Electrolyte composition and battery

The electrolyte composition, featuring a polymer and high-donor-number organic solvents, addresses the conductivity limitations in polymer electrolytes by reducing ion interactions, thereby enhancing alkali metal ion mobility and overall battery performance.

WO2024232341A1PCT designated stage expired Publication Date: 2024-11-14SUMITOMO CHEM CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016894
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-05-02
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Polymer electrolytes in batteries have limitations in ionic conductivity, which hinders the mobility and conductivity of alkali metal ions, particularly due to strong interactions between alkali metal ions and counter anions, leading to lower-than-expected performance.

Method used

An electrolyte composition is developed comprising a polymer capable of conducting alkali metal ions, combined with an organic solvent that has a high donor number, specifically exceeding 16.5, and a proportion of solvents with a donor number of 17 or more, which weakens the interaction between alkali metal ions and their counter anions, enhancing ionic conductivity.

Benefits of technology

The electrolyte composition significantly improves ionic conductivity by allowing greater mobility of alkali metal ions, outperforming conventional polymer electrolytes and enabling more efficient battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016894_14112024_PF_FP_ABST
    Figure JP2024016894_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides an electrolyte composition which contains one or more organic solvents and a polymer that has the ability to conduct alkali metal ions, wherein the total donor number of the organic solvents contained in the electrolyte composition is 16.5 or more. (In the formula, n is the total number of organic solvents contained in the electrolyte composition and is 1 or more, DNi is the donor number of the i-th organic solvent, and fi is the mass fraction of the i-th organic solvent.)
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte composition and battery

[0001] The present disclosure relates to electrolyte compositions and batteries.

[0002] Batteries such as lithium-ion batteries, which charge and discharge through the movement of metal ions between a positive electrode and a negative electrode, have been the subject of vigorous research due to their high capacity. Known electrolytes for lithium-ion batteries and the like include solutions of lithium salts containing organic solvents or ionic liquids. Meanwhile, research into solid electrolytes, polymer electrolytes, and the like is also underway from the perspectives of safety and processability (Patent Document 1). In addition to lithium-ion batteries, research is also underway into batteries that use other alkali ions, such as sodium and potassium, which are more abundant than lithium.

[0003] Japanese Patent Application Laid-Open No. 2001-176556

[0004] However, polymer electrolytes still have room for improvement in terms of ionic conductivity.

[0005] The present disclosure has been made in view of the above circumstances, and has an object to provide an electrolyte composition with high ionic conductivity and a battery using the same.

[0006] The present disclosure provides, for example, the following [1] to [8]: [1] An electrolyte composition comprising a polymer capable of conducting alkali metal ions and an organic solvent, wherein the donor number of the organic solvents contained in the electrolyte composition is 16.5 or more. (wherein n is the total number of organic solvents contained in the electrolyte composition and is 1 or more, DNi is the donor number of the i-th organic solvent, and fi is the mass fraction of the i-th organic solvent.) [2] An electrolyte composition comprising a polymer capable of conducting alkali metal ions and an organic solvent, wherein a proportion of the organic solvents contained in the electrolyte composition having a donor number of 17 or more is 10 mass % or more based on the total amount of the organic solvents. [3] The electrolyte composition of [1] or [2], wherein the organic solvent comprises one or more organic solvents selected from the group consisting of ether-based solvents, phosphate ester-based solvents, carbonate-based solvents, fluorine-based solvents, and nitrile-based solvents. [4] The electrolyte composition of any one of [1] to [3], further comprising an anion receptor. [5] The electrolyte composition of [4], wherein the anion receptor is a compound containing a Group 13 element having Lewis acidity. [6] The electrolyte composition according to any one of [1] to [5], wherein the polymer capable of conducting alkali metal ions contains one or more groups selected from the group consisting of an alkali metal ion-modified sulfonylimide group, an alkali metal ion-modified sulfonic acid group, an alkali metal ion-modified carboxylic acid group, and an alkali metal ion-modified phenol group. [7] The electrolyte composition according to any one of [1] to [6], further containing an alkali metal salt. [8] A battery comprising the electrolyte composition according to any one of [1] to [7].

[0007] According to the present invention, it is possible to provide an electrolyte composition with high ionic conductivity and a battery using the same.

[0008] The electrolyte composition of this embodiment contains a polymer capable of conducting alkali metal ions and an organic solvent. The electrolyte composition satisfies at least one of the following conditions (1) to (3), and may also satisfy at least one of conditions (1) and (2): (1) The total donor number of the organic solvents contained in the electrolyte composition is 16.5 or greater. (2) The proportion of organic solvents having a donor number of 17 or greater in the organic solvents contained in the electrolyte composition is 10% by mass or greater relative to the total amount of the organic solvents. (3) The content of organic solvents having a donor number of 17 or greater relative to the total amount of the electrolyte composition is 5% by mass or greater.

[0009] The donor number in this specification means the Gutmann donor number (DN). Specifically, the donor number is the ratio of the Lewis base (organic solvent) to the Lewis acid SbCl 5 The donor number may be defined as (heat of reaction - ΔH (kcal / mol)) between the two. Details about such donor numbers are described, for example, in Hansen Solubility Parameters 50th anniversary conference, preprint 2017 PP. 22-36 (2017), V. Gutmann, "The Donor-Acceptor Approach to Molecular Interactions", Plenum, New York, 1978, etc. In this case, the reaction heat may be measured using a very diluted reactant in 1,2-dichloroethane solution.

[0010] Here, the "total donor number of the organic solvents contained in the electrolyte composition" is represented by the following formula (I). In the formula below, DN on the left side refers to the "total donor number of the organic solvents contained in the electrolyte composition". n is the total number of organic solvents contained in the electrolyte composition and is 1 or more. DNi is the donor number of the i-th organic solvent, and fi is the mass fraction of the i-th organic solvent. i = 1, 2, 3, ... n, and the sum of fi from i = 1 to n is 1. n may be 2 or more.

[0011] In other words, the organic solvent does not have to be a single composition, but may be a mixed solvent containing multiple organic solvents, in which case the weighted average of the donor numbers of each solvent is the overall donor number. That is, the term "overall donor number of organic solvents contained in an electrolyte composition" refers to the donor number of the organic solvent when the electrolyte composition contains only one type of organic solvent, and refers to the weighted average of the donor numbers of all organic solvents contained in the electrolyte composition when the electrolyte composition contains multiple types of organic solvents.

[0012] The electrolyte composition of this embodiment contains an organic solvent that satisfies at least one of the above conditions (1) to (3). In this case, the organic solvent with a high donor number interacts with the alkali metal ion, for example, by forming a coordinate bond, thereby relatively weakening the interaction between the alkali metal ion and its counteranion (e.g., an anionic functional group possessed by the polymer). This can increase the conductivity of the alkali metal ion in the electrolyte composition when a voltage is applied. Organic solvents with a low donor number have a weak interaction with cations, while alkali metal ions (cations) in the electrolyte composition have a relatively strong interaction with counteranions (e.g., anionic functional groups possessed by the polymer). If the counteranion is fixed to the polymer chain or is bulky, the mobility of the alkali metal ion as a whole tends to decrease, and conventional polymer electrolytes do not exhibit the expected ionic conductivity. On the other hand, the electrolyte composition of the present disclosure contains an organic solvent that satisfies the above conditions, and therefore has superior ionic conductivity compared to organic solvent blends that do not satisfy the above conditions.

[0013] The organic solvent contained in the electrolyte composition may be an aprotic solvent. The organic solvent may contain only an organic solvent having a donor number of 16.5 or more, or may contain both an organic solvent having a donor number of 16.5 or more and an organic solvent having a donor number less than 16.5. The organic solvent may contain only an organic solvent having a donor number of 17 or more, or may contain both an organic solvent having a donor number of 17 or more and an organic solvent having a donor number less than 17.

