Transition metal supported catalyst with improved hydrogenation activity and use thereof

By modifying the alumina support with an alkyl group-attached silica precursor and reducing transition metal precursors on the catalyst, the issues of agglomeration and spinel formation are addressed, resulting in improved hydrogenation activity and hydrogen storage capabilities.

WO2024232632A1PCT designated stage expired Publication Date: 2024-11-14INDUSTRY UNIVERSITY COOPERATION FOUNDATION HANYANG UNIVERSITY +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Transition metal catalysts tend to agglomerate, leading to reduced activity and formation of inactive spinel phases when supported on alumina, limiting their effectiveness in hydrogenation reactions, especially in large-scale synthesis and hydrogen storage applications involving liquid organic hydrogen carriers.

Method used

A catalyst is developed by modifying the alumina support with an alkyl group-attached silica precursor and introducing a transition metal precursor, followed by reduction under elevated temperature conditions to improve dispersibility and reducibility of transition metal nanoparticles, thereby reducing strong interactions and enhancing acid site properties.

Benefits of technology

The modified catalyst exhibits improved hydrogenation activity and stability, effectively supporting hydrogen storage and release in liquid organic hydrogen carriers, with enhanced dispersibility and reducibility of transition metal nanoparticles, leading to superior hydrogen storage performance compared to conventional catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006123_14112024_PF_FP_ABST
    Figure KR2024006123_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present disclosure are a catalyst and use thereof for application in a hydrogenation reaction, the catalyst having improved dispersibility and reducibility of transition metal particles as well as acid sites by grafting an alkyl group-attached silica precursor onto an alumina support to modify (surface-modify) the alumina support and then introducing a precursor of a transition metal having hydrogenation activity into the modified alumina support to reduce same.
Need to check novelty before this filing date? Find Prior Art

Description

Transition metal-supported catalyst with improved hydrogenation activity and use thereof

[0001] The present disclosure relates to a transition metal-supported catalyst with improved hydrogenation activity and its use. More specifically, the present disclosure relates to a catalyst in which an alumina support is modified (surface-modified) by grafting an alkyl group-attached silica precursor onto the alumina support, and then a precursor of a transition metal having hydrogenation activity is introduced into the modified alumina support and reduced, thereby improving not only acid sites but also the dispersion and reducibility of transition metal particles, and its use in a hydrogenation reaction.

[0002] Transition metal catalysts typically have a tendency to easily agglomerate or aggregate transition metal particles during the synthesis and / or reaction processes employed. To address this issue, alumina supports, which induce strong metal-support interactions, are widely used. Among these, gamma-alumina is particularly well-known as a commercial catalyst support, exhibiting excellent physical properties and thermal stability. It can induce strong metal-support interactions and possesses electron-deficient Lewis acid sites that can strongly interact with electron-rich aromatic molecules.

[0003] However, an excessively strong interaction between the transition metal and the alumina support may promote the formation of a spinel phase that is rather inactive, thereby reducing the number of metal active sites.

[0004] In this regard, improvement of the synthetic method for mild interaction between transition metal and alumina support, use of other metal oxides (ZrO2, MgO, La2O3, CeO2, Pr6O) as cocatalysts or promoters on alumina 11Methods for adding alumina (e.g., nitride) have been reported (Chem. Eng. J. 436 (2022) 135195; Fuel 284 (2021) 119082; Appl. Catal., B 264 (2020) 118448; Fuel Process. Technol. 198 (2020) 106223; Appl. Catal., B 263 (2020) 118177, etc.). However, the aforementioned methods have many limitations in large-scale synthesis processes using commercial alumina.

[0005] Therefore, it would be even more useful if a catalyst were developed that effectively alleviates the interaction between the transition metal and the alumina support while using commercial alumina, and furthermore, can be applied not only to conventional hydrogenation reactions (e.g., hydrocracking, hydrodeoxygenation, hydrodesulfurization, hydrodenitrification, etc.) but also to hydrogenation reactions accompanying hydrogen storage by liquid organic hydrogen carriers (LOHCs), which have recently been widely spotlighted as an alternative energy source. Representative examples of LOHC materials include toluene, benzyltoluene, and dibenzyltoluene. These LOHCs are composed of a pair of hydrogen-lean and hydrogen-rich (hetero)aromatic compounds, and store or release hydrogen through hydrogenation and dehydrogenation reactions, respectively, by the catalyst. In particular, catalysts for hydrogen storage (hydrogenation catalysts) must exhibit high activity under mild conditions to minimize the influence of impurities (e.g., chlorine-containing compounds, fluorine derivatives, water, methane, carbon dioxide, carbon monoxide, etc.).

[0006] To this end, a catalyst manufacturing technology is required that provides good hydrogenation activity by alleviating the strong interaction between the transition metal and the alumina support that induces the formation of an inactive spinel, and improving the dispersion and reducibility of the transition metal particles, including the acid site characteristics.

[0007] In one specific example of the present disclosure, it is intended to provide a hydrogenation catalyst and a method for producing the same, which effectively suppresses deactivation due to strong interaction between a transition metal, which is an active component, and an alumina support in a supported hydrogenation catalyst, while increasing the acid site of the catalyst and improving the dispersion and reducibility of transition metal nanoparticles.

[0008] According to another specific example of the present disclosure, it is intended to provide an effective LOHC hydrogen storage method using the above-described catalyst.

[0009] According to the first page of this disclosure,

[0010] a) providing an alumina support;

[0011] b) Alkyl group (C) on the alumina support n )-A step of preparing a modified alumina support by grafting an attached silica precursor;

[0012] c) a step of introducing a transition metal precursor having hydrogenation activity into the modified alumina support to form a modified alumina support containing a precursor of a transition metal; and

[0013] d) The above alkyl group (C n ) - a step of reducing the precursor-containing modified alumina support of the transition metal under elevated temperature conditions to remove alkyl groups derived from the attached silica precursor and form transition metal nanoparticles;

[0014] A method for producing a catalyst for hydrogenation reaction including a .

[0015] According to an exemplary embodiment, the process can be performed without calcination treatment for each of the modified alumina support and the precursor-containing modified alumina support of the transition metal.

[0016] According to an exemplary embodiment, the transition metal having hydrogenation activity may be at least one selected from the group consisting of nickel (Ni), zinc (Zn), iron (Fe), manganese (Mn), cobalt (Co), and copper (Cu).

[0017] According to an exemplary embodiment, the alkyl group (C n )-alkyl group of the attached silica precursor (C n ) may be at least one silicon-containing compound having a carbon number (n) in the range of 1 to 18 and selected from the group consisting of silane, siloxane, silazane and silanol.

[0018] According to an exemplary embodiment, the alkyl group (C n )-attached silica precursor can be represented by the following general formula 1.

[0019] [General Formula 1]

[0020] R m -Si-X 4-m

[0021] In the above formula, R is an alkyl group (C n ) and,

[0022] m is 1 to 3, and

[0023] X may be at least one selected from the group consisting of an alkoxy group and a halogen group having 1 to 4 carbon atoms.

[0024] According to an exemplary embodiment, the alkyl group (C n )-attached silica precursor may be at least one selected from the group consisting of alkyltrialkoxysilane, dialkyldialkoxysilane and trialkylalkoxysilane.

[0025] According to an exemplary embodiment, the amount of hydrogen used to reduce the oxide of the transition metal in the hydrogenation catalyst may be at least 0.6 mol (H2) / mol (transition metal), as measured by temperature reduction analysis (TPR).

[0026] According to an exemplary embodiment, the ratio of Si / Al in the catalyst can be controlled in the range of 0.01 to 5 mol%.

[0027] According to an exemplary specific example, the content (support amount) of the transition metal in the catalyst can be determined in the range of 0.1 to 30 wt%.

[0028] According to the second page of this disclosure,

[0029] modified alumina support; and

[0030] Transition metal nanoparticles having hydrogenation activity supported on the above modified alumina support;

[0031] As a hydrogenation catalyst comprising:

[0032] The content (support amount) of the transition metal in the above hydrogenation catalyst is determined in the range of 0.1 to 30 wt%,

[0033] The above modified alumina support is a silica modified alumina support, and

[0034] A hydrogenation catalyst is provided wherein the amount of hydrogen used to reduce an oxide of a transition metal in the catalyst is at least 0.6 mol (H2) / mol (transition metal), as measured by temperature reduction analysis (TPR).

[0035] According to an exemplary embodiment, the degree of dispersion (measured by H2 chemisorption) of the transition metal nanoparticles supported on the modified alumina support in the catalyst may be at least 2%.

[0036] According to an exemplary embodiment, the size (measured by high-angle annular dark-field scanning transmission electron microscopy) of the transition metal nanoparticles supported on the modified alumina support in the catalyst may be 10 nm or less.

[0037] According to an exemplary embodiment, the amount of acid sites in the catalyst may be at least 100 μmol / g when analyzed by pyridine-chemisorbed FT-IR spectrum.

[0038] According to the third page of this disclosure,

[0039] A hydrogenation step of storing hydrogen in a liquid organic hydrogen carrier in the presence of a catalyst; and

[0040] A dehydrogenation step for releasing hydrogen from the hydrogenated liquid organic hydrogen carrier in the presence of a catalyst,

[0041] The catalyst used in the above hydrogenation step is:

[0042] modified alumina support; and

[0043] A transition metal having hydrogenation activity supported on the above modified alumina support;

[0044] Includes,

[0045] The content (support amount) of the transition metal in the above hydrogenation catalyst is determined in the range of 0.1 to 30 wt%,

[0046] The above modified alumina support is a silica modified alumina support,

[0047] When measured by temperature reduction analysis (TPR), the amount of hydrogen used to reduce the oxide of the transition metal in the catalyst is at least 0.6 mol (H2) / mol (transition metal), and

[0048] A method for storing hydrogen or releasing hydrogen is provided by alternately performing the above hydrogenation step and dehydrogenation step.

[0049] According to a specific example of the present disclosure, the alumina support comprises an alkyl group (C n )- grafted with a silica precursor, and then introducing a hydrogenated transition metal, and manufacturing a hydrogenation catalyst by directly reducing it, and further excluding the calcination treatment for each of the modified alumina support and the transition metal-containing modified alumina support, the dispersion and reducibility of the transition metal nanoparticles, and the acid site characteristics can be improved compared to a conventional transition metal-supported alumina catalyst. The catalyst having such improved hydrogenation activity can be effectively applied to hydrogen storage using a liquid organic hydrogen carrier (LOHC). In particular, the method presented in this specific example can be easily applied even when using commercial alumina as a support, and thus can be advantageous in terms of mass production of the catalyst.

[0050] Figure 1 is Ni / SGA_C in an embodiment. n A drawing showing a schematic procedure for manufacturing a TES catalyst;

[0051] Figure 2 is an FT-IR spectrum of Al2O3 and C3TES-on-Al2O3;

[0052] Figure 3 is a graph showing the carbon content and actual Si / Al ratio of Al2O3 and C3TES-on-Al2O3;

[0053] Figure 4 shows the N2 physisorption results of Al2O3 and C3TES-on-Al2O3 (specific surface area: S BET , pore volume: V p ) is a graph representing;

[0054] Figure 5 shows the XRD analysis results of Al2O3 and C3TES-on-Al2O3;

[0055] Figure 6 shows the N2 physisorption results of Al2O3(r) and SGA_C3TES(r) (specific surface area: S BET , pore volume: V p ) is a graph representing;

[0056] Figure 7 is a graph showing the actual Si / Al ratio and surface Si / Al ratio of Al2O3(r) and SGA_C3TES(r), respectively;

[0057] Figure 8 shows the XRD analysis results of Al2O3(r) and SGA_C3TES(r);

[0058] Figure 9 shows the results of Al2O3(r) and SGA_C3TES(r). 27 Al MAS NMR analysis results (Al in tetrad: Al IV , Al in 5-coordinate system: Al V , 6-coordinate Al: Al VI ) and;

[0059] Figure 10 shows the measurement results of the water contact angle (θ) of Al2O3 and C3TES-on-Al2O3;

[0060] Figure 11 shows the XRD analysis results of Ni / Al2O3 and Ni / SGA_C3TES catalysts;

[0061] Figure 12 shows HAADF-STEM images of Ni / Al2O3 and Ni / SGA_C3TES catalysts (Ni particle size: D Ni , standard deviation: σ);

[0062] Figure 13 shows the H2 chemisorption results (hydrogen adsorption amount: V) of Ni / Al2O3 and Ni / SGA_C3TES catalysts. H2 ) is a graph representing;

[0063] Fig. 14 XPS Ni 2p of Ni / Al2O3 and Ni / SGA_C3TES catalysts 3 / 2 It's a spectrum;

[0064] Figure 15 shows the H2-TPR analysis results of oxidized Ni / Al2O3 and Ni / SGA_C3TES catalysts (amount of hydrogen consumed per Ni atom: A H2-TPR ) is a graph representing;

[0065] Figure 16 is a pyridine-chemisorbed FT-IR spectrum (amount of Lewis acid sites: L) of Ni / Al2O3 and Ni / SGA_C3TES catalysts;

[0066] Figure 17 shows the H0-BT hydrogenation activity (degree of hydrogenation: DoH) of Ni / Al2O3 and Ni / SGA_C3TES catalysts. l ) is a graph showing the measurement results (reaction mode: batch A; 10 g H0-BT, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h);

[0067] Figure 18 Ni / Al2O3 and Ni / SGA_C n This is a graph showing the actual Si / Al ratio and the surface Si / Al ratio of the TES catalyst, respectively;

[0068] Figure 19: Ni / Al2O3 and Ni / SGA_C n H0-BT hydrogenation activity of TES catalyst (H0-BT conversion: X H0-BT ) is a graph showing the measurement results (reaction conditions: batch A: 10 g H0-BT, 160 ℃, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h);

[0069] Fig. 20 shows Al2O3 and 2.9C n N2 physisorption results of TES-on-Al2O3 (specific surface area: S BET , pore volume: V p ) and;

[0070] Fig. 21 Al2O3 and 2.9C n The measurement results of the water contact angle (θ) of TES-on-Al2O3;

[0071] Fig. 22 Ni / Al2O3 and Ni / SGA_2.9C n N2 physisorption results of TES catalyst (specific surface area: S BET , pore volume: V p ) is a graph representing;

[0072] Fig. 23 Ni / Al2O3 and Ni / SGA_2.9C n XRD analysis results of the TES catalyst;

[0073] Fig. 24 Ni / Al2O3 and Ni / SGA_2.9C n HAADF-STEM image of TES catalyst (Ni particle size: D Ni , standard deviation: σ);

[0074] Fig. 25 Ni / Al2O3 and Ni / SGA_2.9C n H2 chemisorption results of TES catalyst (hydrogen adsorption amount: V H2 ) is a graph representing;

