of the plastic carbon material in the water containing bisphenol A is 0.1 mg / mL.

[0029] As a preferred embodiment of the present application, the 24-hour unit mass adsorption capacity of bisphenol A by the plastic carbon material is 6.21 mg / g, 14.55 mg / g, 34.47 mg / g, 16.77 mg / g, 35.29 mg / g or 5.92 mg / g.

[0030] As a preferred embodiment of the present application, the maximum adsorption capacity of the plastic carbon material for bisphenol A is 29.27 mg / g, 15.98 mg / g, 65.77 mg / g, 26.61 mg / g, 52.39 mg / g or 15.36 mg / g.

[0031] The working principle of ferric chloride in the preparation of plastic carbon materials:

[0032] The present application uses ferric chloride to pyrolyze plastic particles. On the one hand, the surface morphology of the plastic particles is destroyed, the pyrolysis temperature is maintained at 700°C, the flaky substances disappear and a flower-like structure is formed, which greatly increases the specific surface area of ​​the plastic carbon material and the formation of some Fe crystal cluster particles is easily observed on its surface, indicating that Fe has a strong binding force with the plastic particles. On the other hand, the presence of iron reduces the number of strong absorption bands, but absorption bands attributable to aromatic C=C, C=O or C=O carboxyl groups, CO and COC and Fe=O bonds appear, indicating that Fe accelerates the normalization of functional groups. Based on the above two aspects, ferric chloride is bound to the surface of plastic carbon through interaction with the functional groups on the surface of plastic carbon, resulting in a high yield of plastic carbon material and strong adsorption of bisphenol A.

[0033] Compared with the existing technology, the beneficial effects of the present application are: the preparation method of plastic carbon material based on the recycling of waste plastics is simple and easy to operate, with fewer process steps. It not only has a wide source of materials, low cost, high product yield, and good adsorption performance for bisphenol A, but also does not require the use of toxic reagents or organic solvents in the process, thereby realizing the resource recycling of waste plastics and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a scanning electron microscope image of the plastic carbon materials prepared in Examples 1-6 of the present application; wherein (a) is the plastic carbon material prepared in Example 1, denoted as PE-Fe; (b) is the plastic carbon material prepared in Example 2, denoted as PP-Fe; (c) is the plastic carbon material prepared in Example 3, denoted as PET-Fe; (d) is the plastic carbon material prepared in Example 4, denoted as PMMA-Fe; and (e) is the plastic carbon material prepared in Example 5, denoted as mixed carbon-Fe.

[0035] FIG2 shows the adsorption capacity of bisphenol A by the plastic carbon materials described in Examples 1-5 at different adsorption times and the fitting curves of pseudo-first-order and pseudo-second-order kinetic models.

[0036] FIG3 shows the changes in the adsorption capacity of the plastic carbon materials described in Examples 1-5 for bisphenol A at different initial concentrations, as well as the fitting curves of the Langmuir isotherm model and the Freundlich isotherm model. DETAILED DESCRIPTION

[0037] In order to better illustrate the purpose, technical solutions and advantages of this application, this application will be further described below in conjunction with specific embodiments.

[0038] Example 1

[0039] This embodiment provides a method for preparing a plastic carbon material based on recycling waste plastics, comprising the following steps:

[0040] (1) The waste polyethylene plastic particles were washed several times with ultrapure water and then dried at 60°C;

[0041] (2) mixing the waste polyethylene plastic particles treated in step (1) with ferric chloride in a mass ratio of 1:1, adding ultrapure water and stirring continuously for 24 hours, and then freeze-drying at -40°C for 72 hours;

[0042] (3) The freeze-dried mixture was heated to 700 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and pyrolyzed for 4 h. The mixture was then ground and sieved using a 200-mesh sieve to obtain a plastic carbon material labeled PE-Fe.

[0043] Example 2

[0044] The only difference between the preparation method of plastic carbon material based on waste plastic recycling described in this embodiment and that in Example 1 is that the waste polyethylene plastic particles in step (1) are replaced with polyethylene plastic particles, and the obtained plastic carbon material is labeled PP-Fe.

