Ultrahigh-strength aluminum alloy material and processing method therefor, and extrusion component

By optimizing the alloy composition and processing technology of aluminum alloy materials, high-density Mg2Si nano-precipitation phase and fibrous structure are formed, which solves the problem of difficulty in taking into account the strength and toughness of conventional 6000 series aluminum alloy materials, and achieves ultra-high strength and high toughness Aluminum alloy materials meet the needs of the automotive industry.

WO2024230780A1PCT designated stage expired Publication Date: 2024-11-14BEIJING CHEHEJIA AUTOMOBILE TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/091977
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-09
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The strength and toughness of conventional 6000 series aluminum alloy materials are difficult to take into account, and cannot meet the needs of the automotive industry for high strength and high toughness.

Method used

By optimizing the alloy composition and processing technology of aluminum alloy materials, the density of Mg2Si nano-precipitation phase is increased, and fibrous tissue is formed through high-temperature extrusion and aging treatment, thereby improving the tensile strength and bending angle of the material.

Benefits of technology

The tensile strength of aluminum alloy materials reaches more than 400MPa and improves toughness, meeting the automotive industry's demand for high strength and high toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024091977_14112024_PF_FP_ABST
    Figure CN2024091977_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides an ultrahigh-strength aluminum alloy material and a processing method therefor, and an extrusion component. The ultrahigh-strength aluminum alloy material, on the basis that the mass of aluminum alloy material is 100 wt.%, comprises: 0.8-1.2 wt.% of Si; 0.1-0.3 wt.% of Fe; 0.3-0.7 wt.% of Cu; 0.4-0.8 wt.% of Mn; 0.8-1.2 wt.% of Mg; 0.05-0.2 wt.% of Cr; 0.01-0.1 wt.% of Ti; 0.01-0.2 wt.% of V; and the balance of Al.
Need to check novelty before this filing date? Find Prior Art

Description

Ultra-high strength aluminum alloy material, processing method thereof, and extruded component

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on the Chinese patent application with application number 202310532228.4 and application date May 11, 2023, and claims the priority of the Chinese patent application. The entire content of the Chinese patent application is hereby introduced into this application as a reference. Technical Field

[0003] The present application relates to the technical field of metal materials, and in particular to ultra-high strength aluminum alloy materials, processing methods thereof, and extruded components. Background Art

[0004] Aluminum alloy extruded profiles have been widely used in the automotive industry, but the automotive industry currently mainly uses medium-strength 6000 series aluminum profiles. Among them, the 6000 series aluminum profiles are aluminum-magnesium-silicon alloy series, which have excellent processing performance, excellent welding characteristics and electroplating properties, good corrosion resistance, high toughness and no deformation after processing, dense and defect-free materials and easy polishing, easy color film, and excellent oxidation effect.

[0005] At present, the 6000 series aluminum profiles used in automobiles mainly include alloys such as 6061 aluminum profiles, 6063 aluminum profiles and 6082 aluminum profiles. Among them, the yield strength of 6061 aluminum profiles is not less than 240MPa, the tensile strength is not less than 260MPa, and the elongation is not less than 7%; the bending angle is not less than 40°; the yield strength of 6063 aluminum profiles is not less than 170MPa, the tensile strength is not less than 215MPa, and the elongation is not less than 6%; the bending angle is not less than 120°; the yield strength of 6082 aluminum profiles is not less than 250MPa, the tensile strength is not less than 290MPa, the elongation is not less than 6%; the bending angle is not less than 80°. With the increasing demand for lightweight automobiles, the yield strength of high-strength aluminum profiles used in automobiles must be no less than 350MPa, the tensile strength must be no less than 400MPa, the elongation must be no less than 10%, and the bending angle must be no less than 60°; therefore, the performance of conventional 6000 series aluminum profiles can no longer meet the development needs of the automotive industry.

[0006] Therefore, there is an urgent need to redesign the alloy composition and preparation process parameters of conventional 6000 series aluminum alloy materials, significantly improve the mechanical properties and material toughness of 6000 series aluminum profiles, and provide better material selection solutions for lightweight automotive design.

