Ni 3al / carbide composite material powder, laser cladding method therefor, and use thereof

By optimizing the chemical composition and laser cladding process of Ni3Al/carbide composite powder, an in-situ self-generating carbide-enhanced Ni3Al base alloy reinforcement layer was formed, and cracks in the laser cladding process of Ni3Al/carbide composite in the prior art were solved. It is also suitable for the modification of the surface of heavy-duty diesel engine parts.

WO2024230845A1PCT designated stage expired Publication Date: 2024-11-14CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD

Patent Information

Application Number
PCT/CN2024/093986
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-17
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing Ni3Al/carbide composite materials are prone to cracks and uneven distribution of carbides during laser cladding, which affects their mechanical processing performance and wear resistance.

Method used

Ni3Al/carbide composite powder was used, with chemical compositions of Al: 9.5% to 10.0%, C: 1.1% to 1.6%, Cr: 18.0% to 19.5%, B: 0.05% to 0.07%, O≤200ppm, N≤ 50ppm, H≤10ppm, the atomic ratio of nickel equivalent to aluminum equivalent is 2.5 to 2.9, and includes NiAl phase and Cr7C3 phase. In situ autogenerated carbide-enhanced Ni3Al base alloy reinforcement layer is formed by laser cladding.

Benefits of technology

It effectively improves the mechanical processing performance and hardness of the cladding layer, maintains good wear resistance, enhances the bonding strength between the Ni3Al base alloy reinforcement layer and the substrate, and meets the performance requirements of the surface of heavy-duty diesel engine parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024093986_14112024_PF_FP_ABST
    Figure CN2024093986_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of laser processing of materials, and relates to Ni3Al / carbide composite material powder, a laser cladding method therefor, and a use thereof. The Ni3Al / carbide composite material powder comprises the following components in percentage by mass: Al: 9.5%-10.0%; C: 1.1%-1.6%; Cr: 18.0%-19.5%; B: 0.05%-0.07%; O: ≤200 ppm; N: ≤50 ppm; H: ≤10 ppm; and the balance being Ni. The atomic ratio of a nickel equivalent to an aluminum equivalent is 2.5-2.9. The Ni3Al / carbide composite material powder contains a NiAl phase. The carbide structure is Cr7C3, and the mass content of Cr7C3 is 13%-18%. The present application effectively improves the machining performance of a cladding layer, and improves the hardness of the cladding layer to keep good wear resistance of the cladding layer, thereby satisfying requirements for the surface performance of a key part of a heavily loaded diesel engine.
Need to check novelty before this filing date? Find Prior Art

Description

A Ni3Al / carbide composite material powder and its laser cladding method and application Technical Field

[0001] The present application relates to the technical field of laser processing materials, and in particular to a Ni3Al / carbide composite material powder and a laser cladding method and application thereof. Background Art

[0002] In recent years, heavy-duty diesel engines have been developing towards high mechanical and thermal loads, as well as low emissions, resulting in increasingly harsh internal operating environments. This harsh operating environment places extremely high demands on the surface wear resistance, fatigue resistance, thermal insulation, and oxidation resistance of key components in these engines. However, existing material structures, coating systems, and coating technologies all present significant limitations. Therefore, developing new coating systems and their preparation technologies to improve the quality and performance of key components has become a critical technical challenge urgently needed by diesel engine developers and users both domestically and internationally.

[0003] Ni3Al alloys and Ni3Al / carbide composites are considered ideal high-temperature, high-strength, and wear-resistant materials. Chinese Patent 201410822105.5 describes a method for using laser cladding to produce Ni3Al / Cr3C2 composite coatings with a dense microstructure, strong substrate bonding, and excellent wear resistance. This method holds promise for applications in heavy-duty, high-power diesel engines. However, this technique, which uses a mixture of Ni3Al alloy powder and Cr3C2 powder as the cladding powder, is prone to cracking and uneven carbide distribution, severely impacting the engineering applications of the Ni3Al / Cr3C2 composite coating. In order to solve the above problems, Chinese patent application publication number CN115011843A discloses a method for preparing an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer using laser cladding technology. Within a larger range of cladding process parameters, the formation of cladding cracks is suppressed and the uniform distribution of carbides in the cladding layer is promoted. However, due to the use of this technology, the proportion of Cr7C3 carbides in the cladding layer is relatively high (mass content is 22% to 28%), resulting in poor machinability (cutting) of the Ni3Al / Cr7C3 cladding layer.