[0075] Fig. 26 Ni / Al2O3 and Ni / SGA_2.9C n XPS Ni 2p of TES catalyst 3 / 2 It's a spectrum;

[0076] Figure 27 shows oxidized Ni / Al2O3 and Ni / SGA_2.9C. n H2-TPR analysis results of TES catalyst (amount of hydrogen consumed per Ni atom: A H2-TPR ) is a graph representing;

[0077] Fig. 28 Ni / Al2O3 and Ni / SGA_2.9C n Pyridine-chemisorbed FT-IR spectrum of TES catalyst (amount of Lewis acid sites: L);

[0078] Fig. 29 Ni / Al2O3, Ni / SGA_2.9C n TES, Ni / SGA_2.9C n H0-BT hydrogenation activity of TES(c) and Ni / SIRAL1 catalysts (H0-BT conversion: X H0-BT ) Measurement results (reaction mode: batch A; 10 g H0-BT, 160 ℃, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h);

[0079] Figure 30 shows the results of measuring the H0-BT hydrogenation activity of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts (reaction mode: batch B; 10 g H0-BT, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm), which are (a) the degree of hydrogenation (DoH) and (b) the rate constant (k);

[0080] Figure 31 shows the results of H0-BT hydrogenation activity measurements of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts (reaction mode: batch B; 10 g H0-BT, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm), where (a) time for complete hydrogenation (t full ), and (b) rate constant (k) and activation energy (E a ) and;

[0081] Figure 32 shows the XRD analysis results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c), and Ni / SIRAL1 catalysts;

[0082] Figure 33 shows HAADF-STEM images of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts (Ni particle size: D Ni , standard deviation: σ);

[0083] Figure 34 shows the H2 chemisorption results (hydrogen adsorption amount: V) of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts. H2 ) is a graph representing;

[0084] Figure 35 shows the measurement results of the water contact angle (θ) of Al2O3, 2.9C3TES-on-Al2O3, SGA_2.9C3TES(c), and SIRAL1;

[0085] Fig. 36 shows the XPS Ni 2p of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts. 3 / 2 It's a spectrum;

[0086] Figure 37 shows the H2-TPR analysis results of oxidized Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts (amount of hydrogen consumed per Ni atom: A H2-TPR ) is a graph representing;

[0087] Figure 38 shows the H2-TPD analysis results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts (the relative amount of hydrogen desorbed per Ni atom, the peak area of ​​the Ni catalyst compared to the peak area of ​​Ni / Al2O3: A H2-TPD,Ni catalyst / A H2-TPD,Ni / Al2O3 ) and;

[0088] Figure 39 shows the TGA results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts adsorbed with H0-BT;

[0089] Figure 40 is a pyridine-chemisorbed FT-IR spectrum (amount of Lewis acid sites: L) of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts;

[0090] Figure 41 shows the results of measuring the H0-BT hydrogenation activity of Ni / Al2O3, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) catalysts through continuous experiments (H0-BT conversion: X H0-BT , H6-BT Selectivity: S H6-BT , H 12 -BT Selectivity: S H12-BT , degree of hydrogenation: DoH) and (reaction mode: continuous, (a) 180 ℃, 40 bar H2, WHSV = 6 h -1, H2 / H0-BT = 20; (b) 220 °C, 40 bar H2, WHSV = 15 h -1 , H2 / H0-BT = 20);

[0091] Figure 42 shows the N2 physisorption results (specific surface area: S) of Ni / Al2O3, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) catalysts before (fresh) and after (spent) continuous experiments. BET , pore volume: V p ) is a graph representing; and

[0092] Figure 43 shows HAADF-STEM images of Ni / Al2O3, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) catalysts before (fresh) and after (spent) continuous experiments (Ni particle size: D Ni , standard deviation: σ).

[0093] The present invention can be fully achieved by the following description. It should be understood that the following description describes preferred embodiments of the present invention and is not necessarily limited thereto. Furthermore, it should be understood that the attached drawings are provided for illustrative purposes only and are not intended to limit the present invention.

[0094] The terms used in this specification may be defined as follows.

[0095] “Support” may mean a material (typically a solid material) having a high specific surface area to which the catalytically active component is attached.

[0096] “Nanoparticle” can broadly mean a particle whose feature has a maximum dimension in the nanometer range, for example, in the range of about 0.1 to 1000 nm, and specifically in the range of about 1 to 700 nm.

[0097] "Spinel" is a type of mineral with a cubic crystal structure, which can be represented by the general formula AB2X4.

[0098] "Hydrogenation" may mean a reaction that increases the hydrogen content in a compound by chemically adding hydrogen to at least a portion of the compound by contacting the compound with a catalyst under a supply of hydrogen.

[0099] "Dehydrogenation" can mean a reaction in which hydrogen is removed from a compound and further in which the removed hydrogen is released from the compound.

[0100] "Impregnation" may refer to a method of manufacturing a catalyst by contacting a separately synthesized support with a solution containing a dissolved catalyst precursor, and then, if necessary, subjecting it to a drying and / or calcination (or reduction) treatment process.

[0101] “Salt” can broadly mean a compound in which a metal cation is combined with an inorganic anion or an organic anionic species.

[0102] When a numerical range is specified herein with lower and / or upper limits, it is understood that any sub-combination within that numerical range is also disclosed. For example, when "1 to 5" is described, it can include 1, 2, 3, 4, and 5, as well as any sub-combination therebetween.

[0103] Where any component or member in this specification is described as being "connected" to another component or member, unless otherwise stated, it is to be understood that this includes not only the case where it is directly connected to said other component or member, but also the case where it is connected through the intervention of said other component or member.

[0104] Similarly, the term "contact" may be understood to include not only direct contact but also contact under the intervention of other components or absences.

[0105] The expressions "on" and "above" can be understood as referring to relative positional concepts. Therefore, not only may other components or layers be directly present on the mentioned layer, but other layers (intermediate layers) or components may also be present or interposed between them. Similarly, the expressions "below," "underneath," and "beneath," as well as the expression "between," can also be understood as relative concepts of position. Furthermore, the expression "sequentially" can also be understood as a relative positional concept.

[0106] In this specification, when it is said that a component "includes", it means that it may further include other components and / or steps, unless otherwise stated.

[0107]

[0108] Overall disclosure

[0109] According to one specific example of the present disclosure, first, an alkyl group (C) is added to a support, alumina, particularly commercial alumina. n ) - grafting a silica precursor is performed. In this way, in a catalyst in which a transition metal having hydrogenation activity is supported on an alumina support, the strong interaction between the transition metal and the alumina support, which promotes the formation of an inactive spinel, can be alleviated by modifying the surface of the alumina support with a metal oxide, specifically, silica.

[0110] Also, alkyl group (C n)-A precursor of a transition metal is introduced onto an alumina support grafted (modified) with a silica precursor, thereby forming a precursor-containing modified alumina support of a transition metal, and a direct reduction step is performed under elevated temperature conditions. Specifically, a reduction treatment can be performed without performing a heat treatment step (or a calcination step) under an oxygen-containing atmosphere for each of the modified alumina support and the precursor-containing modified alumina support of a transition metal.

[0111] As described above, the alkyl group (C n )-modification (surface modification) of alumina using a silica precursor attached thereto, and a hydrogenation catalyst manufactured through direct reduction treatment without additional calcination process can improve the dispersion and reducibility of transition metal nanoparticles, and further increase the acid sites that favorably affect the hydrogenation reaction by forming silica-alumina. The catalyst with improved properties in this way can be applied to various hydrogenation reactions, and in particular, when applied to the hydrogenation reaction accompanying hydrogen storage during the hydrogen storage / release process of LOHC such as benzyltoluene (H0-BT), it can achieve superior hydrogen storage performance compared to conventional transition metal-supported alumina catalysts.

[0112]

[0113] Hydrogenation catalyst and its preparation

[0114] According to one specific example, the hydrogenation catalyst may be a heterogeneous catalyst, using a porous inorganic oxide, specifically alumina, as a support. In this regard, alumina not only possesses a pore structure that facilitates relatively easy control of the hydrogenation reaction, but also offers a relatively high surface area, high packing density, stability under high temperature and high pressure conditions, physical strength, and regenerative properties. Furthermore, since alumina possesses Lewis acid sites, it may be advantageous for the adsorption of reactants during the hydrogenation reaction.

[0115] According to an exemplary embodiment, the present embodiment may use commercial alumina used in the manufacture of various catalysts in the art, but is not limited thereto. Accordingly, various aluminas may be used without particular limitation as long as they have suitable properties as a support for a hydrogenation catalyst.

[0116] According to an exemplary embodiment, the shape of the alumina support is not particularly limited, but considering the stability and efficiency of the catalyst, it may be advantageous to have a ball shape. Alternatively, structures of other shapes such as a tablet shape, a granule shape, a pellet shape, etc. are also possible. In this case, the size (or diameter) of the alumina support may be, for example, in the range of about 0.1 to 10 mm, specifically about 0.5 to 5 mm, and more specifically about 1 to 3 mm, but this can be understood as an exemplary purpose.

[0117] In the present specific example, the alumina that can be used as a support may have a specific surface area and pore volume above a certain level, and pores of a controlled size. For example, the specific surface area (BET) of the alumina support may be determined in consideration of the high dispersion of the transition metal particles, and may be, for example, in the range of about 50 to 500 m2 / g, specifically about 100 to 350 m2 / g, and more specifically about 150 to 300 m2 / g. In addition, the pore volume of the alumina may be, for example, in the range of about 0.2 to 2 cm3 / g, specifically about 0.3 to 1 cm3 / g, and more specifically about 0.4 to 0.7 cm3 / g. The pore volume of the alumina may affect the diffusion of the reactants during the hydrogenation reaction, the concentration of the reactants within the pores, etc., and thus, it may be advantageous to control the pore volume within the aforementioned range. However, the present disclosure is not limited thereto.

[0118] Meanwhile, according to an exemplary specific example, the pore size (diameter) of the alumina support may be in the range of, for example, about 3 to 15 nm, specifically about 4 to 10 nm, and more specifically about 5 to 8 nm, considering that the molecular size of the reactant is mostly large and thus affects the diffusion rate of the reactant.

[0119] According to one specific example, a step of modifying (surface modifying) the alumina support is performed for the purpose of suppressing the deactivation factor caused when the hydrogenation-active transition metal is supported on the alumina support in the form of nanoparticles and improving the catalytic activity. To this end, an alkyl group (C) is added to the alumina support. n )-modification can be performed by grafting a silica precursor.

[0120] According to an exemplary embodiment, the surface of the alumina support is provided with an alkyl group (C n )-a step of contacting the attached silica precursor can be performed. According to a specific embodiment, a dispersion of an alumina support is prepared, and an alkyl group (C n )-modification can be performed by adding a silica precursor (liquid modification).

[0121] According to an exemplary embodiment, an alkyl group (C n )-The silica precursor may be selected from a silicon-containing compound that is easy to graft onto the surface of an alumina support, for example, at least one selected from silane, siloxane, silazane, silanol, etc. In this case, the alkyl group (C) attached to the silica precursor n ) can be determined by considering the fact that the number of carbon atoms is a factor affecting hydrophobicity and further the loading of Ni species, and may be in the range of about 1 to 18 carbon atoms, specifically about 2 to 12, more specifically about 3 to 8 carbon atoms.

[0122] According to an exemplary embodiment, an alkyl group (C n )-attached silica precursor can be represented by the following general formula 1.

[0123] [General Formula 1]

[0124] R m -Si-X 4-m

[0125] In the above formula, R is an alkyl group (C n ) and,

[0126] m is 1 to 3, and

[0127] X may be at least one selected from the group consisting of an alkoxy group and a halogen group having 1 to 4 carbon atoms.

[0128] According to a specific embodiment, an alkyl group (C n )-attached silica precursor is an alkyl group (C n ) can be adjusted in the range of about 1 to 18, specifically about 2 to 12, and more specifically about 3 to 8.