[0014] The organic solvent may not be liquid at room temperature, but may become liquid (i.e., a solvent) upon use, and may have a melting point of, for example, 60°C or less.

[0015] The organic solvent may contain one or more organic solvents selected from the group consisting of ether-based solvents, phosphate ester-based solvents, carbonate-based solvents, fluorine-based solvents, and nitrile-based solvents, or may contain one or more organic solvents selected from the group consisting of ether-based solvents, phosphate ester-based solvents, carbonate-based solvents, fluorine-based solvents, and may contain a phosphate ester.

[0016] Examples of organic solvents having a donor number of 17 or greater include solvents having an amino group (amine solvents), solvents having an amide bond (amide solvents), alcohols, solvents having an ether bond (—O—) (ether solvents), solvents having a sulfide bond (—S—) (sulfide solvents), phosphoric acid esters, phosphoric acid amides, ester solvents, nitrogen-containing aromatic compounds (compounds containing nitrogen as a ring member of the aromatic ring, which may be either monocyclic or fused ring systems), urea compounds, solvents having a sulfoxide group (sulfoxide solvents), ketones, solvents having a carbonate group (carbonate solvents), and solvents having a nitrile group (nitrile solvents). One or more types of organic solvents having a donor number of 17 or greater can be used.

[0017] Examples of the amine solvent having a donor number of 17 or greater include triethylamine, 2-methyl-2-propaneamine, ethylamine, piperidine, aniline, and N-methylaniline. The amino solvent may have at least one of a primary amino group, a secondary amino group, and a tertiary amino group. The amino solvent may also have a ring, such as a piperidine ring.

[0018] Examples of the amide solvents having a donor number of 17 or greater include cyclic amide solvents having a ring structure containing an amide bond, such as a lactam ring, and acyclic amide solvents having no ring structure containing an amide bond. Examples of the acyclic amide solvents include N,N-diethylacetamide, N,N-dimethylacetamide, N,N-diethylformamide, N,N-dimethylformamide, N-methylformamide, and formamide. Examples of the cyclic amide solvents include 1,3-dimethyltetrahydropyrimidin-2(1H)-one, N-methylpyrrolidone, and 1,3-dimethyl-2-imidazolidinone.

[0019] Examples of the alcohols having a donor number of 17 or more include 2-methyl-2-butanol, 3-methyl-1-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 2-propanol, octanol, decanol, benzyl alcohol, 2-phenylethanol, 1-propanol, ethanol, and methanol.

[0020] Examples of the ether solvents having a donor number of 17 or greater include cyclic ether solvents having a ring structure containing an ether bond within the ring, and chain ether solvents having no ring structure containing an ether bond within the ring. Examples of the cyclic ether solvents include tetrahydrofuran, 2-methyltetrahydrofuran, 1,3,3-trimethyl-2-oxabicyclo[2.2.2]octane, tetrahydropyran, and 1,3-dioxolane. Examples of the chain ether solvents include 1,2-diethoxyethane, ethoxymethoxyethane, diethyl ether, 1,2-dimethoxyethane, dibenzyl ether, dibutyl ether, and diisopropyl ether.

[0021] Examples of the phosphate ester having a donor number of 17 or more include compounds represented by the following chemical formula (P). (In the formula, R 11 ~R 13 are each independently an organic group having 1 to 8 carbon atoms.

[0022] R in the above formula (P) 11 ~13 Examples of R include hydrocarbon groups and monovalent groups having an -O- (ether bond) in the hydrocarbon group chain. The hydrocarbon group may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be any of linear, branched, and cyclic, and may be linear or branched. The aliphatic hydrocarbon group may contain an unsaturated bond, but may be a saturated aliphatic hydrocarbon group. R in the above formula (P) 11 ~ 13 The number of carbon atoms in each of R in the above formula (P) may be 1 to 6, 1 to 4, 1 to 3, or 1 or 2. 11 ~ 13 may all be the same or different.

[0023] Examples of the phosphate ester include trimethyl phosphate (TMP), triethyl phosphate (TEP), tris(2,2,2-trifluoroethyl) phosphate (TFEP), and tributyl phosphate.

[0024] Examples of the phosphoric acid amide (phosphoramide) having a donor number of 17 or more include tripyrrolidinophosphine oxide, hexamethylphosphoramide, and hexaethylphosphoramide.

[0025] Examples of the ester solvents having a donor number of 17 or more include tert-butyl acetate, isopropyl acetate, and ethyl chloroformate.

[0026] Examples of the nitrogen-containing aromatic compounds having a donor number of 17 or more include pyridine, 3-methylpyridine, 4-methylpyridine, and quinoline.

[0027] Examples of the urea compounds having a donor number of 17 or more include N,N,N',N'-tetramethylurea.

[0028] Examples of the sulfoxide solvents having a donor number of 17 or more include dibutyl sulfoxide and dimethyl sulfoxide.

[0029] Examples of the ketones having a donor number of 17 or more include cyclohexanone and cyclopentanone.

[0030] Examples of the carbonate solvents having a donor number of less than 17 include chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; and cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate.

[0031] Examples of the fluorine-based solvent include hydrofluorocarbons such as perfluorooctane, hydrofluoroethers such as methyl nonafluorobutyl ether and ethyl nonafluorobutyl ether, and hydrofluoroolefins such as 1,3,3,3-tetrafluoropropene. The donor number of the fluorine-based solvent may be less than 17.

[0032] Examples of the nitrile solvent include acetonitrile, succinonitrile, etc. The donor number of the nitrile solvent may be less than 17.

[0033] The donor number of the entire organic solvents contained in the electrolyte composition may be 17.0 or more, 17.5 or more, 17.8 or more, 18.0 or more, 18.5 or more, or 19.0 or more. The donor number of the entire organic solvents contained in the electrolyte composition may be 40.0 or less, 35.0 or less, 30.0 or less, 25.0 or less, 23.0 or less, 22.0 or less, or 21.0 or less.

[0034] The proportion of the organic solvent having a donor number of 17 or greater in the organic solvent contained in the electrolyte composition may be 10% by mass or greater, 25% by mass or greater, 30% by mass or greater, 35% by mass or greater, or 40% by mass or greater, relative to the total amount of organic solvent. The proportion of the organic solvent having a donor number of 17 or greater in the organic solvent contained in the electrolyte composition may be 90% by mass or less, 80% by mass or less, 70% by mass or less, 65% by mass or less, or 60% by mass or less, relative to the total amount of organic solvent. The proportion of the organic solvent having a donor number of 17 or greater in the organic solvent contained in the electrolyte composition may be 10 to 90% by mass, 25 to 80% by mass, 25 to 70% by mass, 25 to 60% by mass, 30 to 60% by mass, 35 to 65% by mass, 35 to 60% by mass, or 40 to 60% by mass, relative to the total amount of organic solvent.

[0035] The electrolyte composition of this embodiment may contain 5% by mass or more, 10% by mass or more, or 15% by mass or more of an organic solvent having a donor number of 17 or more, relative to the total amount of the electrolyte composition. The electrolyte composition of this embodiment may contain 60% by mass or less, 50% by mass or more, or 40% by mass or less of an organic solvent having a donor number of 17 or more, relative to the total amount of the electrolyte composition. The electrolyte composition of this embodiment may contain 5 to 60% by mass, or 10 to 40% by mass, of an organic solvent having a donor number of 17 or more, relative to the total amount of the electrolyte composition.

[0036] The content of the organic solvent in the electrolyte composition may be 100 to 600 parts by mass, 100 to 500 parts by mass, 150 to 450 parts by mass, 200 to 400 parts by mass, or 250 to 350 parts by mass relative to 100 parts by mass of the polymer capable of conducting alkali metal ions.

[0037] The content of the organic solvent in the electrolyte composition may be 30 to 90 mass %, 35 to 85 mass %, 40 to 80 mass %, 45 to 75 mass %, 50 to 70 mass %, or 60 to 70 mass %, relative to the total amount of the electrolyte composition.

