Ethylene-vinyl alcohol copolymer composition and method for producing same, pellet, film, and method for producing same
The incorporation of a silicone mixture into the EVOH resin composition addresses thermal instability and adhesion issues, enhancing film formability and long-run performance, thereby improving productivity and film quality.
Patent Information
- Application Number
- PCT/JP2024/016774
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
EVOH resin tends to deteriorate easily due to heat during melt molding, leading to thermal degradation and reduced productivity in extrusion molding, especially with complex equipment and higher functionality demands, and existing solutions either improve melt fluidity but poor in extrusion molding or maintain long-run properties but suffer from thermal instability.
Incorporating a silicone mixture into the EVOH resin composition, which reduces metal adhesion between the resin and processing machine surfaces, improving long-run performance and film formability by using a silicone blend with dry silica and ensuring the silicone mixture remains solid at elevated temperatures.
The EVOH resin composition with a silicone mixture enhances film formability, reduces thermal degradation, and maintains excellent long-run properties, improving productivity and film formation quality by minimizing metal adhesion and viscosity issues.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Ethylene-vinyl alcohol copolymer composition and method for producing the same, as well as pellets, film and method for producing the same
[0001] The present invention relates to an ethylene-vinyl alcohol copolymer (hereinafter, sometimes referred to as "EVOH resin") composition, a method for producing the EVOH resin composition, and pellets, a film, and methods for producing the same.
[0002] EVOH resins are excellent in transparency, gas barrier properties such as oxygen barrier properties, aroma retention properties, solvent resistance, oil resistance, mechanical strength, etc., and are molded into films, sheets, bottles, etc., and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and agricultural chemical packaging materials.
[0003] However, EVOH resins have relatively active hydroxyl groups in their molecules, and therefore tend to be easily deteriorated by heat, which can easily cause discoloration problems during melt molding.
[0004] To address the above-mentioned problems, for example, Patent Document 1 discloses a resin composition containing EVOH resin (A), acetic acid (B), and magnesium acetate and / or calcium acetate (C), wherein the content of (B) is 0.05 parts by mass or less per 100 parts by mass of (A), and the content of (C) is 0.001 to 0.02 parts by mass, calculated as metal, per 100 parts by mass of (A). It is disclosed that use of this resin composition results in molded articles that have excellent long-run properties during melt molding, are less prone to fisheyes, streaks, and discoloration, and have excellent appearance. Furthermore, when the molded articles are used as laminates, odors are reduced, and the laminates also have excellent interlayer adhesion even after secondary processing such as stretching and deep drawing.
[0005] Patent Document 2 discloses a polyarylene sulfide-based resin composition containing, relative to 100 parts by weight of polyarylene sulfide (A), 1 to 50 parts by weight of EVOH resin (B), 1 to 25 parts by weight of a compatibilizer (C) which is one of a modified polysiloxane compound (C1) having at least one functional group selected from the group consisting of an amino group, an epoxy group, and a carboxyl group at both ends and / or a polyisocyanate compound (C2) having two or more isocyanate groups in the molecule, 30 to 250 parts by weight of magnesium hydroxide (D), and 15 to 250 parts by weight of a fibrous filler (E). The document discloses that the use of this resin composition not only provides excellent electrical properties such as tracking resistance, but also excellent toughness, as well as excellent mechanical strength, melt fluidity, mold releasability, and molded product appearance, making it useful for electrical component applications such as electrical and electronic components and automotive electrical components.
[0006] JP 11-106592 A JP 2013-82792 A
[0007] The technology disclosed in Patent Document 1 provides excellent long-run properties during melt extrusion molding, and produces molded products with few fish eyes, streaks, and coloration, and excellent appearance. However, in recent years, extrusion molding devices have become more sophisticated due to the diversification of feedblock and die shapes in extrusion molding devices and demands for various high-performance features, such as thinner multilayer structures and an increased number of layers in final products. As a result, resins tend to thermally deteriorate in extrusion molding devices that have become more complex due to the increased functionality, resulting in a decrease in product productivity (long-run properties), and further improvements are needed.
[0008] The technology disclosed in Patent Document 2 is particularly excellent in toughness, and is also excellent in mechanical strength, melt fluidity, mold releasability, and molded product appearance. However, although it improves melt fluidity and the like in injection molding, it has poor processability in melt extrusion molding, leaving room for improvement.
[0009] In view of this background, the present invention provides an EVOH resin composition that reduces metal adhesion between the EVOH resin and the surfaces of processing machines (barrels, dies, etc.) to prevent excessive deterioration of the resin during film formation, and that has excellent long-run properties and film-forming properties.
[0010] However, in view of these circumstances, the present inventors have conducted extensive research and have found that by incorporating a silicone admixture into a resin composition containing an EVOH resin, metal adhesion during film formation is reduced, and long-term run properties and film formability are improved.