[0045] Example 3

[0046] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this embodiment and that in Example 1 is that the waste polyethylene plastic particles in step (1) are replaced with polyethylene terephthalate plastic particles, and the obtained plastic carbon material is labeled PET-Fe.

[0047] Example 4

[0048] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this embodiment and that in Example 1 is that the waste polyethylene plastic particles in step (1) are replaced with polymethyl methacrylate plastic particles, and the obtained plastic carbon material is labeled PMMA-Fe.

[0049] Example 5

[0050] The only difference between the preparation method of plastic carbon material based on waste plastic recycling described in this embodiment and Example 1 is that the waste polyethylene plastic particles in step (1) are replaced by a mixture of four plastic particles of polyethylene, polypropylene, polyethylene terephthalate and polymethyl methacrylate, and the obtained plastic carbon material is labeled mixed carbon-Fe; the mass ratio of polyethylene, polypropylene, polyethylene terephthalate and polymethyl methacrylate is 1:1:1:1.

[0051] Example 6

[0052] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this embodiment and that in Example 1 is that in step (2), the waste polyethylene plastic particles treated in step (1) are mixed with ferric chloride in a mass ratio of 5:1 to obtain a plastic carbon material labeled PE-Fe-0.

[0053] Comparative Example 1

[0054] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this comparative example and that in Example 1 is that the waste polyethylene plastic particles in step (1) are replaced by ABS plastic, and the obtained plastic carbon material is labeled ABS-Fe; ABS plastic is a ternary copolymer of three monomers: acrylonitrile, butadiene, and styrene.

[0055] Comparative Example 2

[0056] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this comparative example and that in Example 1 is that the ferric chloride in step (2) is replaced by zinc chloride, and the obtained plastic carbon material is labeled PE-Zn.

[0057] Comparative Example 3

[0058] The method for preparing the plastic carbon material based on the recycling of waste plastics described in this comparative example comprises the following steps:

[0059] (1) The waste polyethylene plastic particles were washed several times with ultrapure water and then dried at 60°C;

[0060] (2) mixing the waste polyethylene plastic particles treated in step (1) with ferric chloride in a mass ratio of 1:1, adding ultrapure water, stirring continuously for 24 hours, and then drying at 60°C;

[0061] (3) The dried mixture was heated to 700 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and pyrolyzed for 4 h, then ground and sieved using a 200-mesh sieve to obtain a plastic carbon material labeled PE-Fe-1.

[0062] Comparative Example 4

[0063] The method for preparing the plastic carbon material based on the recycling of waste plastics described in this comparative example comprises the following steps:

[0064] (1) The waste polyethylene plastic particles were washed several times with ultrapure water and then dried at 60°C.

[0065] (2) Mixing the waste polyethylene plastic particles treated in step (1) with ferric chloride in a mass ratio of 1:1 to obtain a mixture.

[0066] (3) The mixture was heated to 700 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and pyrolyzed for 4 h. The mixture was then ground and sieved using a 200-mesh sieve to obtain a plastic carbon material labeled PE-Fe-2.

[0067] Comparative Example 5

[0068] The only difference between the preparation method of the plastic carbon material based on the recycling of waste plastics described in this comparative example and that in Example 1 is that in step (2), the waste polyethylene plastic particles treated in step (1) are mixed with ferric chloride in a mass ratio of 6:1 to obtain a plastic carbon material labeled PE-Fe-3.

[0069] Test Example 1

[0070] To explore the adsorption amount and adsorption equilibrium time of plastic carbon materials at different adsorption times, this test example used the plastic carbon materials obtained in Examples 1-6 and Comparative Examples 1-5 to adsorb bisphenol A in water, specifically comprising the following steps:

[0071] S1: Prepare a 10 mg / L bisphenol A solution, and add 0.1 M NaOH and 0.1 M HCl to adjust the pH to 7.

[0072] S2: Weigh 5 mg of each of the plastic carbon materials prepared in Examples 1-6 and Comparative Examples 1-5, place them in a brown glass bottle, and set up three parallel samples at different adsorption times.