[0007] Summary of the Invention

[0008] The present application aims to solve one of the technical problems in the related art at least to a certain extent.

[0009] To this end, this application proposes ultra-high strength aluminum alloy materials, processing methods and extruded components thereof. By optimizing the alloy composition and preparation process of conventional 6000 series aluminum profiles, an ultra-high strength 6000 series aluminum alloy with excellent comprehensive performance is obtained, so that its tensile strength is as high as 400MPa or more and it has strong toughness.

[0010] To achieve the above-mentioned object, according to a first aspect of the present application, an ultra-high strength aluminum alloy material is provided. Based on 100 wt.% of the mass of the aluminum alloy material, the aluminum alloy material comprises:

[0011] Si: 0.8-1.2wt.%;

[0012] Fe: 0.1-0.3wt.%;

[0013] Cu: 0.3-0.7wt.%;

[0014] Mn: 0.4-0.8wt.%;

[0015] Mg: 0.8-1.2wt.%;

[0016] Cr: 0.05-0.2wt.%;

[0017] Ti: 0.01-0.1wt.%;

[0018] V: 0.01-0.2 wt.%; the balance is Al.

[0019] In some embodiments, the aluminum alloy material comprises:

[0020] Si: 0.8-1.1wt.%;

[0021] Fe: 0.1-0.2wt.%;

[0022] Cu: 0.3-0.5wt.%;

[0023] Mn: 0.4-0.6wt.%;

[0024] Mg: 0.8-1.1wt.%;

[0025] Cr: 0.1-0.2wt.%;

[0026] Ti: 0.05-0.1wt.%;

[0027] V: 0.01-0.1wt.%.

[0028] In some embodiments, the aluminum alloy material further includes unavoidable impurities, the total amount of the impurities being ≤0.15 wt.%, wherein a single impurity is ≤0.05 wt.%.

[0029] In some embodiments, in the aluminum alloy material, 0.8≤Mg / Si≤1.5.

[0030] In some embodiments, in the aluminum alloy material, 1.0≤Mg / Si≤1.2.

[0031] According to a second aspect of the present application, a method for forming an extruded component from the aluminum alloy material described in any of the above embodiments is provided, comprising the following steps:

[0032] The raw materials are mixed according to the proportion of the aluminum alloy material, and are subjected to smelting, casting, homogenization heat treatment, extrusion shaping, and aging treatment to obtain an extruded component; wherein the metal structure of the extruded component is strictly restricted.

[0033] In some embodiments, the homogenization heat treatment is performed at a temperature of 500-580° C. and a holding time of 5-20 h.

[0034] In some embodiments, the extrusion molding is performed first by hot extrusion, and the extruded component is stretched and straightened after cooling; wherein the process parameters of the hot extrusion are: the extrusion outlet temperature is 530-580°C, and the extrusion ratio is ≥20.

[0035] In some embodiments, the process parameters of the aging treatment are: first, keep at 160-200° C. for 6-20 hours, and then air-cool to room temperature.

[0036] In some embodiments, the metal structure of the extruded component is strictly constrained as follows: the grain morphology of the extruded component is a fibrous structure along the extrusion direction.

[0037] According to a third aspect of the present application, an extruded component is provided that is formed by the processing method described in any one of the above embodiments.

[0038] In some embodiments, the extruded component has a yield strength of at least 350 MPa, a tensile strength of at least 400 MPa, an elongation of at least 10%, and a bend angle of at least 60°.

