Composite substrate for surface acoustic wave devices

The composite substrate with a piezoelectric single crystal thin film and an intervening layer addresses energy leakage and spurious noise issues in surface acoustic wave filters, achieving low loss and high reliability by controlling wave attenuation and speed characteristics, thereby enhancing filter performance.

WO2024232192A1PCT designated stage expired Publication Date: 2024-11-14SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013466
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Surface acoustic wave filters using composite substrates suffer from energy leakage and spurious noise due to wave reflection and trapping at the bonding interface, leading to increased loss and deteriorated frequency characteristics.

Method used

A composite substrate comprising a piezoelectric single crystal thin film, a supporting substrate, and an intervening layer with a total thickness less than twice the wavelength of the surface acoustic wave, where the intervening layer has specific attenuation and transverse wave speed characteristics to minimize energy leakage and spurious noise.

Benefits of technology

The solution results in a surface acoustic wave device with reduced loss in the passband and improved reliability, suppressing spurious noise and maintaining high Q values and temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013466_14112024_PF_FP_ABST
    Figure JP2024013466_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a composite substrate for surface acoustic wave devices, the composite substrate comprising: a piezoelectric single crystal thin film; a supporting substrate; and at least one intervening layer that is provided between the piezoelectric single crystal thin film and the supporting substrate. The intervening layer is in contact with the piezoelectric single crystal thin film. The total thickness of the intervening layer is equal to or less than twice the wavelength of the surface acoustic wave. The attenuation of a longitudinal wave in the intervening layer as calculated by a Brillouin oscillation method at a frequency of 40 GHz to 60 GHz is 8 × 10-2 (nm-1∙THz-2) or less. According to the present invention, it is possible to provide a composite substrate for surface acoustic wave devices, the composite substrate having a small loss in the pass band of a filter, a small spurious component, and excellently high performance and high reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Composite substrates for surface acoustic wave devices

[0001] The present invention relates to a composite substrate for a surface acoustic wave device, which comprises a piezoelectric single crystal thin film and a support substrate.

[0002] Mobile phones and the like use surface acoustic wave (SAW) devices, which have interdigital transducers (IDTs) formed on a piezoelectric substrate to excite surface acoustic waves, as frequency adjustment and selection components. Surface acoustic wave devices are required to be small, have low insertion loss, and block unwanted waves. 3 ;LT) and lithium niobate (LiNbO 3 Piezoelectric materials such as ZnO (LiNbO) are used.

[0003] On the other hand, under the communication standards for fourth-generation and later mobile phones, the piezoelectric materials used in surface acoustic wave devices must have sufficiently small temperature-dependent characteristic variations. Furthermore, to prevent unwanted noise from spilling over between bands, filters, duplexers, and multiplexers must have extremely low insertion loss and extremely steep shoulder characteristics, requiring the resonators that make up the filters to have a high Q (Quality Factor). Furthermore, filters must be able to handle a wide bandwidth depending on the band used.

[0004] Regarding materials used in such surface acoustic wave devices, composite substrates made of piezoelectric materials and other materials have been considered. For example, Patent Document 1 discloses an acoustic wave device having a piezoelectric film, the acoustic wave device including a support substrate, a high acoustic velocity film formed on the support substrate and having a bulk wave acoustic velocity faster than the acoustic wave acoustic velocity propagating through the piezoelectric film, a low acoustic velocity film laminated on the high acoustic velocity film and having a bulk wave acoustic velocity slower than the bulk wave acoustic velocity propagating through the piezoelectric film, the piezoelectric film laminated on the low acoustic velocity film, and an IDT electrode formed on one surface of the piezoelectric film.

[0005] Furthermore, Patent Document 2 discloses a piezoelectric element including a support substrate, a medium layer laminated on the support substrate, a piezoelectric body laminated on the medium layer and through which bulk waves propagate, and an IDT electrode formed on one surface of the piezoelectric body, wherein the medium layer is a low-velocity medium in which the propagation velocity of bulk waves, which are the same as the bulk waves that are the main components of the elastic waves, is slower than the sound velocity of the elastic waves that propagate through the piezoelectric body, and an IDT electrode formed on one surface of the piezoelectric body, wherein the medium layer is a low-velocity medium in which the propagation velocity of bulk waves, which are the same as the bulk waves that are the main components of the elastic waves, is faster than the sound velocity of the elastic waves that propagate through the piezoelectric body. and a high-speed medium having a high sound velocity, wherein when the sound velocity of the main vibration mode when the medium layer is formed from the high-speed medium is VH and the sound velocity of the main vibration mode when the medium layer is formed from the low-speed medium is VL, the sound velocity of the main vibration mode in the elastic wave device having the medium layer formed thereon is VL < sound velocity of the main vibration mode < VH, and the thickness of the medium layer is 1λ or more when the period of the IDT is λ.

[0006] Patent No. 5713025 Patent No. 5861789

[0007] However, when a surface acoustic wave filter is fabricated using the composite substrate of Patent Document 1 or Patent Document 2, the energy of the acoustic waves leaks from the piezoelectric body into the low-velocity medium and remains there, resulting in the generation of noise called spurious or ripple within the passband of the surface acoustic wave filter or at higher frequencies. This noise is generated by wave reflection at the bonding interface between the piezoelectric crystal film and the support substrate, or by acoustic waves being trapped in an intervening layer between the piezoelectric crystal film and the support substrate, and is undesirable because it deteriorates the frequency characteristics of the surface acoustic wave filter and causes an increase in loss in the passband of the filter.