[0038] The electrolyte composition includes a polymer (hereinafter simply referred to as polymer) capable of conducting alkali metal ions. The polymer can have a superior alkali metal ion transport number when measured at room temperature (25°C) for a composition containing 33 mass% of the polymer and 67 mass% of a non-ionic plasticizer, or a composition containing 31.9 mass% of the polymer, an alkali metal salt, and the remainder being a non-ionic plasticizer.

[0039] The polymer may have an alkali metal ion transport number of 0.4 or more, 0.5 or more, 0.6 or more, or 0.7 or more. When the polymer has an anionic functional group, the alkali metal ion contained in the composition may be a counter cation of the anionic functional group, or may be added as an alkali metal salt. The polymer capable of conducting alkali metal ions may be a polymer capable of preferentially conducting alkali metal ions.

[0040] The nonionic plasticizer used in measuring the transference number of the alkali metal ions mentioned above includes at least one of an organic solvent and other resins such as fluorine-based resins.

[0041] The organic solvent used in measuring the transference number of the alkali metal ion may be an aprotic solvent. The aprotic solvent used in measuring the transference number of the alkali metal ion may be at least one selected from the group consisting of carbonate solvents, fluorine-based solvents, and ether-based solvents. A specific example of the organic solvent used in measuring the transference number of the alkali metal ion may be the organic solvent contained in the electrolyte composition.

[0042] The fluororesin used in measuring the alkali metal ion transference number is preferably a resin having a carbon chain as the main chain, and the carbon chain may be formed by radical polymerization of an ethylenically unsaturated group.

[0043] The polymer may have an anionic functional group and an alkali metal ion as a counter cation of the anionic functional group (referred to as an alkali metalated group). The alkali metalated group may include one or more groups selected from the group consisting of an alkali metalated sulfonylimide group, an alkali metalated sulfonic acid group, an alkali metalated carboxylic acid group, and an alkali metalated phenol group, or may include at least one of an alkali metalated carboxylic acid group and an alkali metalated phenol group, or may include an alkali metalated carboxylic acid group.

[0044] Here, in this specification, an alkali metal ionized group refers to a group in which an anionic functional group, which is a conjugate base of the acid form of the group, forms a salt with an alkali metal ion. Specifically, an alkali metal ionized sulfonylimide group is a sulfonylimide acid group (-SO 2 -NH-SO 2 - group) in which H is substituted with an alkali metal element A 2 -NA-SO 2 - group ([-SO 2 -N-SO 2 -] - A + The alkali metal sulfonic acid group refers to a sulfonic acid group (—SO 3 H group) in which H is replaced by an alkali metal element A. 3 A group ([-SO 3 ] - A + The alkali metal carboxylic acid group refers to a —COOA group ([—COO] group) in which H of a carboxylic acid group (—COOH group) is substituted with an alkali metal element A. - A + The alkali metal phenol group refers to an —OA group (—O group) in which the H of the —OH group, which is a phenolic hydroxyl group, is substituted with an alkali metal element A. - A + This refers to the group.

[0045] The structure of the polymer may include one having a carbon chain as the main chain, and the carbon chain may be formed by radical addition polymerization of a monomer having an ethylenically unsaturated group.

[0046] The alkali metal element A in the alkali metal ionized group may include at least one selected from the group consisting of lithium, sodium, potassium, rubidium, and cesium, may include at least one selected from the group consisting of lithium, sodium, and potassium, may include at least one of lithium and sodium, or may include lithium.

[0047] The content of one alkali metal element among the alkali metal elements contained in the polymer may be 80 mol % or more, 85 mol %, or 90 mol %. The one alkali metal element may be potassium, sodium, or lithium, or may be sodium or lithium, or may be lithium.

[0048] The polymer may have a structural unit (also referred to as structural unit (A)) having the anionic functional group and an alkali metal ion as a counter cation of the anionic functional group. The polymer may have one or more types of structural unit (A).

[0049] Examples of the structural unit (A) include a structural unit (A1) represented by the following formula (A1). (In formula (A1), R 1 is a -COOA group or a monovalent organic group having a -COOA group, and R 2 ~R 4 are each independently a hydrogen atom or a monovalent substituent, or R 2 and R 3 is a hydrogen atom or a monovalent substituent, and the other is R 4 and form a ring together. * indicates the bonding site of the structural unit (A1) to another structural unit.

[0050] R in the above formula (A1) 1may be a -COOA group itself, or may be a monovalent organic group having a -COOA group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. The monovalent organic group may have one or more -COOA groups, or may have one -COOA group. Examples of the organic group include monovalent groups having a -COOA group as a substituent, such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group of -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The -COOA group is represented by R 1 is bonded to a carbon atom of another moiety in the above. The monovalent group may have a substituent that replaces a hydrogen atom bonded to the carbon atom. Examples of the substituent include an electron-withdrawing group such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be any of a linear hydrocarbon group, a branched hydrocarbon group, and a cyclic hydrocarbon group. The hydrocarbon group may be any of a saturated hydrocarbon group and an unsaturated hydrocarbon group. In this specification, an aromatic hydrocarbon group refers to a hydrocarbon group having an aromatic moiety such as a benzene ring, and may have an aliphatic moiety. In this specification, a cyclic hydrocarbon group refers to a hydrocarbon group having an aliphatic carbon ring moiety, and may have a linear or branched aliphatic moiety.

[0051] R in the above formula (A1) 1 is -R 9 -COOA, where R 9is a divalent organic group. The divalent organic group may have 1 to 19 carbon atoms, 1 to 14 carbon atoms, 1 to 9 carbon atoms, 1 to 4 carbon atoms, or 1 or 2 carbon atoms. Examples of the divalent organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The divalent group may also have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include an electron-withdrawing group such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group.

[0052] R in the above formula (A1) 1 Examples of the electron-withdrawing group that may be contained include a halogen atom, a sulfonic acid group or a salt thereof, a sulfonic acid ester, a nitro group, a nitrile group, a carboxyl group or a salt thereof, etc. The halogen atom may be at least one of Cl and F, and may be F.

[0053] R in the above formula (A1) 4 When R is a monovalent substituent, examples of the substituent include a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the monovalent organic group include a group having a -COOA group as a substituent, such as a hydrocarbon group, a group having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group of -O-, -S-, -C(=O)-, or -C(=O)O-, and a group having a heterocycle. R in the above formula (A1) 4 may be a hydrogen atom or a methyl group.

[0054] R in the above formula (A1)2 or R 3 When R is a monovalent substituent, the substituent may be a monovalent organic group. 4 Examples of R in the above formula (A1) include: 2 and R 3 may be a hydrogen atom, and R 2 and R 3 may both be hydrogen atoms.

[0055] R in the above formula (A1) 2 and R 3 One of them is R 4 When the ring is formed together with the carbon atom, the number of ring members may be 4 to 10, 5 to 8, or 5 or 6. A substituent may be bonded to the carbon atom that is a ring member.

[0056] The structural unit (A) also includes a structural unit (A2) represented by the following formula (A2). (In formula (A2), X is a divalent organic group having 1 to 20 carbon atoms, Y is a halogen atom or a monovalent organic group having 1 to 20 carbon atoms, and A + is an alkali metal ion, and * represents the position where the structural unit (A2) is bonded to another structural unit.

[0057] X in the formula (A2) is not particularly limited and may be a hydrocarbon group or a group having a heteroatom, or may have a heterocycle. More specific examples of X include divalent groups such as hydrocarbon groups and groups having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. When there are multiple linking groups, the linking groups are not adjacent to each other. The divalent group may have a substituent substituting a hydrogen atom bonded to a carbon atom. The substituent may be a monovalent substituent, such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. X in the above formula (A2) may be bonded to one or both of the nitrogen atom of the maleimide group and the sulfur atom of the sulfonyl group via a carbon atom contained in X.