[0004] To improve the machinability (cutting) of the in-situ carbide-reinforced Ni3Al-based alloy layer, reducing the carbide ratio in the cladding layer is an effective method. However, maintaining high hardness and good wear resistance of the Ni3Al-based alloy layer while reducing the carbide ratio is a difficult problem.

[0005] Summary of the Invention

[0006] In view of the above analysis, the present application aims to provide a Ni3Al / carbide composite material powder and its laser cladding method and application, so as to solve at least one of the following existing problems: improving the machining performance of Ni3Al / carbide composite material powder, so that the material maintains high hardness, good wear resistance and interface shear strength.

[0007] The purpose of this application is mainly achieved through the following technical solutions:

[0008] The present application provides a Ni3Al / carbide composite material powder, whose chemical composition, in mass percentage, is: Al: 9.5% to 10.0%, C: 1.1% to 1.6%, Cr: 18.0% to 19.5%, B: 0.05% to 0.07%, O≤200ppm, N≤50ppm, H≤10ppm, and the remainder is Ni; in the Ni3Al / carbide composite material powder, the atomic number ratio of nickel equivalent to aluminum equivalent is 2.5 to 2.9, the Ni3Al / carbide composite material powder contains a NiAl phase, and the carbide structure of the Ni3Al / carbide composite material powder is Cr7C3, and the mass content of Cr7C3 is 13% to 18%.

[0009] Preferably, the particle size of the Ni3Al / carbide composite material powder ranges from 53 μm to 124 μm.

[0010] The present application also provides a laser cladding method for Ni3Al / carbide composite material powder, comprising the following steps: Step 1: using a coaxial powder feeding method to transport the Ni3Al / carbide composite material powder to the surface of a steel material; Step 2: using a laser cladding method to clad the Ni3Al / carbide composite material powder on the surface of the steel material to form an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0011] Preferably, the coaxial powder feeding method has a coaxial powder feeding rate of 10 g / min to 30 g / min.

[0012] Preferably, the power of the laser cladding is 1400W to 2600W, and the scanning speed is 0.12m / min to 0.60m / min.

[0013] Preferably, the laser beam of the laser cladding method is a circular spot or a rectangular spot.

[0014] In addition, the present application also provides an in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer, which is formed on the surface of a steel material by a laser cladding method. The Ni3Al-based alloy strengthening layer includes a Ni3Al phase, a NiAl phase and a carbide Cr7C3, wherein the carbide Cr7C3 is dispersed in the Ni3Al phase. The average hardness of the Ni3Al-based alloy strengthening layer is 620-680 HV, and the wear rate is ≤0.8×10 -5 mm 3 / (N·m), and the shear strength of the bonding interface with steel materials is 400-600 MPa.

[0015] Preferably, the Ni3Al-based alloy strengthening layer is produced by the laser cladding method.

[0016] Preferably, the steel material is one of carbon steel, alloy steel, heat-resistant stainless steel and cast iron.

[0017] In addition, the present application also provides an application of Ni3Al / carbide composite material powder, wherein the Ni3Al / carbide composite material powder is used for surface modification of steel or nickel-based alloy components of heavy-duty diesel engines.

[0018] Compared with the prior art, this application can achieve at least one of the following beneficial effects:

[0019] A) In the present application, the content of carbide Cr7C3 is about 13-18%, which can effectively improve the machining (cutting) performance of the cladding layer; at the same time, the equivalent atomic ratio of nickel to aluminum is 2.5-2.9, which promotes the formation of NiAl hard phase, improves the hardness of the cladding layer, and maintains good wear resistance. Overall, while reducing the proportion of carbides in the cladding layer, the Ni3Al-based alloy strengthening layer can maintain a high hardness and good wear resistance, which can meet the surface performance requirements of key components of heavy-duty diesel engines.

