Method for producing bimodal carbon nanostructures for use in supercapacitors
The method for producing bimodal carbon structures using P-cyclodextrin and controlled processing conditions addresses the challenge of achieving high specific capacitance and power density in supercapacitors, resulting in improved energy storage and voltage stabilization capabilities.
Patent Information
- Application Number
- PCT/PL2023/050032
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for producing carbon structures for supercapacitors do not adequately achieve high specific capacitance and power density values, which are essential for efficient energy storage and voltage stabilization in electrical grids and power-enhancing components.
A method involving the use of P-cyclodextrin as a raw material, with a process that includes burning, treatment with an alkaline reagent, activation, and purification steps, specifically using a shielding gas atmosphere and controlled temperature and pressure conditions to create bimodal carbon structures with optimized porosity and surface chemistry.
The method results in carbon structures with significantly increased specific capacitance above 200 F/g and enhanced power density, as demonstrated by bimodal pore distribution and energy density improvements in supercapacitors, facilitating better energy storage and voltage stabilization.
Smart Images

Figure 000011 
Figure 00000010_0000
Abstract
Description
[0001] METHOD FOR PRODUCING BIMODAL CARBON NANOSTRUCTURES FOR USE
[0002] IN SUPERCAPACITORS
[0003] Field of the invention
[0004] The invention relates to a method for producing bimodal carbon structures with high values of specific capacitance and power density at the same time, for use in supercapacitors, devices that smooth out voltage collapses and peak overloads of low- and high-power electrical grids, and in power-enhancing components for solar cells and chemical power sources.
[0005] State of the art
[0006] Supercapacitors are devices with a large electrical capacity, far exceeding the capacity of ordinary capacitors. A supercapacitor contains two porous electrodes, an electrolyte and a separator. Its special properties are achieved through the use of active carbon structures, which are the main building blocks of the electrodes in the capacitor. The properties of a supercapacitor are therefore dependent on the properties of the electrodes used, and in particular on the specific carbon structures. A key factor to achieve the best possible parameters for capacitor capacitance is to obtain carbon structures with optimum porosity and the right surface chemistry, which are influenced by the type of raw material and the preparation conditions. Carbon structures are obtained from various carbon-containing source materials, such as, e.g., bamboo, coconutshells, willow peat, wood, coconut fibre, lignite and petroleum tar. Methods for obtaining active carbon structures for use in supercapacitors are known in the art.
[0007] One of these is a method for the pyrolytic formation of carbon nanostructures for use in supercapacitors, described in CN103539118B. The method relates to the preparation of active carbon, involving pre-treatment of the rice husk raw material, charring, pre-treatment of the charred material, activation and post treatment. Pre-treatment of the raw material includes treatment with alkaline reagents, mixed reagents and pre-treatment by water infiltration. The sources of rice husk raw material used are large, which helps to reduce costs. Carbon obtained by this method has potential for use as an electrode material in super capacitors.
[0008] In addition, CN102826549A describes a method for preparing active carbon for use in supercapacitors, involving the following steps: crushing of petroleum coke, milling, sifting and carbonisation of the coke under a nitrogen atmosphere, treatment of the carbonised petroleum coke with HNO3 solution at 30-50°C for 4h, filtering and washing until neutralised, drying at 50°C, expanding at 130-160°C, mixing the expanded petroleum coke with KOH in a weight ratio of 1 :3, activating the coke by heating its mixture with KOH at 800-850°C under a nitrogen atmosphere for 2-3 hours, boiling the product in an aqueous HC1 solution for 5 minutes, washing with deionised water until neutralised, thus obtaining activated carbon. This treatment allows the distance between layers of petroleum coke graphite microcrystals to be increased and the thickness of these microcrystals to be reduced, which facilitates the activation of petroleum coke and improves such properties of activated carbon as specific surface area and specific volume.
[0009] EP3445712B1 discloses the production of active carbons characterised by a BET specific surface area between 1000 m2 / g and 3500 m2 / g, with the method comprising the following steps: mixing the carbon precursor with a first component containing a first salt (potassium carbonate, potassium bicarbonate or potassium chloride) and one or more second components containing at least one second salt, which is phosphate; preheating the mixture to a first temperature of 150°C to 600°C and soaking for 10 min to 10 h in an inert medium, and activating the mixture in an inert medium by increasing the temperature to a second, higher temperature of 600°C to 1000°C and soaking for 10 min to 20 h. The method is carried out without using any strong acids or alkalines. Petroleum tar, coconut shell powder, brown coal, municipal waste, industrial by-products, asphaltenes, biowaste, organic waste, biomass, agricultural waste, wood byproducts, fruit shells, nut shells, carbon fibres, synthetic polymers, carbohydrates, resins, and combinations of these can be used as carbon precursors in this method.