[0129] According to an exemplary embodiment, an alkyl group (C n)-attached silica precursor, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, methyltripropoxysilane, dimethyldipropoxysilane, trimethylpropoxysilane, methyltributoxysilane, dimethyldibutoxysilane, trimethylbutoxysilane, methyltrifluorosilane, dimethyldifluorosilane, trimethylfluorosilane, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, methyltribromosilane, dimethyldibromosilane, trimethylbromosilane, methyltriiodosilane, dimethyldiiodosilane, trimethyliodosilane, ethyltrimethoxysilane, diethyldimethoxysilane, triethylmethoxysilane, Ethyltriethoxysilane, diethyldiethoxysilane, triethylethoxysilane, ethyltripropoxysilane, diethyldipropoxysilane, triethylpropoxysilane, ethyltributoxysilane, diethyldibutoxysilane, triethylbutoxysilane, ethyltrifluorosilane, diethyldifluorosilane, triethylfluorosilane, ethyltrichlorosilane, diethyldichlorosilane, triethylchlorosilane, ethyltribromosilane, diethyldibromosilane, triethylbromosilane, ethyltriiodosilane, diethyldiiodosilane, triethyliodosilane, propyltrimethoxysilane, dipropyldimethoxysilane, tripropylmethoxysilane, propyltriethoxysilane, dipropyldiethoxysilane, tripropylethoxysilane, propyltripropoxysilane, dipropyldipropoxysilane, Tripropylpropoxysilane, propyltributoxysilane, dipropyldibutoxysilane, tripropylbutoxysilane, propyltrifluorosilane, dipropyldifluorosilane, tripropylfluorosilane, propyltrichlorosilane, dipropyldichlorosilane, tripropylchlorosilane, propyltribromosilane, dipropyldibromosilane, tripropylbromosilane, propyltriiodosilane, dipropyldiiodosilane, tripropyliodosilane, butyltrimethoxysilane, dibutyldimethoxysilane, tributylmethoxysilane, butyltriethoxysilane, dibutyldiethoxysilane, tributylethoxysilane, butyltripropoxysilane, dibutyldipropoxysilane, tributylpropoxysilane, butyltributoxysilane, dibutyldibutoxysilane, tributylbutoxysilane,Butyltrifluorosilane, dibutyldifluorosilane, tributylfluorosilane, butyltrichlorosilane, dibutyldichlorosilane, tributylchlorosilane, butyltribromosilane, dibutyldibromosilane, tributylbromosilane, butyltriiodosilane, dibutyldiiodosilane, tributyliodosilane, hexyltrimethoxysilane, dihexyldimethoxysilane, trihexylmethoxysilane, hexyltriethoxysilane, dihexyldiethoxysilane, trihexylethoxysilane, hexyltripropoxysilane, dihexyldipropoxysilane, trihexylpropoxysilane, hexyltributoxysilane, dihexyldibutoxysilane, trihexylbutoxysilane, hexyltrifluorosilane, dihexyldifluorosilane, Trihexylfluorosilane, hexyltrichlorosilane, dihexyldichlorosilane, trihexylchlorosilane, hexyltribromosilane, dihexyldibromosilane, trihexylbromosilane, hexyltriiodosilane, dihexyldiiodosilane, trihexyliodosilane, octyltrimethoxysilane, dioctyldimethoxysilane, trioctylmethoxysilane, octyltriethoxysilane, dioctyldiethoxysilane, trioctylethoxysilane, octyltripropoxysilane, dioctyldipropoxysilane, trioctylpropoxysilane, octyltributoxysilane, dioctyldibutoxysilane, trioctylbutoxysilane, octyltrifluorosilane, dioctyldifluorosilane, trioctylfluorosilane, octyltrichlorosilane, dioctyldichlorosilane, Trioctylchlorosilane, octyltribromosilane, dioctyldibromosilane, trioctylbromosilane, octyltriiodosilane, dioctyldiiodosilane, trioctyliodosilane, decyltrimethoxysilane, didecyldimethoxysilane, tridecylmethoxysilane, decyltriethoxysilane, didecyldiethoxysilane, tridecylethoxysilane, decyltripropoxysilane, didecyldipropoxysilane, tridecylpropoxysilane, decyltributoxysilane, didecyldibutoxysilane, tridecylbutoxysilane, decyltrifluorosilane, didecyldifluorosilane, tridecylfluorosilane, decyltrichlorosilane, didecyldichlorosilane, tridecylchlorosilane, decyltribromosilane, didecyldibromosilane, Tridecylbromosilane, decyltriiodosilane, didecyldiiodosilane, tridecyliodosilane, dodecyltrimethoxysilane, didodecyldimethoxysilane, tridodecylmethoxysilane,Dodecyltriethoxysilane, didodecyldiethoxysilane, tridodecylethoxysilane, dodecyltripropoxysilane, didodecyldipropoxysilane, tridodecylpropoxysilane, dodecyltributoxysilane, didodecyldibutoxysilane, tridodecylbutoxysilane, dodecyltrifluorosilane, didodecyldifluorosilane, dodecyltrichlorosilane, didodecyldichlorosilane, tridodecylchlorosilane, dodecyltribromosilane, didodecyldibromosilane, tridodecylbromosilane, dodecyltriiodosilane, didodecyldiiodosilane, tridodecyliodosilane, hexadecyltrimethoxysilane, dihexadecyldimethoxysilane, Trihexadecylmethoxysilane, hexadecyltriethoxysilane, dihexadecyldiethoxysilane, trihexadecylethoxysilane, hexadecyltripropoxysilane, dihexadecyldipropoxysilane, trihexadecylpropoxysilane, hexadecyltributoxysilane, dihexadecyldibutoxysilane, trihexadecylbutoxysilane, hexadecyltrifluorosilane, dihexadecyldifluorosilane, trihexadecylfluorosilane, hexadecyltrichlorosilane, dihexadecyldichlorosilane, trihexadecylchlorosilane, hexadecyltribromosilane, dihexadecyldibromosilane, trihexadecylbromosilane, hexadecyltriiodosilane, dihexadecyldiiodosilane, Trihexadecyliodosilane, octadecyltrimethoxysilane, dioctadecyldimethoxysilane, trioctadecylmethoxysilane, octadecyltriethoxysilane, dioctadecyldiethoxysilane, trioctadecylethoxysilane, octadecyltripropoxysilane, dioctadecyldipropoxysilane, trioctadecylpropoxysilane, octadecyltributoxysilane, dioctadecyldibutoxysilane, trioctadecylbutoxysilane, octadecyltrifluorosilane, dioctadecyldifluorosilane, trioctadecylfluorosilane, octadecyltrichlorosilane, dioctadecyldichlorosilane, trioctadecylchlorosilane, octadecyltribromosilane, dioctadecyldibromosilane, trioctadecylbromosilane, At least one selected from octadecyltriiodosilane, dioctadecyldiiodosilane, trioctadecyliodosilane, etc. can be exemplified.

[0130] According to an exemplary specific example, in general formula 1, X may be an alkoxy group having 3 to 8 carbon atoms, which may be advantageous in that it may exhibit low price and high hydrogenation activity.

[0131] In this regard, alkyl group (C n )-attached silica precursor may be at least one selected from, for example, methyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldiethoxysilane, trimethylmethoxysilane, triethylmethoxysilane, trimethylethoxysilane, triethylethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, dipropyldimethoxysilane, dipropyldiethoxysilane, etc. According to a specific embodiment, in general formula 1, an alkyl group (C n ) has a carbon number (n) of 3, m is 1, and X can be an ethoxy group (i.e., propyltriethoxysilane).

[0132] According to an exemplary embodiment, when preparing a dispersion of an alumina support, a medium (liquid medium) can be selected from a solvent having a boiling point comparable to or higher than the contact temperature and capable of inhibiting the condensation reaction of the silica precursor, for example, a ketone (e.g., methyl ethyl ketone, etc.); an ether (e.g., octyl ether, butyl ether, hexyl ether, etc.); a heterocyclic-containing solvent (e.g., tetrahydrofuran (THF)); an aromatic (e.g., toluene, xylene, mesitylene, benzene, etc.); a sulfoxide (e.g., dimethyl sulfoxide (DMSO)); an amide (e.g., dimethylformamide (DMF)), a hydrocarbon (e.g., pentane, hexane, heptane, octane, decane, dodecane, tetradecane, hexadecane, etc.); Alcohols (e.g., octanol, decanol, etc.) can be exemplified, and one or more of the types listed above can be used in combination.

[0133] According to a specific embodiment, toluene may be used as a medium for preparing an alumina dispersion, which may be advantageous in suppressing the condensation reaction of a silica precursor (e.g., a silane compound). In addition, the concentration of the alumina dispersion may be adjusted to ensure sufficient dispersion of the alumina support within the liquid medium, and may be, for example, in a range of about 0.01 to 50 wt%, specifically about 1 to 20 wt%, and more specifically about 3 to 10 wt%.

[0134] In this regard, the amount of the added silica precursor can be controlled in a theoretical or nominal Si / Al ratio range of, for example, about 0.01 to 50 mol%, specifically about 0.1 to 20 mol%, and more specifically about 1 to 10 mol%.

[0135] According to an exemplary embodiment, the contact temperature between the alumina support and the silica precursor can be controlled in a range of, for example, about 25 to 200° C., specifically about 50 to 150° C., and more specifically about 100 to 120° C. In addition, the contact time can be controlled in a range of, for example, at least about 0.1 hour, specifically about 1 to 7 hours, and more specifically about 2 to 5 hours.

[0136] After contact between the silica precursor and the alumina support as described above has been performed, a conventional post-treatment procedure may be performed, for example, washing may be performed at least about once, specifically about 2 to 5 times, using the solvent used in preparing the alumina dispersion as described above to remove residual silica precursor, and additionally drying may be performed.

[0137] The above-mentioned alkyl group (C n)-The hydrophobicity of the surface of the alumina support increases through surface modification by the attached silica precursor. For example, the water contact angle (θ) of the alumina before modification may be, for example, about 20° or less, specifically about 17° or less, more specifically in the range of about 14 to 15°, but after modification, it may be, for example, at least about 25°, specifically at least about 30°, more specifically in the range of about 35 to 160°. The increased hydrophobicity of the surface of the alumina support may act as a factor in supporting the transition metal, which is an active ingredient, with good dispersion without agglomeration. At this time, the alkyl group (C) in the silica precursor n ) may show a tendency for the water contact angle of the surface of the modified alumina support to increase as the carbon number (n) of the modified alumina support increases. In addition, as the amount of silica precursor attached on the alumina support increases (i.e., as the Si / Al ratio increases), the water contact angle of the modified alumina support may show a tendency for increasing.

[0138] In addition, as a result of modification by grafting of the silica precursor, the pore properties of the alumina support may change, for example, the specific surface area, pore volume, and pore size may tend to slightly decrease compared to before modification. As an example, the specific surface area (BET) of the modified alumina support may be, for example, in the range of about 40 to 480 m2 / g, specifically about 90 to 330 m2 / g, and more specifically about 140 to 280 m2 / g. Meanwhile, the pore volume of the modified alumina support may be, for example, in the range of about 0.1 to 1.8 cm3 / g, specifically about 0.2 to 1.5 cm3 / g, and more specifically about 0.3 to 0.6 cm3 / g. Additionally, the pore size (diameter) of the modified alumina support may be in the range of, for example, about 2 to 14 nm, specifically about 3 to 9 nm, and more specifically about 4 to 7 nm.

[0139] According to one specific example, a step of introducing (attaching) a precursor of a transition metal having hydrogenation activity onto an alumina support grafted (modified) with a silica precursor is performed. In order to introduce the precursor of the transition metal into the modified alumina support, techniques known in the art, such as an impregnation method (specifically, a dry impregnation method, a wet impregnation method, and specifically, an initial wet impregnation method), an ion exchange method, an electrostatic adsorption method, and a precipitation method, can be applied, and specifically, an impregnation method can be applied. For this purpose, a metal precursor such as a salt or complex of the metal known in the art can be used without any particular limitation.

[0140] In this regard, in the present specific example, a transition metal precursor can be introduced into a previously modified alumina support without separate calcination treatment. In this case, the hydrophobicity of the alkyl group attached to the silica precursor suppresses the phenomenon of transition metal particles agglomerating with each other in a hydrophobic medium and induces the transition metal particles to be attracted to the silica side rather than to the alumina side, thereby alleviating the strong interaction between the alumina support and the transition metal, thereby improving the reducibility of the transition metal particles.

[0141] According to an exemplary embodiment, the transition metal having hydrogenation activity may be at least one selected from nickel (Ni), zinc (Zn), iron (Fe), manganese (Mn), cobalt (Co), copper (Cu), molybdenum (Mo), rhenium (Re), and the like. According to a specific embodiment, the transition metal may be nickel (Ni), which may be advantageous in that it can strongly adsorb a large amount of hydrogen during a hydrogenation reaction.

[0142] However, many of the transition metals with hydrogenation activity can show a tendency to form an inactive spinel (i.e., aluminum spinel) phase due to strong interaction with the support alumina, such as MgAl2O4, ZnAl2O4, FeAl2O4, MnAl2O4, (Mg,Fe)Al2O 4, CoAl2O4 , CuAl2O4, etc. can be used as an example. As such a spinel phase is formed, the hydrogenation activity decreases due to a decrease in the number of metal active sites. However, when commercial alumina manufactured by a general method is used as a support, the formation of spinel can be prominent. Therefore, in the present specific example, as described above, by grafting or modifying the surface of the alumina support using a specific silica precursor, the interaction between the supported transition metal and the alumina support can be effectively alleviated.

[0143] According to an exemplary specific example, as a precursor of a transition metal having hydrogenation activity, any precursor that can be supported on a support can be applied without particular limitation, for example, acetate, nitrate, sulfate, carbonate, hydroxide, halide, hydrate thereof, etc., and as a complex, an acetylacetonate complex, a phosphine complex, etc. can be exemplified. In addition, the above-mentioned transition metal precursors can be used alone or in combination. In particular, a nitrate or a hydrate thereof can be used.

[0144] When nickel (Ni) is used as a transition metal, at least one selected from, for example, nickel nitrate, nickel sulfate, nickel phosphate, nickel halide, nickel carboxylate, nickel hydroxide, nickel carbonate, nickel acetylacetonate complex, and nickel acetate hydrates thereof can be used. More specifically, nickel nitrate and / or its hydrate (for example, Ni(NO3)2·6H2O) can be used.

[0145] According to an exemplary embodiment, for impregnation (specifically wet impregnation) or ion exchange, a solution containing a transition metal precursor, specifically an aqueous solution or an organic solution, can be prepared and used to attach the transition metal precursor onto the modified alumina support.

[0146] According to a specific embodiment, the metal precursor can be contacted with the modified alumina support in the form of an organic solution dissolved in an organic solvent. In order to support the precursor of the transition metal, which is an active ingredient, on the support, it is generally applied in the form of an aqueous solution, but in the present embodiment, the form of an organic solution can be applied, considering that the hydrophobicity of the surface of the alumina support is increased through the above-described modification process. At this time, the solvent that can be used to prepare the organic solution of the transition metal precursor can be selected from a type that exhibits relatively hydrophobicity, for example, ketones (e.g., methyl ethyl ketone); ethers (e.g., octyl ether, butyl ether, hexyl ether); heterocyclic-containing solvents (e.g., tetrahydrofuran (THF)); sulfoxides (e.g., dimethyl sulfoxide (DMSO)); amides (e.g., dimethylformamide (DMF)), etc. can be used in combination of one or two or more thereof.

[0147] At this time, the metal content (based on element) in the metal precursor solution can be controlled in consideration of the physical properties of the support, and may be, for example, in the range of about 0.1 to 30 wt%, specifically about 1 to 10 wt%, and more specifically about 2 to 5 wt%.

[0148] In this way, the modified alumina support in the loading process comes into contact with the transition metal precursor solution. At this time, the loading (impregnation or ion exchange) temperature is not particularly limited, but may be, for example, about 15 to 40°C, specifically about 20 to 30°C, and more specifically, at room temperature. The contact time is also not particularly limited, but may be controlled in the range of, for example, about 0.1 to 24 hours, specifically about 1 to 12 hours, and more specifically about 2 to 5 hours. The above-described loading conditions may be understood to be exemplary.

[0149] After loading the transition metal precursor, conventional subsequent procedures, such as filtration and / or drying to remove moisture or solvent, may be performed, wherein the drying temperature may be controlled, for example, between about 50 and 130°C (specifically, between about 70 and 120°C, and more specifically, between about 80 and 110°C). It should be understood that these drying conditions are exemplary.

[0150] According to one specific example, an alkyl group (C) grafted onto an alumina support n )-A reduction treatment step is performed for the purpose of removing alkyl groups derived from the attached silica precursor and also converting the transition metal precursor into nanoparticles of the transition metal. Through the reduction treatment, the transition metal precursor is converted into a reduced metal (i.e., a metal element), while the silica precursor used for surface modification of the alumina support can be converted into silica. In this regard, when spinel is formed due to a strong interaction between the transition metal and alumina (for example, the interaction between the transition metal oxide and Al2O3), reduction of the transition metal is difficult, but in the present specific example, the formation of spinel can be suppressed by modifying with a specific silica precursor.

[0151] In an exemplary embodiment, as the atmospheric gas used in the reduction treatment, at least one selected from hydrogen, carbon monoxide, carbon dioxide, methane, etc., specifically hydrogen, may be used.