[0058] The number of carbon atoms possessed by X in the above formula (A2) may be 1 to 15, 2 to 10, or 3 to 8. X may be a group having an aromatic ring or a group having an aromatic carbon ring such as a benzene ring. A substituent such as an alkyl group, a halogen atom, or an electron-withdrawing group may be bonded to a carbon atom that is a member of the carbon ring. The hydrocarbon group represented by X is preferably a phenylene group, an alkylene group having 1 to 8 carbon atoms, a polyoxyalkylene group, or a group in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms such as fluorine atoms, and more preferably a phenylene group or a substituted phenylene group substituted with an alkyl group, a halogen atom, an electron-withdrawing group, or the like. Examples of the electron-withdrawing group include a halogen atom, a sulfonic acid group or a salt thereof, a sulfonic acid ester, a nitro group, and a nitrile group.

[0059] In the above formula (A2), when Y is a monovalent organic group, the organic group is not particularly limited and may be a hydrocarbon group or a group having a heteroatom, or may have a heterocycle. More specific examples of Y include monovalent groups such as hydrocarbon groups and groups having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. When there are multiple linking groups, the linking groups are not adjacent to each other. The monovalent group may also have a substituent substituting a hydrogen atom bonded to a carbon atom. The substituent may be a monovalent substituent, such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group.

[0060] The number of carbon atoms owned by Y in formula (A2) may be 1 to 15, 1 to 10, 1 to 8, 1 to 5, or 1 to 3. The hydrocarbon group represented by Y is preferably a phenyl group, an alkyl group having 1 to 5 carbon atoms, or one of these groups in which some or all of the hydrogen atoms bonded to the carbon atoms have been substituted with halogen atoms such as fluorine atoms, more preferably a fluorinated alkyl group having 1 to 5 carbon atoms, and even more preferably a fluorinated alkyl group having 1 to 3 carbon atoms such as a trifluoromethyl group. The fluorinated alkyl group may be a perfluorinated alkyl group.

[0061] When Y in formula (A2) is a halogen atom, the halogen atom is preferably a fluorine atom or a chlorine atom, and more preferably a fluorine atom.

[0062] The structural unit (A) may also be a structural unit (A3) represented by the following formula (A3).

[0063] (In formula (A3), Y 2R is a group having a phenolic hydroxyl group modified with an alkali metal or a group having a sulfonic acid group modified with an alkali metal, and * indicates the bonding position of the structural unit (A3) to other structural units. 15 ~R 17 are each independently a hydrogen atom or a monovalent substituent, or R 16 is a hydrogen atom or a monovalent substituent, and R 15 and R 17 together form a divalent substituent.)

[0064] R in the above formula (A3) 15 ~R 17 One or more of may be hydrogen atoms, or all may be hydrogen atoms.

[0065] R in the above formula (A3) 15 ~R 17 is a monovalent substituent, the monovalent substituent may be a monovalent organic group. The number of carbon atoms in the organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the organic group include monovalent substituents such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The monovalent substituent may also have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Examples of the hydrocarbon group include a methyl group, an ethyl group, a propyl group, and a phenyl group.

[0066] R in the above formula (A3) 15 ~R 17In the above formula, the monovalent substituent may have an electron-withdrawing group or may be the electron-withdrawing group itself. The electron-withdrawing group may be bonded to the monovalent organic group, or the monovalent organic group may be the electron-withdrawing group. Examples of the electron-withdrawing group include a halogen atom, a sulfonic acid group or a salt thereof, a sulfonic acid ester, a nitro group, and a nitrile group. The halogen atom may be a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom.

[0067] R in the above formula (A3) 15 and R 17 When these together form a divalent organic group, the number of carbon atoms in the divalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the organic group include hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and divalent substituents such as groups having a heterocycle. The divalent organic group may also have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Examples of the hydrocarbon group include a propylene group and a butylene group.

[0068] Y in the above formula (A3) 2 is a group having a phenolic hydroxyl group, 2 may be a group represented by any one of the following formulae (A21) to (A26). (In formula (A21), R A At least one of the groups is an -OA group, and the rest are hydrogen atoms or monovalent substituents. BAt least one of the groups is an —OA group, and the rest are hydrogen atoms or monovalent substituents. C At least one of the groups is an -OA group, and the rest are hydrogen atoms or monovalent substituents. D At least one of the groups is an -OA group, and the rest are hydrogen atoms or monovalent substituents. E At least one of the groups is an -OA group, and the rest are hydrogen atoms or monovalent substituents. F At least one of the groups is an -OA group, and the rest are hydrogen atoms or monovalent substituents.

[0069] The groups represented by the above formulae (A21) to (A26) may have 1 to 3 -OA groups, may have 1 or 2 -OA groups, or may have 1 -OA group.

[0070] In the above formulae (A21) to (A26), the monovalent substituent is preferably an electron-withdrawing group. Examples of the electron-withdrawing group include a halogen atom, a sulfonic acid group or a salt thereof, a sulfonic acid ester, a nitro group, and a nitrile group. The halogen atom may be any of F, Cl, Br, and I.

[0071] Furthermore, in formulas (A21) to (A26), the monovalent substituent may be an organic group having 1 to 20 carbon atoms. The number of carbon atoms in the organic group may be 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. Furthermore, the monovalent group may have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. Furthermore, the hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Examples of the hydrocarbon group include a methyl group, an ethyl group, a propyl group, a phenyl group, etc. The monovalent organic group itself may be an electron-withdrawing group.

[0072] Y in the above formula (A3) 2 is a group having a conjugated anion of sulfonic acid, 2 Examples of the group include a group represented by the following formula (A4). (In formula (A4), R 19 is a covalent bond or a divalent organic group. A is an alkali metal element.

[0073] In the above formula (A4), the number of carbon atoms in the divalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the organic group include hydrocarbon groups, and divalent substituents such as groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The divalent organic group may also have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Examples of the hydrocarbon group include a methylene group and a phenylene group.

[0074] The group having a conjugated anion of the above-mentioned sulfonic acid is —SO 3 A, -CH 2 -SO 3 A, -C 6 H 4 -SO 3 Examples include A.

[0075] The polymer may contain a structural unit (B) represented by the following formula (B): The structural unit (B) is a structural unit other than the structural unit (A), and does not need to contain an alkali metal group. (In formula (B), R 5 is a hydrogen atom or a monovalent substituent, and R 6 ~R 8 are each independently a hydrogen atom or a monovalent substituent, or R 6 and R 7 is a hydrogen atom or a monovalent substituent, and the other is R 8 and form a ring. * indicates the bonding site of the structural unit (B) to another structural unit.

[0076] R in the above formula (B)5 is a monovalent substituent, it may be a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 2 to 15, or 4 to 10. The monovalent organic group may have one or more -COOA groups, or may have one -COOA group. Examples of the organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle, and may be a group having an aromatic ring. The aromatic ring may have at least one of a carbocyclic ring and a heterocyclic ring, and may be a carbocyclic ring. R in the above formula (B) 5 is a carbon atom of the ethylene group in formula (B) (R 5 may be bonded to the carbon atom to which R is directly bonded, 5 A carbon atom that is a ring member of the aromatic ring of formula (B) may be bonded to a carbon atom of the ethylene group in formula (B). The group having an aromatic ring may be either a monocyclic or condensed ring system, or may be a group having a benzene ring. The group having an aromatic ring may have a monovalent substituent, and the monovalent substituent may be bonded to a carbon atom that is a ring member of the aromatic ring.

[0077] The monovalent substituent bonded to the aromatic ring may be a monovalent organic group, an electron-withdrawing group such as a halogen atom (excluding monovalent organic groups), an amino group (-NH 2 The monovalent substituent bonded to the aromatic ring includes a substituted or unsubstituted hydrocarbon group, a group represented by the formula: -R 41 -(O-R 42 ) n -OR 43 Examples include groups represented by the formula: -R 41 -(O-R 42 ) n -OR 43 The group represented by the formula (I) may be bonded to the para position of the benzene ring. 1may be a divalent group such as -O-, -S-, -C(=O)- or -C(=O)O-, or may be -O-. 2 may be a divalent group such as —O—, —S—, —C(═O)— or —C(═O)O—, or may be —O—.