[0039] This application addresses the problem that it is difficult to strike a balance between the strength and toughness of conventional 6000 series aluminum profiles. On the one hand, the composition of conventional 6000 series aluminum alloy materials is optimized, and the technical feature of conventional 6000 series aluminum profiles that strengthens the material through nano-sized Mg2Si precipitation phase is changed. This application promotes the transformation of Mg2Si nano-precipitation phase into Q phase (Mg-Si-Cu) with better strengthening effect, thereby greatly improving the strength of the material. In addition, this application reduces the impact of impurities on the corrosion resistance and toughness of aluminum alloys by controlling the content of unavoidable impurities, and optimizes the strength, corrosion resistance and high toughness of aluminum alloy materials. On the other hand, based on the optimization of the composition of aluminum alloy materials, this application improves the processing method of conventional 6000 series aluminum alloys; through higher extrusion temperatures, alloying elements such as Mg, Si, and Cu are dissolved into the aluminum alloy matrix, ensuring the high strength of the extruded parts generated by the aluminum alloy material; and through a larger extrusion ratio, the compounds and coarse grains formed during the casting process improve the toughness of the extruded parts.

[0040] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:

[0042] FIG1 is a processing method for forming an extruded component from an aluminum alloy according to an embodiment of the present application;

[0043] FIG2 is a diagram showing the metal structure grain morphology of the extruded component proposed in Example 1 of the present application;

[0044] FIG3 is a diagram showing the metal structure grain morphology of the extruded component proposed in Comparative Example 1 of the present application;

[0045] FIG4 is a diagram of a tensile test sample of a metal material proposed in an embodiment of the present application. DETAILED DESCRIPTION

[0046] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described in detail below with reference to the following embodiments. It is apparent that the embodiments described are only a portion of the embodiments of this application, rather than all of them. All other technical solutions derived by those of ordinary skill in the art based on the embodiments in this application are intended to fall within the scope of protection of this application.

[0047] This application proposes an ultra-high-strength aluminum alloy material, a processing method thereof, and an extruded component. By optimizing the alloy composition and preparation process of conventional 6000 series aluminum alloy profiles, an ultra-high-strength 6000 series aluminum alloy with excellent comprehensive performance is obtained, so that its tensile strength is as high as 400 MPa or more and it has strong toughness.

[0048] To achieve the above objectives, this application is implemented through the following aspects:

[0049] By controlling the content and ratio of alloying elements such as Mg, Si, Cu, and Mn, as well as strictly controlling the processing parameters, the density and strengthening capacity of the nano-sized Q-phase (Mg-Si-Cu) precipitation strengthening phase within the extruded component formed by the aluminum alloy material are increased, thereby significantly improving the strength of the extruded component. By strictly controlling the impurity elements in the aluminum alloy material, controlling the trace elements (Mn, Cr, V, etc.), and strictly constraining the metal structure of the final extruded component, the toughness of the extruded component is improved, so that the aluminum alloy material of the present application and the extruded component formed therefrom have the combined properties of ultra-high strength and high toughness.

[0050] According to a first exemplary embodiment, the composition of the aluminum alloy includes, based on 100 wt.% of the aluminum alloy mass:

[0051] Si: 0.8-1.2 wt.%; for example, 0.8 wt.%, 0.9 wt.%, 1.0 wt.%, 1.2 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0052] Fe: 0.1-0.3 wt.%; for example, 0.1 wt.%, 0.2 wt.%, 0.25 wt.%, 0.3 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0053] Cu: 0.3-0.7 wt.%; for example, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0054] Mn: 0.4-0.8 wt.%; for example, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.8 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0055] Mg: 0.8-1.2 wt.%; for example, it can be 0.8 wt.%, 0.9 wt.%, 1.0 wt.%, 1.2 wt.%, but it is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable;

[0056] Cr: 0.05-0.2 wt.%; for example, 0.05 wt.%, 0.08 wt.%, 0.1 wt.%, 0.12 wt.%, 0.15 wt.%, 0.18 wt.%, 0.2 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0057] Ti: 0.01-0.1 wt.%; for example, 0.01 wt.%, 0.04 wt.%, 0.06 wt.%, 0.08 wt.%, 0.1 wt.%, but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0058] V: 0.01-0.2 wt.%; for example, it can be 0.01 wt.%, 0.04 wt.%, 0.1 wt.%, 0.15 wt.%, 0.2 wt.%, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable;

[0059] The balance in the aluminum alloy of this embodiment is Al. The aluminum alloy also includes inevitable impurities, wherein the total amount of impurities is ≤0.15 wt.%; and the amount of a single impurity is ≤0.05 wt.%.