[0010] KR101982987B1 describes a method for producing active carbon for high-power energy storage, including: a step of impregnating and pulverising cellulose-based biomass; a step of loading the impregnated and pulverised biomass into an oven; a step of activating the biomass; a step of cooling the activated biomass; and a step of cleaning the cooled biomass with a cleaning solution to produce active carbon, with either active gas or inert gas being supplied to the oven.
[0011] However, there is a continuing need to provide a method for obtaining carbon structures for use as electrode materials in supercapacitors, which structures would be characterised by increased values of specific capacitance and power density. Summary of the invention
[0012] The objective of the present invention was to provide a method for obtaining carbon structures for use as electrode materials in supercapacitors that would allow improved specific capacitance and power density values to be obtained in supercapacitors built with these structures. Unexpectedly, it turned out that the combination of an alternative raw material, a sequence of steps and process parameters set out below allowed this objective to be met.
[0013] In its first aspect, the present invention relates to a method for producing carbon structures, comprising the following steps: a) burning a raw material; b) treating the biochar with an alkaline reagent solution and drying the biochar; c) activating the biochar; d) purifying the biochar;
[0014] In the method according to the invention, P-cyclodextrin is used as the raw material. In step a), the raw material is exposed to a temperature of 80 to 120°C, preferably 100°C, for 1 to 3 h, preferably 2 h, in a shielding gas atmosphere, then stabilised at a temperature of 450 to 550°C, preferably 500°C, for 2 to 8 h, preferably 5 h, and carbonised at a temperature of 700 to 900°C, preferably 800°C, for 3.5 to 4.5 h, preferably 4 h. In step b), a solution of alkaline reagent at a mass concentration of 25 to 35%, preferably 30%, is used, which is mixed with the biochar over a period of 22 to 26 h, preferably 24 h, in a mass ratio of biochar : alkaline reagent of 1 : 2.5 to 1:3.5, preferably 1:3. In step c), additional activation of the biochar is carried out by supplying the reaction medium with an aqueous aerosol in a shielding gas.
[0015] Preferably, argon is used as the shielding gas.
[0016] Preferably, the pressure in step a) is IkPa.
[0017] Preferably, in step a), the gaseous products are removed by a stream of shielding gas delivered at a rate of 2-5 1 / min.
[0018] Preferably, in step b), the biochar is dried at a temperature of 100-110°C. Preferably in step c), the activation of the biochar is carried out at a temperature of 700°C for 90 minutes in the flowing argon at a pressure of 1 kPa with simultaneous removal of the gaseous reaction products by a stream of shielding gas delivered at a rate of 1-2 1 / min.
[0019] Preferably in step c), the aerosol used in the additional activation contains water droplets of 5- 20 pm.
[0020] Preferably in step d), the biochar is washed with water until the pH of the washing water reaches a value below 8.5-9 and then dried at a temperature of 100-110°C.
[0021] In its second aspect, the present invention relates to the use of carbon structures by the method according to the invention defined above as an electrode material in super capacitors.
[0022] Advantages of the invention
[0023] The method for producing carbon structures according to the invention leads to an optimum, bimodal carbon structure with pores adapted to the electrolytes used in supercapacitors and to the energy topology of defects in the solid. The pore bimodality obtained by the method according to the invention ensures good diffusion contact between micro- and mesopore ions, which significantly reduces the resistance of the entire supercapacitor system and consequently increases its power density. Based on modelling with density functional theory (DFT) of nitrogen adsorption-desorption isotherms, a conclusion was drawn about the bimodality of the pores in the resulting carbon. The modelling results are shown in Fig. 1, which clearly shows two peaks in the pore distribution diagram. In addition, the carbon structures thus formed, which have an optimally selected porous structure and energy topology of defects resulting from dosed additives, provide a high specific capacitance value above 200 F / g in the negative potential range, which ultimately increases the energy density of the supercapacitor (specific capacitance measured by galvanostatic charging and discharging method).