[0078] The monovalent substituent bonded to the aromatic ring is represented by the formula: -R 41 -(O-R 42 ) n -OR 43 In the case where R in the group is a group represented by 41 is a covalent bond or a divalent organic group. The divalent organic group may be a divalent hydrocarbon group. The divalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the divalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the divalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The divalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, and may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a 1,2-propylene group, a 1,3-propylene group, or a group in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine atoms, and may be a methylene group.

[0079] The monovalent substituent bonded to the aromatic ring is represented by the formula: -R 41 -(O-R 42 ) n -OR 43 In the case where R in the group is a group represented by 42is a divalent organic group and may be a divalent hydrocarbon group. The divalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the divalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the divalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The divalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, and may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a 1,2-propylene group, a 1,3-propylene group, or a group in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine atoms, and may be an ethylene group. Formula: -R 41 -(O-R 42 ) n -OR 43 In the group represented by the formula (I), n may be 1 to 10, 1 to 5, or 1 to 3. The above n may be an integer or a rational number (for example, n may be an average value over all structural units (B) when the polymer has a plurality of structural units (B)). 42 When there are multiple, they may be different or the same.

[0080] The monovalent substituent bonded to the aromatic ring is represented by the formula: -R 41 -(O-R 42 ) n -OR 43 In the case where R in the group is a group represented by 43may be a hydrogen atom or a divalent hydrocarbon group. The monovalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the monovalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the monovalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The monovalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, and may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methyl group, an ethyl group, an isopropyl group, an n-propyl group, or a group in which some or all of the hydrogen atoms in these groups have been substituted with halogen atoms such as fluorine atoms, and may be a methyl group.

[0081] The structural unit (B) may contain at least one structural unit derived from a monomer represented by the following formula (B1). (wherein m is 0 to 4 and n is 0 to 10. R 20 may be a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. The alkyl group may be a methyl group or an ethyl group, or may be a methyl group.

[0082] In the above formula (B1), m may be 1 to 3, may be 1 or 2, or may be 1. The above m may be an integer, or may be an average value across all structural units derived from the monomer represented by formula (B1) contained in the polymer (in this case, m is a rational number). In the above formula (B1), n ​​may be 1 to 4, or may be 1 to 3. The above n may be an integer, or may be an average value across all structural units derived from the monomer represented by formula (B1) contained in the polymer (in this case, n is a rational number).

[0083] The number average molecular weight (Mn) of the polymer may be 5,000 to 400,000, 8,000 to 200,000, 10,000 to 150,000, or 10,000 to 100,000. The weight average molecular weight (Mw) of the polymer may be 5,000 to 600,000, 10,000 to 400,000, 20,000 to 200,000, or 20,000 to 100,000. The molecular weight distribution (Mw / Mn) of the polymer may be 1.0 to 5.0, 1.2 to 3.0, or 1.3 to 2.5.

[0084] When the polymer contains the structural unit (A1) and the structural unit (B), the number average molecular weight (Mn) of the polymer may be 5,000 to 200,000, 8,000 to 120,000, 10,000 to 100,000, or 10,000 to 50,000.

[0085] The number average molecular weight and weight average molecular weight of the polymer in this specification can be measured by gel permeation chromatography. The gel permeation chromatography (GPC) is performed under the conditions shown below. In preparing the calibration curve, a standard sample of polymethyl methacrylate (manufactured by Polymer Laboratories, Mn 800 to 2,200,000) is used as the standard substance. <GPC measurement conditions> Apparatus: GPC-104 (Shodex) DU-H2000 precision pump 74S-RI refractive-index detector 41-UV UV / vis detector Column: Shodex LF-404 Temperature: 40°C Solvent: tetrahydrofuran (THF) Flow rate: 0.3 mL / min Back pressure: 3.0 MPa Detection: RI Sample concentration: 0.5% by mass THF solution Injection volume: 10 μL

[0086] The electrolyte composition may contain an anion receptor. The anion receptor is a chemical species that captures anions by forming electrostatic interactions, hydrogen bonds, acid-base complexes, or the like with the anions. The anion receptor captures counter anions of alkali metal ions and promotes dissociation of the counter anions from the alkali metal ions. This increases the mobility of the metal ions. This also tends to improve the conductivity and transport number of the alkali metal ions in the electrolyte composition.

[0087] Low molecular weight chemical species (compounds, etc.) that function as the anion receptor are known, and examples of such compounds include those described in U.S. Patent Nos. 6,022,643, 5,705,689, and 6,120,941. The anion receptor may have a formula weight (molecular weight) of, for example, 1,000 or less, 800 or less, or 500 or less.

[0088] The anion receptor may have Lewis acidity. In this case, the anion receptor can capture the anion by accepting the unshared electron pair of the anion and forming an acid-base complex. Examples of such compounds include compounds having an electron-deficient atom. Note that an electron-deficient atom refers to an atom that is covalently bonded to another atom but has fewer than eight electrons in its outermost shell. Examples of the electron-deficient atom include atoms belonging to Group 13 of the periodic table, and more specifically, may be at least one of an aluminum atom and a boron atom, or may be a boron atom. The anion receptor may also be a compound containing a Group 13 element having Lewis acidity.

[0089] Examples of anion receptors having a boron atom include boron compounds that function as Lewis acids, such as diborane and compounds represented by the following chemical formulas IA to IE.

[0090]

[0091] In Formula IA, R 31is a halogen atom or a monovalent organic group. The halogen atom may be a fluorine atom or a chlorine atom, or may be a fluorine atom. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula IA via a carbon atom in the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. 31 may be different from each other or may all be the same.

[0092] In formula IB, R 32is a hydrogen atom or a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. Here, the monovalent organic group is bonded to the oxygen atom (O) in Formula IB via a carbon atom in the monovalent organic group. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule, there are multiple R 32 may be different from each other or may all be the same.

[0093] In formula IC, R 35 is a divalent organic group, Z 2 is a covalent bond or an oxygen atom. The number of carbon atoms in the divalent organic group may be 1 to 15, 2 to 10, or 3 to 8. In formula IC, R 35 , two Zs 2 and the boron atom (B) form a ring, and the ring may have 4 to 8 ring members, or may have 5 or 6 ring members. The divalent organic group is not particularly limited and may be a hydrocarbon group, a divalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, etc. 2 is an oxygen atom, the divalent organic group is connected to Z in formula IC by the carbon atom contained in the divalent organic group. 2 and the above Z 2is a covalent bond, the divalent organic group is bonded to the boron atom (B) in formula IC via a carbon atom contained in the divalent organic group. The hydrogen atom bonded to the hydrocarbon portion of the divalent organic group may be substituted with a substituent. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The divalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule represented by formula IC, multiple Z 2 may be different from each other or may all be the same.

[0094] In formula IC, R 36 is a hydrogen atom or a monovalent organic group. The monovalent organic group may be a group that bonds to the boron atom (B) in formula IC via a carbon atom that the monovalent organic group has, but -OR 37 The above-mentioned —OR 37 R in the group represented by 37 is a hydrogen atom or a monovalent organic group. 37 The monovalent organic group represented by the formula (I) is -OR 37 The oxygen atom of the above R 36 When R is a monovalent organic group, the number of carbon atoms in the organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. 37The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula IA via a carbon atom possessed by the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group.

[0095] In Formula ID, R 33 is a hydrogen atom, a halogen atom, or a monovalent organic group. The halogen atom may be a fluorine atom or a chlorine atom, or may be a fluorine atom. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula ID via a carbon atom in the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. 33 may be different from each other or may all be the same.