[0060] In the present application, manganese (Mn), chromium (Cr), titanium (Ti), and vanadium (V) are the main trace additive elements in 6000 series aluminum alloys, and their addition is mainly used to control grain size; Mn and Cr are used to optimize the extruded grain size, while Ti is mainly used to optimize the grain size of aluminum alloy cast rods. The Mn and Cr contents need to be strictly controlled, otherwise a mixed structure of recrystallized and non-recrystallized is easily formed in the structure, which reduces the toughness of the material; in the process of forming extruded parts using aluminum alloy materials, Mn and Cr elements can form Al6Mn, Al-Cr-Mn and other dispersed phases during the homogenization process of the aluminum alloy cast rods. These dispersed phases will control the grain morphology during the extrusion of the aluminum alloy material, prevent abnormal grain growth and the appearance of a coarse grain layer on the surface; however, if Mn and Cr elements are added in excess, they will combine with Fe elements during the casting process to form micron-sized Al-Fe-Mn-Si compounds. These compounds not only have no effect on optimizing the grain size, but will be the most likely crack source during the deformation of the material, greatly reducing the toughness of the material; therefore, the content of Mn and Cr elements needs to be limited. The content of Ti element is required to ensure that the extruded parts formed by the aluminum alloy material do not crack during the casting process and the ingot grain size meets the requirements; the addition of V element has the effect of refining the recrystallization structure and increasing the recrystallization temperature during the process of forming the extruded parts of the aluminum alloy material. In this application, the controlled composition ranges of Mn, Cr, Ti, and V are: Mn is 0.4-0.6wt.%; Cr is 0.1-0.2wt.%; Ti is 0.05-0.1wt.%, and V is 0.01-0.1wt.%.

[0061] According to a second exemplary embodiment, based on 100 wt.% of the aluminum alloy, the aluminum alloy comprises Si: 0.8-1.1 wt.%; Fe: 0.1-0.2 wt.%; Cu: 0.3-0.5 wt.%; Mn: 0.4-0.6 wt.%; Mg: 0.8-1.1 wt.%; Cr: 0.1-0.2 wt.%; Ti: 0.05-0.1 wt.%; V: 0.01-0.1 wt.%; and the balance being Al. The aluminum alloy further includes unavoidable impurities, wherein the total amount of the impurities is ≤ 0.15 wt.% and the amount of any individual impurity is ≤ 0.05 wt.%.

[0062] According to a third exemplary embodiment, based on 100 wt.% of the aluminum alloy, the aluminum alloy comprises 1 wt.% Si, 0.1 wt.% Fe, 0.4 wt.% Cu, 0.6 wt.% Mn, 1 wt.% Mg, 0.1 wt.% Cr, 0.02 wt.% Ti, and 0.02 wt.% V, with the balance being Al. The aluminum alloy further includes unavoidable impurities, wherein the total amount of the impurities is ≤ 0.15 wt.% and the amount of any individual impurity is ≤ 0.05 wt.%.

[0063] In some embodiments, the aluminum alloy composition has a ratio of 0.8 ≤ Mg / Si ≤ 1.5, and optionally, 1.0 ≤ Mg / Si ≤ 1.2. Mg and Si are the primary strengthening elements in 6000 series aluminum alloys, and the higher the Mg and Si content, the higher the alloy strength. However, excessive Mg and Si content can easily lead to the formation of a large amount of coarse Mg2Si phases in the microstructure. Once formed, these phases cannot be eliminated through subsequent processing, resulting in a decrease in material toughness. Therefore, the Mg and Si content needs to be limited to 0.8-1.2 wt.% for Mg and 0.8-1.2 wt.% for Si.

[0064] According to the second aspect of the present application, a processing method for forming an extruded component from the aluminum alloy according to any of the above embodiments is proposed, comprising the following steps: mixing the raw materials according to the composition ratio of the aluminum alloy, and obtaining the extruded component through smelting, casting, homogenization heat treatment, extrusion shaping, and aging treatment; wherein the metal structure of the extruded component is strictly constrained.