[0073] S3: Add 50 mL of bisphenol A solution to the brown glass bottle containing the sample in S2, and place it in a shaker at 25°C for adsorption. The adsorption time is 0, 1, 2, 4, 6, 20, 14, and 24 h at a rotation speed of 180 rpm.

[0074] S4: After the adsorption is completed, 1 mL of the adsorbed solution is taken and centrifuged at 16,000 rpm for 5 min. The supernatant is taken for detection by high performance liquid chromatography. The concentration of the adsorbed solution is obtained from the standard curve. Then, according to the change in the concentration of the solution before and after adsorption, the adsorption amount of bisphenol A by the plastic carbon material at different adsorption times is calculated using formula (1).

[0075] In formula (1), t is the adsorption time, in h; Q t is the adsorption capacity per unit mass of adsorbent at time t, in mg g -1 ; C0 and C t are the initial concentration of bisphenol A in the solution and the concentration at time t, respectively, in mg·L -1 ; V is the volume of the solution, in L; m is the amount of plastic carbon material added, in g.

[0076] S5: Fitting the kinetic data using pseudo-first-order and pseudo-second-order kinetic equations:

[0077] Pseudo-first-order kinetic equation:

[0078] Pseudo-second-order kinetic equation:

[0079] In formulas (2) and (3), t is the adsorption time in h; Q e is the adsorption capacity per unit mass of adsorbent at adsorption equilibrium, in mg g -1 ;Q t is the adsorption amount in time t, in mg·L -1 ; k1 and k2 are the adsorption rate constants of pseudo-first-order kinetic equation and pseudo-second-order kinetic equation respectively, and the unit of k1 is h -1 , k2 unit is g·mg -1 ·h -1 .

[0080] As can be seen from Figure 1, the surface of the plastic carbon material is uneven, rough, with obvious wrinkles and layered structures and a relatively dense distribution, providing a considerable number of adsorption sites for the adsorption reaction to occur.

[0081] As shown in Figure 2, the adsorption of bisphenol A by plastic carbon material basically reaches adsorption equilibrium after about 24 hours of contact. The nonlinear fitting curves of pseudo-first-order and pseudo-second-order equations are shown in Figure 2 and Table 1. It can be seen from the calculation that the correlation coefficient (R) of the pseudo-second-order adsorption kinetic equation of bisphenol A by plastic carbon material is 2 ) are all greater than pseudo-first-order kinetics, which shows that it is reliable to use the pseudo-second-order adsorption kinetics equation to simulate and analyze the removal rate of bisphenol A by plastic carbon materials.

[0082] Table 1 Nonlinear fitting curve data of pseudo-first-order and pseudo-second-order equations for adsorption of bisphenol A by plastic carbon materials in Examples 1-5

[0083] Table 2 Comparison of the adsorption capacity per unit mass of the plastic carbon materials of Examples 1-6 and Comparative Examples 1-5 in 24 hours and the yield of the plastic carbon materials prepared

[0084] According to Table 2, the yield and adsorption capacity of the plastic carbon materials of Examples 1-6 are better than those of the materials prepared in the comparative example, indicating that the preparation method described in the present application has a high yield, is simple to prepare, and can be produced on a large scale. Combined with the better adsorption effect on bisphenol A, the recycling of waste plastics can be combined with the removal of bisphenol A in water bodies, making a greater contribution to the environment.

[0085] Test Example 2

[0086] To explore the adsorption of bisphenol A solutions with different concentrations by plastic carbon materials, this test example used the plastic carbon materials obtained in Examples 1-6 and Comparative Examples 1-5 to adsorb bisphenol A in water, specifically comprising the following steps:

[0087] S1: Prepare bisphenol A solutions of different concentrations, and add 0.1 M NaOH and 0.1 M HCl to adjust the pH to 7; the concentrations of bisphenol A solutions are 5, 10, 15, 25, 50, and 75 mg / L, respectively.

[0088] S2: Weigh 5 mg of each of the plastic carbon materials prepared in Examples 1-6 and Comparative Examples 1-5, place them in a brown glass bottle, and set up two parallel samples under different concentrations of bisphenol A solution.