[0008] The present invention has been made in view of the above circumstances, and has an object to provide a composite substrate for a surface acoustic wave device that has small loss in the filter passband, few spurious components, excellent performance, and high reliability.

[0009] As a result of extensive research, the inventors discovered that by providing a piezoelectric single crystal thin film, a support substrate, and at least one intervening layer between the piezoelectric single crystal thin film and the support substrate, and by specifying the total thickness of the intervening layer and the attenuation of longitudinal waves, it is possible to reduce loss in the passband of the filter and obtain high reliability, and thus completed the present invention. The gist of the present invention is as follows: [1] A composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intervening layer provided between the piezoelectric single crystal thin film and the support substrate, wherein the intervening layer is in contact with the piezoelectric single crystal thin film, the total thickness of the intervening layer is equal to or less than twice the wavelength of the surface acoustic wave, and the attenuation of longitudinal waves in the intervening layer calculated at frequencies from 40 GHz to 60 GHz by the Brillouin oscillation method is 8×10 -2 (nm -1 ・THz -2 [2] The composite substrate for a surface acoustic wave device according to [1], wherein the sound velocity of a shear wave in the intermediate layer is faster than the sound velocity of a slow shear wave in the piezoelectric single crystal thin film. [3] The piezoelectric single crystal thin film contains 120 ppm or less of iron, and the volume resistivity of the piezoelectric single crystal thin film is 2×10 11 The composite substrate for surface acoustic wave devices according to [1] or [2], wherein the resistivity is Ω·cm or less. [4] The composite substrate for surface acoustic wave devices according to any one of [1] to [3], wherein the intermediate layer is either SiOx (1.8<x<2.05) or SiOyNz (0.02<z / (y+z)<0.1). [5] The composite substrate for surface acoustic wave devices according to any one of [1] to [4], wherein the main component of the piezoelectric single crystal thin film is lithium tantalate or lithium niobate. [6] The composite substrate for surface acoustic wave devices according to any one of [1] to [5], wherein the support substrate is any one of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate. [7] The composite substrate for surface acoustic wave devices according to any one of [1] to [5], wherein the support substrate is composed of a silicon single crystal and a polysilicon layer formed on the silicon single crystal. [8] The content of Li ions in the intervening layer is 1 × 10 17 atom / cm 3 The composite substrate for a surface acoustic wave device according to any one of [1] to [7] below:

[0010] According to the present invention, it is possible to provide a composite substrate for a surface acoustic wave device that has small loss in the filter passband and high reliability.

[0011] FIG. 1 shows SiO 1.7 Fig. 2 is a diagram showing an example of the spectrum of Brillouin oscillations of a thin film. Fig. 2 is a diagram showing a waveform obtained by Fourier transform of only the reflected light of ultrasonic waves (longitudinal waves) in a thin film. Fig. 3 is a diagram showing the dependency relationship between the LSAW sound velocity of a thin film and the value obtained by normalizing the thin film thickness with the wavelength of the ultrasonic waves (thickness of thin film / wavelength), and the calculation result of the sound velocity of an elastic wave obtained by the finite element method. Fig. 4 is a diagram showing the dependency relationship between the LSAW sound velocity of a thin film and the value obtained by normalizing the thin film thickness with the wavelength of the ultrasonic waves (thickness of thin film / wavelength), and the calculation result of the sound velocity of an elastic wave obtained by the finite element method. 1.7 FIG. 5 is a diagram showing an example of a calculation result of the displacement distribution of a wave in which energy is concentrated in the surface layer of a thin film in a thin film / (111)Si substrate configuration. FIG. 5 is a diagram showing an example of a cross-sectional TEM observation photograph of a composite substrate manufactured in Example 1. FIG. 6 is a diagram showing a composite substrate having Al microelectrodes formed on the surface. FIG. 7 is a diagram showing the resonance waveform (input impedance (Zin) and Q value) of a SAW obtained in Example 1. FIG. 8 is a diagram showing the resonance waveform (input impedance (Zin) and Q value) of a SAW obtained in Example 2. FIG. 9 is a diagram showing the resonance waveform (input impedance (Zin) and Q value) of a SAW obtained in Comparative Example 1. FIG. 10 is a diagram showing the resonance waveform (input impedance (Zin) and Q value) of a SAW obtained in Comparative Example 2.

[0012] The composite substrate for a surface acoustic wave device of the present invention will be described in detail below, but the present invention is not limited to the embodiments. Furthermore, a numerical range defined using the symbol "to" is intended to include both the upper and lower limits of the range.

[0013] [Composite Substrate for Surface Acoustic Wave Device] The composite substrate for a surface acoustic wave device of the present invention is a composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intervening layer provided between the piezoelectric single crystal thin film and the support substrate, wherein the intervening layer is in contact with the piezoelectric single crystal thin film, the total thickness of the intervening layer is equal to or less than twice the thickness of the wavelength of the surface acoustic wave, and the attenuation of the longitudinal wave of the intervening layer calculated at frequencies of 40 GHz to 60 GHz by the Brillouin oscillation method is 8×10 -2 (nm -1・THz -2 ) below.