[0065] Wherein, the temperature of the above-mentioned homogenization heat treatment is 500-580 ℃, and the holding time is 5-20h; optionally, the temperature of the homogenization heat treatment is 550-580 ℃, and the holding time is 8-12h. Homogenization heat treatment is also called homogenization heat treatment. The main purpose of homogenization heat treatment in this application is to eliminate the coarse Mg2Si phase formed during the casting process and promote the transformation of the elongated AlFeSi phase to the rounded AlFeMnSi phase. Since the crystallization process is a non-equilibrium process and the alloying degree of the material is relatively high. Therefore, in addition to the Mg2Si phase, other compounds (such as Cu-containing phases) are also formed in the structure. Therefore, single-stage or multi-stage homogenization heat treatment is adopted to promote the dissolution of different types or the same type of phases. In the homogenization heat treatment, the temperature and holding time of the homogenization heat treatment are very critical. The exemplary homogenization heat treatment temperatures are 500°C, 510°C, 530°C, 550°C, and 580°C, but are not limited to the listed values. Other unlisted values ​​within the range of 500-580°C are also applicable. The holding time is 5h, 8h, 10h, 14h, 18h, and 20h, but are not limited to the listed values. Other unlisted values ​​within the range of 5-20h are also applicable.

[0066] The extrusion molding process involves hot extrusion, followed by stretching and straightening of the extruded component after cooling. The hot extrusion process parameters are: an extrusion outlet temperature of 530-580°C and an extrusion ratio of 20 or higher, or alternatively, an extrusion temperature of 530-550°C and an extrusion ratio of 20 or higher. On the one hand, the higher extrusion temperature allows alloying elements such as Mg, Si, and Cu to be dissolved into the aluminum alloy matrix, ensuring the high strength of the aluminum alloy. If the extrusion temperature is too low, such as below 530°C, sufficient Mg, Si, and Cu cannot be dissolved into the aluminum alloy matrix, reducing the material's strength. If the temperature is too high, such as above 580°C, defects such as cracking and overburning may occur during the extrusion process to form the extruded component. On the other hand, a higher extrusion temperature, such as an extrusion ratio of at least 20, allows compounds and coarse grains to form during the casting process, improving the material's toughness. If the extrusion ratio is too low, such as less than 20, compounds and coarse grains cannot be formed during the casting process, resulting in reduced toughness.

[0067] In this application, extrusion shaping is used to improve material properties. The extrusion process needs to ensure a high temperature so that the material has high mechanical properties and excellent metal structure. In particular, the Mg2Si particles generated during casting need to be dissolved during the extrusion process, so the entire extrusion process must have a high temperature. In addition, in order to make the material have higher mechanical properties in the future, the online quenching strength of the material must be improved. The higher the quenching intensity, the greater the content of alloy elements dissolved in the matrix and the greater the vacancy solubility, the higher the strength and plasticity after subsequent aging; therefore, the extrusion shaping process of this application is: the extrusion outlet temperature is 530-580 ° C, the extrusion ratio is ≥20, and water cooling or water mist cooling is used after extrusion, and the extruded parts are stretched and straightened.

[0068] Among them, the process parameters of the above-mentioned aging treatment are: first keep warm at 160-200℃ for 6-20h, and then air-cool to room temperature; optionally, first keep warm at 180-200℃ for 10-20h. In this application, aging treatment is the last key process to improve the strength of 6000 series aluminum alloy. Before aging treatment, the higher the solute atom content and the greater the vacancy concentration in the matrix that can participate in aging, the higher the mechanical properties after aging. Aging can be done in single or multi-stage. Single-stage aging is easy to produce, while multi-stage aging is easy to improve comprehensive performance, but may reduce production efficiency. Therefore, the aging process selection of this application is: the treatment temperature of the single-stage aging treatment is 160-200°C, such as 160°C, 170°C, 180°C, 190°C, 200°C, etc., but not limited to the listed values; the treatment time of the single-stage aging treatment is 6-20h, such as 6h, 7h, 8h, 9h, 10h, 14h, 18h and 20h, etc., but not limited to the listed values.