[0011] That is, the present invention has the following aspects. [1] An ethylene-vinyl alcohol copolymer composition containing an ethylene-vinyl alcohol copolymer (A) and a silicone blend (B), wherein the silicone blend (B) is solid at 25°C. [2] The ethylene-vinyl alcohol copolymer composition according to [1], wherein the content of the silicone blend (B) is 0.01 to 5 mass% based on the total mass of the ethylene-vinyl alcohol copolymer (A) and the silicone blend (B). [3] The ethylene-vinyl alcohol copolymer composition according to [1] or [2], wherein the silicone blend (B) contains silicone and dry silica. [4] The ethylene-vinyl alcohol copolymer composition according to [3], wherein the mass ratio of the silicone to the dry silica (silicone / fumed silica) is 90 / 10 to 50 / 50. [5] The ethylene-vinyl alcohol copolymer composition according to [3] or [4], wherein the dry silica is fumed silica. [6] The ethylene-vinyl alcohol copolymer composition according to any one of [1] to [5], wherein the silicone blend (B) is solid at 250°C. [7] A method for producing an ethylene-vinyl alcohol copolymer composition, comprising a step of melt-mixing a raw composition containing an ethylene-vinyl alcohol copolymer (A) and a silicone blend (B), wherein the silicone blend (B) is solid at 25°C. [8] Pellets comprising the ethylene-vinyl alcohol copolymer composition according to any one of [1] to [6]. [9] A film comprising the ethylene-vinyl alcohol copolymer composition according to any one of [1] to [6].
[10] The film according to [9], wherein the silicone blend (B) has a maximum dispersion diameter of 0.1 to 3 μm in the film.
[11] A method for producing a film, comprising a step of melt-molding the pellets according to [8].
[0012] The EVOH resin composition of the present invention reduces the metal adhesion between the EVOH resin and the surface of the processing machine to prevent excessive deterioration of the resin during film formation, and is excellent in long-run properties and film formability.
[0013] The present invention will be described in more detail below based on examples of the present invention, but the present invention is not limited to these examples.
[0014] In this specification, when "X to Y" (X and Y are any numbers) is used, it means "X or more and Y or less," unless otherwise specified, and also includes the meaning of "preferably greater than X" or "preferably smaller than Y." Furthermore, when "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also includes the meaning of "preferably greater than X" or "preferably less than Y." In this specification, "x and / or y (x and y are any constituents or components)" means at least one of x and y, and refers to three combinations: x only, y only, and x and y. With regard to the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values shown in the examples.
[0015] <EVOH Resin Composition> An EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin (A) as a main component and silicone blend (B). That is, the present EVOH resin composition has EVOH resin (A) as a base resin, and the content of EVOH resin (A) in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more. Each component will be described below.
[0016] [EVOH Resin (A)] The EVOH resin (A) used in the present embodiment is a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.
[0017] Vinyl acetate is typically used as the vinyl ester monomer because of its commercial availability and the efficiency of impurity removal during production. Examples of vinyl ester monomers other than vinyl acetate include aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate. Typically, an aliphatic vinyl ester having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms, is used. These are typically used alone, but multiple types may be used simultaneously as necessary.
[0018] The copolymerization of ethylene and vinyl ester monomers can be carried out using any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, but solution polymerization using methanol as a solvent is generally used. The resulting ethylene-vinyl ester copolymer can also be saponified by a known method. The EVOH resin (A) produced in this manner mainly contains ethylene-derived structural units and vinyl alcohol structural units, with a small amount of vinyl ester structural units remaining unsaponified.
[0019] The content of ethylene structural units in the EVOH resin (A) is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural units can be controlled by the ethylene pressure when copolymerizing the vinyl ester monomer with ethylene. If the content is too low, the gas barrier properties and melt moldability under high humidity conditions tend to decrease, while if the content is too high, the gas barrier properties tend to decrease. The content of the ethylene structural units can be measured in accordance with ISO 14663.
[0020] The saponification degree of the EVOH resin (A) is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. The saponification degree can be controlled by the amount, temperature, time, etc. of a saponification catalyst (usually an alkaline catalyst such as sodium hydroxide) used when saponifying the ethylene-vinyl ester copolymer. If the saponification degree is too low, the gas barrier properties, thermal stability, moisture resistance, etc. tend to decrease. The saponification degree of the EVOH resin (A) can be measured in accordance with JIS K6726 (wherein the EVOH resin is used as a solution uniformly dissolved in a water / methanol solvent).
[0021] The melt flow rate (MFR) (210°C, 2160 g load) of the EVOH resin (A) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, stability during film formation tends to be impaired, while if it is too low, the viscosity tends to be too high, making melt extrusion difficult. The MFR is an index of the degree of polymerization of the EVOH resin (A) and can be adjusted by the amount of polymerization initiator and the amount of solvent used when copolymerizing ethylene and a vinyl ester monomer.
[0022] The EVOH resin (A) may further contain structural units derived from the following comonomers (for example, 10 mol % or less of the EVOH resin (A)) within the range that does not impair the effects of the present invention.Examples of the comonomer include olefins such as propylene, 1-butene, and isobutene; hydroxyl group-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, and derivatives thereof such as esters and acylation products; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyloxy-2-methylenepropane; hydroxyalkylvinylidene diacetates such as hydroxy-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, or their salts or mono- or di-alkyl esters in which the alkyl group has 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its acid salts or quaternary salts thereof acrylamides such as methacrylamide, N-alkylmethacrylamides in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidopropanesulfonic acid or a salt thereof, methacrylamidepropyldimethylamine or an acid salt or a quaternary salt thereof; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, and N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; alkyl vinyl ethers in which the alkyl group has 1 to 18 carbon atoms, hydrochloric acid vinyl ethers such as alkoxyalkyl vinyl ether and alkoxyalkyl vinyl ether; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; and comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamido-2-methylpropanesulfonic acid.These may be used alone or in combination of two or more.
[0023] Among these, hydroxy group-containing α-olefins are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the hydroxy group-containing α-olefins are copolymerized, the resulting EVOH resin has primary hydroxyl groups in the side chains. Such EVOH resins having primary hydroxyl groups in the side chains, particularly EVOH resins having a 1,2-diol structure in the side chains, are preferred in that they exhibit good secondary moldability while maintaining gas barrier properties.