[0020] B) In this application, laser cladding technology is used to create an in-situ, carbide-reinforced Ni3Al-based alloy strengthening layer. The Cr7C3 is melted and then re-formed in situ, reducing the Cr7C3 size and improving its bonding with the Ni3Al-based phase. The Ni3Al-based alloy strengthening layer is metallurgically bonded to the substrate, achieving an interfacial shear strength of 400-600 MPa.

[0021] Other features and advantages of the present application will be described in the subsequent description, and some will become apparent from the description or be understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings are only for the purpose of illustrating particular embodiments and are not to be considered as limiting the present application. Like reference symbols denote like components throughout the drawings.

[0023] FIG1 is a morphology of Ni3Al / carbide composite material powder prepared by vacuum induction melting-inert gas atomization method in Example 1 provided in the present application;

[0024] FIG2 is a morphology diagram of the in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer formed after laser cladding in Example 1 provided in the present application.

[0025] FIG3 is a microstructural morphology diagram of the in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer formed after laser cladding in Example 1 provided in the present application. DETAILED DESCRIPTION

[0026] The preferred embodiments of the present application are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present application and are used together with the embodiments of the present application to illustrate the principles of the present application.

[0027] The present application provides a Ni3Al / carbide composite material powder, whose chemical composition, in mass percentage, is: Al: 9.5%~10.0%, C: 1.1%~1.6%, Cr: 18.0%~19.5%, B: 0.05%~0.07%, O≤200ppm, N≤50ppm, H≤10ppm, and the balance is Ni; in the Ni3Al / carbide composite material powder, the atomic number ratio of nickel equivalent to aluminum equivalent is 2.5~2.9, the Ni3Al / carbide composite material powder contains a NiAl phase with a mass content of approximately 2.5%-8.5%, and the carbide structure of the Ni3Al / carbide composite material powder is Cr7C3, with a mass content of Cr7C3 of 13%~18%, which is dispersed in the Ni3Al matrix phase.

[0028] Specifically, in this application, the calculation principle of the number of nickel equivalent atoms is:

[0029] The calculation principle of the number of aluminum equivalent atoms is:

[0030] Among them, Cr Ni3Al溶 The content of Ni3Al / carbide composite material powder is 4% to 10%, wherein Ni represents the mass percentage of Ni element in the Ni3Al / carbide composite material powder, and Al represents the mass percentage of Al element in the Ni3Al / carbide composite material powder.

[0031] Specifically, as a preference, the mass percentages of the components are: Al: 9.6% to 9.95%, C: 1.3% to 1.45%, Cr: 18.9% to 19.5%, B: 0.05% to 0.06%, O: 40 to 180 ppm, N: 26 to 37 ppm, H: 3 to 4 ppm. Preferably, the atomic ratio of nickel equivalent to aluminum equivalent is 2.75 to 2.85, and the mass content of Cr7C3 is 15% to 17%.

[0032] It should be noted that, generally, the nickel-to-aluminum equivalent atomic ratio of the Ni3Al phase is 3. This application reduces the nickel content and increases the aluminum content, thereby reducing the nickel-to-aluminum equivalent atomic ratio and promoting the formation of the NiAl phase, so that both the Ni3Al phase and the NiAl phase coexist in the Ni3Al / carbide composite powder. The hardness of the Ni3Al phase is 300-400 HV, the hardness of the NiAl phase is 500-700 HV, and the hardness of the Cr7C3 carbide exceeds 1200 HV. Therefore, the increase in the NiAl phase helps to increase the hardness of the cladding layer after laser cladding, providing a basis for maintaining good wear resistance.

[0033] It should be noted that when the atomic ratio of nickel equivalent to aluminum equivalent is less than 2.5, the proportion of NiAl phase is large, the plasticity of NiAl phase is poor, and crack formation is easily caused.