[0069] Among the aforementioned structural constraints, the extruded component's grain morphology is a fibrous structure along the extrusion direction. By strictly constraining the extruded component's metal structure to a fibrous structure along the extrusion direction, the strength and toughness of the extruded component are improved. This strict structural constraint is achieved through the aluminum alloy composition and the processing method used to form the extruded component.

[0070] In some embodiments, according to a third aspect of the present application, an extruded component formed by the processing method according to any of the above embodiments is provided, wherein the extruded component has a yield strength of at least 350 MPa, a tensile strength of at least 400 MPa, an elongation of at least 10%, and a bend angle of at least 60°.

[0071] The extruded component formed in this embodiment can be used in a vehicle. Many different types of components can be formed through the extrusion process, such as front and rear bumper beams, body-in-white components, suspension components, or chassis components. Following the extrusion process, the method may include an optional heat treatment or other finishing process.

[0072] Example 1

[0073] The ultra-high-strength aluminum alloy includes, based on 100wt.% of the aluminum alloy, the following components: Si: 0.8wt.%; Fe: 0.1wt.%; Cu: 0.4wt.%; Mn: 0.6wt.%; Mg: 1.2wt.%; Cr: 0.1wt.%; Ti: 0.02wt.%; V: 0.01wt.%; the remainder being Al and unavoidable impurities.

[0074] The processing method is shown in Figure 1: the materials are prepared according to the proportion of aluminum alloy components, and the raw materials are melted and cast to obtain round aluminum rods. The aluminum rods are subjected to homogenization heat treatment, and the temperature in the homogenization heat treatment process is 550°C and the time is 12 hours; the aluminum rods are preheated and then extruded, and the extrusion process requirements are: the extrusion ratio is 20; the extrusion outlet temperature is 530°C, and water cooling is performed after extrusion. The extruded parts are stretched and straightened, and then artificially aged, and the treatment process is: temperature: 180°C, time 10 hours. The metal structure of the extruded parts is strictly constrained: the grain morphology of the extruded parts is a fibrous structure along the extrusion direction to improve the strength and toughness of the extruded parts. The metal structure grain morphology of the extruded parts in this embodiment is shown in Figure 2, while the metal structure grain morphology of the extruded parts of Example 1, in which the metal structure is not strictly constrained, is shown in Figure 3.

[0075] In Examples 2 to 20, and Comparative Examples 1 to 18, the mass percentages of Si, Cu, Mg, Mn, Cr, and Ti in the aluminum alloy components and the processing parameters are adjusted according to Table 1, and the remaining technical features are the same as those in Example 1. The metal structure of the extruded parts of Examples 2 to 20 is also strictly constrained: the grain morphology of the extruded parts is a fibrous structure along the extrusion direction. Comparative Examples 2 to 18 do not strictly constrain the metal structure of the extruded parts as in Comparative Example 1. Automobile anti-collision beams are prepared according to the aluminum alloy components and processing methods in each embodiment and comparative example, and the ASTME8 / E8M-21 (standard test method for tensile testing of metal materials) test method is used according to the cross-section of the automobile anti-collision beam as shown in Figure 4 to conduct yield strength, tensile strength, elongation mechanical property tests and bending angle tests according to the VDA-238 standard. The test results are also shown in Table 1 below.

[0076] Table 1 Aluminum alloy material composition, processing method and mechanical properties test results of pressurized components

[0077] As can be seen from the data in Table 1, by comparing Examples 1 to 20 with Comparative Examples 1-18, the following results can be found:

[0078] From the comparison between Examples 1-3 and Comparative Examples 1-2, it can be seen that when the Si element content is low, the amount of reinforcing phases in the extruded component will be reduced, causing the strength of the extruded component to fail to meet the requirement of at least 400 MPa tensile strength in this application; when the Si element content is high, excess Si elements will precipitate in the extruded component in the form of elemental Si, thereby reducing the bending angle of the extruded component, causing the toughness of the extruded component to fail to meet the requirement of at least 350 MPa in this application.