[0024] When the EVOH resin (A) used in the present embodiment has a primary hydroxyl group in a side chain, the content of the structural unit derived from a monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol %, of the EVOH resin (A).
[0025] Furthermore, as the EVOH resin (A), EVOH resins that have been "post-modified" by esterification, urethanization, acetalization, cyanoethylation, oxyalkylenation, or the like can also be used.
[0026] When the post-modified EVOH resin is used, the modification rate is usually 10 mol % or less, and preferably 4 mol % or less. If the modification rate of the EVOH resin used is too high, the resin tends to be susceptible to thermal degradation and the long-run properties tend to be reduced.
[0027] Furthermore, the EVOH resin (A) may be a mixture of EVOH resins having different ethylene structural unit contents, saponification degrees, polymerization degrees, copolymerization components, and the like.
[0028] [Silicone mixture (B)] The silicone mixture (B) is a mixture containing silicone as an essential component, and refers to a mixture of silicone (oil) and a thermoplastic resin and / or a particulate carrier such as silica. In particular, the silicone mixture (B) is preferably a mixture of silicone and a particulate carrier such as silica.
[0029] The silicone mixture (B) does not have a melting point, and is preferably solid at 25°C from the viewpoint of handling during processing, and is preferably solid even at a high temperature of 250°C from the viewpoint of film-forming properties. The silicone mixture (B) is preferably in a pellet form from the viewpoint of handling during processing, and is preferably in a solid pellet form at 25 to 250°C. If the silicone mixture (B) becomes liquid at 25°C, the dispersibility of the silicone mixture (B) in the resin composition will be poor, and the effects of the present invention will tend to be difficult to achieve. The pellet diameter of the silicone mixture (B) is preferably 0.5 to 10 mm, more preferably 1 to 6 mm, from the viewpoint of dispersibility of the silicone mixture (B) in the resin composition.
[0030] (Silicone) The silicone, which is an essential component of the silicone mixture (B), is not particularly limited, and specifically includes polydimethylsiloxane, polyphenylmethylsiloxane, methylhydrogenpolysiloxane, and mixtures thereof, among which polydimethylsiloxane and polyphenylmethylsiloxane are preferred, and polydimethylsiloxane is more preferred. These may be used alone or in combination of two or more.
[0031] In addition, in consideration of affinity with the EVOH resin (A), modified silicones may be used, such as modified silicones in which some of the functional groups (side chains or terminals) of poly(diorganosiloxane) are substituted with chlorophenyl groups, alkyl groups, fatty acid ester groups, hydroxy groups, nitrile groups, carboxy groups, amino groups, epoxy groups, fluoroalkyl groups, etc.
[0032] As the silicone, unmodified silicone and modified silicone may be used alone, or two or more types of unmodified silicone and / or modified silicone may be used in combination. However, since modified silicone tends to thicken due to crosslinking under high-temperature extrusion conditions, resulting in poor long-run properties, it is preferable to use unmodified silicone.
[0033] Silicone has the effect of reducing metal adhesion and can reduce stickiness due to bleeding out onto the surface of the EVOH resin (A).5 mm 2 It is preferable to use a high molecular weight silicone having a molecular weight of 1 / s or more and / or a high molecular weight silicone having a weight average molecular weight (Mw) of about 400,000 to 700,000.
[0034] High molecular weight silicones have a smaller change in dynamic viscosity with temperature changes than petroleum-based oils, and their viscosity does not decrease even when the temperature is raised, making them difficult to disperse in other materials. Therefore, from the viewpoint of uniformly dispersing the highly viscous high molecular weight silicone oil and from the viewpoint of improving workability when adding it to a resin, it is preferable to use a pellet-shaped masterbatch that has been mixed in advance with a thermoplastic resin and / or a particulate carrier such as silica.
[0035] For example, the above-mentioned silicone can be supported on a fine particle carrier such as silica (silicon dioxide). Carriers other than silica include carbonates such as calcium carbonate and barium carbonate, silicates such as calcium silicate, barium silicate and magnesium silicate, phosphates such as calcium phosphate, barium phosphate, magnesium phosphate, zirconium phosphate and apatite, metal oxides such as alumina, graphite, zeolite, layered clay minerals, polyethylene, polyurethane, cellulose, polyamide, polyvinyl formal, phenolic resin, epoxy resin, urea resin, etc. These can be used alone or in combination of two or more.
[0036] Examples of the silica particles include dry silica such as fumed silica, calcined silica, and fused silica, precipitated silica, pulverized silica, and calcined silica, and these can be used alone or in combination of two or more. Among them, dry silica is preferred as a carrier from the viewpoint of dispersibility, and fumed silica is more preferred. Examples of commercially available products in which silicone is supported on dry silica include GENIOPLAST™ PELLET S manufactured by Wacker Asahi Kasei Silicone Co., Ltd.
[0037] The average particle size of the silica particles is usually 10 to 400 nm, preferably in the range of 30 to 100 nm. The average particle size used here can be determined as the median diameter (d50, volume basis) based on cumulative distribution from particle size distribution measured by a laser diffraction / scattering method using a commercially available laser diffraction / scattering particle size distribution analyzer. The content ratio of silicone to dry silica contained in the silicone mixture (B) (silicone oil / dry silica) is preferably 90 / 10 to 50 / 50, more preferably 85 / 25 to 60 / 40, and even more preferably 80 / 20 to 70 / 30, from the viewpoint of film-forming properties.