[0152] According to an exemplary embodiment, the reduction treatment can be performed under elevated temperature conditions. At this time, the reduction temperature can be controlled so that the transition metal precursor can be reduced into transition metal nanoparticles while effectively suppressing the agglomeration of the transition metal particles and the formation of spinel, for example, in the range of about 500 to 900°C (specifically, about 600 to 800°C, more specifically, about 650 to 750°C). In addition, the heating rate can be controlled, for example, in the range of about 1 to 10°C / min, specifically, in the range of about 3 to 6°C / min. In addition, the reduction treatment time can be set within a range of time sufficient for the transition metal precursor to be reduced into transition metal nanoparticles, for example, in the range of about 1 to 10 hours, specifically, about 2 to 8 hours, more specifically, about 3 to 6 hours. In an exemplary embodiment, the pressure (partial pressure of the reducing gas) during the reduction process is not particularly limited, but may be, for example, in the range of about 1 to 5 bar, specifically about 1.5 to 4 bar, and more specifically about 2 to 3 bar. Alternatively, the reduction step may be performed by flowing (flowing) the reducing gas into the heat treatment device. The above-described reduction process conditions may be understood as illustrative and are not necessarily limited thereto.

[0153] According to an exemplary embodiment, the size (diameter) of the supported transition metal particles may be significantly lower than that of a transition metal-supported alumina support catalyst prepared by a conventional method. As an example, the size (diameter; which may be measured by high-angle annular dark-field scanning transmission electron microscopy) of the transition metal particles in the catalyst may be, for example, in the range of about 10 nm or less, specifically about 0.5 to 7 nm, and more specifically about 1 to 2.7 nm.

[0154] According to an exemplary embodiment, the ratio of silicon (Si) to aluminum (Al) in the hydrogenation catalyst (the Si / Al ratio) can be controlled in a range of, for example, about 0.01 to 5 mol%, specifically about 1 to 4.5 mol%, more specifically about 1.5 to 4.2 mol%, particularly specifically about 2 to 4 mol%, and further about 2.5 to 3.5 mol%. According to a specific embodiment, the Si / Al ratio can be set in a range of, for example, about 2.7 to 3.4 mol%, specifically about 2.8 to 3.3 mol%, more specifically about 2.9 to 3.2 mol%. These values, when compared to the theoretical (or nominal) Si / Al ratio selected during the preparation of the catalyst above, are determined by the surface hydroxyl groups of alumina and the surface 5-coordinated Al (Al V ) may be at a reduced level due to a lack of species.

[0155] According to an exemplary embodiment, the content (support amount) of the transition metal in the hydrogenation catalyst may be in the range of, for example, about 0.1 to 30 wt%, specifically about 1 to 10 wt%, and more specifically about 2 to 5 wt%.

[0156] What is notable in this specific example is that, in a typical method for preparing a hydrogenation catalyst, a step of calcining (i.e., heat treatment in an oxygen-containing atmosphere) is performed on a modified alumina support containing a transition metal precursor to remove ligands of the transition metal precursor and moisture within the support, but this calcination is excluded in this specific example. In this regard, in a typical method for preparing a hydrogenation catalyst that performs reduction after calcination, the formed transition metal oxide tends to have increased fluidity due to the low melting point of the formed transition metal oxide, causing the formed transition metal nanoparticles to aggregate. However, by directly reducing the transition metal precursor supported (loaded) on the modified alumina support without calcination, the fluidity (movement) of the transition metal nanoparticles in the form of metal due to the high melting point is suppressed, thereby suppressing the aggregation of the transition metal nanoparticles.

[0157] Meanwhile, the hydrogenation catalyst according to the present specific example may have a significantly increased degree of dispersion of the transition metal, which is an active component. For example, the degree of dispersion (measured by H2 chemisorption) of the transition metal nanoparticles supported on the modified alumina support within the catalyst may be, for example, at least about 2%, specifically about 3 to 30%, more specifically about 3 to 15%, and particularly specifically about 5 to 7%.

[0158] In this way, the catalyst according to the present specific example can exhibit a characteristic in which the adsorption amount of hydrogen, which is a reactant of the hydrogenation reaction, is significantly increased due to the improved support form of the transition metal (e.g., small particle size, high dispersity, etc.). In this regard, the amount of hydrogen used to reduce the oxide of the transition metal in the catalyst (i.e., the amount of hydrogen adsorption per transition metal) can be used as an indicator, and for example, it can be at least about 0.6 mol (H2) / mol (transition metal), specifically at least about 0.7 mol (H2) / mol (transition metal), more specifically in the range of about 0.75 to 0.9 mol (H2) / mol (transition metal), and in a specific specific example, it can be in the range of about 0.78 to 0.82 mol (H2) / mol (transition metal).

[0159] For reference, the hydrogen adsorption per transition metal of the transition metal-supported alumina catalyst that is not modified with a silica precursor can be, for example, in a range of less than about 0.6 mol (H2) / mol (transition metal) (specifically, from about 0.4 to 0.55 mol (H2) / mol (transition metal)). In addition, the hydrogen adsorption per transition metal of the transition metal-supported alumina catalyst prepared according to the same procedure as in the present specific example, except that the calcination treatment is performed prior to the reduction treatment of the transition metal precursor-attached modified alumina support, can be, for example, in a range of less than about 0.6 mol (H2) / mol (transition metal) (specifically, from about 0.5 to 0.59 mol (H2) / mol (transition metal)).

[0160] In this way, the catalyst according to the present specific example can achieve a higher hydrogen adsorption amount per transition metal compared to an unmodified transition metal / alumina catalyst, a transition metal / alumina catalyst that has undergone a reduction treatment after calcination treatment, etc.

[0161] According to an exemplary embodiment, as silica-alumina is formed in the hydrogenation catalyst, the acid sites that enhance the hydrogenation activity may increase, and the acid sites of the catalyst may be quantified by pyridine-chemisorbed FT-IR spectra. As an example, the amount of acid sites in the catalyst according to the present embodiment may be, for example, at least about 100 μmol / g, specifically at least about 120 μmol / g, more specifically about 130 to 180 μmol / g, and particularly specifically about 138 to 155 μmol / g.

[0162] According to an exemplary embodiment, the pore shape of the hydrogenation catalyst according to the present embodiment can be changed to have a shape in which the specific surface area (BET) is somewhat reduced while the pore volume and pore size are somewhat increased compared to modified alumina.

[0163] As an example, the BET surface area of ​​the hydrogenation catalyst can be in the range of, for example, about 30 to 460 m2 / g, specifically about 80 to 310 m2 / g, more specifically about 130 to 260 m2 / g. Further, according to an exemplary embodiment, the pore volume of the hydrogenation catalyst can be in the range of, for example, about 0.15 to 1.9 cm3 / g, specifically about 0.21 to 1.7 cm3 / g, more specifically about 0.32 to 0.65 cm3 / g. Further, the pore size of the hydrogenation catalyst can be in the range of, for example, about 2.5 to 14.5 nm, specifically about 3.5 to 9.5 nm, more specifically about 4.5 to 7.5 nm.

[0164] According to an exemplary embodiment, the shape of the hydrogenation catalyst is not particularly limited, but considering the stability and efficiency of the catalyst, it can be applied as a structure such as a ball shape, a tablet shape, a granule shape, a pellet shape, etc. In this case, the size (or diameter) of the catalyst can be, for example, in the range of about 0.1 to 10 mm, specifically about 0.5 to 5 mm, and more specifically about 1 to 3 mm, but this can be understood as an exemplary purpose.

[0165]

[0166] Hydrogenation / dehydrogenation reactions using liquid organohydrogen carrier compounds (storage and release of hydrogen)

[0167]

[0168] According to one specific example of the present disclosure, a liquid organic hydrogen carrier (LOHC) can be used as a hydrogen storage material, wherein the liquid organic hydrogen carrier system is composed of hydrogen-lean and hydrogen-rich organic compounds, and can store (hydrogenate) and release (dehydrogenate) hydrogen through repeated catalytic hydrogenation and dehydrogenation cycles in the liquid or gas phase. In particular, by handling hydrogen in the form of a liquid organic hydrogen carrier, existing fuel equipment can be utilized, and unlike hydrogen storage by hydrogenation of a gas (e.g., carbon dioxide or nitrogen), when releasing hydrogen from a liquid organic hydrogen carrier, pure hydrogen can be produced after condensation of a carrier compound having a relatively high boiling point.

[0169] According to this specific example, the hydrogenation catalyst described above can be applied to hydrogen storage, i.e., hydrogenation reaction, of a liquid organic hydrogen carrier (LOHC).

[0170] According to an exemplary embodiment, the above-described hydrogenation catalyst can be effectively applied to a wide range of liquid organic hydrogen carriers, including nitrogen-containing heterocyclic liquid organic hydrogen carriers and liquid organic hydrogen carriers composed of hydrocarbons (specifically, aromatic hydrocarbon-based liquid organic hydrogen carriers such as toluene, monobenzyltoluene, dibenzyltoluene, etc.). Such compounds can typically have at least one conjugated bond in the molecule.

[0171] According to one specific example, the liquid organic hydrogen carrier may be at least one (in hydrogen-dilute form) selected from compounds represented by the following general formulae 2 to 11:

[0172]

[0173] [General Formula 2]

[0174]

[0175] [General Formula 3]

[0176]

[0177] [General Formula 4]

[0178]

[0179] [General Formula 5]

[0180]

[0181] [General Formula 6]

[0182]

[0183] [General Formula 7]

[0184]

[0185] [General Formula 8]

[0186]

[0187] [General Formula 9]

[0188]

[0189] [General Formula 10]

[0190]

[0191] [General Formula 11]

[0192]

[0193] In the above formula, R, R1, R2, R3, R4, R5, R6, R7. R8, R9, R 10 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 and R 20 Each is hydrogen or an alkyl group of C1 to C6, and X is -(CHR 21 ) n -(n is an integer from 1 to 3, and R 21 is H, OH, or an alkyl group of C1 to C6), and Y is CH or N.

[0194] The liquid organic hydrogen carrier compound exemplified above can exhibit a melting point of, for example, about 100°C or less, specifically about 0 to 80°C, more specifically about 10 to 60°C, and can maintain a liquid phase at room temperature, and further can have a boiling point of at least about 380°C, specifically about 130 to 350°C, more specifically about 180 to 300°C. Due to these melting point and boiling point characteristics, a hydrogen storage and release system using a liquid organic hydrogen carrier has the advantage of being able to omit the use of a separate solvent and / or additive for improving reactivity.

[0195] Meanwhile, the hydrogenation / dehydrogenation reaction can be carried out using a known reactor in the art, such as a batch reactor, a continuous reactor, a semi-continuous reactor, etc., and in particular, in the case of a liquid organic hydrogen carrier, especially a liquid organic hydrogen carrier compound having a relatively high boiling point, the reactor may be equipped with a stirrer as the hydrogenation and dehydrogenation reactions can occur in the liquid phase. According to an exemplary embodiment, the reaction can be carried out in a fixed bed reactor using a particle-shaped catalyst.

[0196] In the alternate operation mode of hydrogen storage / release according to an exemplary embodiment, the hydrogen storage mode may involve a step of contacting an organic compound (specifically, a liquid form) which is a liquid organic hydrogen carrier in a hydrogen-lean state with the aforementioned transition metal-supported alumina catalyst within the reaction system. According to an exemplary embodiment, the ratio of transition metal / LOHC (M / R) in the catalyst during hydrogen storage (hydrogenation reaction) may be set lower than that during hydrogen release (dehydrogenation) reaction. At this time, if the M / R ratio is excessively low, there is a limit to lowering the activation energy of the reaction, which may result in insufficient reaction activity. On the other hand, if the M / R ratio is excessively high, the volume of the solid catalyst significantly increases compared to that of the liquid reactant, forming an excessive slurry state. This makes stirring difficult during the reaction process, and diffusion limitation may occur, which may result in a phenomenon in which the active sites of the catalyst cannot be sufficiently utilized. Therefore, it may be advantageous to appropriately control the M / R ratio within the aforementioned range. However, the above ratio may vary depending on the type of liquid organic hydrogen carrier used.

[0197] As an example, the ratio of M / R in a hydrogenation reaction (hydrogen storage) can be controlled in a range of, for example, about 0.01 to 1 mol% (specifically about 0.1 to 0.5 mol%, more specifically about 0.15 to 0.4 mol%, and particularly specifically about 0.2 to 0.35 mol%), but this can be understood as an example.

[0198] When performing a hydrogenation reaction to store hydrogen in a hydrogen storage material (liquid organic hydrogen carrier), the reaction temperature may be, for example, in the range of about 50 to 250°C, specifically, in the range of about 80 to 220°C, and more specifically, in the range of about 100 to 190°C. In addition, the hydrogenation reaction pressure may be, for example, in the range of about 5 to 100 bar, specifically, in the range of about 20 to 80 bar, more specifically, in the range of about 25 to 70 bar, and particularly specifically, in the range of about 30 to 50 bar. In addition, the hydrogenation reaction time is not particularly limited, but may be, for example, in the range of about 0.5 to 24 hours, specifically, in the range of about 1 to 12 hours, and more specifically, in the range of 1.5 to 6 hours. However, the above-described hydrogenation reaction conditions may be understood as exemplary and may be changed depending on the type of hydrogen storage material used, etc.

[0199] According to an exemplary embodiment, the hydrogenation reaction can be carried out in a continuous mode, in which case the molar ratio of H2 / hydrogen-lean LOHC can be controlled in a range of, for example, about 5 to 40, specifically about 10 to 30, more specifically about 15 to 25. In addition, the space velocity (WHSV) can be, for example, about 1 to 30 h -1 , specifically about 3 to 25 h -1 , more specifically about 5 to 20 h -1 It can be controlled within the range of . However, the hydrogenation reaction conditions described above can be understood as an example.

[0200] Meanwhile, in the case of the hydrogenation reaction and the reversible dehydrogenation reaction (hydrogen evolution), a catalyst known to be usable in the dehydrogenation reaction of LOHC can be applied without any particular limitation. In this regard, as the dehydrogenation catalyst, for example, catalysts such as Pt / Al2O3, Pt / C, Pd / Al2O3, and Pd / C can be used. According to an exemplary specific example, in the case of the dehydrogenation reaction (hydrogen evolution), the ratio of M / R can be controlled in a range of, for example, about 0.05 to 2 mol% (specifically, about 0.2 to 1 mol%, more specifically, about 0.25 to 0.7 mol%, and particularly specifically, about 0.3 to 0.5 mol%), but this can be understood as an exemplary purpose.