[0096] In formula IE, R 34 is a hydrogen atom or a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the oxygen atom (O) in Formula IE via a carbon atom possessed by the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule represented by formula IE, multiple R 34 may be different from each other or may all be the same.

[0097] Specific examples of boron compounds include diborane, boron trifluoride, boric acid, boroxine, trimethylborane, triethylborane, tri-n-propylborane, triisopropylborane, triphenylborane, trimethylborate, triethylborate, triphenylborate, tri-n-propylborate, triisopropylborate, 2-methoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane, and 2-ethoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane. Examples thereof include organic boron compounds such as oran, 2,4,6-trimethylboroxine, 2,4,6-triethylboroxine, 2,4,6-trivinylboroxine, 2,4,6-trimethoxyboroxine, 2,4,6-trimethoxyboroxine, and triphenylboroxine; and halogen-substituted hydrocarbon groups such as tris(2,2,2-trifluoroethyl)borate, 2,4,6-tris(4-fluorophenyl)boroxine, and 2,4,6-tris(3,4,5-trifluorophenyl)boroxine.

[0098] The anion receptor having an aluminum atom includes an aluminum compound that functions as a Lewis acid, and has the formula AlX 1 3 (X in the formula 1 is a halogen atom, which may be a fluorine atom), the formula: Al(OR 35 ) 3 (R in the formula 35 is a hydrocarbon group, which may be an alkyl group.

[0099] The anion receptor may also be an azaether. An azaether is an ether compound in which —O— is replaced by —NR E - (where R E is a hydrogen atom or an organic group). The azaether may be either a linear azaether or a cyclic azaether. The azaether may have an electron-withdrawing group, for example, in the hydrocarbon moiety.

[0100] The content of the anion receptor in the electrolyte composition may be 10 to 200 parts by mass, 30 to 180 parts by mass, 50 to 150 parts by mass, or 80 to 130 parts by mass relative to 100 parts by mass of the polymer capable of conducting alkali metal ions.

[0101] The electrolyte composition may contain an alkali metal salt, such as MF, MCl, MBr, MI, or MClO, where M is an alkali metal. 4 , MPF 6 , MBF 4 , M 2 SO 4 , M[(C h F 2h+1 ) SO 3 ] (h is 0 to 3), M[(C h F 2h+1 ) SO 2 ] 2 N (h is 0 to 3), M{[(C h F 2h+1 ) SO 2 ]N[(C i F 2i+1 ) SO 2]} (h and i are 0 to 3). One or more types of alkali metal salts may be used. The alkali metal contained in the alkali metal salt may be the same alkali metal element as the alkali metal element contained in the structural unit (A) described in the description of the polymer of the present disclosure.

[0102] The content of the alkali metal salt in the electrolyte composition may be 10 to 200 parts by mass, 20 to 150 parts by mass, 30 to 100 parts by mass, or 40 to 75 parts by mass relative to 100 parts by mass of the polymer capable of conducting alkali metal ions.

[0103] The electrolyte composition may further contain other resins (binder resins, etc.) such as fluorine-based resins, fabrics such as nonwoven fabrics, porous materials, viscosity adjusters, etc. The electrolyte composition may contain, as the fluorine-based resin, a resin having a carbon chain as the main chain. The carbon chain may be formed by radical polymerization of an ethylenically unsaturated group. Examples of fluorine-based resins include poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), etc.

[0104] The content of the other resin in the electrolyte composition may be 10 to 100 parts by mass, 20 to 80 parts by mass, 30 to 70 parts by mass, or 40 to 60 parts by mass relative to 100 parts by mass of the polymer capable of conducting alkali metal ions.

[0105] The method for producing the electrolyte composition is not particularly limited, and examples thereof include a method in which a dry film of the polymer of this embodiment or a dry film is produced by mixing the polymer of this embodiment with a binder resin, and then the dry film is impregnated with an organic solvent. When the electrolyte composition contains an alkali metal salt or an anion receptor, the polymer, optionally a binder resin, and the alkali metal salt or anion receptor may be mixed to produce a dry film, and then an organic solvent may be added, or the alkali metal salt or anion receptor may be dissolved in an organic solvent and added to the dry film.

[0106] The electrolyte composition of this embodiment can be used as a composition for forming an electrolyte for batteries, capacitors, etc. That is, the electrolyte of this embodiment includes the above-described electrolyte composition. Examples of the battery include batteries that perform charging and discharging by the movement of alkali metal ions, such as lithium ion batteries and sodium ion batteries. The battery may be a primary battery, a secondary battery, or a solid-state battery.

[0107] The battery of this embodiment includes a positive electrode, a negative electrode, and an electrolyte disposed between the positive electrode and the negative electrode. The positive electrode may be a layer containing a positive electrode material formed on a current collector. The negative electrode may be a layer containing a negative electrode material formed on a current collector. The following description will be given taking a lithium-ion battery as an example.

[0108] The negative electrode of the lithium ion battery is not particularly limited and may contain a negative electrode active material and, if necessary, a conductive additive, a binder, etc. Examples of the negative electrode active material include simple elements such as Li, Si, P, Sn, Si—Mn, Si—Co, Si—Ni, In, and Au, alloys or composites containing these elements, carbon materials such as graphite, substances in which lithium ions are inserted between the layers of the carbon material, and oxides containing titanium.

[0109] The positive electrode of the lithium ion battery is not particularly limited, and may contain a positive electrode active material and, if necessary, a conductive additive, a binder, etc. Examples of the positive electrode active material include lithium composite metal oxides containing lithium and a transition metal element. The transition metal element may be at least one selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Cu, and Al, and may contain Ni. Examples of the lithium composite metal oxides include LiCoO 2 , LiNiO 2 , LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 , Li 2 MnO 3 , LiNi x Mn y Co 1-x-y O 2[0<x+y<1]), LiNi x Co y Al 1-x-y O 2 [0<x+y<1]), LiCr 0.5 Mn 0.5 O 2 , LiFePO 4 , Li 2 FeP 2 O 7 , LiMnPO 4 , LiFeBO 3 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 CuO 2 , Li 2 FeSiO 4 , Li 2 MnSiO 4 When the positive electrode active material contains an alkali metal element other than Li, specific examples thereof include those in which Li in the above specific examples is replaced with another alkali metal.

[0110] The positive electrode (positive electrode material) of this embodiment may further contain a solid electrolyte material, a binding resin (binder), a conductive additive, and the like.

[0111] The battery may have a separator. The separator may be a porous material, such as a porous resin material. Specific examples of the separator include a porous polyolefin membrane and a porous ceramic membrane.

[0112] Example 1 The lithiated carboxyl group-containing copolymer of Example 1 was produced by the following method.

[0113] Saccharin methacrylamide (SacM) (1.8848 g, 7.5 mmol, synthetic product), styrene (St) (0.86 mL, 7.5 mmol), tetralin (0.15 mL), and azobisisobutyronitrile (24.7 mg, 0.15 mmol) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile=1:1 (volume ratio)) (12.1 mL), and the solution was stirred at 60° C. for 24 hours to obtain a copolymer of saccharin methacrylamide and styrene (raw material copolymer).

[0114] Next, a 25 mM phenothiazine solution in 1,4-dioxane (45.0 mL, 1.13 mmol) and 100 equivalents of water were added to the resulting raw copolymer, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.61 g).

[0115] The composition ratio of the structural units in the polymer was MAA:St = 48:52 (molar ratio). 1 The carboxyl group content was calculated by measuring the H-NMR spectrum. Then, the -COOH group-containing copolymer (0.61 g, 3.21 mmol) was dissolved in dimethylformamide (12 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (449.1 mg, 18.82 mmol) relative to the amount of SacM initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days. As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer had been converted to -COOLi was obtained (0.43 g).

[0116] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 18,200.