[0038] These silicone mixtures (B) may be used alone or in combination of two or more.
[0039] The content of the silicone mixture (B) is preferably 0.01 to 5% by mass, more preferably 0.05 to 4% by mass, and even more preferably 0.1 to 3% by mass, based on the total mass of the ethylene-vinyl alcohol copolymer (A) and the silicone mixture (B). If the content is too high, the viscosity of the resin when melted decreases, and the fluidity becomes too high, tending to cause vent-up and poor discharge. If the content is too low, the effect of reducing metal adhesion cannot be obtained, and long-run performance tends to be poor.
[0040] The content of the silicone admixture (B) can be measured in terms of silicon by a known analytical method. For example, a certain amount of the EVOH resin composition is weighed, mixed with a flux, and heated to melt. The resulting mixture is dissolved in water to prepare a test solution, and the silicon content is quantified by a molybdenum blue absorbance method. Alternatively, a simpler method can be used in which the EVOH resin of the EVOH resin composition is dissolved by heating in a water / alcohol solvent, and the resulting solution is filtered while hot to obtain a residue. The content of the silicone admixture (B) can be measured from the mass of the residue.
[0041] [Boron Compound] The present EVOH resin composition preferably further contains a boron compound, since this can further enhance the effect of suppressing thickening over time during melt molding.
[0042] Examples of the boron compound include boric acid or a metal salt thereof, such as boric acid, calcium borate, cobalt borate, zinc borate (e.g., zinc tetraborate, zinc metaborate), aluminum potassium borate, ammonium borate (e.g., ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate), cadmium borate (e.g., cadmium orthoborate, cadmium tetraborate), potassium borate (e.g., potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate), silver borate (e.g., silver metaborate, silver tetraborate), copper borate (e.g., cupric borate, copper metaborate, copper tetraborate), sodium borate (e.g., sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate), Examples of suitable borate include lead borate (lead metaborate, lead hexaborate, etc.), nickel borate (nickel orthoborate, nickel diborate, nickel tetraborate, nickel octaborate, etc.), barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), bismuth borate, magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate, etc.), manganese borate (manganese borate, manganese metaborate, manganese tetraborate, etc.), lithium borate (lithium metaborate, lithium tetraborate, lithium pentaborate, etc.), as well as borate minerals such as borax, kernite, inyoite, kotoite, suianite, and seiberite. These may be used alone or in combination of two or more. Of these, borax, boric acid, and sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate, etc.) are preferred.
[0043] The content of the boron compound is not particularly limited, but the lower limit of the content is preferably 1 ppm or more, more preferably 10 ppm or more, particularly preferably 20 ppm or more, and especially preferably 50 ppm or more, calculated as boron relative to the EVOH resin (A). The upper limit of the content is preferably 1000 ppm or less, more preferably 500 ppm or less, particularly preferably 300 ppm or less, and especially preferably 100 ppm or less, calculated as boron relative to the EVOH resin (A). By keeping the content within the above range, it is possible to suppress thickening over time during melt molding. The reason why excellent effects are obtained by using a specific amount of boron compound is not clear, but it is presumed that this is because the dischargeability of the resin composition is improved by adjusting the melt viscosity.
[0044] The content of the boron compound in terms of boron can be measured by a known analytical method. For example, the EVOH resin composition is wet decomposed, and the resulting solution is subjected to a constant volume, and the amount of boron can be quantified by inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0045] [Other Thermoplastic Resins] The EVOH resin composition may contain thermoplastic resins other than the EVOH resin (A) within a range that does not impair the effects of the present invention (for example, typically 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less of the EVOH resin composition). The lower limit is typically 0% by mass. Examples of other thermoplastic resins that can be used include known thermoplastic resins, such as polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, and chlorinated polypropylene. These may be used alone or in combination of two or more.
[0046] [Other Compounding Agents] The EVOH resin composition may contain compounding agents generally compounded with EVOH resins, provided that the effects of the present invention are not impaired. Examples of such compounding agents include inorganic double salts (e.g., hydrotalcite, etc.), plasticizers (e.g., aliphatic polyhydric alcohols such as ethylene glycol, glycerin, and hexanediol), oxygen absorbers (e.g., inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, its fatty acid esters and metal salts, etc.; gallic acid; polyhydric phenols such as hydroxyl group-containing phenolaldehyde resins; terpene compounds; blends of tertiary hydrogen-containing resins and transition metals (e.g., a combination of polypropylene and cobalt); and blends of carbon-carbon unsaturated bond-containing resins and transition metals. Polymeric oxygen absorbers such as blends with transition metals (e.g., a combination of polybutadiene and cobalt), photooxidatively degradable resins (e.g., polyketones), anthraquinone polymers (e.g., polyvinyl anthraquinone), and combinations thereof with the addition of photoinitiators (e.g., benzophenone), antioxidants other than those mentioned above, and deodorants (e.g., activated carbon) may also be added, as well as heat stabilizers, light stabilizers, ultraviolet absorbers, colorants, antistatic agents, surfactants (excluding those used as lubricants), antibacterial agents, antiblocking agents, and fillers (e.g., inorganic fillers). These compounds may be used alone or in combination of two or more.
[0047] [Method for Producing EVOH Resin Composition] The EVOH resin composition can be produced by mixing the EVOH resin (A) and the silicone mixture (B) by a known method, such as a dry blending method or a melt mixing method, and among these, it is preferable to produce the EVOH resin composition by a method including a step of melt mixing a raw material composition containing the EVOH resin (A) and the silicone mixture (B). Furthermore, these production methods can be used in any combination.