[0201] According to an exemplary embodiment, by using the above-described transition metal / alumina catalyst, the hydrogenation reaction efficiency (defined as the number of moles of hydrogen actually stored by the hydrogenation reaction relative to the number of moles of hydrogen that can theoretically be stored from 1 mole of dehydrogenation reactant) can be, for example, at least about 30%, specifically at least about 50%, more specifically at least about 70%. In this case, the selectivity for the hydrogenation product corresponding to the hydrogen storage compound can be, for example, at least about 30%, specifically at least about 50%, more specifically at least about 70%.

[0202] Meanwhile, a dehydrogenation reaction may be performed to release hydrogen from a hydrogen storage material (liquid organic hydrogen carrier). Since this dehydrogenation reaction is an endothermic reaction, it may be performed at a higher reaction temperature (for example, a temperature range higher by about 50 to 150°C, specifically by about 60 to 120°C, and more specifically by about 80 to 100°C compared to the hydrogenation reaction temperature) than a hydrogenation reaction (exothermic reaction) of the same hydrogen storage material. According to an exemplary embodiment, the dehydrogenation reaction temperature may be in the range of, for example, about 100 to 350°C, specifically by about 150 to 320°C, and more specifically by about 180 to 290°C. In addition, unlike the reaction temperature, the dehydrogenation reaction pressure may be lower than the pressure conditions of the hydrogenation reaction, for example, about 1 to 10 bar, specifically by about 1 to 5 bar, and more specifically under atmospheric pressure conditions. Additionally, the dehydrogenation reaction time is not particularly limited, but may be set within a range of, for example, about 0.5 to 24 hours, specifically about 2 to 12 hours, and more specifically about 3 to 8 hours. However, the above-described dehydrogenation reaction conditions are to be understood as exemplary and may be changed depending on the type of hydrogen storage material used, etc.

[0203] According to an exemplary embodiment, the dehydrogenation reaction can be carried out in a continuous mode, in which case the space velocity (WHSV) is, for example, about 1 to 30 h -1 , specifically about 3 to 25 h -1 , more specifically about 5 to 20 h -1 It can be controlled within the range of . However, the above-described dehydrogenation reaction conditions can be understood as an example.

[0204] The present invention can be more clearly understood by the following examples, which are provided merely for the purpose of illustrating the present invention and are not intended to limit the scope of the invention.

[0205]

[0206] Example

[0207]

[0208] Manufacturing of catalysts

[0209] 10 g of gamma alumina (γ-Al2O3) was added to 200 ml of toluene at 25 ℃ and alkyltriethoxysilane (C) was added so that the theoretical (nominal) Si / Al ratios were 2 mol%, 4 mol%, 5 mol% and 8 mol%, respectively. n After injecting TES, it was aged at 112 ℃ for 3 hours.

[0210] Afterwards, it was washed three times with toluene and dried overnight at 113°C. The alumina prepared in this way, on which alkyltriethoxysilane was grafted (i.e., modified alumina support), was prepared by xC n It is referred to as TES-on-Al2O3 (x: actual Si / Al ratio, n = 1, 3, 8).

[0211] Next, 3 g of the modified alumina support was added to a solution of nickel (II) nitrate hexahydrate (Ni (NO 3 ) 2 6H 2 O) dissolved in 30 ml of tetrahydrofuran (THF) (theoretical Ni content: 3 wt %). Subsequently, the mixture was stirred at 25 ° C. for 2 h, the solvent was removed under vacuum at 38 ° C., and dried at 105 ° C. overnight.

[0212] Finally, under hydrogen atmosphere at 700 ℃ (5 ℃ min -1 ) was reduced for 5 hours to remove alkyl groups and form Ni particles in metallic form, thereby preparing a Ni-supported catalyst. The Ni-supported catalyst thus prepared was Ni / SGA_xC n It is referred to as TES (x: actual Si / Al ratio, n = 1, 3, 8).

[0213] Meanwhile, in the case of a catalyst loaded with Ni on another support, it was manufactured by performing the same Ni loading procedure as described above. At this time, C n Al2O3 support grafted with TES (C n Ni / SGA_xC is a catalyst supported on a support that has been calcined (fired) with TES-on-Al2O3. n It is referred to as TES(c).

[0214]

[0215] Methods for characterizing catalysts

[0216] The catalyst manufactured in the examples was characterized according to the following method.

[0217]

[0218] - Nitrogen physical adsorption (N2physisorption) analysis

[0219] N2 physisorption analysis was performed at 77 K using ASAP 2020 (Micromeritics) equipment. At this time, 100 mg of sample was heated under vacuum at 105 ℃ (10 ℃ min -1 ) was pretreated for 2 hours.

[0220]

[0221] - X-ray diffraction (XRD) analysis

[0222] XRD analysis was performed using a MiniFlex600 diffractometer (Rigaku) ​​equipped with a +Cu Kα radioactive source at a current of 15 mA and a voltage of 40 kV. Diffraction patterns were measured in the 2θ range from 10° to 90° with a step size of 0.02°.

[0223]

[0224] - X-ray photoelectron spectroscopy (XPS) analysis

[0225] XPS analysis was performed using a K-alpha spectrometer (Thermo Scientific) equipped with a monochromatic Al Kα X-ray source operating at a photon energy of 1486.6 eV. Spectra were measured at a pass energy of 40 eV with a step size of 0.1 eV and aligned relative to the C 1s binding energy of 284.6 eV.

[0226]

[0227] - Measurement of water contact angle

[0228] The water contact angle was measured by dropping 1.5 μl of H2O onto the sample surface pelleted in a 0.65 cm diameter circular disk at 25 °C using a DSA 100 (Kruss) instrument.

[0229]

[0230] - High-Angle Annular Dark Field-Scanning Transmission Electron Microscopy (HAADF-STEM) analysis

[0231] HAADF-STEM images were analyzed at 200 kV using a NEO ARM microscope (JEOL). The sample, which had been dispersed in ethanol, was dropped onto a 300-mesh copper grid and dried overnight at 60°C under vacuum.

[0232]

[0233] - Inductively Coupled Plasma-Optical Emission Spectrometry (ICP-OES) analysis

[0234] The actual contents of Ni, Al, and Si were analyzed by ICP-OES using an iCAP 7000 spectrometer (Thermo Scientific). The samples were dissolved in a mixture of nitric and hydrochloric acids (1:6) and pretreated in a Mileston Ehos Easy Microwave.

[0235]

[0236] - Elemental Analysis (EA)

[0237] Carbon content was analyzed through EA analysis using Flash EA1112 (Thermo Scientific) equipment.

[0238]

[0239] - Thermogravimetric Analysis (TGA)

[0240] TGA was performed using Discovery TGA550 Auto (TA Instrument). At this time, 5 mg of sample was heated at 700 ℃ (5 ℃ min) under nitrogen atmosphere -1 ) was heated to .

[0241]

[0242] - Noble 27 Al magic angle spinning nuclear magnetic resonance (solid-state 27 Al Magic-Angle Spinning Nuclear Magnetic Resonance; 27 Al MAS NMR) analysis

[0243] An Advance III HD spectrometer (Brucker) equipped with a 4 mm broadband MAS probe was used at an NMR frequency of 130.3 MHz, 1024 scans, and a spinning speed of 10 kHz. 27 Al MAS NMR spectra were measured.

[0244]

[0245] - Fourier-Transform Infrared (FT-IR) analysis

[0246] FT-IR analysis was performed using a Nicolet 6700 (Thermo Scientific) spectrometer. At this time, the pelletized sample in a 0.65 cm diameter circular disk was heated under vacuum at 105 ℃ (10 ℃ min -1 ) for 1 hour, then 4 cm under the same conditions -1 The spectrum was measured at a resolution of 32 scans.

[0247]

[0248] - Pyridine-chemisorbed FT-IR analysis

[0249] Pyridine chemisorption FT-IR analysis was performed using a Nicolet 6700 (Thermo Scientific) spectrometer. The pelletized sample in a 0.65 cm diameter circular disk was heated under vacuum at 300 °C (10 °C min -1 ) was pretreated for 1 hour and then cooled to 100 ℃. Then, 5 μl of pyridine was injected, adsorbed for 10 minutes, and physically adsorbed pyridine was removed for 30 minutes, and the mixture was heated at 100 ℃, 200 ℃, and 300 ℃, respectively, at a distance of 4 cm. -1 The spectrum was measured at a resolution of 32 scans.

[0250]

[0251] - Hydrogen chemisorption analysis

[0252] H2 chemisorption analysis was performed using Autochem 2920 (Micromeritics) equipment. At this time, 100 mg of sample was heated at 500 ℃ (5 ℃ min) under 10% H2 / Ar -1) was pretreated for 1 hour. Afterwards, it was purged under Ar at the same temperature for 30 minutes and cooled to 100 °C under the same flow. Then, a 10% H2 / Ar pulse was injected until the peak area was saturated.

[0253]

[0254] - Hydrogen Temperature-Programmed Reduction (H2-TPR) analysis

[0255] H2-TPR analysis was performed using Autochem 2920 (Micromeritics) equipment. At this time, 50 mg of sample was heated at 500 ℃ (5 ℃ min) under 10% O2 / He -1 ) for 1 hour, cooled to 50 ℃, and purged under Ar at the same temperature for 30 minutes. Then, it was purified at 650 ℃ (2.5 ℃ min) under 10% H2 / Ar. -1 ) was heated to .

[0256]

[0257] - Hydrogen Temperature-Programmed Desorption (H2-TPD) Analysis

[0258] H2-TPD analysis was performed using an Autochem 2929 (Micromeritics) equipped with a QGA spectrometer (Hiden). 100 mg of the sample was heated at 500 ℃ (5 ℃ min) under 10% H2 / Ar. -1 ) for 1 hour, purged under Ar at the same temperature for 30 minutes, and cooled to 100 ℃ under the same flow. Then, exposed for 1 hour under 10% H2 / Ar at the same temperature, purged for 1 hour under Ar flow, and then heated to 600 ℃ (10 ℃ min) under Ar -1 ) was heated to .

[0259]

[0260] Method for evaluating hydrogenation performance of catalysts

[0261]

[0262] - Batch A

[0263] A high-pressure batch reactor (Parr high-pressure reactor; 100 cm3) containing 10 g of H0-BT (Sasol; Lot No. S190595790) and a Ni catalyst (0.3 mol% Ni / H0-BT) was purged with hydrogen for 5 min and then pressurized to 50 bar with hydrogen. The reactor pressure was maintained constant throughout the reaction using a back pressure regulator (BPR). The reactor was heated to the desired temperature (160 °C, 170 °C, 180 °C) under stirring conditions of 1,200 rpm, and the reaction was carried out for 1 h. After completion of the reaction, the reactor was cooled to room temperature without stirring to recover the product and gas chromatography (GC) analysis (Agilent Technologies 7890A gas chromatography) was performed.

[0264]

[0265] - Batch B

[0266] A high-pressure batch reactor (Parr high-pressure reactor; 100 cm3) equipped with a high-pressure gas burette was used, and the pressure of the reactor was maintained at the same level throughout the entire reaction by supplying hydrogen gas from the burette to the reactor in an amount equivalent to that consumed during the reaction.

[0267] A high-pressure batch reactor containing 10 g of H0-BT and a Ni catalyst (0.3 mol% Ni / H0-BT) was purged three times with hydrogen and then pressurized to 5 bar. The reactor was heated to the desired temperature (180 °C, 190 °C, 200 °C) under stirring conditions of 1200 rpm, pressurized to 50 bar with hydrogen, and the reaction was performed until there was no change in the pressure in the burette.

[0268]

[0269] - Continuous experiment

[0270] A reactor filled with glass beads in the upper part, glass beads and Ni catalyst in the middle part, and spacers in the lower part was heated to the desired temperature (180°C or 220°C) under a hydrogen flow and then pressurized with hydrogen to 40 bar. The reactor pressure was maintained constant throughout the entire reaction using a back pressure regulator (BPR).

[0271] Next, H0-BT was supplied from a preheater (80°C) to the reactor using a liquid pump to perform the reaction (H2 / H0-BT molar ratio: 20). At this time, the sample collected in the trap was periodically recovered and subjected to GC analysis.

[0272]

[0273] Results and Discussion

[0274]

[0275] A. Characterization of C3TES-on-Al2O3

[0276]

[0277] The elemental composition, specific surface area, and pore properties of Al2O3, C3TES-on-Al2O3, Al2O3(r), and SGA_C3TES(r) are shown in Table 1 below.

[0278]

[0279] Material name: Si / Al a [mol%]Si / Al b [mol%]Si / Al c [mol%] carbon d [wt%]S BET e [㎡ / g]V p e [㎤ / g]D p e[nm]Al2O30.00.00.00.002700.586.11.4C3TES-on-Al2O32.01.4-1.332510.495.52.6C3TES-on-Al2O34.02 .6-2.452460.445.12.9C3TES-on-Al2O35.02.9-2.782460.435.03.0C3TES-on-Al2O38.03.0-2.852370.435. 0Al2O3(r)0.00.00.00.002700.586.1SGA_1.4C3TES(r)2.01.43.60.002600.546.1SGA_2.6C3TES(r)4.02.66 .40.002560.536.0SGA_2.9C3TES(r)5.02.98.20.002540.536.0SGA_3.0C3TES(r)8.03.08.30.002500.526.0

[0280] a : Theoretical (nominal) Si / Al ratio

[0281] b : Actual Si / Al ratio (calculated using ICP-OES analysis results)

[0282] c : Surface Si / Al ratio (calculated using XPS analysis results)

[0283] d : Carbon content

[0284] e : Specific surface area (S BET ), pore volume (V p ), pore diameter (D p )

[0285]

[0286] - The FT-IR spectra of Al2O3 and C3TES-on-Al2O3 are shown in Fig. 2. Referring to the drawing, C3TES-on-Al2O3 has a wavelength of 2962 cm corresponding to the CH bond of the alkyl group. -1 , 2934 cm -1 , 2910 cm -1 and 2877 cm -1In addition, as the amount of grafted C3TES increased, the size of the peak gradually increased and then became constant, indicating the presence of an alkyl group in C3TES-on-Al2O3. Meanwhile, as the amount of grafted C3TES increased, the size of the peak increased from 3800 to 3000 cm -1 The peak corresponding to the surface hydroxyl group observed in decreased convergence. This indicates that C3TES interacts with and grafts the surface hydroxyl group of Al2O3.

[0287] - The carbon content and actual Si / Al ratio of Al2O3 and C3TES-on-Al2O3 are shown in Fig. 3. The table and figure show the carbon content and actual Si / Al ratio according to the theoretical (nominal) Si / Al ratio of Al2O3 and C3TES-on-Al2O3. As the theoretical Si / Al ratio increased from 0 mol% to 8 mol%, the carbon content and the actual Si / Al ratio increased convergently to 2.85 wt% and 3.0 mol%, respectively.