[0089] S3: Add 50 mL of bisphenol A solution to the brown glass bottle containing the sample in S2, and place it in a shaker at 25°C for 24 hours at a rotation speed of 180 rpm.

[0090] S4: After the adsorption is completed, 1 mL of the adsorbed solution is taken and centrifuged at 16,000 rpm for 5 min. The supernatant is taken for detection by high performance liquid chromatography. The concentration of the adsorbed solution is obtained from the standard curve. Then, according to the change in the concentration of the solution before and after adsorption, the adsorption amount of bisphenol A by the plastic carbon material at different adsorption times is calculated using formula (1).

[0091] In formula (4), Q e is the equilibrium adsorption capacity of bisphenol A, in mg g -1 ; C e is the solution concentration at adsorption equilibrium, expressed in mg·L -1 ; C0 is the initial concentration of bisphenol A in the solution, in mg·L -1 ; V is the volume of the solution, in L; m is the amount of plastic carbon material added, in g.

[0092] S5: Nonlinear fitting of the isotherm data was performed using the Langmuir isotherm model and the Freundlich isotherm model. The equations for each model are as follows:

[0093] Langmuir isotherm model:

[0094] Freundlich isotherm model:

[0095] In formulas (5) and (6), Q e is the equilibrium adsorption capacity of bisphenol A, in mg g -1 ; C eis the solution concentration at adsorption equilibrium, expressed in mg·L -1 ;K L is the Langmuir isotherm adsorption constant, in L·mg -1 ;K F and n are the Freundlich equation constant and dimensionless constant respectively, K F Unit is (mg / g)(L / mg) 1 / n ;Q m The theoretical maximum adsorption capacity, in mg g -1 .

[0096] According to Figure 3, the fitting curves of the Langmuir isotherm adsorption model and the Freundlich isotherm adsorption model are shown in Figure 3 and Table 3. As the concentration of bisphenol A in the mixed system continues to increase, the adsorption amount of bisphenol A by the plastic carbon material also increases. The correlation coefficient of the Freundlich model (R 2 ) is less than the correlation coefficient of the Langmuir model, which shows that the Langmuir model is a better fit for the results of the adsorption of bisphenol A by plastic carbon materials than the Freundlich model. Through Langmuir fitting, it can be seen that the maximum adsorption capacity Q of bisphenol A by plastic carbon materials is m It is 71.55 mg / g; this shows that plastic carbon materials can be well used in the removal of bisphenol A.

[0097] Table 3 Langmuir isotherm adsorption model and Freundlich isotherm adsorption model fitting curve data of bisphenol A adsorption on plastic carbon materials of Examples 1-5

[0098] Table 4 Comparison of the maximum adsorption capacity of the plastic carbon materials of the embodiment and the comparative example

[0099] According to Table 4, the maximum adsorption capacity of the plastic carbon materials of Examples 1-6 is better than that of the materials prepared in the comparative examples, indicating that the plastic carbon materials prepared by the preparation method described in the present application have excellent adsorption properties for bisphenol A. According to Tables 2 and 4, compared with Example 1 and Comparative Example 1, the adsorption performance and yield of Comparative Example 1 are relatively low because ABS is an amorphous polymer with a very smooth surface and poor thermal decomposition with ferric chloride, so the yield is low, and the PE plastic used in this application is more widely used and has greater research significance. Compared with Example 1 and Comparative Example 2, the adsorption performance and yield of Comparative Example 2 are relatively low because PE-Zn is an amorphous material composed of graphite-like crystallites, and when the pyrolysis temperature is maintained at 700°C, part of the ferric chloride in the ferric chloride-modified plastic carbon will produce zero-valent iron, which has strong reducibility and a large specific surface area and has better adsorption properties and reactivity for organic pollutants. According to Comparative Example 3 and Example 1, the adsorption performance and yield of Comparative Example 3 are relatively low, because after ferric chloride and plastic granule mixture are refrigerated and dried, the two degrees of combination are better than drying, and pyrolysis yield is also higher. According to Comparative Example 4 and Example 1, the adsorption performance and yield of Comparative Example 4 are relatively low, because directly by the two mixtures pyrolyzed, part of plastics can be taken out of tubular furnace along with nitrogen gas flow, and adding water and refrigerating can better make ferric chloride and plastic granule fixed together, reach higher yield and better adsorption performance. According to Comparative Example 4 and Example 1,6, the mass ratio of ferric chloride and plastic granule has a larger impact on the yield and adsorption performance of plastic carbon material, and the mass ratio of ferric chloride and plastic granule is within the application's limited range, and prepared plastic carbon material has good yield and adsorption performance.