[0014] (Piezoelectric Single Crystal Thin Film) The piezoelectric single crystal thin film in the surface acoustic wave device composite substrate according to one embodiment of the present invention is not particularly limited as long as it can be used as a piezoelectric film. 3 :LT), or lithium niobate (LiNbO 3 :LN). By using the above-mentioned components as the main component of the piezoelectric single crystal thin film, an acoustic wave device with high electromechanical coupling can be obtained. In the present invention, the term "the main component of the piezoelectric single crystal thin film is lithium tantalate or lithium niobate" means that 50 mass % or more of the components constituting the piezoelectric single crystal thin film are lithium tantalate or lithium niobate. Furthermore, the piezoelectric single crystal thin film may contain components other than lithium tantalate and lithium niobate, such as iron and magnesium.

[0015] Furthermore, it is preferable that the piezoelectric single crystal thin film contains 120 ppm or less of iron. By containing a small amount of iron in the piezoelectric single crystal thin film, the electric field at which the polarization of the piezoelectric single crystal thin film is destroyed, i.e., the coercive electric field, increases, making it possible to make the polarization less likely to be destroyed. From the above points of view, the iron content is more preferably 10 ppm or more and 120 ppm or less, and even more preferably 50 ppm or more and 100 ppm or less.

[0016] In addition, the initial volume resistivity of the piezoelectric single crystal thin film is 2×10 11 It is preferable that the initial volume resistivity of the piezoelectric single crystal thin film is 2×10 11 When the resistivity is Ω·cm or less, the constant temperature resistance of the composite substrate for a surface acoustic wave device of the present invention can be improved. 10 Ω・cm or more 2×10 11 It is more preferable that the resistivity is Ω cm or less, and 2×10 10 Ω・cm or more 1×10 11 It is more preferable that the resistivity is Ω·cm or less.

[0017] (Support Substrate) The support substrate in the surface acoustic wave device composite substrate according to one embodiment of the present invention can be any of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate. A surface acoustic wave resonator manufactured using a surface acoustic wave device composite substrate using any of the above substrates as the support substrate has a high Q value, further suppresses out-of-band spurious emissions, and provides a surface acoustic wave device with excellent temperature characteristics.

[0018] The support substrate may be made of single crystal silicon and a polysilicon layer formed on the single crystal silicon. By appropriately adjusting the thickness of the polysilicon layer of the support substrate, out-of-band spurious emissions can be further suppressed. The thickness of the polysilicon layer is preferably 0.2 μm or more and 2 μm or less, more preferably 0.5 μm or more and 1.9 μm or less, and even more preferably 0.5 μm or more and 1.2 μm or less.

[0019] (Intervening Layer) The surface acoustic wave device composite substrate of the present invention includes an intervening layer between the piezoelectric single crystal thin film and the support substrate, and the intervening layer is provided in contact with the piezoelectric single crystal thin film. The intervening layer in the surface acoustic wave device composite substrate of one embodiment of the present invention is preferably either SiOx (1.8<x<2.05) or SiOyNz (0.02<z / (y+z)<0.1). The surface acoustic wave device composite substrate of the present invention also includes at least one intervening layer. The intervening layer may be one layer or two or more layers, and in the case of two or more layers, the layers may be made of the same material or different materials.

[0020] The content of Li ions in the intervening layer is 1×10 17 atom / cm 3 Li ions mainly diffuse from the piezoelectric single crystal thin film to the intermediate layer, and the content of Li ions in the intermediate layer is preferably 1×10 or less. 17 atom / cm 3By setting the thickness to the value below, it is possible to prevent the intermediate layer from softening and to suppress in-band and out-of-band spurious emissions.

[0021] Furthermore, the thickness of the intermediate layer is, when there is one intermediate layer, the thickness of the intermediate layer itself, and when there are two or more intermediate layers, the total thickness is equal to or less than twice the wavelength of the surface acoustic wave of the intermediate layer. If the thickness of the intermediate layer exceeds twice the wavelength of the surface acoustic wave of the intermediate layer, the acoustic wave is more likely to be trapped within the intermediate layer, resulting in a problem of increased out-of-band spurious. The total thickness of the intermediate layer is preferably equal to or less than twice the wavelength of the surface acoustic wave, and more preferably equal to or less than twice the wavelength.

[0022] In addition, the attenuation of longitudinal waves in the intervening layer calculated at frequencies of 40 GHz to 60 GHz by the Brillouin oscillation method was 8×10 -2 (nm -1 ・THz -2 ) or less. If the acoustic attenuation of the longitudinal wave in the intermediate layer is large, the acoustic wave is likely to be trapped in the intermediate layer. In this case, the surface acoustic wave resonator made of the composite substrate for a surface acoustic wave device of the present invention will have the problem of increased spurious out-of-band. -2 (nm -1 ・THz -2 ) or less, the Q value of the surface acoustic wave resonator is high, and out-of-band spurious can be further suppressed. The attenuation of longitudinal waves in the intermediate layer is 2×10 -2 (nm -1 ・THz -2 ) or less, and -2 (nm -1 ・THz -2 ) or less is more preferable.