[0034] In addition, the finely dispersed Cr7C3 hard phase provides support, separating the friction surfaces and reducing direct interaction between the friction pairs, thereby improving wear resistance. The Cr7C3 content in the composite material powder provided in this application is 13% to 18% by mass. Compared to the Chinese patent application with publication number CN115011843A, the reduced carbide content helps improve the machinability of the Ni3Al-based alloy reinforcement layer. When the Cr7C3 content is less than 13% by mass, the high-hardness carbide reinforcement phase is insufficient to effectively separate the friction surfaces, resulting in a decrease in the wear resistance of the cladding layer.

[0035] It should be noted that Ni3Al alloy has room temperature brittleness. A small amount of B can improve the room temperature ductility of Ni3Al and inhibit crack formation. However, when the B element is excessive, B is enriched on the grain boundaries, which promotes the formation of hot cracks. Within the chemical composition range of the composite material powder of this application, when the B content is lower than 0.05%, it cannot play a role in improving the plasticity of Ni3Al, and when the B content is higher than 0.07%, the cladding layer has a greater tendency to hot cracks. The B content of this application is determined to be 0.05% to 0.07%, which can not only ensure the room temperature ductility of the Ni3Al base phase of the cladding layer, but also inhibit the formation of hot cracks.

[0036] It should be noted that during the laser cladding process of Ni3Al / carbide composite material powder, impurity elements such as O, H, and N will participate in metallurgical reactions. For carbide-reinforced Ni3Al-based alloy cladding layers, excessive O content is prone to fatigue problems and increased wear; excessive N content can easily lead to AlN formation and increase cracking tendency; excessive H content increases the brittleness of the cladding layer. The limit value of the impurity element content has extremely important engineering value and determines the metallurgical process technology and economy of the powder material. This application limits the content of O, N, and H elements in the powder to ≤200ppm, ≤50ppm, and ≤10ppm.

[0037] Specifically, the particle size of the Ni3Al / carbide composite material powder ranges from 53 μm to 124 μm, preferably from 75 μm to 105 μm.

[0038] It should be noted that if the particle size of the composite material powder is too large, unmelted powder will appear during laser cladding, while if the particle size is too small, it is easy to rub against the powder feeding equipment during laser cladding and block the equipment.

[0039] The Ni3Al / carbide composite material powder provided in the present application is prepared by a plasma rotating electrode method or a vacuum induction melting-inert gas atomization method.

[0040] It should be noted that the plasma rotating electrode method or vacuum induction melting-inert gas atomization method used in this application is based on the chemical composition of the composite material powder to be prepared, and then the plasma rotating electrode method or vacuum induction melting-inert gas atomization method is used to obtain the pre-alloyed composite material powder.

[0041] The present application also provides a method for laser cladding of Ni3Al / carbide composite material powder, comprising the following steps:

[0042] Step 1: Using a coaxial powder feeding method, the Ni3Al / carbide composite material powder is delivered to the surface of the steel material.

[0043] Step 2: Use the laser cladding method to clad the Ni3Al / carbide composite material powder on the surface of the steel material to form an in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer.

[0044] Specifically, the steel material is one of carbon steel, alloy steel, heat-resistant stainless steel and cast iron.

[0045] It should be noted that the carbide Cr7C3 is distributed in the Ni3Al-based alloy powder in an in-situ autogenous manner, which can improve the distribution uniformity of Cr7C3 in the alloy powder; when the alloy coating is prepared by laser cladding technology, Cr7C3 is melted and formed again in situ, which can reduce the size of Cr7C3 and make Cr7C3 more evenly distributed in the alloy coating.

[0046] Specifically, the coaxial powder feeding amount of the coaxial powder feeding method is 10 g / min to 30 g / min. Preferably, the coaxial powder feeding amount is 15 g / min to 20 g / min.

[0047] It should be noted that when the powder feeding rate is low, the dilution rate of the matrix (steel material) is high, and the hardness and wear resistance of the Ni3Al-based alloy strengthening layer are greatly reduced; when the powder feeding rate is high, the dilution rate of the matrix (steel material) is small, the metallurgical bonding between the Ni3Al-based alloy strengthening layer and the matrix is ​​insufficient, and unmelted powder may appear.