[0288] - The N2 physisorption results of Al2O3 and C3TES-on-Al2O3 are shown in Fig. 4. According to the table and drawing, as the amount of grafted C3TES increases, the specific surface area (S BET ) and pore volume (V p ) all decreased convergently. From this, it can be seen that the grafted C3TES filled the pores of Al2O3.

[0289] - The XRD analysis results of Al2O3 and C3TES-on-Al2O3 are shown in Fig. 5. According to the figure, all samples exhibited only the diffraction pattern of γ-Al2O3 with similar peak sizes. Therefore, it can be seen that the grafted C3TES does not affect the crystallinity of γ-Al2O3.

[0290] - The N2 physisorption results of Al2O3(r) and SGA_C3TES(r) are shown in Fig. 6 (700 ℃ (5 ℃ min) under hydrogen atmosphere -1 ) for 3 hours). Referring to the above drawing, as the amount of C3TES grafted onto C3TES-on-Al2O3 increases, the S decreases. BET and V p After reduction treatment, it recovered to a level close to the initial value. This indicates that the alkyl group of grafted C3TES was removed by hydrogen reduction.

[0291] - The actual Si / Al ratio and the surface Si / Al ratio of Al2O3(r) and SGA_C3TES(r) are shown in Fig. 7, respectively. In the figure, when the actual Si / Al ratio and the surface Si / Al ratio are compared according to the theoretical (nominal) Si / Al ratio of Al2O3(r) and SGA_C3TES(r), as the theoretical Si / Al ratio increases up to 8 mol%, the actual Si / Al ratio and the surface Si / Al ratio increase convergently to 3.0 mol% and 8.3 mol%, respectively.

[0292] - The XRD analysis results of Al2O3(r) and SGA_C3TES(r) are shown in Fig. 8. Referring to the figure, all samples exhibited only the diffraction pattern of γ-Al2O3 with similar peak sizes, indicating that SiO2 generated by hydrogen reduction was grafted onto the surface of Al2O3 rather than being bound within the Al2O3 lattice.

[0293] - Al2O3(r) and SGA_C3TES(r) 27 The results of Al MAS NMR analysis are shown in Fig. 9. Referring to the drawing, as the amount of grafted C3TES increases, the 5-coordinate Al (Al V) species ratio decreased convergently, which means that C3TES is grafted while interacting with the Al species of the 5-coordinated Al2O3. In particular, the unstable surface 5-coordinated Al(Al V ) Considering that the decrease in species is due to the stabilizing effect of metal oxide, it is believed that the amount of C3TES grafted on the surface of Al2O3 depends on the surface properties of Al2O3.

[0294] - The measurement results of the water contact angle (θ) of Al2O3 and C3TES-on-Al2O3 are shown in Fig. 10. Referring to the figure, as the amount of grafted C3TES increases, the water contact angle increases convergently. This is due to the increased hydrophobicity due to the alkyl group of the grafted C3TES, and it can be seen that the amount of C3TES grafted onto the surface of Al2O3 increases and then converges.

[0295]

[0296] B. Characteristics and activity evaluation of Ni / SGA_C3TES catalyst

[0297]

[0298] The physicochemical properties of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Table 2 below.

[0299]

[0300] Catalyst name Ni a [wt.%]Si / Al b [mol%]Si / Al c [mol%] carbon d [wt%]S BET e [㎡ / g]V p e [㎤ / g]D p e [nm]V H2 f [㎤ / g cat ]D Ni g[nm]Ni / Al2O33.10.00.00.002450.506.10.374.1±0.7Ni / SGA_1.4C3TES3.21.44.00.002390.476.00.533.2±0.6Ni / SGA_2.6C3TES3.22.266.90 .002350.465.90.602.7±0.6Ni / SGA_2.9C3TES3.22.98.50.002350.455. 90.662.3±0.6Ni / SGA_3.0C3TES3.23.08.80.002300.455.90.672.3±0.6

[0301] a : Actual Ni content

[0302] b : Actual Si / Al ratio (calculated using ICP-OES analysis results)

[0303] c : Surface Si / Al ratio (calculated using XPS analysis results)

[0304] d : Carbon content

[0305] e : Specific surface area (S BET ), pore volume (V p ), pore diameter (D p )

[0306] f : Hydrogen adsorption capacity

[0307] g : Ni particle size

[0308]

[0309] - The XRD analysis results of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Fig. 11. According to the figure, all catalysts show only the diffraction peak of γ-Al2O3, indicating that Ni particles are well dispersed.

[0310] - HAADF-STEM images of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Fig. 12. According to the figure, as the ratio of Si / Al increases, the size of Ni particles (D Ni ) gradually decreased (4.1 nm for Ni / Al2O3 and 2.3 nm for Ni / SGA_3.0C3TES).

[0311] - The H2 chemisorption results of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Fig. 13. From the figure, as the ratio of Si / Al increases, the hydrogen adsorption amount (V H2 ) was confirmed to gradually increase. In this way, it can be seen that when the Si / Al ratio increases, the dispersion of Ni particles improves.

[0312] - XPS Ni 2p of Ni / Al2O3 and Ni / SGA_C3TES catalysts 3 / 2 The spectrum is shown in Fig. 14. According to the figure, as the ratio of Si / Al increases, Ni 0 Species fraction (F) metallic Ni ) has increased.

[0313] - The H2-TPR analysis results of oxidized Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Fig. 15. Referring to the figure, as the ratio of Si / Al increases, the amount of hydrogen consumed per Ni atom (A H2-TPR ) increased. In addition, the fraction of the high-temperature peak observed at 418 ℃ decreased due to the strong interaction between NiO and Al2O3, and the fraction of the newly generated peak at the low temperature of 310 ℃ increased. Considering the results of Figs. 14 and 15, it can be seen that the formation of NiAl2O4 spinel, which exhibits inactivity, is suppressed as the Si / Al ratio increases.

[0314] - The pyridine-chemisorbed FT-IR spectra of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Fig. 16. Referring to the figure, the amount of Lewis acid sites of the Ni / SGA_C3TES catalyst was further increased compared to Ni / Al2O3. This was due to the presence of not only Al-O defect sites but also Si + -O indicates the creation of defect sites. Meanwhile, in the case of the Ni / SGA_C3TES catalyst, the amount of Lewis acid sites gradually decreased as the Si / Al ratio increased (Ni / SGA_1.4C3TES: 176 μmol / g, Ni / SGA_3.0C3TES: 146 μmol / g). This can be attributed to the suppression of the formation of NiAl2O4 spinel, which is known to create Lewis acid sites, as the Si / Al ratio increased.

[0315]

[0316] - The results of measuring the H0-BT hydrogenation activity of Ni / Al2O3 and Ni / SGA_C3TES catalysts are shown in Table 3 below.

[0317]

[0318] Catalyst name T b [℃]X H0-BT c [%]S H4-BT d [%]S H6-BT d [%]S H10-BT d [%]S H12-BT d [%]DoH l e[%]Ni / Al2O316030.32.790.14.52.715.917059.01.290.83.44.631.418078.10.888.83.17.342.6Ni / SGA_1.4C3TES16038.84.586 .93.05.620.617067.10.089.53.86.736.618094.60.082.33.414.355.1Ni / SGA_2.6C3TES16068.62.185.83.68.537.817095.50.07 5.03.022.059.218099.00.022.22.775.187.5Ni / SGA_2.9C3TES16080.20.982.73.612.846.117099.30.066.53.130.465.8180100 .00.020.01.678.489.8Ni / SGA_3.0C3TES16080.30.683.43.013.046.217099.30.066.53.130.465.8180100.00.020.01.678.489.8

[0319] a : Reaction conditions: Batch A; 10 g H0-BT, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h

[0320] b : Reaction temperature

[0321] c : H0-BT conversion rate

[0322] d : H4-BT selectivity (S H4-BT ), H6-BT selectivity (S H6-BT ), H 10 -BT selectivity (S H10-BT ), H 12 -BT selectivity (S H12-BT )

[0323] e : Degree of hydrogenation

[0324]

[0325] In addition, the H0-BT hydrogenation activity (degree of hydrogenation: DoH) of Ni / Al2O3 and Ni / SGA_C3TES catalysts l) The measurement results are shown in Fig. 17. According to the table and drawings above, the hydrogenation performance increased as the Si / Al ratio increased. This is related to the fact that as the Si / Al ratio increases, the metallic Ni species become more abundant and smaller Ni particles are formed. In other words, this means that the active sites of the Ni / SGA_C3TES catalyst for the hydrogenation reaction of aromatic LOHC become more abundant as the Si / Al ratio increases. In this way, the evaluation results of the hydrogenation activity suggest that a unique metal-support interface is formed due to the structural characteristics of C3TES-on-Al2O3.

[0326]

[0327] All. Ni / SGA_C n Characterization and activity evaluation of TES catalysts

[0328]

[0329] Ni / Al2O3 and Ni / SGA_C n The elemental composition of the TES catalyst and the results of measuring H0-BT hydrogenation activity are shown in Table 4 below.

[0330]

[0331] Material name Ni b [wt%]Si / Al c [mol%]Si / Al d [mol%] carbon e [wt%]X H0-BT f [%]S H4-BT g [%]S H6-BT g [%]S H10-BT g [%]S H12-BT g [%]DoH l h[%]Ni / Al2O33.10.00.00.0030.32.790.14.52.715.9Ni / SGA_1.4C1TES3.21.44.70.0032.12. 388.14.25.417.2Ni / SGA_2.6C1TES3.22.67.50.0056.22.286.34.47.130.7Ni / SGA_2.9C1TES3 .22.99.00.0056.81.088.33.47.331.0Ni / SGA_3.0C1TES3.23.09.10.0059.21.286.63.68.63 2.7Ni / SGA_1.4C3TES3.21.44.20.0038.84.586.93.05.620.6Ni / SGA_2.6C3TES3.22.67.20.00 76.61.182.84.611.543.7Ni / SGA_2.9C3TES3.22.98.50.0080.20.982.73.612.846.1Ni / SGA_ 3.0C3TES3.23.08.80.0080.30.683.43.013.046.2Ni / SGA_1.4C8TES3.21.44.00.0031.43.388 .44.43.916.6Ni / SGA_2.6C8TES3.22.67.10.0067.91.889.53.75.036.3Ni / SGA_2.9C8TES3.22 .98.60.0073.10.486.83.09.840.8Ni / SGA_3.0C8TES3.23.08.80.0074.70.784.53.311.542.3

[0332] a : Reaction conditions: Batch A; 10 g H0-BT, 160 ℃, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h

[0333] b : Actual Ni content

[0334] c : Actual Si / Al ratio (calculated using ICP-OES analysis results)

[0335] d : Surface Si / Al ratio (calculated using XPS analysis results)

[0336] e : Carbon content

[0337] f : H0-BT conversion rate

[0338] g : H4-BT selectivity (S H4-BT ), H6-BT selectivity (S H6-BT ), H 10 -BT selectivity (S H10-BT ), H 12 -BT selectivity (S H12-BT )

[0339] h : Degree of hydrogenation

[0340]

[0341] - Ni / Al2O3 and Ni / SGA_C n The actual Si / Al ratio and surface Si / Al ratio of the TES catalyst are shown in Fig. 18, respectively. Referring to the above figure, all C n As the theoretical Si / Al ratio for TES increased to 8 mol%, the actual Si / Al ratio and the surface Si / Al ratio increased to approximately 3.0 mol% and 8.9 mol%, respectively. It is particularly noteworthy that the maximum amount of grafted silica was C n C present in TES-on-Al2O3 n C, not the length of the alkyl group of TES n It is said that the amount of TES was maintained almost constant.

[0342] - Ni / Al2O3 and Ni / SGA_C n H0-BT hydrogenation activity of TES catalyst (H0-BT conversion: X H0-BT ) The measurement results are shown in Fig. 19. Referring to the drawing, all Ni / SGA_C n As the Si / Al ratio increased for TES, the hydrogenation performance increased. In addition, Ni / SGA_2.9C showed the highest hydrogenation activity. n The TES catalysts were in the order of Ni / Al2O3< Ni / SGA_2.9C1TES < Ni / SGA_2.9C8TES < Ni / SGA_2.9C3TES, Cn As the length of the alkyl group of TES increased, Ni / SGA_2.9C3TES showed the best volcanic tendency.

[0343]

[0344] - Al2O3 and 2.9C n The N2 physisorption results of TES-on-Al2O3 are shown in Fig. 20. According to the figure, the grafted C n The longer the alkyl group of TES, the more S BET and V p The decrease was more pronounced. From this, the grafted C n It can be seen that TES fills the pores of Al2O3.

[0345] - Al2O3 and 2.9C n The measurement results of the water contact angle (θ) of TES-on-Al2O3 are shown in Fig. 21. According to the drawing, the grafted C n As the length of the alkyl group of TES increased, the water contact angle (i.e., hydrophobicity) increased.

[0346]

[0347] - Ni / Al2O3 and Ni / SGA_2.9C n The physicochemical properties of TES catalysts are shown in Table 5 below.

[0348]

[0349] Catalyst name S BET a,b [㎡ / g]V p a,b [㎠ / g]D p a,b [nm]V H2 c [㎤ / g cat ]D Ni d[nm]Ni / Al2O3245 (270)0.50 (0.58)6.1 (6.1)0.374.1±0.7Ni / SGA_2.9C1TES241 (253)0.46 (0.51)5.9 (5.3)0.652.4±0.5Ni / SGA_2.9C3TES235 (246)0.45 (0.43)5.9 (5.0)0.662.3±0.6Ni / SGA_2.9C8TES224 (240)0.45 (0.38)5.7 (4.4)0.562.7±0.5

[0350] a : The values ​​in parentheses are the characteristics of the support material.

[0351] b : Specific surface area (S BET ), pore volume (V p ), pore diameter (D p )

[0352] c : Hydrogen adsorption capacity

[0353] d : Ni particle size

[0354]

[0355] Also, Ni / Al2O3 and Ni / SGA_2.9C n The N2 physisorption results of the TES catalyst are shown in Fig. 22. According to the table and drawing, C grafted by hydrogen reduction n After the alkyl group of TES is removed, S BET and V p has almost recovered to its initial value.

[0356] - Ni / Al2O3 and Ni / SGA_2.9C n The XRD analysis results of the TES catalyst are shown in Fig. 23. Referring to the figure, all catalysts showed only the diffraction peak of γ-Al2O3, indicating that the Ni particles were well dispersed.

[0357] - Ni / Al2O3 and Ni / SGA_2.9C nThe HAADF-STEM image of the TES catalyst is shown in Fig. 24. Referring to the drawing, C n As the length of the alkyl group of TES increases, D Ni Ni / SGA_2.9C3TES showed the smallest reverse volcanic tendency, with the order being Ni / Al2O3 (4.1 nm) > Ni / SGA_2.9C8TES (2.7 nm) > Ni / SGA_2.9C1TES (2.4 nm) > Ni / SGA_2.9C3TES (2.3 nm).