[0023] Furthermore, it is preferable that the acoustic velocity of the shear waves in the intervening layer be faster than the acoustic velocity of the slow shear waves in the piezoelectric single crystal thin film. By making the shear wave (bulk wave) velocity in the intervening layer faster than the slow shear wave (bulk wave) in the piezoelectric single crystal thin film, the passband loss of the surface acoustic wave filter obtained using the composite substrate for surface acoustic wave devices can be improved. If the shear wave velocity in the intervening layer is slower than the slow shear wave in the piezoelectric single crystal thin film, there is a concern that the acoustic wave may be easily trapped within the intervening layer. Furthermore, since the piezoelectric single crystal thin film is an anisotropic material, there are two types of shear waves in the piezoelectric single crystal thin film: fast shear waves and slow shear waves.

[0024] For example, LiTaO as an example of a piezoelectric single crystal thin film 3 In this case, 46° rotated Y-cut LiTaO 3 The slow shear wave is 3330 m / s. 1.85 , or SiO 1.94 N 0.06 In the formula, SiO 1.85 , or SiO 1.94 N 0.06 The sound velocities of the shear waves in SiO are high, at 3850 m / s and 3750 m / s, respectively. 1.85 , or SiO 1.94 N 0.06 The acoustic velocity of the shear wave of LSAW in the piezoelectric single crystal thin film will be described in detail later, but can be determined from the measured acoustic velocity of the shear wave of LSAW in the piezoelectric single crystal thin film by a linear convergent beam acoustic microscope and an analysis by the finite element method, as described in, for example, Tatsuya Omori1, Kensuke Sakamoto, Satoshi Suzuki, Jun-ichi Kushibiki, Satoru Matsuda, and Ken-ya Hashimoto, "Characterization of Elastic Properties of SiO2 Thin Films by Ultrasonic Microscopy." 1.85 , or SiO 1.94 N 0.06 and the piezoelectric single crystal thin film was LiTaO 3 By doing so, the sound velocity of the transverse waves in the intervening layer can be made faster than the sound velocity of the slow transverse waves in the piezoelectric single crystal thin film.

[0025] In addition, the attenuation of the longitudinal wave in the intermediate layer calculated at frequencies of 40 GHz to 60 GHz by the Brillouin oscillation method was found to be 0.01%. 1.85 is that the attenuation is 1.2 × 10 -2 (nm -1 ・THz -2 ), SiO 1.94 N 0.06 The attenuation is 0.1 × 10 -2 (nm -1 ・THz -2 ) and the attenuation of the longitudinal wave is 8 × 10 -2 (nm -1 ・THz -2 ) can be as follows:

[0026] Here, the Brillouin oscillation method can be performed using the method described in H. Ogi et al., "Elastic constant and Brillouin oscillations in sputtered vitreous SiO2 thin films", PHISICAL REVIEW B 78, 13204 (2008). 1.7 In this case, the SiO 1.7 An example of the spectrum of Brillouin oscillations of a thin film is shown.

[0027] SiO used in the measurement of Figure 1 1.7 The thin film (hereinafter simply referred to as "thin film") is made of SiO.sub.2 having the same composition and by the same manufacturing method as the intermediate layer. 1.7 A thin film was formed on a Si substrate to a thickness of 1055 nm (the thickness is defined as d), and then SiO 1.7 An Al film of 10 nm was formed on the thin film. The method for producing the thin film is not particularly limited, but may be, for example, a CVD method. 1.7 Ultra-short pulsed light is irradiated onto a structure consisting of a thin film and a Si substrate to generate ultra-high frequency ultrasonic waves. Furthermore, delayed pulsed light with a reference wavelength (λ) of 400 nm is irradiated. The longitudinal wave velocity of the thin film can be determined by detecting the light diffracted by the ultrasonic waves within the thin film.

[0028] At this time, the density of the thin film and the refractive index at 400 nm were determined in advance. The refractive index (n) of the thin film at 400 nm was found to be 1.728 by the prism coupler method. The density (ρ) of the thin film was also found to be 2300 kg / m by XPS (X-ray photoelectron spectroscopy). 3 The first half of the Brillouin spectrum shown in Figure 1 shows the intensity of reflected light due to diffraction by ultrasonic waves (longitudinal waves) within the thin film. By performing a Fourier transform on only the light reflected by ultrasonic waves (longitudinal waves) within the thin film, the frequency of the ultrasonic waves (longitudinal waves) within the thin film shown in Figure 2 can be obtained. From Figure 2, the frequency (f) of the ultrasonic waves (longitudinal waves) within the thin film can be calculated to be 54.5 GHz.

[0029] At this time, the sound velocity vl of the ultrasonic waves (longitudinal waves) in the thin film can be calculated by the following formula (1): vl = f × λ / (2 × n) Formula (1) The sound velocity of the ultrasonic waves (longitudinal waves) in the thin film shown in Figure 2 calculated by formula (1) was 6,325 m / s. In addition, the elastic constant C11 of the thin film can be calculated by vl = √(C11 / ρ), and the elastic constant C11 of the thin film was found to be 92 GPa.

[0030] Next, SiO 1.7 A method for determining the shear wave velocity of a film using a linear convergent beam acoustic microscope and the finite element method will now be described. First, using a linear convergent beam acoustic microscope, as described in the aforementioned Tatsuya Omori1, Kensuke Sakamoto, Satoshi Suzuki, Jun-ichi Kushibiki, Satoru Matsuda, and Ken-ya Hashimoto, "Characterization of Elastic Properties of SiO2 Thin Films by Ultrasonic Microscopy," the LSAW sound velocity of the thin film was measured at frequencies ranging from 160 MHz to 275 MHz, and the dependence of the film thickness normalized to the ultrasonic wavelength (thickness / wavelength) was determined. A diagram of this relationship is shown in Figure 3.