[0048] Specifically, the power of the laser cladding is 1400-2600 W, the scanning speed is 0.12-0.60 m / min, and the laser beam is a circular spot or a rectangular spot; when the laser beam is a circular spot, the diameter of the circular spot is 2-5 mm; when the laser beam is a rectangular spot, the length of the rectangular spot is 5-20 mm and the width is 1-6 mm.

[0049] Preferably, the power of the laser cladding is 1600-2200W, the scanning speed is 0.18-0.30m / min, and when the laser beam is a circular spot, the diameter of the circular spot is 3-4mm; when the laser beam is a rectangular spot, the length of the rectangular spot is 5-10mm and the width is 2-3mm.

[0050] It should be noted that when the laser power is small or the scanning speed is fast, the dilution rate of the substrate (steel material) is small, the metallurgical bonding of the Ni3Al-based alloy strengthening layer to the substrate is insufficient, and unmelted powder may appear in the cladding layer; when the laser power is large or the scanning speed is low, the dilution rate of the substrate (steel material) is high, and the hardness and wear resistance of the Ni3Al-based alloy strengthening layer are greatly reduced.

[0051] It should be noted that when the spot size is small, the powder falling within the spot size is less, the energy density is high, the dilution rate of the matrix (steel material) is high, and the hardness and wear resistance of the Ni3Al-based alloy strengthening layer are greatly reduced; when the spot size is large, the powder falling within the spot size is more, the energy density is reduced, the dilution rate of the matrix (steel material) is reduced, the metallurgical bonding of the Ni3Al-based alloy strengthening layer matrix is ​​insufficient, and unmelted powder may appear in the cladding layer.

[0052] Specifically, the Ni3Al-based alloy strengthening layer obtained by the laser cladding method includes Ni3Al phase, NiAl phase, and carbide Cr7C3. The carbide Cr7C3 is dispersed in the Ni3Al-based phase. The thickness of the Ni3Al-based alloy strengthening layer exceeds 1.2 mm, preferably 1.2 mm to 2.5 mm. The bonding strength with the steel material is high (metallurgical bonding), and the shear strength of the interface is 400 to 600 MPa. Specifically, for example, the shear strength of the interface with the 42CrMo steel base material is 500 to 600 MPa. The average hardness of the Ni3Al-based alloy strengthening layer obtained by the laser cladding method is 620 to 680 HV, and the wear rate is ≤0.8×10 -5 mm 3 / (N·m).

[0053] The present application also provides an application of Ni3Al / carbide composite alloy powder for surface modification of steel parts or nickel-based alloy parts of heavy-duty diesel engines.

[0054] The Ni3Al / carbide composite material powder, its laser cladding method and application provided in the present application have a carbide content of approximately 13 to 18%, which can effectively improve the machining (cutting) performance of the cladding layer; at the same time, the equivalent atomic ratio of nickel to aluminum is 2.5 to 2.9, which promotes the formation of NiAl hard phase, improves the hardness of the cladding layer, and maintains good wear resistance. Overall, while reducing the proportion of carbides in the cladding layer, the Ni3Al-based alloy strengthening layer can maintain a high hardness and good wear resistance, which can meet the surface performance requirements of key components of heavy-duty diesel engines.

[0055] The preferred embodiments of the present application are described in detail below to illustrate the principles of the present application, but are not intended to limit the scope of the present application.

[0056] Example 1

[0057] The morphology of the Ni3Al / carbide composite powder prepared by vacuum induction melting-inert gas atomization is shown in Figure 1. The particle size of the Ni3Al / carbide alloy powder ranges from 53μm to 124μm.

[0058] In terms of mass percentage, the chemical composition of the Ni3Al / carbide composite material powder is: Al: 9.80%, C: 1.31%, Cr: 18.93%, B: 0.06%, O: 138ppm, N: 26ppm, H: 3ppm, and the remainder is Ni. The atomic number ratio of nickel equivalent to aluminum equivalent is approximately 2.83, the mass content of NiAl phase is approximately 4.3%, and the mass content of in-situ self-generated carbide Cr7C3 is approximately 16.5%.