[0048] However, since the EVOH resin (A) and the silicone mixture (B) are poorly miscible with each other, the EVOH resin composition of the present invention is usually in a state where the silicone mixture (B) is dispersed as fine particles in the matrix of the EVOH resin (A).
[0049] The dry blending method may be, for example, a method in which pellets of the EVOH resin (A) and the silicone mixture (B) are dry blended using a tumbler or the like.
[0050] Examples of the melt mixing method include (i) a method in which pellet-like EVOH resin (A) and a silicone admixture (B) are dry-blended, and the resulting dry blend is melt-kneaded to obtain pellets or a molded product; and (ii) a method in which a masterbatch in which a silicone admixture is blended in high concentration with EVOH resin is prepared in advance, and this masterbatch is added to molten EVOH resin (A), followed by melt-kneading to obtain pellets or a molded product.
[0051] As described above, these various methods can be combined to obtain the present EVOH resin composition. Among them, method (i) is preferred in terms of productivity and the ability to obtain a resin composition that is more effective in the present invention. When using other thermoplastic resins and other compounding agents, they may be compounded in a conventional manner according to the above-described production method.
[0052] The EVOH resin composition thus obtained may have any shape, but is preferably in the form of pellets. The pellets may be, for example, spherical, oval, cylindrical, cubic, or rectangular, but are typically oval or cylindrical. From the viewpoint of convenience when subsequently used as a molding material, the size of the pellets is such that, in the case of an oval pellet, the minor axis is typically 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the major axis is typically 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In the case of a cylindrical pellet, the diameter of the base is typically 1 to 6 mm, preferably 2 to 5 mm, and the length is typically 1 to 6 mm, preferably 2 to 5 mm. The pellet-like EVOH resin (A) used in each of the above production methods preferably has the same shape and size.
[0053] When the EVOH resin composition is in the form of pellets, it is preferable to adhere a known lubricant to the surface of the pellets in order to stabilize the feedability during melt molding. Examples of lubricants include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, etc.; unsaturated higher fatty acid amides such as oleic acid amide, erucic acid amide, etc.; bis-higher fatty acid amides such as ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low-molecular-weight polyolefins (e.g., low-molecular-weight polyethylene or low-molecular-weight polypropylene with a molecular weight of about 500 to 10,000, or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, and fluorinated ethylene resins. These compounds may be used alone or in combination of two or more. The content of such lubricants in the EVOH resin composition is usually 5% by mass or less, preferably 1% by mass or less. The lower limit is usually 0% by mass.
[0054] The present EVOH resin composition is prepared in various forms, such as pellets, powder, or liquid, and is provided as a molding material for various molded products. In particular, in the present embodiment, when the EVOH resin composition is provided as a material for melt molding, the effects of the present invention tend to be more efficiently obtained, which is preferable.
[0055] The peel strength of the present EVOH resin composition with an aluminum plate is preferably less than 100%, more preferably 95% or less, and even more preferably 90% or less, from the viewpoint of reducing metal adhesion, assuming the peel strength of a system not containing the silicone admixture (B) to be 100%. The lower limit is usually 0%, and is preferably 10% or more, more preferably 50% or more, and even more preferably 80% or more. The peel strength of the present EVOH resin composition with an aluminum plate can be measured, for example, by the method described in the Examples below.
[0056] The viscosity increase rate of the present EVOH resin composition is preferably in the range of 60 to 150%, more preferably 70 to 140%, and even more preferably 75 to 130%, assuming the torque of a system not containing the silicone admixture (B) at 230°C, 50 rpm, and 1 hour to be 100%. Furthermore, the upper limit is preferably 100% or less, more preferably 95% or less, and even more preferably 90% or less. The viscosity increase rate of the present EVOH resin composition can be measured, for example, by the method described in the Examples below.
[0057] The present EVOH resin composition also includes resin compositions obtained by mixing resins other than the EVOH resin (A) used in the present EVOH resin composition.
[0058] The present EVOH resin composition is prepared as a resin composition in various forms, such as pellets or powder, and is provided as a material for various molded articles and multilayer structures. For example, a molded article is produced by melt-molding resin composition pellets. Examples of such molded articles include molded articles (e.g., single-layer films) formed from the present EVOH resin composition, as well as multilayer structures having a layer made of the present EVOH resin composition. The resulting EVOH resin composition exhibits reduced metal adhesion during film formation and excellent long-run properties and film formability, resulting in molded articles and multilayer structures that are also excellent in these respects. When a film is produced as a molded article, it has no thickness unevenness and a good appearance.
[0059] [Molded Article] A molded article according to one embodiment of the present invention (hereinafter referred to as the "present molded article") is obtained by molding the present EVOH resin composition.
[0060] Examples of the shape of the molded article include films, sheets, tapes, cups, trays, tubes, bottles, containers, pipes, filaments, irregular cross-section extrusions, and various irregularly shaped articles.
[0061] The resin composition may be molded by any method that is generally applicable to resin compositions, such as extrusion molding, blow molding, injection molding, and thermoforming.
[0062] The silicone mixture (B) in this molded article is incompatible with the EVOH resin (A) and remains solid rather than melted during molding, so that the silicone mixture (B) is finely dispersed as dispersed particles in the matrix of the EVOH resin (A).Since the silicone mixture (B) is finely dispersed as dispersed particles in the molded article, excellent film-forming properties are achieved.