[0079] From the comparison of Examples 4-6 and Comparative Examples 3-4, it can be seen that, similar to the effect of Si element, when the Cu element content is low, the amount of reinforcing phase in the extruded component will be reduced, causing the strength of the extruded component to fail to meet the requirements of this application; but when the Cu element content is low, excessive Cu element will increase the strength of the material, but reduce the elongation and bending angle of the extruded component, causing the toughness of the extruded component to fail to meet the requirements of this application.

[0080] From the comparison of Examples 7-8 and Comparative Examples 5-6, it can be seen that when the Mg element content is low, the number of reinforcing phases in the extruded component will be reduced, causing the strength of the extruded component to fail to meet the requirements of this application; but when the Mg element content is high, excessive Mg elements will increase the strength of the material, but reduce the elongation and bending angle of the extruded component, causing the toughness of the extruded component to fail to meet the requirements of this application.

[0081] From the comparison of Examples 9-10 and Comparative Examples 7-8, it can be seen that when the Mn element content is low, the number of dispersed phases in the extruded part will be reduced, and the fibrous structure will not be well controlled, resulting in a decrease in the bending angle of the extruded part, which does not meet the requirements of this application; but when the Mn element content is high, excessive Mn elements will form coarse Al-Fe-Mn phases during the casting process, which cannot be completely broken during the extrusion process, not only reducing the bending angle of the extruded part but also reducing the elongation of the extruded part, causing the toughness of the extruded part to fail to meet the requirements of this application.

[0082] Comparison of Examples 11-12 and Comparative Examples 9-10 shows that the role of Cr, similar to that of Mn, is to form a dispersed phase and control the metal structure. When the Cr content is low, the number of dispersed phases in the extruded component decreases, resulting in poor control of the fibrous structure, which in turn reduces the bending angle of the extruded component and fails to meet the requirements of this application. However, when the Cr content is high, excessive Cr will form coarse Al-Fe-Cr phases during the casting process, which cannot be completely broken down during extrusion. This not only reduces the bending angle of the extruded component but also reduces the elongation of the extruded component, causing the toughness of the extruded component to fail to meet the requirements of this application.

[0083] From the comparison of Examples 13-14 and Comparative Examples 11-12, it can be seen that when the Ti element content is low, the ingot grain size will be coarse, and the size of compounds such as Mg2Si phase and Al-Fe-Mn-Si at the grain boundary will be coarse, thereby causing the strength and bending angle of the extruded parts to decrease and fail to meet the requirements of this application; but when the Ti element content is high, excessive Ti elements will form solid solution strengthening and increase the strength of the extruded parts, but will also cause the elongation and bending angle of the extruded parts to decrease, and the toughness will not meet the requirements of this application.

[0084] From the comparison of Examples 15-16 and Comparative Examples 13-14, it can be seen that when the homogenization heat treatment temperature is low, the homogenization of the aluminum rod will not be complete (Mg2Si is not completely dissolved, and the long strip Al-Fe-Si compound is not completely transformed into a rounded Al-Fe-Mn-Si phase), which will not only reduce the strength of the extruded component but also reduce the elongation and bending angle of the extruded component, which does not meet the requirements of this application; when the homogenization heat treatment temperature is high, it will cause the aluminum rod to overburn, thereby reducing the elongation and bending angle of the extruded component, causing the toughness of the extruded component to fail to meet the requirements of this application.

[0085] From the comparison of Examples 17-18 and Comparative Examples 15-16, it can be seen that when the extrusion outlet temperature of the extruded component is low, Mg2Si cannot be completely dissolved into the extruded component during the extrusion process, thereby reducing the bending angle of the extruded component and failing to meet the requirements of this application; when the extrusion outlet temperature is high, the extruded component will be difficult to weld at the outlet of the extrusion die and cannot be extruded normally.