[0059] The above-mentioned Ni3Al / carbide composite material powder was used for laser cladding on the surface of 42CrMo steel. The laser power was 2000 W, the scanning speed was 0.18 m / min, the laser rectangular spot size was 5 mm × 2 mm, and the coaxial powder feeding rate was 17.5 g / min, forming an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0060] The morphology of the in-situ carbide-reinforced Ni3Al-based alloy strengthening layer prepared in this example is shown in Figures 2 and 3. According to Figure 2, the Ni3Al-based alloy strengthening layer obtained in this example is crack-free, has a dense microstructure, and has uniformly distributed carbides. According to Figure 3, the microstructure shown in region 1 is Cr7C3, the microstructure shown in region 2 is Ni3Al, and the microstructure shown in region 3 is NiAl.

[0061] The Ni3Al-based alloy strengthening layer of this embodiment has a thickness of 2.3 mm, an average hardness of 645 HV, and an interface shear strength of 556 MPa. Under dry friction conditions (surface friction, the grinding material is gray cast iron), the wear rate of the Ni3Al-based alloy strengthening layer is 0.21×10 -5 mm 3 / (N·m), the wear rate of the grinding material gray cast iron is 0.29×10 -5 mm 3 / (N·m).

[0062] Example 2

[0063] The particle size of Ni3Al / carbide composite powder prepared by plasma rotating electrode method ranges from 53μm to 124μm.

[0064] In terms of mass percentage, the chemical composition of the Ni3Al / carbide composite material powder is: Al: 9.95%, C: 1.45%, Cr: 19.45%, B: 0.06%, O: 40ppm, N: 28ppm, H: 3ppm, and the balance is Ni. The atomic number ratio of nickel equivalent to aluminum equivalent is approximately 2.76, the mass content of NiAl phase is approximately 6.0%, and the mass content of in-situ self-generated carbide Cr7C3 is approximately 17.0%.

[0065] The above-mentioned Ni3Al / carbide composite material powder was used for laser cladding on the surface of compacted graphite cast iron. The laser power was 2200 W, the scanning speed was 0.18 m / min, the laser rectangular spot size was 5 mm × 2 mm, and the coaxial powder feeding rate was 20 g / min, forming an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0066] The in-situ carbide-reinforced Ni3Al-based alloy strengthening layer prepared in this embodiment has no cracks and is evenly distributed with carbides. The Ni3Al-based alloy strengthening layer has a thickness of 2.5 mm, an average hardness of 665 HV, and an interface shear strength of 423 MPa. Under dry friction conditions (surface friction, with the grinding material being gray cast iron), the wear rate of the Ni3Al-based alloy strengthening layer is 0.18×10 -5 mm 3 / (N·m), the wear rate of the grinding material gray cast iron is 0.37×10 -5 mm 3 / (N·m).

[0067] Example 3

[0068] The particle size of Ni3Al / carbide composite powder prepared by vacuum induction melting-inert gas atomization method ranges from 53μm to 124μm.

[0069] In terms of mass percentage, the chemical composition of the Ni3Al / carbide composite material powder is: Al: 9.64%, C: 1.19%, Cr: 18.79%, B: 0.05%, O: 172ppm, N: 37ppm, H: 4ppm, and the balance is Ni. The atomic number ratio of nickel equivalent to aluminum equivalent is approximately 2.89, the mass content of NiAl phase is approximately 2.8%, and the mass content of in-situ self-generated carbide Cr7C3 is approximately 15.0%.