[0024] Brief description of the figures of drawing
[0025] The invention in an embodiment is illustrated in the drawing, in which Fig. 1 shows the distribution of specific volume V [cm3 / g] as a function of pore size (radius r [nm]), clearly indicating the bimodal nature of the material obtained.
[0026] Detailed description of the invention
[0027] Below, in the description of the present invention, the following terminology is adopted: In the context of the present invention, the term "raw material" means a raw material of organic origin, more specifically 0-cyclodextrin. Cyclodextrins are cyclic glucose oligomers that are obtained by hydrolysis of starch.
[0028] In the context of the present invention, the term "biochar" means the residue after carbonisation of an organic raw material, while the term "carbonisation" means a thermal process leading to an increase in the carbon content of the processed raw material.
[0029] In the context of the present invention, the term "shielding gas" means an inert gas, in particular a noble gas, with which the reactor volume is filled. "Reactor" in the context of the present invention means any process apparatus capable of maintaining stable reaction conditions, including in particular pressure and temperature.
[0030] As indicated above, the object of the invention is a method for producing carbon structures.
[0031] This method is adapted to the processing of organic raw material, and more precisely - 0- cyclodextrin.
[0032] The method for producing carbon structures according to the invention comprises four steps, which will be described in detail below.
[0033] The first step is the burning of the organic raw material. For this purpose, the raw material, i.e. P-cyclodextrin, preferably in a powder form, is placed in the reactor, and then a vacuum is created and shielding gases are fed into the reactor. Any inert gas can be used as a shielding gas, with argon being preferable. The shielding gas fills the reactor volume and is then pressurised to a value of 0.5 to 2 kPa above atmospheric pressure. The contents of the reactor are heated at a constant rate to a temperature of 80 to 120°C, preferably 100°C, and are left at this temperature for 1 to 3 h, preferably 2 h. Then, a stabilisation treatment is carried out at a temperature of 450 to 550°C, preferably 500°C, for a period of 2 to 8 h, preferably 5 h, followed by carbonisation at a temperature of 700 to 900°C, preferably 800°C for a period of 3.5 to 4.5 h, preferably 4 h.
[0034] Gaseous reaction products should be removed when carrying out this step. They are removed by a stream of shielding gas, preferably argon, flowing through the reactor. Preferably, there is an excess of shielding gas maintained in the reactor at about 1 kPa above atmospheric pressure. Once carbonisation is complete, the reactor cools spontaneously. In the second step, after cooling, the biochar is unloaded from the reactor and mixed with an alkaline reagent solution having a mass concentration of 25 to 35%, preferably 30%. The solution is added to the biochar, respecting a mass ratio of biochar : alkaline reagent of 1:2.5 to 1:3.5, preferably 1:3. The treatment of the biochar with the alkaline reagent solution with simultaneous stirring, in particular using a magnetic stirrer, is carried out over a period of 22 to 26 h, preferably 24 h. Any substance of an alkaline nature, preferably an alkali metal or alkaline earth metal hydroxide, e.g. potassium hydroxide (KOH), can be used as the alkaline reagent. After this period, the biochar together with the remaining solution is placed back in the oven and dried at a temperature higher than room temperature, preferably in the range of 100-110°C.
[0035] In the third step, the dried biochar is placed in the thermal reactor, where its activation is carried out at a temperature of 600 to 800°C, preferably 700°C for a period of 75 to 105 minutes, preferably 90 minutes, in the flowing shielding gas. During the activation of the biochar, the gaseous products are removed along with the fed stream of shielding gas that flows through the reactor. In this step, an additional activation of the biochar is also carried out by delivering an aqueous aerosol with a water droplet size of 5-20 pm into the shielding gas atmosphere, directly from an ultrasonic aerosol generator to the reactor. At the end of the third step, the reactor contents are spontaneously cooled.
[0036] In the fourth step, the activated carbon is washed with water to remove the alkaline reagent. Rinsing is carried out until the rinse water reaches a pH value of less than 8.5-9. The carbon is then dried at a temperature in the range of 100-110°C.