[0031] The LSAW sound velocity (vertical axis) measured by a linear convergent beam acoustic microscope in FIG. 3 is the same as that of the intermediate layer, and is the same as that of the SiO 1.7A thin film was formed on a Si (111) oriented substrate with a thickness of 2830 nm, and the SiO was then applied to the substrate via pure water as a couplant so that the linear convergent beam of the linear convergent beam ultrasonic microscope was shifted 45 degrees clockwise from the (110) direction in the Si substrate plane as viewed from the thin film side. 1.7 This was obtained by propagating LSAW on the surface layer of a thin film / Si substrate structure.

[0032] On the other hand, using the two-dimensional finite element method, SiO 1.7 A ZnO film and an Al electrode, which are sufficiently thin compared to the electrode period, are placed on the surface of the thin film of the thin film / (111) Si substrate structure. An elastic wave is excited in a direction shifted 45 degrees clockwise from the <110> direction of the Si of the thin film-attached Si substrate. The wavelength determined by the electrode period is changed in the model of the finite element method calculation to obtain the SiO 1.7 The relationship between the acoustic wave velocity of the thin film / (111) Si substrate structure and the intervening layer normalized by wavelength was calculated. 1.7 Because the elastic constant C12 of the thin film is an unknown quantity, a tentative value was input for C12, and C12 was determined so as to match the measurement results of the LSAW sound velocity using a linear convergent beam acoustic microscope shown in Figure 3. The other constants (C11, ρ) were calculated using the values ​​mentioned above.

[0033] The C12 calculated above was 20 GPa. 1.7 The results of calculation of the acoustic velocity of the elastic wave by the finite element method when the elastic constant C12 of the thin film is 20 GPa are shown in Figure 3. As an example, in a calculation model by the finite element method when the elastic wave wavelength is 18 μm, the elastic wave is 1.7 FIG. 4 shows an example of the calculation result of the displacement distribution of a wave whose energy is concentrated on the surface layer of a thin film having a thin film / (111) Si substrate structure.

[0034] From the above considerations, SiO 1.7 The shear wave acoustic velocity Vs (=√((C11-C12) / ρ)) of the thin film alone was calculated, and Vs = 3960 m / s was obtained. In the calculation model using the finite element method of the present application, the elastic constants of the Si substrate, ZnO film, and Al film were the values ​​given in the Surface Acoustic Wave Data Book (edited by the Japan Electronics Industry Association), (p. 66 (ZnO), p. 165 (Si), p. 172 (Al)).

[0035] Furthermore, in the study of this application, as an original attempt, attention was paid to the fact that the reflected light intensity due to diffraction by ultrasonic waves (longitudinal waves) in the thin film layer, which is the first half of the Brillouin spectrum shown in Figure 1, attenuates exponentially with time. That is, in the envelope of the reflected light intensity shown by the dotted line in Figure 1, if the amplitude intensity at time 0 psec is A0 and the amplitude intensity at the time when the ultrasonic waves reach Si is A, the attenuation constant (β) of the ultrasonic waves (longitudinal waves) in the thin film is expressed by equation (2): A = A0 exp(-β f 2 d) ...Equation (2) In the case of Figure 2, A0 was 0.03 and A was 0.004. From the above, the damping constant β is calculated from equation (3). β = -1 / (f 2 d) In(A / A0) Equation (3) In the case of Figure 2, β is 10.8 × 10 -2 (nm -1 ・THz -2 ) was.

[0036] For the various interlayers described above, longitudinal wave attenuation was calculated using the Brillouin oscillation method at frequencies between 40 GHz and 60 GHz using the same method. When the interlayer exhibits high longitudinal wave attenuation, acoustic waves are more likely to be trapped within the interlayer. In this case, it was confirmed that surface acoustic wave resonators made of composite substrates for surface acoustic wave devices suffer from increased out-of-band spurious emissions. On the other hand, when the interlayer of the present invention has a high acoustic velocity and low longitudinal wave attenuation, acoustic waves are unable to concentrate excessively on the interlayer, allowing wave energy to be concentrated in the piezoelectric single crystal thin film. Therefore, surface acoustic wave resonators using the composite substrate for surface acoustic wave devices of the present invention have a high Q value, further suppressing out-of-band spurious emissions, which is preferable.

[0037] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to these examples.

[0038] Example 1 A polysilicon layer was formed to a thickness of 1.7 μm on the surface of a high-resistivity silicon substrate having a diameter of 150 mm and a (111) orientation.

[0039] Next, a melt with a composition in which the amount of lithium was reduced based on the amount of lithium contained in the lithium tantalate crystal of the congruent composition was prepared, and an iron-substituted lithium tantalate crystal was grown from the melt with the prepared composition. The amount of iron added was adjusted so that the iron content in the iron-substituted lithium tantalate crystal was 95 mass ppm, and a 6-inch iron-containing 42° Y-cut lithium tantalate (LT) substrate was prepared. The iron-containing 42° Y-cut lithium tantalate (LT) substrate was subjected to a reduction treatment to reduce the volume resistivity to 2.2×10 10 The resistance was adjusted to Ω·cm.