[0086] By comparing Examples 19-20 and Comparative Examples 17-18, it can be seen that when the artificial aging treatment temperature of the extruded component is low, the density of the precipitated phase during the artificial aging treatment will be insufficient, the extruded component will be in an under-aged state, and the strength of the extruded component will be reduced, failing to meet the requirements of the present application; when the artificial aging treatment temperature is high, the precipitated phase will grow during the artificial aging treatment and lose its semi-coherent relationship with the aluminum matrix, resulting in the extruded component being in an under-aged state, which will also reduce the strength of the extruded component and failing to meet the requirements of the present application.

[0087] Throughout this specification, reference to terms such as "one embodiment," "some embodiments," "examples," "specific examples," or "some examples" means that a specific feature, structure, material, or characteristic described in conjunction with that embodiment or example is included in at least one embodiment or example of the present application. In this specification, schematic representations of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0088] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. An ultra-high strength aluminum alloy material, based on the mass of the aluminum alloy material being 100wt.%, the aluminum alloy material comprises: Si: 0.8-1.2wt.%; Fe: 0.1-0.3wt.%; Cu: 0.3-0.7wt.%; Mn: 0.4-0.8wt.%; Mg: 0.8-1.2wt.%; Cr: 0.05-0.2wt.%; Ti: 0.01-0.1wt.%; V: 0.01-0.2wt.%; the balance is Al.

2. The aluminum alloy material according to claim 1, wherein: The aluminum alloy material comprises: Si: 0.8-1.1wt.%; Fe: 0.1-0.2wt.%; Cu: 0.3-0.5wt.%; Mn: 0.4-0.6wt.%; Mg: 0.8-1.1wt.%; Cr: 0.1-0.2wt.%; Ti: 0.05-0.1wt.%; V: 0.01-0.1wt.%.

3. The aluminum alloy material according to claim 1 or 2, wherein: Also included are inevitable impurities, the total amount of which is ≤0.15wt.%, and the amount of a single impurity is ≤0.05wt.%.

4. The aluminum alloy material according to claim 3, wherein: In the aluminum alloy material, 0.8≤Mg / Si≤1.

5.

5. The aluminum alloy material according to claim 3, wherein: In the aluminum alloy material, 1.0≤Mg / Si≤1.

2.

6. A method for forming an extruded component from the aluminum alloy material according to any one of claims 1 to 5, comprising the following steps: The raw materials are mixed according to the proportion of the aluminum alloy material, and the extruded parts are obtained through smelting, casting, homogenization heat treatment, extrusion shaping and aging treatment; wherein the metal structure of the extruded parts is strictly constrained.

7. The processing method according to claim 6, wherein: The temperature of the homogenization heat treatment is 500-580° C., and the insulation time is 5-20 hours.

8. The processing method according to claim 6 or 7, wherein: In the extrusion shaping, hot extrusion is first performed, and the extruded part is stretched and straightened after cooling; wherein the process parameters of hot extrusion are: extrusion outlet temperature is 530-580°C, and extrusion ratio is ≥20.

9. The processing method according to any one of claims 6 to 8, wherein: The process parameters of the aging treatment are: keeping at 160-200° C. for 6-20 hours and air cooling to room temperature.

10. The processing method according to any one of claims 6 to 9, wherein: The metal structure of the extruded component is strictly constrained as follows: the grain morphology of the extruded component is a fibrous structure along the extrusion direction.

11. An extruded component formed by the processing method according to any one of claims 6 to 10.

12. The extruded component according to claim 11, wherein The extruded component has a yield strength of at least 350 MPa, a tensile strength of at least 400 MPa, an elongation of at least 10%, and a bending angle of at least 60°.

Citation Information

Patent Citations

  • Improved 6XXX aluminum alloys, and methods for producing the same

    CN104428434A

  • High strength aluminum alloy sheet

    CN105838927A

  • High strength products extruded from 6xxx aluminium alloys having excellent crash performance

    CN106605004A

  • Aluminum alloy and aluminum alloy extruded profile machining method

    CN108118210A

  • Al-Mg-Si-BASED ALUMINUM ALLOY HOLLOW EXTRUDED MATERIAL AND METHOD FOR PRODUCING SAME

    CN111801433A