[0117] Example 2 tert-Butyl methacrylate (tBMA) (1.22 mL, 7.5 mmol), styrene (St) (0.86 mL, 7.5 mmol), and azobisisobutyronitrile (20.0 mg, 0.12 mmol) were dissolved in toluene (13.0 mL) and stirred at 60°C for 24 hours to obtain a copolymer of tert-butyl methacrylate and styrene (raw copolymer) (0.59 g). The composition ratio of the structural units in the raw polymer was tBMA:St = 46:54 (molar ratio). The composition ratio was determined by dissolving the raw polymer in deuterated chloroform, 1 This was confirmed by measuring the H NMR spectrum.

[0118] Next, excess trifluoroacetic acid (15.0 mL, 196 mmol) was added to the obtained raw copolymer (0.59 g), and the mixture was stirred at 40° C. for 24 hours. As a result, the —C(═O)—O—C(CH 3 ) 3 The groups were substituted with —COOH groups (that is, the structural units derived from tBMA were converted to methacrylic acid (MAA) units), and a —COOH group-containing copolymer was obtained (0.36 g).

[0119] Then, the -COOH group-containing copolymer (0.36 g) was dissolved in dimethylformamide (3.0 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH relative to the amount of tBMA initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days. As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer had been converted to -COOLi was obtained (0.26 g). The obtained lithiated carboxyl group-containing copolymer was dissolved in deuterated dimethyl sulfoxide. 1 By measuring the H NMR spectrum, it was found that the composition ratio of the structural units in the lithiated carboxyl group-containing copolymer was lithiated MAA:St=47:53 (molar ratio). The number average molecular weight of the raw copolymer was 18,000.

[0120] (Preparation of Electrolyte Compositions) Each component was mixed according to the compositions shown in Tables 1 and 2 to prepare each electrolyte composition.

[0121] The abbreviations in Tables 1 and 2 are as follows: TMP: trimethyl phosphate (DN=23.0) TEP: triethyl phosphate (DN=23.4) EC: ethylene carbonate (DN=16.4) PC: propylene carbonate (DN=15.1) PVDF-HFP: vinylidene fluoride-co-hexafluoropropylene

[0122] <Measurement of Ionic Conductivity> The ionic conductivity of the electrolyte composition was measured by the following method. Ionic conductivity (σ 25 ) are shown in Tables 1 and 2.

[0123] First, in a glove box under a dry argon atmosphere, an evaluation cell of the coin-type battery CR2032 was assembled. Specifically, a test laminate was prepared by laminating each layer in the following order in the evaluation cell: stainless steel plate / electrolyte composition / stainless steel plate.

[0124] Measurements are made using an impedance measuring device under the conditions of 25°C, a frequency range of 0.1 Hz to 1 MHz, and an applied voltage of 10 mV (vs. open circuit voltage). The ionic conductivity σ can be calculated using the following formula. In the formula, R represents the impedance value, A represents the area of ​​the sample, and t represents the thickness of the sample. σ (S cm -1 )=t(cm) / (R(Ω)×A(cm 2 ))

[0125] <Activation Energy> Ion conductivity measurements using the above evaluation cell were also performed under conditions of 25°C, 30°C, 40°C, 50°C, 60°C, and 70°C to measure the change in ionic conductivity with respect to temperature. Activation energy was calculated from the slope of a graph of the common logarithm of ionic conductivity versus the reciprocal of temperature using the Arrhenius equation (logk = logA - Ea / RT, where k is the reaction rate constant, A is the frequency factor, Ea is the activation energy, R is the gas constant, and T is the absolute temperature). The results are shown in Tables 1 and 2.

[0126]

[0127]

[0128] (Preparation of Electrolyte Compositions) Each component was mixed according to the compositions shown in Tables 3 and 4 to prepare each electrolyte composition containing an anion receptor, and the ionic conductivity and activation energy at 25° C. were determined by the methods described above.

[0129] The abbreviations in Tables 3 and 4 are as follows: Lithium (bistrifluoromethanesulfonyl)imide (LiTFSI) was used as the lithium salt in Table 4. MTD: 2-methoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane TEB: tris(2,2,2-trifluoroethyl)borate TFB: 2,4,6-tris(4-fluorophenyl)boroxine PVDF-HFP: vinylidene fluoride-co-hexafluoropropylene

[0130]

[0131]

[0132] Example 3 The lithiated carboxyl group-containing copolymer of Example 2 was produced by the following method.

[0133] In the following Examples 3 to 5, the monomer represented by the following formula (i.e., 4-(2-methoxyethoxy)methoxystyrene) was used in place of the styrene in Example 1. (Here, m = 1 and n = 1. Hereinafter, the compound represented by the above formula will be referred to as St m n Also written as.)

[0134] Saccharin methacrylamide (SacM) (628.8 mg, 2.5 mmol) and St 1 1 (0.49 mL, 2.5 mmol), azobisisobutyronitrile (8.8 mg, 0.05 mmol), and tetralin (0.05 mL) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile = 1:1 (volume ratio)) (3.75 mL), and the mixture was stirred at 60 °C for 24 hours to obtain SacM and St. 1 1 A copolymer (raw copolymer) was obtained.

[0135] Next, a 25 mM phenothiazine solution in 1,4-dioxane (15.0 mL, 0.38 mmol) and 100 equivalents of water were added to the resulting raw copolymer, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.28 g).

[0136] The composition ratio of the structural units in the polymer is MAA:St 1 1 The molar ratio was 47:53. The polymer was dissolved in deuterated dimethyl sulfoxide, 1 It was calculated by measuring the H NMR spectrum.

[0137] Then, the -COOH group-containing copolymer (0.28 g, 1.00 mmol) was dissolved in dimethylformamide (4.6 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (149.0 mg, 6.22 mmol) relative to the amount of SacM initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days (24 hours). As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer were converted to -COOLi was obtained (0.23 g). In the synthesized copolymer, -COO - Because the groups were fixed on the copolymer, they did not move even when a voltage was applied, and the transference number of lithium ions was sufficiently high.

[0138] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 30,100.

[0139] (Example 4) Saccharin methacrylamide (SacM) (628.7 mg, 2.5 mmol) and St 1 2(0.58 mL, 2.5 mmol), azobisisobutyronitrile (8.6 mg, 0.05 mmol), and tetralin (0.05 mL) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile = 1:1 (volume ratio)) (3.75 mL), and the mixture was stirred at 60 °C for 24 hours to obtain SacM and St 1 2 A copolymer (raw copolymer) was obtained.

[0140] Next, a 25 mM phenothiazine solution in 1,4-dioxane (15.0 mL, 0.38 mmol) and 100 equivalents of water were added to the resulting raw copolymer, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.33 g).

[0141] The composition ratio of the structural units in the polymer is MAA:St 1 2 The molar ratio was 48:52. The polymer was dissolved in deuterated dimethyl sulfoxide, 1 It was calculated by measuring the H NMR spectrum.

[0142] Then, the -COOH group-containing copolymer (0.33 g, 1.02 mmol) was dissolved in dimethylformamide (6.0 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (147.9 g, 6.25 mmol) relative to the amount of SacM initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days (24 hours). As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer were converted to -COOLi was obtained (0.29 g). In the synthesized copolymer, -COO - Because the groups were fixed on the copolymer, they did not move even when a voltage was applied, and the transference number of lithium ions was sufficiently high.

[0143] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 30,100.

[0144] (Example 5) Saccharin methacrylamide (SacM) (0.6284 g, 2.5 mmol) and St 1 3 (0.68 g, 2.5 mmol), azobisisobutyronitrile (8.9 mg, 0.05 mmol), and tetralin (0.05 mL) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile = 1:1 (volume ratio)) (3.70 mL), and the mixture was stirred at 60 °C for 24 hours to obtain SacM and St 1 3 A copolymer (raw copolymer) was obtained.

[0145] Next, a 25 mM phenothiazine solution in 1,4-dioxane (15.0 mL, 0.38 mmol) and 100 equivalents of water were added to the resulting raw copolymer, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.60 g).