[0040] Next, hydrogen molecular ions were implanted into the 6-inch iron-containing lithium tantalate (LT) substrate from the side of the surface to be bonded. The dose was 9×10 16 atm / cm 2 The acceleration voltage was 160 KeV. Subsequently, a 0.4 μm thick layer of SiO 2 was formed on the ion-implanted surface of a 6-inch iron-containing lithium tantalate (LT) substrate into which hydrogen molecular ions had been implanted. 1.85 The intermediate layer was formed by CVD. Then, the silicon substrate on which the polysilicon layer was formed and a 0.4 μm thick SiO 1.85 The iron-containing LT substrate having the intervening layer was subjected to surface activation treatment by plasma treatment. 1.85 The iron-containing LT substrate was bonded to the substrate with an intervening layer made of the compound.

[0041] Next, the bonded body was heat-treated at 350°C under nitrogen to prevent the introduction of crystal defects due to misalignment at the bonding interface. The heat-treated bonded body was then heated to 110°C, and a wedge was driven into one end of the ion-implanted portion of the iron-containing lithium tantalate (LT) substrate to separate it into the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate and the remaining iron-containing lithium tantalate (LT) substrate. The thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate after separation was measured using a spectrophotometer and found to be 0.52 μm. Next, the composite substrate consisting of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was heated at 500°C for 6 hours.

[0042] Furthermore, the surface layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film of the composite substrate was polished by 20 nm, and the thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was measured using a spectrophotometer, and it was found to be 0.5 μm. Figure 5 shows an example of a cross-sectional TEM observation photograph of the composite substrate of Example 1 manufactured by the above method, and Figure 5(b) is a further enlarged photograph of a part of Figure 5(a).

[0043] The intermediate layer (SiO 1.85 The amount of Li in the SiO layer was measured by secondary ion mass spectrometry (SIMS). 1.85 The amount of Li in the layer is up to 2 × 10 16 atom / cm 3 In addition, the intermediate layer (SiO 1.85 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0044] Furthermore, an intermediate layer (SiO 1.85 The density of the layer was determined by XPS (X-ray photoelectron spectroscopy) and found to be 2240 g / cm 3 In addition, the intervening layer (SiO 1.85 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.85 The longitudinal wave velocity in the layer is 6200 m / s, and the acoustic attenuation rate is 1.2 × 10 at 55 GHz.-3 (nm -1 ・THz -2 ) In addition, the intermediate layer (SiO 1.85 The shear wave velocity of the intervening layer (SiO 1.85 The shear wave velocity of the single layer was 3850 m / s.

[0045] Next, an Al film was sputtered to a thickness of 0.14 μm on the surface of the composite substrate obtained above, and after applying a resist, a resist pattern with a line width of approximately 0.5 μm was formed by i-line exposure. Then, the Al was etched by dry etching to form the first layer of a one-port SAW resonator. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.85 The thickness of the second layer (layer) is 0.2 wavelengths. Furthermore, a second layer of pads with an Al film thickness of 0.6 μm was formed on the composite substrate by the lift-off method. Figure 6 shows the composite substrate with Al microelectrodes formed on its surface.

[0046] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 7. The resonance frequency (fr), anti-resonance frequency (fa), and electromechanical coupling coefficient (k 2 ), maximum Q value (Qmax), amplitude of input impedance (ΔZ), fractional bandwidth value (fractional bandwidth = (anti-resonance frequency - resonance frequency) / resonance frequency), and spurious intensity between 2400 and 2800 MHz are shown in Table 1.

[0047]

[0048] Next, the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again using a network analyzer. The resulting characteristics were the same as those in Table 1. Furthermore, this 350°C hot plate heating, cooling, and measurement were repeated for a total cumulative time of 4 hours, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were no different from those in Table 1.

[0049] (Example 2) In Example 1, the thickness was 0.4 μm and the composition was SiO 1.85 Instead of the intermediate layer having a thickness of 0.3 μm and a composition of SiO 1.94 N 0.06 A composite substrate was prepared in the same manner as in Example 1, except that an intervening layer of iron-containing lithium tantalate (LT) was used.

[0050] The intervening layer (SiO 1.94 N 0.06 The amount of Li in the layer was measured by secondary ion mass spectrometry (SIMS). 1.94 N 0.06 The amount of Li in the layer is 1×10 14 atom / cm 3 Furthermore, the intermediate layer (SiO 1.94 N 0.06 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0051] In addition, the LT layer of a composite substrate made of an iron-containing lithium tantalate (LT) piezoelectric single crystal thin film bonded to a silicon substrate was removed, and the intervening layer (SiO 1.94 N 0.06 The density of the intermediate layer (SiO 1.94 N 0.06 The density of the layer is 2210 g / cm3 In addition, the LT layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate was removed, and the intermediate layer (SiO 1.94 N 0.06 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.94 N 0.06 The longitudinal wave velocity in the layer is 6190 m / s, and the acoustic attenuation rate is 1.2 × 10 at 55 GHz. -3 (nm -1 ・THz -2 ) In addition, the intermediate layer, SiO 1.94 N 0.06 The shear wave acoustic velocity of the layer alone was determined by combining the linear convergent beam acoustic microscope and finite element analysis. 1.94 N 0.06 The shear wave velocity of the layer alone was 3750 m / s.