[0358] - Ni / Al2O3 and Ni / SGA_2.9C n The results of H2 chemisorption of the TES catalyst are shown in Fig. 25. According to the drawing, C n As the length of the alkyl group of TES increases, V H2 showed the highest volcanic tendency in Ni / SGA_2.9C3TES.

[0359] - Ni / Al2O3 and Ni / SGA_2.9C n XPS Ni 2p of TES catalyst 3 / 2 The spectrum is shown in Fig. 26. According to the drawing, C n As the length of the alkyl group of TES increases, F metallic Ni This has increased.

[0360] - Oxidized Ni / Al2O3 and Ni / SGA_2.9C n The results of H2-TPR analysis of the TES catalyst are shown in Fig. 27. According to the drawing, C n A depending on the length of the alkyl group of TES H2-TPR This increased. In addition, the fraction of the high-temperature peak observed at 418 ℃ decreased due to the strong interaction between NiO and Al2O3, and the fraction of the newly generated peak at the low temperature of 310 ℃ increased.

[0361] From the results of the above-mentioned Figs. 26 and 27, C nIt can be seen that the longer the alkyl group of TES, the more the formation of NiAl2O4 spinel, which shows inactivity, is suppressed (F metallic Ni : 23.5% and A H2-TPR : 523 mmol H2 / mol Ni (Ni / Al2O3); F metallic Ni : 36.0% and A H2-TPR : 814 mmol H2 / mol Ni (Ni / SGA_2.9C8TES)).

[0362] - Ni / Al2O3 and Ni / SGA_2.9C n The pyridine-chemisorbed FT-IR spectrum of the TES catalyst is shown in Fig. 28. Referring to the figure, Ni / SGA_2.9C is higher than Ni / Al2O3. n The amount of Lewis acid sites in the TES catalyst was more abundant. Meanwhile, Ni / SGA_2.9C n For TES catalysts, C n As the length of the alkyl group of TES increased, the formation of NiAl2O4 spinel was suppressed, and the amount of Lewis acid sites decreased (Ni / SGA_2.9C1TES: 155 μmol / g, Ni / SGA_2.9C8TES: 138 μmol / g).

[0363]

[0364] La. C n Ni / SGA_C induced by TES-on-Al2O3 n Characterization of TES catalysts

[0365]

[0366] Ni / Al2O3, Ni / SGA_2.9C n TES, Ni / SGA_2.9C n The results of measuring the H0-BT hydrogenation activity of TES(c) and Ni / SIRAL1 catalysts are shown in Table 6 below.

[0367]

[0368] Catalyst name X H0-BT b[%]S H4-BT c [%]S H6-BT c [%]S H10-BT c [%]S H12-BT c [%]DoH l d [%]Ni / Al2O330.32.790.14.52.715.9Ni / SIRAL141.72.689.14.63.722.1Ni / SGA_2.9 C1TES56.81.088.33.47.331.0Ni / SGA_2.9C1TES(c)50.32.486.06.15.527.4Ni / SGA_ 2.9C3TES80.20.982.73.612.846.1Ni / SGA_2.9C3TES(c)50.12.587.14.65.827.1Ni / SGA_2.9C8TES73.10.486.83.09.840.8Ni / SGA_2.9C8TES(c)51.31.987.63.76.827.9

[0369] a : Reaction conditions: Batch A; 10 g H0-BT, 160 ℃, 50 bar H2, 0.3 mol% Ni / H0-BT, 1200 rpm, 1 h

[0370] b : H0-BT conversion rate

[0371] c : H4-BT selectivity (S H4-BT ), H6-BT selectivity (S H6-BT ), H 10 -BT selectivity (S H10-BT ), H 12 -BT selectivity (S H12-BT )

[0372] d : Degree of hydrogenation

[0373]

[0374] Additionally, the physicochemical properties of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c), and Ni / SIRAL1 catalysts are shown in Table 7 below.

[0375]

[0376] Catalyst name Ni b [wt%]Si / Al c [mol%]Si / Al d [mol%]S BET a,e [㎡ / g]V p a,e [㎠ / g]D p a,e [nm]V H2 f [㎠ / g cat ]D Ni g [nm]Ni / Al2O33.10.00.0245 (270)0.50 (0.58)6.1 (6.1)0.374.1±0.7Ni / SIRAL13.21.02.8282 (283)0.70 (0.78)7.9 (8.1)0.473.3±0.4Ni / SGA_2.9C3TES3.22.98.5235 (246)0.45 (0.43)5.9 (5.0)0.662.3±0.6Ni / SGA_2.9C3TES(c)3.12.98.4237 (261)0.47 (0.52)6.0 (6.0)0.483.3±0.5

[0377] a : The characteristics of the support are in parentheses.

[0378] b : Actual Ni content

[0379] c : Actual Si / Al ratio (calculated using ICP-OES analysis results)

[0380] d : Surface Si / Al ratio (calculated using XPS analysis results)

[0381] e : Specific surface area (S BET ), pore volume (V p ), pore diameter (D p )

[0382] f : Hydrogen adsorption capacity

[0383] g : Ni particle size

[0384]

[0385] - Ni / Al2O3, Ni / SGA_2.9C n TES, Ni / SGA_2.9C n The results of the H0-BT hydrogenation activity measurement of TES(c) and Ni / SIRAL1 catalysts are shown in Fig. 29. At this time, Ni / SGA_2.9C n TES(c) catalyst is 2.9C n TES-on-Al2O3 was heated at 600℃ (5℃ min) in air atmosphere -1 ) is manufactured by calcination (sintering) treatment for 5 hours, according to the table and drawing above, Ni / Al2O3, Ni / SGA_2.9C n TES, Ni / SGA_2.9C n X is an indicator of the H0-BT hydrogenation activity of TES(c) and Ni / SIRAL1 catalysts. H0-BT Looking at Ni / SGA_2.9C n The hydrogenation performance of TES(c) catalysts was similar to each other, but higher than that of Ni / Al2O3, but Ni / SGA_2.9C. n It was lower than that of the TES catalyst. From these results, C n It can be seen that the alkyl group of TES-on-Al2O3 affects the Ni species. Meanwhile, the hydrogenation activity of Ni / SIRAL1 was higher than that of Ni / Al2O3, but Ni / SGA_2.9C n It was lower than the TES(c) catalyst.

[0386] - The time for complete hydrogenation (t) was obtained as an activity result index by evaluating the H0-BT hydrogenation activity of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts in real time. full ), rate constant (k), and activation energy (E a) are shown in Figs. 30 and 31, respectively. Referring to the above drawings, results consistent with the activity evaluation results confirmed in Fig. 29 were obtained (Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) > Ni / SIRAL1 > Ni / Al2O3).

[0387] - The XRD analysis results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c), and Ni / SIRAL1 catalysts are shown in Fig. 32. Referring to the figure, all catalysts exhibited only the diffraction peak of γ-Al2O3. This indicates that the Ni particles are well dispersed.

[0388] - HAADF-STEM images of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts are shown in Fig. 33. Referring to the above drawing, D Ni It increased in the order of Ni / Al2O3(4.1 nm) > Ni / SIRAL1 = Ni / SGA_2.9C3TES(c) (3.3 nm) > Ni / SGA_2.9C3TES (2.3 nm).

[0389] - The H2 chemisorption results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts are shown in Fig. 34. In the figure, V H2 It increased in the order of Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) = Ni / SIRAL1 > Ni / Al2O3.

[0390] Considering the results according to the aforementioned Figs. 33 and 34, the grafted C n It was confirmed that the alkyl group of TES effectively suppresses the agglomeration of Ni particles.

[0391] - The measurement results of the water contact angle (θ) of Al2O3, 2.9C3TES-on-Al2O3, SGA_2.9C3TES(c) and SIRAL1 are shown in Fig. 35. From the above figure, the grafted C n It can be seen that the alkyl group of TES is the source of hydrophobicity, and furthermore, this hydrophobicity contributes to suppressing the mutual aggregation of Ni particles.

[0392] - XPS Ni 2p of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES (c) and Ni / SIRAL1 catalysts 3 / 2 The spectrum is shown in Fig. 36. Referring to the drawing, F metallic Ni (i.e., inhibition of the formation of NiAl2O4 spinel, which indicates inactivity) increased in the order of Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) = Ni / SIRAL1 > Ni / Al2O3, which means that the grafted C n This suggests that the alkyl group of TES contributes to improving the reducibility of Ni species.

[0393] - The H2-TPR analysis results of oxidized Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts are shown in Fig. 37. According to the drawing, A H2-TPR And the fraction of newly generated peaks at low temperatures of 310 ℃ increased in the order of Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) > Ni / SIRAL1 > Ni / Al2O3. From these results, the grafted C n It was confirmed that the alkyl group of TES alleviates the interaction between NiO and Al2O3, thereby suppressing the formation of NiAl2O4 spinel.

[0394] - The H2-TPD analysis results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts are shown in Fig. 38. Referring to the figure, the relative amount of hydrogen desorbed per Ni atom (A H2-TPD,Ni catalyst / A H2-TPD,Ni / Al2O3 ) increased in the order of Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) > Ni / SIRAL1 > Ni / Al2O3, which is consistent with the evaluation results of the dispersibility and reducibility of the previously obtained Ni particles. In this regard, the peak observed at a high temperature of 281 to 341 °C indicates hydrogen adsorption originating from NiAl2O4 spinel, and the peak observed at a low temperature of 184 to 204 °C indicates hydrogen adsorption originating from metallic Ni species. At this time, the hydrogen adsorbed on the metallic Ni species observed at a low temperature is the hydrogen that actually participates in the reaction.

[0395] - The TGA results of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c), and Ni / SIRAL1 catalysts adsorbed with H0-BT are shown in Fig. 39. Referring to the figure, the mass reduction of Ni / Al2O3 was 6.2 wt%, while the mass reductions in the other Ni catalysts were around 8.2 wt%. In addition, Ni / Al2O3 exhibited a single DTG peak at 137°C, while the other Ni catalysts exhibited two DTG peaks at about 130 to 210°C.

[0396] - The pyridine-chemisorbed FT-IR spectra of Ni / Al2O3, Ni / SGA_2.9C3TES, Ni / SGA_2.9C3TES(c), and Ni / SIRAL1 catalysts are shown in Fig. 40. As shown in the figure, the total amount and intensity of Lewis acid sites of the Ni / Al2O3 catalyst were lower than those of the other catalysts. In particular, the catalyst in which Ni was supported on a support combined with silica-alumina exhibited almost the same acid behavior. In this regard, electron-rich aromatic compounds can typically be preferentially adsorbed on electron-deficient Lewis acid sites. This suggests that the adsorption capacity of the Ni catalyst for H0-BT is related to the Lewis acid sites, as discussed above.

[0397]

[0398] Evaluation of catalyst stability through continuous experiments of Ni / Al2O3, Ni / SGA_2.9C3TES, and Ni / SGA_2.9C3TES(c)

[0399]

[0400] - The results of measuring the H0-BT hydrogenation activity of Ni / Al2O3, Ni / SGA_2.9C3TES, and Ni / SGA_2.9C3TES(c) catalysts through continuous experiments are shown in Fig. 41. Referring to the figure, the hydrogenation performance was shown in the order of Ni / SGA_2.9C3TES > Ni / SGA_2.9C3TES(c) > Ni / Al2O3 under all reaction conditions. In addition, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) showed similar catalytic stability, whereas Ni / Al2O3 showed lower catalytic stability.

[0401] - The N2 physisorption results of Ni / Al2O3, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) catalysts before (fresh) and after (spent) continuous experiments are shown in Fig. 42. According to the figure, almost similar catalytic activities were observed before and after the hydrogenation experiment.

[0402] - HAADF-STEM images of Ni / Al2O3, Ni / SGA_2.9C3TES and Ni / SGA_2.9C3TES(c) catalysts before (fresh) and after (spent) continuous experiments are shown in Fig. 43. Referring to the drawing, each D before and after the hydrogenation experiment Ni showed almost similar values, which means that there was almost no structural change in the Ni catalyst before and after the hydrogenation experiment, and it can be seen that this catalyst stability evaluation result is derived from the Lewis acid site for adsorbing H0-BT.

[0403]

[0404] B. Quantitative evaluation of hydrogen adsorption capacity according to catalyst

[0405]

[0406] The H2-TPR analysis results (reduction characteristics of nickel oxide) according to FIGS. 15, 27 and 37, and the H2 chemisorption analysis results (hydrogen adsorption per catalyst) according to FIGS. 13, 25 and 34 were converted into hydrogen adsorption per nickel, and the hydrogen adsorption capacity of each of the Ni / Al2O3, Ni / SGA_1.4C3TES, Ni / SGA_2.6C3TES, Ni / SGA_2.9C3TES, Ni / SGA_3.0C3TES, Ni / SGA_2.9C1TES, Ni / SGA_2.9C8TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1 catalysts was evaluated, and the results are shown in Table 8 below.

[0407]

[0408] Catalyst nameNi(wt%)TPD V H2 (㎤ / gcat )TPD V H2 (㎤ / mol Ni )TPD V H2 (mmol H2 / mol Ni )relative TPD V H2 (Standard: Ni / Al2O3)TPR V H2 (mmol H2 / mol Ni )relative TPR V H2 (standard: Ni / Al2O3)Ni / Al2O33.10.3770031.31.005231.00Ni / SGA_1.4C3TES3.20.5397243.41.395711.09Ni / SGA_2. 6C3TES3.20.60110049.11.577161.37Ni / SGA_2.9C3TES3.20.66121054.01.737981.53Ni / SGA_3.0C3TES3.2 0.67122954.91.757991.53Ni / SGA_2.9C1TES3.20.65119253.21.706881.32Ni / SGA_2.9C8TES3.20.5610274 5.91.478141.56Ni / SGA_2.9C3TES(c)3.20.4888039.31.265851.12Ni / SIRAL13.20.4786238.51.235451.04

[0409]

[0410] Referring to the above table, it was observed that Ni / SGA_2.6C3TES, Ni / SGA_2.9C3TES, Ni / SGA_3.0C3TES, Ni / SGA_2.9C1TES and Ni / SGA_2.9C8TES catalysts showed higher hydrogen adsorption per nickel compared to other catalysts (Ni / Al2O3, Ni / SGA_1.4C3TES, Ni / SGA_2.9C3TES(c) and Ni / SIRAL1). In particular, based on Ni / Al2O3, relative TPD V H2 is about 1.47 to 1.75 times higher, and also the relative TPR V H2is approximately 1.32 to 1.56 times higher, which indicates that the dispersion of metal nickel is excellent (i.e., the interaction between nickel, which is a hydrogenation metal, and the alumina support is alleviated) and the adsorption amount of hydrogen, which is an essential reactant for the hydrogenation reaction, is increased.