[0146] The composition ratio of the structural units in the polymer is MAA:St 1 3 The molar ratio was 49:51. The polymer was dissolved in deuterated dimethyl sulfoxide, 1 It was calculated by measuring the H NMR spectrum.

[0147] Then, the -COOH group-containing copolymer (0.49 g, 1.34 mmol) was dissolved in dimethylformamide (10.0 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (150.2 mg, 6.27 mmol) relative to the amount of SacM initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days (24 hours). As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer were converted to -COOLi was obtained (0.43 g). In the synthesized copolymer, -COO - Because the groups were fixed on the copolymer, they did not move even when a voltage was applied, and the transference number of lithium ions was sufficiently high.

[0148] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 32,000.

[0149] Each electrolyte composition was prepared by mixing the components according to the composition shown in Table 5, and the ionic conductivity and activation energy at 25° C. were determined by the above-mentioned method.

[0150]

[0151] Example 6 A copolymer of styrene and a monomer A1 represented by the following formula was produced as follows. First, monomer A1 was produced as follows.

[0152] (Synthesis of Monomer A1) Under a nitrogen atmosphere, trifluoromethanesulfonamide (52.5 mmol, 7.83 g, manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in dehydrated acetonitrile (150 mL, manufactured by Kanto Chemical Co., Ltd.). To this solution, lithium hydroxide (105 mmol, 2.51 g, manufactured by Tokyo Chemical Industry Co., Ltd.) and 4-acetamidobenzenesulfonyl chloride (50 mmol, 11.68 g, manufactured by Tokyo Chemical Industry Co., Ltd.) were added in that order, and the mixture was heated under reflux for 5 hours. After cooling to room temperature, an excess amount of acetonitrile (700 mL) was added to precipitate a solid, which was separated by filtration and washed with dichloromethane (manufactured by Kanto Chemical Co., Ltd.) to obtain Intermediate 1. The yield was 97.1%. -Structural formula of Intermediate 1:

[0153] Under a nitrogen atmosphere, 5% hydrochloric acid (22.5 mL) was added to Intermediate 1 (15 mmol, 5.28 g) and stirred at 90°C for 2 hours. After cooling to room temperature, an aqueous lithium hydroxide solution was added until the pH reached 7 or higher, while checking with pH test paper, and then the mixture was dried under reduced pressure to obtain a solid. The obtained solid was extracted with an acetonitrile solution and dried under reduced pressure to obtain Intermediate 2. The yield was 92.6% based on the raw materials for Intermediate 1. Structural formula of Intermediate 2:

[0154] Under a nitrogen atmosphere, maleic anhydride (13.3 mmol, 1.30 g, manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in dehydrated 1,4-dioxane (manufactured by Kanto Chemical Co., Ltd.). To this solution, the entire amount of a solution of intermediate 2 (13.2 mmol, 4.09 g) in dehydrated tetrahydrofuran (26.4 mL, manufactured by Kanto Chemical Co., Ltd.) prepared under a nitrogen atmosphere was added dropwise, and the mixture was stirred at room temperature for 12 hours. After the reaction, the precipitate was filtered and dried in vacuum at 60°C for 4 hours to obtain a solid containing intermediate 3. Structural formula of intermediate 3:

[0155] Under a nitrogen atmosphere, a solid containing Intermediate 3 (14.0 mmol, 5.70 g) and lithium acetate (13.3 mmol, 1.09 g, manufactured by Tokyo Chemical Industry Co., Ltd.) were added to acetic anhydride (12.3 mL, manufactured by Tokyo Chemical Industry Co., Ltd.) and stirred at 70°C for 3 hours. The entire solution after the reaction was added dropwise to an excess amount of diethyl ether (manufactured by Kanto Chemical Co., Ltd.) at 0°C, and the precipitate was collected by filtration. Under an inert atmosphere, the precipitate was extracted with dehydrated acetonitrile (manufactured by Kanto Chemical Co., Ltd.) and dried under reduced pressure to obtain Monomer A1. The yield throughout the entire process was 72.8%.

[0156] 0.558 g of monomer A1, 0.149 g of styrene, and 11.7 mg of azobisisobutyronitrile were dissolved in 6.7 mL of dehydrated acetonitrile, and the monomer consumption rate was confirmed by adding tetralin as an internal standard substance, while the reaction was carried out at 60°C for 24 hours under a nitrogen atmosphere. The polymerization solution was dialyzed in acetonitrile and vacuum dried at 120°C, thereby obtaining 0.640 g (yield 87%) of a copolymer (copolymer of Example A1). The monomer introduction ratio of Example A1:styrene was 52:48. 1 Calculated from H-NMR.

[0157] Number average molecular weight of the copolymer Mn = 9.4 × 10 4 , weight average molecular weight Mw=4.2×10 5 The molecular weight distribution Mw / Mn was 4.45. The number average molecular weight and the weight average molecular weight were measured by gel permeation chromatography. Styrene was a commercially available reagent with a purity of >98% manufactured by Aldrich Co., Ltd., dissolved in CaCl 2 and dried overnight. 2 The purity was improved by adding HCl and distilling under reduced pressure, and then the product was used.

[0158] Each component was mixed according to the composition shown in Table 6 to prepare each electrolyte composition, and the ionic conductivity, activation energy, and transport number at 25° C. were determined by the above-mentioned methods.

[0159]

[0160] <Measurement of Lithium Ion Transference Number> The lithium ion transference numbers of the electrolyte compositions prepared as described above were measured by the following method. The results are shown in Table 7.

[0161] An evaluation cell of a coin-type lithium battery CR2032 was assembled in a glove box under a dry argon atmosphere. Specifically, a test laminate was prepared by stacking layers in the evaluation cell in the order of lithium / electrolyte composition / lithium.

[0162] The lithium ion transport number measurement method is introduced in Polymer, 28, 2324 (1987). That is, 10 mV is applied to the test laminate at room temperature (25° C.), and the initial current value (I 0 ) and steady-state current value (I ss ) was measured, and the interface resistance measured value R 0 and the measured interface resistance R after voltage application SS The lithium ion transport number (t Li+ ) was calculated. V in the formula is the applied voltage. Li+ =I ss (VI 0 R 0 ) / I 0 (VI SS R SS )

[0163]

Claims

1. An electrolyte composition comprising a polymer capable of conducting alkali metal ions and an organic solvent, wherein the donor number of the organic solvent contained in the electrolyte composition represented by the following formula (I) is 16.5 or more. (In the formula, n is the total number of organic solvents contained in the electrolyte composition and is 1 or more, DNi is the donor number of the i-th organic solvent, and fi is the mass fraction of the i-th organic solvent.) 2. An electrolyte composition comprising a polymer capable of conducting alkali metal ions and an organic solvent, wherein the proportion of the organic solvent having a donor number of 17 or more in the organic solvent contained in the electrolyte composition is 10 mass % or more relative to the total amount of the organic solvent.

3. The electrolyte composition according to claim 1 or 2, wherein the organic solvent comprises one or more organic solvents selected from the group consisting of ether-based solvents, phosphate-based solvents, carbonate-based solvents, fluorine-based solvents, and nitrile-based solvents.

4. The electrolyte composition according to claim 1 or 2, further comprising an anion receptor.

5. The electrolyte composition according to claim 4, wherein the anion receptor is a compound containing a Group 13 element having Lewis acidity.

6. The electrolyte composition according to claim 1 or 2, further comprising an alkali metal salt.

7. The electrolyte composition of claim 1 or 2, wherein the polymer capable of conducting alkali metal ions contains one or more groups selected from the group consisting of an alkali metal substituted sulfonylimide group, an alkali metal substituted sulfonic acid group, an alkali metal substituted carboxylic acid group, and an alkali metal substituted phenol group.

8. A battery comprising the electrolyte composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Ionic polymer

    JP2012107219A

  • Secondary battery, and method of manufacturing secondary battery

    JP2014112526A

  • Polymer electrolytes for electrochemical cells

    US20220271337A1