[0052] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 8. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.94 N 0.06 The thickness of the layer is 0.15 wavelength. The resonant frequency (fr), anti-resonant frequency (fa), and electromechanical coupling coefficient (k 2 ), the maximum value of Q (Qmax), the amplitude of the input impedance (ΔZ), the value of the relative bandwidth, and the spurious intensity between 2400 and 2800 MHz are shown in Table 1.

[0053]

[0054] Next, an iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to a silicon substrate with a one-port SAW resonator pattern, fabricated in the same manner as in Example 1, was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again using a network analyzer. The resulting characteristics were the same as those in Table 2. Furthermore, this 350°C hot plate heating, cooling, and measurement were repeated for a cumulative time of 4 hours, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were unchanged from those in Table 2.

[0055] Comparative Example 1 A polysilicon layer was formed to a thickness of 1.7 μm on the surface of a high-resistivity silicon substrate having a diameter of 150 mm and a (111) orientation.

[0056] Next, the amount of lithium in the melt was adjusted to a composition in which it was reduced based on the amount of lithium contained in the lithium tantalate crystal of the congruent composition, and an iron-substituted lithium tantalate crystal was grown from the melt of the adjusted composition. A 6-inch iron-containing 42° Y-cut lithium tantalate (LT) substrate was prepared by adding iron in an amount such that the iron content in the iron-substituted lithium tantalate crystal was 95 ppm by mass. The iron-containing 42° Y-cut lithium tantalate (LT) substrate was subjected to a reduction treatment to reduce the volume resistivity to 2.2×10 10 The resistance was adjusted to Ω·cm.

[0057] Next, hydrogen molecular ions were implanted into the 6-inch iron-containing lithium tantalate (LT) substrate from the side of the surface to be bonded. The dose was 9×10 16 atm / cm 2 The acceleration voltage was 160 KeV. Subsequently, a 0.4 μm thick layer of SiO 2 was formed on the ion-implanted surface of a 6-inch iron-containing lithium tantalate (LT) substrate into which hydrogen molecular ions had been implanted. 1.7 The intermediate layer was formed by CVD. Then, the silicon substrate on which the polysilicon layer was formed and a 0.4 μm thick SiO 1.7The iron-containing LT substrate having the intervening layer using the above-mentioned polysilicon layer was subjected to surface activation treatment by plasma treatment. 1.7 The iron-containing LT substrate was bonded to the substrate with an intervening layer made of the above.

[0058] Next, the bonded body was heat-treated at 350°C under nitrogen to prevent the introduction of crystal defects due to misalignment at the bonding interface. The heat-treated bonded body was then heated to 110°C, and a wedge was driven into one end of the ion-implanted portion of the iron-containing lithium tantalate (LT) substrate to separate it into the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the support substrate and the remaining iron-containing lithium tantalate (LT) substrate. The thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate after separation was measured using a spectrophotometer and found to be 0.52 μm. Next, the composite substrate consisting of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film bonded to the silicon substrate was heated at 500°C for 6 hours.

[0059] Furthermore, the surface layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film of the composite substrate was polished by 20 nm, and the thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was measured using a spectrophotometer, and was found to be 0.5 μm.

[0060] The intermediate layer (SiO 1.7 The amount of Li in the SiO layer was measured by secondary ion mass spectrometry (SIMS). 1.7 The amount of Li in the layer is up to 2 × 10 17 atom / cm 3 The intermediate layer (SiO 1.7 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0061] In addition, the intermediate layer (SiO 1.7 The density of the layer was determined by XPS (X-ray photoelectron spectroscopy) and found to be 2240 g / cm 3 In addition, the intervening layer (SiO 1.7The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.7 The longitudinal wave velocity in the layer is 6325 m / s, and the acoustic attenuation rate is 10.8 × 10 at 55 GHz. -2 (nm -1 ・THz -2 ) In addition, the intermediate layer (SiO 1.7 The shear wave velocity of the intervening layer (SiO 1.7 The shear wave velocity of the single layer was 3960 m / s.

[0062] Next, an Al film was sputtered to a thickness of 0.14 μm on the surface of the composite substrate obtained above, and after applying a resist, a resist pattern with a line width of approximately 0.5 μm was formed by i-line exposure. The Al was then etched by dry etching to form the first layer of a one-port SAW resonator. Furthermore, a second layer pad portion with an Al film thickness of 0.6 μm was formed on the composite substrate by the lift-off method. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.7 The thickness of the layer is 0.2 wavelengths.

[0063] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 9. The resonance frequency (fr), anti-resonance frequency (fa), and electromechanical coupling coefficient (k 2 ), the maximum value of Q (Qmax), the amplitude of the input impedance (ΔZ), the value of the relative bandwidth, and the spurious intensity between 2400 and 2800 MHz are shown in Table 3.

[0064]

[0065] Next, the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again using a network analyzer. The resulting characteristics were the same as those in Table 3. Furthermore, this 350°C hot plate heating, cooling, and measurement were repeated for a total of 4 hours of cumulative heating at 350°C, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were no different from those in Table 3.

[0066] Comparative Example 2 A polysilicon layer was formed to a thickness of 1.7 μm on the surface of a high-resistivity silicon substrate having a diameter of 150 mm.