[0411] In addition, TPR V of Ni / SGA_2.6C3TES, Ni / SGA_2.9C3TES, Ni / SGA_3.0C3TES, Ni / SGA_2.9C1TES and Ni / SGA_2.9C8TES catalysts H2 (i.e., the amount of hydrogen used for the reduction of nickel oxide is 600 mmol H2 / mol Ni (0.6 mol H2 / mol Ni ) above, which suggests that not only does the reducibility of nickel oxide (NiO) increase (see Figs. 15, 27 and 37), but also that reduction at temperatures below 300°C increases.

[0412] Simple modifications or changes of the present invention can be easily utilized by those skilled in the art, and all such modifications or changes can be considered to be included in the scope of the present invention.

Claims

1. a) providing an alumina support; b) Alkyl group (C) on the alumina support n )-A step of preparing a modified alumina support by grafting an attached silica precursor; c) a step of introducing a transition metal precursor having hydrogenation activity into the modified alumina support to form a modified alumina support containing a precursor of a transition metal; and d) The above alkyl group (C n ) - a step of reducing the precursor-containing modified alumina support of the transition metal under elevated temperature conditions to remove alkyl groups derived from the attached silica precursor and form transition metal nanoparticles; A method for producing a catalyst for hydrogenation reaction comprising:

2. A method for producing a catalyst for hydrogenation reaction, characterized in that the method is performed without calcination treatment for each of the modified alumina support and the modified alumina support containing the precursor of the transition metal in the first paragraph.

3. A method for producing a catalyst for hydrogenation reaction, characterized in that the transition metal having the hydrogenation activity is at least one selected from the group consisting of nickel (Ni), zinc (Zn), iron (Fe), manganese (Mn), cobalt (Co), and copper (Cu).

4. In the first paragraph, the alkyl group (C n )-alkyl group of the attached silica precursor (C n ) is characterized in that the number of carbon atoms (n) is in the range of 1 to 18 and at least one silicon-containing compound selected from the group consisting of silane, siloxane, silazane and silanol.

5. In the first paragraph, the alkyl group (C n )-attached silica precursor is characterized by a method for producing a catalyst for hydrogenation reaction represented by the following general formula 1: [General Formula 1] R m -Si-X 4-m In the above formula, R is an alkyl group (C n ) and, m is 1 to 3, and X is at least one selected from the group consisting of an alkoxy group and a halogen group having 1 to 4 carbon atoms.

6. In the fifth paragraph, the alkyl group (C n )-A method for producing a catalyst for hydrogenation reaction, characterized in that the attached silica precursor is at least one selected from the group consisting of alkyltrialkoxysilane, dialkyldialkoxysilane, and trialkylalkoxysilane.

7. In the fifth paragraph, the alkyl group (C n )-attached silica precursors are methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, methyltripropoxysilane, dimethyldipropoxysilane, trimethylpropoxysilane, methyltributoxysilane, dimethyldibutoxysilane, trimethylbutoxysilane, methyltrifluorosilane, dimethyldifluorosilane, trimethylfluorosilane, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, methyltribromosilane, dimethyldibromosilane, trimethylbromosilane, methyltriiodosilane, dimethyldiiodosilane, trimethyliodosilane, ethyltrimethoxysilane, diethyldimethoxysilane, triethylmethoxysilane, Ethyltriethoxysilane, diethyldiethoxysilane, triethylethoxysilane, ethyltripropoxysilane, diethyldipropoxysilane, triethylpropoxysilane, ethyltributoxysilane, diethyldibutoxysilane, triethylbutoxysilane, ethyltrifluorosilane, diethyldifluorosilane, triethylfluorosilane, ethyltrichlorosilane, diethyldichlorosilane, triethylchlorosilane, ethyltribromosilane, diethyldibromosilane, triethylbromosilane, ethyltriiodosilane, diethyldiiodosilane, triethyliodosilane, propyltrimethoxysilane, dipropyldimethoxysilane, tripropylmethoxysilane, propyltriethoxysilane, dipropyldiethoxysilane, tripropylethoxysilane, propyltripropoxysilane, dipropyldipropoxysilane, Tripropylpropoxysilane, propyltributoxysilane, dipropyldibutoxysilane, tripropylbutoxysilane, propyltrifluorosilane, dipropyldifluorosilane, tripropylfluorosilane, propyltrichlorosilane, dipropyldichlorosilane, tripropylchlorosilane, propyltribromosilane, dipropyldibromosilane, tripropylbromosilane, propyltriiodosilane, dipropyldiiodosilane, tripropyliodosilane, butyltrimethoxysilane, dibutyldimethoxysilane, tributylmethoxysilane, butyltriethoxysilane, dibutyldiethoxysilane, tributylethoxysilane, butyltripropoxysilane, dibutyldipropoxysilane, tributylpropoxysilane, butyltributoxysilane, dibutyldibutoxysilane, tributylbutoxysilane,Butyltrifluorosilane, dibutyldifluorosilane, tributylfluorosilane, butyltrichlorosilane, dibutyldichlorosilane, tributylchlorosilane, butyltribromosilane, dibutyldibromosilane, tributylbromosilane, butyltriiodosilane, dibutyldiiodosilane, tributyliodosilane, hexyltrimethoxysilane, dihexyldimethoxysilane, trihexylmethoxysilane, hexyltriethoxysilane, dihexyldiethoxysilane, trihexylethoxysilane, hexyltripropoxysilane, dihexyldipropoxysilane, trihexylpropoxysilane, hexyltributoxysilane, dihexyldibutoxysilane, trihexylbutoxysilane, hexyltrifluorosilane, dihexyldifluorosilane, Trihexylfluorosilane, hexyltrichlorosilane, dihexyldichlorosilane, trihexylchlorosilane, hexyltribromosilane, dihexyldibromosilane, trihexylbromosilane, hexyltriiodosilane, dihexyldiiodosilane, trihexyliodosilane, octyltrimethoxysilane, dioctyldimethoxysilane, trioctylmethoxysilane, octyltriethoxysilane, dioctyldiethoxysilane, trioctylethoxysilane, octyltripropoxysilane, dioctyldipropoxysilane, trioctylpropoxysilane, octyltributoxysilane, dioctyldibutoxysilane, trioctylbutoxysilane, octyltrifluorosilane, dioctyldifluorosilane, trioctylfluorosilane, octyltrichlorosilane, dioctyldichlorosilane, Trioctylchlorosilane, octyltribromosilane, dioctyldibromosilane, trioctylbromosilane, octyltriiodosilane, dioctyldiiodosilane, trioctyliodosilane, decyltrimethoxysilane, didecyldimethoxysilane, tridecylmethoxysilane, decyltriethoxysilane, didecyldiethoxysilane, tridecylethoxysilane, decyltripropoxysilane, didecyldipropoxysilane, tridecylpropoxysilane, decyltributoxysilane, didecyldibutoxysilane, tridecylbutoxysilane, decyltrifluorosilane, didecyldifluorosilane, tridecylfluorosilane, decyltrichlorosilane, didecyldichlorosilane, tridecylchlorosilane, decyltribromosilane, didecyldibromosilane, Tridecylbromosilane, decyltriiodosilane, didecyldiiodosilane, tridecyliodosilane, dodecyltrimethoxysilane, didodecyldimethoxysilane, tridodecylmethoxysilane,Dodecyltriethoxysilane, didodecyldiethoxysilane, tridodecylethoxysilane, dodecyltripropoxysilane, didodecyldipropoxysilane, tridodecylpropoxysilane, dodecyltributoxysilane, didodecyldibutoxysilane, tridodecylbutoxysilane, dodecyltrifluorosilane, didodecyldifluorosilane, dodecyltrichlorosilane, didodecyldichlorosilane, tridodecylchlorosilane, dodecyltribromosilane, didodecyldibromosilane, tridodecylbromosilane, dodecyltriiodosilane, didodecyldiiodosilane, tridodecyliodosilane, hexadecyltrimethoxysilane, dihexadecyldimethoxysilane, Trihexadecylmethoxysilane, hexadecyltriethoxysilane, dihexadecyldiethoxysilane, trihexadecylethoxysilane, hexadecyltripropoxysilane, dihexadecyldipropoxysilane, trihexadecylpropoxysilane, hexadecyltributoxysilane, dihexadecyldibutoxysilane, trihexadecylbutoxysilane, hexadecyltrifluorosilane, dihexadecyldifluorosilane, trihexadecylfluorosilane, hexadecyltrichlorosilane, dihexadecyldichlorosilane, trihexadecylchlorosilane, hexadecyltribromosilane, dihexadecyldibromosilane, trihexadecylbromosilane, hexadecyltriiodosilane, dihexadecyldiiodosilane, Trihexadecyliodosilane, octadecyltrimethoxysilane, dioctadecyldimethoxysilane, trioctadecylmethoxysilane, octadecyltriethoxysilane, dioctadecyldiethoxysilane, trioctadecylethoxysilane, octadecyltripropoxysilane, dioctadecyldipropoxysilane, trioctadecylpropoxysilane, octadecyltributoxysilane, dioctadecyldibutoxysilane, trioctadecylbutoxysilane, octadecyltrifluorosilane, dioctadecyldifluorosilane, trioctadecylfluorosilane, octadecyltrichlorosilane, dioctadecyldichlorosilane, trioctadecylchlorosilane, octadecyltribromosilane, dioctadecyldibromosilane, trioctadecylbromosilane, A method for producing a catalyst for hydrogenation reaction, characterized in that at least one selected from the group consisting of octadecyltriiodosilane, dioctadecyldiiodosilane, and trioctadecyliodosilane.

8. A method for producing a catalyst for hydrogenation reaction, characterized in that in the first paragraph, the reduction treatment is performed at 500 to 900°C under a reducing gas atmosphere in which at least one gas is selected from the group consisting of hydrogen, carbon monoxide, carbon dioxide, and methane.

9. A method for producing a catalyst for hydrogenation reaction, characterized in that, in the first paragraph, the amount of hydrogen used to reduce the oxide of the transition metal in the hydrogenation catalyst is at least 0.6 mol (H2) / mol (transition metal) when measured by temperature reduction analysis (TPR).

10. A method for producing a catalyst for hydrogenation reaction, characterized in that in paragraph 1, the ratio of Si / Al in the catalyst is controlled in the range of 0.01 to 5 mol%.

11. A method for producing a catalyst for hydrogenation reaction, characterized in that in paragraph 1, the content (support amount) of the transition metal in the catalyst is set in the range of 0.1 to 30 wt%.

12. In the first paragraph, the alumina support has a specific surface area (BET) of 50 to 500 m2 / g, a pore volume of 0.2 to 2 cm3 / g, and a pore size of 3 to 15 nm, and A method for producing a catalyst for hydrogenation reaction, wherein the modified alumina support has a specific surface area (BET) of 40 to 480 m2 / g, a pore volume of 0.1 to 1.8 cm3 / g, and a pore size of 2 to 14 nm.

13. Modified alumina support; and Transition metal nanoparticles having hydrogenation activity supported on the above modified alumina support; As a hydrogenation catalyst comprising: The content (support amount) of the transition metal in the above hydrogenation catalyst is determined in the range of 0.1 to 30 wt%, The above modified alumina support is a silica modified alumina support, and A hydrogenation catalyst, wherein the amount of hydrogen used to reduce an oxide of a transition metal in the catalyst is at least 0.6 mol (H2) / mol (transition metal), as measured by temperature-induced reduction analysis (TPR).

14. A hydrogenation catalyst according to claim 13, characterized in that the dispersion (measured by H2 chemisorption) of transition metal nanoparticles supported on the modified alumina support in the catalyst is at least 2%.

15. A hydrogenation catalyst according to claim 13, characterized in that the size of the transition metal nanoparticles supported on the modified alumina support in the base catalyst (measured by high-angle annular dark-field scanning transmission electron microscopy) is 10 nm or less.

16. A hydrogenation catalyst according to claim 13, characterized in that the amount of acid sites in the catalyst is at least 100 μmol / g when analyzed by pyridine-chemisorbed FT-IR spectrum.

17. In the 13th paragraph, the hydrogenation catalyst is characterized in that it has a specific surface area (BET) of 30 to 460 m2 / g, a pore volume of 0.15 to 1.9 cm3 / g, and a pore size of 2.5 to 14.5 nm.

18. A hydrogenation step of storing hydrogen in a liquid organic hydrogen carrier in the presence of a catalyst; and A dehydrogenation step for releasing hydrogen from the hydrogenated liquid organic hydrogen carrier in the presence of a catalyst, The catalyst used in the above hydrogenation step is: modified alumina support; and A transition metal having hydrogenation activity supported on the above modified alumina support; Includes, The content (support amount) of the transition metal in the above hydrogenation catalyst is determined in the range of 0.1 to 30 wt%, The above modified alumina support is a silica modified alumina support, When measured by temperature reduction analysis (TPR), the amount of hydrogen used to reduce the oxide of the transition metal in the catalyst is at least 0.6 mol (H2) / mol (transition metal), and A method for storing hydrogen or releasing hydrogen by alternately performing the above hydrogenation step and dehydrogenation step.

19. In the 18th paragraph, the liquid organic hydrogen carrier is characterized in that at least one compound selected from compounds represented by the following general formulae 2 to 11: [General Formula 2] [General Formula 3] [General Formula 4] [General Formula 5] [General Formula 6] [General Formula 7] [General Formula 8] [General Formula 9] [General Formula 10] [General Formula 11] In the above formula, R, R1, R2, R3, R4, R5, R6, R7. R8, R9, R 10 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 and R 20 Each is hydrogen or an alkyl group of C1 to C6, and X is -(CHR 21 ) n -(n is an integer from 1 to 3, and R 21 is H, OH, or an alkyl group of C1 to C6), and Y is CH or N. .

20. A method according to claim 19, characterized in that the ratio (M / R) of transition metal / LOHC in the catalyst in the hydrogenation step is set in the range of 0.01 to 1 mol%.

21. A method according to claim 19, characterized in that the hydrogenation step is performed at a temperature of 50 to 250°C and a pressure of 5 to 100 bar.

Citation Information

Patent Citations

  • Catalyst for hydrogenation and dehydrogenation of organic hydrogen storage liquid, preparation method of catalyst and hydrogenation and dehydrogenation method of organic hydrogen storage liquid

    CN114700084A

  • Carrier for kids and operation system thereof

    KR1020210005422A

  • Compositions and manufacturing method thereof

    KR1020240150191A

  • Sol Gel Functionalized Silicate Catalyst and Scavenger

    US20090036297A1

  • Silica-alumina composite materials for hydroprocessing applications

    WO2021091952A1