[0070] The above-mentioned Ni3Al / carbide composite material powder was used for laser cladding on the surface of 42CrMo steel. The laser power was 1600W, the scanning speed was 0.30m / min, the laser circular spot diameter was 3mm, and the coaxial powder feeding rate was 15g / min to form an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0071] The in-situ carbide-reinforced Ni3Al-based alloy strengthening layer prepared in this embodiment has no cracks and is evenly distributed with carbides. The Ni3Al-based alloy strengthening layer has a thickness of 1.7 mm, an average hardness of 631 HV, and an interface shear strength of 532 MPa. Under dry friction conditions (surface friction, with the grinding material being gray cast iron), the wear rate of the Ni3Al-based alloy strengthening layer is 0.35×10 -5 mm 3 / (N·m), the wear rate of the grinding material gray cast iron is 0.48×10 -5 mm 3 / (N·m).

[0072] Comparative Example 1

[0073] The particle size of the Ni3Al / carbide composite powder prepared by vacuum induction melting-inert gas atomization method ranges from 53μm to 124μm.

[0074] In terms of mass percentage, the chemical composition of the Ni3Al / carbide composite material powder is: Al: 9.22%, C: 1.35%, Cr: 19.01%, B: 0.06%, O: 146ppm, N: 25ppm, H: 3ppm, the remainder is Ni, the atomic number ratio of nickel equivalent to aluminum equivalent is about 3, and the mass content of in-situ self-generated carbide Cr7C3 is about 16.5%.

[0075] The above-mentioned Ni3Al / carbide composite material powder was used for laser cladding on the surface of 42CrMo steel. The laser power was 2000 W, the scanning speed was 0.18 m / min, the laser rectangular spot size was 5 mm × 2 mm, and the coaxial powder feeding rate was 17.5 g / min, forming an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0076] The in-situ carbide-reinforced Ni3Al-based alloy strengthening layer prepared in this comparative example has no cracks and is evenly distributed with carbides. The Ni3Al-based alloy strengthening layer has a thickness of 2.3 mm, an average hardness of 546 HV, and an interface shear strength of 538 MPa. Under dry friction conditions (surface friction, with the grinding material being gray cast iron), the wear rate of the Ni3Al-based alloy strengthening layer is 1.19×10 -5 mm 3 / (N·m), the wear rate of the grinding material gray cast iron is 3.05×10 -5 mm 3 / (N·m).

[0077] Compared with Example 1, this comparative example has the same carbide ratio as Example 1, but the nickel-aluminum atomic ratio is 3, and the NiAl phase is not added. Although the machining performance is improved, the hardness and wear resistance of the cladding layer are low.

[0078] Comparative Example 2

[0079] The particle size of the Ni3Al / carbide composite powder prepared by vacuum induction melting-inert gas atomization method ranges from 53μm to 124μm.

[0080] In terms of mass percentage, the chemical composition of the Ni3Al / carbide composite material powder is: Al: 8.71%, C: 2.13%, Cr: 25.92%, B: 0.05%, O: 151ppm, N: 32ppm, H: 4ppm, and the remainder is Ni. The atomic number ratio of nickel equivalent to aluminum equivalent is approximately 2.83, the mass content of NiAl phase is approximately 3.8%, and the mass content of in-situ self-generated carbide Cr7C3 is approximately 25%.

[0081] The above-mentioned Ni3Al / carbide composite material powder was used for laser cladding on the surface of 42CrMo steel. The laser power was 2000 W, the scanning speed was 0.18 m / min, the laser rectangular spot size was 5 mm × 2 mm, and the coaxial powder feeding rate was 17.5 g / min, forming an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

[0082] The carbide distribution of the in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer prepared in this comparative example is uniform, with a thickness of 2.1 mm, an average hardness of 729 HV, and an interface shear strength of 517 MPa. However, cracks appeared in the cladding layer, and the crack tendency increased significantly. The friction and wear specimens were prepared in the crack-free cladding layer area. Under dry friction conditions (surface friction, the grinding material is gray cast iron), the wear rate of the laser cladding layer was 0.20×10 -5 mm 3 / (N·m), the wear rate of the grinding material gray cast iron is 0.72×10 -5 mm 3 / (N·m).

[0083] Compared with Example 1, this comparative example has the same nickel-aluminum atomic ratio as Example 1, but the mass content of the in-situ self-generated carbide Cr7C3 is about 25%. Although it maintains a relatively high hardness and good wear resistance, the proportion of high-hardness carbide strengthening phase is relatively high, resulting in poor machinability (cutting) of the cladding layer.