[0063] Regarding the shape of the dispersed particles of the silicone mixture (B) in such a molded product, the maximum diameter of the dispersed particles is preferably 3 μm or less, more preferably 2.5 μm or less, even more preferably 2 μm or less, and particularly preferably 1.5 μm or less. The lower limit is usually 0.01 μm or more, and preferably 0.1 μm or more. The minimum diameter of the dispersed particles is preferably 2 μm or less, more preferably 1.5 μm, even more preferably 1 μm, and particularly preferably 0.8 μm or less. The lower limit is usually 0.01 μm or more, and preferably 0.1 μm or more. Furthermore, the circular area of the dispersed particles is 3.5 μm or less. 2 Preferably it is less than 3 μm, more preferably it is less than 3 μm 2 More preferably, it is 2 μm or less. 2 Below 1.5 μm, particularly preferably 2 The lower limit is usually 0.01 μm. 2 More preferably, it is 0.05 μm or more. 2The maximum diameter, minimum diameter and circular area of the silicone mixture (B) particles can be measured, for example, by the method described in the Examples below.
[0064] [Multilayer Structure] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the multilayer structure") includes a layer made of the present EVOH resin composition. The layer made of the present EVOH resin composition (hereinafter simply referred to as "the present EVOH resin composition layer") can be laminated with another substrate (hereinafter the resin used for the substrate may be referred to as "substrate resin") containing a thermoplastic resin other than the present EVOH resin composition as a main component, to impart additional strength, protect the present EVOH resin composition layer from the effects of moisture, etc., or impart other functions.
[0065] Examples of the base resin include polyethylene-based resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene-based resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin-based resins such as polybutene, polypentene, and polycyclic olefin-based resins (polymers having a cyclic olefin structure in at least one of the main chain and side chain); and polyolefins obtained by dissolving these polyolefins in an unsaturated carboxylic acid or Examples include polyolefin resins in the broad sense, including modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins graft-modified with an ester thereof, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.
[0066] Among these, hydrophobic resins such as polyamide-based resins, polyolefin-based resins, polyester-based resins, and polystyrene-based resins are preferred, and more preferred are polyolefin-based resins such as polyethylene-based resins, polypropylene-based resins, polycyclic olefin-based resins, and unsaturated carboxylic acid-modified polyolefin-based resins thereof. In particular, polycyclic olefin-based resins are preferably used as hydrophobic resins.
[0067] The layer structure of the present multilayer structure can be any combination such as a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, or b2 / b1 / a / b1 / a / b1 / b2, where a represents the present EVOH resin composition layer and b represents the base resin layer (b1, b2, ...). Furthermore, when R represents a recycled layer containing a mixture of the present EVOH resin composition and a thermoplastic resin other than the present EVOH resin composition, obtained by remelting and molding edges or defective products generated during the production of the multilayer structure, the layer structure can also be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, or b / R / a / R / a / R / b. The total number of layers in the present multilayer structure is usually 2 to 15, and preferably 3 to 10. In the above layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the respective layers, if necessary.
[0068] Known adhesive resins can be used, and may be selected appropriately depending on the type of thermoplastic resin used in the base resin layer "b." Representative examples include modified polyolefin polymers containing carboxy groups, which are obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin via addition reaction, graft reaction, or the like. Examples of modified polyolefin polymers containing carboxy groups include maleic anhydride-grafted polyethylene, maleic anhydride-grafted polypropylene, maleic anhydride-grafted ethylene-propylene (block and random) copolymers, maleic anhydride-grafted ethylene-ethyl acrylate copolymers, maleic anhydride-grafted ethylene-vinyl acetate copolymers, maleic anhydride-grafted polycyclic olefin resins, and maleic anhydride-grafted polyolefin resins. These may be used alone or in combination of two or more.
[0069] In the present multilayer structure, when adhesive resin layers are used between the present EVOH resin composition layer and the base resin layer, it is preferable to use an adhesive resin with excellent hydrophobicity, since the adhesive resin layers are located on both sides of the present EVOH resin composition layer.
[0070] The base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, waxes, etc., within a range that does not impair the spirit of the present invention (for example, 30% by mass or less, preferably 10% by mass or less, based on the total mass of the resin). These may be used alone or in combination of two or more kinds.
[0071] The lamination of the EVOH resin composition layer and the base resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. Examples include a method of melt-extrusion laminating the base resin onto a film, sheet, etc. of the EVOH resin composition, a method of melt-extrusion laminating the EVOH resin composition onto a base resin layer, a method of co-extruding the EVOH resin composition and the base resin, a method of dry-laminating the EVOH resin composition (layer) and the base resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, or a polyurethane compound, and a method of applying a solution of the EVOH resin composition onto a base resin and then removing the solvent. Among these, from the viewpoints of cost and the environment, it is preferable to produce the EVOH resin composition by including a step of melt-molding the EVOH resin composition layer, and specifically, a co-extrusion method is preferred.
[0072] The multilayer structure may be subjected to a (heat) stretching treatment, if necessary. The stretching treatment may be either uniaxial stretching or biaxial stretching, and in the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. Furthermore, the stretching method may be a roll stretching method, tenter stretching method, tubular stretching method, stretch-blow method, vacuum pressure forming, or the like, whichever provides a higher stretch ratio. The stretching temperature is a temperature near the melting point of the multilayer structure, and is usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. If the stretching temperature is too low, the stretchability will be poor, and if it is too high, it will be difficult to maintain a stable stretched state.