[0067] Next, an iron-free lithium tantalate crystal was grown on the lithium tantalate crystal of the congruent composition. The iron-free lithium tantalate crystal was processed to prepare a 6-inch iron-free 42° Y-cut lithium tantalate (LT) substrate. The iron-free 42° Y-cut lithium tantalate (LT) substrate was subjected to a reduction treatment to reduce the volume resistivity to 2.2× 10 The resistance was adjusted to Ω·cm.

[0068] Next, hydrogen molecular ions were implanted into the 6-inch iron-free lithium tantalate (LT) substrate from the surface to be bonded. The dose was 9×10 16 atm / cm 2 The acceleration voltage was 160 KeV.

[0069] Next, a 0.4 μm thick film having a composition of SiO was applied to the ion-implanted surface of a 6-inch iron-free lithium tantalate (LT) substrate. 2 The intermediate layer was formed by CVD. Then, the silicon substrate on which the polysilicon layer was formed and a 0.4 μm thick SiO 2 The iron-free LT substrate having the intervening layer using the above-mentioned polysilicon layer was subjected to surface activation treatment by plasma treatment. 2 The iron-free LT substrate was bonded to the substrate with an intervening layer made of the compound.

[0070] Subsequently, the surface layer of the bonded body (bonded substrate) was removed by grinding and polishing. The thickness of the iron-free lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the thinned silicon substrate was measured using a spectrophotometer and found to be 0.5 μm.

[0071] The intermediate layer (SiO 2 The amount of Li in the SiO layer was measured by secondary ion mass spectrometry (SIMS). 2 The amount of Li in the layer is up to 5 × 10 19 atom / cm 3 The intermediate layer (SiO 2 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0072] In addition, the LT layer of the composite substrate manufactured by the above method was removed, and the intermediate layer (SiO 2 The density of the intermediate layer (SiO 2 The density of the layer is 2100 g / cm 3 The LT layer of the composite substrate was removed, and the intermediate layer (SiO 2 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 2 The longitudinal wave velocity in the layer is 5400 m / s, and the acoustic attenuation rate is 5 x 10 at 55 GHz. -1 (nm -1 ・THz -2 ) In addition, the intermediate layer, SiO 2 The shear wave acoustic velocity of the layer alone was determined by combining the linear convergent beam ultrasonic microscope and finite element analysis. 2 The shear wave velocity of the layer alone was 3150 m / s.

[0073] Next, the electrical characteristics of the one-port SAW resonator on the iron-free lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 10. The resonance frequency (fr), anti-resonance frequency (fa), and electromechanical coupling coefficient (k 2 ), the maximum value of Q (Qmax), the amplitude of the input impedance (ΔZ), the relative bandwidth, and the spurious intensity between 2400 and 2800 MHz are shown in Table 4. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 2 The thickness of the layer is 0.2 wavelengths.

[0074]

[0075] Next, the iron-free lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again using a network analyzer. The resulting characteristics were the same as those in Table 4. Furthermore, this 350°C hot plate heating, cooling, and measurement were repeated for a total of four hours of cumulative heating at 350°C, and the electromechanical coupling coefficient (k 2 ) begins to decrease from the value in Table 3, and after a cumulative heating time of 4 hours, the electromechanical coupling coefficient (k 2 ) had decreased to 5%.

Claims

1. A composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intermediate layer provided between the piezoelectric single crystal thin film and the support substrate, the intermediate layer being in contact with the piezoelectric single crystal thin film, the total thickness of the intermediate layer being equal to or less than twice the wavelength of the surface acoustic wave, and the attenuation of the longitudinal wave of the intermediate layer calculated at frequencies between 40 GHz and 60 GHz by the Brillouin oscillation method being equal to or less than 8 x 10 -2 (nm -1 ・THz -2 ) or less.

2. The composite substrate for surface acoustic wave devices according to claim 1, wherein the sound velocity of the shear waves in said intermediate layer is faster than the sound velocity of the slow shear waves in said piezoelectric single crystal thin film.

3. The piezoelectric single crystal thin film contains 120 ppm or less of iron, and the volume resistivity of the piezoelectric single crystal thin film is 2×10 11 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein the resistivity is Ω·cm or less.

4. The composite substrate for surface acoustic wave devices according to claim 1 or 2, wherein the intermediate layer is any one of SiOx (1.8<x<2.05) and SiOyNz (0.02<z / (y+z)<0.1).

5. A composite substrate for surface acoustic wave devices according to claim 1 or 2, wherein the main component of said piezoelectric single crystal thin film is lithium tantalate or lithium niobate.

6. The composite substrate for a surface acoustic wave device according to claim 1 or 2, wherein the supporting substrate is any one of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate.

7. The composite substrate for a surface acoustic wave device according to claim 1 or 2, wherein the supporting substrate is made of a silicon single crystal and a polysilicon layer formed on the silicon single crystal.

8. The content of Li ions in the intermediate layer is 1×10 17 atom / cm 3 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein:

Citation Information

Patent Citations

  • Elastic wave apparatus and method for manufacturing the same

    JP5713025B2

  • Elastic wave device

    JP5861789B2

  • Composite substrate for surface acoustic wave device, manufacturing method and surface acoustic wave device

    CN113872557A

  • Composite substrate for surface acoustic wave device and manufacturing method thereof

    JP2021005785A

  • Composite substrate for surface acoustic wave device and method for manufacturing the same