[0037] Exemplary embodiment
[0038] The method for producing carbon structures was carried out as follows:
[0039] 1) P-cyclodextrin in a dry powder form was placed in the thermal reactor for burning. A vacuum was created and the shielding gas, argon, was introduced. The reactor volume was filled with argon to equalize the pressure, and then the pressure was increased to a level of about 1 kPa above atmospheric pressure. The reactor contents were then heated at a constant rate of temperature increase of l°C / min until the temperature reached 100°C, after which the reactor contents were left at this temperature for 2 h. A stabilisation treatment was then carried out by maintaining the reactor contents at a temperature of 500°C for 5 h, after which the reactor contents were subjected to carbonisation at 800°C for 4 h. The gaseous reaction products were removed by a stream of argon, which was delivered at a rate of 2-5 1 / min, through a hydrovalve in a controlled manner. The excess pressure of argon was maintained in the reactor at a level of about 1 kPa. Once this step was completed, the oven was switched off and cooled spontaneously.
[0040] 2) After cooling to room temperature, the biochar was placed in a KOH solution with a mass concentration of 30% while maintaining a mass ratio of biochar : KOH = 1 :3. The biochar was then stirred in the KOH solution for 24 hours with a magnetic stirrer. After this period, the biochar together with the remaining solution was moved to the oven and dried at a temperature in the range of 100-110°C.
[0041] 3) In the next step, the dried biochar was moved to the thermal reactor, where its activation was carried out at 700°C for 90 minutes in the flowing argon. The gaseous reaction products were removed by a stream of argon, fed at a flow rate of 1-2 1 / min, through the hydrovalve in a controlled manner. The excess pressure of argon was maintained in the reactor at a level of about 1 kPa. An additional activation was carried out by delivering an aqueous aerosol into the argon atmosphere, directly from an ultrasonic aerosol generator to the reactor. The size of water droplets is 5-20 pm, the efficiency of the generator is 3.0±0.5 cm3 / min., the frequency of the ultrasound emitter is 2.64 MHz. Once this step was completed, the oven was switched off and cooled spontaneously.
[0042] 4) After cooling to room temperature, the activated carbon was withdrawn from the reactor and washed with water to remove the KOH activator. The carbon was then dried in the oven at a temperature in the range of 100-110°C until a constant mass was obtained.
[0043] The carbon structures produced had a specific surface area of more than 1,500 m2. These data were obtained using BET analysis of nitrogen adsorption isotherms, which were obtained with a Nova Touch LX2 porometer.
Claims
Claims1. A method for producing bimodal carbon structures, comprising the following steps: a) burning a raw material; b) treating the biochar with an alkaline reagent solution and drying the biochar; c) activating the biochar; d) purifying the biochar; characterised in that P-cyclodextrin is used as the raw material, wherein in step a), the raw material is exposed to a temperature of 80 to 120°C for 1 to 3h in a shielding gas atmosphere, then stabilised at a temperature of 450 to 550°C for 2 to 8h, and carbonised at a temperature of 700 to 900°C for 3.5 to 4.5h, wherein in step b), a solution of alkaline reagent at a mass concentration of 25 to 35% is used, which is mixed with the biochar over a period of 22 to 26 h in a mass ratio of biochar : alkaline reagent of 1:2.5 to 1:3.5, wherein in step c), additional activation of the biochar is carried out by supplying the reaction medium with an aqueous aerosol in a shielding gas.2 The method according to claim 1, wherein argon is used as the shielding gas.3 The method according to claim 1 or 2, wherein the pressure in step a) is IkPa.4 The method according to one of claims 1-3, wherein in step a), the gaseous products are removed by a stream of shielding gas delivered at a rate of 2-5 1 / min.5 The method according to one of claims 1-4, wherein in step b), the biochar is dried at a temperature of 100-110°C.6 The method according to one of claims 1-5, wherein in step c), the activation of the biochar is carried out at a temperature of 700°C for 90 minutes in the flowing argon at a pressure of 1 kPa with simultaneous removal of the gaseous reaction products by a stream of shielding gas delivered at a rate of 1 -2 1 / min.7 The method according to one of claims 1-6, wherein in step c), the aerosol used in the additional activation contains water droplets of 5-20 pm.
8. The method according to one of claims 1-6, wherein in step d), the biochar is washed with water until the pH of the washing water reaches a value below 8.5-9 and then dried at a temperature of 100-110°C.
9. Use of bimodal carbon structures by the method according to one of claims 1-8 as an electrode material in super capacitors.