[0073] The stretched multilayer structure may be heat-set to provide dimensional stability. Heat-setting can be performed by known means, for example, by subjecting the stretched multilayer structure to heat treatment while maintaining tension, typically at 80 to 180°C, preferably 100 to 165°C, for typically 2 to 600 seconds.
[0074] When the stretched multilayer structure is to be used as a shrink film, the heat-shrinkability can be imparted to the multilayer structure by, for example, cooling and fixing the multilayer structure by applying cold air thereto, without carrying out the heat-setting process described above.
[0075] The thickness of the present multilayer structure (including the stretched one), and further the thickness of the present EVOH resin composition layer, base resin layer, and adhesive resin layer constituting the multilayer structure, cannot be generally determined depending on the layer configuration, type of base resin, type of adhesive resin, intended use, packaging form, required physical properties, etc., but the thickness of the present multilayer structure (including the stretched one) is usually 10 to 5,000 μm, preferably 30 to 3,000 μm, and particularly preferably 50 to 2,000 μm. The thickness of the present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm; the thickness of the base resin layer is usually 5 to 3,000 μm, preferably 10 to 2,000 μm, and particularly preferably 20 to 1,000 μm; and the thickness of the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.
[0076] Furthermore, the thickness ratio of the present EVOH resin composition layer to the base resin layer in the present multilayer structure (present EVOH resin composition layer / base resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60. Furthermore, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (present EVOH resin composition layer / adhesive resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10.
[0077] The multilayer structure can also be used to produce cup- or tray-shaped multilayer containers. In this case, a drawing method is typically used, specifically vacuum forming, pressure forming, vacuum-pressure forming, plug-assisted vacuum-pressure forming, etc. Furthermore, blow molding is used to produce tube- or bottle-shaped multilayer containers (laminate structure) from a multilayer parison (a hollow tubular preform before blowing). Specific examples include extrusion blow molding (double-head, mold-moving, parison-shift, rotary, accumulator, horizontal parison, etc.), cold parison blow molding, injection blow molding, and biaxial stretch blow molding (extrusion-type cold parison biaxial stretch blow molding, injection-type cold parison biaxial stretch blow molding, injection-molding in-line biaxial stretch blow molding, etc.). The resulting laminate may be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making, deep drawing, box processing, tube processing, splitting processing, etc. as required.
[0078] Single-layer films formed from the present EVOH resin composition, bags made from the present multilayer structure, and containers and lids made from cups, trays, tubes, bottles, etc. are useful as packaging materials for a variety of items, including general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.
[0079] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the examples, "parts" means parts by mass.
[0080] Prior to the examples, the following ingredients were prepared:
[0081] [EVOH] EVOH (A1): ethylene content 29 mol%, MFR 8 g / 10 min (210°C, load 2160 g), saponification degree 99.7 mol%
[0082] [Polysiloxane compounds] Silicone mixture (B1): "GENIOPAST Pellet-S" manufactured by Asahi Wacker Silicone Co., Ltd. (polydimethylsiloxane content in the masterbatch: approximately 70% by mass, fumed silica content: approximately 30% by mass, solid at 25 to 250 ° C., melting point: none) Silicone oil (B2): unmodified polydimethylsiloxane (straight silicone oil), "KF-96" manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity 500 mm 2 Silicone oil (B3): Unmodified polydimethylsiloxane (straight silicone oil), Shin-Etsu Chemical Co., Ltd. "KF-96H", kinematic viscosity 10,000 mm 2 / s
[0083] Example 1 An EVOH (A1) having an ethylene content of 29 mol% and GENIOPAST Pellet-S (B1) were dry-blended so that the amount of (B1) was 0.2 mass% relative to the total amount of (A1) and (B1) to obtain a mixture. The mixture was then fed to a twin-screw extruder (20 mmφ) equipped with a two-hole die and extruded under the following extrusion conditions. The extruded strand was cooled and solidified in a water bath. Next, air was blown onto the solidified strand to remove water droplets from the surface of the strand, and the strand was then cut to obtain pellets of an EVOH resin composition.
[0084] [Extrusion conditions] Extruder set temperatures (°C): C1 / C2 / C3 / C4 / C5 / C6 = 150 / 200 / 210 / 210 / 210 / 210 Screw rotation speed: 300 rpm
[0085] [Preparation of Melt-Extruded Monolayer Film] The obtained pellets of the EVOH resin composition were extruded under the following conditions to obtain a melt-extruded monolayer film: Extruder: Plastograph EC-plus manufactured by Brabender Screw: Single screw, 20 mm diameter, full flight Cylinder temperature setting: 190 to 210°C Chill roll temperature setting: 80°C Film thickness: 20 μm
[0086] Examples 2 to 4, Comparative Examples 1 to 8 Pellets of EVOH resin compositions were obtained in the same manner as in Example 1, except that the type, content, and kinematic viscosity of the polysiloxane compound were changed as shown in Table 1. Furthermore, melt-extruded monolayer films were obtained from the pellets of the EVOH resin compositions in the same manner as in Example 1.
[0087] The pellets of the EVOH resin compositions of Examples 1 to 4 and Comparative Examples 1 to 8 and the melt-extruded monolayer films obtained from the pellets were subjected to the following various evaluations. The results are shown in Table 2 below.