[0100] Although the above embodiment provides a detailed description of the present application, it is only a part of the embodiments of the present application rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present application.

Claims

1. A method for preparing plastic carbon materials based on the recycling of waste plastics, characterized in that: The method comprises the following steps: mixing treated waste plastic particles with ferric chloride, adding water and freeze-drying the mixture; then pyrolyzing the freeze-dried mixture to obtain plastic carbon material; the waste plastic particles are at least one of polyethylene, polypropylene, polyethylene terephthalate and polymethyl methacrylate.

2. The preparation method according to claim 1, characterized in that The mass ratio of the waste plastic particles to ferric chloride is 1-5:

1.

3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the waste plastic particles to ferric chloride is 1:

1.

4. The preparation method according to claim 1, characterized in that: The treated waste plastic particles are waste plastic particles that have been washed with water and then dried; the drying temperature is 60°C.

5. The preparation method according to claim 1, characterized in that: The pyrolysis temperature is 700° C., the time is 4 hours, the heating rate to the pyrolysis temperature is 5° C. / min, and the pyrolysis is carried out in a nitrogen atmosphere.

6. The preparation method according to claim 1, characterized in that: After the pyrolysis, the method further comprises: grinding and filtering the pyrolysis products in sequence; the filtering is performed through a 200-mesh screen.

7. The preparation method according to claim 1, characterized in that: Before the freeze drying, the method further comprises: continuously stirring the mixture of the waste plastic particles, ferric chloride and water for 24 hours.

8. The preparation method according to claim 1, characterized in that: The freeze-drying temperature is -40°C, and the freeze-drying time is 72h.

9. The preparation method according to claim 1, characterized in that: The yield of the plastic carbon material is 12.1%, 11.1%, 14.3%, 10.1%, 15.6% or 9.8%.

10. The plastic carbon material prepared by the preparation method according to any one of claims 1 to 9.

11. Use of the plastic carbon material according to claim 10 in adsorbing bisphenol A in water.

12. The use according to claim 11, characterized in that The application method is: adding the plastic carbon material into a water body containing bisphenol A for adsorption.

13. The use according to claim 12, characterized in that The adsorption was carried out under shaking conditions; the shaking speed was 180 rpm.

14. The use according to claim 12, characterized in that The adsorption temperature is 25° C. and the adsorption time is 24 h.

15. The use according to claim 12, characterized in that The pH value of the bisphenol A-containing water body is 7.

16. The use according to claim 12, characterized in that The concentration of bisphenol A in the bisphenol A-containing water is 5 mg / L, 10 mg / L, 15 mg / L, 25 mg / L, 50 mg / L or 75 mg / L.

17. The use according to claim 12, characterized in that The dosage of the plastic carbon material in the water containing bisphenol A is 0.1 mg / mL.

18. The use according to claim 12, characterized in that The 24-hour unit mass adsorption capacity of bisphenol A by the plastic carbon material is 6.21 mg / g, 14.55 mg / g, 34.47 mg / g, 16.77 mg / g, 35.29 mg / g or 5.92 mg / g.

19. The use according to claim 12, characterized in that The maximum adsorption capacity of the plastic carbon material for bisphenol A is 29.27 mg / g, 15.98 mg / g, 65.77 mg / g, 26.61 mg / g, 52.39 mg / g or 15.36 mg / g.

Citation Information

Patent Citations

  • Activated carbon material for efficiently removing flame retardant organic pollutants in water as well as preparation method and application of activated carbon material

    CN114307959A

  • Plastic carbon material based on waste plastic recycling as well as preparation method and application of plastic carbon material

    CN116272874A

  • Method for efficiently removing bisphenol pollutants from water body and compound biochar material

    EP4166509A1