[0084] Specifically, the performance of Examples 1-3 and Comparative Examples 1-2 provided in this application are shown in Table 1.

[0085] Table 1 Performance of Examples 1-3 and Comparative Examples 1-2

[0086] The above is only a preferred specific implementation method of the present application, but the scope of protection of the present application is not limited thereto. Any changes or replacements that can be easily thought of by any technician familiar with this technical field within the technical scope disclosed in this application should be covered by the scope of protection of the present application.

Claims

1. A Ni3Al / carbide composite material powder, characterized in that: The chemical composition is as follows by mass percentage: Al: 9.5% to 10.0%, C: 1.1% to 1.6%, Cr: 18.0% to 19.5%, B: 0.05% to 0.07%, O≤200ppm, N≤50ppm, H≤10ppm, and the balance is Ni; In the Ni3Al / carbide composite material powder, the atomic ratio of nickel equivalent to aluminum equivalent is 2.5 to 2.9, and the Ni3Al / carbide composite material powder contains NiAl phase. The carbide structure of the Ni3Al / carbide composite material powder is Cr7C3, and the mass content of Cr7C3 is 13% to 18%.

2. The composite material powder according to claim 1, characterized in that: The particle size of the Ni3Al / carbide composite material powder ranges from 53 μm to 124 μm.

3. A laser cladding method for Ni3Al / carbide composite material powder according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: using a coaxial powder feeding method to deliver Ni3Al / carbide composite material powder to the surface of the steel material; Step 2: Using a laser cladding method, the Ni3Al / carbide composite material powder is clad on the surface of the steel material to form an in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer.

4. The laser cladding method according to claim 3, characterized in that: The coaxial powder feeding amount of the coaxial powder feeding method is 10 g / min to 30 g / min.

5. The laser cladding method according to claim 3, characterized in that: The power of the laser cladding is 1400W to 2600W, and the scanning speed is 0.12m / min to 0.60m / min.

6. The laser cladding method according to claim 3, characterized in that: The laser beam of the laser cladding method is a circular spot or a rectangular spot.

7. An in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer, characterized in that: The in-situ self-generated carbide-reinforced Ni3Al-based alloy strengthening layer is formed on the surface of the steel material by a laser cladding method. The Ni3Al-based alloy strengthening layer includes a Ni3Al phase, a NiAl phase and a carbide Cr7C3. The carbide Cr7C3 is dispersed in the Ni3Al phase. The average hardness of the Ni3Al-based alloy strengthening layer is 620-680 HV, and the wear rate is ≤0.8×10 -5 mm 3 / (N·m), and the shear strength of the bonding interface with steel materials is 400~600MPa.

8. The in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer according to claim 7, characterized in that: The Ni3Al-based alloy strengthening layer is produced by the laser cladding method as described in any one of claims 3-6.

9. The in-situ self-generated carbide reinforced Ni3Al-based alloy strengthening layer according to claim 7, characterized in that: The steel material is one of carbon steel, alloy steel, heat-resistant stainless steel and cast iron.

10. An application of Ni3Al / carbide composite material powder, characterized in that: The Ni3Al / carbide composite material powder as described in any one of claims 1 to 2 is used for surface modification of steel or nickel-based alloy parts of heavy-duty diesel engines.

Citation Information

Patent Citations

  • Method for preparing composite coating Ni3Al / Cr3C2 by use of laser cladding technique

    CN104532231A

  • New powder composition and use thereof

    CN107530771A

  • Method for preparing Fe3Al / Cr3C2 composite coating through laser cladding

    CN107988595A

  • Fe3Al / Cr7C3 powder and preparation method thereof and corresponding coating

    CN109986074A

  • In-situ synthesized carbide reinforced Ni3Al-based alloy powder as well as laser cladding method and application thereof

    CN115011843A

Cited By

  • Plasma cladding welding method for arc-shaped coaling plate of potassium mining machine