[0088] [Evaluation of Metal Adhesion] A sheet having a thickness of 1 to 2 mm was prepared from the EVOH resin composition pellets using a vacuum hot press. A resin piece having a size of 10 mm length x 10 mm width was cut from the obtained sheet, and the EVOH resin piece was sandwiched between two aluminum plates (pure aluminum A1050P, 10 cm length x 3 cm width) at a position 2 cm from the end of the long side and 1.5 cm from the end of the short side, and heated at 230°C under a pressure of 3.06 kg / cm. 2 The EVOH resin composition was heat-pressed under the conditions of 1 minute of heating (3 minutes of preheating, 1 minute of cooling), and the two plates were bonded together to obtain a peel test specimen. The aluminum plate was opened at the center of the prepared test specimen, and both aluminum plates were pulled in opposite directions at a tensile speed of 100 mm / min using an autograph (AGS-H, manufactured by Shimadzu Corporation), to determine the peel strength (adhesion strength) between the EVOH resin composition and the aluminum plate. Five tests were conducted, and the average of the stable values of the peel test force (N) was calculated. The evaluation results are shown as the percentage decrease in adhesive strength (%) when the blank (here, Comparative Example 7) is taken as 100%, and are also shown according to the following criteria. (Evaluation criteria) ◎ (Excellent): Excellent reduction effect on metal adhesion (80% to 95%) ○ (Very good): Excessive reduction effect on metal adhesion (less than 80%) △ (Good): Moderate reduction effect on metal adhesion (more than 95% to less than 100%) × (Poor): No reduction in metal adhesion (100%)
[0089] [Thickening evaluation] Using a Brabender Plastograph, EVOH resin composition pellets were kneaded at 230°C, 50 rpm, and 1 hour, and the evaluation results are shown as the thickening rate (%) when the torque of the blank (here, Comparative Example 7) after 1 hour of kneading is taken as 100%, and are also shown according to the following criteria: (Evaluation criteria) ⊚ (Excellent): Torque reduction confirmed ◯ (Very good): Equivalent to blank × (Poor): Significant thickening behavior observed compared to blank
[0090] [Film Formability] The appearance of the melt-extruded monolayer film after film formation was evaluated on a scale of A to E according to the following criteria, and the results are shown below. (Evaluation criteria) A: Good appearance with no unevenness in thickness B: Good appearance with slight unevenness in thickness C: Fine holes observed during film formation D: Holes of 1 cm or more observed during film formation E: Film formation was not possible at all
[0091] [Dispersed particle size] The obtained monolayer film was cut out using a microtome in a cross section parallel to the film formation flow to obtain a sample. This sample was observed at 2365x magnification using a laser microscope (OLS5000, manufactured by Olympus Corporation), and the "maximum diameter, minimum diameter, and particle circular area" of each polysiloxane particle observed in the cross section were measured and averaged. The dispersed particle size was measured using image analysis software Quick Grain.
[0092]
[0093]
[0094] As can be seen from Table 2, the EVOH resin compositions of Examples 1 to 4 containing the silicone blend (B) were able to reduce metal adhesion during film formation and suppress thickening behavior within an acceptable range compared to the EVOH resin composition of Comparative Example 7, which did not contain the silicone blend (B). This prevented excessive resin deterioration during film formation and improved long-run properties. The EVOH resin compositions of Comparative Examples 1 to 6 and 8, which contained silicone oil instead of the silicone blend (B), were inferior in film formability. In particular, Comparative Example 8 frequently exhibited vent-up, resulting in poor processability and making it difficult to produce the EVOH resin composition. Furthermore, since the EVOH resin compositions reduced metal adhesion between the EVOH resin and the processing machine surfaces (barrel, die) and exhibited excellent long-run properties and film formability, the multilayer structures comprising a layer made of the EVOH resin composition of the Examples also reduced metal adhesion between the EVOH resin and the processing machine surfaces (barrel, die) and exhibited excellent long-run properties and film formability.
[0095] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0096] This EVOH resin composition reduces metal adhesion between the EVOH resin and the surface of the processing machine to prevent excessive deterioration of the resin during film formation, and has excellent long-run properties and film-forming properties, making it useful as a packaging material for a variety of foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.
Claims
1. An ethylene-vinyl alcohol copolymer composition comprising an ethylene-vinyl alcohol copolymer (A) and a silicone blend (B), wherein the silicone blend (B) is a solid at 25°C.
2. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein the content of the silicone mixture (B) is 0.01 to 5 mass % based on the total mass of the ethylene-vinyl alcohol copolymer (A) and the silicone mixture (B).
3. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein the silicone mixture (B) contains silicone and fumed silica.
4. The ethylene-vinyl alcohol copolymer composition according to claim 3, wherein the mass ratio of said silicone to said fumed silica (silicone / fumed silica) is from 90 / 10 to 50 / 50.
5. The ethylene-vinyl alcohol copolymer composition of claim 3, wherein the dry silica is fumed silica.
6. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein the silicone compound (B) is a solid at 250°C.
7. A method for producing an ethylene-vinyl alcohol copolymer composition, comprising a step of melt-mixing a composition raw material containing an ethylene-vinyl alcohol copolymer (A) and a silicone blend (B), wherein the silicone blend (B) is a solid at 25°C.
8. A pellet comprising the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 6.
9. A film comprising the ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 6.
10. The film according to claim 9, wherein the maximum dispersed diameter of said silicone mixture (B) in the film is 0.1 to 3 μm.
11. A method for producing a film, comprising the step of melt-molding the pellets according to claim 8.
Citation Information
Patent Citations
Resin composition and its laminate
JP1999106592A
Water cup with scratch resistance and high barrier property and preparation method thereof
CN106432903A
Warm-keeping barrier film for fabric and preparation method thereof
CN108727682A
Kaishitsuechiren sakusanbinirukyojugotaikenkabutsuno seizohoho